Modified nanocrystalline ribbons, methods for making and uses thereof - Patents.com

The modification of nanocrystalline ribbons through a specific manufacturing process addresses issues of non-uniformity and high losses in wireless charging systems, enhancing power transmission efficiency by improving insulation and magnetic field distribution.

JP7562839B2Active Publication Date: 2024-10-07HENGDIAN GRP DMEGC MAGNETICS CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2023512348
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-12-22
Filing Date
2021-04-20
Publication Date
2024-10-07
Estimated Expiration
2041-04-20

AI Technical Summary

Technical Problem

Nanocrystalline composite magnetic sheets used in wireless charging systems suffer from non-uniform microstructure, poor insulation, and high eddy current losses, leading to inefficient power transmission due to uneven magnetic field distribution and reduced magnetic permeability.

Method used

A manufacturing process involving roll press treatment, acid etching, alkali cleaning, and micro-oxidation to modify nanocrystalline ribbons, forming a composite structure with graded magnetic permeability to improve insulation and reduce eddy current losses.

Benefits of technology

The modified nanocrystalline ribbons enhance power transmission efficiency by optimizing magnetic field distribution and reducing losses, resulting in a more efficient wireless charging system.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007562839000013
    Figure 0007562839000013
  • Figure 0007562839000001
    Figure 0007562839000001
  • Figure 0007562839000002
    Figure 0007562839000002
Patent Text Reader

Abstract

The present invention discloses a modified nanocrystalline ribbon, its manufacturing method, and its use, which includes: performing a roll press treatment on a nanocrystalline ribbon with double-sided tape attached to one side to obtain a pulverized nanocrystalline ribbon; performing an acid etching surface treatment on the pulverized nanocrystalline ribbon; performing an alkali washing surface treatment on the acid-etched nanocrystalline ribbon; sequentially washing the alkali-washed nanocrystalline ribbon with water and alcohol, followed by drying; and performing a micro-oxidation treatment on the dried nanocrystalline ribbon to obtain a modified nanocrystalline ribbon.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present application is in the field of materials technology and relates to wireless charging materials, their manufacture and use, such as modified nanocrystalline ribbons, their manufacture and use. [Background technology]

[0002] In recent years, wireless charging technology is becoming the standard configuration of smartphones. The receiving end of wireless charging for mobile phones mainly consists of two parts: a coil and a magnetic sheet. Among them, the coil mainly receives the excitation magnetic field from the transmitting end and converts it into AC current. The magnetic sheet mainly plays a magnetic blocking and permeability role, improving the charging efficiency of the entire system while avoiding magnetic field leakage. Currently, wireless charging for mobile phones mainly adopts the Qi standard, and the operating frequency is 100-200kHz. The main materials of the magnetic sheet of the receiving end include ferrite and nanocrystalline alloy. Among them, the nanocrystalline magnetic sheet is becoming mainstream because of its high saturation magnetization and high magnetic permeability.

[0003] Nanocrystalline alloy materials have low resistivity and high eddy current loss at high frequencies. Therefore, in order to improve the resistivity and high frequency properties of nanocrystalline materials and reduce the eddy current loss, the industry usually uses a method of pulverizing nanocrystalline ribbons to solve the problem. The pulverization of nanocrystalline ribbons is generally achieved by roll pressing with two metal rolls, and the degree of pulverization is controlled by the roll pressing pattern, pressure and number of roll pressings to adjust the permeability real part and permeability imaginary part of the ribbon, and finally, several pulverized ribbon units are pasted with double-sided tape to form a composite magnetic sheet for the receiving end of wireless charging.

[0004] CN108597793A discloses a high performance, high frequency response composite magnetic material having a laminated structure in which an underlayer material, a top layer material, and an intermediate layer material are laminated in order. The underlayer material is a layer of black or matte black non-transparent double-sided pressure-sensitive adhesive, the top layer material is a layer of black or matte black single-sided adhesive, and the intermediate layer material is a magnetic material laminated structure in which any two or three types of soft magnetic materials selected from ferrite, nanocrystalline, and amorphous are alternately laminated.

[0005] CN108231381A discloses a magnetic permeable sheet structure for wireless charging, which includes a first magnetic layer and a second magnetic layer stacked in order, and the magnetic permeability and thermal conductivity of the first magnetic layer are respectively smaller than those of the second magnetic layer. By performing gradient setting for the magnetic permeability of the first magnetic layer and the second magnetic layer, the magnetic permeability of the second magnetic layer is set high to improve the blocking performance of the magnetic permeable sheet structure, and the magnetic permeability of the first magnetic layer is set low to reduce the generation of eddy currents, and the thermal conductivity of the first magnetic layer and the second magnetic layer gradually increases, thereby improving the temperature uniformity and heat dissipation performance of the magnetic permeable sheet structure.

[0006] Although the composite magnetic sheet structure made of nanocrystalline ribbon is widely used in the wireless charging system of mobile phones, there are some problems and room for optimization, such as the following. The microstructure of the nanocrystalline ribbon that has been pulverized is not sufficiently uniform, the shape and size of the pulverized units are not uniform, and the insulation uniformity between each pulverized unit is also poor, so that the magnetic field is concentrated at the sharp corners and the contact points of each pulverized unit, resulting in an uneven magnetic field distribution and even serious local heating. Since the nanocrystalline material has good electrical conductivity, even if it is pulverized, the eddy current loss of the magnetic sheet is relatively serious, which greatly restricts the further improvement of the efficiency of the entire system. If the nanocrystalline ribbon is pulverized excessively, the pulverized unit can be made small, which effectively reduces the influence of the eddy current effect, but at the same time, the permeability is significantly reduced, and both the magnetic shielding effect and the magnetic permeability effect are deteriorated. The frequency characteristics of the nanocrystalline ribbon, especially the loss characteristics at high frequencies, are not particularly good due to the limitations of the material itself, specifically, the imaginary part of the permeability of the nanocrystalline ribbon is high, which further affects the efficiency of the entire wireless charging system. Currently, most nanocrystalline composite magnetic sheets are made up of nanocrystalline ribbons with similar performance and specifications, and the structure still has room for further optimization.

[0007] In response, there is a need to provide wireless charging materials that have high magnetic permeability and low loss characteristics. Summary of the Invention [Problem to be solved by the invention]

[0008] The present application aims to provide a modified nanocrystalline ribbon, its manufacturing method and use, which has a lower imaginary part of magnetic permeability and lower loss, which further contributes to the wireless charging system obtaining high power transmission efficiency, and when applied to a nanocrystalline composite structure magnetic sheet, can improve the power transmission efficiency of the wireless charging system. [Means for solving the problem]

[0009] In order to achieve the object of the present invention, the present application provides the following technical solutions.

[0010] In a first aspect, the present application provides a method for producing a method for manufacturing a semiconductor device comprising: (1) performing a roll press process on a nanocrystalline ribbon having a double-sided tape attached to one side thereof to obtain a finely pulverized nanocrystalline ribbon; (2) subjecting the pulverized nanocrystalline ribbons obtained in step (1) to an acid etching surface treatment; (3) subjecting the acid-etched surface-treated nanocrystalline ribbons of step (2) to an alkaline cleaning surface treatment; (4) washing the nanocrystalline ribbons that have been subjected to the alkaline washing surface treatment in step (3) with water and then with alcohol, followed by drying; (5) performing a micro-oxidation treatment on the dried nanocrystalline ribbon of step (4) to obtain a modified nanocrystalline ribbon.

