Light control film

The light control film with indium tin composite oxide electrode layers and optional near-infrared layers addresses the heat shielding inadequacy of existing films, enhancing reflectivity and shielding properties against sunlight.

JP7561957B1Active Publication Date: 2024-10-04NITTO DENKO CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023216181
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2023-12-21
Publication Date
2024-10-04
Estimated Expiration
2043-12-21

AI Technical Summary

Technical Problem

Existing light control films do not effectively address the need for improved heat shielding properties against sunlight, as the electrodes contain free electrons with significant reflectivity to heat rays, occupying a large area and affecting heat shielding efficiency.

Method used

A light control film with a first electrode layer made of indium tin composite oxide containing 11% by mass or more tin oxide, and a second electrode layer with similar composition, enhancing the number of carriers to improve heat shielding properties, combined with optional near-infrared absorption and reflection layers.

Benefits of technology

The film achieves superior heat shielding against sunlight by increasing the reflectivity of the electrode layers to heat rays, ensuring good heat shielding properties while maintaining transparency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007561957000001_ABST
    Figure 0007561957000001_ABST
Patent Text Reader

Abstract

To provide a light control film suitable for realizing good heat shielding properties against sunlight. [Solution] The light control film X of the present invention includes a base film 10, an electrode layer 20, a light control layer 30, and an electrode layer 40 in this order in the thickness direction H. The electrode layer 20 is an indium tin composite oxide layer with a tin oxide ratio of 11 mass % or more. The electrode layer 20 has a thickness of 10×10 15 cm -2 It has the above number of carriers.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a light management film. [Background technology]

[0002] A light control film that is attached to window glass of a building, a vehicle, etc. is known. The light control film includes a light control section and a transparent substrate film that supports the light control section. The light control section includes, for example, a transparent conductive layer, a light control layer, and a transparent conductive layer in this order in the thickness direction. The light control layer is sandwiched between two transparent conductive layers. The light control layer is formed from an electrochromic (EC) material. The EC material is a material that can be reversibly changed between a colored non-transparent state and a colorless transparent state, for example, by electrochemical oxidation-reduction. Each transparent conductive layer is an electrode layer. By turning on and off the voltage between the electrodes (transparent conductive layers), the light control layer is switched, for example, between a non-transparent state (light blocking state) and a transparent state (non-light blocking state). In a window glass to which such a light control film is attached, the transmittance of light such as visible light through the window glass with the light control film can be switched by turning on and off the voltage between the electrodes (switching control of light transmittance). The technology relating to such light control films is described, for example, in Patent Document 1 listed below. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2019-101206 A Summary of the Invention [Problem to be solved by the invention]

[0004] From the viewpoint of improving comfort in buildings and vehicles and reducing the cooling load, etc., light control films are required to have heat shielding properties against sunlight.

[0005] Meanwhile, the present inventors have discovered the following about light-control films. The electrode (transparent conductive layer) contains free electrons as carriers that have significant reflectivity to heat rays in sunlight (electromagnetic waves such as near-infrared rays that transmit heat by radiation). In light-control films, such electrodes are provided over the entire surface of the light-control layer. That is, the surface area ratio of the electrodes in the surface direction of the light-control film is large. In such light-control films, the heat-shielding properties of the film against sunlight can be efficiently controlled by adjusting the number of carriers in the electrodes. The present invention is based on such findings.

[0006] The present invention provides a light control film suitable for achieving good heat shielding properties against sunlight. [Means for solving the problem]

[0007] The present invention [1] is a light-controlling film comprising a base film, a first electrode layer, a light-controlling layer, and a second electrode layer in this order in the thickness direction, the first electrode layer being an indium tin composite oxide layer having a tin oxide ratio of 11 mass% or more, and the first electrode layer being an indium tin composite oxide layer having a tin oxide ratio of 10×10 15 cm -2 This includes light-control films having the above number of carriers.

[0008] The present invention [2] includes the light control film according to the above [1], in which the second electrode layer is an indium tin composite oxide layer having a tin oxide ratio of 11 mass % or more.

[0009] The present invention [3] includes the light control film according to the above [1] or [2], in which the base film has a near-infrared absorbing layer and / or a near-infrared reflective layer.

[0010] The present invention [4] includes the light control film according to any one of the above [1] to [3], which has an average transmittance of 50% or less at wavelengths of 800 nm to 1300 nm. Effect of the Invention

[0011] As described above, the light control film of the present invention includes a base film, a first electrode layer, a light control layer, and a second electrode layer in this order in the thickness direction. The first electrode layer is an indium tin composite oxide layer having a tin oxide ratio of 11% by mass or more, and has a thickness of 10×10 15 cm -2 The light control film has a carrier number of 100 or more. Such a light control film is suitable for ensuring the number of free electrons (number of carriers) per unit area in plan view in the first electrode layer. The greater the number of free electrons per unit area in the first electrode layer, the higher the reflectivity of the first electrode layer against heat rays in sunlight. The higher the reflectivity of the first electrode layer against heat rays, the higher the shielding property (heat shielding property) against heat rays of a light control film including such a first electrode layer. Therefore, the light control film of the present invention is suitable for achieving good heat shielding property against sunlight. [Brief description of the drawings]

[0012] [Figure 1] FIG. 1 is a schematic cross-sectional view of one embodiment of a light control film of the present invention. [Diagram 2] 2A and 2B show some steps in an example of a method for producing the light-controlling film shown in Fig. 1. Fig. 2A shows a substrate film preparation step, Fig. 2B shows a transparent conductive layer formation step, Fig. 2C shows a crystallization step, and Fig. 2D shows a light-controlling layer formation step. [Diagram 3] This shows a lamination step subsequent to the step shown in FIG. 2D. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] The light control film X according to one embodiment of the present invention includes a base film 10 (first base film), an electrode layer 20 (first electrode layer), a light control layer 30, an electrode layer 40 (second electrode layer), and a base film 50 (second base film) in this order in the thickness direction H. The base film 10 has a first surface 10a and a second surface 10b opposite to the first surface 10a. The electrode layer 20 is disposed on the first surface 10a. The electrode layer 20 and the first surface 10a are in contact with each other. The light control layer 30 is disposed on the electrode layer 20. The light control layer 30 and the electrode layer 20 are in contact with each other. The electrode layer 40 is disposed on the light control layer 30. The electrode layer 40 and the light control layer 30 are in contact with each other. The base film 50 is disposed on the electrode layer 40. The base film 50 has a first surface 50a on the electrode layer 40 side and a second surface 50b on the opposite side to the first surface 50a. The electrode layer 40 and the first surface 50a are in contact with each other. The light control film X has a sheet shape that spreads in a direction (plane direction) perpendicular to the thickness direction H.

[0014] In the light control film X, the base film 10 and the electrode layer 20 form an electrode-attached base film Y1.

[0015] In this embodiment, the base film 10 includes a resin film 11 and a cured resin layer 12, which are arranged in this order in the thickness direction H. The cured resin layer 12 is in contact with the resin film 11. The cured resin layer 12 forms a first surface 10a of the base film 10.

