Delayed fracture test apparatus and delayed fracture test method, press forming method
The delayed fracture test device and method apply uniaxial tensile stress to accurately detect cracks in press-formed products, addressing the inaccuracy of existing methods and enabling the prevention of delayed fractures in critical regions.
Patent Information
- Application Number
- JP2022100083
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-06-22
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2042-06-22
AI Technical Summary
Existing methods for evaluating delayed fracture in press-formed products using high-strength steel sheets are inaccurate and cannot reliably detect cracks under uniaxial tensile stress, leading to errors in determining delayed fracture characteristics and making it difficult to prevent such fractures in critical regions.
A delayed fracture test device and method that applies uniaxial tensile stress to a test piece in a hydrogen penetration environment, using a jig to detect strain and crack occurrence in the parallel portion, allowing for accurate detection of cracks through strain time history analysis.
Enables precise detection of cracks in press-formed products, determining delayed fracture characteristics, and allows for the establishment of press forming conditions to prevent delayed fracture, ensuring the production of fracture-resistant products.
Smart Images

Figure 0007563424000002 
Figure 0007563424000003 
Figure 0007563424000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a delayed fracture testing apparatus and a delayed fracture testing method for determining the delayed fracture characteristics of a portion of a press-formed product where delayed fracture is a concern, and a press forming method for press-forming a portion of a press-formed product using a steel plate that is at risk of delayed fracture by taking measures against delayed fracture. [Background technology]
[0002] In response to stricter regulations on reducing carbon dioxide emissions, there is a demand for lighter car bodies to improve fuel efficiency. At the same time, there is also a demand for improved collision safety performance. In response to these needs, the use of high-tensile steel plates with a tensile strength of 1 GPa or more in the structural components of car bodies is progressing.
[0003] Automobile body structural parts are generally manufactured by press forming. However, there are concerns about delayed fracture in structural parts (press-formed products) press-formed using high-tensile steel plates with a tensile strength of over 980 MPa. Delayed fracture is thought to be caused by strain and stress (residual stress) that occurs from the press forming process to the process of assembling the structural parts, and by hydrogen that enters the structural parts during the manufacture and use of the automobile.
[0004] Therefore, several methods and devices have been proposed for evaluating the delayed fracture properties of press-formed products made from high-tensile steel sheets according to the manufacturing conditions (press forming conditions). For example, Patent Document 1 discloses a method for evaluating delayed fracture properties by applying stress to the bent portion of a thin steel plate bent into a V shape and holding the plate in this state in a hydrogen penetration environment based on the occurrence of cracks in the bent portion, and also discloses a stress application jig for applying stress to the bent portion. Furthermore, Patent Document 2 discloses a technique in which a thin steel plate is bent into a U-shape and subjected to a load stress, and then hydrogen is charged into a U-shaped test piece, and the hydrogen embrittlement properties (delayed fracture properties) of the thin steel plate are evaluated taking into account the effects of the load stress, residual stress, bending R, etc. of the test piece. Furthermore, Patent Document 3 discloses a technique for evaluating delayed fracture properties based on the time until cracks occur in a U-bent portion having a strain gauge attached to the surface. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2010-107297 A [Patent Document 2] JP 2005-134152 A [Patent Document 3] Japanese Patent Application Publication No. 7-146225 Summary of the Invention [Problem to be solved by the invention]
[0006] According to the technology disclosed in Patent Document 1, it is possible to apply uniaxial tensile stress to the processed surface of a bent part, and according to the technology disclosed in Patent Document 2, it is possible to control the hydrogen concentration distribution in a part that has been U-bent and loaded with stress. However, in order to detect the occurrence of delayed fracture using these technologies, the occurrence of cracks must be judged visually, so it is not possible to detect the occurrence of cracks with high accuracy, and there are cases where a large error occurs in the crack judgment results, which is a problem. In addition, in the technology disclosed in Patent Document 3, a strain gauge is attached to the processed surface of the part after U-bending, and the change in the load acting on the processed part is detected based on the strain measured by the strain gauge, so the error in crack judgment is small. However, this technology has problems such as the fact that the contact of the strain gauge with the solution and material affects the evaluation results of delayed fracture properties, and that it cannot be used to evaluate delayed fracture properties in places where a strain gauge cannot be attached, such as the processed surface of a V-bend.
[0007] Furthermore, conventional delayed fracture testing equipment and evaluation methods use bent test pieces, but because bending has a stress distribution in the thickness direction, it is more complicated than a uniaxial stress state, and there was a problem that it could not be applied to evaluations other than the bent parts of parts.
[0008] As described above, several techniques for evaluating delayed fracture properties have been proposed so far, but no delayed fracture test method or device has been proposed that can accurately detect the occurrence of delayed fracture (cracks) and apply uniaxial tensile stress uniformly. As a result, it has not been possible to take appropriate measures to prevent delayed fracture from occurring in areas where delayed fracture is a concern (areas where delayed fracture is a concern) in press-formed products using steel sheets.
[0009] The present invention has been made in order to solve the above-mentioned problems, and an object of the present invention is to provide a delayed fracture testing apparatus capable of detecting cracks with high accuracy in a delayed fracture test in which a uniaxial tensile test piece loaded with a predetermined tensile stress is held in a predetermined hydrogen penetration environment. Another object of the present invention is to provide a delayed fracture testing method for determining the presence or absence of delayed fracture in a portion of a press-formed product where delayed fracture is suspected, based on the results of a delayed fracture testing using a delayed fracture testing apparatus. Furthermore, the present invention aims to provide a press-forming method for a press-formed product in which measures are appropriately taken to suppress the occurrence of delayed fracture in a portion of a press-formed product using a steel plate where delayed fracture is a concern. [Means for solving the problem]
[0010] (1) The delayed fracture testing apparatus according to the present invention is for carrying out a delayed fracture test in which a uniaxial tensile test piece is held in a predetermined hydrogen penetration environment while a predetermined uniaxial tensile stress is applied to a parallel portion of the uniaxial tensile test piece, A jig is provided for applying a predetermined uniaxial tensile stress to the parallel portion of the uniaxial tensile test piece, and a strain is generated in association with the parallel portion, The jig is characterized by having a function of acquiring the time history of strain generated in the jig so as to enable detection of cracks that occur in the parallel portion of the uniaxial tensile test piece that is held in a hydrogen penetration environment while being loaded with uniaxial tensile stress using the jig.
[0011] (2) The delayed fracture test apparatus according to the present invention is for carrying out a delayed fracture test in which a uniaxial tensile test piece is held in a predetermined hydrogen penetration environment while a predetermined uniaxial tensile stress is applied to a parallel portion of the uniaxial tensile test piece, A jig including a pair of gripping parts for gripping both ends of the uniaxial tensile test piece, and a stress loading part having a rod-shaped body that applies a predetermined uniaxial tensile stress to the parallel part of the uniaxial tensile test piece by applying a load in a direction to pull the pair of gripping parts in a state where the both ends of the uniaxial tensile test piece are gripped, and generates a strain in conjunction with the parallel part; a strain gauge attached to the rod-shaped body to detect strain generated in the rod-shaped body; and a strain time history acquisition unit that acquires the time history of the strain detected by the strain gauge.
[0012] (3) A delayed fracture testing method according to the present invention uses the delayed fracture testing apparatus described in (1) or (2) above to determine delayed fracture initiation characteristics of a delayed fracture susceptible portion in a press-formed product, which is susceptible to delayed fracture, and comprises: A press molding condition setting process for setting press molding conditions for the press molded product; A delayed fracture risk portion stress and strain calculation step of calculating stress and strain at the delayed fracture risk portion of the press-formed product; a uniaxial tensile test piece production process for producing a uniaxial tensile test piece in which the calculated strain of the portion at risk of delayed fracture is imparted to a parallel portion; a delayed fracture test step of applying the stress calculated in the delayed fracture risk region stress and strain calculation step to the parallel portion of the uniaxial tensile test piece produced in the uniaxial tensile test piece production step using the jig of the delayed fracture test apparatus, and holding the uniaxial tensile test piece in a predetermined hydrogen penetration environment while applying the stress, and acquiring a time history of the strain generated in the jig; A uniaxial tensile test piece crack detection process for detecting a crack occurring in the parallel portion of the uniaxial tensile test piece based on the acquired time history of the strain, and acquiring a crack occurrence time at which the detected crack occurs; and a delayed fracture characteristic acquisition process for determining the delayed fracture characteristics of the portion of the press-formed product at which delayed fracture is suspected, based on the acquired crack initiation time in the parallel portion, the strain applied to the parallel portion of the uniaxial tensile test piece, and the stress loaded on the parallel portion.