[0011] The acid etching surface treatment can etch the nanocrystalline material, and compared with the smooth surface of the nanocrystalline ribbon, the acid etching is more likely to occur at the cracks and sharp corners of the pulverized material, which can improve the insulation between each pulverized unit and restore the shape of the pulverized unit.

[0012] The alkaline washing surface treatment can chemically react with the remaining acidic solution. Since the gaps between each fine grinding unit are small, it is difficult to remove the excess acidic solution. The alkaline washing surface treatment can effectively solve this problem.

[0013] The water washing can remove salts generated by the reaction between the alkaline and acidic solutions, but the water-washed nanocrystalline ribbons are prone to rust or excessive oxidation during the drying process. The alcohol washing effectively dilutes the deionized water with absolute ethanol, avoiding the reaction between the deionized water and the nanocrystalline ribbons during the drying process.

[0014] Through the micro-oxidation treatment, a thin oxide film layer can be formed on the surface of the nanocrystalline ribbon and on the cross section of each pulverized unit, which can effectively improve the resistivity of the nanocrystalline ribbon and reduce the eddy current loss.

[0015] Preferably, the nanocrystalline ribbon comprises 73.5 wt% Fe, 13.5 wt% Si, 9 wt% B, 3 wt% Nb and 1 wt% Cu. 73.5 S 13.5 It may be expressed as B9Nb3Cu, where the numerical subscripts indicate the percentage of each element relative to the total mass of the nanocrystalline ribbon.

[0016] The nanocrystalline ribbon according to the present application is an annealed nanocrystalline ribbon, and the real part of the magnetic permeability and the imaginary part of the magnetic permeability of the resulting nanocrystalline ribbon vary depending on the annealing conditions.

[0017] Preferably, the pressure of the roll press in step (1) is 60 to 70 kg, and may be, for example, 60 kg, 61 kg, 62 kg, 63 kg, 64 kg, 65 kg, 66 kg, 67 kg, 68 kg, 69 kg or 70 kg, but is not limited to the recited numerical values, and other unrecited numerical values ​​within the numerical range may be used as well.

[0018] The roll pressing in the present application is performed using a roll pressing machine well known in the art, in which the round roll in the roll pressing machine and the nanocrystalline ribbon are in line contact, and the roll pressing pressure is set to 60 to 70 kg, thereby enabling the nanocrystalline ribbon to be finely ground.

[0019] Preferably, the number of times of roll pressing in step (1) is 1 to 5 times, and may be, for example, 1 time, 2 times, 3 times, 4 times, or 5 times.

[0020] Preferably, the acid etching surface treatment in step (2) is to apply an acid solution to the surface of the pulverized nanocrystalline ribbons to perform surface acid treatment, and then wash with deionized water after the treatment is completed.

[0021] Preferably, the acidic solution is a hydrochloric acid solution having a mass fraction of 0.5 to 1.2 wt %.

[0022] The mass fraction of the hydrochloric acid solution used in the acid etching surface treatment is 0.5-1.2 wt%, and may be, for example, 0.5 wt%, 0.6 wt%, 0.7 wt%, 0.8 wt%, 0.9 wt%, 1 wt%, 1.1 wt%, or 1.2 wt%, but is not limited to the recited values, and other unrecited values ​​within the numerical range may be used as well.

[0023] Preferably, the time for the surface acid treatment is 3 to 8 min, and may be, for example, 3 min, 4 min, 5 min, 6 min, 7 min or 8 min, but is not limited to the listed values, and other unlisted values ​​within the numerical range may be used as well.

[0024] If the mass fraction of the hydrochloric acid solution used is too low and / or the time of the surface acid treatment is too short, it cannot perform an effective acid etching action. If the mass fraction of the hydrochloric acid solution is too high and / or the time of the surface acid treatment is too long, it will cause excessive corrosion and the magnetic permeability of the nanocrystalline ribbon will be poor. Although the eddy current loss can be reduced to a certain extent, at the same time, the hysteresis loss will increase significantly, so that the total loss will increase instead of decrease.

[0025] Preferably, the alkaline cleaning surface treatment in step (3) is to apply an alkaline solution to the surface of the acid-etching surface-treated nanocrystalline ribbon to perform surface alkaline treatment, and then wash with deionized water after the treatment is completed.

[0026] Preferably, the alkaline solution comprises any one or a combination of at least two of a sodium bicarbonate solution, a potassium hydroxide solution or a sodium hydroxide solution, preferably a sodium hydroxide solution.

[0027] Preferably, the mass fraction of the sodium hydroxide solution is 0.5-2 wt%, and may be, for example, 0.5 wt%, 0.8 wt%, 1 wt%, 1.2 wt%, 1.5 wt%, 1.6 wt%, 1.8 wt% or 2 wt%, but is not limited to the recited values ​​and other unrecited values ​​within the numerical range may be used as well.

[0028] Preferably, the time of the surface alkali treatment is 5 to 10 min, and may be, for example, 5 min, 6 min, 7 min, 8 min, 9 min or 10 min, but is not limited to the recited values, and other unrecited values ​​within the numerical range may be used as well.

[0029] If the mass fraction of sodium hydroxide solution used is too low and / or the time of surface alkali treatment is too short, the purpose of removing the acid solution cannot be achieved. If the concentration of sodium hydroxide solution is too high, the local chemical reaction will be strong and the reaction will be uneven. If the time of surface alkali treatment is too long, the test and production costs will be wasted.

[0030] Preferably, the number of water washes in step (4) is at least 3, and may be, for example, 3, 4, 5, 6, 7, or 8, but is not limited to the recited numbers, and other unrecited numbers within the numerical range may be used as well.

[0031] Preferably, the alcohol wash in step (4) is at least 3 washes with absolute ethanol, and may be, for example, 3, 4, 5, 6, 7 or 8 washes, but is not limited to the recited numbers, and other unrecited numbers within the numerical range may be used as well.

[0032] Preferably, the micro-oxidation treatment in step (5) is carried out in an oxygen gas atmosphere having an oxygen gas concentration of 85 vol % or more.

[0033] The micro-oxidation treatment is performed in an oxygen gas atmosphere, and the oxygen gas concentration in the oxygen gas atmosphere is 85 vol% or more, and may be, for example, 85 vol%, 90 vol%, 92 vol%, 95 vol%, 98 vol% or 100 vol%, but is not limited to the recited numerical values, and other unrecited numerical values ​​within the numerical range may be used as well.

[0034] Preferably, the temperature of the micro-oxidation treatment in step (5) is 60-85°C, and may be, for example, 60°C, 65°C, 70°C, 75°C, 80°C or 85°C, but is not limited to the recited values, and other unrecited values ​​within the numerical range may be used as well.

[0035] Preferably, the time of the micro-oxidation treatment in step (5) is 15-30 min, and may be, for example, 15 min, 18 min, 20 min, 25 min, 28 min or 30 min, but is not limited to the recited values, and other unrecited values ​​within the numerical range may be used as well.

[0036] Through the micro-oxidation treatment, a thin oxide film layer can be formed on the surface of the nanocrystalline ribbon and on the cross section of each pulverized unit, which can effectively improve the resistivity of the nanocrystalline ribbon and reduce the eddy current loss. If the oxygen gas concentration is too low, the treatment temperature is too low, or the treatment time is too short, the purpose of the micro-oxidation treatment cannot be effectively realized. If the oxygen gas concentration is too high, the treatment temperature is too high, or the treatment time is too long, it will cause excessive oxidation, and the magnetic permeability of the nanocrystalline ribbon will be obviously poor. Although the eddy current loss will be reduced to a certain extent, the hysteresis loss will increase significantly, which will cause the total loss to increase without any decrease.

