Method for producing water-based polyester resin, water-based polyester resin, method for producing water-based coating composition, and water-based coating composition

A production method for water-based polyester resin using recycled materials enhances dispersibility and stability, matching non-recycled resin properties, and reduces environmental impact by optimizing ester formation and polycondensation processes.

JP7561438B2Active Publication Date: 2024-10-04GOO CHEM IND
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
JP2022003933
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-01-13
Publication Date
2024-10-04
Estimated Expiration
2042-01-13

AI Technical Summary

Technical Problem

Existing water-based polyester resins produced from recycled polyester suffer from low water dispersibility and stability, which is exacerbated by the use of surfactants that contaminate the resin film and reduce environmental sustainability.

Method used

A method involving an ester formation and polycondensation process using recycled polyester, divalent and trivalent polycarboxylic acid components, and polyhydric alcohol components, with specific ratios and acid values to enhance water dispersibility and stability without surfactants, incorporating terephthalic acid residues from recycled polyester.

Benefits of technology

The method produces a water-based polyester resin with excellent water resistance, dispersibility, and stability, maintaining long-term dispersion and reducing environmental impact, while achieving properties comparable to resins derived from non-recycled terephthalic acid.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007561438000001
    Figure 0007561438000001
  • Figure 0007561438000002
    Figure 0007561438000002
  • Figure 0007561438000003
    Figure 0007561438000003
Patent Text Reader

Abstract

To provide a method for producing a water-based polyester resin which, while reducing an environmental load, has excellent water resistance, has excellent water dispersibility, and also has excellent stability of a resin dispersion, which, while having a terephthalic acid residue derived from recycled polyester, has resin characteristics such as adhesiveness and transparency of the same level as those obtained when terephthalic acid not derived from recycled polyester and the like are used, and a resin dispersion of which has excellent long-period water dispersibility and can improve stability such as temporal stability of solution haze.SOLUTION: A method for producing a water-based polyester resin comprises a first step, a second step, and a third step. In the first step, an ester formation reaction and a depolymerization reaction are carried out using recycled polyester, a first polycarboxylic acid component including a dibasic polycarboxylic acid residue, and a polyhydric alcohol component. In the second step, an ester formation reaction is carried out using a reaction product of step 1 and a second polycarboxylic acid component including a tribasic or more polybasic carboxylic acid residue. In the third step, a polycondensation reaction is carried out by evacuation.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a method for producing an aqueous polyester resin, an aqueous polyester resin, and an aqueous coating composition, and more particularly to a method for producing an aqueous polyester resin having a terephthalic acid residue derived from recycled polyester, an aqueous polyester resin, and an aqueous coating composition containing the aqueous polyester resin, and a method for producing the aqueous coating composition containing the aqueous polyester resin. [Background technology]

[0002] From an environmental consideration perspective, it has been considered to use recycled polyester as a raw material and copolymerize a hydrophilic component to produce an aqueous polyester resin dispersible in water or water containing a hydrophilic solvent (see Patent Documents 1 to 4). However, the aqueous polyester resins produced by the production methods described therein tend to have low water dispersibility, and it is difficult to maintain the dispersion of the aqueous polyester resin in liquid for a long period of time, that is, the stability of the resin dispersion also tends to be low. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Japanese Patent Application Publication No. 5-271612 [Patent Document 2] Special Publication No. 2001-505608 [Patent Document 3] Special Publication No. 2005-517050 [Patent Document 4] JP 2004-163808 A Summary of the Invention [Problem to be solved by the invention]

[0004] This tendency is considered to be due to, for example, the fact that the main component of recycled polyester is polyethylene terephthalate (PET), which is a resin with high crystallinity, and also because the molecular weight of the recycled polyester in circulation is not uniform due to differences in the type of recycled waste polyester material and the post-treatment method of the waste polyester material, etc. In other words, it is considered to be related to the rigidity of the molecular structure of the water-based polyester resin and the difference in the degree of depolymerization reaction of the recycled polyester during its production.

[0005] On the other hand, as a method for improving the water dispersibility of the water-based polyester resin and the stability of the resin dispersion, there is a method for lowering the blending ratio of recycled polyester and a method for adding a surfactant as a dispersion aid to the resin dispersion. However, from the viewpoint of environmental consideration, it is preferable that the blending ratio of recycled polyester is high. In addition, when a surfactant is used, the surfactant bleeds out onto the resin coating formed from the resin dispersion, which may reduce the physical properties of the resin coating or contaminate other materials by contact. In addition, the use of heterogeneous materials such as surfactants reduces the recyclability of materials and leads to an increase in environmental load.

[0006] Thus, there is a demand for aqueous polyester resins from recycled polyesters that have excellent water dispersibility even without surfactants and have excellent resin dispersion stability. In addition, aqueous polyester resins produced from recycled polyesters may be required to have excellent water resistance and properties equivalent to those produced from new terephthalic acid or terephthalic acid derivatives that are not derived from recycled polyesters. In particular, the characteristics of aqueous polyester resins are required to be good adhesion to resins and metals, excellent transparency such as low haze, and the like, and the dispersions of aqueous polyester resins are required to have excellent water dispersibility for a long period of time and improved stability such as stability of solution haze over time.

[0007] An object of the present disclosure is to provide a method for producing an aqueous polyester resin, which can produce an aqueous polyester resin that has excellent water resistance, excellent water dispersibility, and excellent resin dispersion stability while reducing the environmental load, and that has resin properties such as adhesion and transparency equivalent to those of terephthalic acid or a terephthalic acid derivative not derived from recycled polyester, even if it contains terephthalic acid residues derived from recycled polyester, and the resin dispersion has excellent water dispersibility over a long period of time and further improved stability, such as the stability of solution haze over time, and a method for producing an aqueous coating composition and an aqueous coating composition. [Means for solving the problem]

[0008] A method for producing an aqueous polyester resin according to one embodiment of the present disclosure is a method for producing an aqueous polyester resin using a recycled polyester. The method includes a first step, a second step, and a third step. In the first step, an ester forming reaction and a depolymerization reaction are carried out using the recycled polyester, a first polycarboxylic acid component containing a divalent polycarboxylic acid residue other than a terephthalic acid residue, and a polyhydric alcohol component. In the second step, an ester forming reaction is carried out using the reaction product of the first step and a second polycarboxylic acid component containing a trivalent or higher polycarboxylic acid residue. In the third step, a polycondensation reaction is carried out by reducing pressure. In the first step, the recycled polyester is used in an amount such that the ratio of the terephthalic acid residue to the total of the terephthalic acid residue contained in the recycled polyester and the polycarboxylic acid residues contained in the first polycarboxylic acid component and the second polycarboxylic acid component is 20% by mass or more and 72% by mass or less. The acid value of the obtained aqueous polyester resin is 30 mgKOH / g or more and 120 mgKOH / g or less.

[0009] The aqueous polyester resin according to one embodiment of the present disclosure has a terephthalic acid residue derived from a recycled polyester and a polycarboxylic acid residue other than the terephthalic acid residue. The polycarboxylic acid residue includes a first divalent polycarboxylic acid residue and a second trivalent or higher polycarboxylic acid residue. The ratio of the terephthalic acid residue to the total of the terephthalic acid residue, the first polycarboxylic acid residue, and the second polycarboxylic acid residue is 20% by mass or more and 72% by mass or less. The acid value of the aqueous polyester resin is 30 mgKOH / g or more and 120 mgKOH / g or less.

[0010] A method for producing a water-based coating composition according to one embodiment of the present disclosure includes the method for producing the water-based polyester resin and a step of neutralizing at least a portion of the carboxy groups of the water-based polyester resin with a base.