[0016] The resin film 11 is a base material that ensures the strength of the light control film X. The resin film 11 is a transparent resin film having flexibility. Examples of the material of the resin film 11 include polyester resin, polyolefin resin, acrylic resin, polycarbonate resin, polyethersulfone resin, polyarylate resin, melamine resin, polyamide resin, polyimide resin, cellulose resin, and polystyrene resin. Examples of the polyester resin include polyethylene terephthalate (PET), polybutylene terephthalate, and polyethylene naphthalate. Examples of the polyolefin resin include polyethylene, polypropylene, and cycloolefin polymer. Examples of the acrylic resin include polymethacrylate. From the viewpoints of transparency and strength, the material of the resin film 11 is preferably polyester resin, and more preferably PET.

[0017] The surface of the resin film 11 on the side of the cured resin layer 12 may be subjected to a surface modification treatment. Examples of the surface modification treatment include corona treatment, plasma treatment, ozone treatment, primer treatment, glow treatment, and coupling agent treatment (the same applies to the surface modification treatment of the resin film 51 described below).

[0018] The thickness of the resin film 11 is preferably 10 μm or more, more preferably 20 μm or more, and even more preferably 30 μm or more, from the viewpoint of ensuring the strength of the light control film X. The thickness of the resin film 11 is preferably 300 μm or less, more preferably 200 μm or less, and even more preferably 150 μm or less, from the viewpoint of ensuring the handleability of the resin film 11 in the roll-to-roll system. The thickness of the resin film 11 is preferably 10 to 300 μm, more preferably 20 to 200 μm, and even more preferably 30 to 150 μm, from the viewpoint of achieving both the strength and the handleability of the light control film X.

[0019] The visible light transmittance of the resin film 11 is preferably 70% or more, more preferably 80% or more, and even more preferably 85% or more, from the viewpoint of ensuring the transparency required for the light control film in the transparent state in the light control film X. The visible light transmittance of the resin film 11 is, for example, 100% or less. The visible light transmittance is the transmittance in the wavelength range of 380 nm to 780 nm.

[0020] In this embodiment, the cured resin layer 12 is an optical adjustment layer (refractive index adjustment layer) for improving the optical characteristics of the light control film X. The cured resin layer 12 may have a function of blocking moisture and organic gases generated from the resin film 11 in the transparent conductive layer forming step (FIG. 2B) described later. In this embodiment, the cured resin layer 12 is a cured product of a curable first resin composition. The first resin composition contains a resin. Examples of the resin include melamine resin, alkyd resin, organic silane condensate, polyester resin, acrylic urethane resin, acrylic resin (excluding acrylic urethane resin), urethane resin (excluding acrylic urethane resin), amide resin, silicone resin, and epoxy resin. These resins may be used alone or in combination of two or more kinds. From the viewpoint of ensuring the adhesion of the electrode layer 20 to the base film 10, the resin in the first resin composition is preferably at least one selected from the group consisting of melamine resin, alkyd resin, and organic silane condensate. The first resin composition may be an ultraviolet-curable resin composition or a thermosetting resin composition.

[0021] The thickness of the cured resin layer 12 is preferably 5 nm or more, more preferably 10 nm or more, even more preferably 20 nm or more, and even more preferably 30 nm or more, from the viewpoint of improving the light transmission characteristics of the light control film X. The thickness of the cured resin layer 12 is preferably 1000 nm or less, more preferably 100 nm or less, even more preferably 50 nm or less, and even more preferably 40 nm or less, from the viewpoint of thinning the light control film X. The thickness of the cured resin layer 12 is preferably 5 to 1000 nm, more preferably 10 to 100 nm, even more preferably 20 to 50 nm, and even more preferably 30 to 40 nm, from the viewpoint of achieving both the light transmission characteristics and thinning of the light control film X.

[0022] The base film 10 may have another cured resin layer on the opposite side of the resin film 11 to the cured resin layer 12. Examples of the other cured resin layer include a hard coat layer and an anti-blocking layer. In Fig. 1, the other cured resin layer in the base film 10 is shown by a phantom line as cured resin layer 13.

[0023] The other cured resin layer is, for example, a cured product of a curable second resin composition. The second resin composition contains a resin. Examples of the resin include polyester resin, acrylic urethane resin, acrylic resin (excluding acrylic urethane resin), urethane resin (excluding acrylic urethane resin), amide resin, silicone resin, epoxy resin, and melamine resin. These resins may be used alone or in combination of two or more kinds. The second resin composition may be an ultraviolet-curable resin composition or a thermosetting resin composition.

[0024] The second resin composition may contain particles. Examples of the particles include inorganic oxide particles and organic particles. Examples of the material of the inorganic oxide particles include silica, alumina, titania, zirconia, calcium oxide, tin oxide, indium oxide, cadmium oxide, and antimony oxide. Examples of the material of the organic particles include polymethyl methacrylate, polystyrene, polyurethane, acrylic-styrene copolymer, benzoguanamine, melamine, and polycarbonate. The particles are preferably inorganic oxide particles, and more preferably at least one selected from the group consisting of silica particles and zirconia particles.

[0025] The thickness of the other cured resin layer is preferably 0.5 μm or more, more preferably 1 μm or more, and even more preferably 2 μm or more, from the viewpoint of ensuring the function of the cured resin layer. The thickness of this cured resin layer is preferably 10 μm or less, more preferably 5 μm or less, and even more preferably 3 μm or less, from the viewpoint of reducing the thickness of the light control film X. The thickness of this cured resin layer is preferably 0.5 to 10 μm, more preferably 1 to 5 μm, and even more preferably 2 to 3 μm, from the viewpoint of both ensuring the function of the layer and reducing the thickness of the light control film X.

[0026] The thickness of the base film 10 is preferably 10 μm or more, more preferably 30 μm or more, even more preferably 50 μm or more, and even more preferably 60 μm or more, from the viewpoint of ensuring the handleability of the light control film X. The thickness of the base film 10 is preferably 500 μm or less, more preferably 300 μm or less, even more preferably 200 μm or less, and even more preferably 150 μm or less, from the viewpoint of thinning the light control film X. The thickness of the base film 10 is preferably 10 to 500 μm, more preferably 30 to 300 μm, even more preferably 50 to 200 μm, and even more preferably 60 to 150 μm, from the viewpoint of achieving both the handleability and thinning of the light control film X.

[0027] The visible light transmittance of the base film 10 is preferably 70% or more, more preferably 80% or more, and even more preferably 85% or more, from the viewpoint of ensuring the transparency required for the light control film in the transparent state in the light control film X. The visible light transmittance of the base film 10 is, for example, 100% or less.

[0028] The substrate film 10 preferably has a near-infrared absorbing layer and / or a near-infrared reflective layer (each layer is not shown). The near-infrared absorbing layer means a layer that exhibits significant absorption ability for near-infrared rays (wavelength 700 nm to 2500 nm). The near-infrared reflective layer means a layer that exhibits significant reflection ability for near-infrared rays (wavelength 700 nm to 2500 nm).