[0037] As a preferred technical solution of the manufacturing method according to the present application, the manufacturing method comprises: (1) performing a roll press process on a nanocrystalline ribbon having a double-sided tape attached to one side thereof to obtain a pulverized nanocrystalline ribbon, the nanocrystalline ribbon comprising, by mass percentage, 73.5 wt% Fe, 13.5 wt% Si, 9 wt% B, 3 wt% Nb, and 1 wt% Cu; (2) performing an acid etching surface treatment on the pulverized nanocrystalline ribbons obtained in step (1), the acid etching surface treatment being carried out by applying a hydrochloric acid solution having a mass fraction of 0.5-1.2 wt% to the surface of the pulverized nanocrystalline ribbons for 3-8 minutes, and then washing with deionized water after the treatment is completed; (3) performing an alkaline cleaning surface treatment on the nanocrystalline ribbon that has been surface-treated by acid etching in step (2), in which the alkaline cleaning surface treatment is performed by applying a sodium hydroxide solution having a mass fraction of 0.5-2 wt% to the surface of the nanocrystalline ribbon that has been surface-treated by acid etching for 5-10 minutes, and then washing the surface with deionized water after the treatment is completed; (4) washing the nanocrystalline ribbons that have been subjected to the alkaline washing surface treatment in step (3) with water at least three times and then with absolute ethanol at least three times, followed by drying; (5) The method includes a step of subjecting the dried nanocrystalline ribbon from step (4) to a micro-oxidation treatment (wherein the temperature of the micro-oxidation treatment is 60-85°C) for 15-30 minutes in an oxygen gas atmosphere having an oxygen gas concentration of 85 vol% or more to obtain a modified nanocrystalline ribbon.

[0038] In a second aspect, the present application provides modified nanocrystalline ribbons produced by the method described in the first aspect.

[0039] In a third aspect, the present application provides the use of the modified nanocrystalline ribbons described in the first aspect in the manufacture of nanocrystalline composite structure magnetic sheets.

[0040] Preferably, the nanocrystalline composite magnetic sheet includes a release film layer, a first modified nanocrystalline ribbon, a second modified nanocrystalline ribbon, a third modified nanocrystalline ribbon and a fourth modified nanocrystalline ribbon, which are laminated in sequence.

[0041] The double-sided tape of the first modified nanocrystalline ribbon is connected to a release film layer, and the double-sided tape of two adjacent layers of modified nanocrystalline ribbon is connected to a nanocrystalline ribbon.

[0042] The first modified nanocrystalline ribbon, the second modified nanocrystalline ribbon, the third modified nanocrystalline ribbon, and the fourth modified nanocrystalline ribbon are each independently a modified nanocrystalline ribbon as described in claim 7.

[0043] The release film layer according to the present application is a typical release film layer in the art, and the present application does not specifically limit it.

[0044] Preferably, the thickness of the modified nanocrystalline ribbon is between 18 and 22 μm, and may be, for example, 18 μm, 19 μm, 20 μm, 21 μm, or 22 μm, but is not limited to the recited values, and other unrecited values ​​within the numerical range may be used as well.

[0045] Preferably, the thickness of the double-sided tape is 4 to 6 μm, and may be, for example, 4 μm, 4.5 μm, 5 μm, 5.5 μm or 6 μm, but is not limited to the numerical values ​​listed, and other unlisted numerical values ​​within the numerical range may be used as well.

[0046] Preferably, the first modified nanocrystalline ribbon has a real permeability at a test frequency of 128 kHz of 400 to 500, such as, but not limited to, 400, 420, 450, 480 or 500, and other unrecited values ​​within the range may be used as well; and an imaginary permeability of 40 or less, such as, but not limited to, 5, 10, 15, 20, 25, 30, 35 or 40, and other unrecited values ​​within the range may be used as well.

[0047] Preferably, the second modified nanocrystalline ribbon has a real part of permeability at a test frequency of 128 kHz of 600 to 800, such as, for example, 600, 650, 700, 750 or 800, but is not limited to the recited values ​​and other unrecited values ​​within the numerical range may be used as well, and an imaginary part of permeability of 60 or less, such as, for example, 10, 20, 30, 40, 50 or 60, but is not limited to the recited values ​​and other unrecited values ​​within the numerical range may be used as well.

[0048] Preferably, the third modified nanocrystalline ribbon has a real part of permeability at a test frequency of 128 kHz of 1000 to 1400, such as, but not limited to, 1000, 1050, 1100, 1150, 1200, 1250, 1300, 1350 or 1400, but not limited to the recited values ​​and other unrecited values ​​within the numerical range may be used as well, and an imaginary part of permeability of 90 or less, such as, but not limited to, 10, 20, 30, 40, 50, 60, 70, 80 or 90, but not limited to the recited values ​​and other unrecited values ​​within the numerical range may be used as well.

[0049] Preferably, the fourth modified nanocrystalline ribbon has a real part of permeability at a test frequency of 128 kHz of 5000 to 10000, such as, but not limited to, 5000, 6000, 7000, 8000, 9000 or 10000, but not limited to the recited values, and other unrecited values ​​within the numerical range may be used as well, and an imaginary part of permeability of 170 or less, such as, but not limited to, 100, 110, 120, 130, 140, 150, 160 or 170, but not limited to the recited values, and other unrecited values ​​within the numerical range may be used as well.

[0050] The magnetic permeability in this application is the complex magnetic permeability measured by an E4990A tester. During the test, the nanocrystalline ribbon to be tested is cut into a ring with an outer diameter of 19.9 mm and an inner diameter of 8.8 mm. The higher the real part of the magnetic permeability, the better the magnetic permeability performance, and the higher the imaginary part of the magnetic permeability, the greater the magnetic loss of the magnetic shielding sheet.

[0051] The nanocrystalline composite magnetic sheet of the present application strictly limits the magnetic properties of the nanocrystalline ribbons of each layer to form a composite structure with gradient magnetic permeability properties. The first modified nanocrystalline ribbon is the end closest to the receiving end in the wireless charging system, and its low loss properties ensure the efficiency of the wireless charging system. The fourth modified nanocrystalline ribbon of the outermost layer has a high real part of magnetic permeability and has excellent magnetic shielding effect, avoiding magnetic field radiation of the wireless charging system. In the present application, the combination of the first modified nanocrystalline ribbon, the second modified nanocrystalline ribbon, the third modified nanocrystalline ribbon and the fourth modified nanocrystalline ribbon makes the nanocrystalline composite magnetic sheet have good power transmission efficiency.

[0052] Compared with the prior art, the present application has the following beneficial effects:

[0053] (1) Compared with the conventional manufacturing process of nanocrystalline ribbon for wireless charging, the modified nanocrystalline ribbon obtained by the manufacturing method of the present application has a lower imaginary part of magnetic permeability and lower loss, which further contributes to the wireless charging system achieving high power transmission efficiency. In the present application, the pulverized nanocrystalline ribbon is acid-etched, so that dilute hydrochloric acid penetrates into the micro-cracks to corrode and remove the bridges between the pulverized units and the sharp corners of the pulverized units, optimizing the ribbon's microstructure and avoiding the concentration and uneven distribution of the magnetic field during operation. Then, the acid, salt (sodium chloride due to acid-base reaction) and deionized water remaining on the surface of the nanocrystalline ribbon are removed by alkaline washing, water washing and alcohol washing, and finally, a very thin oxide film layer is formed on the surface and edges of the pulverized units in the nanocrystalline ribbon by micro-oxidation treatment, which improves the insulation of the nanocrystalline ribbon and further reduces the eddy current loss of the nanocrystalline ribbon.

