Compound, method for producing said compound, leveling agent, coating composition, resist composition and article
A compound with polymerizable monomers at both ends of a silicone chain addresses the issue of unevenness in coating films by enhancing smoothness and reducing additive use, achieving improved film quality.
Patent Information
- Application Number
- JP2024505948
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-03-08
- Filing Date
- 2023-02-02
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2043-02-02
AI Technical Summary
Existing leveling agents fail to provide high smoothness and suppress unevenness in coating films, particularly due to temperature differences during drying, and there is a demand for a leveling agent that can achieve smoothness with reduced additives.
A compound with polymerizable monomers at both ends of a silicone chain, having a dispersity of 1.0 to 2.0, is used to enhance smoothness and suppress unevenness in coating films.
The compound achieves high smoothness and suppresses pin unevenness in coating films, even when used in small amounts, improving film quality and reducing additive usage.
Smart Images

Figure 0007563651000001 
Figure 0007563651000002 
Figure 0007563651000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a compound, a method for producing the compound, a leveling agent, a coating composition, a resist composition, and an article. [Background technology]
[0002] A leveling agent is an additive that improves cissing and unevenness in a coating film obtained by applying a coating composition such as a paint composition or a resist composition. Specifically, by adding a leveling agent to a coating composition, the leveling agent is oriented on the coating film surface, reducing the surface tension of the coating film, and the coating film obtained is smoothed. In a coating film with a smooth surface, the occurrence of repelling and unevenness can be improved.
[0003] Leveling agents have a wide variety of applications, including, for example, color resist compositions for use in the production of color filters for liquid crystal displays. The manufacture of color filters generally includes a process of applying a color resist composition onto a glass substrate by a coating method such as spin coating or slit coating, exposing the dried coating film using a mask, and then developing the film to form a colored pattern. If the coating film is not smooth and has uneven thickness, or if there is uneven coating or repelling, there is a risk of uneven color in pixels.
[0004] By adding a leveling agent to the color resist composition, the smoothness of the resulting coating film is improved, and the surfaces of the red (R), green (G), and blue (B) pixels and the black matrix (BM) formed between these pixels can exhibit high smoothness, resulting in a color filter with minimal color unevenness. As a leveling agent that provides smoothness to such coating films, a silicone polymer leveling agent has been proposed (Patent Documents 1 and 2). [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2018-199765 A [Patent Document 2] JP 2002-179991 A Summary of the Invention [Problem to be solved by the invention]
[0006] As described above, a coating film formed by applying a coating composition containing a leveling agent onto a substrate can exhibit high smoothness. This coating film is generally dried in a vacuum drying apparatus to evaporate the solvent in the coating film, and the coating film on the substrate is supported by a support pin in the drying apparatus chamber and dried. At this time, a temperature difference occurs between the portion where the support pin and the substrate contact each other and the other portion, which causes a problem of pin unevenness (drying unevenness) due to the difference in drying speed. This pin unevenness has been difficult to solve even when a leveling agent is added. Furthermore, in recent coating compositions, there is a demand to reduce not only the amount of impurities but also the amount of additives such as leveling agents, and there is a demand for leveling agents that can provide the required leveling effect even in small amounts (for example, 0.1 mass % or less of the solid content).
[0007] The problem to be solved by the present invention is to provide a compound that can function as a leveling agent that imparts high smoothness and pin mark suppression effects to a coating film. Another problem to be solved by the present invention is to provide a leveling agent which can impart high smoothness to a coating film even when added in a small amount, and which also has the effect of suppressing pin unevenness. Another object of the present invention is to provide a coating composition and a resist composition that can impart high smoothness and pin mark suppression effects to a coating film. Another problem to be solved by the present invention is to provide a cured product having high smoothness and suppressed pin unevenness. [Means for solving the problem]
[0008] As a result of extensive research, the present inventors have discovered that a compound having polymer blocks of polymerizable monomers at both ends of a silicone chain and having a degree of dispersion within a specific range can impart high smoothness to a coating film and suppress pin unevenness, thereby completing the present invention.
[0009] That is, the present invention relates to a compound having living polymer blocks of polymerizable monomers at both ends of a silicone chain. Effect of the Invention
[0010] The present invention can provide a compound that functions as a leveling agent that imparts high smoothness and pin mark suppression effects to a coating film. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] An embodiment of the present invention will be described below. The present invention is not limited to the following embodiment, and can be implemented by making appropriate modifications within the scope that does not impair the effects of the present invention. In this specification, the term "(meth)acrylate" refers to either or both of acrylate and methacrylate.
[0012] [Compound] The compound of the present invention is a compound having polymer blocks of polymerizable monomers at both ends of a silicone chain, and has a polydispersity (Mw / Mn), which is the ratio of weight average molecular weight to number average molecular weight, in the range of 1.0 to 2.0. Here, "both ends of the silicone chain" refers to both ends of the main chain of the silicone chain (the longest molecular chain among the molecular chains that make up the silicone chain).
[0013] The compound of the present invention has a dispersity (Mw / Mn) in the range of 1.0 to 2.0 and is a compound with little variation in molecular weight, so that the proportion of molecular weight suitable for the leveling effect is relatively high compared to conventional compounds with high dispersity. As a result, the compound can achieve the effect with a low amount of addition, whereas conventional compounds required an amount of addition to achieve the effect.
[0014] The number average molecular weight of the silicone chain is, for example, in the range of 100 to 50,000, preferably in the range of 500 to 20,000, more preferably in the range of 1,000 to 15,000, and further preferably in the range of 1,000 to 10,000. The number average molecular weight of the silicone chain is 29 It can be measured by SiNMR analysis.
[0015] The proportion of the silicone chains is, for example, in the range of 1 to 95 mass %, preferably in the range of 5 to 70 mass %, more preferably in the range of 10 to 65 mass %, and further preferably in the range of 20 to 60 mass %. Here, the silicone chain ratio is a value based on the mass of the compound of the present invention (mass of silicone chain / mass of compound). The silicone chain ratio is a value calculated from the charge ratio of raw materials during production, and can be adjusted by the charge ratio of the silicone compound and polymerizable monomer used in the production of the compound of the present invention.
[0016] The silicone chain contained in the compound of the present invention is preferably a silicone chain represented by the following formula (1).
[0017] [ka] (In the above formula (1), R 11 , R 12 , R 13 and R 14 are each independently an alkyl group having 1 to 18 carbon atoms or a phenyl group. L 11 and L 12 each independently represents a divalent organic group or a single bond. n is an integer.)
[0018] R 11 , R 12 , R 13 and R 14The alkyl group having 1 to 18 carbon atoms is preferably an alkyl group having 1 to 6 carbon atoms, and more preferably a methyl group.
[0019] If n is an integer equal to or greater than 2, multiple R 13 may be the same or different, and multiple R 14 may be the same or different from each other.
[0020] The number average of n is preferably an integer in the range of 5 to 300, more preferably an integer in the range of 10 to 250, even more preferably an integer in the range of 10 to 200, and most preferably an integer in the range of 40 to 150.
[0021] L 11 and L 12 The divalent organic group is preferably an alkylene group having 1 to 50 carbon atoms or an alkyleneoxy group having 1 to 50 carbon atoms.
[0022] L 11 and L 12 Examples of the alkylene group having 1 to 50 carbon atoms include a methylene group, an ethylene group, an n-propylene group, an n-butylene group, an n-pentylene group, an n-hexylene group, an n-heptylene group, an n-octylene group, an n-nonylene group, an n-decylene group, an n-dodecylene group, an isopropylene group, a 2-methylpropylene group, a 2-methylhexylene group, and a tetramethylethylene group.
[0023] L 11 and L 12 The alkylene group having 1 to 50 carbon atoms is preferably an alkylene group having 1 to 15 carbon atoms, more preferably an alkylene group having 1 to 5 carbon atoms, and further preferably a methylene group, an ethylene group, an n-propylene group or an isopropylene group.
[0024] L 11 and L 12 The alkyleneoxy group having 1 to 50 carbon atoms is, for example, a group in which one or more -CH2- within the alkylene group is substituted with -O-. L 11and L 12 The alkyleneoxy group having 1 to 50 carbon atoms is preferably an alkyleneoxy group having 1 to 15 carbon atoms, more preferably an alkyleneoxy group having 1 to 8 carbon atoms, and even more preferably a methyleneoxy group, an ethyleneoxy group, a propyleneoxy group, an oxytrimethylene group, a butyleneoxy group, an oxytetramethylene group, a pentyleneoxy group, a heptyleneoxy group, or an octyleneoxy group.
[0025] L 11 and L 12 When the divalent organic group is an alkylene group having 1 to 50 carbon atoms or an alkyleneoxy group having 1 to 50 carbon atoms, a part of the -CH2- in these divalent organic groups may be replaced by a carbonyl bond (-C(=O)-), an ester bond (-C(=O)O-), an amide bond (-C(=O)-NH-) or a phenylene group.
[0026] L 11 and L 12 When the divalent organic group is an alkylene group having 1 to 50 carbon atoms or an alkyleneoxy group having 1 to 50 carbon atoms, the carbon atom may be further substituted with a hydroxyl group or the like.
[0027] In the formula (1), L 11 and L 12 The bond possessed by the group is a bond that is bonded to a polymer block of a polymerizable monomer directly or via a linking group.
[0028] Regarding the polymer block of a polymerizable monomer contained in the compound of the present invention, the term "polymerizable monomer" means a compound having a polymerizable unsaturated group, and the term "polymer block" means a segment consisting of a repeating structure derived from the polymerizable monomer.
[0029] Examples of the polymerizable unsaturated group include a (meth)acryloyl group, a (meth)acryloyloxy group, a (meth)acryloylamino group, a vinyl ether group, an allyl group, a styryl group, a maleimide group, etc. Among these, a (meth)acryloyl group and a (meth)acryloyloxy group are preferred because of the availability of raw materials and good polymerization reactivity.
[0030] The polymer block of the polymerizable monomer contained in the compound of the present invention is preferably a polymer block of a polymerizable monomer (2) that can exhibit compatibility with the base polymer of the coating composition.
[0031] The polymerizable monomer (2) is preferably a polymerizable monomer having one or more selected from an alkyl group having 1 to 18 carbon atoms, an aromatic group having 6 to 18 carbon atoms, a group containing a polyoxyalkylene chain, and a group containing a polyester chain.
[0032] The alkyl group having 1 to 18 carbon atoms contained in the polymerizable monomer (2) may be any of a linear alkyl group, a branched alkyl group, and a cyclic alkyl group, and specific examples thereof include a methyl group, an ethyl group, a normal propyl group, an isopropyl group, a n-butyl group, a t-butyl group, a n-hexyl group, a cyclohexyl group, a n-octyl group, and a hexadecyl group. The alkyl group having 1 to 18 carbon atoms contained in the polymerizable monomer (2) is preferably an alkyl group having 1 to 6 carbon atoms.