[0029] The near-infrared absorbing layer may be disposed between the resin film 11 and the cured resin layer 12, or may be disposed on the opposite side of the resin film 11 to the cured resin layer 12. The resin film 11 may be a near-infrared absorbing layer, or may have a multi-layer structure including a near-infrared absorbing layer. The near-infrared absorbing layer includes, for example, a near-infrared absorbing agent and a binder resin. Examples of the near-infrared absorbing agent include inorganic near-infrared absorbing agents and organic near-infrared absorbing agents. Examples of the inorganic near-infrared absorbing agent include CFM complex oxide particles and tungsten oxide particles. The CFM complex oxide is a complex oxide of copper, iron, and manganese. Examples of the material of the binder resin include the materials described above with respect to the resin film 11.

[0030] The near-infrared reflective layer may be disposed between the resin film 11 and the cured resin layer 12, or may be disposed on the opposite side of the resin film 11 to the cured resin layer 12. The resin film 11 may be a near-infrared reflective layer, or may have a multilayer structure including a near-infrared reflective layer. The near-infrared reflective layer has, for example, a multilayer structure including a plurality of resin thin layers having different optical properties, and preferably has a multilayer structure in which a first resin thin layer and a second resin thin layer having different optical properties are alternately arranged in the thickness direction H. Examples of the optical properties include an in-plane average refractive index. The difference in the in-plane average refractive index between the first resin thin layer and the second resin thin layer is preferably 0.01 or more, more preferably 0.03 or more, and is preferably 0.15 or less, more preferably 0.12 or less. The number of laminated resin thin layers forming the multilayer structure is, for example, 20 or more, and, for example, 700 or less. Examples of the material of the resin thin layer include the materials described above for the resin film 11.

[0031] The electrode layer 20 is a layer that has both optical transparency and electrical conductivity. Such an electrode layer 20 is made of a transparent conductive material. That is, the electrode layer 20 is a transparent conductive layer.

[0032] The electrode layer 20 is formed of indium tin oxide (ITO) as a transparent conductive material. That is, the electrode layer 20 is an indium tin oxide layer. ITO may contain a metal or semimetal other than In and Sn in an amount less than the respective contents of In and Sn.

[0033] The ratio of the content of tin oxide to the total content of indium oxide (In2O3) and tin oxide (SnO2) in ITO (tin oxide ratio) is 11 mass% or more, preferably 12 mass% or more, and more preferably 12.5 mass% or more, from the viewpoint of appropriately suppressing the growth of crystal grains in the transparent conductive layer in the crystallization step (FIG. 2C) described later and ensuring the number of carriers in the electrode layer 20. The tin oxide ratio is preferably 18 mass% or less, more preferably 16 mass% or less, and even more preferably 14 mass% or less, from the viewpoint of reducing the resistance of the electrode layer 20. The tin oxide ratio is preferably 11 to 18 mass%, more preferably 12 to 16 mass%, and even more preferably 12.5 to 14 mass%, from the viewpoint of both ensuring the number of carriers and reducing the resistance.

[0034] The tin oxide ratio in ITO can be identified, for example, as follows. First, the abundance ratio of indium atoms (In) and tin atoms (Sn) in ITO, which is the object to be measured, is determined by X-ray photoelectron spectroscopy. From the abundance ratios of In and Sn in ITO, the ratio of the number of Sn atoms to the number of In atoms in ITO is determined. This gives the tin oxide ratio in ITO. The tin oxide ratio in ITO can also be determined from the tin oxide (SnO2) content of the ITO target used during sputtering film formation.

[0035] The electrode layer 20 is preferably a crystalline film. The electrode layer 20 is preferably a crystalline film from the viewpoint of reducing the resistance of the electrode layer 20, and is also preferable for realizing good infrared reflection characteristics in the electrode layer 20 and the light control film X.

[0036] Whether an electrode layer (electrode layers 20 and 40 in the light control film X) made of a conductive oxide is a crystalline film can be determined, for example, by the following method. First, the electrode layer is immersed in hydrochloric acid with a concentration of 5% by mass at 20°C for 15 minutes. Next, the electrode layer is washed with water and then dried. Next, the resistance between a pair of terminals separated by a distance of 15 mm (inter-terminal resistance) is measured on the exposed surface of the electrode layer. In this measurement, if the inter-terminal resistance is 10 kΩ or less, the electrode layer can be determined to be a crystalline film.

[0037] The number of carriers (the number of free electrons) in the plan view (plane direction) of the electrode layer 20 is 10×10 15 cm -2 or more, preferably 12×10 15 cm -2 More preferably, 14×10 15 cm -2 More preferably, 14.5×10 15 cm -2 This number of carriers represents the number of carriers (free electrons) per unit area (1 square centimeter) in a plan view of the electrode layer 20. From the viewpoint of ensuring the visible light transmittance of the electrode layer 20, the number of carriers (free electrons) in a plan view of the electrode layer 20 is preferably 100×10 15 cm -2 Less than or equal to 60×10 15 cm -2 Less than 40×10, more preferably 15 cm -2 More preferably, 20×10 15 cm -2 The number of carriers in the electrode layer 20 is preferably 10×10 from the viewpoint of ensuring both the heat shielding property of the electrode layer 20 and the visible light transmittance. 15 ~100×10 15 cm -2 , more preferably 12×10 15 ~60×10 15 cm -2 , and more preferably 14×10 15 ~40×10 15 cm -2 , more preferably 14.5×10 15~20×10 15 cm -2 The method for adjusting the number of carriers in the electrode layer 20 includes, for example, adjusting the composition of the electrode layer 20, adjusting the thickness of the electrode layer 20, and adjusting the film formation temperature in the transparent conductive layer forming step (FIG. 2B) described below. The adjustment of the composition of the electrode layer 20 includes adjusting the composition of the target used in the sputtering film formation in the transparent conductive layer forming step, and adjusting the ratio of the amount of oxygen introduced. The method for measuring the number of carriers in the electrode layer is as described below in relation to the examples.

[0038] The thickness of the electrode layer 20 is preferably 50 nm or more, more preferably 80 nm or more, even more preferably 100 nm or more, and even more preferably 120 nm or more, from the viewpoint of ensuring the number of carriers in the electrode layer 20. A thick electrode layer 20 is also preferable from the viewpoint of reducing the resistance of the electrode layer 20. The thickness of the electrode layer 20 is preferably 300 nm or less, more preferably 200 nm or less, even more preferably 170 nm or less, and even more preferably 140 nm or less, from the viewpoint of ensuring the bending resistance of the electrode layer 20 (suppressing cracking of the electrode layer 20 when bent). The thickness of the electrode layer 20 is preferably 50 to 300 nm, more preferably 80 to 200 nm, even more preferably 100 to 170 nm, and even more preferably 120 to 140 nm, from the viewpoint of ensuring the number of carriers in the electrode layer 20, reducing the resistance, and bending resistance.