[0054] (2) The nanocrystalline composite magnetic sheet of the present application strictly limits the magnetic properties of the nanocrystalline ribbons of each layer to form a composite structure with gradient magnetic permeability properties. The first modified nanocrystalline ribbon is the end closest to the receiving end in the wireless charging system, and its low loss properties ensure the efficiency of the wireless charging system. The fourth modified nanocrystalline ribbon of the outermost layer has a high real part of magnetic permeability and excellent magnetic shielding effect, thereby avoiding magnetic field radiation of the wireless charging system. That is, the combination of the first modified nanocrystalline ribbon, the second modified nanocrystalline ribbon, the third modified nanocrystalline ribbon and the fourth modified nanocrystalline ribbon ensures that the nanocrystalline composite magnetic sheet has good power transmission efficiency. [Brief description of the drawings]

[0055] [Figure 1] 1 is a schematic diagram of the structure of a nanocrystalline composite magnetic sheet according to the present application. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0056] The technical solution of the present application will be further described below by means of specific embodiments. Those skilled in the art should understand that the above examples are merely for the purpose of helping to understand the present application, and should not be regarded as specifically limiting the present application.

[0057] Example 1 This embodiment provides a nanocrystalline composite structure magnetic sheet including a release film layer 1, a first modified nanocrystalline ribbon 3, a second modified nanocrystalline ribbon 4, a third modified nanocrystalline ribbon 5 and a fourth modified nanocrystalline ribbon 6 stacked in order as shown in Figure 1.

[0058] The double-sided tape 2 of the first modified nanocrystalline ribbon 3 is connected to the release film layer 1, and the double-sided tape 2 of two adjacent layers of modified nanocrystalline ribbon is connected to the nanocrystalline ribbon. The thickness of the double-sided tape 2 is 5 μm, and the thickness of each layer of modified nanocrystalline ribbon is 20 μm.

[0059] The first modified nanocrystalline ribbon 3, the second modified nanocrystalline ribbon 4, the third modified nanocrystalline ribbon 5, and the fourth modified nanocrystalline ribbon 6 are each independently modified nanocrystalline ribbons produced by the following production method. (1) A nanocrystalline ribbon (Fe 73.5 S 13.5 B9Nb3Cu, where the subscripts are the percentages of each element relative to the total mass of the nanocrystalline ribbon, to obtain pulverized nanocrystalline ribbons, the pressure of the roll press is 60 kg, and the number of roll presses is 3; (2) performing an acid etching surface treatment on the pulverized nanocrystalline ribbons obtained in step (1), the acid etching surface treatment being performed by applying a hydrochloric acid solution having a mass fraction of 0.8 wt% to the surface of the pulverized nanocrystalline ribbons for 5 minutes, and then washing with deionized water after the treatment is completed; (3) performing an alkaline cleaning surface treatment on the nanocrystalline ribbons that have been subjected to the acid etching surface treatment in step (2), in which the alkaline cleaning surface treatment is carried out by applying a sodium hydroxide solution having a mass fraction of 1.5 wt% to the surface of the nanocrystalline ribbons that have been subjected to the acid etching surface treatment for 8 minutes, and then washing the surface with deionized water after the treatment is completed; (4) washing the nanocrystalline ribbons that have been subjected to the alkaline washing surface treatment in step (3) with water three times and then with absolute ethanol three times, followed by drying; (5) The method includes a step of subjecting the dried nanocrystalline ribbon in step (4) to a micro-oxidation treatment in an oxygen gas atmosphere having an oxygen gas concentration of 95 vol% for 21 minutes (the temperature of the micro-oxidation treatment is 75°C) to obtain a modified nanocrystalline ribbon.

[0060] The real part μ' of magnetic permeability and the imaginary part μ'' of magnetic permeability in the first modified nanocrystalline ribbon 3, the second modified nanocrystalline ribbon 4, the third modified nanocrystalline ribbon 5 and the fourth modified nanocrystalline ribbon 6 are as shown in Table 1. [Table 1]

[0061] Comparative Example 1 This comparative example is similar to Example 1, except that a nanocrystalline composite structure magnetic sheet is provided, and the second modified nanocrystalline ribbon 4, the third modified nanocrystalline ribbon 5 and the fourth modified nanocrystalline ribbon 6 are substituted for the first modified nanocrystalline ribbon 3.

[0062] Comparative Example 2 This comparative example is similar to Example 1, except that a nanocrystalline composite structure magnetic sheet is provided, and the first modified nanocrystalline ribbon 3, the third modified nanocrystalline ribbon 5 and the fourth modified nanocrystalline ribbon 6 are replaced with the second modified nanocrystalline ribbon 4.

[0063] Comparative Example 3 This comparative example is similar to Example 1, except that a nanocrystalline composite structure magnetic sheet is provided, and the first modified nanocrystalline ribbon 3, the second modified nanocrystalline ribbon 4 and the fourth modified nanocrystalline ribbon 6 are replaced with a third modified nanocrystalline ribbon 5.

[0064] Comparative Example 4 This comparative example is similar to Example 1, except that a nanocrystalline composite structure magnetic sheet is provided, and the first modified nanocrystalline ribbon 3, the second modified nanocrystalline ribbon 4 and the third modified nanocrystalline ribbon 5 are replaced with a fourth modified nanocrystalline ribbon 6.

[0065] The charging efficiency test was carried out using the receiving end device of the P9221-EVK wireless charging system manufactured by IDT, the power of the test system was 15W, and it complies with the Qi standard. During the test, after removing the release film, the nanocrystalline composite structure magnetic sheet was fixed on the back of the coil to test the power transmission efficiency. The results are shown in Table 2. [Table 2]

[0066] As can be seen from the above table, the power transmission efficiency of a wireless charging system using a magnetic sheet having a gradient permeability composite structure is higher than the power transmission efficiency of a wireless charging system using a conventional composite magnetic sheet having a single permeability.

[0067] Example 2 This embodiment provides a nanocrystalline composite structure magnetic sheet as shown in Figure 1, which includes a release film layer 1, a first modified nanocrystalline ribbon 3, a second modified nanocrystalline ribbon 4, a third modified nanocrystalline ribbon 5 and a fourth modified nanocrystalline ribbon 6 stacked in sequence.

[0068] The real part μ′ of magnetic permeability and the imaginary part μ″ of magnetic permeability in the first modified nanocrystalline ribbon 3, the second modified nanocrystalline ribbon 4, the third modified nanocrystalline ribbon 5 and the fourth modified nanocrystalline ribbon 6 are as shown in Table 3. The rest are the same as in Example 1. [Table 3]

[0069] Comparative Example 5 This comparative example is similar to Example 2, except that a nanocrystalline composite structure magnetic sheet is provided, and the second modified nanocrystalline ribbon 4 is replaced with the first modified nanocrystalline ribbon 3, and the third modified nanocrystalline ribbon 5 and the fourth modified nanocrystalline ribbon 6 are replaced with the second modified nanocrystalline ribbon 4.