[0011] An aqueous coating composition according to one embodiment of the present disclosure is an aqueous coating composition containing an aqueous polyester resin, the aqueous polyester resin including a neutralized product of the aqueous polyester resin. Effect of the Invention

[0012] According to the present disclosure, it is possible to provide a method for producing an aqueous polyester resin, which can produce an aqueous polyester resin that has excellent water resistance, excellent water dispersibility, and excellent resin dispersion stability while reducing the environmental load, and that has resin properties such as adhesion and transparency equivalent to those of terephthalic acid or a terephthalic acid derivative that is not derived from recycled polyester, even if it contains terephthalic acid residues derived from recycled polyester, and the resin dispersion has excellent water dispersibility over a long period of time and further improved stability, such as the stability of solution haze over time, as well as a method for producing an aqueous coating composition and an aqueous coating composition. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] <Method of producing water-based polyester resin> The method for producing an aqueous polyester resin according to this embodiment (hereinafter also referred to as production method (X)) is a method for producing an aqueous polyester resin using recycled polyester. The production method (X) includes a first step, a second step, and a third step.

[0014] According to the production method (X) of this embodiment, it is possible to produce an aqueous polyester resin that has excellent water resistance, excellent water dispersibility, and excellent resin dispersion stability while reducing the environmental load, and has resin properties such as adhesion and transparency equivalent to those of terephthalic acid or a terephthalic acid derivative not derived from recycled polyester even if it has a terephthalic acid residue derived from recycled polyester, and the resin dispersion has excellent long-term water dispersibility and can further improve stability such as stability over time of solution haze. The inventors have found that the above problem can be solved by using a trivalent or higher polycarboxylic acid compound in addition to a divalent polycarboxylic acid compound as a hydrophilic component when producing an aqueous polyester resin using recycled polyester, setting the ratio of the recycled polyester used within a specific range, setting the acid value of the aqueous polyester resin within a specific range, and blending the trivalent or higher polycarboxylic acid compound at a specific time during production.

[0015] The reason for this can be presumed to be, for example, as follows. By setting the proportion of recycled polyester to a certain value or more, the amount of raw materials derived from fossil fuels can be reduced, waste can be reduced, and the environmental load can be reduced by using water or water containing a hydrophilic organic solvent to prepare the resin dispersion of the obtained aqueous polyester resin, and there is no need to use a surfactant or the like. In addition, by setting the proportion of recycled polyester to a specific range and using a trivalent or higher polycarboxylic acid compound to set the acid value of the aqueous polyester resin to a specific range, the balance between the ratio of hydrophobic parts and hydrophilic parts of the aqueous polyester resin can be made appropriate, and the aqueous polyester resin has excellent water dispersibility even without a surfactant or the like, and the stability of the resin dispersion can be improved and water resistance can be improved. Furthermore, in the production method (X), after the first step using a divalent polycarboxylic acid compound, the second step using a trivalent or higher polycarboxylic acid compound can suppress the generation of a crosslinked structure in the obtained aqueous polyester resin and set the acid value to a specific range. Another reason is that the depolymerization reaction can be appropriately carried out for recycled polyesters of various molecular weights by reacting the recycled polyester with a divalent polycarboxylic acid compound in the first step. For the same reason that the above-mentioned water-based polyester resin has excellent water dispersibility and resin dispersion stability, it is considered that the same properties can be obtained in terms of resin physical properties such as adhesion and transparency, and stability such as long-term water dispersibility and time-dependent stability of solution haze, regardless of whether the terephthalic acid residue is derived from recycled polyester or formed from new terephthalic acid or a terephthalic acid derivative.

[0016] The aqueous polyester resin (hereinafter also referred to as resin (Y)) obtained by production method (X) is a polyester resin, and has a structural unit consisting of a polycarboxylic acid residue and a structural unit consisting of a polyhydric alcohol residue. The polycarboxylic acid residue contained in resin (Y) or the polycarboxylic acid component is usually represented by the following formula (1). The polyhydric alcohol residue contained in resin (Y) or the polyhydric alcohol component is usually represented by the following formula (2). Resin (Y) has a terephthalic acid residue derived from recycled polyester as a structural unit consisting of a polycarboxylic acid residue.

[0017] [ka]

[0018] In formula (1), R 1 is a substituted or unsubstituted hydrocarbon group having 1 to 50 carbon atoms. In formula (2), R 2 is a substituted or unsubstituted hydrocarbon group having 1 to 50 carbon atoms. In formulas (1) and (2), * indicates a group adjacent to the residue represented by formula (1) or (2) or a bonding site to the adjacent residue.

[0019] R 1 and R 2 Examples of the substituent on the hydrocarbon group in the formula include hydroxy groups such as alcoholic hydroxy groups and phenolic hydroxy groups, carboxy groups, acyl groups, acyloxy groups, halogen atoms, alkoxy groups, and alkoxycarbonyl groups.

[0020] Examples of compounds that provide polycarboxylic acid residues include a first polycarboxylic acid component and a second polycarboxylic acid component. The "first polycarboxylic acid component" refers to a compound containing a divalent polycarboxylic acid residue other than a terephthalic acid residue, and examples thereof include at least one selected from a divalent polycarboxylic acid other than terephthalic acid, its esters, and its anhydrides. The "second polycarboxylic acid component" refers to a compound containing a trivalent or higher polycarboxylic acid residue, and examples thereof include at least one selected from a trivalent or higher polycarboxylic acid, its esters, and its anhydrides. The trivalent or higher polycarboxylic acid residue provided by the second polycarboxylic acid component is usually represented by R in formula (1). 1 The hydrocarbon group has one or more carboxy groups or the like as a substituent.

[0021] Examples of compounds that give polyhydric alcohol residues include dihydric polyhydric alcohol compounds and trihydric or higher polyhydric alcohol compounds. The trihydric or higher polyhydric alcohol residues given by trihydric or higher polyhydric alcohol compounds are usually represented by the formula (2): R 2 The hydrocarbon group has one or more alcoholic hydroxy groups or the like as a substituent. Each step will be described below.

[0022] [1st step] In the first step, an ester forming reaction and a depolymerization reaction are carried out using the recycled polyester, a first polyvalent carboxylic acid component, and a polyhydric alcohol component.

[0023] The ester forming reaction refers to a reaction in which a polyvalent carboxylic acid component and a polyhydric alcohol component form an ester compound by dehydration condensation or dealcoholization condensation or the like. The depolymerization reaction refers to a reaction in which a polyester having a lower molecular weight is formed by the recycled polyester and a polyvalent carboxylic acid component, a polyhydric alcohol component, or an ester compound formed therefrom.

[0024] In the first step, all of the reactant components used in the first step may be mixed at once, or one or more components that are part of the reactant components or a certain amount of components may be mixed successively. Also, a part of the reactant components may be mixed and reacted, and then another part of the reactant components may be mixed and reacted. These mixing and reactions may be repeated.

[0025] In the first step, the recycled polyester, the first polycarboxylic acid component, and the polyhydric alcohol component may be blended together, and then an ester formation reaction and a depolymerization reaction may be carried out. Alternatively, the first polycarboxylic acid component and the polyhydric alcohol component may be blended together, and then an ester formation reaction may be carried out, and then the recycled polyester may be blended together, and then a depolymerization reaction may be carried out. The reactant materials are usually blended into an apparatus for carrying out the production process (X), such as a reactor.

[0026] Each of the reaction raw materials used in the first step will be described below. (Recycled polyester) The recycled polyester contains polyethylene terephthalate as a main component. The main component refers to the component with the largest content. The proportion of polyethylene terephthalate in the recycled polyester is preferably 90% by mass or more, more preferably 95% by mass or more, and even more preferably 99% by mass or more. In this case, mono-materialization of the aqueous polyester resin can be promoted. The proportion may be 100% by mass.

[0027] Examples of recycled polyester include material recycled polyester, mechanically recycled polyester, and chemically recycled polyester. Material recycled polyester refers to polyester obtained by removing contaminants and foreign matter from used or discarded polyester molded products such as bottles, containers, and films through sorting, crushing, washing, etc., and then flaking them. Mechanically recycled polyester refers to polyester obtained by treating flakes of material recycled polyester at high temperature and reduced pressure for a certain period of time to remove contaminants from inside the resin and by repolymerizing part of the polyester to adjust the degree of polymerization. What is chemically recycled polyester? It refers to a polyester obtained by breaking down a polyester to the monomer level and then repolymerizing the monomer.

[0028] The intrinsic viscosity (IV value, unit: dl / g) of the recycled polyester is preferably 0.40 to 1.20, more preferably 0.45 to 1.00, from the viewpoint of more appropriately carrying out the depolymerization reaction in the first step. The intrinsic viscosity is generally used as an index of the polymerization degree of a polymer.

