Universal monocrystalline silicon texturing additive, texturing liquid containing same, and preparation method and application of texturing liquid
By adjusting the ratio of texturing additives and alkali solution, and using polyhydroxy vegetable gum and block polyether-modified organic silicon anionic surfactants, the pyramid size on the surface of single crystal silicon is controllable, solving the problem of the impact of different battery technologies on the pyramids. The difference in size requirements reduces costs and improves texturing efficiency.
Patent Information
- Application Number
- CN202410759510.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-13
- Publication Date
- 2024-10-01
AI Technical Summary
Different battery technology routes have different requirements for the pyramid size after texturing the monocrystalline silicon surface, resulting in complex supply chain management, high procurement costs, and difficult production line adjustment.
By changing the ratio of texturing additive to alkali solution, a universal monocrystalline silicon texturing additive was designed, including polyhydroxy vegetable gum natural polymer compounds, block polyether modified organic silicon anionic surfactants and Polycarboxylic etching catalyst enables the pyramid size to be adjusted within the range of 0.8-3μm.
It achieves controllable preparation of pyramids of different sizes, reduces raw material and environmentally friendly processing costs, improves texturing efficiency and cost-effectiveness, while ensuring the uniformity of pyramid size and reflective properties.
Smart Images

Figure CN118727156A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of semiconductor manufacturing technology, and in particular relates to a universal single crystal silicon texturing additive, a texturing liquid containing the same, and a preparation method and use thereof. Background Art
[0002] The Chinese government has been guiding the domestic photovoltaic industry to improve product technology and change the downstream's excessive reliance on subsidies, thereby forcing all links in the industry chain to reduce costs and improve efficiency. Technology is the ultimate driving force for achieving continuous cost reduction and efficiency improvement. In order to improve power generation efficiency, following the monocrystalline PERC cell, a variety of new high-efficiency cell technologies such as TOPCon cell, HJT cell and XBC cell have emerged.
[0003] Texturing additives are one of the keys to reducing costs and increasing efficiency in the process of preparing solar cells. High-quality additives can effectively reduce the amount of chemicals such as NaOH and HF used in texturing, etching, and cleaning, effectively reducing the raw material costs and environmental protection costs of solar companies; on the other hand, they can accelerate the reaction rate and improve the photoelectric efficiency of solar cells. Therefore, with the continuous innovation of battery technology and the urgent need to reduce costs and increase efficiency, higher requirements are also placed on the performance and diversification of texturing additives.
[0004] At present, the surface of single crystal silicon is mainly textured by adding some additives to alkali solution. The surface morphology obtained is generally similar to the morphology of the pyramid structure. Different technical routes have different requirements for the size of the pyramid. At this stage, the size of the pyramid is mainly changed by changing the additive formula to adapt to the requirements of different technical routes for the size of the pyramid, which leads to complex supply chain management, high procurement costs, and difficult production line adjustments.
[0005] Therefore, developing a universal texturing method for single-crystal silicon wafers that is applicable to a variety of battery technologies has become one of the main problems that need to be solved urgently. Summary of the invention
[0006] The technical problem solved by the present invention is that different technical routes have different requirements for the size of the pyramids obtained after texturing the surface of single-crystal silicon, which leads to complex supply chain management, high procurement costs and difficult production line adjustment.
[0007] In view of the technical problems existing in the prior art, the present invention designs a universal monocrystalline silicon texturing additive, a texturing solution containing the same, a preparation method and use thereof. By changing the ratio of the texturing additive to the alkali solution, controllable preparation of pyramids of different sizes can be achieved, and the pyramid size can be adjusted within the range of 0.8-3μm.
[0008] It should be noted that, in the present invention, unless otherwise specified, the specific meaning of "including" in relation to composition limitations and descriptions includes both open-ended "including", "comprising" and similar meanings, and closed-ended "consisting of..." and similar meanings.
[0009] In order to solve the above-mentioned technical problems, the present invention adopts the following solutions:
[0010] [The first technical solution]
[0011] The invention provides a universal single crystal silicon texturing additive, characterized in that it comprises the following components calculated by weight:
[0012] 0.001-0.1 part of velvet remover;
[0013] Surfactant 0.01-1 part;
[0014] 1-10 parts of a polycarboxyl etching catalyst;
[0015] 0.5-5 parts of inorganic base;
[0016] 50-90 parts of deionized water.
