Thermally conductive silicone composition
A thermally conductive silicone composition with a specific blend of organopolysiloxane, organohydrogenpolysiloxane, and cyclic organopolysiloxane addresses viscosity and pumping-out issues, ensuring reliable and efficient heat dissipation in electronic components.
Patent Information
- Application Number
- JP2021132142
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-08-16
- Publication Date
- 2024-10-07
- Estimated Expiration
- 2041-08-16
AI Technical Summary
Existing thermally conductive silicone compositions face challenges in maintaining appropriate viscosity, coating workability, and preventing pumping-out, especially when containing a large amount of thermally conductive filler, which affects their reliability and handling.
A thermally conductive silicone composition comprising an addition reaction product of organopolysiloxane, organohydrogenpolysiloxane, and a thermally conductive filler, along with cyclic organopolysiloxane, to maintain viscosity and improve coating workability and pumping-out resistance.
The composition achieves both excellent coating workability and pumping-out resistance, allowing it to be compressed into a thin layer for low thermal resistance, enhancing the reliability of electronic components and facilitating easy handling at room temperature.
Smart Images

Figure 0007562490000001 
Figure 0007562490000002 
Figure 0007562490000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a thermally conductive silicone composition. [Background technology]
[0002] As a heat countermeasure for electronic component packages and power modules, thermal grease is suitable from the viewpoint of heat dissipation performance because it can be compressed thin and has excellent penetration into the gap between the heat generating part and the cooling member. Thermal grease can be broadly divided into two types: "hardening type" that can be hardened after being compressed to the desired thickness, and "non-hardening type" that does not harden and remains in a grease-like form.
[0003] "Hardening" thermal grease is compressed to the desired thickness and then hardened, which makes it less likely for the thermal grease to flow out (pumping out) due to expansion and contraction caused by the thermal history of repeated heating and cooling of the heat-generating part, and increases the reliability of semiconductor packages. However, it also has disadvantages in practical use.
[0004] For example, many addition-curing thermal greases have been proposed in the past as a measure against heat in electronic component packages and power modules (for example, Patent Document 1). However, most of these greases have poor shelf life at room temperature and require freezing or refrigeration, which can make product management difficult. In addition, they require heating for a certain period of time to harden, which leads to a decrease in production efficiency due to the complication and prolongation of the process, and is also not desirable from the perspective of the environmental impact of the heating process.
[0005] Condensation-curing type thermal grease is also listed as one of the "curing types" (for example, Patent Document 2). Condensation-curing type thermal grease thickens and hardens due to moisture in the air, so it can be transported and stored at room temperature as long as it is protected from moisture, and product management is relatively easy. Condensation-curing type thermal grease has the advantage that the curing reaction can proceed without the need for a heating process as long as a certain amount of moisture is present, but since low-boiling point eliminated components are generated during the curing reaction, major issues remain in terms of odor and contamination of electronic components by the eliminated components.
[0006] On the other hand, "non-hardening" thermal grease is generally characterized by its ease of handling, such as the ability to be transported and stored at room temperature, but it has the issue of being prone to the aforementioned pumping-out. Increasing the viscosity of the grease is an effective measure to reduce pumping-out in "non-hardening" thermal grease, but the trade-off is that it reduces ease of application.
[0007] As mentioned above, the use of "curing type" thermal grease is preferable for improving the reliability of electronic component packages and power modules. However, it is difficult to say that this is desirable from the viewpoints of the need for strict temperature control, the complicated curing process, and the environmental impact it places.
[0008] On the other hand, "non-hardening" thermal grease is easy to handle and has a small environmental impact, but is prone to pumping out and requires high viscosity to ensure the reliability of electronic component packages and power modules, resulting in the issue of sacrificing ease of application.
[0009] Furthermore, in order to achieve low thermal resistance by compressing it thinly, it was necessary to precisely control the particle size distribution of the thermally conductive filler.
[0010] Patent Document 3 proposes a non-curable thermally conductive silicone composition that has improved pumping-out resistance by blending a specific ratio of a silicone gel cross-linked product, a hydrolyzable organopolysiloxane, and aluminum nitride particles with a controlled particle size distribution, but further improvement in pumping-out resistance is desired. [Prior art documents] [Patent documents]
[0011] [Patent Document 1] JP 2016-053140 A [Patent Document 2] JP 2011-219664 A [Patent Document 3] Patent Publication No. 2021-098804 Summary of the Invention [Problem to be solved by the invention]
[0012] The present invention has been made in view of the above circumstances, and has as its object to provide a thermally conductive silicone composition which is a "non-curing" thermally conductive silicone composition (such as a thermally conductive grease) that contains a large amount of a thermally conductive filler, yet maintains an appropriate viscosity, resulting in excellent application workability, and also has good pumping-out resistance, and can be compressed thinly to achieve low thermal resistance. [Means for solving the problem]
[0013] In order to solve the above problems, the present invention provides a thermally conductive silicone composition, comprising: (A) an addition reaction product of the following components (a) and (b): (a) At least one aliphatic unsaturated hydrocarbon group per molecule, and a kinetic viscosity of 60 mm at 25°C 2 / s or more, (b) an organohydrogenpolysiloxane having two or more hydrogen atoms bonded to silicon atoms in one molecule: an amount such that the number of hydrogen atoms bonded to silicon atoms (SiH groups) relative to the total number of aliphatic unsaturated hydrocarbon groups in component (a) is 0.3 to 20; (B) at least one thermally conductive filler selected from the group consisting of metals, metal oxides, metal hydroxides, metal nitrides, metal carbides, and allotropes of carbon: in an amount of 10 to 96% by mass based on the total mass of the composition; and (C) a cyclic organopolysiloxane represented by the following general formula (1): 1 to 20 parts by mass per 100 parts by mass of the component (A) [ka] (In the formula, R 1 is a monovalent hydrocarbon group having 1 to 18 carbon atoms, which may have a substituent, and each R 1 may be the same or different. 2is a group having an oxirane ring, and each R 2 may be the same or different. X is an alkylene group having 1 to 20 carbon atoms which may contain a heteroatom, and each X may be the same or different. m is an integer of 3 to 20. The present invention provides a thermally conductive silicone composition comprising:
[0014] The thermally conductive silicone composition of the present invention is a "non-curing" thermally conductive silicone composition that contains a large amount of thermally conductive filler, yet maintains an appropriate viscosity, resulting in excellent application workability, good resistance to pumping out, and the composition can be compressed thinly to achieve low thermal resistance.