[0033] Examples of the aromatic group having 6 to 18 carbon atoms contained in the polymerizable monomer (2) include a phenyl group, a naphthyl group, an anthracen-1-yl group, and a phenanthren-1-yl group.
[0034] The group containing a (poly)oxyalkylene chain contained in the polymerizable monomer (2) is a monovalent group containing a repeating oxyalkylene moiety or a divalent linking group containing a repeating oxyalkylene moiety.
[0035] When the polymerizable unsaturated group of the polymerizable monomer (2) is a (meth)acryloyl group, the polymerizable monomer having a group containing a (poly)oxyalkylene chain is, for example, a compound represented by the following formula (2-poa1) or (2-poa2), preferably the compound represented by the formula (2-poa1).
[0036] [ka] (In the above formulas (2-poa1) and (2-poa2), R a21 are each independently a hydrogen atom or a methyl group. R a22 is a hydrogen atom or an alkyl group having 1 to 18 carbon atoms. p is an integer of 0 or greater, q is an integer of 0 or greater, r is an integer of 0 or greater, and p+q+r is an integer of 1 or greater. X, Y, and Z each independently represent an alkylene group having 1 to 6 carbon atoms.
[0037] In the above formulas (2-poa1) and (2-poa2), -(XO) p -(YO) q -(ZO) r -R a22 and -(XO) p -(YO) q -(ZO) r The group represented by - corresponds to a group containing a (poly)oxyalkylene chain.
[0038] In the above formulas (2-poa1) and (2-poa2), the alkylene group having 1 to 6 carbon atoms for X, Y and Z is preferably an alkylene group having 2 to 4 carbon atoms.
[0039] Examples of the polymerizable monomer (2) having an alkyl group having 1 to 18 carbon atoms and in which the polymerizable unsaturated group is a (meth)acryloyl group include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, s-butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, n-pentyl (meth)acrylate, n-hexyl (meth)acrylate, n-heptyl (meth)acrylate, n-octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, decyl (meth)acrylate, and ethyl (meth)acrylate. (meth)acrylic acid alkyl esters having 1 to 18 carbon atoms, such as dicyclopentanyloxylethyl (meth)acrylate, isobornyloxylethyl (meth)acrylate, isobornyl (meth)acrylate, adamantyl (meth)acrylate, dimethyladamantyl (meth)acrylate, dicyclopentanyl (meth)acrylate, dicyclopentenyl (meth)acrylate, and the like; and (meth)acrylic acid bridged cyclic alkyl esters having 1 to 18 carbon atoms, such as dicyclopentanyloxylethyl (meth)acrylate, isobornyloxylethyl (meth)acrylate, isobornyl (meth)acrylate, adamantyl (meth)acrylate, dimethyladamantyl (meth)acrylate, dicyclopentanyl (meth)acrylate, dicyclopentenyl (meth)acrylate, and the like.
[0040] Examples of the polymerizable monomer (2) having a phenylalkyl group having 7 to 18 carbon atoms or a phenoxyalkyl group having 7 to 18 carbon atoms and in which the polymerizable unsaturated group is a (meth)acryloyl group include benzyl (meth)acrylate, phenoxymethyl (meth)acrylate, and 2-phenoxyethyl (meth)acrylate.
[0041] Examples of the polymerizable monomer (2) having an alkyl group having 1 to 18 carbon atoms and in which the polymerizable unsaturated group is a vinyl ether group include alkyl vinyl ethers such as methyl vinyl ether, ethyl vinyl ether, n-propyl vinyl ether, isopropyl vinyl ether, n-butyl vinyl ether, isobutyl vinyl ether, tert-butyl vinyl ether, n-pentyl vinyl ether, n-hexyl vinyl ether, n-octyl vinyl ether, n-dodecyl vinyl ether, 2-ethylhexyl vinyl ether, and cyclohexyl vinyl ether; and cycloalkyl vinyl ethers.
[0042] Examples of the polymerizable monomer (2) having an aromatic group having 6 to 18 carbon atoms include styrene, α-methylstyrene, p-methylstyrene, and p-methoxystyrene.
[0043] Examples of the polymerizable monomer (2) having an alkyl group having 1 to 18 carbon atoms and in which the polymerizable unsaturated group is a (meth)acryloylamino group include N,N-dimethylacrylamide, N,N-diethylacrylamide, N-isopropylacrylamide, diacetoneacrylamide, and acroylmorpholine.
[0044] Examples of the polymerizable monomer (2) having an alkyl group having 1 to 18 carbon atoms and in which the polymerizable unsaturated group is a maleimide group include methylmaleimide, ethylmaleimide, propylmaleimide, butylmaleimide, hexylmaleimide, octylmaleimide, dodecylmaleimide, stearylmaleimide, and cyclohexylmaleimide.
[0045] Examples of the polymerizable monomer (2) having a group containing a polyoxyalkylene chain and in which the polymerizable unsaturated group is a (meth)acryloyl group include polypropylene glycol mono(meth)acrylate, polyethylene glycol mono(meth)acrylate, polytrimethylene glycol mono(meth)acrylate, polytetramethylene glycol mono(meth)acrylate, poly(ethylene glycol-propylene glycol) mono(meth)acrylate, polyethylene glycol-polypropylene glycol mono(meth)acrylate, poly(ethylene glycol-tetramethylene glycol) mono(meth)acrylate, polyethylene glycol-polytetramethylene glycol mono(meth)acrylate, poly(propylene glycol-tetramethylene glycol) mono(meth)acrylate, polypropylene glycol-polytetramethylene glycol mono(meth)acrylate, poly(propylene glycol-1,2-butylene glycol) mono(meth)acrylate, polypropylene glycol-poly1,2-butylene glycol mono(meth)acrylate, Poly(ethylene glycol·1,2-butylene glycol) mono(meth)acrylate, Polyethylene glycol·poly 1,2-butylene glycol mono(meth)acrylate, Poly(tetraethylene glycol·1,2-butylene glycol) mono(meth)acrylate, Polytetraethylene glycol·poly 1,2-butylene glycol mono(meth)acrylate, Poly 1,2-butylene glycol mono(meth)acrylate, Poly(ethylene glycol·trimethylene glycol) mono(meth)acrylate, Polyethylene Glycol·Polytrimethylene glycol mono(meth)acrylate, Poly(propylene glycol·trimethylene glycol) mono(meth)acrylate, Polypropylene glycol·Polytrimethylene glycol mono(meth)acrylate, Poly(trimethylene glycol·tetramethylene glycol) mono(meth)acrylate, Polytrimethylene glycol·polytetramethylene glycol mono(meth)acrylate, Poly(1,2-butylene glycol·trimethylene glycol) mono(meth)acrylate, Poly 1,Examples include 2-butylene glycol polytrimethylene glycol mono(meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, poly(1,2-butylene glycol tetramethylene glycol) mono(meth)acrylate, poly(1,2-butylene glycol polytetramethylene glycol mono(meth)acrylate, etc. In addition, the above "poly(ethylene glycol-propylene glycol)" means a random copolymer of ethylene glycol and propylene glycol, and "polyethylene glycol-polypropylene glycol" means a block copolymer of ethylene glycol and propylene glycol.
[0046] The polymerizable monomer (2) is preferably at least one selected from the group consisting of a compound represented by the following formula (2-1), a compound represented by the following formula (2-2), a compound represented by the following formula (2-3), a compound represented by the following formula (2-4), and a compound represented by the following formula (2-5), and is more preferably at least one selected from the group consisting of a compound represented by the following formula (2-1), a compound represented by the following formula (2-2), a compound represented by the following formula (2-3), and a compound represented by the following formula (2-4). These compounds can exhibit high compatibility when the polymer of the present invention is used as a leveling agent.
[0047] [ka] (In the formulas (2-1), (2-2), (2-3), (2-4) and (2-5), R 21 is a hydrogen atom or a methyl group, R 22 is an alkyl group having 1 to 18 carbon atoms, R 23 is a hydrogen atom or a methyl group, R 24 is a hydrogen atom or an alkyl group having 1 to 18 carbon atoms, R 25 is a hydrogen atom or a methyl group, R 26 is an alkyl group having 1 to 18 carbon atoms or an alkyl group having 1 to 18 carbon atoms and an ether bond, R 27 is a hydrogen atom or a methyl group, R 28 is an alkyl group having 1 to 18 carbon atoms or an alkyl group having 1 to 18 carbon atoms and an ether bond, L 2 is a divalent organic group or a single bond, R 29 is a hydrogen atom or a methyl group, R 30 each independently represents an alkyl group having 1 to 6 carbon atoms or an alkoxy group having 1 to 6 carbon atoms, n is an integer ranging from 1 to 4, m is an integer ranging from 1 to 200, p is an integer ranging from 1 to 10, q is an integer ranging from 1 to 100, and l is an integer ranging from 0 to 5.
[0048] In the formula (2-2), the m n's in the parentheses may be the same or different. In the above formula (2-3), the q p's in the parentheses may be the same or different. In the above formula (2-4), the q p's in the parentheses may be the same or different.
[0049] L in the formulas (2-3) and (2-4) 2 The divalent organic group is L 11 The divalent organic groups are the same as those mentioned above.
[0050] The polymerizable monomer (2) preferably includes at least one selected from the group consisting of the compound represented by the formula (2-2), the compound represented by the formula (2-3), and the compound represented by the formula (2-4). In the case where the polymerizable monomer (2) contains one or more selected from the group consisting of the compound represented by the formula (2-2), the compound represented by the formula (2-3), and the compound represented by the formula (2-4), the total amount of the compound represented by the formula (2-2), the compound represented by the formula (2-3), and the compound represented by the formula (2-4) is preferably 50 mass% or more based on the total amount of the polymerizable monomer (2).
[0051] The polymerizable monomer (2) can be produced by a known method. Commercially available products may be used as the polymerizable monomer (2). For example, commercially available products of the polymerizable monomer (2) having a group containing a polyoxyalkylene chain and in which the polymerizable unsaturated group is a (meth)acryloyl group include "NK Ester M-20G", "NK Ester M-40G", "NK Ester M-90G", "NK Ester M-230G", "NK Ester AM-90G", "NK Ester AMP-10G", "NK Ester AMP-20G", and "NK Ester AMP-60G" manufactured by Shin-Nakamura Chemical Co., Ltd., and "Blenmer PE-90", "Blenmer PE-200", "Blenmer PE-350", and "Blenmer PME-100" manufactured by NOF Corporation. Examples of such products include "Blenmer PME-200", "Blenmer PME-400", "Blenmer PME-4000", "Blenmer PP-1000", "Blenmer PP-500", "Blenmer PP-800", "Blenmer 70 PEP-350B", "Blenmer 55 PET-800", "Blenmer 50 POEP-800B", "Blenmer 10 PPB-500B", "Blenmer NKH-5050", "Blenmer AP-400", "Blenmer AE-350", the Plaxel F series manufactured by Daicel Corporation, and the Viscoat series manufactured by Osaka Organic Chemical Industry Co., Ltd.