[0013] (4) In the above (3), In the delayed fracture risk portion stress and strain calculation step, an equivalent plastic strain and a maximum principal stress in the delayed fracture risk portion are calculated, In the uniaxial tensile test piece manufacturing step, a strain corresponding to the calculated equivalent plastic strain is applied to the parallel portion, The delayed fracture test step is characterized in that a uniaxial tensile stress equivalent to the calculated maximum principal stress is applied to the parallel portion.
[0014] (5) A press-forming method according to the present invention is a method for applying a measure to suppress the occurrence of delayed fracture to a portion at which delayed fracture is likely to occur in a press-formed product using a steel plate, and press-forming the press-formed product, A temporary press molding condition setting process for setting temporary press molding conditions for the press-molded product; a delayed fracture risk portion stress and strain calculation step of calculating stress and strain of a delayed fracture risk portion in the press-formed product press-formed under the tentative press-forming conditions; a uniaxial tensile test piece production process for producing a uniaxial tensile test piece by applying the calculated strain to a parallel portion; a delayed fracture test step of applying the stress calculated in the delayed fracture suspected portion stress and strain calculation step to the parallel portion of the manufactured uniaxial tensile test piece using the jig of the delayed fracture test apparatus according to claim 1, and holding the uniaxial tensile test piece in a predetermined hydrogen penetration environment while applying the stress, and acquiring a time history of the strain detected by the strain gauge attached to the jig; A uniaxial tensile test piece crack occurrence determination process for determining whether or not cracks have occurred in the parallel portion of the uniaxial tensile test piece based on the acquired time history of strain generated in the jig; A temporary press molding condition changing process for changing the temporary press molding conditions when it is determined that cracks have occurred in the uniaxial tensile test piece crack occurrence determining process; A repeating process of repeatedly executing the provisional press forming condition changing process, the delayed fracture risk portion stress and strain calculating process, the uniaxial tensile test piece manufacturing process, the delayed fracture testing process, and the uniaxial tensile test piece crack occurrence determining process until it is determined that no cracks have occurred in the uniaxial tensile test piece crack occurrence determining process; When it is determined that no cracks occur in the uniaxial tensile test piece crack occurrence determination process, the tentative press molding conditions in that case are determined as the press molding conditions of the press molded product. and a press forming step of press-forming the steel sheet into the press-formed product under the determined press forming conditions.
[0015] (6) A press-forming method according to the present invention is a method for applying a measure to suppress the occurrence of delayed fracture to a portion at which delayed fracture is likely to occur in a press-formed product using a steel plate, and press-forming the press-formed product, A temporary press molding condition setting process for setting temporary press molding conditions for the press-molded product; a delayed fracture risk portion stress and strain calculation step of calculating stress and strain of a delayed fracture risk portion in the press-formed product press-formed under the tentative press-forming conditions; a uniaxial tensile test piece production process for producing a uniaxial tensile test piece by applying the calculated strain to a parallel portion; a delayed fracture test step of applying the stress calculated in the delayed fracture suspected portion stress and strain calculation step to the parallel portion of the manufactured uniaxial tensile test piece using the jig of the delayed fracture test apparatus according to claim 1, and holding the uniaxial tensile test piece in a predetermined hydrogen penetration environment while applying the stress, and acquiring a time history of the strain detected by the strain gauge attached to the jig; A uniaxial tensile test piece crack occurrence determination process for determining whether or not cracks have occurred in the parallel portion of the uniaxial tensile test piece based on the acquired time history of strain generated in the jig; A stress and strain changing process for changing the strain applied to the parallel portion of the uniaxial tensile test piece and / or the stress applied to the parallel portion when it is determined that a crack has occurred in the uniaxial tensile test piece crack occurrence determining process; A repeating process of repeatedly executing the stress and strain changing process, the uniaxial tensile test piece manufacturing process, the delayed fracture testing process, and the uniaxial tensile test piece crack occurrence determining process until it is determined that no cracks have occurred in the uniaxial tensile test piece crack occurrence determining process; When it is determined that no cracks occur in the uniaxial tensile test piece crack occurrence determination process, a press molding condition determination process is performed to determine the press molding conditions of the press molded product so that the stress and strain in that case are obtained; and a press forming step of press-forming the steel sheet into the press-formed product under the determined press forming conditions.
[0016] (7) In the above (5) or (6), the delayed fracture risk portion stress and strain calculation step calculates an equivalent plastic strain and a maximum principal stress in the delayed fracture risk portion, In the uniaxial tensile test piece manufacturing step, a strain corresponding to the calculated equivalent plastic strain is applied to the parallel portion, The delayed fracture test step is characterized in that a uniaxial tensile stress equivalent to the calculated maximum principal stress is applied to the parallel portion. Effect of the Invention
[0017] According to the present invention, in a delayed fracture test in which the stress and strain of a portion of a press-formed product at which delayed fracture is suspected is reproduced in the parallel portion of a uniaxial tensile test piece, cracks occurring in the parallel portion can be detected with high accuracy, and the delayed fracture characteristics of the portion of a press-formed product at which delayed fracture is suspected can be determined. Furthermore, according to the present invention, press-molding conditions capable of preventing delayed fracture in the portion at which delayed fracture is suspected can be determined based on the delayed fracture characteristics of the portion at which delayed fracture is suspected in the press-molded product, thereby making it possible to manufacture a press-molded product with measures taken against delayed fracture. [Brief description of the drawings]
[0018] [Figure 1] FIG. 1 is a diagram illustrating the configuration of a delayed fracture testing device according to the first embodiment. [Diagram 2] FIG. 2 is a diagram for explaining one embodiment of a jig for applying a constant tensile stress to a parallel portion of a uniaxial tensile test piece in the delayed fracture testing apparatus according to the first embodiment. [Diagram 3] FIG. 2 is a flow chart showing a process flow of the delayed fracture testing method according to the first embodiment. [Figure 4] 1 is a graph showing the time history of strain generated in a jig in a delayed fracture test using a delayed fracture testing apparatus according to the first embodiment, and the detection of cracks generated in a parallel portion of a uniaxial tensile test piece based on the time history of strain. [Diagram 5] 2 is a graph showing the results of the crack initiation time at which a crack occurred in a uniaxial tensile test piece, obtained by a delayed fracture test using the delayed fracture testing apparatus according to the first embodiment of the present invention. [Figure 6]FIG. 11 is a diagram for explaining another embodiment of the jig for applying a constant tensile stress to the parallel portion of the uniaxial tensile test piece in the delayed fracture testing apparatus according to the first embodiment. [Figure 7] FIG. 11 is a diagram showing a process flow in a press-molding method according to one aspect of the second embodiment of the present invention. [Figure 8] FIG. 11 is a diagram showing a process flow in a press-molding method according to another aspect of the second embodiment of the present invention. [Figure 9] 1A and 1B are diagrams showing a press-formed product that was the subject of a delayed fracture test and measures against delayed fracture in the examples ((a) is a perspective view, (b) is a cross-sectional view). [Figure 10] FIG. 2 is a contour diagram showing the longitudinal maximum principal stress distribution and the equivalent plastic strain distribution calculated for a press-formed product in the examples ((a) longitudinal maximum principal stress distribution, (b) equivalent plastic strain distribution). [Figure 11] This graph shows the relationship between strain and hydrogen concentration obtained by a hydrogen charging test using test pieces to which strain was applied in various deformation modes, with an immersion time of 30 hours ((a) relationship between equivalent plastic strain and hydrogen concentration, (b) relationship between strain mode and hydrogen concentration). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] <Background to the invention> As described above, in press-formed products of high-tensile steel sheets, there is concern about delayed fracture due to strain and stress generated in the press-formed product during press forming and hydrogen that penetrates into the press-formed product. Therefore, a possible measure to suppress delayed fracture in the press-formed product is to manufacture the press-formed product under press forming conditions that prevent delayed fracture from occurring in the region where delayed fracture is a concern.
[0020] In order to find press forming conditions under which delayed fracture does not occur, the inventors considered it necessary to determine the stress and strain in areas where delayed fracture is a concern, simulate the determined stress and strain in a test piece, conduct a delayed fracture test, and accurately detect cracks that occur in the test piece. The researchers then came up with the idea that by repeatedly conducting such delayed fracture tests, it might be possible to determine the press-molding conditions for manufacturing press-molded products so that the stress and strain would not cause delayed fracture in areas where delayed fracture is a concern.