[0015] The thermally conductive silicone composition of the present invention further comprises (D) an organopolysiloxane represented by the following general formula (2): [ka] (In the formula, R 3 is a monovalent hydrocarbon group having 1 to 18 carbon atoms, which may have a substituent, and each R 3 may be the same or different, and n is an integer of 5 to 100. It is preferable that the composition contains
[0016] Such a thermally conductive silicone composition can achieve both excellent application workability and resistance to pumping out.
[0017] The thermally conductive silicone composition of the present invention further comprises (E) an organopolysiloxane represented by the following general formula (3): [ka] (In the formula, R 1 , R 2 and X has the same meaning as above. o is an integer of 5 to 200. It is preferable that the composition contains
[0018] Such a thermally conductive silicone composition can achieve both excellent application workability and resistance to pumping out.
[0019] The thermally conductive silicone composition of the present invention preferably has an absolute viscosity at 25°C of at least 200 Pa·s.
[0020] Such a thermally conductive silicone composition can exhibit better pumping-out resistance. Effect of the Invention
[0021] As described above, the thermally conductive silicone composition of the present invention can achieve both excellent application workability and pumping-out resistance, can be compressed thinly, and can achieve low thermal resistance. That is, according to the present invention, it is possible to provide a thermally conductive silicone composition that can respond to the increase in heat generation, the increase in size, and the increase in structural complexity of semiconductor devices in recent years. In addition, the thermally conductive silicone composition of the present invention can be made into a composition such as a "non-curing type" heat dissipation grease that contains a large amount of thermally conductive filler, and by maintaining an appropriate viscosity, it becomes a "non-curing type" composition that can achieve both excellent application workability and pumping-out resistance. And, the thermally conductive silicone composition of the present invention can be transported and stored at room temperature, so it is easy to handle. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0022] As mentioned above, there has been a need for the development of a thermally conductive silicone composition that is a "non-curing" composition that contains a large amount of thermally conductive filler, yet maintains an appropriate viscosity, thereby providing excellent application workability, and also has good pumping-out resistance, and can be compressed thinly to achieve low thermal resistance.
[0023] As a result of intensive research conducted by the present inventors in order to achieve the above-mentioned object, it was discovered that by blending an organopolysiloxane addition reaction product consisting of specific components, a cyclic organopolysiloxane containing a group having an oxirane ring, and a thermally conductive filler in specific ratios, it is possible to obtain a thermally conductive silicone composition which maintains an appropriate viscosity and therefore has excellent application workability, good pumping-out resistance, and which can be compressed thinly to achieve low thermal resistance, and thus completed the present invention.
[0024] That is, the present invention provides a thermally conductive silicone composition, (A) an addition reaction product of the following components (a) and (b): (a) At least one aliphatic unsaturated hydrocarbon group per molecule, and a kinetic viscosity of 60 mm at 25°C 2 / s or more, (b) an organohydrogenpolysiloxane having two or more hydrogen atoms bonded to silicon atoms in one molecule: an amount such that the number of hydrogen atoms bonded to silicon atoms (SiH groups) relative to the total number of aliphatic unsaturated hydrocarbon groups in component (a) is 0.3 to 20; (B) at least one thermally conductive filler selected from the group consisting of metals, metal oxides, metal hydroxides, metal nitrides, metal carbides, and allotropes of carbon: in an amount of 10 to 96% by mass based on the total mass of the composition; and (C) a cyclic organopolysiloxane represented by the following general formula (1): 1 to 20 parts by mass per 100 parts by mass of the component (A) [ka] (In the formula, R 1 is a monovalent hydrocarbon group having 1 to 18 carbon atoms, which may have a substituent, and each R 1 may be the same or different. 2 is a group having an oxirane ring, and each R 2 may be the same or different. X is an alkylene group having 1 to 20 carbon atoms which may contain a heteroatom, and each X may be the same or different. m is an integer of 3 to 20. The thermally conductive silicone composition is characterized by comprising:
[0025] The thermally conductive silicone composition of the present invention can achieve both excellent application workability and pumping-out resistance. Furthermore, since it can be compressed thin and achieve low thermal resistance, the reliability of the electronic components mounted thereon can be improved. The thermally conductive silicone composition of the present invention can be a "non-curing" heat dissipating grease that contains a large amount of a thermally conductive filler. However, since the thermally conductive silicone composition of the present invention maintains an appropriate viscosity, it can be a "non-curing" heat dissipating grease that can achieve both excellent application workability and pumping-out resistance. Furthermore, the thermally conductive silicone composition of the present invention can be transported and stored at room temperature, making it easy to handle.