[0052] Regarding the polymer block of the polymerizable monomer contained in the compound of the present invention, the polymerizable monomer constituting the polymer block may be one type alone or two or more types. Furthermore, when the polymer block is a copolymer of two or more polymerizable monomers, the polymerization form of the copolymer is not particularly limited, and may be a random copolymer of two or more polymerizable monomers having mutually different structures, or may be a block copolymer of two or more polymerizable monomers having mutually different structures.
[0053] The number average molecular weight (Mn) of the compound of the present invention is preferably in the range of 1,000 to 200,000, more preferably in the range of 1,500 to 50,000, and further preferably in the range of 2,000 to 20,000. The weight average molecular weight (Mw) of the compound of the present invention is preferably in the range of 1,000 to 400,000, more preferably in the range of 2,000 to 100,000, and further preferably in the range of 4,000 to 40,000. The number average molecular weight (Mn) and weight average molecular weight (Mw) of the compound of the present invention are measured by the method described in the Examples.
[0054] The dispersity (Mw / Mn) of the compound of the present invention is in the range of 1.0 to 2.0, preferably in the range of 1.0 to 1.8, and more preferably in the range of 1.0 to 1.6. In order to achieve a degree of dispersity in the above range, it is necessary to carry out living radical polymerization, which will be described later, in the production of the compound, and it is not possible to achieve a degree of dispersity in the above range by so-called free radical polymerization.
[0055] [Method of manufacturing the compound] The compound of the present invention can be produced by generating radicals from compound (1) having functional groups capable of generating radicals at both ends of a silicone chain and polymerizable monomer (2) in a reaction system containing the compound (1), and living radical polymerizing the polymerizable monomer (2) at both ends of the compound (1).
[0056] The number average molecular weight of the silicone chain in compound (1) is, for example, in the range of 100 to 50,000, preferably in the range of 500 to 20,000, more preferably in the range of 1,000 to 15,000, and even more preferably in the range of 1,000 to 10,000.
[0057] Examples of the functional group capable of generating radicals that compound (1) has include an organic group having a halogen atom, an organic group having an alkyltellurium group, an organic group having a dithioester group, an organic group having a peroxide group, and an organic group having an azo group. From the viewpoints of ease of synthesis, ease of polymerization control, and the variety of applicable polymerizable monomers, the functional group capable of generating radicals that the compound (1) has is preferably an organic group having a halogen atom.
[0058] Examples of the organic group having a halogen atom include organic groups containing a 2-bromo-2-methylpropionyloxy group, a 2-bromo-propionyloxy group, and a parachlorosulfonylbenzoyloxy group.
[0059] The compound (1) having functional groups capable of generating radicals at both ends of a silicone chain is preferably a compound represented by the following formula (1-1).
[0060] [ka] (In the above formula (1-1), R 11 , R 12 , R 13 and R 14 are each independently an alkyl group having 1 to 18 carbon atoms or a phenyl group. L 11 and L 12 each independently represents a divalent organic group or a single bond. n is an integer. X 1 and X 2 are each independently a functional group capable of generating radicals.
[0061] In the formula (1-1), R 11 , R 12 , R 13 , R 14 , L 11 , L 12 A preferred embodiment of n is R 11 , R 12 , R 13 , R 14 , L 11 , L 12 and n are the same as the preferred embodiments.
[0062] In the formula (1-1), X 1 and X 2 The functional group capable of generating radicals is, for example, a functional group having a halogen atom, and is preferably a functional group represented by the following formula (X-1).
[0063] [ka] (In the formula (X-1), R HAL is a halogen atom. R 16 and R 17 are each independently an alkyl group having 1 to 6 carbon atoms. Q is an oxygen atom or a sulfur atom.
[0064] Specific examples of the compound (1) having functional groups capable of generating radicals at both ends of the silicone chain include the following compounds.
[0065] [ka] (In the formula, n is an integer.)
[0066] The compound (1) having functional groups capable of generating radicals at both ends of the silicone chain can be produced by a known method.
[0067] The polymerizable monomer (2) used in the method for producing the compound of the present invention is the same as the polymerizable monomer (2) described in the compound of the present invention, and may be used alone or in combination of two or more kinds.
[0068] The reaction raw materials used in the production of the compound of the present invention are not limited to only the compound (1) having functional groups capable of generating radicals at both ends of the silicone chain and the polymerizable monomer (2), and monomers other than the compound (1) and the polymerizable monomer (2) may be used as long as the effects of the present invention are not impaired. Examples of the other monomers include hydroxyalkyl (meth)acrylate, paravinyl benzoic acid, N-phenylmaleimide, etc. The other monomers as reaction raw materials may be used alone or in combination of two or more kinds.
[0069] The charging ratio of the compound (1) having functional groups capable of generating radicals at both ends of the silicone chain and the polymerizable monomer (2) is not particularly limited, and is, for example, 1 / 99 to 99 / 1, preferably 5 / 95 to 80 / 20, and more preferably 10 / 90 to 70 / 30, in terms of weight ratio (compound (1) / polymerizable monomer (2)).
[0070] In the living radical polymerization, a dormant species whose active polymerization terminal is protected by an atom or an atomic group reversibly generates a radical and reacts with a monomer, so that a propagation reaction proceeds. Even if the first monomer is consumed, the propagation terminal does not lose activity, and reacts with the second monomer that is added sequentially to obtain a block polymer. Examples of such living radical polymerization include atom transfer radical polymerization (ATRP), reversible addition-fragmentation radical polymerization (RAFT), nitroxide-mediated radical polymerization (NMP), and radical polymerization using organotellurium (TERP). Of these, there is no particular restriction on which method is used, but ATRP is preferred because of ease of control. In ATRP, polymerization is carried out using an organic halide or a sulfonyl halide compound as a polymerization initiator and a metal complex consisting of a transition metal compound and a ligand as a catalyst. In the method for producing a compound of the present invention, the compound (1) can function as a polymerization initiator, and the compound (1) can be subjected to living radical polymerization of a polymerizable monomer (2).
[0071] The transition metal compounds that can be used in ATRP are M n+ X n It is expressed as follows. M n+ X n The transition metal M of the transition metal compound represented by n+ As for the + , Cu 2+ , Fe 2+ , Fe 3+ , Ru 2+ , Ru 3+ , Cr 2+ , Cr 3+ , Mo 0 , Mo + , Mo 2+ , Mo 3+ , W 2+ , W 3+ , Rh 3+ , Rh 4+ , Co + , Co 2+ , Re 2+ , Re 3+ , Ni 0 , Ni + , Mn 3+ , Mn 4+ , V 2+ , V 3+ , Zn + , Zn 2+ , Au + , Au 2+ , Ag + and Ag 2+ The compound may be selected from the group consisting of: M n+ X n X in the transition metal compound represented by the formula (1) is a halogen atom, an alkoxyl group having 1 to 6 carbon atoms, (SO4) 1 / 2 , (PO4) 1 / 3 , (HPO4) 1 / 2 , (H2PO4), triflate, hexafluorophosphate, methanesulfonate, arylsulfonate (preferably benzenesulfonate or toluenesulfonate), SeR11 , CN and R 12 COO, where R 11 represents an aryl group or a linear or branched alkyl group having 1 to 20 carbon atoms (preferably having 1 to 10 carbon atoms); R 12 represents a hydrogen atom or a linear or branched alkyl group having 1 to 6 carbon atoms (preferably a methyl group) which may be substituted 1 to 5 times with halogen (preferably 1 to 3 times with fluorine or chlorine). M n+ X n In the transition metal compound represented by the formula (I), n represents a formal charge on the metal and is an integer of 0 to 7.
[0072] Examples of the ligand compound capable of forming a coordinate bond with the transition metal of the above-mentioned transition metal compound include a compound having a ligand containing one or more nitrogen atoms, oxygen atoms, phosphorus atoms, or sulfur atoms capable of coordinating with the transition metal via a σ bond, a compound having a ligand containing two or more carbon atoms capable of coordinating with the transition metal via a π bond, and a compound having a ligand capable of coordinating with the transition metal via a μ bond or η bond.
[0073] The transition metal complex is not particularly limited, but preferred examples include complexes of transition metals of Groups 7, 8, 9, 10, and 11, and more preferred examples include complexes of zero-valent copper, monovalent copper, divalent ruthenium, divalent iron, or divalent nickel.
[0074] Specific examples of catalysts that can be used in ATRP include complexes with ligands such as 2,2'-bipyridyl and its derivatives, 1,10-phenanthroline and its derivatives, and polyamines such as tetramethylethylenediamine, pentamethyldiethylenetriamine, hexamethyltris(2-aminoethyl)amine, tris[2-(dimethylamino)ethyl]amine, and tris(2-pyridylmethyl)amine, when the central metal is copper. Examples of divalent ruthenium complexes include dichlorotris(triphenylphosphine)ruthenium, dichlorotris(tributylphosphine)ruthenium, dichloro(cyclooctadiene)ruthenium, dichlorobenzeneruthenium, dichlorop-cymeneruthenium, dichloro(norbornadiene)ruthenium, cis-dichlorobis(2,2'-bipyridine)ruthenium, dichlorotris(1,10-phenanthroline)ruthenium, and carbonylchlorohydridotris(triphenylphosphine)ruthenium. Further, examples of the divalent iron complex include a bistriphenylphosphine complex and a triazacyclononane complex.
[0075] The atom transfer radical polymerization (ATRP) is not limited to the above, and other ATRPs can be used. For example, AGET ATRP, ARGET ATRP, ICAR ATRP, etc. described in "Macromol. Rapid. Commun. 2018, 1800616" can also be used.
[0076] In the living radical polymerization, it is preferable to use a solvent. Examples of solvents used in living radical polymerization include ester-based solvents such as ethyl acetate, butyl acetate, and propylene glycol monomethyl ether acetate; ether-based solvents such as diisopropyl ether, dimethoxyethane, and diethylene glycol dimethyl ether; halogen-based solvents such as dichloromethane and dichloroethane; aromatic solvents such as toluene, xylene, and anisole; ketone-based solvents such as methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; alcohol-based solvents such as methanol, ethanol, and isopropanol; and aprotic polar solvents such as dimethylformamide and dimethyl sulfoxide. The above solvents may be used alone or in combination of two or more kinds.
[0077] The polymerization temperature during the living radical polymerization is preferably in the range of room temperature to 120°C.
[0078] When the compound of the present invention is produced by living radical polymerization, metals resulting from the transition metal compound used in the polymerization may remain in the resulting compound. The metals remaining in the resulting polymer may be removed using activated alumina or the like after the polymerization is completed.
[0079] [Coating composition] The compound of the present invention can be suitably used as a leveling agent for a coating composition, and the coating composition of the present invention contains the compound of the present invention. The compound of the present invention can be a fluorine atom-free leveling agent that does not contain fluorine atoms, and therefore is a leveling agent that has low environmental accumulation and low environmental load.