[0017] Furthermore, the fleece-forming agent is a polyhydroxylated plant gum-type natural macromolecular compound;
[0018] The polycarboxyl etching catalyst is one or more of nitrilotriacetic acid, triethanolaminetriacetic acid, aminotriacetic acid, glycyl-glycine, glycyl-glycyl-glycine, L-leucylglycylglycine, chloroacetylglycylglycine, (2,4-dichlorobenzoyl)glycyl-glycine, N-(2-bromo-1-oxopropyl)glycyl-glycine and their sodium salts;
[0019] The inorganic base is one of NaOH and KOH or a mixture of the two.
[0020] Furthermore, the polyhydroxylated plant gum natural polymer compound is one or a mixture of fennel gum, bletilla striata gum, locust bean gum, agar-agar gum, cashew nut shell gum, and aloe vera gum;
[0021] The polycarboxyl etching catalyst is one or more of chloroacetyl glycyl glycine, (2,4-dichlorobenzoyl) glycyl-glycine, N-(2-bromo-1-oxopropyl)-glycyl-glycine and sodium salts thereof.
[0022] Furthermore, the surfactant is a block polyether modified organosilicon anionic surfactant in the following formula:
[0023]
[0024] In the formula, m represents the addition number of -(CH3)2SiO groups, and its value is an integer from 0 to 5;
[0025] n represents -(CH3)SiO(C3H6O(C2H4) a (C3H6O) b The number of addition of R) groups is an integer from 1 to 5;
[0026] a represents the addition number of ethylene oxide groups, which is an integer from 3 to 14;
[0027] b represents the addition number of propylene oxide groups, which is an integer of 4-20;
[0028] R is an anionic group, which is either a sulfonic acid group or a carboxyl group;
[0029] The molecular weight of the surfactant is 500-10000.
[0030] In the present invention, in order to further optimize the function of the additive, each component can be optimized: 0.003-0.07 parts of linting agent; 0.1-0.5 parts of surfactant; 2-6 parts of polycarboxyl etching catalyst; 1-5 parts of inorganic base; 50-80 parts of deionized water.
[0031] It may be more preferably: 0.005-0.05 parts of linting agent; 0.2-0.3 parts of surfactant; 3-5 parts of polycarboxyl etching catalyst; 1-3 parts of inorganic base; 70-80 parts of deionized water.
[0032] In the present invention, the plant gum natural polymer compound is preferably one or a mixture of agar-agar, cashew nut shell gum and aloe vera gel, and more preferably aloe vera gel.
[0033] In the present invention, the polycarboxyl etching catalyst is more preferably one of chloroacetyl-glycyl-glycine, (2,4-dichlorobenzoyl)glycyl-glycine and sodium salts thereof, or a mixture of several thereof.
[0034] In the present invention, the inorganic base is preferably KOH.
[0035] In the present invention, the surfactant may further preferably have a value of m of 0-2, a value of n of 1-3, a:b≈1 / 3-1 / 2, and a molecular weight of 500-2000.
[0036] The polyhydroxy plant gum natural macromolecular compound of the present invention has unique effects:
[0037] First, it is environmentally friendly, resource-rich, cheap and easily available.
[0038] Secondly, the hydroxyl content in its molecules is extremely high, and the cashmere yield is high. An extremely low amount of addition can meet the required cashmere yield effect, which has excellent cost-effectiveness.
[0039] Thirdly, polyhydroxy natural plant gum-like natural polymer compounds also have good surface activity and corrosion inhibition, which provides a guarantee for controlling the etching rate and improving the cleaning ability.
[0040] The surfactant in the present invention has unique effects:
[0041] First, the surfactant molecule contains both siloxane chains and polyether groups. The structural characteristics of the surfactant give it the low-foaming properties of block polyether.
[0042] Secondly, because of the siloxane chain, that is, the polarity of the siloxane chain is between hydrophobic and hydrophilic, the existence of the silicone surfactant forms a relatively stable interface between the water phase and the oil phase, which makes it have higher stability and surface activity, ensuring that it can better reduce the surface tension under high temperature conditions and improve the wettability of the solution.