[0026] The present invention will be described in detail below, but the present invention is not limited thereto.
[0027] [Thermal conductive silicone composition] The present invention relates to a thermally conductive silicone composition that maintains an appropriate viscosity and has good reliability even when it contains a large amount of a thermally conductive filler. The thermally conductive silicone composition of the present invention can be made into a "non-curing" thermal dissipative grease.
[0028] The thermally conductive silicone composition of the present invention is characterized by containing (A) an organopolysiloxane addition reaction product, (B) a thermally conductive filler, and (C) a cyclic organopolysiloxane containing a group having an oxirane ring. In other words, the above components (A) to (C) can be said to be essential components of the thermally conductive silicone composition of the present invention. Furthermore, the thermally conductive silicone composition of the present invention can contain organopolysiloxane components (D) and (E) represented by specific formulas described below, as well as other components, as necessary. These components will be described below.
[0029] Component (A) Component (A) is an organopolysiloxane addition reaction product obtained by a hydrosilylation reaction between components (a) and (b) below: Component (A) serves as the base polymer for the thermally conductive silicone composition of the present invention.
[0030] (a) At least one aliphatic unsaturated hydrocarbon group per molecule, and a kinetic viscosity of 60 mm at 25°C 2 / s or more, (b) Organohydrogenpolysiloxane having two or more hydrogen atoms bonded to silicon atoms in one molecule: an amount such that the number of SiH groups relative to the total number of aliphatic unsaturated hydrocarbon groups in component (a) is 0.3 to 20
[0031] Component (a) has at least one aliphatic unsaturated hydrocarbon group per molecule and has a kinetic viscosity of 60 mm at 25°C. 2 / s or more.
[0032] The molecular structure is not particularly limited, and examples thereof include a linear structure, a branched structure, and a linear structure having a partial branched structure or a cyclic structure. In particular, a linear structure in which the main chain is composed of a repeating diorganosiloxane unit and both ends of the molecular chain are blocked with triorganosiloxy groups is preferred. The organopolysiloxane having a linear structure may also have a partially branched structure or a cyclic structure.
[0033] The kinetic viscosity of component (a) is 60mm at 25°C. 2 / s or more, preferably 100 mm 2 / s or more. 60mm 2 If the kinematic viscosity is less than 1 / s, pumping out may occur due to expansion and contraction caused by the thermal history of repeated heating and cooling of the heat generating part, or the addition reaction product of component (A) may become non-uniform. There is no particular upper limit for the kinematic viscosity of component (a), but for example, it is preferably 50,000,000 mm at 25°C. 2 / s or less. In the present invention, the kinematic viscosity is a value measured at 25° C. using an Ostwald viscometer (the same applies hereinafter).
[0034] The organopolysiloxanes may be used alone or in combination of two or more.
[0035] Component (b) is an organohydrogenpolysiloxane having at least 2 hydrogen atoms bonded to silicon atoms (SiH groups) in one molecule, preferably 3 to 100, and more preferably 5 to 20. Any organohydrogenpolysiloxane may be used as long as the SiH groups in the molecule can undergo a hydrosilylation reaction with the aliphatic unsaturated hydrocarbon groups in component (a) in the presence of a platinum group metal catalyst to form a crosslinked structure.
[0036] The molecular structure of the organohydrogenpolysiloxane is not particularly limited as long as it has the above-mentioned properties, and examples thereof include a linear structure, a branched structure, a cyclic structure, a linear structure having a partially branched structure or a cyclic structure, etc. A linear structure or a cyclic structure is preferred.
[0037] The organohydrogenpolysiloxane preferably has a kinetic viscosity at 25° C. of 1 to 1,000 mm 2 / s, more preferably 10 to 100 mm 2 / s. The kinetic viscosity is 1 mm 2 / s or more, there is no risk of the physical properties of the silicone composition being deteriorated, and 2 If the viscosity is less than or equal to 1 / s, there is no risk of the silicone composition having poor extensibility.
[0038] The organohydrogenpolysiloxanes may be used alone or in combination of two or more.
[0039] The amount of organohydrogenpolysiloxane (b) is such that the number of SiH groups in (b) relative to the total number of aliphatic unsaturated hydrocarbon groups in (a) is 0.3 to 20, preferably 0.5 to 15. If the amount of (b) is less than the lower limit, the addition reaction does not proceed sufficiently, resulting in insufficient crosslinking. If the amount exceeds the upper limit, the crosslinked structure may become nonuniform.
[0040] For example, a conventional platinum group metal catalyst (component (F) described below) can be used to promote the hydrosilylation reaction. Examples include platinum-based, palladium-based, and rhodium-based catalysts, and among these, platinum or platinum compounds, which are relatively easy to obtain, are preferred. Examples include simple platinum, platinum black, chloroplatinic acid, platinum-olefin complexes, platinum-alcohol complexes, platinum coordination compounds, and the like. The platinum group metal catalysts may be used alone or in combination of two or more.
