Surface-treated steel sheet and its manufacturing method
By controlling the Al, Si, Mg, and Co composition in the plating film and applying a chemical conversion film, the steel sheet achieves stable corrosion and white rust resistance, addressing variability and surface defects in existing technologies.
Patent Information
- Application Number
- JP2022001318
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-01-06
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2042-01-06
AI Technical Summary
Existing hot-dip Al-Zn-Si-Mg coated steel sheets face variability in corrosion resistance and white rust resistance, with techniques failing to consistently improve these properties due to uncontrolled phase compositions and the presence of impurities like Co, leading to surface defects and reduced effectiveness.
Control the composition of the plating film with specific ratios of Al, Si, Mg, and Co, and apply a chemical conversion film containing resins and metal compounds to stabilize the phase ratios and enhance corrosion resistance and white rust resistance.
The controlled composition and chemical conversion film result in a steel sheet with consistently excellent corrosion resistance and white rust resistance, improving surface appearance and bath stability.
Smart Images

Figure 0007564134000004 
Figure 0007564134000001 
Figure 0007564134000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a surface-treated steel sheet having stable and excellent corrosion resistance and white rust resistance, and a method for producing the same. [Background technology]
[0002] Hot-dip Al-Zn-coated steel sheets, such as 55% Al-Zn-based, are known to have high corrosion resistance among hot-dip galvanized steel sheets, because they combine the sacrificial corrosion protection of Zn with the high corrosion resistance of Al. Therefore, hot-dip Al-Zn-coated steel sheets are mainly used in the field of building materials such as roofs and walls that are exposed to the outdoors for long periods of time, and in the field of civil engineering and construction such as guardrails, wiring and piping, and soundproof walls, due to their excellent corrosion resistance. In particular, the demand for materials with excellent corrosion resistance and maintenance-free materials in more severe usage environments such as acid rain caused by air pollution, the spraying of deicing agents to prevent road ice in snowy areas, and coastal area development has been increasing in recent years, and the demand for hot-dip Al-Zn-coated steel sheets has been increasing in recent years.
[0003] The coating of hot-dip Al-Zn coated steel sheets is composed of α-Al phases, which are areas where Al containing supersaturated Zn has solidified in the form of dendrites, and Zn-Al eutectic structures that exist in the gaps between dendrites (interdendritic structures), and is characterized by a structure in which the α-Al phases are layered in the thickness direction of the coating. This characteristic coating structure makes the corrosion progression path from the surface complex, making it difficult for corrosion to progress easily, and it is also known that hot-dip Al-Zn coated steel sheets can achieve superior corrosion resistance compared to hot-dip galvanized steel sheets with the same coating thickness.
[0004] Attempts have been made to further extend the life of such hot-dip Al-Zn coated steel sheets, and hot-dip Al-Zn-Si-Mg coated steel sheets to which Mg has been added have been put to practical use. As such a hot-dip Al-Zn-Si-Mg-plated steel sheet, for example, Patent Document 1 discloses a hot-dip Al-Zn-Si-Mg-plated steel sheet that contains an Al-Zn-Si alloy containing Mg in a plating film, the Al-Zn-Si alloy being an alloy containing 45 to 60 wt % of elemental aluminum, 37 to 46 wt % of elemental zinc, and 1.2 to 2.3 wt % of Si, and the concentration of the Mg is 1 to 5 wt %. Furthermore, Patent Document 2 discloses a hot-dip Al-Zn-Si-Mg plated steel sheet in which the plating film contains one or more of 2-10% Mg and 0.01-10% Ca to improve corrosion resistance and to enhance protective action after the base steel sheet is exposed. Furthermore, Patent Document 3 discloses a hot-dip Al-Zn-Si-Mg plated steel sheet in which a coating layer is formed containing, by mass%, 1-15% Mg, 2-15% Si, 11-25% Zn, with the balance being Al and unavoidable impurities, and the size of intermetallic compounds such as Mg2Si phase and MgZn2 phase present in the plating film is set to 10 μm or less, thereby improving the corrosion resistance of the flat plate and end faces.