[0043] Thirdly, after the surfactant is dissolved in the alkaline aqueous solution, the oxygen atoms in the Si-O bond and the CO bond will be exposed, and then combined with the -OH on the surface of the single crystal silicon through the force of hydrogen bonding, forming a network film layer on the surface of the single crystal silicon, which becomes the starting point for nucleation and assists in the production of velvet.
[0044] The polycarboxyl etching catalyst of the present invention has unique effects:
[0045] First, it is an etching catalyst containing amino, carboxyl or halogen atoms, which reduces the interaction between metal ions and the silicon surface by complexing with metal ions through the carboxyl, amino or halogen atoms in the molecule;
[0046] Secondly, it can adjust the contact performance between the texturing liquid and the silicon surface through its high affinity with silicon, thereby promoting the dissolution of silicon.
[0047] Thirdly, when the etching catalyst is consumed to a certain concentration, it also has the function of balancing the etching rate, avoiding over-etching of single crystal silicon and ensuring the velvet removal effect.
[0048] [Second technical solution]
[0049] The invention provides a method for preparing a universal single crystal silicon texturing additive, comprising the following steps:
[0050] Step 1: Weigh the required amount of each component of the texturing additive according to the weight ratio;
[0051] Step 2: At room temperature, first add all components except deionized water to 1 / 3-1 / 2 deionized water, stir magnetically until all components are completely mixed, then add the remaining deionized water, and continue stirring for 2-3 hours to obtain the universal single crystal silicon texturing additive.
[0052]
Third technical solution
[0053] The purpose is to provide a universal single crystal silicon texturing additive prepared by the above preparation method and its use in the field of single crystal silicon wet etching texturing.
[0054]
The fourth technical solution
[0055] The invention provides a texturing liquid, comprising the above-mentioned universal single crystal silicon texturing additive, alkali and deionized water.
[0056] The mass ratio of the universal single crystal silicon texturing additive to the alkali is 0.1-2:100;
[0057] The alkali is NaOH and / or KOH.
[0058] The amount of deionized water used is mainly to dissolve the universal single crystal silicon texturing additive.
[0059] In the present invention, the mass ratio of the universal single crystal silicon texturing additive to the alkali is preferably 0.3-1.5:100.
[0060]
Fifth technical solution
[0061] The invention provides a method for preparing the above-mentioned texturing liquid, comprising the following steps:
[0062] The universal single crystal silicon texturing additive, alkali and deionized water are weighed according to the mass ratio, and the universal single crystal silicon texturing additive and alkali are added to the deionized water at 80-85° C. and stirred to mix evenly, so as to prepare the texturing liquid.
[0063] In the present invention, by changing the ratio of the universal single crystal silicon texturing additive and the alkali, the controllable preparation of pyramids of different sizes can be achieved, and the size of the pyramid is adjustable within the range of 0.8-3 μm.
[0064] [Sixth technical solution]
[0065] A method for using the above-mentioned texturing liquid is provided, comprising the following steps:
[0066] The single crystal silicon wafer is placed in the texturing liquid for texturing reaction, the texturing temperature is 80-85°C, and the texturing time is 360-420s. After the reaction is completed, the single crystal silicon wafer is taken out and the front and back sides of the silicon wafer are rinsed with deionized water and ethanol respectively, and then placed in a N2 atmosphere for drying.
[0067] In the method for using the texturing liquid of the present invention, the texturing temperature may be preferably 82° C., and the texturing time may be preferably 400 seconds. The single crystal silicon wafer is taken out and rinsed with deionized water and ethanol respectively on the front and back sides of the silicon wafer for 5-30 seconds, preferably 10-20 seconds.
[0068] The polyhydroxy plant gum natural polymer compound of the present invention is used as a fleece-making agent, and a low-foaming and high-efficiency block polyether modified silicone anionic surfactant is compounded with an etching catalyst to produce fleece. The fleece-making window is relatively wide. Within a certain range, by changing the ratio of the additive to the alkali solution, controllable preparation of pyramids of different sizes can be achieved.