[0021] The inventors then investigated a method for realizing this idea. First, regarding the stress and strain in areas of a press-formed product where delayed fracture is a concern, the inventors considered that these could be obtained by CAE analysis using the finite element method, such as press forming analysis, shear analysis of cutting, trimming, piercing, etc. of the plate material before press forming, and springback analysis.
[0022] Next, in order to perform a delayed fracture test by simulating the stress and strain found for the portion at which delayed fracture is suspected in a test piece, the inventors investigated the stress and strain to be reproduced in the test piece and the shape of the test piece.
[0023] In fracture mechanics, it is believed that the stress that initiates and propagates cracks is not stress in the compression direction, but stress in the tension direction. Based on this idea, the inventors considered that there is a risk of delayed fracture occurring in the areas of press-formed products where tensile stress occurs. To verify this, the inventors placed bent press-formed products in a specified hydrogen penetration environment for a certain period of time and investigated the areas where delayed fracture occurs. As a result, it was confirmed that cracks (delayed fracture) occurred in the press-formed products in the center of the plate thickness near the bend apex, where the maximum principal stress, which corresponds to the stress in the tension direction, is the largest.
[0024] From the above investigation, the inventors have concluded that delayed fracture is a concern in the press-formed product at the part where the value of the maximum principal stress corresponding to the stress in the tensile direction is high. Therefore, the inventors have considered that it is preferable to uniformly apply the stress in the tensile direction, i.e., the positive maximum principal stress, to the test piece in order to reproduce the stress at the part where delayed fracture is a concern in the delayed fracture test using the test piece. And, in order to realize this, it has been found that a test piece with a shape that can uniformly apply the positive maximum principal stress and a jig that can apply the stress equivalent to the maximum principal stress are required.
[0025] In addition, delayed fracture is caused by hydrogen that penetrates into press-formed products, and the more hydrogen that penetrates, the more likely delayed fracture occurs. The amount of hydrogen that penetrates into press-formed products is thought to be related to the plastic strain that occurs in the press-formed products. In other words, it is thought that as the plastic strain increases, the number of defects that trap hydrogen increases, and the amount of hydrogen that penetrates into press-formed products also increases.
[0026] On the other hand, press-formed products made by press-forming high-tensile steel sheets have strains caused by various deformation modes, such as bending (plane strain), extension (biaxial tension), uniaxial tension, uniaxial compression, etc. Therefore, the inventors prepared test pieces of high-tensile steel sheets to which strains were applied in various deformation modes, and after placing the test pieces in a hydrogen penetration environment for a certain period of time, carried out a hydrogen charging test to measure the amount of hydrogen in the test pieces, and investigated the relationship between strains caused by different deformation modes and hydrogen concentration. In this study, 1.2 mm thick, 1470 MPa grade cold rolled steel sheets were used as test materials, and strain was applied in the deformation modes of rolling (plane strain), uniaxial tension, uniaxial compression, or biaxial tension-compression.
[0027] Figure 11 shows an example of the results of measuring the amount of hydrogen in a test piece with strain applied in various deformation modes after immersing it in ammonium thiocyanate and McIlvaine buffer solution with a pH of 4.0 and a concentration of 0.1% for 30 hours, and then summarizing the results in terms of the relationship between hydrogen concentration and strain. Here, Figure 11(a) shows the equivalent plastic strain ε p eq and hydrogen concentration, and Fig. 11(b) shows the relationship between the equivalent plastic strain ε p eq 11(b) shows the relationship between the deformation mode and hydrogen concentration when the strain ratio is constant (=0.01, 0.02). Regarding the relationship between the ratio of the maximum principal strain to the minimum principal strain (hereinafter referred to as the "strain ratio") and the deformation mode in Fig. 11(b), a strain ratio of 1 represents biaxial tension, a strain ratio of 0 represents plane strain, and a strain ratio of -2 represents uniaxial tension and uniaxial compression.
[0028] As shown in FIG. 11, the inventors found that the hydrogen concentration is independent of the deformation mode and is proportional to the equivalent plastic strain ε p eq The reason why the hydrogen concentration increases with increasing equivalent plastic strain is thought to be that the number of defects in the test specimen that trap hydrogen increases with increasing equivalent plastic strain, and therefore the amount of hydrogen that penetrates into the test specimen increases.
[0029] Therefore, it was found that in order to reproduce the strain in a portion of a press-formed product where delayed fracture is a concern, it is preferable to impart to a test piece a strain equivalent to the equivalent plastic strain in the portion where delayed fracture is a concern.
[0030] For example, in the case of a 1,470 MPa grade cold-rolled steel sheet having a thickness of 1.2 mm, if the equivalent plastic strain is 0.03 or less, a uniform uniaxial or biaxial strain equivalent to the desired equivalent plastic strain can be applied by uniaxial tension, uniaxial compression, or biaxial tension.
[0031] However, when the equivalent plastic strain exceeds 0.03, necking, which is a localized deformation, occurs in uniaxial tension and biaxial tension, and buckling, which is a localized out-of-plane deformation, occurs in uniaxial compression, making it difficult to impart uniform strain. Therefore, when the equivalent plastic strain exceeds 0.03, it was decided to impart a uniform plane strain by rolling.
[0032] Next, the inventors conducted a study on a test piece that reproduces the stress and strain of a portion of a press-formed product where delayed fracture is a concern. Although the shape of the test piece to which the strain equivalent to the desired equivalent plastic strain is uniformly applied is not considered to be particularly limited, the inventors decided to utilize a uniaxial tensile test piece used in a normal uniaxial tensile test, because in the uniaxial tensile test piece, a uniaxial tensile stress equivalent to the maximum positive principal stress can be uniformly applied to the parallel part where cracks occur in a normal uniaxial tensile test. Therefore, we decided to produce uniaxial tensile test specimens in which a strain equivalent to the equivalent plastic strain in the area of concern for delayed fracture was uniformly applied to the parallel portion by cutting out steel plates to which uniform strain had been applied through bending (plane strain), extension (biaxial tension), uniaxial tension, uniaxial compression, etc.
[0033] Next, the inventors conducted a study on detecting cracks in test pieces with high accuracy in delayed fracture tests. In conventional delayed fracture tests, a strain gauge is attached to a test piece and placed in an environment that allows hydrogen to penetrate, such as an acid solution. However, this method has two problems: contact between the strain gauge and the test piece, and contact between the strain gauge and the solution.
[0034] When a strain gauge is attached to a test specimen, the part of the test specimen where the strain gauge is attached does not come into contact with the solution, which may prevent hydrogen from penetrating into the test specimen and affect the occurrence of delayed fracture.
[0035] In addition, if the lead wires of the strain gauge or the adhesive used to attach the strain gauge react with the solution, the pH of the solution changes, reducing the amount of hydrogen that penetrates into the test piece. Therefore, the adhesives and lead wires used with the strain gauge must be made of components that do not react with the solution.
[0036] Furthermore, when changing test conditions such as the strain applied to the test piece or the stress applied, or when repeating tests under the same test conditions, it is necessary to attach a strain gauge to the test piece for each test. Therefore, attaching a strain gauge to the test piece is inconvenient for use in delayed fracture tests that require many tests, and there is a problem in terms of test efficiency.
[0037] In order to solve these inconveniences and problems, the inventors have conducted extensive research and have come up with the idea of embedding a strain gauge in a jig for applying stress to a uniaxial tensile test piece, and detecting cracks in the parallel portion of the uniaxial tensile test piece based on the time history of strain generated in the jig in conjunction with the parallel portion of the uniaxial tensile test piece.
[0038] In this case, it is necessary that the strain occurring in the parallel part of the uniaxial tensile test piece is interlocked with the strain occurring in the jig, and that the change in the strain in the parallel part can be detected. On the other hand, there is an advantage that the problem of the strain gauge coming into contact with the solution and the uniaxial tensile test piece can be eliminated. Furthermore, since it is not necessary to attach the strain gauge to the uniaxial tensile test piece every time a delayed fracture test is performed, it is considered to be excellent in test efficiency.