[0080] The content of the compound of the present invention contained in the coating composition of the present invention varies depending on the type of base resin, the coating method, the intended film thickness, etc., but is, for example, in the range of 0.001 to 10 parts by mass, preferably in the range of 0.01 to 5 parts by mass, more preferably in the range of 0.02 to 2 parts by mass, and even more preferably in the range of 0.02 to 1 part by mass, relative to 100 parts by mass of the solid content of the coating composition. The compound of the present invention can exert a leveling effect even in a small amount, and can suppress the occurrence of defects such as foaming during coating.
[0081] The application of the coating composition of the present invention is not particularly limited, and it can be used for any application that requires leveling property. For example, the coating composition of the present invention can be used as various paint compositions or photosensitive resin compositions.
[0082] When the coating composition of the present invention is used as a paint composition, examples of the paint composition include paints using natural resins such as petroleum resin paints, shellac paints, rosin-based paints, cellulose-based paints, rubber-based paints, lacquer paints, cashew resin paints, and oil-based vehicle paints; and paints using synthetic resins such as phenolic resin paints, alkyd resin paints, unsaturated polyester resin paints, amino resin paints, epoxy resin paints, vinyl resin paints, acrylic resin paints, polyurethane resin paints, silicone resin paints, and fluororesin paints. By adding the compound of the present invention to the above coating composition, smoothness can be imparted to the resulting coating film.
[0083] Various additives may be added to the coating composition as needed, such as colorants such as pigments, dyes, and carbon; inorganic powders such as silica, titanium oxide, zinc oxide, aluminum oxide, zirconium oxide, calcium oxide, and calcium carbonate; organic fine powders such as higher fatty acids, polyacrylic resins, and polyethylene; and light resistance improvers, weather resistance improvers, heat resistance improvers, antioxidants, thickeners, and anti-settling agents.
[0084] Regarding the coating method of the coating composition of the present invention, any method can be used so long as it is a publicly known and publicly used coating method, and examples thereof include methods such as a slit coater, a slit & spin coater, a spin coater, a roll coater, electrostatic coating, a bar coater, a gravure coater, a die coater, a knife coater, an inkjet, dipping coating, spray coating, shower coating, screen printing, gravure printing, offset printing, and reverse coating.
[0085] The photosensitive resin composition changes its physical properties, such as solubility, viscosity, transparency, refractive index, conductivity, and ion permeability, when irradiated with light such as visible light or ultraviolet light. Among photosensitive resin compositions, resist compositions (photoresist compositions, color resist compositions for color filters, etc.) are required to have high leveling properties. The resist composition is usually applied by spin coating to a thickness of about 1 to 2 μm on a silicon wafer or a glass substrate on which various metals are deposited. In this case, if the applied film thickness fluctuates or uneven application occurs, the linearity and reproducibility of the pattern decreases, and a problem occurs in which a resist pattern with the desired accuracy cannot be obtained. In addition to these problems, there are various leveling-related problems such as drip marks, overall unevenness, and a bead phenomenon in which the film thickness is thicker at the edge compared to the center. The coating composition of the present invention can solve the above problems when used as a resist composition because the compound of the present invention exhibits high leveling properties and can form a uniform coating film (cured product).
[0086] When the coating composition of the present invention is used as a photoresist composition, the photoresist composition contains an alkali-soluble resin, a radiation-sensitive substance (photosensitive substance), a solvent, and the like in addition to the compound of the present invention.
[0087] The alkali-soluble resin contained in the photoresist composition is a resin that is soluble in an alkaline solution, which is the developer used when patterning the resist. Examples of the alkali-soluble resin include novolak resins obtained by condensing an aromatic hydroxy compound derivative such as phenol, cresol, xylenol, resorcinol, phloroglucinol, or hydroquinone with an aldehyde compound such as formaldehyde, acetaldehyde, or benzaldehyde; polymers or copolymers of vinylphenol compound derivatives such as o-vinylphenol, m-vinylphenol, p-vinylphenol, or α-methylvinylphenol; (meth)acrylic acid-based polymers or copolymers such as acrylic acid, methacrylic acid, or hydroxyethyl (meth)acrylate; polyvinyl alcohol; modified resins in which a radioactive ray-sensitive group such as a quinone diazide group, a naphthoquinone azide group, an aromatic azide group, or an aromatic cinnamoyl group has been introduced via a portion of the hydroxyl groups of these various resins; and urethane resins containing an acidic group such as a carboxylic acid or sulfonic acid in the molecule. These alkali-soluble resins may be used alone or in combination of two or more.
[0088] The radiation-sensitive substance contained in the photoresist composition is a substance that changes the solubility of the alkali-soluble resin in a developer when irradiated with energy rays such as ultraviolet rays, far ultraviolet rays, excimer laser light, X-rays, electron beams, ion beams, molecular beams, and gamma rays. Examples of radiation-sensitive substances include quinone diazide compounds, diazo compounds, azide compounds, onium salt compounds, halogenated organic compounds, mixtures of halogenated organic compounds and organometallic compounds, organic acid ester compounds, organic acid amide compounds, organic acid imide compounds, and poly(olefin sulfone) compounds.
[0089] Examples of the quinone diazide compounds include 1,2-benzoquinone azide-4-sulfonic acid ester, 1,2-naphthoquinone diazide-4-sulfonic acid ester, 1,2-naphthoquinone diazide-5-sulfonic acid ester, 2,1-naphthoquinone diazide-4-sulfonic acid ester, 2,1-naphthoquinone diazide-5-sulfonic acid ester, and sulfonic acid chlorides of quinone diazide derivatives such as 1,2-benzoquinone azide-4-sulfonic acid chloride, 1,2-naphthoquinone diazide-4-sulfonic acid chloride, 1,2-naphthoquinone diazide-5-sulfonic acid chloride, 2,1-naphthoquinone diazide-4-sulfonic acid chloride, and 2,1-naphthoquinone diazide-5-sulfonic acid chloride.
[0090] Examples of the diazo-based compound include salts of condensates of p-diazodiphenylamine with formaldehyde or acetaldehyde, inorganic diazo resin salts which are reaction products of the above-mentioned condensates with hexafluorophosphates, tetrafluoroborates, perchlorates or periodates, and organic diazo resin salts which are reaction products of the above-mentioned condensates with sulfonic acids as described in USP 3,300,309.
[0091] Examples of the azide-based compounds include azidochalconic acid, diazidobenzalmethylcyclohexanones, azidocinnamylideneacetophenones, aromatic azide compounds, and aromatic diazide compounds.
[0092] Examples of the halogenated organic compound include halogen-containing oxadiazole-based compounds, halogen-containing triazine-based compounds, halogen-containing acetophenone-based compounds, halogen-containing benzophenone-based compounds, halogen-containing sulfoxide-based compounds, halogen-containing sulfone-based compounds, halogen-containing thiazole-based compounds, halogen-containing oxazole-based compounds, halogen-containing trizole-based compounds, halogen-containing 2-pyrone-based compounds, halogen-containing aliphatic hydrocarbon-based compounds, halogen-containing aromatic hydrocarbon-based compounds, halogen-containing heterocyclic compounds, and sulfenyl halide-based compounds. In addition to the above, compounds used as halogen-based flame retardants such as tris(2,3-dibromopropyl)phosphate, tris(2,3-dibromo-3-chloropropyl)phosphate, chlorotetrabromomethane, hexachlorobenzene, hexabromobenzene, hexabromocyclododecane, hexabromobiphenyl, tribromophenyl allyl ether, tetrachlorobisphenol A, tetrabromobisphenol A, bis(bromoethyl ether)tetrabromobisphenol A, bis(chloroethyl ether)tetrachlorobisphenol A, tris(2,3-dibromopropyl)isocyanurate, 2,2-bis(4-hydroxy-3,5-dibromophenyl)propane, and 2,2-bis(4-hydroxyethoxy-3,5-dibromophenyl)propane, and compounds used as organic chloro-based pesticides such as dichlorophenyltrichloroethane are also exemplified as halogenated organic compounds.
[0093] Examples of the organic acid ester include carboxylate ester and sulfonate ester. Examples of the organic acid amide include carboxylate amide and sulfonate amide. Examples of the organic acid imide include carboxylate imide and sulfonate imide. The radiation sensitive substance may be used alone or in combination of two or more kinds.
[0094] In the photoresist composition, the content of the radiation-sensitive substance is preferably in the range of 10 to 200 parts by mass, and more preferably in the range of 50 to 150 parts by mass, per 100 parts by mass of the alkali-soluble resin.
[0095] Examples of the solvent for the photoresist composition include ketones such as acetone, methyl ethyl ketone, cyclohexanone, cyclopentanone, cycloheptanone, 2-heptanone, methyl isobutyl ketone, and butyrolactone; alcohols such as methanol, ethanol, n-propyl alcohol, isopropyl alcohol, n-butyl alcohol, isobutyl alcohol, tert-butyl alcohol, pentanol, heptanol, octanol, nonanol, and decanol; ethers such as ethylene glycol dimethyl ether, ethylene glycol diethyl ether, and dioxane; alcohol ethers such as ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monopropyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, and propylene glycol monopropyl ether; ethyl formate, propyl formate, butyl formate, methyl acetate, ethyl acetate, butyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, butyl propionate, methyl butyrate, butyl esters such as ethyl butyrate, butyl butyrate, propyl butyrate, ethyl lactate, butyl lactate, etc.; monocarboxylic acid esters such as methyl 2-oxypropionate, ethyl 2-oxypropionate, propyl 2-oxypropionate, butyl 2-oxypropionate, methyl 2-methoxypropionate, ethyl 2-methoxypropionate, propyl 2-methoxypropionate, butyl 2-methoxypropionate, etc.; cellosolve acetate, methyl cellosolve acetate, ethyl cellosolve acetate, propyl cellosolve acetate, butyl cellosolve acetate. cellosolve esters such as propylene glycol, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, propylene glycol monobutyl ether acetate, and other propylene glycols; diethylene glycols such as diethylyl glycol monomethyl ether, diethylyl glycol monoethyl ether, diethylyl glycol dimethyl ether, diethylyl glycol diethyl ether, and diethylyl glycol methyl ethyl ether;Examples of such solvents include halogenated hydrocarbons such as trichloroethylene, fluorocarbon solvents, HCFCs, and HFCs; fully fluorinated solvents such as perfluorooctane, aromatics such as toluene and xylene; and polar solvents such as dimethylacetamide, dimethylformamide, N-methylacetamide, and N-methylpyrrolidone. These solvents may be used alone or in combination of two or more.
[0096] When the coating composition of the present invention is used as a color resist composition, the color resist composition contains an alkali-soluble resin, a polymerizable compound, a colorant, and the like in addition to the compound of the present invention.
[0097] The alkali-soluble resin contained in the color resist can be the same as the alkali-soluble resin contained in the above-mentioned photoresist composition.