[0069] The present invention provides a universal single crystal silicon texturing additive, a texturing liquid containing the same, a preparation method and use thereof, adopts cheap and readily available polyhydroxy natural plant gum as a texturing agent, and is compounded with a low-foaming and high-efficiency block polyether modified organic silicon anionic surfactant to cooperate with an etching catalyst for texturing, which has the following beneficial effects:
[0070] 1. The present invention adopts plant gum natural polymer velvet-making agent, synergistic block polyether modified organosilicon anionic surfactant and multi-carboxyl etching catalyst to make velvet, and its velvet-making window is relatively wide. Within a certain range, by changing the ratio of additives and alkali solution, the controllable preparation of pyramids of different sizes can be achieved, and the size uniformity of the pyramids under various size conditions is good. Under the premise that the reflection meets the requirements, the pyramid size can be adjusted within the range of 0.8-3μm.
[0071] 2. The polyhydroxyl natural plant gum polymer used in the present invention is not only environmentally friendly, abundant in resources, cheap and easy to obtain, but also has a very high hydroxyl content in its molecules, a high lint yield rate, and a very low addition amount can meet the required lint yield effect, which has excellent cost-effectiveness. At the same time, the polyhydroxyl natural plant gum also has good surface activity and corrosion inhibition, which provides a guarantee for the control of etching rate and the improvement of cleaning ability.
[0072] 3. The block polyether modified organosilicon anionic surfactant used in the present invention contains both siloxane chains and polyether groups in the molecule. The structural characteristics of the surfactant give it the low-foaming characteristics of the block polyether, and the presence of the siloxane chain makes it have higher stability and surface activity, ensuring that it can better reduce the surface tension under high temperature conditions and improve the wettability of the solution. In addition, after the surfactant is dissolved in an alkaline aqueous solution, the oxygen atoms in the Si-O bond and the CO bond will be exposed, and then combined with the -OH on the surface of the single crystal silicon through the hydrogen bond force, forming a network film layer on the surface of the single crystal silicon, which becomes the nucleation starting point and assists in the production of velvet.
[0073] 4. The etching catalyst containing amino, carboxyl or halogen atoms used in the present invention, on the one hand, reduces the interaction between metal ions and the silicon surface through the carboxyl, amino or halogen atoms in the molecule and the metal ions complex; on the other hand, through its own high affinity with silicon, it adjusts the contact performance between the texturing liquid and the silicon surface, thereby promoting silicon dissolution. At the same time, when the etching catalyst is consumed to a certain concentration, it also has the function of balancing the etching rate, avoiding over-etching of single crystal silicon, and ensuring the texturing effect.
[0074] 5. The present invention relates to an alkaline water-based texturing additive system of polyhydroxy natural plant gum polymer, block polyether modified organosilicon anionic surfactant and polycarboxyl etching catalyst. When the mass ratio of the texturing additive to the alkali is 0.3-1.5:100, the texturing process at 82°C takes only 400 seconds to obtain a better texturing effect, and the reflection of the velvet pyramid size in the range of 0.8-3μm meets the texturing requirements. BRIEF DESCRIPTION OF THE DRAWINGS
[0075] Figure 1 : This is a 2500-fold magnified SEM picture of the velvet surface of a silicon wafer obtained under different mass ratios of the velvet additive and the alkali in Example 1 of the present invention:
[0076] Figure 2 : This is a SEM picture of the cross-section of the silicon wafer texture obtained under different mass ratios of the texture-making additive and the alkali in Example 1 of the present invention, which is magnified 10,000 times. DETAILED DESCRIPTION
[0077] The present invention will be further described below in conjunction with specific embodiments and accompanying drawings:
[0078] Examples 1-7 and Comparative Examples 1-6 disclose a variety of universal single crystal silicon texturing additives, the components and mass ratios of which are shown in Table 1.
[0079] The preparation method of the universal single crystal silicon texturing additive is as follows:
[0080] Step 1: Weigh the required amount of each component of the texturing additive according to the weight ratio;
[0081] Step 2: Divide the deionized water into two parts, with the mass ratio of the first part of deionized water to the second part of deionized water being 1:2. Under room temperature, first add all the components to the first part of deionized water, stir magnetically until all the components are completely mixed, then add the second part of deionized water, and continue stirring for 3 hours to obtain the universal single crystal silicon texturing additive.