[0029] From the viewpoint of further reducing the environmental load, the recycled polyester preferably contains at least one of material recycled polyester and mechanically recycled polyester, and from the viewpoint of improving the quality of the aqueous polyester resin, it is more preferable that the recycled polyester contains mechanically recycled polyester, and it is even more preferable that the recycled polyester contains mechanically recycled polyester obtained by recovering PET bottles, PET films, or polyester fibers (PET fibers).

[0030] (First polycarboxylic acid component) The first polybasic carboxylic acid component contains at least one selected from, for example, dibasic polybasic carboxylic acids other than terephthalic acid containing a dibasic polybasic carboxylic acid residue other than a terephthalic acid residue, and esters and anhydrides thereof.

[0031] Examples of the first polyvalent carboxylic acid component include Examples of the dicarboxylic acids include aromatic dicarboxylic acids such as phthalic acid, isophthalic acid, 2,6-naphthalenedicarboxylic acid, 2,7-naphthalenedicarboxylic acid, 1,4-naphthalenedicarboxylic acid, and 2,5-furandicarboxylic acid; alicyclic dicarboxylic acids such as 1,4-cyclohexanedicarboxylic acid; and aliphatic dicarboxylic acids such as succinic acid, adipic acid, sebacic acid, and dodecanedioic acid, as well as their esters and anhydrides.

[0032] From the viewpoint of reducing the environmental load, it is also preferable to use a first polycarboxylic acid component derived from biomass. Examples of the first polycarboxylic acid component derived from biomass include 2,5-furandicarboxylic acid, succinic acid, adipic acid, and sebacic acid.

[0033] From the viewpoint of more appropriately lowering the crystallinity of the aqueous polyester resin and thereby further enhancing the water dispersibility of the resin (Y) and the stability of the resin dispersion, the first polyvalent carboxylic acid component preferably contains at least one selected from aromatic dicarboxylic acids, their esters and anhydrides, and more preferably contains at least one selected from isophthalic acid and 2,6-naphthalenedicarboxylic acid.

[0034] It is preferable that the first polycarboxylic acid component does not contain a polycarboxylic acid compound having a metal sulfonate group, such as a polycarboxylic acid having a metal sulfonate group, its ester, or its anhydride. If a polycarboxylic acid having a metal sulfonate group is used, the water resistance of the resin (Y) may decrease. The metal sulfonate group refers to a metal base of a sulfo group (-SO3H), for example, -SO3 - (M n+ ) 1 / n (M n+ is an n-valent metal cation, where n is an integer of 1 to 6.) Examples of the metal cation include alkali metal ions such as sodium ion and potassium ion. Examples of polyvalent carboxylic acid compounds containing a metal sulfonate group include sodium 5-sulfoisophthalate and sodium dimethyl 5-sulfoisophthalate.

[0035] (Polyhydric alcohol component) Resin (Y) usually has, as a polyhydric alcohol residue, an ethylene glycol residue derived from recycled polyester.

[0036] Examples of the polyhydric alcohol component include dihydric alcohol compounds and trihydric or higher alcohol compounds.

[0037] Examples of dihydric alcohol compounds include Examples of the diols include aliphatic diols such as ethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,3-butanediol, 1,4-butanediol, neopentyl glycol, and 1,6-hexanediol; alicyclic diols such as 1,4-cyclohexanedimethanol; aromatic diols such as 1,4-benzenedimethanol and 9,9-bis[4-(2-hydroxyethoxy)phenyl]fluorene; and ether group-containing diols such as diethylene glycol, polyethylene glycol, dipropylene glycol, polypropylene glycol, and polytetramethylene ether glycol.

[0038] The dihydric alcohol compound preferably contains a dihydric alcohol compound having a branched chain. In this case, the resin dispersion of the resin (Y) can further improve stability such as stability over time of solution haze.

[0039] An example of the branched dihydric alcohol compound is a compound represented by the following formula (3).

[0040] [ka]

[0041] In formula (3), R 3 is a branched divalent hydrocarbon group having 3 to 50 carbon atoms.

[0042] R 3Examples of the branched divalent hydrocarbon group represented by the formula (I) include a propane-1,2-diyl group, a butane-1,2-diyl group, a butane-1,3-diyl group, a 2-methylpropane-1,3-diyl group, a pentane-1,2-diyl group, a pentane-1,2-diyl group, a pentane-1,3-diyl group, a pentane-1,4-diyl group, a 2,2-dimethylpropane-1,3 -diyl group, 2-methylbutane-1,4-diyl group, hexane-1,2-diyl group, hexane-2,5-diyl group, 2,4-diethylpentane-1,5-diyl group, and the like.

[0043] Examples of the dihydric alcohol compound having a branched chain include neopentyl glycol, 1,2-propanediol, 1,2-butanediol, 1,3-butanediol, 1,2-pentanediol, 1,2-hexanediol, 2,5-hexanediol, 2,4-diethyl-1,5-pentanediol, etc. Among these, neopentyl glycol, 1,2-propanediol and 1,3-butanediol are preferred.

[0044] Examples of trihydric or higher alcohol compounds include Examples of the triol include aliphatic triols such as glycerin and trimethylolpropane; alicyclic triols such as 1,2,4-cyclohexanetrimethanol; aromatic triols such as benzenetrimethanol; and tetraol compounds such as pentaerythritol.

[0045] It is preferable that the polyhydric alcohol component does not contain a trihydric or higher polyhydric alcohol compound. In this case, the resin (Y) can have a reduced crosslinking structure caused by the trihydric or higher polyhydric alcohol compound, and as a result, the water dispersibility and the stability of the resin dispersion can be further improved.

[0046] From the viewpoint of reducing the environmental load, it is also preferable to use a polyhydric alcohol component derived from biomass. Examples of the polyhydric alcohol component derived from biomass include ethylene glycol, 1,3-propanediol, 1,3-butanediol, and 1,4-butanediol.

[0047] In the first step, it is important to use recycled polyester in an amount such that the ratio of terephthalic acid residues contained in the recycled polyester is 20% by mass or more and 72% by mass or less based on the total of the terephthalic acid residues contained in the recycled polyester and the polycarboxylic acid residues contained in the first polycarboxylic acid component and the second polycarboxylic acid component. If the ratio is less than 20% by mass, the reduction in environmental load is insufficient. If the ratio exceeds 72% by mass, the resin (Y) does not become less crystalline and its water dispersibility is reduced. The ratio is preferably 30% by mass or more, more preferably 40% by mass or more, even more preferably 45% by mass or more, and particularly preferably 50% by mass or more. The ratio is preferably 71% by mass or less, more preferably 70% by mass or less, even more preferably 69% by mass or less, and particularly preferably 68% by mass or less.

[0048] In the first step, it is preferable to use the first polycarboxylic acid component in an amount such that the ratio of the divalent polycarboxylic acid residue is 5% by mass or more and 50% by mass or less with respect to the total of the terephthalic acid residue contained in the recycled polyester and the polycarboxylic acid residue contained in the first polycarboxylic acid component and the second polycarboxylic acid component. By setting the ratio within the above range, the crystallinity of the resin (Y) can be more appropriately reduced, and the water dispersibility and the stability of the resin dispersion can be further improved. The ratio is more preferably 10% by mass or more, even more preferably 14% by mass or more, and particularly preferably 18% by mass or more. The ratio is more preferably 40% by mass or less, even more preferably 30% by mass or less, and particularly preferably 26% by mass or less.

[0049] When the polyhydric alcohol component contains a dihydric alcohol compound having a branched chain, it is preferable to use a dihydric alcohol compound having a branched chain in an amount such that the ratio of the residue of the dihydric alcohol compound having a branched chain is 10% by mass or more and 90% by mass or less with respect to the total polyhydric alcohol residues contained in the resin (Y). In this case, the resin dispersion of the resin (Y) can further improve the stability such as the stability over time of the solution haze. The ratio is preferably 15% by mass or more and 85% by mass or less, more preferably 20% by mass or more and 80% by mass or less, and even more preferably 25% by mass or more and 75% by mass or less.