[0098] The polymerizable compound contained in the color resist composition is, for example, a compound having a photopolymerizable functional group that can undergo a polymerization or crosslinking reaction when irradiated with active energy rays such as ultraviolet rays. Examples of the polymerizable compound include unsaturated carboxylic acids such as (meth)acrylic acid, esters of monohydroxy compounds and unsaturated carboxylic acids, esters of aliphatic polyhydroxy compounds and unsaturated carboxylic acids, esters of aromatic polyhydroxy compounds and unsaturated carboxylic acids, esters obtained by esterification reactions of unsaturated carboxylic acids with polyvalent carboxylic acids and polyvalent hydroxy compounds such as the above-mentioned aliphatic polyhydroxy compounds and aromatic polyhydroxy compounds, polymerizable compounds having a urethane skeleton obtained by reacting a polyisocyanate compound with a (meth)acryloyl group-containing hydroxy compound, and polymerizable compounds having an acid group. The polymerizable compounds may be used alone or in combination of two or more kinds.
[0099] Examples of the esters of aliphatic polyhydroxy compounds and unsaturated carboxylic acids include (meth)acrylic acid esters such as ethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, trimethylolethane tri(meth)acrylate, pentaerythritol di(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, and glycerol (meth)acrylate. In addition, examples of the (meth)acrylic acid portion of these acrylates include itaconic acid esters in which itaconic acid is substituted, crotonic acid esters in which crotonic acid is substituted, and maleic acid esters in which maleic acid is substituted.
[0100] Examples of the esters of aromatic polyhydroxy compounds and unsaturated carboxylic acids include hydroquinone di(meth)acrylate, resorcinol di(meth)acrylate, and pyrogallol tri(meth)acrylate. The ester obtained by the esterification reaction of the unsaturated carboxylic acid, the polycarboxylic acid, and the polyhydroxy compound may be a single substance or a mixture. Examples of such esters include esters obtained from (meth)acrylic acid, phthalic acid, and ethylene glycol, esters obtained from (meth)acrylic acid, maleic acid, and diethylene glycol, esters obtained from (meth)acrylic acid, terephthalic acid, and pentaerythritol, and esters obtained from (meth)acrylic acid, adipic acid, butanediol, and glycerin.
[0101] Examples of the polymerizable compound having a urethane skeleton obtained by reacting the polyisocyanate compound with a hydroxy compound containing a (meth)acryloyl group include reaction products of aliphatic diisocyanates such as hexamethylene diisocyanate and trimethylhexamethylene diisocyanate; alicyclic diisocyanates such as cyclohexane diisocyanate and isophorone diisocyanate; and aromatic diisocyanates such as tolylene diisocyanate and diphenylmethane diisocyanate, with a hydroxy compound having a (meth)acryloyl group, such as 2-hydroxyethyl (meth)acrylate and 3-hydroxy[1,1,1-tri(meth)acryloyloxymethyl]propane.
[0102] The polymerizable compound having an acid group is, for example, an ester of an aliphatic polyhydroxy compound and an unsaturated carboxylic acid, and a polyfunctional polymerizable compound having an acid group by reacting an unreacted hydroxyl group of an aliphatic polyhydroxy compound with a non-aromatic carboxylic acid anhydride is preferable. The aliphatic polyhydroxy compound used for preparing the polyfunctional polymerizable compound is preferably pentaerythritol or dipentaerythritol. The acid value of the polyfunctional polymerizable compound is preferably in the range of 0.1 to 40, and more preferably in the range of 5 to 30, in order to improve developability, curability, etc. When two or more polyfunctional polymerizable compounds having an acid group are used in combination, or when a polyfunctional polymerizable compound having an acid group and a polyfunctional polymerizable compound not having an acid group are used in combination, it is preferable that the acid value of the mixture of polymerizable compounds is adjusted to be within the above range.
[0103] Specific examples of the polymerizable compound having an acid group include a mixture mainly composed of dipentaerythritol hexaacrylate, dipentaerythritol pentaacrylate, and a succinic acid ester of dipentaerythritol pentaacrylate, and the mixture is commercially available as ARONIX TO-1382 (manufactured by Toagosei Co., Ltd.).
[0104] Examples of polymerizable compounds other than those mentioned above include (meth)acrylamides such as ethylene bis(meth)acrylamide; allyl esters such as diallyl phthalate; and compounds having a vinyl group such as divinyl phthalate.
[0105] In the color resist composition, the content of the polymerizable compound is preferably in the range of 5 to 80 mass % of the total solid content of the color resist composition, more preferably in the range of 10 to 70 mass %, and even more preferably in the range of 20 to 50 mass %.
[0106] The colorant for the color resist composition is not particularly limited as long as it is capable of imparting color, and may be, for example, a pigment or a dye. Either organic or inorganic pigments can be used as the pigment. As the organic pigment, pigments of various hues such as red pigments, green pigments, blue pigments, yellow pigments, purple pigments, orange pigments, and brown pigments can be used. In addition, examples of the chemical structure of the organic pigment include azo-based, phthalocyanine-based, quinacridone-based, benzimidazolone-based, isoindolinone-based, dioxazine-based, indanthrene-based, and perylene-based pigments. In addition, examples of the inorganic pigment include barium sulfate, lead sulfate, titanium oxide, yellow lead, red iron oxide, and chromium oxide. In addition, "CI" below stands for color index.
[0107] Examples of the red pigment include CI Pigment Red 1, 2, 3, 4, 5, 6, 7, 8, 9, 12, 14, 15, 16, 17, 21, 22, 23, 31, 32, 37, 38, 41, 47, 48, 48:1, 48:2, 48:3, 48:4, 49, 49:1, 49:2, 50:1, 52:1, 52:2, 53, 53:1, and 53:2. , 53:3, 57, 57:1, 57:2, 58:4, 60, 63, 63:1, 63:2, 64, 64:1, 68, 69, 81, 81:1, 81:2, 81:3, 81:4, 83, 88, 90:1, 101, 101:1, 104, 108, 108:1, 109, 112, 113, 114, 122, 123, 144, 146, 147, 1 49, 151, 166, 168, 169, 170, 172, 173, 174, 175, 176, 177, 178, 179, 181, 184, 185, 187, 188, 190, 193, 194, 200, 202, 206, 207, 208, 209, 210, 214, 216, 220, 221, 224, 230, 231, 232, 23 3, 235, 236, 237, 238, 239, 242, 243, 245, 247, 249, 250, 251, 253, 254, 255, 256, 257, 258, 259, 260, 262, 263, 264, 265, 266, 267, 268, 269, 270, 271, 272, 273, 274, 275, 276, etc. Among these, CI Pigment Red 48:1, 122, 168, 177, 202, 206, 207, 209, 224, 242 or 254 is preferable, and CI Pigment Red 177, 209, 224 or 254 is more preferable.
[0108] Examples of the green pigment include CI Pigment Green 1, 2, 4, 7, 8, 10, 13, 14, 15, 17, 18, 19, 26, 36, 45, 48, 50, 51, 54, 55, and 58. Among these, CI Pigment Green 7, 36, or 58 is preferred.
[0109] Examples of the blue pigment include CI Pigment Blue 1, 1:2, 9, 14, 15, 15:1, 15:2, 15:3, 15:4, 15:6, 16, 17, 19, 25, 27, 28, 29, 33, 35, 36, 56, 56:1, 60, 61, 61:1, 62, 63, 66, 67, 68, 71, 72, 73, 74, 75, 76, 78, and 79. Among these, CI Pigment Blue 15, 15:1, 15:2, 15:3, 15:4, or 15:6 is preferred, and CI Pigment Blue 15:6 is more preferred.
[0110] Examples of the yellow pigment include CI Pigment Yellow 1, 1:1, 2, 3, 4, 5, 6, 9, 10, 12, 13, 14, 16, 17, 24, 31, 32, 34, 35, 35:1, 36, 36:1, 37, 37:1, 40, 41, 42, 43, 48, 53, 55, 61, 62, 62:1, 63, 65, 73, 74, 75, 81, 83, 87, 93, 94, 95, 97, 100, 101, 104, 105, 108, 109, 110, 111, 116, 117, 119, 120, 126, 127, 127:1, 128, 129, 133, 134, 136, 138, 139, 142, 147, 148, 150, 151, 153, 154, 155, 157, 158, 159, 160, 161, 162, 163, 164, 165, 166, 167, 168, 169, 170, 172, 173, 174, 175, 176, 180, 181, 182, 183, 184, 185, 188, 189, 190, 191, 191:1, 192, 193, 194, 195, 196, 197, 198, 199, 200, 202, 203, 204, 205, 206, 207, 208, etc. Among these, CI Pigment Yellow 83, 117, 129, 138, 139, 150, 154, 155, 180 or 185 is preferable, and CI Pigment Yellow 83, 138, 139, 150 or 180 is more preferable.
[0111] Examples of the purple pigment include CI Pigment Violet 1, 1:1, 2, 2:2, 3, 3:1, 3:3, 5, 5:1, 14, 15, 16, 19, 23, 25, 27, 29, 31, 32, 37, 39, 42, 44, 47, 49, and 50. Among these, CI Pigment Violet 19 or 23 is preferable, and CI Pigment Violet 23 is more preferable.
[0112] Examples of the orange pigment include CI Pigment Orange 1, 2, 5, 13, 16, 17, 19, 20, 21, 22, 23, 24, 34, 36, 38, 39, 43, 46, 48, 49, 61, 62, 64, 65, 67, 68, 69, 70, 71, 72, 73, 74, 75, 77, 78, and 79. Among these, CI Pigment Orange 38 or 71 is preferred.
[0113] The three primary color pixels of color filters used in liquid crystal display devices and organic EL display devices are red (R), green (G), and blue (B). Therefore, the red, green, and blue pigments are used as the main components, and organic pigments of colors such as yellow, purple, and orange may be used for hue adjustment in order to improve color reproducibility.
[0114] The average particle size of the organic pigment is preferably 1 μm or less, more preferably 0.5 μm or less, and even more preferably 0.3 μm or less, in order to increase the brightness of color liquid crystal display devices and organic EL display devices. It is preferable to use the organic pigment after dispersing it so that the average particle size falls within the above range. The average primary particle size of the organic pigment is preferably 100 nm or less, more preferably 50 nm or less, even more preferably 40 nm or less, and particularly preferably in the range of 10 to 30 nm. The average particle size of the organic pigment is measured using a dynamic light scattering particle size distribution analyzer, and can be measured using, for example, Nanotrac particle size distribution analyzers "UPA-EX150" and "UPA-EX250" manufactured by Nikkiso Co., Ltd.
[0115] When the color resist composition is used to form a black matrix (BM), the colorant is not particularly limited as long as it is black, and examples thereof include carbon black, lamp black, acetylene black, bone black, thermal black, channel black, furnace black, graphite, iron black, titanium black, etc. Among these, carbon black and titanium black are preferred from the viewpoints of light shielding rate and image characteristics. In addition, two or more organic pigments may be mixed to produce a black color.