[0070] Comparative Example 6 This comparative example is similar to Example 2, except that a nanocrystalline composite structure magnetic sheet is provided, and the second modified nanocrystalline ribbon 4 is replaced with the first modified nanocrystalline ribbon 3, and the third modified nanocrystalline ribbon 5 is replaced with the fourth modified nanocrystalline ribbon 6.

[0071] Comparative Example 7 This comparative example is similar to Example 2, except that a nanocrystalline composite structure magnetic sheet is provided, and the first modified nanocrystalline ribbon 3 is replaced with a second modified nanocrystalline ribbon 4, and the third modified nanocrystalline ribbon 5 is replaced with a fourth modified nanocrystalline ribbon 6.

[0072] Comparative Example 8 This comparative example is similar to Example 2, except that a nanocrystalline composite structure magnetic sheet is provided, and the first modified nanocrystalline ribbon 3 and the second modified nanocrystalline ribbon 4 are replaced with a third modified nanocrystalline ribbon 5, and the third modified nanocrystalline ribbon 5 and the fourth modified nanocrystalline ribbon 6 are replaced with the second modified nanocrystalline ribbon 4.

[0073] Comparative Example 9 This comparative example is similar to Example 2, except that a nanocrystalline composite structure magnetic sheet is provided and the fourth modified nanocrystalline ribbons 6 are replaced with the third modified nanocrystalline ribbons 5 .

[0074] Comparative Example 10 This comparative example is similar to Example 2, except that a nanocrystalline composite structure magnetic sheet is provided and the third modified nanocrystalline ribbons 5 are replaced with fourth modified nanocrystalline ribbons 6 .

[0075] The charging efficiency test was carried out using the receiving end device of the P9221-EVK wireless charging system manufactured by IDT, the power of the test system was 15W, and it complies with the Qi standard. During the test, after removing the release film, the nanocrystalline composite structure magnetic sheet was fixed on the back of the coil to test the power transmission efficiency. The results are shown in Table 4. [Table 4]

[0076] As can be seen from the above table, the charging efficiency of Example 2 is higher than the charging efficiency of Comparative Examples 5 to 10. This shows that the magnetic sheet having the gradient permeability composite structure according to the present application has the best magnetic blocking effect, magnetic permeability effect, and the most excellent structure.

[0077] Example 3 This embodiment provides a nanocrystalline composite structure magnetic sheet as shown in Figure 1, which includes a release film layer 1, a first modified nanocrystalline ribbon 3, a second modified nanocrystalline ribbon 4, a third modified nanocrystalline ribbon 5 and a fourth modified nanocrystalline ribbon 6 stacked in sequence.

[0078] The double-sided tape 2 of the first modified nanocrystalline ribbon 3 is connected to the release film layer 1, and the double-sided tape 2 of two adjacent layers of modified nanocrystalline ribbon is connected to the nanocrystalline ribbon. The thickness of the double-sided tape 2 is 5 μm, and the thickness of each layer of modified nanocrystalline ribbon is 20 μm.

[0079] The first modified nanocrystalline ribbon 3, the second modified nanocrystalline ribbon 4, the third modified nanocrystalline ribbon 5, and the fourth modified nanocrystalline ribbon 6 are each independently modified nanocrystalline ribbons produced by the following production method. (1) A nanocrystalline ribbon (Fe 73.5 S 13.5 B9Nb3Cu, where the subscripts are the percentages of each element relative to the total mass of the nanocrystalline ribbon, to obtain finely pulverized nanocrystalline ribbons, the pressure of the roll press is 65 kg, and the number of roll presses is 5; (2) performing an acid etching surface treatment on the pulverized nanocrystalline ribbons obtained in step (1), the acid etching surface treatment being performed by applying a hydrochloric acid solution having a mass fraction of 1 wt% to the surface of the pulverized nanocrystalline ribbons for 5 minutes, and then washing with deionized water after the treatment is completed; (3) performing an alkaline cleaning surface treatment on the nanocrystalline ribbons that have been subjected to the acid etching surface treatment in step (2), in which the alkaline cleaning surface treatment is performed by applying a sodium hydroxide solution having a mass fraction of 1.5 wt% to the surface of the nanocrystalline ribbons that have been subjected to the acid etching surface treatment for 9 minutes, and then washing the surface with deionized water after the treatment is completed; (4) washing the nanocrystalline ribbons that have been subjected to the alkaline washing surface treatment in step (3) with water three times and with absolute ethanol three times, followed by drying; (5) The method includes a step of subjecting the dried nanocrystalline ribbon in step (4) to a micro-oxidation treatment in an oxygen gas atmosphere having an oxygen gas concentration of 90 vol% for 28 minutes (the temperature of the micro-oxidation treatment is 80°C) to obtain a modified nanocrystalline ribbon.

[0080] The real part μ' of magnetic permeability and the imaginary part μ'' of magnetic permeability of the first modified nanocrystalline ribbon 3, the second modified nanocrystalline ribbon 4, the third modified nanocrystalline ribbon 5 and the fourth modified nanocrystalline ribbon 6 are as shown in Table 5. [Table 5]

[0081] Comparative Example 11 This comparative example is similar to Example 3, except that a nanocrystalline composite structure magnetic sheet is provided and steps (2), (3), (4) and (5) are not performed when manufacturing the first modified nanocrystalline ribbon 3.

[0082] Comparative Example 12 This comparative example provides a nanocrystalline composite structure magnetic sheet, which is similar to Example 3, except that in producing the first modified nanocrystalline ribbon 3, the mass fraction of the hydrochloric acid solution in step (2) is 0.45 wt %.

[0083] Comparative Example 13 This comparative example provides a nanocrystalline composite structure magnetic sheet, which is similar to Example 3, except that in producing the first modified nanocrystalline ribbon 3, the mass fraction of the hydrochloric acid solution in step (2) is 1.4 wt %.

[0084] Comparative Example 14 This comparative example provides a nanocrystalline composite structure magnetic sheet, which is similar to Example 3, except that in producing the first modified nanocrystalline ribbon 3, the surface acid treatment time in step (2) is 2.5 min.

[0085] Comparative Example 15 This comparative example provides a nanocrystalline composite structure magnetic sheet, which is similar to Example 3, except that in producing the first modified nanocrystalline ribbon 3, the surface acid treatment time in step (2) is 10 minutes.

[0086] The magnetic permeability of the first modified nanocrystalline ribbons 3 obtained in Example 3 and Comparative Examples 11 to 15, and the power transmission efficiency of the nanocrystalline composite structure magnetic sheets are shown in Table 6. [Table 6]

[0087] As can be seen from the above table, compared with the nanocrystalline ribbons 1 in Comparative Examples 11 to 15, the first modified nanocrystalline ribbon 3 in Example 3 has a high real part of magnetic permeability and a low imaginary part of magnetic permeability, and at the same time, has a higher power transmission efficiency. As can be seen from the results, the manufacturing method of the nanocrystalline ribbon according to the present application has good magnetic permeability and magnetic shielding effect, and at the same time, has low loss. When the process parameters of the acid etching surface treatment exceed a certain range, the magnetic shielding effect and magnetic permeability effect of the nanocrystalline ribbon, as well as the charging efficiency of the wireless charging system constructed therewith, are both poor.

[0088] Example 4 This embodiment provides a nanocrystalline composite structure magnetic sheet as shown in Figure 1, which includes a release film layer 1, a first modified nanocrystalline ribbon 3, a second modified nanocrystalline ribbon 4, a third modified nanocrystalline ribbon 5 and a fourth modified nanocrystalline ribbon 6 stacked in sequence.