[0082] Table 1 Example 1-Example 7
[0083]
[0084]
[0085] Table 2 Comparative Examples 1-6
[0086]
[0087] The preparation method of the texturing liquid of the present invention is as follows:
[0088] The universal single crystal silicon texturing additive, KOH and deionized water prepared above are weighed separately, and the texturing additive and KOH are added into the deionized water at 85° C. and stirred to mix evenly, so as to prepare the single crystal silicon etching texturing liquid.
[0089] About the use of velvet liquid:
[0090] The single crystal silicon wafer is placed in the texturing liquid for texturing reaction. The texturing temperature is 82°C and the texturing time is 400s. After the reaction is completed, the single crystal silicon wafer is taken out and the front and back sides of the silicon wafer are rinsed with deionized water and ethanol respectively for 20s, and then placed in a N2 atmosphere for drying.
[0091] About performance testing and description:
[0092] Performance test 1 Velvet performance test:
[0093] The texturing liquid is used for texturing, and the texture surface size of the texturing silicon wafer can be adjusted in the range of 0.8-3μm.
[0094] Performance Test 2 Reflectivity Measurement:
[0095] The absolute reflectivity was measured using a film thickness meter, and the obtained data was then integrated to obtain the weighted average reflectivity. The test results are shown in Table 3.
[0096] Table 3 Reflectivity test data of Examples 1-7 and Comparative Examples 1-6
[0097]
[0098] Analysis of the test results:
[0099] It can be seen from the test data in Table 3 that with the increase of the mass ratio of the texturing additive to the alkali, in the embodiment, the reflectivity is always maintained within the reflectivity standard value (9%-10.5%), proving that the texturing additive system proposed in the present invention successfully achieves the controllable preparation of the pyramid;
[0100] In the comparative example, the reflectivity is always greater than 10.5%, which proves that the comparative example system cannot achieve a good texturing effect.
[0101] The comparative example has a large suede surface and a high reflectivity, which is compared with the smaller suede surface of the present invention, where the reflectivity is still maintained at 9%-10.5%. The present invention is more adaptable to different battery circuit requirements.
[0102] When the mass ratio of the texturing additive to the alkali is the same, the reflectivity of the texturing liquid provided by Examples 1-7 of the present invention is within the reference standard range of 9%-10.5%, which proves that it meets the texturing requirements.
[0103] The reflectivity of comparative examples 1-6 is between 13% and 33%, which is above the standard value, proving that the suede surface prepared by the present invention is smaller, has a lower reflectivity, and is more adaptable to different battery circuit requirements.
[0104] The present invention adopts a combination of a velvet removal agent, a surfactant and a polycarboxyl etching catalyst, which can significantly improve the light trapping property of a velvet-made silicon wafer and successfully realize the controllable preparation of a velvet surface.
[0105] When the mass ratio of texturing additive to alkali is the same, only etching catalyst is added to the texturing additive of comparative example 1. Due to the lack of texturing and degassing components, the texturing and degassing cannot be effectively carried out, resulting in the silicon wafer floating on the water surface during texturing and texturing cannot be carried out. As the mass ratio of texturing additive to alkali increases, the reflectivity gradually increases.
[0106] The texturing additive of Comparative Example 2 contains only surfactant, which cannot effectively inhibit corrosion and remove the fluff due to the lack of key fluff-removing components, resulting in the etching reaction being too fast and uncontrollable, and causing the surface of the resulting texturized silicon wafer to be in a nearly polished state.
[0107] In comparative example 3, only a de-bubbling agent is added to the de-bubbling additive. Due to the lack of key de-bubbling and de-bubbling auxiliary components, de-bubbling cannot be done in time. The surfactant de-bubbling also has a certain de-bubbling auxiliary effect, resulting in a large number of one-sided raindrop defects.
[0108] Compared with Example 1, Comparative Example 4 does not add a linting agent. Since the system lacks effective linting components, the lint cannot be removed well, resulting in a nearly polished state on one side, and the effect is close to that of Comparative Example 2.
[0109] Compared with Example 1, Comparative Example 5 does not add surfactant. Due to the lack of effective defoaming components, defoaming cannot be done in time, resulting in a large number of poor raindrops on one side. The effect is close to that of Comparative Example 3.