[0005] The above-mentioned hot-dip Al-Zn coated steel sheet has a beautiful appearance with a spangle pattern of white metallic luster, and therefore is often used without painting, and there are strong demands for its appearance. Therefore, technologies to improve the appearance of hot-dip Al-Zn coated steel sheet have been developed. For example, Patent Document 4 discloses a hot-dip Al-Zn-Si-Mg plated steel sheet in which wrinkle-like irregular defects are suppressed by including 0.01 to 10% of Sr in the plated film. Patent Document 5 also discloses a hot-dip Al-Zn-Si-Mg plated steel sheet in which mottling defects are suppressed by including 500 to 3000 ppm of Sr in the plated film.
[0006] However, the above-mentioned hot-dip Al-Zn-plated steel sheets have a problem in that, when used in a severe corrosive environment, the plating film corrodes and white rust occurs. Since this white rust deteriorates the appearance of the steel sheet, plated steel sheets with improved white rust resistance are being developed. For example, Patent Document 6 discloses a hot-dip Al-Zn-Si-Mg plated steel sheet in which the mass ratio of Mg in the Si-Mg phase to the total amount of Mg in the plating layer is optimized for the purpose of improving the white rust resistance of processed parts. Furthermore, Patent Document 7 discloses a technology for improving resistance to blackening and white rust by forming a chemical conversion coating containing a urethane resin on the plating coating of a hot-dip Al-Zn-Si-Mg-plated steel sheet. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] Patent No. 5020228 [Patent Document 2] Patent No. 5000039 [Patent Document 3] JP 2002-12959 A [Patent Document 4] Patent No. 3983932 [Patent Document 5] Special Publication No. 2011-514934 [Patent Document 6] Patent No. 5751093 [Patent Document 7] JP 2019-155872 A Summary of the Invention [Problem to be solved by the invention]
[0008] However, the techniques disclosed in Patent Documents 1 to 3 for incorporating Mg into a plating film do not necessarily uniquely improve corrosion resistance. In the hot-dip Al-Zn-Si-Mg-plated steel sheets disclosed in Patent Documents 1 to 3, the corrosion resistance is improved only by including Mg in the plating components, but the effects of components other than the above four elements (Al, Zn, Si, Mg) and the characteristics of the metal phase and intermetallic compound phase that constitute the plating film are not taken into consideration, and it is not possible to uniformly discuss the superiority or inferiority of the corrosion resistance. Therefore, even when hot-dip Al-Zn-Si-Mg-plated steel sheets are manufactured using a plating bath composition with the same content of the above four element components, there is a problem that the corrosion resistance varies when an accelerated corrosion test is performed and the steel sheets are not necessarily superior to Al-Zn-plated steel sheets without added Mg. Similarly, in improving the appearance of the plating, wrinkle-like irregular defects cannot necessarily be eliminated by merely adding Sr to the plating film, and there have been cases where both corrosion resistance and appearance have not been achieved in the hot-dip Al-Zn-Si-Mg-plated steel sheets disclosed in Patent Documents 4 and 5. In addition, since Mg is an element that is easily oxidized, Mg contained in the plating bath may generate oxides (top dross) near the bath surface, and in the case of hot-dip plating, FeAl-based compounds (bottom dross) containing iron that are unevenly distributed in the bath or at the bottom of the plating bath over time may be generated, and these dross may adhere to the surface of the plating film, causing convex defects and impairing the appearance of the plating film surface. It is also known that when a steel sheet is plated in a molten Al-Zn-Si bath containing Mg, the Mg2Si phase, MgZn2 phase, and Si phase precipitate in addition to the α-Al phase in the plated film. However, the effect of the amount and abundance ratio of each phase on corrosion resistance has not been clarified. Furthermore, none of the techniques have been able to sufficiently improve white rust resistance. For the hot-dip Al-Zn-Si-Mg-plated steel sheet of Patent Document 6, although the improvement of white rust resistance in processed parts and flat parts after heating is described, the white rust resistance in unheated flat parts is not considered, and realization of stable white rust resistance remains a challenge. In addition, for the hot-dip Al-Zn-Si-Mg-plated steel sheet of Patent Document 7, it is not necessarily possible to obtain stable excellent corrosion resistance and white rust resistance, and further improvement is desired.