[0041] The amount of platinum group metal catalyst to be added should be an effective amount as a catalyst, that is, an effective amount required to promote the reaction and obtain the silicone gel crosslinked product of component (A). It is preferably 0.1 to 500 ppm, more preferably 1 to 200 ppm, calculated as platinum group metal atoms, based on the total mass of components (a) and (b). If the amount of catalyst to be added is within the above-mentioned preferred range, sufficient catalytic effect can be obtained economically.
[0042] In addition, when obtaining an addition reaction product (silicone gel crosslinked product) of component (A) by hydrosilylation reaction, a reaction inhibitor (component (G) described below) may be added to uniformly proceed with the reaction. The reaction inhibitor may be a conventionally known reaction inhibitor. Examples of such reaction inhibitors include acetylene compounds such as acetylene alcohols (e.g., ethynylmethyldecylcarbinol, 1-ethynyl-1-cyclohexanol, 3,5-dimethyl-1-hexyn-3-ol), various nitrogen compounds such as tributylamine, tetramethylethylenediamine, and benzotriazole, organic phosphorus compounds such as triphenylphosphine, oxime compounds, and organic chloro compounds.
[0043] When a reaction inhibitor is used, the amount of the reaction inhibitor is preferably 0.05 to 5 mass %, more preferably 0.1 to 1 mass %, based on the total mass of components (a) and (b). When the amount of the reaction inhibitor is within the above preferred range, the hydrosilylation reaction can proceed more uniformly.
[0044] The reaction inhibitor may be diluted with organo(poly)siloxane, toluene, or the like to improve dispersibility in the silicone composition.
[0045] (B) Component The component (B) is one or more types of thermally conductive filler selected from the group consisting of metals, metal oxides, metal hydroxides, metal nitrides, metal carbides, and allotropes of carbon. Examples include aluminum, silver, copper, metallic silicon, zinc oxide, magnesium oxide, aluminum oxide (alumina), silicon dioxide, cerium oxide, iron oxide, aluminum hydroxide, cerium hydroxide, aluminum nitride, boron nitride, silicon carbide, diamond, graphite, carbon nanotubes, graphene, etc. These may be used alone or in appropriate combination of two or more types, and a combination of a large particle component and a small particle component (a combination of components having different average particle sizes) is preferable.
[0046] The average particle size of the large particle component is preferably in the range of 0.1 to 300 μm, more preferably in the range of 10 to 200 μm, and even more preferably in the range of 10 to 150 μm. The average particle size of the small particle component is preferably in the range of 0.01 μm to 10 μm, and more preferably in the range of 0.1 to 5 μm. If it is in such a range, the viscosity of the composition will not be too high, the extensibility will be excellent, and the obtained composition will be uniform.
[0047] The ratio of the large particle component to the small particle component is not particularly limited, and is preferably in the range of 9:1 to 1:9 (mass ratio). The shapes of the large particle component and the small particle component are not particularly limited and may be spherical, irregular, acicular, etc.
[0048] The average particle size can be determined, for example, as a volume-based average value (median size) in particle size distribution measurement by laser light diffraction method.
[0049] The blending amount of component (B) is 10 to 96% by mass, preferably 40 to 95.5% by mass, and more preferably 70 to 95% by mass, based on the total mass of the composition. If it is more than 96% by mass, the composition will have poor extensibility, and if it is less than 10% by mass, the composition will have poor thermal conductivity.
[0050] (C) Component Component (C) is a cyclic organopolysiloxane containing an oxirane ring-containing group (epoxy group) and is represented by the following general formula (1), and is effective in improving the pumping-out resistance of the thermally conductive silicone composition of the present invention.
[0051] [ka] (In the formula, R 1 is a monovalent hydrocarbon group having 1 to 18 carbon atoms, which may have a substituent, and each R 1 may be the same or different. 2 is a group having an oxirane ring, and each R 2 may be the same or different. X is an alkylene group having 1 to 20 carbon atoms which may contain a heteroatom, and each X may be the same or different. m is an integer of 3 to 20.
[0052] R 1 is a monovalent hydrocarbon group having 1 to 18 carbon atoms which may have a substituent, is preferably a monovalent saturated aliphatic hydrocarbon group which may have a substituent or a monovalent aromatic hydrocarbon group which may have a substituent, and is more preferably a monovalent saturated aliphatic hydrocarbon group which may have a substituent.
[0053] Specific examples of the monovalent saturated aliphatic hydrocarbon group which may have a substituent include linear alkyl groups such as methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, octyl, nonyl, and decyl groups, branched alkyl groups such as isopropyl, isobutyl, tert-butyl, isopentyl, and neopentyl groups, cycloalkyl groups such as cyclopentyl, cyclohexyl, and cycloheptyl groups, and halogen-substituted alkyl groups such as chloromethyl, 3-chloropropyl, 3,3,3-trifluoropropyl, and bromopropyl groups. The number of carbon atoms is preferably 1 to 10, more preferably 1 to 8, and even more preferably 1 to 6.