[0039] From the viewpoint of reducing the resistance of the electrode layer 20, the specific resistance of the electrode layer 20 is preferably 2.5×10 -4 Ω cm or less, preferably 2.3×10 -4 Ω cm or less, more preferably 2.1×10 -4 Ω·cm or less, more preferably 2.0×10 -4 The specific resistance of the electrode layer 20 is preferably 0.1×10 -4 Ω·cm or more, preferably 0.5×10 -4 Ω cm or more, more preferably 1.0×10 -4Ω·cm or more. The method for measuring the resistivity of the electrode layer is as described below in relation to the Examples. An example of a method for adjusting the resistivity is to adjust various conditions for sputtering deposition in the transparent conductive layer formation step (FIG. 2B) described below. Such conditions include, for example, the temperature of the base (substrate film 10 in this embodiment) on which the film is formed, the amount of oxygen introduced into the deposition chamber, the air pressure in the deposition chamber, and the horizontal magnetic field strength above the target.

[0040] When the electrode layer 20 is an amorphous film that is crystallized by heating, the resistivity of such an electrode layer 20 is preferably 4.5×10 -4 Ω cm or more, preferably 4.8×10 -4 Ω cm or more, more preferably 5.0×10 -4 Ω cm or more, more preferably 5.2×10 -4 Ω·cm or more, and preferably 15×10 -4 Ω cm or less, preferably 13×10 -4 Ω cm or less, more preferably 11×10 -4 Ω cm or less, more preferably 9.0×10 -4 Ω·cm or less, more preferably 8.0×10 -4 Ω·cm or less.

[0041] The visible light transmittance of the electrode layer 20 is, for example, 50% or more, preferably 70% or more, more preferably 80% or more, and even more preferably 85% or more, from the viewpoint of ensuring the transparency required for the light control film in the transparent state in the light control film X. The visible light transmittance of the electrode layer 20 is, for example, 100% or less.

[0042] The content ratio of rare gas atoms in the electrode layer 20 is preferably 0.3 atomic % or less, more preferably 0.2 atomic % or less, further preferably 0.1 atomic % or less, and for example, 0.0001 atomic % or more, from the viewpoint of reducing the resistance (reducing the specific resistance) of the electrode layer 20. Examples of rare gas atoms include argon (Ar), krypton (Kr), and xenon (Xe). The rare gas atoms are derived from, for example, a sputtering gas used in the transparent conductive layer forming step (FIG. 2B) described later (sputtering gas is mixed in). Examples of methods for identifying the content ratio of rare gas atoms in the electrode layer 20 include fluorescent X-ray analysis and Rutherford backscattering spectrometry (RBS) (the same applies to the method for identifying the content ratio of rare gas atoms in the electrode layer 40 described later).

[0043] The light-adjusting layer 30 is formed of a material that can be reversibly changed between a colored non-transparent state (light-shielding state) and a transparent state (light-non-shielding state) by the action of, for example, an electric current or an electric field. Examples of the light-adjusting layer 30 include an electrochromic (EC) light-adjusting layer, a light-adjusting layer containing a polymer dispersed liquid crystal (PDLC), a light-adjusting layer containing a polymer network liquid crystal (PNLC), and a suspended particle device (SPD) light-adjusting layer.

[0044] The EC light control layer is formed from an EC material. The EC material is a material that can be reversibly changed between a colored non-transparent state (light-shielding state) and a transparent state (light-non-shielding state) by electrochemical oxidation and reduction. The EC material includes inorganic EC materials and organic EC materials. The inorganic EC materials include, for example, tungsten oxide, vanadium oxide, molybdenum oxide, iridium oxide, rhodium oxide, and indium nitride. The organic EC materials include, for example, polyaniline, viologen, and polyoxotungstate.

[0045] Polymer-dispersed liquid crystal has a structure in which liquid crystal is phase-separated in a polymer. Polymer-network liquid crystal has a structure in which liquid crystal is dispersed in a polymer network, and the liquid crystal in the polymer network forms a continuous phase. In these, examples of liquid crystal compounds include nematic liquid crystal compounds, smectic liquid crystal compounds, and cholesteric liquid crystal compounds. Examples of nematic liquid crystal compounds include biphenyl-based compounds, phenylbenzoate-based compounds, cyclohexylbenzene-based compounds, azoxybenzene-based compounds, azobenzene-based compounds, azomethine-based compounds, terphenyl-based compounds, biphenylbenzoate-based compounds, cyclohexylbiphenyl-based compounds, phenylpyridine-based compounds, cyclohexylpyrimidine-based compounds, and cholesterol-based compounds.

[0046] The thickness of the light-controlling layer 30 is preferably 1 μm or more, more preferably 5 μm or more, and even more preferably 10 μm or more, from the viewpoint of ensuring a large difference in visible light transmittance between the non-transparent state and the transparent state in the light-controlling film X. The thickness of the light-controlling layer 30 is preferably 200 μm or less, more preferably 100 μm or less, and even more preferably 80 μm or less, from the viewpoint of thinning the light-controlling film X and ensuring high transmittance in the transparent state. The thickness of the light-controlling layer 30 is preferably 1 to 200 μm, more preferably 5 to 100 μm, and even more preferably 10 to 80 μm, from the viewpoint of achieving both the above-mentioned visible light transmittance difference in the light-controlling film X and the above-mentioned thinning and high transmittance.

[0047] In the light control film X, the base film 50 and the electrode layer 40 form an electrode-attached base film Y2.

[0048] In this embodiment, the base film 50 includes a resin film 51 and a cured resin layer 52, which are arranged in this order in the thickness direction H. The cured resin layer 52 is in contact with the resin film 51. The cured resin layer 52 forms a first surface 50a of the base film 50.

[0049] The resin film 51 is a base material that ensures the strength of the light control film X. The resin film 51 is a transparent resin film having flexibility. Examples of materials for the resin film 51 include the materials mentioned above as the materials for the resin film 11. The surface of the resin film 51 on the side of the cured resin layer 52 may be subjected to a surface modification treatment. The preferred thickness and preferred visible light transmittance of the resin film 51 are the same as those mentioned above for the resin film 11.

[0050] In this embodiment, the cured resin layer 52 is an optical adjustment layer (refractive index adjustment layer) for improving the optical properties of the light control film X. The cured resin layer 52 may have a function of blocking moisture and organic gases generated from the resin film 51 in the transparent conductive layer forming step. In this embodiment, the cured resin layer 52 is a cured product of a third curing type resin composition. The third curing type resin composition contains a resin. Examples of the resin of the third curing type resin composition include the resins described above with respect to the first resin composition. In addition, the third curing type resin composition may be an ultraviolet curing type resin composition or a thermosetting type resin composition.

[0051] The thickness of the cured resin layer 52 is preferably 5 nm or more, more preferably 10 nm or more, even more preferably 20 nm or more, and even more preferably 30 nm or more, from the viewpoint of improving the light transmission characteristics of the light control film X. The thickness of the cured resin layer 52 is preferably 1000 nm or less, more preferably 100 nm or less, even more preferably 50 nm or less, and even more preferably 40 nm or less, from the viewpoint of thinning the light control film X. The thickness of the cured resin layer 52 is preferably 5 to 1000 nm, more preferably 10 to 100 nm, even more preferably 20 to 50 nm, and even more preferably 30 to 40 nm, from the viewpoint of achieving both the light transmission characteristics and thinning of the light control film X.