[0039] From the above-mentioned investigation results, it was found that the delayed fracture test of a test piece that reproduces the stress and strain in the delayed fracture-prone portion of a press-formed product can be performed, and the occurrence of cracks in the test piece can be detected with high accuracy. Furthermore, it was concluded that by repeatedly performing such delayed fracture tests, it is possible to determine press-forming conditions that can prevent the delayed fracture from occurring in the delayed fracture-prone portion. Then, by performing press-forming under the press-forming conditions determined in this way, it is possible to manufacture a press-formed product in which measures have been taken to suppress the occurrence of delayed fracture.
[0040] The present invention has been made based on the above-mentioned investigation results, and the specific configuration is as follows.
[0041] [Embodiment 1] <Delayed fracture testing equipment> An example of a delayed fracture test apparatus 1 according to the first embodiment of the present invention is shown in FIG. The delayed fracture test apparatus 1 is for carrying out a delayed fracture test in which a uniaxial tensile test piece 101 is held in a predetermined hydrogen entry environment 111 while a predetermined tensile stress is applied to the parallel portion 103 of the uniaxial tensile test piece 101. The delayed fracture test apparatus 1 is equipped with a jig 3 that applies a predetermined uniaxial tensile stress to the parallel portion 103 of the uniaxial tensile test piece 101 and generates strain in conjunction with the parallel portion 103. Furthermore, the delayed fracture test apparatus 1 has a function of acquiring a time history of strain generated in the jig 3 so that a crack generated in the parallel portion 103 of the uniaxial tensile test piece 101 held in a hydrogen entry environment 111 while a uniaxial tensile stress is applied using the jig 3 can be detected.
[0042] A delayed fracture testing apparatus 1 shown in FIG. 1 is an example of a specific aspect of this embodiment, and includes a jig 3, a strain gauge 5, and a strain-time history acquiring unit .
[0043] <Jig> As shown in FIG. 2, the jig 3 includes a pair of gripping portions 9 and a stress applying portion 11 . The pair of gripping portions 9 grip both ends 105 of the uniaxial tensile test piece 101 . The stress loading section 11 loads a predetermined tensile stress on the parallel section 103 of the uniaxial tensile test piece 101 by applying a load in a direction separating the pair of gripping sections 9 that are gripping both ends 105 of the uniaxial tensile test piece 101. Furthermore, the stress loading portion 11 is a rod-shaped body in which strain occurs in conjunction with the parallel portion 103, and has a pair of bolts 13 on either side of the uniaxial tensile test piece 101, and two lock nuts 15, one above and one below, screwed into each bolt.
[0044] The bolts 13 are screwed into both the left and right ends of the upper and lower gripping portions 9 . The lock nut 15 is screwed onto the bolt 13 between the upper and lower gripping portions 9 . Then, by tightening the lock nut 15 screwed onto the bolt 13 to generate a pressing force against the upper and lower gripping portions 9, a load is applied in a direction that pulls the pair of gripping portions 9 apart. At this time, the upper and lower lock nuts 15 receive a reaction force from the gripping portion 9 in a direction that brings them closer to each other, causing a compressive strain to occur in the shaft portion 13a of the bolt 13. Therefore, the strain gauge 5 attached to the shaft portion 13a outputs a strain whose positive and negative polarities are opposite to those of the parallel portion 103 of the uniaxial tensile test piece 101.
[0045] In this way, a uniaxial tensile stress is applied to the parallel portion 103 by the bolt 13 and the lock nut 15 , and in conjunction with the strain generated in the parallel portion 103 , a strain is generated in the shaft portion 13 a of the bolt 13 . By adjusting the tightening torque of the lock nut 15, a predetermined uniaxial tensile stress can be applied to the parallel portion 103 of the uniaxial tensile test piece 101.
[0046] The left and right lock nuts 15 are tightened so that their torque values are the same, thereby preventing a rotational moment from being applied to the uniaxial tensile test piece 101. In addition, by using a lock nut 15 in the stress application portion 11, the tightening force on the gripping portion 9 side is not loosened, and it is preferable to prevent a decrease in the load applied to the parallel portion 103 of the uniaxial tensile test piece 101.
[0047] <Strain gauge> The strain gauge 5 is attached to a shaft portion 13a of a bolt 13, which is a rod-shaped body of the jig 3, and detects strain occurring in the shaft portion 13a. In the present embodiment 1, the strain gauge 5 is embedded in the shaft portion 13a of the bolt 13 as shown in FIG.
[0048] <Strain time history acquisition section> The strain-time history acquisition unit 7 acquires the strain-time history of the shaft portion 13 a of the bolt 13 detected by the strain gauge 5 . In the present embodiment 1, the strain-time history acquiring unit 7 includes a strain measuring instrument that measures strain based on a signal output from the strain gauge 5, and a strain recorder that records the time history of the strain measured by the strain measuring instrument. In the strain-time history acquiring unit 7, the strain measuring instrument is connected to the strain gauge 5 via a lead wire 17.
[0049] <Delayed fracture test method> The delayed fracture testing method according to the first embodiment of the present invention uses the delayed fracture testing apparatus 1 according to the first embodiment described above to determine the delayed fracture properties of a portion of a press-formed product at risk of delayed fracture. As shown in Fig. 3, the delayed fracture testing method includes a step S1 of calculating stress and strain of a portion at risk of delayed fracture, a step S3 of producing a uniaxial tensile test piece, a delayed fracture testing step S5, a step S7 of detecting cracks in the uniaxial tensile test piece, and a step S9 of acquiring delayed fracture properties of a portion at risk of delayed fracture.
[0050] <Process for calculating stress and strain in areas at risk of delayed fracture> The delayed fracture risk portion stress and strain calculation step S1 is a step of calculating the stress and strain in the delayed fracture risk portion of the press-formed product. The stress and strain in a portion of a press-formed product where delayed fracture is a concern can be calculated, for example, by using a computer to perform a CAE analysis using the finite element method of the process of press-forming the press-formed product. In the first embodiment, the delayed fracture suspected region stress and strain calculation step S1 calculates the maximum principal stress as the stress in the delayed fracture suspected region and the equivalent plastic strain as the strain in the delayed fracture suspected region.
[0051] <Uniaxial tensile test piece manufacturing process> The uniaxial tensile test piece production process S3 is a process for producing a uniaxial tensile test piece 101 (Figures 1 and 2) in which the strain of the area at risk of delayed fracture calculated in the stress and strain calculation process S1 is applied to the parallel portion 103.
[0052] In this embodiment 1, the uniaxial tensile test specimen production process S3 involves imparting a strain equivalent to the equivalent plastic strain calculated for the area at risk of delayed fracture to a steel plate, and cutting the steel plate so that the strain becomes the parallel portion 103, thereby producing a uniaxial tensile test specimen 101.
[0053] In this case, when the equivalent plastic strain in the portion at risk of delayed fracture is relatively small, a uniform uniaxial strain or biaxial strain equivalent to the desired equivalent plastic strain can be imparted to the steel plate by uniaxial tension, uniaxial compression or biaxial tension. In contrast, when the equivalent plastic strain in a portion at which delayed fracture is likely to occur is relatively large, a uniform plane strain can be imparted to the steel sheet by rolling.
[0054] For example, in a 1.2 mm thick 1470 MPa grade cold rolled steel sheet, if the equivalent plastic strain is relatively small, 0.03 or less, strain may be imparted by uniaxial tension, uniaxial compression or biaxial tension, whereas if the equivalent plastic strain is relatively large, exceeding 0.03, strain may be imparted by rolling.
[0055] <Delayed fracture test process> In the delayed fracture testing process S5, as shown in FIG. 1, a predetermined stress is applied to the parallel portion 103 of the uniaxial tensile test piece 101 using the jig 3 of the delayed fracture testing apparatus 1, and a delayed fracture test is performed in which the test piece is held under a predetermined hydrogen penetration environment 111, and the time history of the strain generated in the jig 3 is obtained.
[0056] Here, the uniaxial tensile test piece 101 is one that has been produced in the above-mentioned uniaxial tensile test piece production process S3, and a predetermined strain has been applied to the parallel portion 103. In addition, the specified stress applied to the parallel portion 103 is the stress of the portion at risk of delayed fracture calculated in the above-mentioned stress and strain calculation process S1 of the portion at risk of delayed fracture, and in this embodiment, it is the maximum principal stress of the portion at risk of delayed fracture.
[0057] In this embodiment 1, the delayed fracture testing process S5, as shown in Figure 1, uses a strain time history acquisition unit 7 to acquire the time history of strain detected by a strain gauge 5 attached to the shaft portion 13a of a bolt 13, which is a rod-shaped body of the jig 3.