[0050] When the polyhydric alcohol component contains other polyhydric alcohol compounds than ethylene glycol, the ratio of ethylene glycol is preferably 20% by mass or more based on the entire polyhydric alcohol component. In this case, the depolymerization reaction of the recycled polyester can be more easily caused. The ratio is more preferably 25% by mass or more, even more preferably 30% by mass or more, and particularly preferably 35% by mass or more. The ratio may be 100% by mass. That is, from the viewpoint of more easily causing the depolymerization reaction of the recycled polyester, the ratio of the other polyhydric alcohol compounds is preferably 80% by mass or less, more preferably 75% by mass or less, even more preferably 70% by mass or less, and particularly preferably 65% ​​by mass or less based on the entire polyhydric alcohol component. The ratio may be 0% by mass.

[0051] In the first step, in addition to the recycled polyester, the first polycarboxylic acid component, and the polyhydric alcohol component, at least one selected from terephthalic acid, its esters, and its anhydrides, and at least one selected from hydroxycarboxylic acids, their esters, and its anhydrides may be used as long as the effects of the present disclosure are not impaired; however, it is preferable not to use such substances.

[0052] The reaction in the first step can be advanced by, for example, heating the mixed reaction raw materials.

[0053] In the first step, it is preferable to use a catalyst from the viewpoint of further promoting the reaction. Examples of the catalyst include titanium catalysts such as titanium oxalate salts such as potassium titanium oxalate and sodium titanium oxalate, titanium alkoxides such as tetra-n-propyl titanate and tetra-n-butyl titanate, fatty acid titanium salts such as titanium acetate, inorganic titanium compounds such as titanium oxide, fatty acid manganese salts such as manganese acetate, manganese catalysts such as manganese carbonate, antimony catalysts such as antimony trioxide, aluminum catalysts such as aluminum trisacetylacetate, germanium catalysts such as germanium dioxide, and lithium catalysts such as sec-butyllithium.

[0054] The amount of the catalyst used is, for example, from 0.0001% by mass to 0.1% by mass, and preferably from 0.003% by mass to 0.05% by mass, based on all the components mixed in the first step.

[0055] In the reaction in the first step, a reaction solvent may or may not be used, but it is preferable not to use a reaction solvent.

[0056] From the viewpoint of improving the quality of the resin (Y), the reaction in the first step is preferably carried out in an inert gas atmosphere such as a nitrogen atmosphere or an argon atmosphere.

[0057] The first step can be carried out in the following manner (A) or (B). (A) The recycled polyester, the first polyvalent carboxylic acid component, and the polyhydric alcohol component are blended together, and then an ester forming reaction and a depolymerization reaction are carried out. (B) The method includes a step of blending a first polyvalent carboxylic acid component and a polyhydric alcohol component, followed by carrying out an ester formation reaction, and a step of blending a recycled polyester, followed by carrying out a depolymerization reaction.

[0058] [Method (A)] In the method (A), in the first step, a recycled polyester, a first polyvalent carboxylic acid component, and a polyhydric alcohol component are mixed as reaction raw materials, and then an ester formation reaction and a depolymerization reaction are carried out in the mixed reaction raw materials (hereinafter, also referred to as the X1 step). According to the method (A), the resin (Y) can be produced more simply.

[0059] The reaction temperature in step X1 is preferably 150° C. or higher and 270° C. or lower, and more preferably 180° C. or higher and 260° C. or lower. The reaction time is preferably 1 hour or higher and 10 hours or lower, and more preferably 2 hours or higher and 8 hours or lower. From the viewpoint of further promoting the ester formation reaction and the depolymerization reaction in step X1, it is preferable that the reaction system is at normal pressure. The reaction temperature in step X1 may be changed stepwise.

[0060] [Method (B)] Method (B) includes a step of blending a polyvalent carboxylic acid component and a polyhydric alcohol component as reaction raw materials in a first step, followed by an ester formation reaction in the blended reaction raw materials (hereinafter also referred to as step X2-1), and a step of blending a recycled polyester with the reaction product of step X2-1, followed by a depolymerization reaction (hereinafter also referred to as step X2-2). According to method (B), blending and reaction are carried out separately in steps X2-1 and X2-2, so that, for example, the depolymerization reaction of the recycled polyester can be more appropriately carried out, and the water dispersibility of the resin (Y) and the stability of the resin dispersion can be further improved.

[0061] (X2-1 process) In the step X2-1, a polyvalent carboxylic acid component and a polyhydric alcohol component are mixed together, and then an ester forming reaction is carried out.

[0062] The reaction temperature in Step X2-1 is preferably 150° C. or higher and 250° C. or lower, and more preferably 180° C. or higher and 240° C. or lower. The reaction time is preferably 1 hour or higher and 8 hours or lower, and more preferably 2 hours or higher and 5 hours or lower. From the viewpoint of further promoting the ester formation reaction in Step X2-1, the reaction system is preferably at normal pressure. The reaction temperature in Step X2-1 may be changed stepwise.

[0063] (X2-2 process) In the X2-2 step, recycled polyester is further blended and then a depolymerization reaction is carried out.

[0064] The reaction temperature in step X2-2 is preferably 200° C. or higher and 270° C. or lower, and more preferably 210° C. or higher and 260° C. or lower. The reaction time is preferably 1 hour or higher and 8 hours or lower, and more preferably 2 hours or higher and 7 hours or lower. From the viewpoint of further promoting the depolymerization reaction in step X2-2, it is preferable that the reaction system is at normal pressure. The reaction temperature in step X2-2 may be changed stepwise.

[0065] [Second process] In the second step, an ester forming reaction is carried out using the reaction product of the first step and a second polycarboxylic acid component.

[0066] (Second polycarboxylic acid component) The second polyvalent carboxylic acid component includes at least one selected from, for example, a trivalent or higher polyvalent carboxylic acid containing a trivalent or higher polyvalent carboxylic acid residue, and an ester and an anhydride thereof.

[0067] Examples of the second polycarboxylic acid component include Examples of the tricarboxylic acids include aromatic tricarboxylic acids such as trimellitic acid, hemimellitic acid, trimesic acid, and 1,2,5-naphthalenetricarboxylic acid; alicyclic tricarboxylic acids such as 1,2,4-cyclohexanetricarboxylic acid; aliphatic tricarboxylic acids such as 1,2,3-butanetricarboxylic acid; and polyvalent carboxylic acids with 4 or more valences such as pyromellitic acid, their esters, and their anhydrides.

[0068] In the second step, it is preferable to use the second polycarboxylic acid component in an amount such that the ratio of trivalent or higher polycarboxylic acid residues to the total of the terephthalic acid residues contained in the recycled polyester and the polycarboxylic acid residues contained in the first polycarboxylic acid component and the second polycarboxylic acid component is 10% by mass or more and 30% by mass or less. In this case, the acid value of the resin (Y) can be made more appropriate, and as a result, the water resistance of the resin (Y) can be further improved, and the stability such as the long-term water dispersibility and the stability of the solution haze over time of the resin (Y) dispersion can be further improved. The ratio is more preferably 13% by mass or more, even more preferably 15% by mass or more, and particularly preferably 17% by mass or more. The ratio is more preferably 27% by mass or less, even more preferably 25% by mass or less, and particularly preferably 23% by mass or less.

[0069] The second polycarboxylic acid component preferably does not contain a polycarboxylic acid compound having a metal sulfonate group, such as a polycarboxylic acid having a metal sulfonate group, an ester thereof, or an anhydride thereof.

[0070] From the viewpoint of reducing the environmental load, it is preferable that the ratio of the recycled polyester to the total amount of raw materials used to produce the aqueous polyester resin is large. Specifically, it is preferable to use an amount of recycled polyester used in the production of resin (Y) such that the ratio of the recycled polyester is 20% by mass or more and 72% by mass or less relative to the total of the recycled polyester, the polyvalent carboxylic acid component, and the polyhydric alcohol component. The ratio is more preferably 30% by mass or more, and even more preferably 40% by mass or more. The ratio is more preferably 65% ​​by mass or less, and even more preferably 62% by mass or less.