[0110] Compared with Example 1, Comparative Example 6 does not add an etching catalyst. Due to the lack of etching components, the etching rate and etching depth cannot be effectively adjusted, resulting in a higher reflection when the height of the obtained velvet pyramid is below 1.0 μm.
[0111] Further comparison is made through the attached drawings in the specification:
[0112] Figure 1 This is a SEM picture of the surface of the silicon wafer textured surface obtained under different mass ratios of the texturing additive and the alkali in Example 1 of the present invention, magnified 2500 times.
[0113] The mass ratios of the texturing additive and the alkali are (a) 0.3:100; (b) 0.7:100; (c) 1.1:100; and (d) 1.5:100.
[0114] As can be seen from Figure a, when the mass ratio of the texturing additive to the alkali in the texturing solution is 0.3:100, the size of the textured silicon wafer pyramid is between 2.4-2.8μm;
[0115] As can be seen from Figure b, when the mass ratio of the texturing additive to the alkali in the texturing solution is 0.7:100, the size of the textured silicon wafer texture pyramid obtained is between 1.7-2.0μm;
[0116] As can be seen from Figure c, when the mass ratio of the texturing additive to the alkali in the texturing solution is 1.1:100, the size of the textured silicon wafer pyramid is between 1.2-1.5μm;
[0117] As can be seen from Figure d, when the mass ratio of the texturing additive to the alkali in the texturing solution is 1.5:100, the size of the textured surface pyramids of the obtained texturing silicon wafer is between 0.8-1.0μm.
[0118] Figure 2 This is a SEM picture of the cross-section of the textured surface of a silicon wafer obtained under different mass ratios of the texturing additive to the alkali in Example 1 of the present invention, magnified 10,000 times.
[0119] The mass ratios of the texturing additive and the alkali are (a) 0.3:100; (b) 0.7:100; (c) 1.1:100; and (d) 1.5:100.
[0120] As can be seen from Figure a, when the mass ratio of the texturing additive to the alkali in the texturing solution is 0.3:100, the height of the pyramid tower of the texturing silicon wafer is between 2.12-2.31μm;
[0121] As can be seen from Figure b, when the mass ratio of the texturing additive to the alkali in the texturing solution is 0.7:100, the height of the pyramid tower of the texturing silicon wafer is between 1.99-2.06μm;
[0122] As can be seen from Figure c, when the mass ratio of the texturing additive to the alkali in the texturing solution is 1.1:100, the height of the pyramid tower of the texturing silicon wafer is between 1.80-1.89μm;
[0123] As can be seen from Figure d, when the mass ratio of the texturing additive to the alkali in the texturing solution is 1.5:100, the height of the pyramids on the texturing surface of the resulting silicon wafer is between 1.54-1.60μm.
[0124] In summary, by using the texturing liquid in the embodiment for texturing, the texture surface size of the texturing silicon wafer can be adjusted in the range of 0.8-3 μm, and the tower height is controlled in the range of 1.50-2.5 μm.
[0125] Combination Figure 1 and Figure 2 It can be seen that in the embodiment, since polyhydroxy plant gum is introduced into the system to cooperate with block polyether modified silicone anionic surfactant and polycarboxyl etching catalyst, by changing the ratio of additives and alkali solution, controllable preparation of pyramids of different sizes can be achieved, and the size uniformity of the pyramids under various size conditions is good.
[0126] Its most obvious advantages are:
[0127] Advantage 1: The suede size can be adjusted within the range of 0.8-3μm.
[0128] The second advantage is that the suede has a high uniformity under each size condition.
[0129] Advantage three: the reflection of the textured silicon wafer meets the requirements under each size condition.
[0130] The present invention adopts cheap and easily available polyhydroxy natural plant gum as a fleece-making agent, and compounded with a low-foaming and high-efficiency block polyether modified organic silicon anionic surfactant to cooperate with an etching catalyst to make fleece. The fleece-making window is relatively wide. Within a certain range, by changing the ratio of additives to alkali solution, controllable preparation of pyramids of different sizes can be achieved, and the size uniformity of the pyramids under various size conditions is good. On the premise that the reflection meets the requirements, the size of the pyramids can be adjusted within a certain range.