[0054] Specific examples of the monovalent aromatic hydrocarbon group which may have a substituent include aryl groups such as a phenyl group and a tolyl group, aralkyl groups such as a benzyl group and a 2-phenylethyl group, and halogen-substituted aryl groups such as an α,α,α-trifluorotolyl group and a chlorobenzyl group. The number of carbon atoms is preferably 6 to 10, more preferably 6 to 8, and even more preferably 6.
[0055] R 1 Among these, preferred are a methyl group, an ethyl group, a 3,3,3-trifluoropropyl group, and a phenyl group, more preferred are a methyl group, an ethyl group, and a phenyl group, and particularly preferred is a methyl group.
[0056] R 2 The group having an oxirane ring is not particularly limited, but examples thereof include oxirane (ethylene oxide) and a group in which one hydrogen atom has been removed from a linear, branched or cyclic hydrocarbon having one or more oxirane rings. The hydrocarbon may be further substituted with a substituent such as a halogen atom, a cyano group, or an aromatic group such as a phenyl group. Examples of such hydrocarbon groups having an oxirane ring include groups in which one hydrogen atom has been removed from epoxides of aromatic-containing hydrocarbons such as epoxyalkanes such as epoxypropane, 1,2-epoxybutane, 2,3-epoxybutane, and 3-methyl-1,2-epoxybutane; epoxycycloalkanes such as epoxycyclopentane, epoxycyclohexane, epoxycycloheptane, epoxycyclooctane, epoxycyclononane, epoxycyclodecane, epoxycycloundecane, and epoxycyclododecane; epoxycycloalkenes such as epoxycyclopentene, epoxycyclohexene, and epoxycycloheptene; and epoxyethylbenzene and 1-phenyl-1,2-epoxypropane. In addition, the group having an oxirane ring may have two or more oxirane rings therein, and may further be substituted with a heteroatom such as an oxygen atom or a nitrogen atom, or a heteroatom may be present between the carbon-carbon bond or the carbon-hydrogen bond. Examples of such a group having an oxirane ring include groups obtained by removing one hydrogen atom from glycidyl ethers such as diepoxycyclohexane, epoxycyclohexanol, epoxycyclohexanone, methyl glycidyl ether, ethyl glycidyl ether, ethylene glycol monoglycidyl ether, and propanediol monoglycidyl ether, and epoxypiperidine.
[0057] R 2 Examples of the group having an oxirane ring include those represented by the following formulae (4) and (5).
[0058] [ka]
[0059] X is an alkylene group having 1 to 20 carbon atoms, preferably 1 to 8 carbon atoms, which may contain a heteroatom, and the structure of X is not particularly limited, such as linear or branched, but is preferably linear. Examples of heteroatoms include oxygen atoms, nitrogen atoms, and sulfur atoms. Examples of X include alkylene groups which may have an ether bond, a thioether bond, an ester group, an amide group, and the like, and specific examples thereof include those shown below.
[0060] -(CH2) x - (x is an integer from 1 to 20.) -CH2CH2CH2OCH2-
[0061] R 2 Examples of the -X group as a whole include a 3-glycidoxypropyl group, a 2-(3,4-epoxycyclohexyl)ethyl group, a 5,6-epoxyhexyl group, and a 9,10-epoxydecyl group.
[0062] m is an integer of 3 to 20, preferably 4 to 10. If the value of m is less than 3, the pumping-out resistance is insufficient. If the value of m is more than 20, the viscosity increases significantly, making blending difficult, and there is a risk of the viscosity of the resulting composition increasing significantly.
[0063] The blending amount of component (C) is 1 to 20 parts by mass, and preferably 3 to 15 parts by mass, per 100 parts by mass of component (A). If it exceeds 20 parts by mass, the composition may significantly thicken, and if it is less than 1 part by mass, the effect of improving pumping-out resistance is poor.
[0064] The component (C) may be used alone or in combination of two or more different compounds.
[0065] (D) Component The thermally conductive silicone composition of the present invention may further contain (D) an organopolysiloxane represented by general formula (2) below. Component (D) is used to treat the surface of the thermally conductive filler and plays a role in assisting in achieving high loadings of the filler.
[0066] [ka] (In the formula, R 3 is a monovalent hydrocarbon group having 1 to 18 carbon atoms, which may have a substituent, and each R 3 may be the same or different, and n is an integer of 5 to 100.
[0067] R 3 is a monovalent hydrocarbon group having 1 to 18 carbon atoms which may have a substituent, is preferably a monovalent saturated aliphatic hydrocarbon group which may have a substituent, or a monovalent aromatic hydrocarbon group which may have a substituent, and is more preferably a monovalent saturated aliphatic hydrocarbon group which may have a substituent.
[0068] Specific examples of the monovalent saturated aliphatic hydrocarbon group which may have a substituent include linear alkyl groups such as methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, octyl, nonyl, and decyl groups, branched alkyl groups such as isopropyl, isobutyl, tert-butyl, isopentyl, and neopentyl groups, cycloalkyl groups such as cyclopentyl, cyclohexyl, and cycloheptyl groups, and halogen-substituted alkyl groups such as chloromethyl, 3-chloropropyl, 3,3,3-trifluoropropyl, and bromopropyl groups. The number of carbon atoms is preferably 1 to 10, more preferably 1 to 8, and even more preferably 1 to 6.