[0009] In view of the above circumstances, an object of the present invention is to provide a surface-treated steel sheet having stable and excellent corrosion resistance and white rust resistance, and a method for producing the same. [Means for solving the problem]
[0010] As a result of investigations aimed at solving the above-mentioned problems, the inventors have noticed that it is important not only to control the concentrations of Al, Zn, Si and Mg in the composition of the plating film of a surface-treated steel sheet, but also to control the concentrations of elements contained as impurities, and have found that deterioration of corrosion resistance can be effectively suppressed by appropriately controlling the Co content in particular. In addition, it was found that the amount of precipitation of the Mg2Si and Si phases formed in the plating film increases or decreases depending on the balance of each component in the plating film and the plating film formation conditions, and that the ratio of their abundance changes, and that some phases may not precipitate depending on the composition balance, and that the corrosion resistance of the surface-treated steel sheet changes depending on the abundance ratio of these phases, and that the corrosion resistance is stably improved especially when the Si phase is less than the Mg2Si and Si phases. However, it is known that it is very difficult to distinguish the difference between the Mg2Si and Si phases even by observing the plating film from the surface or cross section using a general method, such as a scanning electron microscope, using secondary electron images or backscattered electron images, and although it is possible to obtain microscopic information by observing using a transmission electron microscope, it was not possible to grasp the abundance ratio of the Mg2Si and Si phases, which determines macroscopic information such as corrosion resistance and appearance.
[0011] Therefore, the inventors conducted further intensive research and, as a result, focused on X-ray diffraction method and discovered that by utilizing the intensity ratio of specific diffraction peaks of the Mg2Si phase and the Si phase, it is possible to quantitatively define the abundance ratio of the phases, and further discovered that when the Mg2Si phase and the Si phase satisfy a specific abundance ratio in the plating film, stable and excellent corrosion resistance can be achieved. In addition, the present inventors have found that by controlling the Co content and the abundance ratio of the MgSi phase and the Si phase in the plating film described above, and then controlling the Sr concentration in the plating bath, it is possible to reliably suppress the occurrence of wrinkle-like uneven defects and obtain a plated steel sheet with excellent surface appearance.
[0012] Furthermore, the present inventors also investigated the chemical conversion film formed on the plating film, and found that by forming the chemical conversion film from a specific resin and a specific metal compound, the affinity of the chemical conversion film with the plating film and the rust prevention effect, etc. can be increased, and the white rust resistance can be steadily improved.
[0013] The present invention has been made based on the above findings, and the gist of the present invention is as follows. 1. A surface-treated steel sheet having a plating film and a chemical conversion film formed on the plating film, The plating film has a composition containing 45 to 65 mass% Al, 1.0 to 4.0 mass% Si, and 1.0 to 10.0 mass% Mg, with the remainder being Zn and unavoidable impurities; the Co content in the unavoidable impurities is 0.080 mass% or less with respect to the total mass of the plating film, and the diffraction intensities of Si and MgSi in the plating film, as determined by an X-ray diffraction method, satisfy the following relationship (1), Si (111) / Mg2Si (111)≦0.8 ···(1) Si (111): Diffraction intensity of the Si (111) plane (plane spacing d = 0.3135 nm), Mg2Si (111): Diffraction intensity of the (111) plane of Mg2Si (plane spacing d = 0.3668 nm) The chemical conversion coating film is a surface-treated steel sheet characterized in that it contains at least one resin selected from the group consisting of epoxy resins, urethane resins, acrylic resins, acrylic silicone resins, alkyd resins, polyester resins, polyalkylene resins, amino resins, and fluororesins, and at least one metal compound selected from the group consisting of P compounds, Si compounds, Co compounds, Ni compounds, Zn compounds, Al compounds, Mg compounds, V compounds, Mo compounds, Zr compounds, Ti compounds, and Ca compounds.
[0014] 2. The surface-treated steel sheet according to item 1 above, characterized in that the diffraction intensity of Si in the plating film as determined by an X-ray diffraction method satisfies the following relationship (2): Si(111)=0 (2) Si (111): Diffraction intensity of the Si (111) plane (plane spacing d = 0.3135 nm)
[0015] 3. The surface-treated steel sheet according to 1 or 2 above, wherein the plating film further contains 0.01 to 1.0 mass % of Sr.