[0058] <Uniaxial tensile test piece crack detection process> The uniaxial tensile test specimen crack detection process S7 detects cracks that occur in the parallel portion 103 of the uniaxial tensile test specimen 101 based on the time history of strain occurring in the jig 3 obtained in the delayed fracture testing process S5, and obtains the crack initiation time at which the detected crack occurs.
[0059] <Process for acquiring delayed fracture characteristics for areas at risk of delayed fracture> The delayed fracture characteristic acquisition process S9 of the area at risk of delayed fracture determines the time to crack occurrence in the parallel portion 103 of the uniaxial tensile test piece 101, the strain applied to the parallel portion 103, and the stress loaded on the parallel portion 103 as the delayed fracture characteristics of the area at risk of delayed fracture of the press-molded product.
[0060] In this embodiment 1, the time when a crack occurs in the parallel portion 103 is defined as the time when a crack is detected to have occurred in the parallel portion 103 based on the time history of the strain generated in the jig 3 in the uniaxial tensile test piece crack detection process S7. The strain applied to the parallel portion 103 is defined as an equivalent plastic strain applied to the parallel portion 103 of the uniaxial tensile test piece 101 produced in the uniaxial tensile test piece production step S3. Furthermore, the stress applied to the parallel portion 103 is defined as the maximum principal stress applied to the parallel portion 103 in the delayed fracture test step S5.
[0061] <Action and effect> Regarding the action and effect of the delayed fracture testing apparatus and delayed fracture testing method according to the first embodiment, a delayed fracture test is performed using a uniaxial tensile test piece with a predetermined strain applied to the parallel portion, and an example of the results obtained as the cracks that occur in the parallel portion of the uniaxial tensile test piece and the crack initiation time will be described.
[0062] The uniaxial tensile test piece 101 was produced by applying a strain equivalent to 0.01 equivalent plastic strain to a cold rolled steel sheet having a thickness of 1.2 mm and a tensile strength of 1470 MPa, and cutting out the portion to which the strain was applied as a parallel portion 103.
[0063] Then, a delayed fracture test was performed by immersing the uniaxial tensile test piece 101 in a hydrogen entry environment 111 while a uniaxial tensile stress of 1200 MPa was applied to the parallel part 103 using a jig 3 as shown in Fig. 1. The hydrogen entry environment 111 was a solution of ammonium thiocyanate with a concentration of 0.1% and McIlvaine buffer solution with a pH of 4.0. In the delayed fracture test, the strain time history acquisition unit 7 acquired the time history of strain output from the strain gauge 5 embedded in the shaft part 13a of the bolt 13 of the jig 3.
[0064] Here, the strain time history acquisition unit 7 acquired the strain output from the strain gauge 5 every minute. Figure 4 shows an example of the time history of the strain acquired in the delayed fracture testing process S5.
[0065] 4 shows that the strain of the jig 3 suddenly decreased about 26.2 hours after the start of the delayed fracture test. This indicates that a crack occurred in the parallel part 103 of the uniaxial tensile test piece 101, and it is understood that the crack occurred in the parallel part 103 of the uniaxial tensile test piece 101 can be detected with high accuracy in the delayed fracture test using the delayed fracture test apparatus 1 according to the first embodiment.
[0066] Figure 5 shows a graph of the crack initiation time calculated as the time until a crack was detected based on the strain time history obtained in each delayed fracture test performed three times under the same stress and strain conditions. As shown in Fig. 5, the variation in time to crack occurrence under the same stress and strain conditions was a small maximum of 8.5 hours, demonstrating high reproducibility of the results.
[0067] The above explanation is for the case where the stress and strain set in the delayed fracture test are set within the range of possible stress and strain in a portion of a typical press-formed product where delayed fracture is a concern. Therefore, according to the delayed fracture test device and delayed fracture test method of the first embodiment, the stress and strain in the portion of a press-formed product where delayed fracture is a concern are reproduced in a uniaxial tensile test piece, and a delayed fracture test is performed, so that cracks occurring in the parallel portion of the uniaxial tensile test piece can be detected with high accuracy. Then, based on the results of the delayed fracture test using the uniaxial tensile test piece, the delayed fracture properties in the portion of a press-formed product where delayed fracture is a concern can be appropriately obtained.
[0068] In the delayed fracture testing method according to the first embodiment, the delayed fracture suspected region stress and strain calculation step S1 calculates the equivalent plastic strain and maximum principal stress in the delayed fracture suspected region of the press-formed product. Then, in the uniaxial tensile test piece preparation process S3, a strain equivalent to the calculated equivalent plastic strain is applied to the parallel part 103 of the uniaxial tensile test piece 101. This is because, when a strain equivalent to the equivalent plastic strain is applied to the parallel part 103, it is preferable because it is not necessary to consider the deformation mode when the portion of the press-formed product at risk of delayed fracture is formed, as shown in FIG.
[0069] Furthermore, in the delayed fracture test process S5, a uniaxial tensile stress equivalent to the calculated maximum principal stress is applied to the parallel portion 103. As described above, the maximum principal stress is considered to have a large effect on delayed fracture in the portion susceptible to delayed fracture, so a uniaxial tensile stress equivalent to the maximum principal stress is applied to the parallel portion 103.
[0070] Furthermore, in the above description, a certain uniaxial tensile stress is applied to the parallel portion 103 of the uniaxial tensile test piece 101 by using the jig 3 shown in Fig. 2, and a time history of the strain generated in the shank 13a of the bolt 13 in conjunction with the strain generated in the parallel portion 103 is obtained. However, the delayed fracture testing device according to the present invention may be equipped with a jig 21 shown in Fig. 6.
[0071] The jig 21 includes a pair of gripping portions 23 and 25 , and a bolt 27 . The gripping portion 23 grips the left end portion 105 of the uniaxial tensile test piece 101, and has a pin hole portion 23a into which a pin is inserted and held in place in the uniaxial tensile test piece 101. On the other hand, the gripping portion 25 is used to grip the right end portion 105 of the uniaxial tensile test piece 101, and has a pin hole portion 25a into which a pin is inserted and held in a hole in the right end portion 105 of the uniaxial tensile test piece 101, and a screw hole portion 25b into which a bolt 27 is screwed.
[0072] The bolt 27 functions as a stress applying portion that applies a predetermined uniaxial tensile stress to the parallel portion 103 of the uniaxial tensile test piece 101 . By screwing the bolt 27 into the screw hole 25b of the gripping portion 25 and tightening it, a load is applied in a direction to pull the pair of gripping portions 23 and 25 apart. This allows a predetermined uniaxial tensile stress to be applied to the parallel portion 103 of the uniaxial tensile test piece 101, and makes it possible to generate a strain in the shaft portion 27a of the bolt 27 in conjunction with the parallel portion 103. For this reason, in the jig 21, a strain gauge 5 is embedded in the shaft portion 27a.
[0073] In the jig 21 shown in Fig. 6, there is no need to control the torque of the left and right stress application parts 11 as in the jig 3 shown in Fig. 2. Therefore, by pulling the end part 105 of the uniaxial tensile test piece 101 with one bolt 27, a predetermined uniaxial tensile stress can be easily applied to the parallel part 103.
[0074] [Embodiment 2] <Press molding method> A press forming method according to one aspect of the second embodiment of the present invention uses the delayed fracture testing apparatus 1 according to the first embodiment described above to determine delayed fracture initiation characteristics in a portion of a press-formed product at which delayed fracture is suspected. The press forming method according to the second embodiment includes a provisional press forming condition setting step S11, a delayed fracture suspect portion stress and strain calculation step S13, a uniaxial tensile test piece fabrication step S3, and a delayed fracture test step S5, as shown in Fig. 7. The press forming method according to the second embodiment further includes a uniaxial tensile test piece crack occurrence determination step S15, a provisional press forming condition changing step S17, a repeating step S19, a press forming condition determination step S21, and a press forming step S23.
[0075] Here, the uniaxial tensile test piece preparation step S3 and the delayed fracture test step S5 are the same as the delayed fracture test method according to the embodiment 1 described above. Therefore, the provisional press molding condition setting step S11, the delayed fracture suspected part stress and strain calculation step S13, and the uniaxial tensile test piece crack occurrence determination step S15 will be described below. Furthermore, the provisional press molding condition change step S17, the repeat step S19, the press molding condition determination step S21, and the press molding step S23 will also be described.