[0069] Specific examples of the monovalent aromatic hydrocarbon group which may have a substituent include aryl groups such as a phenyl group and a tolyl group, aralkyl groups such as a benzyl group and a 2-phenylethyl group, and halogen-substituted aryl groups such as an α,α,α-trifluorotolyl group and a chlorobenzyl group. The number of carbon atoms is preferably 6 to 10, more preferably 6 to 8, and even more preferably 6.
[0070] R 3 Among these, preferred are a methyl group, an ethyl group, a 3,3,3-trifluoropropyl group, and a phenyl group, more preferred are a methyl group, an ethyl group, and a phenyl group, and particularly preferred is a methyl group.
[0071] n is an integer of 5 to 100, preferably 5 to 80, and more preferably 10 to 60. When the value of n is 5 or more, oil bleeding from the silicone composition is suppressed and pumping-out resistance is improved. When the value of n is 100 or less, wettability with the filler is sufficient, and the viscosity of the composition does not increase, resulting in a deterioration in application workability.
[0072] When component (D) is blended, the blending amount is preferably 0.5 to 10 mass %, and more preferably 1.0 to 8.0 mass %, of the total composition. Within this range, the thermally conductive silicone composition can be brought into an appropriate viscosity range, and the composition will have better pumping-out resistance.
[0073] The component (D) may be used alone or in combination of two or more types.
[0074] (E) Component The thermally conductive silicone composition of the present invention may further contain (E) an organopolysiloxane represented by the following general formula (3): Component (E) is used to treat the surface of the thermally conductive filler, and plays a role in assisting in achieving high loadings of the filler.
[0075] [ka] (In the formula, R 1 , R 2 and X has the same meaning as above. o is an integer of 5 to 200.
[0076] R in the above formula (3) 1 are independently unsubstituted or substituted monovalent hydrocarbon groups having 1 to 18 carbon atoms, and R 1 Examples of the alkyl group include the same groups as those exemplified in the above, and a methyl group is particularly preferred.
[0077] R in the above formula (3) 2 is a substituent (epoxy group) having an oxirane ring in the structural formula, and R 2 The same examples as those exemplified in are included.
[0078] X in the above formula (3) is an alkylene group having 1 to 20 carbon atoms which may contain a heteroatom, and examples thereof include the same as those exemplified for X in the above formula (1).
[0079] o is an integer of 5 to 200, preferably 10 to 100. When the value of o is 5 or more, the reliability is not impaired due to excessive oil bleeding from the silicone composition. When the value of o is 200 or less, the wettability with the filler is sufficient.
[0080] When component (E) is blended, the blending amount is preferably 0.5 to 10 mass %, and more preferably 1.0 to 8.0 mass %, of the total composition. Within this range, the thermally conductive silicone composition can be brought into an appropriate viscosity range, and the composition will have better pumping-out resistance.
[0081] The component (E) may be used alone or in combination of two or more different compounds.
[0082] Other Ingredients The thermally conductive silicone composition of the present invention may contain any additives in addition to the platinum group metal catalyst (component (F)) and reaction inhibitor (component (G)) described above. For example, to prevent deterioration of the composition, a conventionally known antioxidant such as 2,6-di-tert-butyl-4-methylphenol may be contained as necessary. Furthermore, dyes, pigments, flame retardants, anti-settling agents, thixotropy improvers, etc. may be blended as necessary.
[0083] Step of preparing a thermally conductive silicone composition The method for producing the heat conductive silicone composition of the present invention will be described. The method for producing the silicone composition of the present invention is not particularly limited, but examples include a method in which the above-mentioned components (A) to (C), as well as the above-mentioned components (D) and (E) that are mixed as necessary and other components, are mixed using a mixer such as Trimix, Twinmix, Planetary Mixer (all registered trademarks of mixers manufactured by Inoue Seisakusho Co., Ltd.), Ultra Mixer (registered trademarks of mixers manufactured by Mizuho Kogyo Co., Ltd.), or Hivis Dispermix (registered trademarks of mixers manufactured by Tokushu Kika Kogyo Co., Ltd.).
[0084] The thermally conductive silicone composition of the present invention may be mixed while being heated. There are no particular limitations on the heating conditions, but the temperature is usually 25 to 220°C, preferably 40 to 200°C, and particularly preferably 50 to 200°C, and the heating time is usually 3 minutes to 24 hours, preferably 5 minutes to 12 hours, and particularly preferably 10 minutes to 6 hours. Degassing may also be performed during heating.
[0085] The organopolysiloxane addition reaction product of component (A) may be one that has been prepared in advance by subjecting the previously described components (a) and (b) to a hydrosilylation reaction, or it may be prepared by subjecting the organopolysiloxane addition reaction product to a hydrosilylation reaction during the heating and mixing step in which the thermally conductive silicone composition is produced.
[0086] The thermally conductive silicone composition of the present invention preferably has an absolute viscosity measured at 25° C. of at least 200 Pa·s, and more preferably from 200 to 2,000 Pa·s. If the absolute viscosity at 25° C. is 200 Pa·s or more, better pumping-out resistance can be exhibited, and if it is 2,000 Pa·s or less, there is no risk of deterioration in application workability.
[0087] Furthermore, the thermally conductive silicone composition of the present invention will typically have a thermal conductivity of 1.0 to 15 W / m·K.