[0016] 4. The surface-treated steel sheet according to any one of 1 to 3 above, wherein the Al content in the plating film is 50 to 60 mass %.
[0017] 5. The surface-treated steel sheet according to any one of 1 to 4 above, wherein the Si content in the plating film is 1.0 to 3.0 mass %.
[0018] 6. The surface-treated steel sheet according to any one of 1 to 5 above, wherein the Mg content in the plating film is 1.0 to 5.0 mass %.
[0019] 7. A method for producing a surface-treated steel sheet having a plating film and a chemical conversion film formed on the plating film, comprising: The chemical conversion coating contains at least one resin selected from the group consisting of epoxy resins, urethane resins, acrylic resins, acrylic silicone resins, alkyd resins, polyester resins, polyalkylene resins, amino resins, and fluororesins, and at least one metal compound selected from the group consisting of P compounds, Si compounds, Co compounds, Ni compounds, Zn compounds, Al compounds, Mg compounds, V compounds, Mo compounds, Zr compounds, Ti compounds, and Ca compounds, The method for producing a surface-treated steel sheet, characterized in that the formation of the plating film includes a hot-dip galvanizing process in which a base steel sheet is immersed in a plating bath having a composition containing 45-65 mass% Al, 1.0-4.0 mass% Si, and 1.0-10.0 mass% Mg, with the balance being Zn and unavoidable impurities, and the Co content in the unavoidable impurities of the plating bath is controlled to 0.080 mass% or less with respect to the total mass of the plating bath. 8. The method for producing a surface-treated steel sheet according to 7 above, wherein the coating bath further contains 0.01 to 1.0 mass % of Sr. Effect of the Invention
[0020] According to the present invention, it is possible to provide a surface-treated steel sheet having stably excellent corrosion resistance and white rust resistance, and a method for producing the same. [Brief description of the drawings]
[0021] [Figure 1] FIG. 1 is a diagram for explaining the flow of the Japanese Automotive Standard Combined Cycle Test (JASO-CCT). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0022] <Surface-treated steel sheet> The surface-treated steel sheet of the present invention comprises a plating film on the surface of the steel sheet, and a chemical conversion film formed on the plating film.
[0023] (Plating film) In the coated steel sheet of the present invention, the plating film has a composition containing 45 to 65 mass % Al, 1.0 to 4.0 mass % Si, 1.0 to 10.0 mass % Mg, with the balance being Zn and unavoidable impurities.
[0024] The Al content in the plating film is 45 to 65 mass%, preferably 50 to 60 mass%, in consideration of the balance between corrosion resistance and operation. This is because, if the Al content in the plating film is at least 45 mass%, dendritic solidification of Al occurs, and a plating film structure mainly composed of a dendritic solidification structure of the α-Al phase can be obtained. The dendritic solidification structure has a structure in which it is laminated in the thickness direction of the plating film, so that the corrosion progression path becomes complex, and the corrosion resistance of the plating film itself is improved. In addition, the more the α-Al phase dendrite parts are laminated, the more complex the corrosion progression path becomes, and it becomes difficult for corrosion to reach the base steel sheet, so that the corrosion resistance is improved, and therefore the Al content is preferably 50 mass% or more. On the other hand, if the Al content in the plating film exceeds 65 mass%, most of the Zn changes to a structure in which it is solid-solved in α-Al, and the dissolution reaction of the α-Al phase cannot be suppressed, and the corrosion resistance of the Al-Zn-Si-Mg-based plating is deteriorated. For this reason, the Al content in the plating film must be 65 mass % or less, and is preferably 60 mass % or less.