[0076] <Temporary press molding condition setting process> The provisional press-molding condition setting step S11 is a step of setting provisional press-molding conditions for a press-molded product. For example, when a press-formed product having a bent part obtained by bending a steel plate is targeted, the provisional press-forming conditions set in the provisional press-forming condition setting step S11 include the bending R (punch shoulder radius) of the bent part. Other factors include the clearance between the punch and the die, the thickness of the steel plate, etc. In the case of the draw-bend method (tensile bending / bending extension), further factors include the die shoulder radius, the clearance of the side wall, and the blank holding force.
[0077] <Process for calculating stress and strain in areas at risk of delayed fracture> The stress and strain calculation process S13 for areas at risk of delayed fracture is a process for calculating the stress and strain of areas at risk of delayed fracture in a press-molded product press-molded under the tentative press-molding conditions set in the tentative press-molding condition setting process S11.
[0078] In this embodiment 2, a CAE analysis is performed on the process of press-forming a press-formed product under the tentative press-forming conditions set in the tentative press-forming condition setting process S11, and the stress and strain distributions of the press-formed product are obtained, thereby calculating the stress and strain in the areas at risk of delayed fracture.
[0079] <Process for determining whether or not cracks have occurred in uniaxial tensile test pieces> The uniaxial tensile test specimen crack occurrence determination process S15 is a process for determining whether or not cracks have occurred in the parallel portion of the uniaxial tensile test specimen based on the time history of the strain occurring in the rod-shaped body of the jig obtained in the delayed fracture testing process S5.
[0080] To determine whether or not a crack has occurred based on the time history of the strain, it is sufficient to determine that a crack has occurred at the point in time when the strain changes suddenly in the acquired time history of the strain, similar to the uniaxial tensile test piece crack detection process S7 of the delayed fracture testing method according to the above-mentioned embodiment 1.
[0081] <Temporary press molding condition change process> The provisional press-molding condition changing step S17 is a step of changing the provisional press-molding conditions when it is determined that cracks have occurred in the uniaxial tensile test piece crack occurrence determining step S15. The tentative press forming conditions can be changed so as to reduce the stress and strain in the area where delayed fracture is a concern; for example, the bending radius of the bent area can be increased.
[0082] <Repetitive process> In the repeating step S19, the delayed fracture suspected part stress and strain calculation step S13, the uniaxial tensile test piece production step S3, the delayed fracture test step S5, and the uniaxial tensile test piece crack occurrence determination step S15 are repeatedly performed under the changed provisional press forming conditions. This repetition is performed until it is determined that no cracks have occurred in the uniaxial tensile test piece crack occurrence determination step S15. Therefore, if it is not determined that no cracks have occurred by changing the provisional press forming conditions only once, the provisional press forming condition change step S17 is also repeated.
[0083] <Press molding condition determination process> The press-molding condition determination step S21 is a step for determining the provisional press-molding conditions in the case where it is determined that no cracks have occurred in the uniaxial tensile test piece crack occurrence determination step S15 as the press-molding conditions of the press-molded product. Here, the press-molding conditions are the press-molding conditions calculated as the stress and strain of the portion at risk of delayed fracture in the delayed fracture risk portion stress and strain calculation step S13, where the stress and strain at which no cracks have occurred are the stress and strain at which no cracks have occurred.
[0084] <Press molding process> The press-forming step S23 is a step of press-forming the steel sheet into a press-formed product under the press-forming conditions determined in the press-forming condition determination step S21.
[0085] As described above, the press-forming method according to one aspect of the present embodiment 2 can produce press-formed products while taking measures against delayed fracture by determining press-forming conditions that result in stress and strain that will not cause delayed fracture in areas at risk of delayed fracture.
[0086] In the above description, the press forming conditions are changed to calculate the stress and strain of the portion where delayed fracture is suspected, and the production of the uniaxial tensile test piece and the delayed fracture test are repeatedly performed until it is determined that no cracks occur in the uniaxial tensile test piece in the delayed fracture test.
[0087] In other words, the above-mentioned press-molding method can be preferably applied when producing a press-molded product in which the press-molding conditions can be easily changed so as to alleviate the strain and stress in the area at risk of delayed fracture. However, when it is desired to mitigate delayed fracture while satisfying properties other than stress and strain (stretch flangeability) of the area at risk of delayed fracture, it is thought to be not easy to determine how to change the press forming conditions.
[0088] In such a case, rather than changing the press forming conditions, it is possible to repeat changing the stress and strain, producing a uniaxial tensile test piece, and conducting a delayed fracture test with the changed stress and strain until it is determined that no cracks have occurred in the uniaxial tensile test piece.
[0089] That is, the press forming method according to another aspect of the present embodiment 2 includes a provisional press forming condition setting step S11, a stress and strain calculation step S13 for a region at risk of delayed fracture, a uniaxial tensile test piece production step S3, and a delayed fracture test step S5, as shown in Fig. 8. Furthermore, the press forming method according to another aspect of the present embodiment 2 includes a uniaxial tensile test piece crack occurrence determination step S15, a stress and strain changing step S25, a repeating step S27, a press forming condition determination step S29, and a press forming step S23.
[0090] Here, the provisional press-forming condition setting step S11, the stress and strain calculation step S13 for a portion at risk of delayed fracture, the uniaxial tensile test piece production step S3, and the delayed fracture test step S5 are the same as those in the press-forming method according to one aspect of the present embodiment 2 described above (FIG. 7). Furthermore, the uniaxial tensile test piece crack occurrence determination step S15 and the press-forming step S23 are also the same as those in the press-forming method according to one aspect of the present embodiment 2 described above (FIG. 7). Therefore, the stress and strain changing step S25, the repeating step S27, and the press-forming condition determination step S29 will be described below.
[0091] <Stress and strain change process> The stress and strain changing step S25 is a step of changing the strain applied to the parallel portion 103 of the uniaxial tensile test piece 101 and / or the stress applied to the parallel portion 103 when it is determined that cracks have occurred. Specifically, at least one of the strain applied to the parallel portion 103 in the uniaxial tensile test piece manufacturing step S3 and the stress applied to the parallel portion 103 in the delayed fracture testing step S5 is relaxed so that cracks do not occur in the parallel portion 103 in the delayed fracture testing step.
[0092] <Repetitive process> The repeating step S27 is a step of repeatedly carrying out the uniaxial tensile test piece manufacturing step S3, the delayed fracture test step S5, and the uniaxial tensile test piece crack occurrence judgment step S15 under the changed stress and strain. This repetition is carried out until it is judged that no cracks have occurred in the uniaxial tensile test piece crack occurrence judgment step S15. Therefore, if it is not judged that no cracks have occurred by changing the stress and strain only once, the stress and strain changing step S25 will also be repeated.
[0093] <Press molding condition determination process> The press-molding condition determination step S29 is a step for determining press-molding conditions for the press-molded product when it is determined that no cracks have occurred in the uniaxial tensile test piece crack occurrence determination step S15. In the press-molding condition determination step S29, the press-molding conditions are determined so that the stress and strain of the portion of the press-molded product that is at risk of delayed fracture are the stress and strain when no cracks have occurred in the uniaxial tensile test piece in the delayed fracture test.
[0094] Another aspect of the press-forming method in the second embodiment can be preferably applied when the press-forming conditions cannot be easily changed to alleviate the stress and strain in a portion of the press-formed product at risk of delayed fracture.
[0095] In other words, by using another aspect of the press forming method in this embodiment 2, the stress and strain at which cracks do not occur in a delayed fracture test using a uniaxial tensile test piece are obtained, and the press forming conditions are set so that the obtained stress and strain can be obtained.
[0096] In addition, in the press forming method according to the second embodiment, it is preferable that the stress in the region at risk of delayed fracture is the maximum principal stress, and the strain is the equivalent plastic strain. In this case, the delayed fracture region stress and strain calculation step S13 calculates the maximum principal stress as the stress, and calculates the equivalent plastic strain as the strain. Then, the uniaxial tensile test piece production step S3 produces a uniaxial tensile test piece 101 in which a strain equivalent to the calculated equivalent plastic strain is imparted to the parallel portion 103. Furthermore, the delayed fracture test step loads the parallel portion 103 with a uniaxial tensile stress equivalent to the calculated maximum principal stress.