[0089] The double-sided tape 2 of the first modified nanocrystalline ribbon 3 is connected to the release film layer 1, and the double-sided tape 2 of two adjacent layers of modified nanocrystalline ribbon is connected to the nanocrystalline ribbon. The thickness of the double-sided tape 2 is 5 μm, and the thickness of each layer of modified nanocrystalline ribbon is 20 μm.

[0090] The first modified nanocrystalline ribbon 3, the second modified nanocrystalline ribbon 4, the third modified nanocrystalline ribbon 5, and the fourth modified nanocrystalline ribbon 6 are each independently modified nanocrystalline ribbons produced by the following production method. (1) A nanocrystalline ribbon (Fe 73.5 S 13.5 B9Nb3Cu, where the subscripts are the percentages of each element relative to the total mass of the nanocrystalline ribbon, to obtain pulverized nanocrystalline ribbons, the pressure of the roll press is 62 kg, and the number of roll presses is 4; (2) performing an acid etching surface treatment on the pulverized nanocrystalline ribbons obtained in step (1), the acid etching surface treatment being carried out by applying a hydrochloric acid solution having a mass fraction of 0.9 wt% to the surface of the pulverized nanocrystalline ribbons for 6 minutes, and then washing with deionized water after the treatment is completed; (3) performing an alkaline cleaning surface treatment on the nanocrystalline ribbons that have been surface-treated by acid etching in step (2), in which the alkaline cleaning surface treatment is performed by applying a sodium hydroxide solution having a mass fraction of 1.2 wt% to the surface of the nanocrystalline ribbons that have been surface-treated by acid etching for 6 minutes, and then washing the surface with deionized water after the treatment is completed; (4) washing the nanocrystalline ribbons that have been subjected to the alkaline washing surface treatment in step (3) with water three times and with absolute ethanol three times, followed by drying; (5) The method includes a step of subjecting the dried nanocrystalline ribbon in step (4) to a micro-oxidation treatment in an oxygen gas atmosphere having an oxygen gas concentration of 98 vol% for 18 minutes (the temperature of the micro-oxidation treatment is 70°C) to obtain a modified nanocrystalline ribbon.

[0091] The real part μ' of magnetic permeability and the imaginary part μ'' of magnetic permeability of the first modified nanocrystalline ribbon 3, the second modified nanocrystalline ribbon 4, the third modified nanocrystalline ribbon 5 and the fourth modified nanocrystalline ribbon 6 are as shown in Table 7. [Table 7]

[0092] Comparative Example 16 This comparative example is similar to Example 4, except that a nanocrystalline composite structure magnetic sheet is provided and the alkaline cleaning surface treatment in step (3) is not performed when producing the second modified nanocrystalline ribbons 4.

[0093] Comparative Example 17 This comparative example provides a nanocrystalline composite structure magnetic sheet and is similar to Example 4, except that in producing the second modified nanocrystalline ribbon 4, the mass fraction of the sodium hydroxide solution in step (3) is 0.4 wt%.

[0094] Comparative Example 18 This comparative example provides a nanocrystalline composite structure magnetic sheet and is similar to Example 4, except that in producing the second modified nanocrystalline ribbon 4, the mass fraction of the sodium hydroxide solution in step (3) is 2.5 wt%.

[0095] Comparative Example 19 This comparative example provides a nanocrystalline composite structure magnetic sheet, which is similar to Example 4, except that in producing the second modified nanocrystalline ribbon 4, the surface alkali treatment time in step (3) is 4.5 min.

[0096] Comparative Example 20 This comparative example provides a nanocrystalline composite structure magnetic sheet, and is similar to Example 4, except that in producing the second modified nanocrystalline ribbon 4, the surface alkali treatment time in step (3) is 12 minutes.

[0097] The magnetic permeability of the second modified nanocrystalline ribbons 4 obtained in Example 4 and Comparative Examples 16 to 20, and the power transmission efficiency of the nanocrystalline composite structure magnetic sheets are as shown in Table 8. [Table 8]

[0098] As can be seen from the above table, compared with the nanocrystalline ribbons 2 in Comparative Examples 16 to 19, the second modified nanocrystalline ribbon 4 in Example 4 has a high real part of magnetic permeability and a low imaginary part of magnetic permeability, and at the same time, has a higher power transmission efficiency. The magnetic performance and power transmission efficiency of the second modified nanocrystalline ribbon 4 in Comparative Example 20 are equivalent to those of Example 4, proving that too long an alkaline cleaning time does not improve performance and wastes costs. Therefore, the manufacturing method of the nanocrystalline ribbon according to the present application has good magnetic permeability and magnetic blocking effect, and at the same time, has low loss. If the alkaline cleaning step is not used or the process parameters of the alkaline cleaning exceed a certain range, the magnetic blocking effect and magnetic permeability effect of the nanocrystalline ribbon and the charging efficiency of the wireless charging system constructed therewith are both poor.

[0099] Example 5 This embodiment provides a nanocrystalline composite structure magnetic sheet as shown in Figure 1, which includes a release film layer 1, a first modified nanocrystalline ribbon 3, a second modified nanocrystalline ribbon 4, a third modified nanocrystalline ribbon 5 and a fourth modified nanocrystalline ribbon 6 stacked in sequence.

[0100] The double-sided tape 2 of the first modified nanocrystalline ribbon 3 is connected to the release film layer 1, and the double-sided tape 2 of two adjacent layers of modified nanocrystalline ribbon is connected to the nanocrystalline ribbon. The thickness of the double-sided tape 2 is 5 μm, and the thickness of each layer of modified nanocrystalline ribbon is 20 μm.

[0101] The first modified nanocrystalline ribbon 3, the second modified nanocrystalline ribbon 4, the third modified nanocrystalline ribbon 5, and the fourth modified nanocrystalline ribbon 6 are each independently modified nanocrystalline ribbons produced by the following production method: (1) A nanocrystalline ribbon (Fe 73.5 S 13.5 B9Nb3Cu, where the subscripts are the percentages of each element relative to the total mass of the nanocrystalline ribbon, to obtain finely pulverized nanocrystalline ribbons, the pressure of the roll press is 60 kg, and the number of roll presses is 5; (2) performing an acid etching surface treatment on the pulverized nanocrystalline ribbons obtained in step (1), the acid etching surface treatment being carried out by applying a hydrochloric acid solution having a mass fraction of 0.5 wt% to the surface of the pulverized nanocrystalline ribbons for 8 minutes, and then washing with deionized water after the treatment is completed; (3) performing an alkaline cleaning surface treatment on the nanocrystalline ribbons that have been surface-treated by acid etching in step (2), in which the alkaline cleaning surface treatment is performed by applying a sodium hydroxide solution having a mass fraction of 2 wt% to the surface of the nanocrystalline ribbons that have been surface-treated by acid etching for 5 minutes, and then washing the surface with deionized water after the treatment is completed; (4) washing the nanocrystalline ribbons that have been subjected to the alkaline washing surface treatment in step (3) with water three times and with absolute ethanol three times, followed by drying; (5) The method includes a step of subjecting the dried nanocrystalline ribbon in step (4) to a micro-oxidation treatment in an oxygen gas atmosphere having an oxygen gas concentration of 90 vol% for 15 minutes (the temperature of the micro-oxidation treatment is 85°C) to obtain a modified nanocrystalline ribbon.