[0025] The Si in the plating film is added mainly for the purpose of suppressing the growth of the Fe-Al and / or Fe-Al-Si interfacial alloy layer formed at the interface with the base steel sheet and preventing the deterioration of the adhesion between the plating film and the steel sheet. In fact, when a steel sheet is immersed in an Al-Zn plating bath containing Si, Fe on the steel sheet surface reacts with Al and Si in the bath to form an Fe-Al and / or Fe-Al-Si intermetallic compound layer at the interface between the base steel sheet and the plating film. At this time, since the growth rate of the Fe-Al-Si alloy is slower than that of the Fe-Al alloy, the higher the ratio of the Fe-Al-Si alloy, the more the growth of the entire interfacial alloy layer is suppressed. Therefore, the Si content in the plating film must be 1.0 mass% or more. On the other hand, if the Si content in the plating film exceeds 4.0 mass%, not only is the effect of suppressing the growth of the interfacial alloy layer saturated, but the presence of an excess Si phase in the plating film promotes corrosion, so the Si content is set to 4.0 mass% or less. Furthermore, the Si content in the plating film is preferably 3.0 mass% or less from the viewpoint of suppressing the presence of an excessive Si phase. In addition, the Si content is preferably 1.0 to 3.0 mass% from the viewpoint of easily satisfying the relational expression (1) described later in relation to the Mg content described later.
[0026] The plating film contains 1.0 to 10.0 mass % of Mg. By including Mg in the plating film, the above-mentioned Si can be present in the form of an intermetallic compound of Mg2Si phase, and the promotion of corrosion can be suppressed. Furthermore, when Mg is contained in the plating film, an intermetallic compound, MgZn2 phase, is also formed in the plating film, and the effect of further improving corrosion resistance is obtained. When the Mg content in the plating film is less than 1.0 mass%, Mg is used to dissolve in the α-Al phase, which is the main phase, rather than to form the intermetallic compounds (Mg2Si, MgZn2), and sufficient corrosion resistance cannot be ensured. On the other hand, when the Mg content in the plating film is high, the effect of improving corrosion resistance is saturated, and in addition, the α-Al phase becomes brittle, resulting in a decrease in workability, so the content is set to 10.0% or less. Furthermore, the Mg content in the plating film is preferably set to 5.0 mass% or less from the viewpoints of suppressing the generation of dross during plating formation and facilitating plating bath management. In addition, from the viewpoint of easily satisfying the relational expression (1) described later in relation to the Si content, the Mg content is preferably 3.0 mass%, and in consideration of compatibility with dross suppression, the Mg content is more preferably 3.0 to 5.0 mass%.
[0027] The plating film contains Zn and unavoidable impurities. Among these, the unavoidable impurities contain Fe. This Fe is inevitably contained in the plating film as a result of dissolution of the steel sheet or bath-immersed equipment into the plating bath, and as a result of being supplied by diffusion from the base steel sheet during the formation of the interface alloy layer. The Fe content in the plating film is usually about 0.3 to 2.0 mass%. Other unavoidable impurities include Cr, Ni, Cu, Co, W, etc. These elements are inevitably contained in the plating film due to the fact that they are dissolved in the plating bath from the WC-based or Co-Cr-W-based thermal spray coating applied to the base steel sheet or the bath-immersing equipment made of stainless steel, that they are contained as impurities in the metal ingots that are the raw materials for the plating bath, and that they are produced using pots or bath-immersing equipment that were used in the production of plated steel sheets to which these elements were intentionally added.
[0028] The surface-treated steel sheet of the present invention is characterized in that the Co content in the unavoidable impurities is 0.080 mass% or less with respect to the total mass of the plating film. Since Co contained in the plating film may deteriorate the corrosion resistance of the surface-treated steel sheet, deterioration of the corrosion resistance can be suppressed by appropriately controlling the contents of Al, Zn, Si and Mg in the plating film described above and further reducing the Co content as an unavoidable impurity. From the same viewpoint, the Co content in the unavoidable impurities is preferably 0.020 mass% or less with respect to the total mass of the plating film, more preferably 0.001 mass% or less, and most preferably 0 mass%.
[0029] Co contained in the plating film is mainly present as a solid solution element in α-Al. When Co is contained in a concentration exceeding the solid solubility limit, it may precipitate as Fe-Co-Al compounds or Fe-Co-Al-Si compounds in the alloy layer formed at the base steel / plating interface. In addition, although the mechanism by which the corrosion resistance deteriorates due to the inclusion of Co as an impurity is uncertain, it is hypothesized that the corrosion rate increases due to a decrease in the barrier properties of the α-Al phase in which Co is dissolved, and that the corrosion rate increases due to Co-containing compounds functioning as a cathode in a corrosive environment and forming a local battery with the surrounding solidified structure.