[0071] From the viewpoint of reducing the environmental load, it is preferable that the ratio of the polyhydric alcohol component to the total amount of raw materials used to produce the resin (Y) is small. In detail, it is preferable to use a polyhydric alcohol component whose ratio is 10% by mass or more and 40% by mass or less to the total of the recycled polyester, the polycarboxylic acid component, and the polyhydric alcohol component. The ratio is more preferably 35% by mass or less, and even more preferably 30% by mass or less. The ratio is more preferably 13% by mass or more, and even more preferably 15% by mass or more.

[0072] The polyhydric alcohol component used to produce the resin (Y) is preferably used in an amount larger than the polybasic carboxylic acid component on a molar basis. In this case, the depolymerization reaction of the recycled polyester can be more easily caused. Specifically, the molar ratio of the polyhydric alcohol component to the polybasic carboxylic acid component (polyhydric alcohol component / polybasic carboxylic acid component) is preferably 1.1 / 1 or more and 5 / 1 or less, more preferably 1.3 / 1 or more and 4.0 / 1 or less, even more preferably 1.5 / 1 or more and 3.5 / 1 or less, and particularly preferably 1.7 / 1 or more and 3.0 / 1 or less.

[0073] After the reaction in the first step, the second step may be carried out by adding a second polyvalent carboxylic acid component directly to the reaction system, or the reaction product in the first step may be isolated and, if necessary, a catalyst, a solvent, etc. may be added to carry out the second step.

[0074] In order to further promote the reaction, it is preferable to use a catalyst in the second step. By using the reaction product of the first step as it is, the catalyst contained in the reaction product can be used.

[0075] The reaction temperature in the second step is preferably 150° C. or more and 270° C. or less, more preferably 160° C. or more and 240° C. or less. The reaction time is preferably 10 minutes or more and 3 hours or less, more preferably 20 minutes or more and 2 hours or less. From the viewpoint of further promoting the ester formation reaction in the second step, it is preferable that the reaction system is at normal pressure. The reaction temperature in the second step may be changed stepwise.

[0076] [3rd step] In the third step, the polycondensation reaction is carried out by reducing the pressure in the reaction system to remove the polyhydric alcohol and the like produced by the reaction, thereby accelerating the polycondensation reaction.

[0077] The polycondensation reaction refers to a reaction in which a polyester having a higher molecular weight is formed by carrying out a dealcoholization condensation reaction or the like between the ester compound formed in the first and second steps and a polyester.

[0078] The reaction in the third step can be carried out in the reaction product of the second step by reducing the pressure of the reaction system and, for example, heating it.

[0079] After the reaction in the second step has been carried out, the reaction system may be directly depressurized and the temperature may be adjusted to carry out the third step, or the reaction product in the second step may be isolated, and a catalyst, a solvent, etc. may be added as necessary, and then the reaction system may be depressurized and heated, etc. to carry out the third step.

[0080] The degree of reduced pressure (absolute pressure) in the third step is preferably 25 hPa or less, more preferably 10 hPa or less. The reaction temperature in the third step is preferably 150°C or more and 270°C or less, more preferably 160°C or more and 240°C or less. The degree of reduced pressure and the reaction temperature in the third step may be changed stepwise. The weight average molecular weight, acid value, etc. of the resin (Y) can be adjusted by adjusting the degree of reduced pressure, temperature, and time in the third step.

[0081] By carrying out the above-mentioned production method (X), a water-based polyester resin (resin (Y)) is obtained.

[0082] (Acid value) It is important that the acid value of the resulting resin (Y) is 30 mgKOH / g or more and 120 mgKOH / g or less. When the acid value of the resin (Y) is 30 mgKOH / g or more, the resin (Y) can have excellent water dispersibility. When the acid value is 120 mgKOH / g or less, the resin (Y) can have excellent water resistance. When the acid value is less than 30 mgKOH / g, the water dispersibility is insufficient. When the acid value is more than 120 mgKOH / g, the water resistance decreases. The acid value is preferably 33 mgKOH / g or more, more preferably 35 mgKOH / g or more, and even more preferably 40 mgKOH / g or more. The acid value is preferably 110 mgKOH / g or less, more preferably 100 mgKOH / g or less, and even more preferably 90 mgKOH / g or less. The "acid value" of the resin (Y) refers to the mass (mg) of potassium hydroxide required to neutralize 1 g of the resin (Y). The acid value of the resin (Y) is a value attributable to a carboxy group or the like present on the side chain or terminal of the molecule of the resin (Y).

[0083] (glass transition temperature) The glass transition temperature (Tg) of the obtained resin (Y) is preferably 0°C or higher and 100°C or lower. When Tg is 0°C or higher, the resin (Y) is less likely to develop excessive adhesion, and therefore the handleability is improved, and the occurrence of tack can be further suppressed. When Tg is 100°C or lower, the resin (Y) has better film-forming properties, and the adhesion to the substrate and primer properties are further improved. Tg is more preferably 10°C or higher, and even more preferably 20°C or higher. Tg is more preferably 90°C or lower, and even more preferably 85°C or lower.

[0084] The weight average molecular weight of the resulting resin (Y) is preferably 2,000 or more and 100,000 or less, more preferably 3,000 or more and 50,000 or less, and even more preferably 4,000 or more and 30,000 or less.

[0085] <Water-based polyester resin> The resin (Y) according to the present embodiment has a terephthalic acid residue (hereinafter also referred to as residue (I)) derived from a recycled polyester, and a polycarboxylic acid residue other than the terephthalic acid residue (hereinafter also referred to as residue (II)). The residue (II) includes a first divalent polycarboxylic acid residue (hereinafter also referred to as residue (IIa)) and a second trivalent or higher polycarboxylic acid residue (hereinafter also referred to as residue (IIb)). The ratio of the residue (I) to the total of the residue (I), the residue (IIa), and the residue (IIb) is 20% by mass or more and 72% by mass or less. The acid value of the resin (Y) is 30 mgKOH / g or more and 120 mgKOH / g or less.

[0086] Resin (Y) has excellent water resistance and water dispersibility while reducing the environmental impact, and the stability of the resin dispersion is also excellent. Furthermore, even though it contains terephthalic acid residues derived from recycled polyester, it has resin properties such as adhesion and transparency that are equivalent to those of terephthalic acid or terephthalic acid derivatives that are not derived from recycled polyester. The resin dispersion has excellent long-term water dispersibility and can further improve stability, such as the stability over time of solution haze.

[0087] The resin (Y) has a polycarboxylic acid residue and a polyhydric alcohol residue. (polycarboxylic acid residue) The resin (Y) has, as the polybasic carboxylic acid residue, the residue (I) and the residue (II).

[0088] (Residue (I)) Residue (I) is a terephthalic acid residue derived from recycled polyester. "Terephthalic acid residue derived from recycled polyester" means that the terephthalic acid residue contained in recycled polyester has become the terephthalic acid residue contained in resin (Y). The terephthalic acid residue refers to a residue represented by the following formula (4).

[0089] [ka]

[0090] In formula (4), * indicates a group adjacent to the residue represented by formula (4) or a bonding site with the adjacent residue.

[0091] It is important that the ratio of residue (I) to the total of residue (I), residue (IIa) and residue (IIb) in resin (Y) is 20% by mass or more and 72% by mass or less. The ratio is preferably 30% by mass or more, more preferably 40% by mass or more, even more preferably 45% by mass or more, and particularly preferably 50% by mass or more. The ratio is preferably 71% by mass or less, more preferably 70% by mass or less, even more preferably 69% by mass or less, and particularly preferably 68% by mass or less.

[0092] (residue (II)) Residue (II) includes residues (IIa) and (IIb).

[0093] (Residue (IIa) The residue (IIa) is a divalent polycarboxylic acid residue other than a terephthalic acid residue, and is also referred to as a first polycarboxylic acid residue.

[0094] The ratio of residue (IIa) to the total of residue (I), residue (IIa) and residue (IIb) in resin (Y) is preferably 5% by mass or more and 50% by mass or less. The ratio is more preferably 10% by mass or more, even more preferably 14% by mass or more, and particularly preferably 18% by mass or more. The ratio is more preferably 40% by mass or less, even more preferably 30% by mass or less, and particularly preferably 26% by mass or less.