[0097] As a result, similarly to the delayed fracture testing method according to the first embodiment, there is no need to consider the deformation mode when the region of a press-formed product at risk of delayed fracture is press-formed, as shown in Fig. 11. Furthermore, as described above, it is considered that the delayed fracture at the region at risk of delayed fracture is largely influenced by the maximum principal stress, so that the stress at the region at risk of delayed fracture can be appropriately reproduced in the delayed fracture test using a uniaxial tensile test piece.
[0098] In the press forming method according to the second embodiment, "no delayed fracture occurs in the portion of the press-formed product where delayed fracture is suspected" means that delayed fracture does not occur in a time shorter than a reference time required for the press-formed product as a delayed fracture characteristic. The reference time is usually the time during which the press-formed product can be held in a predetermined hydrogen penetration environment without delayed fracture occurring in the portion where delayed fracture is suspected.
[0099] The press-formed product to be subjected to the press-forming method according to the second embodiment is not particularly limited, but can be preferably applied to body frame members such as center pillars and A-pillar lowers of automobiles. In this case, the method can be used to evaluate delayed fracture properties in parts of the body frame members where stress in the tensile direction is high and delayed fracture is a concern, to judge whether delayed fracture will occur, and to take measures against delayed fracture. EXAMPLES
[0100] Experiments were carried out to confirm the effects of the delayed fracture testing method and press forming method according to the present invention, and these will be described below.
[0101] In this example, the delayed fracture properties of a portion of a press-formed product where delayed fracture is suspected were obtained by the delayed fracture testing method according to the first embodiment described above. Furthermore, by using the press forming method according to the second embodiment described above, press forming conditions were determined that implemented measures against delayed fracture in areas of the press-formed product where delayed fracture is a concern, and the occurrence of delayed fracture in the press-formed product press-formed under those press conditions was verified.
[0102] (A) Delayed fracture test First, a delayed fracture test was carried out on a press-formed product 121, which was press-formed by bending as shown in Fig. 9, using a 1470 MPa-class cold-rolled steel sheet having a thickness of 1.2 mm as a test material. The press-formed product 121 has a bent portion 123 and pieces 125 extending from both ends of the bent portion 123, and the bend radius (bend R) of the bent portion 123 is 4 mm.
[0103] Next, the press-formed product 121 was immersed in ammonium thiocyanate and McIlvaine buffer solution with a pH of 4.0 and a concentration of 0.1% for 30 hours, and the presence or absence of delayed fracture in the press-formed product 121 was observed. As a result, it was confirmed that delayed fracture occurred in the center of the plate thickness near the bend apex of the bent portion 123 of the press-formed product 121. From this, it was found that in the press-formed product 121, the center of the plate thickness of the bent portion 123 is a portion at which delayed fracture is likely to occur.
[0104] Next, a CAE analysis was performed on the process of press-forming the press-formed product 121, and the equivalent plastic strain and maximum principal stress at the center of the plate thickness of the bent portion 123, which is a portion of the press-formed product 121 where delayed fracture is a concern, were calculated. Here, the equivalent plastic strain ε p eq was calculated by the following formula using the strain obtained by CAE analysis, and the maximum principal stress was taken as the stress in the longitudinal direction of the press-formed product.
[0105]
number
[0106] Figure 10 shows the maximum principal stress distribution and equivalent plastic strain distribution of the press-formed product 121 calculated by CAE analysis. From the maximum principal stress distribution and equivalent plastic strain distribution shown in Figure 10, it was calculated that the equivalent plastic strain in the part of the press-formed product 121 where delayed fracture is suspected is 0.09, and the maximum principal stress is 1260 MPa.
[0107] Next, a uniaxial tensile test piece 101 to be used in a delayed fracture test was prepared (see FIG. 1). First, in order to impart a uniform plane strain equivalent to an equivalent plastic strain of 0.09 to a 1470 MPa-class cold-rolled steel sheet (thickness: 1.2 mm), the sheet was rolled to a thickness of 1.11 mm at a thickness reduction rate of 7.5%. Then, the steel sheet to which the equivalent plastic strain had been imparted was cut out to produce a uniaxial tensile test piece 101 in which a strain equivalent to an equivalent plastic strain of 0.09 had been imparted to the parallel portion 103.
[0108] Next, using the jig 3 in which the strain gauge 5 shown in Fig. 2 was embedded in the shaft portion 13a of the bolt 13, a uniaxial tensile stress equivalent to the maximum principal stress (=1260 MPa) in the portion at risk of delayed fracture of the press-formed product 121 was applied to the parallel portion 103 of the uniaxial tensile test piece 101. Then, while still in a state in which the uniaxial tensile stress was applied, the jig 3 was immersed in a solution of ammonium thiocyanate and McIlvaine buffer solution with a concentration of 0.1% and a pH of 4.0, to perform a delayed fracture test. In the delayed fracture test, the time history of the strain output from the strain gauge 5 was acquired by a strain time history acquisition unit 7 connected to the strain gauge 5 embedded in the jig 3 .
[0109] Next, based on the acquired time history of strain, cracks were detected in the parallel part 103 of the uniaxial tensile test piece 101. In this example, as shown in Fig. 4, the strain significantly decreased 29 hours after the start of the delayed fracture test, and therefore it was detected that a crack had occurred in the parallel part 103 of the uniaxial tensile test piece 101 at that time point. From these results, it was determined that in a delayed fracture test in which the hydrogen penetration environment was a pH of 4.0 and a concentration of 0.1% ammonium thiocyanate and McIlvaine buffer solution, delayed fracture would occur in the bent portion 123 of the press-formed product 121 29 hours after the start of the test.
[0110] (B) Press forming under press forming conditions that take measures against delayed fracture Next, the press forming conditions of the press-formed product 121 were changed to take measures to prevent delayed fracture in the bent portion 123, and the press-formed product 121 was then press-formed.
[0111] In this embodiment, the press molding conditions were changed so that the bend R of the bent portion 123 of the press molded product 121 was changed from 4 mm to 8 mm.
[0112] Then, the strain and stress in the bent portion 123 of the press-molded product 121 press-molded under the changed press molding conditions were obtained. As a result, the strain and stress in the bent portion 123 were calculated to be an equivalent plastic strain of 0.05 and a maximum principal stress of 910 MPa.
[0113] Next, a uniaxial tensile test piece 101 was prepared and a delayed fracture test was carried out. Here, the strain applied to the parallel portion 103 of the uniaxial tensile test piece 101 was set to an equivalent plastic strain of 0.05, and the stress applied to the parallel portion 103 was set to a maximum principal stress of 910 MPa. Therefore, a 1470 MPa grade cold-rolled steel sheet was rolled to a thickness of 1.15 mm at a rolling reduction rate of 4.3%, which corresponds to an equivalent plastic strain of 0.05, and cut out to produce a uniaxial tensile test piece 101 in which a strain equivalent to an equivalent plastic strain of 0.05 was imparted to the parallel portion 103.
[0114] 2, a uniaxial tensile stress equivalent to a maximum principal stress of 910 MPa was applied to the parallel portion 103 of the uniaxial tensile test piece 101 using a jig 3, and the parallel portion 103 was held in a hydrogen penetration environment 111 to perform a delayed fracture test. In the delayed fracture test, the time history of the strain in the shaft portion 13a of the bolt 13 was obtained.
[0115] When the time history of the acquired strain was checked, no significant change in strain was detected even after 29 hours had passed since the start of the delayed fracture test. From this, it was determined that no cracks would occur in the parallel part of the uniaxial tensile test piece.
[0116] Next, a press-molded product 121 was newly produced under the press-molding conditions that were determined to result in no delayed fracture after an immersion time of 29 hours in a delayed fracture test.
[0117] Furthermore, a delayed fracture test was carried out on the newly produced press-formed product 121 by immersing it in ammonium thiocyanate and McIlvaine buffer solution with a pH of 4.0 and a concentration of 0.1% for 29 hours, similar to the delayed fracture test on the uniaxial tensile test piece 101. Then, the presence or absence of cracks in the bent part, which is a part of concern for delayed fracture, was confirmed.