[0030] Furthermore, the total content of unavoidable impurities in the plating film is not particularly limited, but if contained in excess, it may affect various properties of the plated steel sheet, so it is preferable that the total content be 5.0 mass% or less.
[0031] In the coated steel sheet of the present invention, the diffraction intensities of Si and Mg2Si in the plating film, as determined by an X-ray diffraction method, are required to satisfy the following relationship (1): Si (111) / Mg2Si (111)≦0.8 ···(1) Si (111): Diffraction intensity of the Si (111) plane (interplanar spacing d = 0.3135 nm), Mg2Si (111): Diffraction intensity of the Mg2Si (111) plane (interplanar spacing d = 0.3668 nm)
[0032] As mentioned above, in the present invention, it is important to control the ratio of the Mg2Si phase and the Si phase that are generated in the plating film due to the inclusion of Mg and Si to a specific ratio. Although the influence of these on the corrosion resistance is still under investigation and many points remain unclear, the following mechanism is presumed.
[0033] When a surface-treated steel sheet is exposed to a corrosive environment, the above-mentioned intermetallic compounds dissolve preferentially over the α-Al phase, resulting in an Mg-rich environment in the vicinity of the formed corrosion products. It is presumed that in such a Mg-rich environment, the formed corrosion products are less likely to decompose, and as a result, the protective effect of the plating film is enhanced. In addition, since the protective effect of the plating film is more reliably expressed when Si in the plating film exists as the Mg2Si phase rather than the Si phase, it is considered effective to reduce the ratio of the Si phase to the Mg2Si phase.
[0034] The abundance ratio of Si and Mg2Si in the plating film is required to satisfy the relationship (1): Si (111) / Mg2Si (111)≦0.8 using the diffraction peak intensity obtained by X-ray diffraction. However, if the abundance ratio of Si and Mg2Si in the plating film does not satisfy the relationship (1), that is, Si (111) / Mg2Si (111)>0.8, the Si phase present in the plating film increases, and the above-mentioned Mg-rich environment cannot be obtained in the vicinity of the corrosion product, making it difficult to obtain the protective effect of the plating film. From the same viewpoint, the abundance ratio of Si to Mg2Si (Si (111) / Mg2Si (111)) is preferably 0.5 or less, more preferably 0.3 or less, and particularly preferably 0.2 or less.
[0035] Here, in the above relationship (1), Si (111) is the diffraction intensity of the Si (111) plane (planar spacing d=0.3135 nm), and Mg2Si (111) is the diffraction intensity of the Mg2Si (111) plane (planar spacing d=0.3668 nm). The method for measuring Si(111) and Mg2Si(111) by X-ray diffraction involves mechanically scraping off a portion of the plating film, powdering it, and performing X-ray diffraction on the powdered state (powder X-ray diffraction measurement method). The diffraction intensity is measured by measuring the diffraction peak intensity of Si corresponding to the interplanar spacing d=0.3135 nm and the diffraction peak intensity of Mg2Si corresponding to the interplanar spacing d=0.3668 nm, and calculating the ratio between these to obtain Si(111) / Mg2Si(111). The amount of the plating film required for carrying out the powder X-ray diffraction measurement (amount of the plating film to be scraped off) is 0.1 g or more, preferably 0.3 g or more, from the viewpoint of accurately measuring Si(111) and Mg2Si(111). When the plating film is scraped off, steel sheet components other than the plating film may be contained in the powder, but these intermetallic compound phases are contained only in the plating film and do not affect the above-mentioned peak intensity. Furthermore, the plating film is powdered and X-ray diffraction is carried out because, when X-ray diffraction is carried out on the plating film formed on the plated steel sheet, it is affected by the plane orientation of the plating film solidification structure, making it difficult to calculate the correct phase ratio.