[0095] (residue (IIb)) The residue (IIb) is a trivalent or higher polyvalent carboxylic acid residue, and is also referred to as a second polyvalent carboxylic acid residue.

[0096] The ratio of residue (IIb) to the total of residue (I), residue (IIa) and residue (IIb) in resin (Y) is preferably 10% by mass or more and 30% by mass or less. The ratio is more preferably 13% by mass or more, even more preferably 15% by mass or more, and particularly preferably 17% by mass or more. The ratio is more preferably 27% by mass or less, even more preferably 25% by mass or less, and particularly preferably 23% by mass or less.

[0097] (polyhydric alcohol residue) The polyhydric alcohol residue is a residue contained in a polyhydric alcohol compound having a plurality of alcoholic hydroxy groups. The resin (Y) usually has an ethylene glycol residue derived from recycled polyester as the polyhydric alcohol residue.

[0098] The polyhydric alcohol residue preferably does not contain a residue of a trivalent or higher polyhydric alcohol compound. That is, the polyhydric alcohol residue preferably contains only a residue of a divalent polyhydric alcohol compound. In this case, by having a suitable crosslinked structure, the water dispersibility of the resin (Y) and the stability and film-forming property of the resin dispersion can be further improved.

[0099] When the polyhydric alcohol residue contains a residue of a dihydric alcohol compound, the residue of the dihydric alcohol compound preferably has a branched chain. In this case, the resin dispersion of the resin (Y) can further improve stability such as stability over time of solution haze.

[0100] When the polyhydric alcohol residue contains a residue of a dihydric alcohol compound having a branched chain, the ratio of the residue of the dihydric alcohol compound having a branched chain to the total polyhydric alcohol residues contained in the resin (Y) is preferably 10% by mass or more and 90% by mass or less. In this case, the resin dispersion of the resin (Y) can further improve stability such as stability over time of solution haze. The ratio is preferably 15% by mass or more and 85% by mass or less, more preferably 20% by mass or more and 80% by mass or less, and even more preferably 25% by mass or more and 75% by mass or less.

[0101] <Method of producing water-based coating composition> The water-based coating composition (hereinafter also referred to as composition (Z)) is a composition containing the above-mentioned water-based polyester resin (resin (Y)). In the composition (Z), it is preferable that the resin (Y) is uniformly dispersed. The resin (Y) can be more uniformly dispersed by neutralizing the carboxyl group with a base.

[0102] The method for producing the aqueous coating composition of this embodiment (hereinafter also referred to as production method (V)) comprises the above-mentioned production method (X) (steps 1 to 3) and a step (hereinafter also referred to as step 4) of neutralizing at least a part of the carboxy groups of the aqueous polyester resin with a base. According to the production method (V), it is possible to obtain a composition (V) in which the resin (Y) is more uniformly dispersed.

[0103] Examples of the base used in the fourth step include ammonia, organic bases such as amines such as trimethylamine, diethylamine, triethylamine, etc., and inorganic bases such as sodium hydroxide, sodium carbonate, etc. Among these, from the viewpoint that when a coating film is formed from the applied composition (Z), the base is removed by heating and the carboxyl group is regenerated, and a coating film having better water resistance can be formed, the base is preferably ammonia or an organic base, and more preferably ammonia, trimethylamine, diethylamine, and triethylamine.

[0104] The amount of base used for neutralization is not particularly limited as long as it can neutralize at least a part of the carboxy groups of the resin (Y), but it is preferable to use an amount that can neutralize 50 mol% to 100 mol% of the carboxy groups of the resin (Y), and more preferably to use an amount that can neutralize 70 mol% to 100 mol% of the carboxy groups. By setting the amount of base used within the above range, it is possible to obtain a composition (Z) in which the resin (Y) is more uniformly dispersed.

[0105] In the fourth step, for example, water or water containing a hydrophilic organic solvent may be added. In this case, for example, the viscosity of the composition (Z) can be appropriately adjusted to further improve the coatability of the composition (Z). When the composition (Z) contains water or water containing a hydrophilic organic solvent, the composition (Z) is a resin dispersion of the resin (Y). This resin dispersion of the resin (Y) has excellent stability and can maintain the dispersion of the resin for a long period of time.

[0106] Examples of hydrophilic organic solvents include alcohols such as methanol, ethanol, 2-propanol, and 1,2-propanediol; glycol ethers such as propylene glycol monomethyl ether, ethyl cellosolve, and n-butyl cellosolve; and ketones such as acetone and methyl ethyl ketone.

[0107] In the fourth step, a crosslinking agent may be added. In this case, when forming a coating film from the applied composition (Z), the carboxyl group of the resin (Y) reacts with the crosslinking agent by heating, forming a crosslinked structure, thereby forming a coating film with excellent water resistance. In addition, it is possible to further improve the water resistance of the resin (Y) having a large acid value. Examples of the crosslinking agent include compounds having two or more functional groups that react with a carboxyl group, such as melamine-based crosslinking agents, isocyanate-based crosslinking agents, epoxy-based crosslinking agents, oxazoline-based crosslinking agents, and carbodiimide-based crosslinking agents.

[0108] In the fourth step, appropriate additives such as water-based resins other than the resin (Y), leveling agents, antioxidants, UV absorbers, antifoaming agents, crosslinking agents, inorganic particles, etc. may be added.

[0109] The composition (Z) can be easily applied by, for example, a bar coating method, a dip coating method, a spray coating method, a spin coating method or the like.

[0110] The resin film (hereinafter also referred to as resin film (W)) formed from the aqueous coating composition (Z) obtained by the production method (V) has excellent water resistance and excellent adhesion to resins having a polar structure such as PET films and metals such as aluminum vapor deposition layers. In addition, the resin film (W) can suppress haze to a low level and has excellent transparency. Furthermore, the resin film (W) also has excellent primer properties.

[0111] <Water-based coating composition> The aqueous coating composition (composition (Z)) of the present embodiment contains an aqueous polyester resin, and the aqueous polyester resin contains a neutralized product of the above-mentioned resin (Y). The "neutralized product of the aqueous polyester resin" refers to an aqueous polyester resin in which a part or all of the carboxyl groups of the aqueous polyester resin have been neutralized with a base.

[0112] The composition (Z) may contain, for example, water or water containing a hydrophilic organic solvent. In this case, for example, by appropriately adjusting the viscosity of the composition (Z), the applicability of the composition (Z) can be further improved. When the composition (Z) contains water or water containing a hydrophilic organic solvent, the composition (Z) is a resin dispersion of the resin (Y). This resin dispersion of the resin (Y) has excellent stability and can maintain the dispersion of the resin for a long time.

[0113] The resin coating (W) formed from the composition (Z) has excellent adhesion to resins having a polar structure, such as PET films, and metals, such as aluminum vapor deposition layers. The resin coating (W) also has excellent transparency, being able to keep haze low. Furthermore, the resin coating (W) also has excellent primer properties.

[0114] The composition (Z) may contain appropriate additives such as an aqueous resin other than the resin (Y), a leveling agent, an antioxidant, an ultraviolet absorber, an antifoaming agent, a crosslinking agent, inorganic particles, and the like. EXAMPLES

[0115] Hereinafter, the present disclosure will be specifically described with reference to examples, but the present disclosure is not limited to only the examples.

[0116] <Production of Water-Based Polyester Resin> Water-based polyester resins were produced according to the following procedure using the raw materials shown in Table 1. Details of the recycled polyester used in the production are as follows. Recycled polyester A: Material made from recycled PET bottles. Intrinsic viscosity (IV value): 0.88 dl / g Recycled polyester B: Material made from recycled PET bottles. Intrinsic viscosity (IV value): 0.67 dl / g Recycled polyester C: Material recycled polyester made from recycled polyester fiber (PET fiber) waste materials, intrinsic viscosity (IV value): 0.59 dl / g Recycled polyester D: Material made from recycled PET film waste, Intrinsic viscosity (IV value): 0.50 dl / g The intrinsic viscosity (IV value) of the recycled polyester was determined from the results of measurement using an Ubbelohde viscometer. The "intrinsic viscosity" referred to here refers to the intrinsic viscosity measured in accordance with JIS K 7390-1:2015).