[0052] Similar to the above-mentioned regarding the base film 10, the base film 50 may have another cured resin layer (e.g., a hard coat layer and an antiblocking layer) on the opposite side of the resin film 51 to the cured resin layer 52. In Fig. 1, the other cured resin layer in the base film 50 is shown by a phantom line as cured resin layer 53.

[0053] The visible light transmittance of the base film 50 is preferably 70% or more, more preferably 80% or more, and even more preferably 85% or more, from the viewpoint of ensuring the transparency required for the light control film in the transparent state in the light control film X. The visible light transmittance of the base film 50 is, for example, 100% or less.

[0054] The substrate film 50 preferably has a near-infrared absorbing layer and / or a near-infrared reflective layer (each layer is not shown).

[0055] In the base film 50, the near-infrared absorbing layer may be disposed between the resin film 51 and the cured resin layer 52, or may be disposed on the opposite side of the resin film 51 to the cured resin layer 52. The resin film 51 may be a near-infrared absorbing layer, or may have a multi-layer structure including a near-infrared absorbing layer. The near-infrared absorbing layer includes, for example, a near-infrared absorbing agent and a binder resin. Examples of the near-infrared absorbing agent include the near-infrared absorbing agents described above for the base film 10. Examples of the material for the binder resin include the materials described above for the resin film 11.

[0056] In the base film 50, the near-infrared reflective layer may be disposed between the resin film 51 and the cured resin layer 52, or may be disposed on the opposite side of the resin film 51 to the cured resin layer 52. The resin film 51 may be a near-infrared reflective layer, or may have a multilayer structure including a near-infrared reflective layer. Examples of the near-infrared reflective layer include the near-infrared reflective layer described above with respect to the base film 10.

[0057] The electrode layer 40 is a layer that has both optical transparency and electrical conductivity. The electrode layer 40 is formed from a transparent conductive material. That is, the electrode layer 40 is a transparent conductive layer. Examples of the transparent conductive material include indium-containing conductive oxides and antimony-containing conductive oxides. Examples of the indium-containing conductive oxides include indium tin composite oxide (ITO), indium zinc composite oxide (IZO), indium gallium composite oxide (IGO), and indium gallium zinc composite oxide (IGZO). Examples of the antimony-containing conductive oxides include antimony tin composite oxide (ATO). From the viewpoint of realizing high transparency and good electrical conductivity, the transparent conductive material is preferably an indium-containing conductive oxide, more preferably ITO. That is, the electrode layer 40 is preferably an indium-containing conductive oxide layer, more preferably an ITO layer. This ITO may contain a metal or semimetal other than In and Sn in an amount less than the respective contents of In and Sn.

[0058] When the electrode layer 40 is made of ITO, the ratio of the content of tin oxide to the total content of indium oxide (In2O3) and tin oxide (SnO2) in ITO (tin oxide ratio) is preferably 11 mass% or more, more preferably 12 mass% or more, and even more preferably 12.5 mass% or more, from the viewpoint of appropriately suppressing the growth of crystal grains in the transparent conductive layer in the crystallization step described below and ensuring the number of carriers in the electrode layer 40. The tin oxide ratio in the electrode layer 40 may be less than 11 mass%. From the viewpoint of reducing the resistance of the electrode layer 40, the tin oxide ratio in the electrode layer 40 is preferably 18 mass% or less, more preferably 16 mass% or less, and even more preferably 14 mass% or less. From the viewpoint of both ensuring the number of carriers and reducing the resistance, the tin oxide ratio in the electrode layer 40 is preferably 11 to 18 mass%, more preferably 12 to 16 mass%, and even more preferably 12.5 to 14 mass%.

[0059] The electrode layer 40 is preferably a crystalline film. The electrode layer 40 is preferably a crystalline film from the viewpoint of reducing the resistance of the electrode layer 40, and is also preferable for realizing good infrared reflection characteristics in the electrode layer 40 and the light control film X.

[0060] The number of carriers (the number of free electrons) in the plan view (plane direction) of the electrode layer 40 is preferably 10×10 15 cm -2 More preferably, 12×10 15 cm -2 More preferably, 14×10 15 cm -2 More preferably, 14.5×10 15 cm -2 The number of carriers in the electrode layer 40 in plan view is 10×10 15 cm -2 The number of carriers (the number of free electrons) in the plan view of the electrode layer 40 is preferably 100×10 15 cm -2 Less than or equal to 60×10 15 cm -2 Less than 40×10, more preferably 15 cm -2 More preferably, 20×10 15 cm -2 The number of carriers in the electrode layer 40 is preferably 10×10 from the viewpoint of ensuring both the heat shielding property of the electrode layer 40 and the visible light transmittance. 15 ~100×10 15 cm -2 , more preferably 12×10 15 ~60×10 15 cm -2 , and more preferably 14×10 15 ~40×10 15 cm -2 , more preferably 14.5×10 15 ~20×10 15 cm -2 The method for adjusting the number of carriers in the electrode layer 40 is the same as the method for adjusting the number of carriers in the electrode layer 20 described above.

[0061] The thickness of the electrode layer 40 is preferably 50 nm or more, more preferably 80 nm or more, even more preferably 100 nm or more, and even more preferably 120 nm or more, from the viewpoint of ensuring the number of carriers in the electrode layer 40. A thick electrode layer 40 is also preferable from the viewpoint of reducing the resistance of the electrode layer 40. The thickness of the electrode layer 40 is preferably 300 nm or less, more preferably 200 nm or less, even more preferably 170 nm or less, and even more preferably 140 nm or less, from the viewpoint of ensuring the bending resistance of the electrode layer 40 (suppressing cracking of the electrode layer 40 when bending). The thickness of the electrode layer 40 is preferably 50 to 300 nm, more preferably 80 to 200 nm, even more preferably 100 to 170 nm, and even more preferably 120 to 140 nm, from the viewpoint of the number of carriers, reducing the resistance, and bending resistance of the electrode layer 40.

[0062] The visible light transmittance of the electrode layer 40 is, for example, 50% or more, preferably 70% or more, more preferably 80% or more, and even more preferably 85% or more, from the viewpoint of ensuring the transparency required for the transparent state of the light control film in the light control film X. The visible light transmittance of the electrode layer 40 is, for example, 100% or less.

[0063] The content of rare gas atoms in the electrode layer 40 is preferably 0.3 atomic % or less, more preferably 0.2 atomic % or less, and further preferably 0.1 atomic % or less, and is, for example, 0.0001 atomic % or more, from the viewpoint of reducing the resistance (reducing the specific resistance) of the electrode layer 40. Examples of rare gas atoms include argon (Ar), krypton (Kr), and xenon (Xe). The rare gas atoms are derived from, for example, a sputtering gas used in the transparent conductive layer forming step (FIG. 2B) described later (sputtering gas is mixed in).

[0064] The visible light transmittance (in a transparent state) of the light control film X is preferably 70% or more, more preferably 80% or more, and even more preferably 85% or more, from the viewpoint of ensuring the transparency of the light control film X. The visible light transmittance of the base film 10 is, for example, 100% or less.