[0036] In addition, in the surface-treated steel sheet of the present invention, since the concentrations of the above-mentioned Al, Zn, Si, Mg, and Co as an unavoidable impurity can be controlled and the corrosion resistance can be more stably improved, it is preferable that the diffraction intensity of Si in the plating film by an X-ray diffraction method satisfies the following relationship (2). Si(111)=0 (2) Si (111): Diffraction intensity of the Si (111) plane (plane spacing d = 0.3135 nm) In general, it is known that in the dissolution reaction of an Al alloy in an aqueous solution, the presence of a Si phase as a cathode site promotes the dissolution of the surrounding α-Al phase. Therefore, reducing the amount of Si phase is also effective in terms of suppressing the dissolution of the α-Al phase. Among these, a coating in which no Si phase exists, as shown in relationship (2) (the diffraction peak intensity of the Si(111) is set to zero) is the most excellent in terms of stabilizing corrosion resistance. The method for measuring the diffraction peak intensity of the Si (111) plane by X-ray diffraction is as described above.
[0037] Here, the method for satisfying the above-mentioned relationship (1) or relationship (2) is not particularly limited. For example, in order to satisfy the relationship (1) or relationship (2), the abundance ratio of Si and Mg2Si (diffraction intensity of Si(111) and Mg2Si(111)) can be controlled by adjusting the balance of the Si content, Mg content, and Al content in the plating film. The balance of the Si content, Mg content, and Al content in the plating film does not necessarily satisfy the relationship (1) or relationship (2) by setting the content ratio of Si, Mg content, and Al to a constant content ratio, and it is necessary to change the content ratio of Mg and Al depending on the Si content (mass%), for example. In addition to adjusting the balance of the Si content, the Mg content, and the Al content in the plating film, the diffraction intensities of Si(111) and MgSi(111) can be controlled so as to satisfy the relationship (1) or (2) by adjusting the conditions for forming the plating film (e.g., the cooling conditions after plating).
[0038] In the surface-treated steel sheet of the present invention, the plating film preferably contains 0.01 to 1.0 mass % of Sr. When the plating film contains Sr, the occurrence of surface defects such as wrinkle-like irregularities can be more reliably suppressed, and good surface appearance can be achieved. The wrinkle-like defect is a wrinkle-like uneven defect formed on the surface of the plating film, and is observed as a whitish streak on the surface of the plating film. Such wrinkle-like defects are likely to occur when a large amount of Mg is added to the plating film. Therefore, in the hot-dip plated steel sheet, by adding Sr to the plating film, Sr is oxidized preferentially over Mg in the surface layer of the plating film, and the oxidation reaction of Mg is suppressed, thereby making it possible to suppress the occurrence of the wrinkle-like defect.
[0039] In addition, since the plating film can improve the stability of corrosion products and retard the progress of corrosion like Mg, it is preferable that the plating film further contains one or more selected from Cr, Mn, V, Mo, Ti, Ca, Sb, and B in a total amount of 0.01 to 10 mass%. The reason why the total content of the above-mentioned components is set to 0.01 to 10 mass% is that a sufficient corrosion retardation effect can be obtained and the effect does not saturate.
[0040] From the viewpoint of satisfying various characteristics, the coating weight of the plating film is set to 45 to 120 g / m2 per side. 2 It is preferable that the coating weight of the plating film is 45 g / m 2 In the above cases, sufficient corrosion resistance is obtained for applications requiring long-term corrosion resistance, such as building materials, and the coating weight of the plating film is 120 g / m 2 This is because, in the following cases, it is possible to realize excellent corrosion resistance while suppressing the occurrence of plating cracks during processing. From the same viewpoint, the coating weight of the plating film is 45 to 100 g / m 2 It is more preferable that:
[0041] The coating weight of the plating film can be derived, for example, by a method in which a specific area of the plating film is dissolved and peeled off with a mixed solution of hydrochloric acid and hexamethylenetetramine as specified in JIS H 0401: 2013, and the coating weight is calculated from the difference in the weight of the steel sheet before and after peeling. To determine the coating weight per side using this method, the plating surface of the non-target side is sealed with tape so as not to be exposed, and then the above-mentioned dissolution is carried out.