[0118] As a result, in the press-formed product 121 produced by changing the press forming conditions, delayed fracture was not observed in the bent portion 123. This demonstrates that by changing the press forming conditions of the bend R of the bent portion 123 from 8 mm to 4 mm, the press-formed product 121 can be obtained by appropriately taking measures to prevent delayed fracture in the bent portion 123. [Explanation of symbols]
[0119] 1. Delayed fracture testing equipment 3. Jig 5 Strain gauge 7. Strain time history acquisition section 9 Grip part 11 Stress load section 13 Volts 13a Shaft 15 Lock nut 17 Lead Wire 21 Jig 23 Grip part 23a Pin hole 25 Grip part 25a Pin hole 25b Screw hole 27 Volts 27a Shaft 101 Uniaxial tensile test piece 103 Parallel section 105 End 111 Hydrogen intrusion environment 121 Press-molded products 123 Bending section 125 One side
Claims
1. A delayed fracture test apparatus for carrying out a delayed fracture test in which a uniaxial tensile test piece is held in a predetermined hydrogen penetration environment while a predetermined uniaxial tensile stress is applied to a parallel portion of the uniaxial tensile test piece, A jig is provided for applying a predetermined uniaxial tensile stress to the parallel portion of the uniaxial tensile test piece, and a strain is generated in association with the parallel portion, A delayed fracture testing apparatus having a function of acquiring a time history of strain generated in the jig so as to be capable of detecting cracks generated in the parallel portion of the uniaxial tensile test piece that is held in a hydrogen penetration environment while being loaded with uniaxial tensile stress using the jig.
2. A delayed fracture test apparatus for carrying out a delayed fracture test in which a uniaxial tensile test piece is held in a predetermined hydrogen penetration environment while a predetermined uniaxial tensile stress is applied to a parallel portion of the uniaxial tensile test piece, A jig including a pair of gripping parts for gripping both ends of the uniaxial tensile test piece, and a stress loading part having a rod-shaped body that applies a predetermined uniaxial tensile stress to the parallel part of the uniaxial tensile test piece by applying a load in a direction to pull the pair of gripping parts in a state where the both ends of the uniaxial tensile test piece are gripped, and generates a strain in conjunction with the parallel part; a strain gauge attached to the rod-shaped body to detect strain generated in the rod-shaped body; and a strain time history acquisition unit that acquires the time history of the strain detected by the strain gauge.
3. A delayed fracture testing method for determining delayed fracture initiation characteristics of a delayed fracture susceptible portion in a press-formed product, which is susceptible to delayed fracture, using the delayed fracture testing apparatus according to claim 1 or 2, comprising: A press molding condition setting process for setting press molding conditions for the press-molded product; A delayed fracture risk portion stress and strain calculation step of calculating stress and strain at the delayed fracture risk portion of the press-formed product; a uniaxial tensile test piece production process for producing a uniaxial tensile test piece in which the calculated strain of the portion at risk of delayed fracture is imparted to a parallel portion; a delayed fracture test step of applying the stress calculated in the delayed fracture risk region stress and strain calculation step to the parallel portion of the uniaxial tensile test piece produced in the uniaxial tensile test piece production step using the jig of the delayed fracture test apparatus, and holding the uniaxial tensile test piece in a predetermined hydrogen penetration environment while applying the stress, and acquiring a time history of the strain generated in the jig; A uniaxial tensile test piece crack detection process for detecting a crack occurring in the parallel portion of the uniaxial tensile test piece based on the acquired time history of the strain, and acquiring a crack occurrence time at which the detected crack occurs; and a delayed fracture characteristic acquisition process for determining the delayed fracture characteristics of the portion at risk of delayed fracture of the press-formed product based on the acquired crack initiation time in the parallel portion, the strain applied to the parallel portion of the uniaxial tensile test piece, and the stress loaded on the parallel portion.
4. In the delayed fracture suspected portion stress and strain calculation step, an equivalent plastic strain and a maximum principal stress in the delayed fracture suspected portion are calculated, In the uniaxial tensile test piece manufacturing step, a strain corresponding to the calculated equivalent plastic strain is applied to the parallel portion, 4. The delayed fracture test method according to claim 3, wherein in the delayed fracture test step, a uniaxial tensile stress equivalent to the calculated maximum principal stress is applied to the parallel portion.
5. A press forming method for performing a measure to suppress the occurrence of delayed fracture in a portion at which delayed fracture is suspected in a press-formed product using a steel plate, and press-forming the press-formed product, comprising: A temporary press molding condition setting process for setting temporary press molding conditions for the press-molded product; a delayed fracture risk portion stress and strain calculation step of calculating stress and strain of a delayed fracture risk portion in the press-formed product press-formed under the tentative press-forming conditions; a uniaxial tensile test piece production process for producing a uniaxial tensile test piece by applying the calculated strain to a parallel portion; a delayed fracture test step of applying the stress calculated in the delayed fracture suspected portion stress and strain calculation step to the parallel portion of the manufactured uniaxial tensile test piece using the jig of the delayed fracture test apparatus according to claim 1, and holding the uniaxial tensile test piece in a predetermined hydrogen penetration environment while applying the stress, and acquiring a time history of the strain detected by the strain gauge attached to the jig; A uniaxial tensile test piece crack occurrence determination process for determining whether or not cracks have occurred in the parallel portion of the uniaxial tensile test piece based on the acquired time history of strain generated in the jig; A temporary press molding condition changing process for changing the temporary press molding conditions when it is determined that cracks have occurred in the uniaxial tensile test piece crack occurrence determining process; A repeating process of repeatedly executing the provisional press forming condition changing process, the delayed fracture risk portion stress and strain calculating process, the uniaxial tensile test piece manufacturing process, the delayed fracture testing process, and the uniaxial tensile test piece crack occurrence determining process until it is determined that no cracks have occurred in the uniaxial tensile test piece crack occurrence determining process; When it is determined that no cracks occur in the uniaxial tensile test piece crack occurrence determination process, the tentative press molding conditions in that case are determined as the press molding conditions of the press molded product. and a press forming step of press-forming the steel sheet into the press-formed product under the determined press forming conditions.
6. A press forming method for performing a measure to suppress the occurrence of delayed fracture in a portion at which delayed fracture is suspected in a press-formed product using a steel plate, and press-forming the press-formed product, comprising: A temporary press molding condition setting process for setting temporary press molding conditions for the press-molded product; a delayed fracture risk portion stress and strain calculation step of calculating stress and strain of a delayed fracture risk portion in the press-formed product press-formed under the tentative press-forming conditions; a uniaxial tensile test piece production process for producing a uniaxial tensile test piece by applying the calculated strain to a parallel portion; a delayed fracture test step of applying the stress calculated in the delayed fracture suspected portion stress and strain calculation step to the parallel portion of the manufactured uniaxial tensile test piece using the jig of the delayed fracture test apparatus according to claim 1, and holding the uniaxial tensile test piece in a predetermined hydrogen penetration environment while applying the stress, and acquiring a time history of the strain detected by the strain gauge attached to the jig; A uniaxial tensile test piece crack occurrence determination process for determining whether or not cracks have occurred in the parallel portion of the uniaxial tensile test piece based on the acquired time history of strain generated in the jig; A stress and strain changing process for changing the strain applied to the parallel portion of the uniaxial tensile test piece and / or the stress applied to the parallel portion when it is determined that a crack has occurred in the uniaxial tensile test piece crack occurrence determining process; A repeating process of repeatedly executing the stress and strain changing process, the uniaxial tensile test piece manufacturing process, the delayed fracture testing process, and the uniaxial tensile test piece crack occurrence determining process until it is determined that no cracks have occurred in the uniaxial tensile test piece crack occurrence determining process; When it is determined that no cracks are generated in the uniaxial tensile test piece crack generation determination process, a press molding condition determination process is performed to determine press molding conditions for the press molded product so that the stress and strain of the delayed fracture concern portion of the press molded product are the stresses when no cracks are generated in the uniaxial tensile test piece in the delayed fracture test. and a press forming step of press-forming the steel sheet into the press-formed product under the determined press forming conditions.
7. In the delayed fracture suspected portion stress and strain calculation step, an equivalent plastic strain and a maximum principal stress in the delayed fracture suspected portion are calculated, In the uniaxial tensile test piece manufacturing step, a strain corresponding to the calculated equivalent plastic strain is applied to the parallel portion, 7. The press forming method according to claim 5, wherein in the delayed fracture test step, a uniaxial tensile stress equivalent to the calculated maximum principal stress is applied to the parallel portion.
Citation Information
Patent Citations
Electronic deformation gauge used for stress ring deformation detection and deformation detection device
CN203857924U
Method for testing stress corrosion cracking
JP1988293441A
JP1992055549U
Delayed fracture characteristic evaluating method for high tensile strength steel plate
JP1995146225A
System for evaluating hydrogen embrittlement of thin sheet steel and its evaluation method
JP2005134152A