[0065] The average transmittance of the light control film X at wavelengths of 800 nm to 1300 nm is preferably 50% or less, more preferably 40% or less, and even more preferably 30% or less, from the viewpoint of ensuring good heat shielding properties against sunlight in the light control film X. The average transmittance of the light control film X is, for example, 0% or more, and preferably 10% or more. The light control film X preferably has such an average transmittance (wavelength 800 nm to 1300 nm) in a colored state or a transparent state, and more preferably has such an average transmittance (wavelength 800 nm to 1300 nm) in both a colored state and a transparent state.

[0066] The light control film X is produced, for example, as follows.

[0067] First, as shown in FIG. 2A, a substrate film 10 is prepared. The substrate film 10 can be produced by forming a cured resin layer 12 on a resin film 11. The cured resin layer 12 can be formed by applying the above-mentioned first resin composition on the resin film 11 to form a coating film, and then curing the coating film. When the first resin composition contains a thermosetting resin, the coating film is cured by heating. When the first resin composition contains an ultraviolet-curable resin, the coating film is cured by ultraviolet irradiation. The exposed surface of the cured resin layer 12 formed on the resin film 11 is subjected to a surface modification treatment as necessary. When a plasma treatment is performed as the surface modification treatment, for example, argon gas is used as an inert gas. The discharge power in the plasma treatment is, for example, 10 W or more, and, for example, 5000 W or less. The above-mentioned other cured resin layer 13 (FIG. 1) may be formed on the opposite side of the cured resin layer 12 in the resin film 11.

[0068] 2B, an amorphous transparent conductive layer 20' is formed on the base film 10 (transparent conductive layer forming step). Specifically, a transparent conductive material is deposited on the cured resin layer 12 of the base film 10 by a sputtering method to form the transparent conductive layer 20'.

[0069] In the sputtering method, it is preferable to use a sputtering deposition apparatus capable of performing a film formation process by a roll-to-roll method. When using a sputtering deposition apparatus of the roll-to-roll method in the manufacture of the light control film X, a material is deposited on the long substrate film 10 while the substrate film 10 is running from a pay-out roll to a take-up roll provided in the apparatus, to form the transparent conductive layer 20'. In addition, in the sputtering method, a sputtering deposition apparatus having one deposition chamber may be used, or a sputtering deposition apparatus having multiple deposition chambers arranged in order along the running path of the substrate film 10 may be used.

[0070] Specifically, in the sputtering method, a sputtering gas (inert gas) is introduced under vacuum conditions into a deposition chamber of a sputter deposition apparatus, while a negative voltage is applied to a target placed on a cathode in the deposition chamber. This generates a glow discharge to ionize gas atoms, and the gas ions collide with the target surface at high speed to eject target material from the target surface, and the ejected target material is deposited on the substrate film 10. For example, the conductive oxide sintered body described above for the electrode layer 20 is used as the target material. For example, a rare gas atom is used as the sputtering gas. For example, argon (Ar), krypton (Kr), and xenon (Xe) are used as the rare gas atom.

[0071] The sputtering method is preferably a reactive sputtering method. In the reactive sputtering method, for example, a sputtering gas (inert gas) and oxygen as a reactive gas are introduced into a film formation chamber. In the reactive sputtering method, the ratio of the amount of oxygen introduced to the total amount of sputtering gas and oxygen introduced into the film formation chamber is preferably 1.5 flow% or more, more preferably 2.0 flow% or more, and even more preferably 2.2 flow% or more, from the viewpoint of ensuring the number of carriers in the electrode layer 20. The ratio of the amount of oxygen introduced is preferably 3.2 flow% or less, more preferably 3.0 flow% or less, and even more preferably 2.8 flow% or less, from the viewpoint of ensuring good crystallinity of the electrode layer 20. The ratio of the amount of oxygen introduced is preferably 1.5 to 3.2 flow%, more preferably 2.0 to 3.0 flow%, and even more preferably 2.2 to 2.8 flow%, from the viewpoint of achieving both the number of carriers and the crystallinity of the electrode layer 20.

[0072] The pressure in the deposition chamber during deposition by sputtering (sputter deposition) is, for example, 0.02 Pa, preferably 0.1 Pa or more, more preferably 0.2 Pa or more, and for example, 1 Pa or less, preferably 0.7 Pa or less, more preferably 0.5 Pa or less.

[0073] The film formation temperature in the sputtering method (the temperature of the substrate film 10 during sputtering film formation) is preferably 50° C. or less, more preferably 30° C. or less, even more preferably 10° C. or less, still more preferably 0° C. or less, and even more preferably −5° C. or less, from the viewpoint of properly forming an amorphous transparent conductive layer capable of crystal growth in the subsequent crystallization step. The film formation temperature is, for example, −30° C. or more or −20° C. or more.

[0074] Examples of power sources for applying voltage to the target include DC power sources, AC power sources, MF power sources, and RF power sources. A DC power source and an RF power source may be used in combination as the power source. The absolute value of the discharge voltage during sputtering deposition is, for example, 50 V or more, and, for example, 500 V or less. The horizontal magnetic field strength on the target is, for example, 10 mT or more, and, for example, 100 mT or less.

[0075] Next, as shown in FIG. 2C, the transparent conductive layer 20' (FIG. 2B) on the base film 10 is crystallized by heating to form an electrode layer 20 (crystalline transparent conductive layer) (crystallization step). In this way, the electrode-attached base film Y1 is produced. Examples of heating means include an infrared heater and an oven (heat medium heating oven, hot air heating oven). The heating temperature is preferably 100° C. or higher, more preferably 120° C. or higher, from the viewpoint of ensuring a high crystallization rate. The heating temperature is preferably 200° C. or lower, more preferably 170° C. or lower, and even more preferably 150° C. or lower, from the viewpoint of suppressing the influence of heating on the base film 10. The heating time is, for example, less than 600 minutes, preferably less than 120 minutes, more preferably 90 minutes or lower, and even more preferably 60 minutes or lower, and is, for example, 1 minute or more, preferably 5 minutes or more.

[0076] Next, as shown in Fig. 2D, the light-controlling layer 30 is formed on the electrode layer 20. When an inorganic EC material is used as the material for forming the light-controlling layer 30, the inorganic EC material is formed into a film on the electrode layer 20 by, for example, a dry coating method. As the dry coating method, a sputtering method is preferable. When an organic EC material is used as the material for forming the light-controlling layer 30, the organic EC material is formed into a film on the electrode layer 20 by, for example, a wet coating method.

[0077] On the other hand, an electrode-attached base film Y2 (base film 50, electrode layer 40) is prepared. Specifically, the method is the same as that for preparing the electrode-attached base film Y1 (FIGS. 2A to 2C).

[0078] 3A and 3B, the electrode-attached substrate film Y1 with the light-adjusting layer 30 and the electrode-attached substrate film Y2 are integrated together. Specifically, the electrode-attached substrate films Y1 and Y2 and the light-adjusting layer 30 are integrated together so that the light-adjusting layer 30 is sandwiched between the electrode-attached substrate films Y1 and Y2.