[0102] The real part μ' of magnetic permeability and the imaginary part μ'' of magnetic permeability of the first modified nanocrystalline ribbon 3, the second modified nanocrystalline ribbon 4, the third modified nanocrystalline ribbon 5 and the fourth modified nanocrystalline ribbon 6 are as shown in Table 9. [Table 9]

[0103] Comparative Example 21 This comparative example is similar to Example 5, except that a nanocrystalline composite structure magnetic sheet is provided and the alcohol washing in step (4) is not performed when producing the third modified nanocrystalline ribbons 5.

[0104] The magnetic permeability of the third modified nanocrystalline ribbon 5 obtained in Example 5 and Comparative Example 21, and the power transmission efficiency of the nanocrystalline composite structure magnetic sheet are as shown in Table 10. [Table 10]

[0105] As can be seen from the above table, compared with the third modified nanocrystalline ribbon 5 in Comparative Example 21, the third modified nanocrystalline ribbon 5 in Example 5 has a higher real part of magnetic permeability and a lower imaginary part of magnetic permeability, while at the same time, the power transmission efficiency is higher. As can be seen from the results, alcohol washing is extremely important in the manufacturing process of nanocrystalline ribbons.

[0106] Example 6 This embodiment provides a nanocrystalline composite structure magnetic sheet as shown in Figure 1, which includes a release film layer 1, a first modified nanocrystalline ribbon 3, a second modified nanocrystalline ribbon 4, a third modified nanocrystalline ribbon 5 and a fourth modified nanocrystalline ribbon 6 stacked in sequence.

[0107] The double-sided tape 2 of the first modified nanocrystalline ribbon 3 is connected to the release film layer 1, and the double-sided tape 2 of two adjacent layers of modified nanocrystalline ribbon is connected to the nanocrystalline ribbon. The thickness of the double-sided tape 2 is 5 μm, and the thickness of each layer of modified nanocrystalline ribbon is 20 μm.

[0108] The first modified nanocrystalline ribbon 3, the second modified nanocrystalline ribbon 4, the third modified nanocrystalline ribbon 5, and the fourth modified nanocrystalline ribbon 6 are each independently modified nanocrystalline ribbons produced by the following production method. (1) A nanocrystalline ribbon (Fe 73.5 S 13.5B9Nb3Cu, where the subscripts are the percentages of each element relative to the total mass of the nanocrystalline ribbon, to obtain pulverized nanocrystalline ribbons, the pressure of the roll press being 70 kg and the number of roll presses being one; (2) performing an acid etching surface treatment on the pulverized nanocrystalline ribbons obtained in step (1), the acid etching surface treatment being performed by applying a hydrochloric acid solution having a mass fraction of 1.2 wt% to the surface of the pulverized nanocrystalline ribbons for 3 minutes, and then washing with deionized water after the treatment is completed; (3) performing an alkaline cleaning surface treatment on the nanocrystalline ribbon that has been surface-treated by acid etching in step (2), in which the alkaline cleaning surface treatment is performed by applying a sodium hydroxide solution having a mass fraction of 0.5 wt% to the surface of the nanocrystalline ribbon that has been surface-treated by acid etching for 10 minutes, and then washing with deionized water after the treatment is completed; (4) washing the nanocrystalline ribbons that have been subjected to the alkaline washing surface treatment in step (3) with water three times and with absolute ethanol three times, followed by drying; (5) The method includes a step of subjecting the dried nanocrystalline ribbon in step (4) to a micro-oxidation treatment in an oxygen gas atmosphere having an oxygen gas concentration of 85 vol% for 30 minutes (the temperature of the micro-oxidation treatment is 60°C) to obtain a modified nanocrystalline ribbon.

[0109] The real part μ' of magnetic permeability and the imaginary part μ'' of magnetic permeability of the first modified nanocrystalline ribbon 3, the second modified nanocrystalline ribbon 4, the third modified nanocrystalline ribbon 5 and the fourth modified nanocrystalline ribbon 6 are as shown in Table 11. [Table 11]

[0110] Comparative Example 22 This comparative example is similar to Example 6, except that a nanocrystalline composite structure magnetic sheet is provided and the micro-oxidation treatment in step (5) is not performed when manufacturing the fourth modified nanocrystalline ribbon 6.

[0111] Comparative Example 23 This comparative example provides a nanocrystalline composite structure magnetic sheet, and is similar to Example 6, except that in producing the fourth modified nanocrystalline ribbon 6, the oxygen gas concentration in step (5) is 83 vol%.

[0112] Comparative Example 24 This comparative example provides a nanocrystalline composite structure magnetic sheet, and is similar to Example 6, except that the temperature of the micro-oxidation treatment in step (5) in producing the fourth modified nanocrystalline ribbon 6 is 55°C.

[0113] Comparative Example 25 This comparative example provides a nanocrystalline composite structure magnetic sheet, and is similar to Example 6, except that the temperature of the micro-oxidation treatment in step (5) in producing the fourth modified nanocrystalline ribbon 6 is 90°C.

[0114] Comparative Example 26 This comparative example provides a nanocrystalline composite structure magnetic sheet and is similar to Example 6, except that in manufacturing the fourth modified nanocrystalline ribbon 6, the time of the micro-oxidation treatment in step (5) is 12 minutes.

[0115] Comparative Example 27 This comparative example provides a nanocrystalline composite structure magnetic sheet and is similar to Example 6, except that in manufacturing the fourth modified nanocrystalline ribbon 6, the time of the micro-oxidation treatment in step (5) is 35 minutes.

[0116] The magnetic permeability of the fourth modified nanocrystalline ribbons 6 obtained in Example 6 and Comparative Examples 22 to 27, and the power transmission efficiency of the nanocrystalline composite structure magnetic sheets are as shown in Table 12. [Table 12]

[0117] As can be seen from the above table, compared with the fourth modified nanocrystalline ribbons 6 in Comparative Examples 22 to 27, the fourth modified nanocrystalline ribbons 6 in Example 6 simultaneously have high real part of magnetic permeability and low imaginary part of magnetic permeability, and have higher power transmission efficiency. As can be seen from the results, the presence or absence of micro-oxidation and the limitations of its process parameters have a significant impact on the magnetic performance and power transmission efficiency of the nanocrystalline ribbons.

[0118] In short, compared with the conventional manufacturing process of nanocrystalline ribbon for wireless charging, the modified nanocrystalline ribbon obtained by the manufacturing method of the present application has a lower imaginary part of magnetic permeability and lower loss, which further contributes to the wireless charging system obtaining high power transmission efficiency. In the present application, the pulverized nanocrystalline ribbon is acid-etched, so that dilute hydrochloric acid penetrates into the micro-cracks, corrodes and removes the bridges between the pulverized units and the sharp corners of the pulverized units, optimizes the ribbon's microstructure, and avoids the concentration and uneven distribution of the magnetic field during the operation process. Then, the residual acid, salt (sodium chloride due to acid-base reaction) and deionized water on the surface of the nanocrystalline ribbon are removed by alkaline washing, water washing and alcohol washing, and finally, a very thin oxide film layer is formed on the surface and edges of the pulverized units in the nanocrystalline ribbon by micro-oxidation treatment, which improves the insulation of the nanocrystalline ribbon and further reduces the eddy current loss of the nanocrystalline ribbon.