[0088] In the present invention, the absolute viscosity of the thermally conductive silicone composition is a value measured at 25°C using a constant test force extrusion capillary rheometer, and the thermal conductivity is a value measured using the hot disc method (ISO 22007-2).
[0089] The thermally conductive silicone composition of the present invention described above can achieve both excellent application workability and pumping-out resistance. Furthermore, since it can be compressed thin and achieve low thermal resistance, the reliability of the electronic components mounted thereon can be improved. In addition, the thermally conductive silicone composition of the present invention can be made into a "non-curing" heat dissipating grease containing a large amount of thermally conductive filler, and by maintaining an appropriate viscosity, it can become a "non-curing" heat dissipating grease that can achieve both excellent application workability and pumping-out resistance. In addition, the thermally conductive silicone composition of the present invention can be transported and stored at room temperature, making it easy to handle. EXAMPLES
[0090] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to the following examples. The kinetic viscosity of each component is the value measured at 25°C using an Ostwald viscometer. The average particle size is the volume-based average value (median size) measured by laser light diffraction method.
[0091] [Preparation of Thermally Conductive Silicone Composition] First, the following components were prepared to prepare the thermally conductive silicone composition of the present invention.
[0092] Component (A) A-1: An addition reaction product prepared by subjecting the following components (a-1) and (b-1) to a hydrosilylation reaction in the heating and mixing step of producing a thermally conductive silicone composition. (The number of SiH groups in component (b-1) relative to the total number of aliphatic unsaturated hydrocarbon groups in component (a-1) = 0.8)
[0093] (a-1): Both ends are blocked with dimethylvinylsilyl groups, and the kinetic viscosity at 25°C is 600mm 2 / s Dimethylpolysiloxane (b-1): Methylhydrogendimethylpolysiloxane represented by the following formula (6) (kinematic viscosity at 25°C: 100 mm 2 / s)
[0094] [ka] (In the formula, the order of the siloxane units in the parentheses is not specified.)
[0095] A-2: An addition reaction product prepared by subjecting the above component (a-1), the following component (a-2), and the above component (b-1) to a hydrosilylation reaction in the heating and mixing step of producing a thermally conductive silicone composition. (The number of SiH groups in component (b-1) relative to the total number of aliphatic unsaturated hydrocarbon groups in components (a-1) and (a-2) = 13, and the total number of aliphatic unsaturated hydrocarbon groups in component (a-1):total number of aliphatic unsaturated hydrocarbon groups in component (a-2) = 56:44)
[0096] (a-2): Dimethyldiphenylpolysiloxane having one end blocked with a dimethylvinylsilyl group, as represented by the following formula (7) (kinematic viscosity at 25°C: 700 mm 2 / s)
[0097] [ka] (In the formula, p / (p+q)=0.05, the order of the siloxane units in the parentheses is not fixed, and Ph represents a phenyl group.)
[0098] (B) Component B-1: Aluminum nitride particles with an average particle size of 120 μm B-2: Aluminum nitride particles with an average particle size of 60 μm B-3: Aluminum nitride particles with an average particle size of 30 μm B-4: Aluminum nitride particles with an average particle size of 20 μm B-5: Aluminum nitride particles with an average particle size of 1 μm
[0099] (C) Component C-1: A cyclic organopolysiloxane represented by the following formula (8) (kinematic viscosity at 25°C: 3,000 mm 2 / s)
[0100] [ka]
[0101] (D) Component D-1: Organopolysiloxane represented by the following formula (9) (kinematic viscosity at 25°C: 30 mm 2 / s)
[0102] [ka]
[0103] (E) Component E-1: Organopolysiloxane represented by the following formula (10) (kinematic viscosity at 25°C: 35 mm 2 / s)
[0104] [ka]
[0105] Other Ingredients (F) Component (platinum group metal catalyst) F-1: A solution in which platinum-divinyltetramethyldisiloxane complex is dissolved in the above component (a-1) (platinum atom content: 1% by mass as platinum atoms).
[0106] Component (G) (reaction regulator) G-1: Ethynylcyclohexanol (formula (11) below)
[0107] [ka]
[0108] [Examples 1 to 6, Comparative Examples 1 to 4] Preparation of Thermally Conductive Silicone Composition The above components (A) to (G) were blended in the amounts shown in Tables 1 and 2 below, by the method shown below, to prepare a thermally conductive silicone composition.
[0109] Component (a-1) or both components (a-1) and (a-2) of component (A), component (B), component (D), and component (E) were added to 5 liters of Trimix (manufactured by Inoue Seisakusho Co., Ltd.) and mixed under reduced pressure at 170° C. for 1 hour. After cooling to below 40° C., the remaining components (b-1), (C), (F), and (G) of component (A) were added to this mixture and mixed at 150° C. for 2 hours to prepare a thermally conductive silicone composition.
[0110] For each of the silicone compositions obtained above, the absolute viscosity and thermal conductivity were measured and resistance to pumping out was evaluated according to the methods described below. The results are shown in Tables 1 and 2.
[0111] [Absolute Viscosity] The absolute viscosity of each silicone composition was measured at 25° C. using a constant test force extrusion type capillary rheometer CFT-500EX manufactured by Shimadzu Corporation.