[0116] Examples of commercially available carbon blacks include MA7, MA8, MA11, MA100, MA100R, MA220, MA230, MA600, #5, #10, #20, #25, #30, #32, #33, #40, #44, #45, #47, #50, #52, #55, #650, #750, #850, #950, #960, #970, #980, #990, #1000, #2200, #2300, #2350, #2400, #2600, #3050, #3150, # 3250, #3600, #3750, #3950, #4000, #4010, OIL7B, OIL9B, OIL11B, OIL30B, OIL31B, and the like. Printex3, Printex3OP, Printex30, Printex30OP, Printex40, Printex45, Printex55, Printex60, Printex75, Printex80, Printex85, Printex90, Printex A, Print ex L, Printex G, Printex P, Printex U, Printex V, PrintexG, SpecialBlack550, SpecialBlack 350, SpecialBlack250, SpecialBlack100, SpecialBlack6, SpecialBlack5, SpecialBlack4, Color Black FW1, Color Black FW2, Color Black FW2V, Color Black FW18, Color Black FW18, Color Black FW200, Color Black S160, Color Black S170, and the like, and Monarch 120, Monarch 280, Monarch 460, Monarch 800, Monarch 880, Monarch 900, Monarch 1000, Monarch 1100, Monarch 1300, Monarch 1400, Monarch 4630, REGAL 99, REGAL 99R, REGAL 415, REGAL 415R, REGAL 250, REGAL 250R, REGAL 330, REGAL 400R, REGAL 55R0, REGAL 660R, BLACK manufactured by Cabot Japan Co., Ltd.PEARLS480, PEARLS130, VULCAN XC72R, ELFTEX-8, etc. are included, and RAVEN11, RAVEN14, RAVEN15, RAVEN16, RAVEN22, RAVEN30, RAVEN35, RAVEN40, RAVEN410, RAVEN420, RAVEN450, RAVEN500, RAVEN780, RAVEN850, RAVEN890H, RAVEN 1000, RAVEN1020, RAVEN1040, RAVEN1060U, RAVEN1080U, RAVEN1170, RAVEN1190U, RAVEN1250, RAVEN1500, RAVEN2000, RAVEN2500U, RAVEN3500, RAVEN5000, RAVEN5250, RAVEN5750, RAVEN7000, and the like.
[0117] Among the above carbon blacks, resin-coated carbon black is preferred because it has the high optical density and high surface resistivity required for the black matrix of a color filter.
[0118] Examples of commercially available titanium black include titanium black 10S, 12S, 13R, 13M, and 13M-C manufactured by Mitsubishi Materials Corporation.
[0119] As a colorant used in forming a black matrix (BM), two or more kinds of organic pigments may be mixed to produce a black color, and examples of the black pigment include a mixture of three color pigments, red, green, and blue. The colorants that can be mixed to prepare black pigments include Victoria Pure Blue (CI 42595), Auramine O (CI 41000), Catilone Brilliant Flavin (Basic 13), Rhodamine 6GCP (CI 45160), Rhodamine B (CI 45170), Safranin OK 70:100 (CI 50240), Erioglaucine X (CI 42080), No. 120 / Leonol Yellow (CI 21090), Leonol Yellow GRO (CI 21090), and Shimla First Yellow. -8GF (CI21105), Benzidine Yellow 4T-564D (CI21095), Shimla First Red 4015 (CI12355), Lionor Red 7B4401 (CI15850), Firstgen Blue TGR-L (CI74160), Lionor Blue SM (CI26150), Lionor Blue ES (CI Pigment Blue 15:6), Lionor Red GD (CI Pigment Red 168), Lionor Green 2YS (CI Pigment Green 36), etc.
[0120] Other colorants that can be mixed and used to prepare a black pigment include, for example, CI Yellow Pigment 20, 24, 86, 93, 109, 110, 117, 125, 137, 138, 147, 148, 153, 154, 166, CI Orange Pigment 36, 43, 51, 55, 59, 61, CI Red Pigment 9, 97, 122, 123, 149, 168, 177, 180, 192, 215, 216, 217, 220, 223, 224, 226, 227, 228, 240, CI Violet Pigment 19, 23, 29, 30, 37, 40, 50, CI Blue Pigment 15, 15:1, 15:4, 22, 60, 64, CI Green Pigment 7, CI Brown Pigment 23, 25, 26, and the like.
[0121] When carbon black is used as the black pigment, the average primary particle size of the carbon black is preferably in the range of 0.01 to 0.08 μm, and more preferably in the range of 0.02 to 0.05 μm because of its good developability.
[0122] Carbon black has a particle shape different from organic pigments, etc., and exists in a state called a structure in which primary particles are fused to each other, and fine pores may be formed on the particle surface by post-treatment. Therefore, in order to express the particle shape of carbon black, it is generally preferable to measure the DBP absorption amount (JIS K6221) and the specific surface area by the BET method (JIS K6217) in addition to the average particle size of the primary particles, which is obtained by the same method as the organic pigments, and use these as indicators of the structure and pore amount. The dibutyl phthalate (DBP) absorption of carbon black is 40-100 cm 3 / 100g is preferable, and 50 to 80 cm is preferable because of its good dispersibility and developability. 3 The specific surface area of carbon black by the BET method is preferably in the range of 50 to 120 m 2 The range of 60 to 95 m / g is preferable because of good dispersion stability. 2 / g range is more preferred.
[0123] Examples of dyes that can be used as colorants in the color resist composition include azo dyes, anthraquinone dyes, phthalocyanine dyes, quinoneimine dyes, quinoline dyes, nitro dyes, carbonyl dyes, and methine dyes.
[0124] Examples of the azo dyes include CI Acid Yellow 11, CI Acid Orange 7, CI Acid Red 37, CI Acid Red 180, CI Acid Blue 29, CI Direct Red 28, CI Direct Red 83, CI Direct Yellow 12, CI Direct Orange 26, CI Direct Green 28, CI Direct Green 59, CI Reactive Yellow 2, CI Reactive Red 17, CI Reactive Red 120, CI Reactive Black 5, CI Disperse Orange 5, CI Disperse Red 58, CI Disperse Blue 165, CI Basic Blue 41, CI Basic Red 18, CI Mordant Red 7, CI Mordant Yellow 5, and CI Mordant Black 7.
[0125] Examples of the anthraquinone dyes include CI Vat Blue 4, CI Acid Blue 40, CI Acid Green 25, CI Reactive Blue 19, CI Reactive Blue 49, CI Disperse Red 60, CI Disperse Blue 56, and CI Disperse Blue 60.
[0126] Examples of the phthalocyanine dyes include CI Pad Blue 5, and the like. Examples of the quinoneimine dyes include CI Basic Blue 3 and CI Basic Blue 9, and the like. Examples of the quinoline dyes include CI Solvent Yellow 33, CI Acid Yellow 3 and CI Disperse Yellow 64, and the like. Examples of the nitro dyes include CI Acid Yellow 1, CI Acid Orange 3 and CI Disperse Yellow 42, and the like.
[0127] It is preferable to use a pigment as the colorant for the color resist composition, since the resulting coating film is excellent in light resistance, weather resistance, and fastness. However, in order to adjust the hue, a dye may be used in combination with the pigment as necessary.
[0128] In the color resist composition, the content of the colorant is preferably 1% by mass or more, more preferably in the range of 5 to 80% by mass, and even more preferably in the range of 5 to 70% by mass, based on the total solid content of the color resist composition.
[0129] When the color resist composition is used to form red (R), green (G), and blue (B) pixels of a color filter, the content of the colorant in the color resist composition is preferably in the range of 5 to 60 mass % of the total solid content of the color resist composition, and more preferably in the range of 10 to 50 mass %.
[0130] When the color resist composition is used to form a black matrix of a color filter, the content of the colorant in the color resist composition is preferably in the range of 20 to 80 mass % of the total solid content of the color resist composition, and more preferably in the range of 30 to 70 mass %.
[0131] In the color resist composition, when the colorant is a pigment, it is preferable to use the pigment as a pigment dispersion prepared by dispersing the pigment in an organic solvent using a dispersant. Examples of the dispersant include surfactants, pigment intermediates or derivatives, dye intermediates or derivatives, and resin-type dispersants such as polyamide resins, polyurethane resins, polyester resins, and acrylic resins. Among these, graft copolymers having nitrogen atoms, acrylic block copolymers having nitrogen atoms, and urethane resin dispersants are preferred. Since these dispersants have nitrogen atoms, the nitrogen atoms have affinity for the pigment surface, and the portions other than the nitrogen atoms increase the affinity for the medium, thereby improving the dispersion stability. These dispersants may be used alone or in combination of two or more kinds.
[0132] Commercially available dispersants include the "EFKA" series (such as "EFKA 46") manufactured by BASF; the "Disperbyk" series and "BYK" series (such as "BYK-160", "BYK-161", and "BYK-2001") manufactured by BYK Japan Co., Ltd.; the "Solsperse" series manufactured by Lubrizol Japan Co., Ltd.; the "KP" series manufactured by Shin-Etsu Chemical Co., Ltd., the "Polyflow" series manufactured by Kyoeisha Chemical Co., Ltd.; the "Disparlon" series manufactured by Kusumoto Chemical Co., Ltd.; and the "Ajisper" series (such as "Ajisper PB-814") manufactured by Ajinomoto Fine-Techno Co., Ltd.
[0133] Examples of organic solvents used in preparing the pigment dispersion include acetate-based solvents such as propylene glycol monomethyl ether acetate and propylene glycol monoethyl ether acetate; propionate-based solvents such as ethoxypropionate; aromatic solvents such as toluene, xylene, and methoxybenzene; ether-based solvents such as butyl cellosolve, propylene glycol monomethyl ether, diethylene glycol ethyl ether, and diethylene glycol dimethyl ether; ketone-based solvents such as methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; aliphatic hydrocarbon-based solvents such as hexane; nitrogen compound-based solvents such as N,N-dimethylformamide, γ-butyrolactam, and N-methyl-2-pyrrolidone; lactone-based solvents such as γ-butyrolactone; and carbamic acid esters. These solvents may be used alone or in combination of two or more.
[0134] The method for preparing the pigment dispersion liquid includes a method that includes a colorant kneading / dispersing step and a fine-dispersing step, and a method that includes only the fine-dispersing step. In the kneading / dispersing step, the colorant, a part of the alkali-soluble resin, and optionally the dispersant are mixed and kneaded. The colorant can be dispersed by dispersing while applying a strong shearing force using a kneader. Examples of machines used for kneading include two-roll machines, three-roll machines, ball mills, tron mills, dispersers, kneaders, co-kneaders, homogenizers, blenders, and single- or twin-screw extruders. It is preferable that the colorant be reduced in particle size by a salt milling method or the like before the above kneading is carried out.
[0135] In the fine dispersion step, a solvent is added to the composition containing the colorant obtained in the kneading and dispersion step, or a mixture of a colorant, an alkali-soluble resin, a solvent, and, if necessary, the dispersant is mixed together with a dispersion medium such as fine particles of glass, zirconia, or ceramic, using a dispersing machine, thereby dispersing the colorant particles to a fine state close to primary particles.