[0119] The nanocrystalline composite magnetic sheet of the present application has a composite structure with gradient magnetic permeability properties formed by strictly limiting the magnetic performance of each layer of nanocrystalline ribbon. The first modified nanocrystalline ribbon is the end closest to the wireless charging system, and its low loss properties ensure the efficiency of the wireless charging system. The fourth modified nanocrystalline ribbon of the outermost layer has a high real part of magnetic permeability and excellent magnetic shielding effect, avoiding magnetic field radiation of the wireless charging system. In other words, the combination of the first modified nanocrystalline ribbon, the second modified nanocrystalline ribbon, the third modified nanocrystalline ribbon and the fourth modified nanocrystalline ribbon ensures that the nanocrystalline composite magnetic sheet has good power transmission efficiency.

[0120] The above is merely a specific embodiment of the present application, and the applicant declares that the scope of protection of the present application is not limited thereto. [Explanation of symbols]

[0121] 1, Release film layer 2. Double-sided tape 3. The first modified nanocrystalline ribbon 4. The second modified nanocrystalline ribbon 5. The third modified nanocrystalline ribbon 6. The fourth modified nanocrystalline ribbon

Claims

1. (1) performing a roll press process on a nanocrystalline ribbon having a double-sided tape attached to one side thereof to obtain a finely pulverized nanocrystalline ribbon; (2) subjecting the pulverized nanocrystalline ribbons obtained in step (1) to an acid etching surface treatment; (3) subjecting the acid-etched surface-treated nanocrystalline ribbons of step (2) to an alkaline cleaning surface treatment; (4) washing the nanocrystalline ribbons that have been subjected to the alkaline washing surface treatment in step (3) with water and then with alcohol, followed by drying; (5) performing a micro-oxidation treatment on the dried nanocrystalline ribbon in step (4) to obtain a modified nanocrystalline ribbon.

2. 2. The method of claim 1, wherein the nanocrystalline ribbon comprises, by mass percentage, 73.5 wt% Fe, 13.5 wt% Si, 9 wt% B, 3 wt% Nb, and 1 wt% Cu.

3. The method according to claim 1 or 2, wherein the pressure of the roll press in step (1) is 60 to 70 kg.

4. The method according to any one of claims 1 to 3, wherein the number of times of roll pressing in step (1) is 1 to 5.

5. The acid etching surface treatment in step (2) is to apply an acid solution to the surface of the pulverized nanocrystalline ribbons to perform surface acid treatment, and then wash with deionized water after the treatment is completed; The acid solution is a hydrochloric acid solution having a mass fraction of 0.5 to 1.2 wt %, The method according to any one of claims 1 to 4, wherein the surface acid treatment is carried out for a period of 3 to 8 minutes.

6. The alkaline cleaning surface treatment in step (3) is to apply an alkaline solution to the surface of the nanocrystalline ribbon that has been subjected to the acid etching surface treatment to perform a surface alkaline treatment, and then wash the surface with deionized water after the treatment is completed; The alkaline solution comprises any one or a combination of at least two of a sodium bicarbonate solution, a potassium hydroxide solution, or a sodium hydroxide solution; The mass fraction of the sodium hydroxide solution is 0.5 to 2 wt %, The method according to any one of claims 1 to 5, wherein the surface alkali treatment is carried out for 5 to 10 minutes.

7. The method according to claim 6, wherein the alkaline solution is a potassium hydroxide solution.

8. The number of water washes in step (4) is at least three; The method according to any one of claims 1 to 7, wherein the alcohol washing in step (4) is washing with absolute ethanol at least three times.

9. The micro-oxidation treatment in step (5) is carried out in an oxygen gas atmosphere having an oxygen gas concentration of 85 vol% or more; The temperature of the micro-oxidation treatment in step (5) is 60 to 85° C.; The method according to any one of claims 1 to 8, wherein the time of the micro-oxidation treatment in step (5) is 15 to 30 minutes.

10. The manufacturing method includes: (1) performing a roll press process on a nanocrystalline ribbon having a double-sided tape attached to one side thereof to obtain a pulverized nanocrystalline ribbon, the nanocrystalline ribbon comprising, by mass percentage, 73.5 wt% Fe, 13.5 wt% Si, 9 wt% B, 3 wt% Nb, and 1 wt% Cu; (2) performing an acid etching surface treatment on the pulverized nanocrystalline ribbons obtained in step (1), the acid etching surface treatment being carried out by applying a hydrochloric acid solution having a mass fraction of 0.5-1.2 wt % to the surface of the pulverized nanocrystalline ribbons for 3-8 min, and washing with deionized water after the treatment is completed; (3) performing an alkaline cleaning surface treatment on the nanocrystalline ribbon that has been surface-treated by acid etching in step (2), in which the alkaline cleaning surface treatment is performed by applying a sodium hydroxide solution having a mass fraction of 0.5-2 wt % to the surface of the nanocrystalline ribbon that has been surface-treated by acid etching for 5-10 minutes, and then washing with deionized water after the treatment is completed; (4) washing the alkaline-washed surface-treated nanocrystalline ribbons in step (3) with water at least three times and then with absolute ethanol at least three times, followed by drying; The method of any one of claims 1 to 9, further comprising: (5) subjecting the dried nanocrystalline ribbon from step (4) to a micro-oxidation treatment in an oxygen gas atmosphere having an oxygen gas concentration of 85 vol% or more for 15 to 30 minutes, the temperature of the micro-oxidation treatment being 60 to 85°C, to obtain a modified nanocrystalline ribbon.

11. The method according to any one of claims 1 to 10, wherein the modified nanocrystalline ribbons are used to manufacture nanocrystalline composite structure magnetic sheets.

12. the nanocrystalline composite magnetic sheet includes a release film layer, a first modified nanocrystalline ribbon, a second modified nanocrystalline ribbon, a third modified nanocrystalline ribbon, and a fourth modified nanocrystalline ribbon, which are laminated in order; The double-sided tape of the first modified nanocrystalline ribbon is connected to a release film layer, and the double-sided tape of two adjacent layers of modified nanocrystalline ribbon is connected to the modified nanocrystalline ribbon; The method of claim 11, wherein the first modified nanocrystalline ribbon, the second modified nanocrystalline ribbon, the third modified nanocrystalline ribbon and the fourth modified nanocrystalline ribbon are each independently modified nanocrystalline ribbons obtained by the method of claim 10.

13. the modified nanocrystalline ribbons have a thickness of 18-22 μm; The thickness of the double-sided tape is 4 to 6 μm, the first modified nanocrystalline ribbon has a real part of magnetic permeability of 400-500 and an imaginary part of magnetic permeability of 40 or less at a test frequency of 128 kHz; the second modified nanocrystalline ribbon has a real part of magnetic permeability of 600-800 and an imaginary part of magnetic permeability of 60 or less at a test frequency of 128 kHz; the third modified nanocrystalline ribbon has a real part of magnetic permeability of 1000 to 1400 and an imaginary part of magnetic permeability of 90 or less at a test frequency of 128 kHz; The method of claim 12, wherein the fourth modified nanocrystalline ribbon has a real part of magnetic permeability of 5,000 to 10,000 and an imaginary part of magnetic permeability of 170 or less at a test frequency of 128 kHz.

Citation Information

Patent Citations

  • Magnetic conductive plate structure for wireless charging

    CN108231381A

  • Low-loss amorphous and nanocrystalline magnetic sheet and preparation method thereof

    CN108666115A

  • Magnetic sheet based on amorphous or nanocrystalline strip material and preparation method thereof

    CN109712800A

  • Magnetic substance sheet, magnetic substance sheet manufacturing method, and radio communication device

    JP2016219795A

  • Soft magnetic sheet and method of manufacturing soft magnetic sheet

    JP2020017696A