[0117] (1) Production by Method (A) (Examples 1, 3, 5, 7 to 9 and Comparative Examples 1 to 3) (1st step) (X1 process) A 1000 mL capacity reaction vessel equipped with a stirrer, nitrogen gas inlet, thermometer, rectification column and cooling condenser was prepared. The recycled polyester, the first polyvalent carboxylic acid component, the polyhydric alcohol component and the catalyst potassium titanium oxalate were placed in the reaction vessel, as shown in Table 1, to obtain a mixture. The mixture was heated to 200°C under normal pressure in a nitrogen atmosphere while being stirred and mixed, and then gradually heated to 250°C over 7 hours, to carry out an ester formation reaction and a depolymerization reaction.

[0118] (2nd process) The temperature of the reaction product of step X1 was stabilized at 200° C. under normal pressure in a nitrogen atmosphere. The second polyvalent carboxylic acid component shown in Table 1 was then added thereto, and the mixture was stirred and mixed for 40 minutes under normal pressure in a nitrogen atmosphere while maintaining the temperature at 200 to 210° C., thereby carrying out an ester formation reaction.

[0119] (3rd step) After the second step, the pressure was gradually reduced to 0.67 hPa (0.5 mmHg) while stirring and mixing at a temperature of 200 to 210° C., and the mixture was maintained in that state for 1 hour to carry out a polycondensation reaction. As a result, a water-based polyester resin was obtained.

[0120] (2) Production by Method (B) (Examples 2, 4, and 6) (1st step) (X2-1 process) A 1000 mL capacity reaction vessel equipped with a stirrer, nitrogen gas inlet, thermometer, rectification column and cooling condenser was prepared. The first polyvalent carboxylic acid component and polyhydric alcohol component shown in Table 1, and titanium potassium oxalate as a catalyst were placed in the reaction vessel to obtain a mixture. The mixture was heated to 200° C. under normal pressure in a nitrogen atmosphere while being stirred and mixed, and then gradually heated to 240° C. over 3 hours to carry out an ester formation reaction.

[0121] (X2-2 process) After completion of the X2-1 step, the recycled polyester shown in Table 1 was placed in a reaction vessel, and the mixture was heated to 250° C. under normal pressure in a nitrogen atmosphere while being stirred and mixed, and was maintained in that state for 5 hours to carry out a depolymerization reaction.

[0122] (2nd process) The temperature of the reaction product of step X2-2 was stabilized at 200° C. under normal pressure in a nitrogen atmosphere. The second polyvalent carboxylic acid component shown in Table 1 was then added thereto, and the mixture was stirred and mixed for 40 minutes under normal pressure in a nitrogen atmosphere while maintaining the temperature at 200 to 210° C., thereby carrying out an ester formation reaction.

[0123] (3rd step) After the second step, the pressure was gradually reduced to 0.67 hPa (0.5 mmHg) while stirring and mixing at a temperature of 200 to 210° C., and the mixture was maintained in that state for 1 hour to carry out a polycondensation reaction. As a result, a water-based polyester resin was obtained.

[0124] (3) Reference examples (Reference examples 1 to 3) The aqueous polyester resins of Examples 3 and 7 and Comparative Example 2 were produced as described above using new dimethyl terephthalate, a terephthalic acid derivative, without using recycled polyester, to obtain the aqueous polyester resins of Reference Examples 1 to 3.

[0125] <Preparation of Water-Based Coating Composition> (1) Examples 1, 2, 7 and 8 A 1000mL reaction vessel equipped with a stirrer, a thermometer and a cooling condenser was prepared. 100 parts by mass of the water-based polyester resin obtained above, 288 parts by mass of water, and 12 parts by mass of a 25% by mass aqueous ammonia solution as a neutralizing base were placed in the reaction vessel, and the temperature was raised to 85°C while stirring and mixing. Then, the mixture was kept at 85°C for 2 hours to neutralize and disperse the water-based polyester resin, thereby obtaining a water-based coating composition with a resin concentration of 25% by mass.

[0126] (2) Examples 3 to 6, 9 and Comparative Examples 1 to 3 The water-based polyester resin obtained above had low water solubility, and the polyester resin could not be dispersed under the condition (1) above. For this reason, the water-based polyester resin was dispersed using n-butyl cellosolve as a hydrophilic organic solvent. In detail, 100 parts by mass of the water-based polyester resin obtained above, 20 parts by mass of n-butyl cellosolve, 274 parts by mass of water, and 6 parts by mass of a 25% by mass aqueous ammonia solution as a neutralizing base were added, and the temperature was raised to 85°C while stirring and mixing. Then, the mixture was kept at a temperature of 85°C for 2 hours to neutralize and disperse the water-based polyester resin, thereby obtaining a water-based coating composition with a resin concentration of 25% by mass.

[0127] (3) Reference examples (Reference examples 1 to 3) The aqueous polyester resins of Reference Examples 1 and 2 obtained above were prepared by the method (1) above, and the aqueous polyester resin of Reference Example 3 was prepared by the method (2) above, to obtain aqueous coating compositions each having a resin concentration of 25% by mass.

[0128] <Evaluation> [Resin properties] The resin properties of the water-based polyester resin thus produced were evaluated by the following methods.

[0129] (Acid value (mgKOH / g)) The acid value of the water-based polyester resin was determined from the measurement results by titration using an ethanol solution of potassium hydroxide.

[0130] (Weight average molecular weight) The weight average molecular weight of the aqueous polyester resin was determined from the results of measurement by gel permeation chromatography (polystyrene equivalent).

[0131] (Glass transition temperature (℃)) The glass transition temperature of the water-based polyester resin was determined from the results of measurement by differential scanning calorimetry.

[0132] [Physical property measurements] The physical properties of the aqueous coating composition (resin dispersion) prepared above were measured by the following methods.

[0133] (Water dispersibility) The appearance of the resin dispersion was observed and the results were evaluated as follows. A: No sediment was observed. B: A small amount of sediment is observed. C: A large amount of sediment is observed. D: The resin does not disperse in the solvent.

[0134] (Stability of resin dispersion) The resin dispersion was placed in a glass bottle, sealed, and left to stand for 15 days at 20° C. After standing, the appearance of the dispersion was observed, and the results were evaluated as follows. A: No separation or sediment is observed in the dispersion. B: A small amount of separation or sediment is observed in the dispersion. C: A large amount of separation or sediment is observed in the dispersion.

[0135] (Stability of solution haze over time) The resin dispersion was placed in a glass bottle, sealed, and left to stand for 15 days at 5° C., 20° C., and 30° C. The haze (%) of the dispersion after standing was measured using a haze meter manufactured by Nippon Denshoku Industries Co., Ltd., and the results were evaluated as follows. A: The rate of change in haze of the dispersion is less than 20% compared to the dispersion before it was left standing. B: The rate of change in haze of the dispersion is 20% or more and less than 40% compared to the dispersion before being left standing. C: The rate of change in haze of the dispersion is 40% or more and less than 60% compared to the dispersion before standing. D: Compared to the dispersion before standing, the rate of change in haze of the dispersion is 60% or more, or the haze of the dispersion is 90% or more.

[0136] (PET film adhesion) An untreated biaxially oriented polyethylene terephthalate (PET) film was prepared as a substrate. The resin dispersion prepared by neutralizing with the base was applied onto the substrate using a bar coater, and then heated at 120°C for 5 minutes. As a result, the base was removed, and a primer layer of about 1 μm in thickness was formed on the substrate by the resin (Y) with the carboxyl group regenerated. Next, cellophane adhesive tape was adhered to the primer layer on the substrate and peeled off, and the state of the remaining primer layer was observed. The results were evaluated as follows. A: No peeling of the primer layer is observed. B: Peeling is observed in part of the primer layer. C: Peeling is observed in most parts of the primer layer.

[0137] (Adhesion to aluminum vapor deposition layer) An untreated biaxially oriented polyethylene terephthalate (PET) film was prepared as the substrate, and a primer layer of about 1 μm in thickness was formed on the substrate in the same manner as in the "PET film adhesion" above. Next, an aluminum vapor deposition layer of about 1 μm in thickness was formed on the primer layer on the substrate by a vacuum deposition process. Cellophane adhesive tape was adhered to this aluminum vapor deposition layer and peeled off, and the state of the remaining aluminum vapor deposition layer was observed. The results were evaluated as follows. A: No peeling of the aluminum vapor deposition layer is observed. B: Peeling is observed in part of the aluminum vapor deposition layer. C: Peeling is observed in most parts of the aluminum vapor deposition layer.