[0131] The present invention is described exemplarily above in conjunction with the embodiments and drawings. It is obvious that the implementation of the present invention is not limited to the above-mentioned methods. As long as various improvements are made using the method concept and technical solution of the present invention, or the concept and technical solution of the present invention are directly applied to other occasions without improvement, they are all within the protection scope of the present invention.
Claims
1. A universal single crystal silicon texturing additive, characterized in that: Calculated by weight, it includes the following components:
2. The universal single crystal silicon texturing additive according to claim 1, characterized in that: The fleece-forming agent is a polyhydroxylated plant gum-type natural macromolecular compound; The polycarboxyl etching catalyst is one or more of nitrilotriacetic acid, triethanolaminetriacetic acid, aminotriacetic acid, glycyl-glycine, glycyl-glycyl-glycine, L-leucylglycylglycine, chloroacetylglycylglycine, (2,4-dichlorobenzoyl)glycyl-glycine, N-(2-bromo-1-oxopropyl)glycyl-glycine and their sodium salts; The inorganic base is one of NaOH and KOH or a mixture of the two.
3. The universal single crystal silicon texturing additive according to claim 2, characterized in that: The polyhydroxy plant gum natural polymer compound is one or a mixture of fennel gum, bletilla striata gum, locust bean gum, agar-agar gum, cashew nut shell gum and aloe vera gum; The polycarboxyl etching catalyst is one or more of chloroacetyl glycyl glycine, (2,4-dichlorobenzoyl) glycyl-glycine, N-(2-bromo-1-oxopropyl)-glycyl-glycine and sodium salts thereof.
4. The universal single crystal silicon texturing additive according to claim 1, characterized in that: The surfactant is a block polyether modified organosilicon anionic surfactant in the following formula: In the formula, m represents the addition number of -(CH3)2SiO groups, and its value is an integer from 0 to 5; n represents -(CH3)SiO(C3H6O(C2H4) a (C3H6O) b The number of addition of R) groups is an integer from 1 to 5; a represents the addition number of ethylene oxide groups, which is an integer from 3 to 14; b represents the addition number of propylene oxide groups, which is an integer of 4-20; R is an anionic group, which is either a sulfonic acid group or a carboxyl group; The molecular weight of the surfactant is 500-10000.
5. A method for preparing the universal single crystal silicon texturing additive according to any one of claims 1 to 4, characterized in that The following steps are involved: Step 1: Weigh the required amount of each component of the texturing additive according to the weight ratio; Step 2: At room temperature, first add all components except deionized water to 1 / 3-1 / 2 deionized water, stir magnetically until all components are completely mixed, then add the remaining deionized water, and continue stirring for 2-3 hours to obtain the universal single crystal silicon texturing additive.
6. Use of the universal single crystal silicon texturing additive as described in any one of claims 1 to 4 in the field of single crystal silicon wet etching texturing.
7. A texturing liquid, characterized in that: It comprises the universal single crystal silicon texturing additive as described in any one of claims 1 to 4, alkali and deionized water.
8. The texturing liquid according to claim 7, characterized in that: The mass ratio of the universal single crystal silicon texturing additive to the alkali is 0.1-2:100; The alkali is NaOH and / or KOH.
9. A method for preparing the texturing liquid according to any one of claims 7 to 8, characterized in that The following steps are involved: The universal single crystal silicon texturing additive, alkali and deionized water are weighed according to the mass ratio, and the universal single crystal silicon texturing additive and alkali are added into the deionized water at 80-85° C. and stirred to mix evenly, so as to prepare the texturing liquid.
10. A method for using the texturing liquid according to any one of claims 7 to 8, characterized in that The following steps are involved: The single crystal silicon wafer is placed in the texturing liquid for texturing reaction, the texturing temperature is 80-85°C, and the texturing time is 360-420s. After the reaction is completed, the single crystal silicon wafer is taken out and the front and back sides of the silicon wafer are rinsed with deionized water and ethanol respectively, and then placed in a N2 atmosphere for drying.
Citation Information
Cited By
Two-step texturing additive, two-step texturing liquid, preparation method and application
CN121087624A
A two-step texturizing additive, a two-step texturizing solution, a preparation method and use thereof
CN121087624B
Roughening and texturing working agent for surface treatment of semiconductor silicon-based parts and preparation method of roughening and texturing working agent
CN121802549A