[0079] In this manner, the light control film X can be manufactured. In the light control film X, the light control layer 30 is switched between a non-transparent state (light blocking state) and a transparent state (light non-blocking state) by turning on and off the voltage between the electrode layers 20 and 40. Such a light control film X is, for example, a light control film that is attached to window glass of buildings and vehicles. In a window glass to which the light control film X is attached, the transmittance of light such as visible light through the window glass with the light control film X attached thereto is switched by turning on and off the voltage between the electrode layers 20 and 40.

[0080] As described above, the light-control film X has an electrode layer 20 that is an indium tin composite oxide layer having a tin oxide ratio of 11% by mass or more, and a thickness of 10×10 15 cm -2 The light control film X has a carrier number of 100 or more. Such a light control film X is suitable for ensuring the number of free electrons (the number of carriers) per unit area in the plan view of the electrode layer 20. The greater the number of free electrons in the electrode layer 20, the higher the reflectivity of the electrode layer 20 against heat rays in sunlight, and therefore the higher the heat shielding property of the light control film X. Therefore, the light control film X is suitable for achieving good heat shielding property against sunlight. Such a light control film X is suitable as a light control film for outdoor use. Examples of light control films for outdoor use include light control films for sunroofs of cars such as private cars, and light control films for windows of buildings such as houses and buildings.

[0081] As described above, the light-control film X is preferably an indium tin composite oxide layer having a tin oxide ratio of 11% by mass or more, and has a thickness of 10×10 15 cm -2 The number of carriers is equal to or greater than 1. The light control film X having the electrode layer 40 in addition to the electrode layer 20 helps to achieve good heat shielding properties against sunlight in the light control film. EXAMPLES

[0082] The present invention will be specifically described below with reference to examples. However, the present invention is not limited to the examples. In addition, the specific numerical values ​​of the blending amounts (contents), physical property values, parameters, etc. described below can be replaced with the upper limit (a numerical value defined as "equal to or less than") or lower limit (a numerical value defined as "equal to or more than") of the blending amounts (contents), physical property values, parameters, etc. corresponding to those described in the above-mentioned "Form for carrying out the invention".

[0083] Example 1 First, a roll of polyethylene terephthalate (PET) film (thickness 100 μm, manufactured by Mitsubishi Chemical Corporation) was prepared as a long resin film. Next, a thermosetting resin composition C1 was applied to one side (first side) of the PET film to form a coating film. The resin composition C1 contains 100 parts by mass of melamine resin, 100 parts by mass of alkyd resin, and 50 parts by mass of an organic silane condensate. Next, the coating film on the PET film was heated and thermally cured. The heating temperature was 185° C. The heating time was 1 minute. As a result, a first cured resin layer was formed as an optical adjustment layer having a thickness of 35 nm. Next, a UV-curable resin composition C2 was applied to the other side (second side) of the PET film to form a coating film. Next, the coating film was cured by UV irradiation. As a result, a second cured resin layer was formed as a hard coat (HC) layer having a thickness of 2 μm. In this manner, a base film (first cured resin layer / base film / second cured resin layer) was produced.

[0084] Next, a 125 nm thick amorphous transparent conductive layer was formed on the first cured resin layer of the base film by reactive sputtering (transparent conductive layer formation process). In this process, a roll-to-roll sputter deposition device (DC magnetron sputter deposition device) was used. The device is equipped with a deposition chamber that can perform the deposition process while running the work film by the roll-to-roll method. The conditions for sputter deposition in this process are as follows:

[0085] In sputtering, the ultimate vacuum in the deposition chamber is 0.5×10 -4After the sputtering deposition apparatus was evacuated to a pressure of 0.3 Pa, argon (Ar) as a sputtering gas (inert gas) and oxygen as a reactive gas were introduced into the deposition chamber, and the pressure in the deposition chamber was set to 0.3 Pa. The ratio of the amount of oxygen introduced to the total amount of argon and oxygen introduced into the deposition chamber was 2.4 flow rate %. In addition, a sintered body of indium oxide and tin oxide (ITO with a tin oxide ratio of 12.5 mass %) was used as the target (first target). A DC power supply was used as the power source for applying a voltage to the target. The horizontal magnetic field strength above the target was 90 mT. The deposition temperature (the temperature of the base film on which the transparent conductive layer is laminated) was -8°C. The resistivity of the formed transparent conductive layer (amorphous) was 6.5×10 -4 The value was Ω·cm.

[0086] Next, the amorphous transparent conductive layer was crystallized by heating in a hot air oven (crystallization step). The heating temperature was 150°C. The heating time was 2 hours. As a result, a crystalline transparent conductive layer having a thickness of 125 nm was formed as an electrode layer. The resistivity of the formed transparent conductive layer was 1.7×10 -4 The value was Ω·cm.

[0087] In this manner, a roll of the electrode layer-attached film was produced. This electrode layer-attached film included a base film (second cured resin layer / resin film / first cured resin layer) and an electrode layer on the base film.

[0088] Next, two sheets of electrode layer-attached film were cut out from the roll of electrode layer-attached film. Next, an adhesive (product name "LUCIACS CS9861UA", manufactured by Nitto Denko Corporation) was applied onto the electrode layer of one of the electrode layer-attached films (first electrode layer-attached film) to form an adhesive layer having a thickness of 25 μm as a pseudo-light control layer. Next, the electrode layer side of the other electrode layer-attached film (second electrode layer-attached film) was attached to the adhesive layer. That is, the two electrode layer-attached films were joined via the adhesive layer.

[0089] In this manner, the laminated film of Example 1 was produced. This laminated film is a pseudo-light control film having a laminated structure similar to that of a light control film (this film has a pseudo shape and does not have a light control function). Specifically, the laminated film of Example 1 has a first base film, a first electrode layer having a thickness of 125 nm, a pseudo-light control layer, a second electrode layer having a thickness of 125 nm, and a second base film in this order in the thickness direction.

[0090] Comparative Example 1 A laminated film of Comparative Example 1 was produced in the same manner as the laminated film of Example 1, except for the following.

[0091] In the reactive sputtering method of the transparent conductive layer formation process, a second target was used instead of the first target, and the ratio of the amount of oxygen introduced to the total amount of argon and oxygen introduced into the film formation chamber was set to 3.4 flow rate %. The second target was a sintered body of indium oxide and tin oxide, and was ITO with a tin oxide ratio of 10.0 mass %. In addition, a crystallization process was not performed. The resistivity of the formed transparent conductive layer was 4.8×10 -4 The value was Ω·cm.

[0092] Comparative Example 2 A laminated film of Comparative Example 2 was produced in the same manner as the laminated film of Example 1, except for the following.

[0093] In the transparent conductive layer formation process, a first amorphous transparent conductive layer (11 nm thick) was formed on the first cured resin layer of the base film by reactive sputtering, and then a second amorphous transparent conductive layer (11 nm thick) was formed on the first layer. A roll-to-roll sputter deposition device (DC magnetron sputter deposition device) was used in this process. The device is equipped with a first deposition chamber and a second deposition chamber that can perform the deposition process while running the work film by the roll-to-roll method. The specific resistance of the transparent conductive layer formed after heating in the crystallization process (150°C for 2 hours) was 3.1 x 10 -4 The value was Ω·cm.