[0136] From the viewpoint of improving the transmittance, contrast, etc. of the color filter, the average particle size of the primary particles of the colorant is preferably 10 to 100 nm, and more preferably 10 to 60 nm. The average particle size of the colorant is measured by a dynamic light scattering type particle size distribution analyzer, and can be measured by, for example, Nanotrac particle size distribution analyzers "UPA-EX150" and "UPA-EX250" manufactured by Nikkiso Co., Ltd.
[0137] As the coating composition, a paint composition, a photoresist composition, and a color resist composition have been exemplified above, but the coating composition is not limited to these.
[0138] Specific examples of applications of the coating composition of the present invention include anti-glare (AG: anti-glare) hard coat materials, anti-reflection (LR) coat materials, low refractive index layer coat materials, high refractive index layer coat materials, clear hard coat materials, and polymerizable liquid crystal coat materials, which are coating materials for various display screens such as liquid crystal displays (hereinafter abbreviated as "LCD"), plasma displays (hereinafter abbreviated as "PDP"), organic electroluminescent displays (hereinafter abbreviated as "OLED"), and quantum dot displays (hereinafter abbreviated as "QDD"); color resists, inkjet inks, printing inks, or paints for forming each pixel such as RGB of color filters (hereinafter abbreviated as "CF") of LCDs, etc.; black resists, inkjet inks, printing inks, or paints for forming black matrices, black column spacers, and black photospacers of CFs of LCDs, etc.; transparent protective film paints for protecting the CF surface used in CFs of LCDs, etc.; resin compositions for liquid crystal materials, column spacers, and photospacers of LCDs; resin compositions for pixel partition walls of LCDs, PDPs, OLEDs, QDDs, etc., positive photoresists for forming electrodes, protective films, insulating films, plastic housings, paints for plastic housings, bezel (frame) inks; prism sheets and light diffusion films which are backlight components of LCDs; paints for organic insulating films in LCD liquid crystal TFT arrays; surface protective coating materials for LCD internal polarizers; phosphors for PDPs; organic EL materials and encapsulants (protective films, gas barriers) for OLEDs; quantum dot inks, encapsulants, and protective films for QDDs; high refractive index lenses, low refractive index encapsulants, and LED pixels for micro (mini) LED displays; positive photoresists, chemically amplified photoresists, anti-reflective films, and other materials used in semiconductor manufacturing. layer materials (SOC, SOG), underlayer films, buffer coats, developers, rinsing solutions, pattern collapse prevention agents, polymer residue removers, cleaning agents and other chemicals, nanoimprint release agents; resin compositions for semiconductor post-processing or printed wiring boards (epoxy resins, phenolic resins, polyphenylene ether resins, liquid crystal polymers, polyimide resins, bismaleimide resins, bisallylnadimide resins, benzoxazine resins and other resin compositions), copper-clad laminates, resin-coated copper foils, build-up films, passivation films, interlayer insulating films, flexible copper-clad laminates, dry film resists;Color resist for image sensors;Liquid repellents for solder flux;Dispersants, paints, green sheets for multilayer ceramic capacitors;Cathode materials, anode materials, separators, electrolytes for lithium-ion batteries;Exterior paints for automobiles, rubber, elastomers, glass, deposition anchor coats, headlamp lenses, solid lubricant paints, heat dissipation substrates, interior paints, repair paints;Wallpaper, flooring, kitchen materials, bathroom and toilet materials for housing facilities;Inkjet inks for printed matter, offset printing inks, gravure printing inks, screen printing inks, photoresists for the printing plate manufacturing process, photosensitive materials for lithographic printing plates (PS plates), packaging adhesives, ballpoint pen inks;Primers for easy adhesion of plastic films, etc.;Water repellents for textiles;Non-diffusing agents for greases;Cleaning fluids for cleaning the surfaces of various products or parts;Hard coat materials for optical recording media such as CDs, DVDs, and Blu-ray discs;Smartphones or Paints or hard coat materials for the housing or screen of a mobile phone; hard coat materials for transfer films for insert molds (IMD, IMF); release films; paints or coating materials for various plastic molded products such as the housing of home appliances; printing inks or paints for various building materials such as decorative panels; coating materials for window glass in houses; paints for woodworking such as furniture; coating materials for artificial and synthetic leather; coating materials for rubber rollers for office equipment such as copy machines and printers; coating materials for glass in the reading parts of office equipment such as copy machines and scanners; optical lenses or coating materials for cameras, video cameras, glasses, contact lenses, etc.; coating materials for windshields and glass for watches such as wristwatches; coating materials for windows of various vehicles such as automobiles and railway cars; paints for anti-reflection films for cover glass or films for solar cells; paints or coating materials for FRP bathtubs; PCM for metal building materials or home appliances; single-layer or multi-layer coating compositions for photofabrication processes, etc.;
[0139] The compound of the present invention has excellent surface tension reducing ability, so that it can be expected to have not only leveling properties, but also wettability, permeability, cleanability, water repellency, oil repellency, antifouling properties, lubricity, antiblocking properties, and releasability.In addition, when the compound of the present invention is mixed into a paint or coating agent containing fine particles, it can improve the dispersibility of fine particles, and it can be expected to have not only leveling properties, but also the function of a dispersant for fine particles.In addition to the above coating composition, the compound of the present invention can be added to an adhesive composition used for adhesive tape, etc., and it can be expected to have not only leveling properties, but also the functions of reducing peeling force, suppressing peeling force fluctuation, and suppressing peeling electrification. EXAMPLES
[0140] The present invention will be specifically described below with reference to examples and comparative examples. However, the present invention is not limited to the following examples.
[0141] In the examples and comparative examples, the weight average molecular weight (Mw) and number average molecular weight (Mn) are values calculated in terms of polystyrene based on gel permeation chromatography (GPC) measurements. The GPC measurement conditions are as follows.
[0142] [GPC measurement conditions] Measurement equipment: Tosoh Corporation's high-speed GPC equipment "HLC-8420GPC" Column: "TSK GUARDCOLUMN SuperHZ-L" manufactured by Tosoh Corporation + "TSK gel SuperHZM-N" manufactured by Tosoh Corporation + "TSK gel SuperHZM-N" manufactured by Tosoh Corporation + "TSK gel SuperHZM-N" manufactured by Tosoh Corporation + "TSK gel SuperHZM-N" manufactured by Tosoh Corporation Detector: RI (differential refractometer) Data processing: Tosoh Corporation "EcoSEC Data Analysis Version 1.07" Column temperature: 40℃ Developing solvent: Tetrahydrofuran Flow rate: 0.35mL / min Measurement sample: 7.5 mg of the sample was dissolved in 10 mL of tetrahydrofuran, and the resulting solution was filtered through a microfilter to prepare a measurement sample. Sample injection volume: 20 μL Standard sample: In accordance with the measurement manual for the above-mentioned "HLC-8420GPC," the following monodisperse polystyrene with known molecular weight was used.
[0143] (monodisperse polystyrene) "A-300" manufactured by Tosoh Corporation "A-500" manufactured by Tosoh Corporation "A-1000" manufactured by Tosoh Corporation "A-2500" manufactured by Tosoh Corporation "A-5000" manufactured by Tosoh Corporation "F-1" manufactured by Tosoh Corporation "F-2" manufactured by Tosoh Corporation "F-4" manufactured by Tosoh Corporation "F-10" manufactured by Tosoh Corporation "F-20" manufactured by Tosoh Corporation "F-40" manufactured by Tosoh Corporation "F-80" manufactured by Tosoh Corporation "F-128" manufactured by Tosoh Corporation "F-288" manufactured by Tosoh Corporation
[0144] (Example 1: Synthesis of compound (1) having living polymer blocks at both ends of the silicone chain) A glass flask equipped with a stirrer, a thermometer, a cooling tube, and a dropping device was charged with 35.10 g of n-heptane as a solvent, 70.00 g of a silicone compound having hydroxyl groups at both ends and represented by the following formula (a-1), and 9.81 g of triethylamine as a catalyst, and the temperature inside the flask was raised to 40°C.
[0145] [ka] (wherein n1 is an average of 65. The molecular weight (Mn) of the silicone chain is 5,000.
[0146] 11.89 g of 2-bromoisobutyric acid bromide was added to the above mixture and stirred at room temperature for 3 hours. Then, 87.73 g of isopropyl ether and 105 g of 10% citric acid aqueous solution were mixed and stirred, and the mixture was allowed to stand, and the citric acid aqueous solution layer was separated and removed. Next, 105g of 1% sodium hydroxide aqueous solution was mixed and stirred, then left to stand, the 1% sodium hydroxide aqueous solution layer was separated and removed, and 105g of 10% saline solution was further mixed and stirred, then left to stand, the 10% saline solution layer was separated and removed.Then, the solvent was distilled off under reduced pressure to obtain a compound represented by the following formula (A-1).
[0147] [ka]
[0148] In a nitrogen-substituted flask, 3.10 g of polypropylene glycol monomethacrylate (average repeat number of propylene glycol: 4-6) and 10.00 g of methyl ethyl ketone as a solvent were charged, and the temperature was raised to 60°C while stirring under a nitrogen stream. Next, 0.67 g of 2,2'-bipyridyl and 0.19 g of cuprous chloride were charged as catalysts, and the flask was stirred for 30 minutes while maintaining the temperature at 60°C. After that, 5.00 g of the compound represented by the formula (A-1) was added as a polymerization initiator, and living polymerization was carried out at 60°C for 27 hours under a nitrogen stream. 30 g of activated alumina was added to the resulting reaction product and stirred. After filtering the activated alumina, the solvent was distilled off under reduced pressure to obtain compound (1) having living polymer blocks of a polymerizable monomer (poly(propylene glycol) monomethacrylate) at both ends of the silicone chain.
[0149] The molecular weight of the obtained compound (1) was measured by GPC, and as a result, the weight average molecular weight (Mw) was 12,100, the number average molecular weight (Mn) was 8,400, and (Mw / Mn) was 1.4. The proportion of silicone chains in compound (1) was 57% by mass.
[0150] (Example 2: Synthesis of compound (2) having living polymer blocks at both ends of the silicone chain) In a nitrogen-substituted flask, 9.00 g of polypropylene glycol monomethacrylate (average repeat number of propylene glycol: 4-6) and 14.35 g of methyl ethyl ketone as a solvent were charged, and the temperature was raised to 60°C while stirring under a nitrogen stream. Next, 0.67 g of 2,2'-bipyridyl and 0.19 g of cuprous chloride were charged as catalysts, and the flask was stirred for 30 minutes while maintaining the temperature at 60°C. After that, 5.00 g of the compound represented by the formula (A-1) was added as a polymerization initiator, and living polymerization was carried out at 60°C for 54 hours under a nitrogen stream. 30 g of activated alumina was added to the resulting reaction product and stirred. After filtering the activated alumina, the solvent was distilled off under reduced pressure to obtain compound (2) having living polymer blocks of a polymerizable monomer (poly(propylene glycol) monomethacrylate) at both ends of the silicone chain.