[0112] [Thermal Conductivity] Each silicone composition was wrapped in kitchen wrap, and the thermal conductivity was measured using the hot disk method (ISO 22007-2) using a Kyoto Electronics Manufacturing Co., Ltd. TPS-2500S.
[0113] [Pumping-out resistance] 0.3 ml of each composition was sandwiched between an aluminum plate and a glass plate with a 0.5 mm spacer between them, and compressed for 15 minutes using two clips of 1.8 kgf (17.65 N). This was placed vertically in a thermal shock tester that repeatedly cycled between -40°C / 30 minutes and 125°C / 30 minutes, and removed after 500 cycles. The vertical movement distance at this point was measured. This thermal history caused the composition to repeatedly expand and contract. The less likely the silicone composition was to flow out vertically downwards due to this, that is, the smaller the vertical movement distance, the better the pumping-out resistance was evaluated to be.
[0114] [Table 1]
[0115] [Table 2]
[0116] From the results in Tables 1 and 2, it is clear that the silicone compositions of Examples 1 to 6, which satisfy the requirements of the present invention, have a small vertical migration distance, which is an index of pumping-out resistance, and are less likely to flow out (pump out) of the silicone composition due to expansion and contraction caused by thermal history. In addition, the silicone compositions have an appropriate viscosity, which makes them easy to apply, and they can be compressed thinly to achieve low thermal resistance.
[0117] On the other hand, with the silicone compositions of Comparative Examples 1 to 4, which did not contain component (C), the vertical migration distance, which is an index of pumping-out resistance, was large, or a paste-like composition was not obtained.
[0118] Therefore, the thermally conductive silicone composition of the present invention is able to achieve good pumping-out resistance even though it is a "non-curing" thermal grease that contains a large amount of thermally conductive filler. In other words, it is possible to provide a thermally conductive silicone composition that can accommodate the increased heat generation, larger size, and more complex structures of recent semiconductor devices.
[0119] The present invention is not limited to the above-described embodiment. The above-described embodiment is merely an example, and anything that has substantially the same configuration as the technical idea described in the claims of the present invention and exhibits similar effects is included in the technical scope of the present invention.
Claims
1. A non-curable thermally conductive silicone composition, comprising: (A) an addition reaction product of the following components (a) and (b): (a) At least one aliphatic unsaturated hydrocarbon group per molecule and a kinetic viscosity at 25°C of 60 mm 2 / s or more (provided that the organopolysiloxane is represented by the following average formula (2): (R 1 3 SiO 1 / 2 ) p (R 2 a R 1 3-a SiO 1 / 2 ) q (SiO 4 / 2 ) r (2) (In the formula, R 1 each independently represents an unsubstituted or substituted monovalent hydrocarbon group having no addition reactive carbon-carbon unsaturated bond, R 2 represents an alkenyl group, p, q, and r represent numbers that satisfy p>0, q>0, r>0, and (p+q+r)=1, and a represents 1 or 2. R 1 and R 2 in the formula apply only to the formula itself.) (b) an organohydrogenpolysiloxane having two or more hydrogen atoms bonded to silicon atoms per molecule: an amount such that the number of hydrogen atoms bonded to silicon atoms (SiH groups) relative to the total number of aliphatic unsaturated hydrocarbon groups in component (a) is 0.3 to 20, (B) at least one thermally conductive filler selected from the group consisting of metals, metal oxides, metal hydroxides, metal nitrides, metal carbides, and allotropes of carbon: in an amount of 10 to 96% by mass based on the total mass of the composition; and (C) a cyclic organopolysiloxane represented by the following general formula (1): 1 to 20 parts by weight per 100 parts by weight of component (A) 【Chemistry 1】 (In the formula, R 1 is a monovalent hydrocarbon group having 1 to 18 carbon atoms, which may have a substituent, and each R 1 may be the same or different. 2 is a group having an oxirane ring, and each R 2 may be the same or different. X is an alkylene group having 1 to 20 carbon atoms which may contain a heteroatom, and each X may be the same or different. m is an integer of 3 to 20. and having an absolute viscosity at 25°C of 200 Pa·s to 2,000 Pa·s.
2. Furthermore, (D) an organopolysiloxane represented by the following general formula (2): in an amount of 0.5 to 10% by mass based on the total mass of the composition, 【Chemistry 2】 (In the formula, R 3 is a monovalent hydrocarbon group having 1 to 18 carbon atoms, which may have a substituent, and each R 3 may be the same or different; n is an integer from 5 to 100.
2. The non-curable thermally conductive silicone composition according to claim 1, which comprises
3. Furthermore, (E) an organopolysiloxane represented by the following general formula (3): in an amount of 0.5 to 10% by mass based on the total mass of the composition, 【Chemistry 3】 (In the formula, R 1 , R 2 and X has the same meaning as above. o is an integer of 5 to 200.
3. The non-curable thermally conductive silicone composition according to claim 1, further comprising:
Citation Information
Patent Citations
Application of modified cyclosiloxane in preparation of thixotropic additional liquid silicone rubber
CN103923464A
Room-temperature moisture-thickened heat-conductive silicone grease composition
JP2011219664A
Silicone composition
JP2016053140A
Addition reaction curing type silicone adhesive composition
JP2020169254A
Heat-conductive silicone composition
JP2021098804A