[0138] (water resistance) An untreated biaxially oriented polyethylene terephthalate (PET) film was prepared as a substrate, and a primer layer of about 1 μm in thickness was formed on the substrate in the same manner as in the above-mentioned "PET film adhesion". Then, the substrate on which the primer layer was formed was immersed in water at 50° C. for 30 minutes. After 30 minutes, it was taken out of the water and left to dry for 24 hours in a room at 20° C. After drying, the state of the primer layer on the substrate was observed. The results were evaluated as follows. A: No whitening or dissolution of the primer layer is observed. B: Whitening or dissolution is observed in part of the primer layer. C: Whitening and dissolution are observed in most of the primer layer.

[0139] (Haze) An untreated biaxially oriented polyethylene terephthalate (PET) film was prepared as the substrate. A resin dispersion was applied onto this substrate using a bar coater, and then heated at 120°C for 5 minutes. As a result, a primer layer with a thickness of about 3 μm was formed on the substrate. Next, the haze of the substrate alone and the haze of the substrate and primer layer combined were measured using a haze meter manufactured by Nippon Denshoku Industries Co., Ltd. The haze of the primer layer (%) was calculated by subtracting the haze of the substrate alone from the haze of the substrate and primer layer combined.

[0140] Table 1 below shows the evaluation results of physical property tests regarding water dispersibility, stability of the resin dispersion, stability of the resin dispersion, stability of the solution haze over time, water resistance, adhesion to PET film, adhesion to aluminum vapor deposition layer, and haze.

[0141] [Table 1]

[0142] As can be seen from the results in Table 1, the aqueous polyester resins obtained by the manufacturing methods of Examples 1 to 9 have excellent water resistance and water dispersibility while reducing the environmental load, and also have excellent resin dispersion stability. Furthermore, even though they contain terephthalic acid residues derived from recycled polyester, they have resin properties such as adhesion and transparency equivalent to those of terephthalic acid or terephthalic acid derivatives not derived from recycled polyester. The resin dispersions have excellent long-term water dispersibility and can further improve stability, such as the stability of solution haze over time.

[0143] The aqueous polyester resin obtained by the manufacturing method of Comparative Example 1 could not be dispersed in water or water containing a hydrophilic organic solvent without a surfactant, etc. The aqueous polyester resins obtained by the manufacturing methods of Comparative Examples 2 and 3 were inferior in the stability of the resin dispersion and the stability of the solution haze over time.

Claims

1. A method for producing an aqueous polyester resin using recycled polyester, comprising the steps of: a first step of carrying out an ester formation reaction and a depolymerization reaction using the recycled polyester, a first polycarboxylic acid component containing a divalent polycarboxylic acid residue other than a terephthalic acid residue, and a polyhydric alcohol component; a second step of carrying out an ester forming reaction using the reaction product of the first step and a second polyvalent carboxylic acid component containing a trivalent or higher polyvalent carboxylic acid residue; A third step of carrying out a polycondensation reaction by reducing pressure. Equipped with In the first step, The recycled polyester, the first polyvalent carboxylic acid component, and the polyhydric alcohol component are mixed to obtain a reaction raw material mixture, and then the ester formation reaction and the depolymerization reaction are carried out in the reaction raw material mixture, In the first step, the recycled polyester is used in an amount such that a ratio of the terephthalic acid residues to a total of the terephthalic acid residues contained in the recycled polyester and the polycarboxylic acid residues contained in the first polycarboxylic acid component and the second polycarboxylic acid component is 20% by mass or more and 72% by mass or less, The method for producing an aqueous polyester resin, wherein the acid value of the resulting aqueous polyester resin is 30 mgKOH / g or more and 120 mgKOH / g or less.

2. 2. The method for producing an aqueous polyester resin according to claim 1, wherein in the first step, the first polycarboxylic acid component is used in an amount such that a ratio of the divalent polycarboxylic acid residue to a total of the terephthalic acid residue contained in the recycled polyester and the polycarboxylic acid residues contained in the first polycarboxylic acid component and the second polycarboxylic acid component is 5% by mass or more and 50% by mass or less.

3. In the second step, a mixture of the terephthalic acid residue contained in the recycled polyester and the polycarboxylic acid residues contained in the first polycarboxylic acid component and the second polycarboxylic acid component is The method for producing an aqueous polyester resin according to claim 1 or 2, wherein the second polyvalent carboxylic acid component is used in an amount such that a ratio of the trivalent or higher polyvalent carboxylic acid residue to the total is 10% by mass or more and 30% by mass or less.

4. The method for producing an aqueous polyester resin according to any one of claims 1 to 3, wherein the first polycarboxylic acid component and the second polycarboxylic acid component do not contain a polycarboxylic acid compound having a metal sulfonate group.

5. The method for producing an aqueous polyester resin according to claim 1 , wherein the polyhydric alcohol component does not contain a trihydric or higher polyhydric alcohol compound.

6. 6. The method for producing an aqueous polyester resin according to claim 1, wherein the polyhydric alcohol component contains a dihydric alcohol compound, the dihydric alcohol compound has a branched chain, and a ratio of residues of the dihydric alcohol compound having a branched chain is 10% by mass or more and 90% by mass or less with respect to all polyhydric alcohol residues contained in the aqueous polyester resin.

7. A method for producing an aqueous polyester resin according to any one of claims 1 to 6, a step of neutralizing at least a portion of the carboxy groups of the aqueous polyester resin with a base; A method for producing a water-based coating composition comprising the steps of:

8. An aqueous polyester resin having a terephthalic acid residue derived from recycled polyester, a polyvalent carboxylic acid residue other than the terephthalic acid residue, and a polyhydric alcohol residue, the polycarboxylic acid residue contains a first divalent polycarboxylic acid residue and a second trivalent or higher polycarboxylic acid residue, the first polycarboxylic acid residue and the second polycarboxylic acid residue do not contain a polycarboxylic acid residue having a metal sulfonate group, a ratio of the terephthalic acid residue to a total of the terephthalic acid residue, the first polycarboxylic acid residue, and the second polycarboxylic acid residue is 45% by mass or more and 72% by mass or less, a ratio of the first polycarboxylic acid residue to a total of the terephthalic acid residue, the first polycarboxylic acid residue, and the second polycarboxylic acid residue is 5% by mass or more and 40% by mass or less, The polyhydric alcohol residue does not contain a residue of a trihydric or higher polyhydric alcohol compound, the polyhydric alcohol residue contains a residue of a dihydric alcohol compound, the residue of the dihydric alcohol compound has a branched chain, and a ratio of the residue of the dihydric alcohol compound having a branched chain to the total polyhydric alcohol residues contained in the aqueous polyester resin is 10 mass% or more and 42 mass% or less; A water-based polyester resin having an acid value of 35 mgKOH / g or more and 120 mgKOH / g or less.

9. 9. The aqueous polyester resin according to claim 8, wherein a ratio of the second polycarboxylic acid residue to a total of the terephthalic acid residue, the first polycarboxylic acid residue, and the second polycarboxylic acid residue is 10% by mass or more and 30% by mass or less.

10. A water-based coating composition containing a water-based polyester resin, 10. An aqueous coating composition comprising the aqueous polyester resin according to claim 8 or 9, wherein the aqueous polyester resin is a neutralized product of the aqueous polyester resin according to claim 8 or 9.

Citation Information

Patent Citations

  • Aqueous coating composition from polyethylene terephthalate

    JP1993271612A

  • Sulfoaryl-modified water-soluble or water-dispersible resins from polyethylene terephthalate or terephthalates

    JP2001505608A

  • Modified polyester resin

    JP2002179783A

  • Method for producing aqueous dispersion of alkyd resin

    JP2003327679A

  • Water-based flame retardant polyester resin, resin composition for filming and fiber fabric using the same

    JP2004067910A