[0094] The conditions for sputtering deposition in the first deposition chamber were the same as those for sputtering deposition in Example 1, except for the following: The deposition temperature was set to 80° C. instead of −8° C. As the target, the above-mentioned second target (ITO with a tin oxide ratio of 10 mass %) was used instead of the first target.

[0095] The conditions for sputtering deposition in the second deposition chamber were the same as those for sputtering deposition in Example 1, except for the following: The deposition temperature was 80°C instead of -8°C. As the target, a third target was used instead of the first target. The third target was a sintered body of indium oxide and tin oxide, and was ITO with a tin oxide ratio of 3 mass%.

[0096] The laminated film of Comparative Example 2 has, in this order in the thickness direction, a first base film, a first electrode layer having a thickness of 22 nm, a pseudo-dimming layer, a second electrode layer having a thickness of 22 nm, and a second base film.

[0097] <Thickness of electrode layer> The thickness of the electrode layer of the electrode layer-attached film obtained in the process of producing each laminated film in the examples and comparative examples was measured by observation with a field emission transmission electron microscope (FE-TEM). Specifically, first, a sample for cross-sectional observation of each electrode layer in the examples and comparative examples (first sample) was produced by FIB (Focused Ion Beam) processing (FIB microsampling method). In the FIB microsampling method, a FIB device (product name "FB2200", manufactured by Hitachi) was used, and the acceleration voltage was set to 10 kV. Next, the cross section of the electrode layer in the first sample was observed by FE-TEM, and the thickness of the electrode layer was measured in the observed image. In the observation, a FE-TEM device (product name "JEM-2800", manufactured by JEOL) was used, and the acceleration voltage was set to 200 kV.

[0098] The thickness of the first layer of the electrode layer (transparent conductive layer) in Comparative Example 2 was measured by FE-TEM observation of a cross-sectional observation sample prepared from an intermediate product before the second layer was formed on the first layer. The thickness of the second layer of the electrode layer (transparent conductive layer) in Comparative Example 2 was determined by subtracting the thickness of the first layer from the total thickness of the electrode layer in Comparative Example 2.

[0099] <Specific resistance> The resistivity of the electrode layer (transparent conductive layer) of the electrode layer-attached film obtained in the process of producing each laminated film in the Examples and Comparative Examples was determined as follows. First, the surface resistance of the electrode layer was measured by the four-terminal method in accordance with JIS K7194 (1994). Next, the resistivity (Ω·cm) of the electrode layer (transparent conductive layer) was determined by multiplying the surface resistance value by the thickness of the electrode layer.

[0100] Number of careers The number of carriers (cm) in the electrode layer of the electrode layer-attached film obtained during the production process of each laminated film in the Examples and Comparative Examples -2 ) was measured using a Hall effect measuring device (product name "HL5500PC", manufactured by Bio-Rad). The measurement results are shown in Table 1.

[0101] <Transmittance, reflectance> For each laminate film of the examples and comparative examples, the solar transmittance (Te) and solar reflectance (Re) in the wavelength range of 300 nm to 2500 nm were measured using a spectrophotometer U-4100 (manufactured by HITACHI). In this measurement, the measurement interval was 5 nm. The measurement results are shown in Table 1. Solar radiation refers to radiation in the wavelength range of 300 nm to 2500 nm. The solar transmittance (Te) is calculated by the spectrophotometer from a predetermined product-sum calculation including the spectral transmittance and the spectral solar irradiance in the formula. The solar reflectance (Re) is calculated by the spectrophotometer from a predetermined product-sum calculation including the spectral reflectance and the spectral solar irradiance in the formula.

[0102] <Solar heat gain rate> The solar heat gain coefficient was determined for each laminate film of the Examples and Comparative Examples. Specifically, the solar heat gain coefficient of the laminate film was determined by the following formulas (1) to (3) based on ISO 13837:2021. In formula (1), Tts represents the solar heat gain coefficient and is an index of heat shielding properties.

[0103] Tts = Te + Qi (1) Qi = Ae × {hi / (hi + he)} (2) Ae = 100- Te - Re (3)

[0104] For each laminated film of the examples and comparative examples, formulas (1) to (3) are as follows. Tts indicates the percentage (%) of the total energy passing through the sample when the total energy of the light (irradiated light) irradiated to the sample (laminated film) is taken as 100%. Te indicates the percentage of the energy of the light (transmitted light) that passes through the sample out of the light irradiated to the sample. The solar transmittance obtained in the above measurement was used as Te. Qi represents the secondary heat flux passing through the sample and is calculated by formula (2). The smaller this value, the less the sample transmits heat and the higher the thermal insulation. In formula (2), Ae indicates the percentage of the energy absorbed by the sample out of the energy of the light irradiated to the sample and is calculated by formula (3). hi is a parameter indicating the ease of heat transmission in the sample in the same direction as the light passing direction. hi is set to 8 W / (m 2 ·K) was used. he is a parameter that indicates the ease of heat transfer in the opposite direction to the light transmission direction in the sample. he is 21 W / (m 2 ·K) was used. In formula (3), Re indicates the ratio of the energy of the light reflected by the sample (reflected light) to the light irradiated to the sample. The solar reflectance obtained in the above measurement was used as Re.

[0105] [Table 1] [Explanation of symbols]

[0106] X-light control film H Thickness direction Y1, Y2 Substrate film with electrodes 10,50 Base film 11,51 Resin film 12,52 Cured resin layer 20 Electrode layer (first electrode layer) 30 Photochromic Layer 40 Electrode layer (second electrode layer)

Claims

1. A light-controlling film including a base film, a first electrode layer, a light-controlling layer, and a second electrode layer in this order in a thickness direction, the first electrode layer is an indium tin composite oxide layer having a tin oxide ratio of 12.5 mass% or more and 18 mass% or less, The first electrode layer is 10×10 15 cm -2 A light-controlling film having a carrier number of 1 or more.

2. The light control film according to claim 1 , wherein the second electrode layer is an indium tin composite oxide layer having a tin oxide ratio of 11% by mass or more.

3. The light control film according to claim 1 , wherein the substrate film has a near-infrared absorbing layer and / or a near-infrared reflective layer.

4. A light-controlling film including a base film, a first electrode layer (not including krypton atoms and xenon atoms), a light-controlling layer, and a second electrode layer in this order in a thickness direction, the first electrode layer is an indium tin composite oxide layer having a tin oxide ratio of 11 mass% or more, The first electrode layer is 10×10 15 cm -2 A light-controlling film having a carrier number of 1 or more.

5. The light control film according to claim 4 , wherein the second electrode layer is an indium tin composite oxide layer having a tin oxide ratio of 11% by mass or more.

6. The light control film according to claim 4 , wherein the substrate film has a near-infrared absorbing layer and / or a near-infrared reflective layer.

7. The light control film according to any one of claims 1 to 6, having an average transmittance of 50% or less at wavelengths of 800 nm to 1300 nm.

Citation Information

Patent Citations

  • Electrochromic device

    JP2018120199A

  • Lighting control film

    JP2019101206A

  • Light-transmitting conductive film and light control film

    WO2020031632A1

  • Transparent conductive film and method for producing transparent conductive film

    WO2021187572A1

  • Laminated glass

    WO2022030582A1