[0151] The molecular weight of the obtained compound (2) was measured by GPC, and as a result, the weight average molecular weight (Mw) was 16,300, the number average molecular weight (Mn) was 11,200, and (Mw / Mn) was 1.5. The proportion of silicone chains in compound (2) was 33 mass %.
[0152] (Example 3: Synthesis of compound (3) having living polymer blocks at both ends of the silicone chain) Into a glass flask equipped with a stirrer, a thermometer, a cooling tube, and a dropping device, 100.00 g of n-heptane as a solvent, 200.00 g of a silicone compound having hydroxyl groups at both ends and represented by the following formula (a-2), and 12.45 g of triethylamine as a catalyst were placed, and the temperature inside the flask was raised to 40°C.
[0153] [ka] (wherein n2 is an average of 130. The molecular weight (Mn) of the silicone chain is 10,000.
[0154] 15.10g of 2-bromoisobutyric acid bromide was added to the above mixture and stirred at room temperature for 3 hours. Then, 250.00g of isopropyl ether and 300g of 10% citric acid solution were mixed and stirred, then left to stand, and the citric acid solution layer was separated and removed. Then, 300g of 1% sodium hydroxide solution was mixed and stirred, then left to stand, and the 1% sodium hydroxide solution layer was separated and removed, and 300g of 10% saline solution was further mixed and stirred, then left to stand, and the 10% saline solution layer was separated and removed. Thereafter, the solvent was distilled off under reduced pressure to obtain a compound represented by the following formula (A-2).
[0155] [ka]
[0156] In a nitrogen-substituted flask, 20.00 g of polypropylene glycol-polybutylene glycol-monomethacrylate (average repeat number of propylene glycol: 1, average repeat number of butylene glycol: 6) and 73.00 g of methyl ethyl ketone as a solvent were charged, and the temperature was raised to 60°C while stirring under a nitrogen stream. Next, 0.63 g of 2,2'-bipyridyl and 0.18 g of cuprous chloride were charged as catalysts, and the flask was stirred for 30 minutes while maintaining the temperature at 60°C. Then, 10.00 g of the compound represented by the formula (A-2) was added as a polymerization initiator, and living polymerization was carried out at 60°C for 74 hours under a nitrogen stream. 20 g of activated alumina was added to the resulting reaction product and stirred. After filtering the activated alumina, the solvent was distilled off under reduced pressure to obtain compound (3) having living polymer blocks of polymerizable monomers (polypropylene glycol-polybutylene glycol-monomethacrylate) at both ends of the silicone chain.
[0157] The molecular weight of the obtained compound (3) was measured by GPC, and as a result, the weight average molecular weight (Mw) was 27,600, the number average molecular weight (Mn) was 19,500, and (Mw / Mn) was 1.4. The proportion of silicone chains in compound (3) was 32 mass %.
[0158] (Comparative Example 1: Synthesis of Compound (1') Having Free Radical Polymer Blocks at Both Ends of Silicone Chain) Mixture A was prepared by mixing 102.6 g of polypropylene glycol monomethacrylate (average number of propylene glycol repeats: 4 to 6), 152.6 g of butyl acetate as a solvent, and 13.5 g of t-butylperoxy-2-ethylhexanoate as an initiator. Mixture B was prepared by mixing 47.4 g of a dimethacrylate compound having a polysiloxane bond represented by the following formula (A-1′) and 47.4 g of butyl acetate as a solvent.
[0159] [ka] (wherein n3 is an average of 65. The molecular weight (Mn) of the silicone chain is 5,000.
[0160] A glass flask equipped with a stirrer, a thermometer, a condenser, and a dropping device was charged with 150.0 g of butyl acetate as a solvent, and the temperature was raised to 105° C. with stirring under a nitrogen stream. The mixed solution A was added dropwise to the glass flask over 140 minutes at 105° C. Five minutes after the start of the dropwise addition of mixed solution A, the mixed solution B was added dropwise over 120 minutes at 105° C. After the dropwise addition was completed, the mixture was stirred for 5 hours at 105° C. After the reaction was completed, the solvent was distilled off to obtain a compound (1') having free radical polymer blocks of a polymerizable monomer at both ends of the silicone chain.
[0161] The molecular weight of the resulting compound (1') was measured by GPC, and as a result, the weight average molecular weight (Mw) was 6,500, the number average molecular weight (Mn) was 1,900, and (Mw / Mn) was 3.4. The proportion of silicone chains in compound (1') was 30 mass %.
[0162] (Comparative Example 2: Synthesis of Compound (2') Having Free Radical Polymer Blocks at Both Ends of Silicone Chain) A glass flask equipped with a stirrer, a thermometer, a condenser, and a dropping device was charged with 150.0 g of butyl acetate as a solvent, and the temperature was raised to 105° C. with stirring under a nitrogen stream. The mixed solution A was added dropwise to the glass flask over 140 minutes at 105° C. Five minutes after the start of the dropwise addition of mixed solution A, the mixed solution B was added dropwise over 120 minutes at 105° C. After the dropwise addition was completed, the mixture was stirred for 10 hours at 105° C. After the reaction was completed, the solvent was distilled off to obtain a compound (2') having free radical polymer blocks of a polymerizable monomer at both ends of the silicone chain.
[0163] The molecular weight of the obtained compound (2') was measured by GPC, and as a result, the weight average molecular weight (Mw) was 7000, the number average molecular weight (Mn) was 2,000, and (Mw / Mn) was 3.5. The proportion of silicone chains in compound (2') was 30 mass %.
[0164] The compounds produced in the Examples and Comparative Examples were evaluated as follows.
[0165] (Coating film formation and evaluation) A resist composition (content of compound (1) was 0.05% by mass of solids) was prepared by mixing 3.0 g of a 40% by mass alkali-soluble resin solution (ACRYDIC ZL-295, manufactured by DIC Corporation), 1.2 g of ARONIX M-402 (manufactured by Toagosei Chemical Industry Co., Ltd., a mixture of dipentaerythritol pentaacrylate and dipentaerythritol hexaacrylate), 0.0024 g of compound (1) in terms of solids content, and 6.23 g of propylene glycol monomethyl ether acetate (PGMEA). 3 ml of the obtained resist composition was dropped onto the center of a 10 cm x 10 cm chrome-plated glass substrate, and spin-coated at a rotation speed of 400 rpm for 20 seconds to obtain a coated substrate. SUS pins were attached to the four corners of a hot plate, and the obtained coated substrate was placed on the support pins and heated and dried at 100°C for 100 seconds to produce a laminate having a coating layer.
[0166] (Smoothness evaluation) The coating layer of the laminate prepared above was visually observed and the smoothness of the coating layer was evaluated according to the following criteria. The results are shown in Table 1. A: No coating unevenness is observed. B: Almost no coating unevenness is observed. C: Coating unevenness is observed throughout the entire surface.
[0167] (Pinmura evaluation) The contact area between the support pin and the coating substrate of the laminate prepared above was visually observed, and pin unevenness of the coating layer was evaluated according to the following criteria: "Pin unevenness" refers to unevenness in film thickness (drying unevenness) that occurs mainly at the contact area between the support pin and the coating substrate, and is confirmed as a ripple-like shape spreading from the contact area between the support pin and the coating substrate. 1: Almost no pin unevenness is observed 2: Pin unevenness is observed
[0168] The same evaluation was carried out using the compounds of Examples 2-3 and Comparative Examples 1-2 instead of compound (1). The results are shown in Table 1.
[0169] [Table 1]
[0170] It can be confirmed that the compounds of Examples 1-3 provide smoothness even when added in a small amount of 0.05 mass% of the solid content of the resist composition, and also suppress pin mura. On the other hand, the compounds of Comparative Examples 1 and 2 do not provide both smoothness and suppress pin mura. To obtain smoothness with the compounds of Comparative Examples 1 and 2, it was necessary to add 0.4 mass% of the solid content of the resist composition.
Claims
1. A color resist composition containing a compound having polymer blocks of polymerizable monomers at both ends of a silicone chain, The color resist composition has a dispersity (Mw / Mn) which is the ratio of the weight average molecular weight to the number average molecular weight of the compound in the range of 1.0 to 2.
0.
2. 2. The color resist composition according to claim 1, wherein the silicone chain is a silicone chain represented by the following formula (1): 【Chemistry 1】 (In the above formula (1), R 11 , R 12 , R 13 and R 14 are each independently an alkyl group having 1 to 18 carbon atoms or a phenyl group. L 11 and L 12 each independently represents a divalent organic group or a single bond. n is an integer.
3. The color resist composition according to claim 1 or 2, wherein the polymerizable monomer is a polymerizable monomer (2) having one or more selected from an alkyl group having 1 to 18 carbon atoms, an aromatic group having 6 to 18 carbon atoms, a group containing a polyoxyalkylene chain, and a group containing a polyester chain.
4. The color resist composition according to claim 1 or 2, wherein the polymerizable monomer is at least one selected from the group consisting of a compound represented by the following formula (2-1), a compound represented by the following formula (2-2), a compound represented by the following formula (2-3), and a compound represented by the following formula (2-4). 【Chemistry 2】 (In the formulas (2-1), (2-2), (2-3) and (2-4), R 21 is a hydrogen atom or a methyl group, R 22 is an alkyl group having 1 to 18 carbon atoms, R 23 is a hydrogen atom or a methyl group, R 24 is a hydrogen atom or an alkyl group having 1 to 18 carbon atoms, R 25 is a hydrogen atom or a methyl group, R 26 is an alkyl group having 1 to 18 carbon atoms or an alkyl group having 1 to 18 carbon atoms and an ether bond, R 27 is a hydrogen atom or a methyl group, R 28 is an alkyl group having 1 to 18 carbon atoms or an alkyl group having 1 to 18 carbon atoms and an ether bond, L 2 is a divalent organic group or a single bond, n is an integer ranging from 1 to 4, m is an integer ranging from 1 to 200, p is an integer ranging from 1 to 10, and q is an integer ranging from 1 to 100.
5. The color resist composition according to claim 4, comprising at least one selected from the group consisting of the compound represented by formula (2-2), the compound represented by formula (2-3), and the compound represented by formula (2-4) as the polymerizable monomer.
6. 3. The color resist composition according to claim 1, wherein the number average molecular weight of the silicone chain is in the range of 1,000 to 15,000.
7. 3. The color resist composition according to claim 1, wherein the proportion of said silicone chains in the entire compound is in the range of 5 to 70% by mass.
8. A cured product obtained by curing the color resist composition according to claim 1 or 2.
Citation Information
Patent Citations
Amphipathic organosilicone segmented copolymer having pH response and preparation method thereof
CN105713157A
Siloxane iniferter compound
JP1991097735A
Preparation of novel homo- and copolymers using atom transfer radical polymerization.
JP2000514479A
Leveling agent for surface coating
JP2002179991A
Leveling agent for coating material using amphiphatic block copolymer
JP2018199765A