[0042] Similarly to the above-mentioned Co content, the composition of the plating film can be confirmed by immersing the plating film in hydrochloric acid or the like to dissolve it, and subjecting the solution to ICP emission spectrometry, atomic absorption spectrometry, etc. This method is merely one example, and any method that can accurately quantify the composition of the plating film may be used, and is not particularly limited.
[0043] The plating film of the coated steel sheet obtained by the present invention has a composition substantially equivalent to that of the plating bath as a whole, and therefore the composition of the plating film can be controlled with high precision by controlling the composition of the plating bath.
[0044] Furthermore, the base steel sheet constituting the surface-treated steel sheet of the present invention is not particularly limited, and cold-rolled steel sheet, hot-rolled steel sheet, etc. can be used as appropriate depending on the required performance and specifications.
[0045] Furthermore, the method for obtaining the base steel sheet is not particularly limited. For example, in the case of the hot-rolled steel sheet, one that has been subjected to a hot rolling process and a pickling process can be used, and in the case of the cold-rolled steel sheet, it can be manufactured by further adding a cold rolling process. Furthermore, in order to obtain the properties of the steel sheet, it is also possible to pass through a recrystallization annealing process or the like before the hot-dip plating process.
[0046] In addition, the conditions for forming the plating film when manufacturing the surface-treated steel sheet of the present invention are not particularly limited to a hot-dip galvanizing process in which the base steel sheet is immersed in a plating bath. The hot-dip galvanizing process can be carried out, for example, by cleaning, heating, and immersing the base steel sheet in a plating bath in a continuous hot-dip galvanizing facility. In the heating process of the steel sheet, recrystallization annealing or the like is carried out to control the structure of the base steel sheet itself, and heating in a reducing atmosphere such as a nitrogen-hydrogen atmosphere is effective in preventing oxidation of the steel sheet and reducing a small amount of oxide film present on the surface.
[0047] As for the plating bath used in the hot-dip plating process, as described above, the composition of the plating film as a whole is approximately the same as the composition of the plating bath, and therefore a plating bath having a composition containing 45 to 65 mass% Al, 1.0 to 4.0 mass% Si, and 1.0 to 10.0 mass% Mg, with the balance being Zn and unavoidable impurities, can be used.
[0048] In the hot-dip galvanizing process, the Co content in the unavoidable impurities of the coating bath must be controlled to 0.080 mass% or less with respect to the total mass of the coating bath. Since the Co contained in the coating film may deteriorate the corrosion resistance of the surface-treated steel sheet as described above, the Al, Zn, Si, and Mg contents in the coating bath are appropriately controlled, and the Co content as an unavoidable impurity is further reduced, thereby preventing deterioration of the corrosion resistance. The content of Co as an unavoidable impurity in the coating bath needs to be controlled to 0.080 mass% or less, more preferably 0.020 mass% or less, and even more preferably 0.001 mass% or less, based on the total mass of the coating bath. If the Co content in the coating bath is 0.080 mass% or less, the produced surface-treated steel sheet can have sufficiently excellent corrosion resistance. If the Co content in the coating bath is 0.020 mass% or less, the produced surface-treated steel sheet can have even better corrosion resistance, and if the Co content is 0.001 mass% or less, the produced surface-treated steel sheet can have particularly excellent corrosion resistance. Thus, since the lower the Co content in the coating bath, the better the corrosion resistance of the surface-treated steel sheet, there is no particular lower limit for the Co content, and it is most preferable that the Co content in the coating bath is 0%.
[0049] Here, the means for reducing the Co content in the plating bath is not particularly limited. For example, since it is effective to prevent the elution of a Co-Cr-W based thermal spray coating applied to a bath-immersed device into the plating bath, it is preferable to use a thermal spray coating that does not contain Co.
[0050] As another means for reducing the Co content in the plating bath, it is preferable to use a metal block having a low Co content among impurities as a raw material for the plating bath. Furthermore, it is also effective not to use pots or bath-immersed equipment used in the production of plated steel sheets to which Co is intentionally added in the production of surface-treated steel sheets, because this can prevent metal lumps containing Co adhering to the pots or bath-immersed equipment from dissolving and being mixed into the plating bath.
[0051] Furthermore, the bath temperature of the plating bath is not particularly limited, but is preferably in the range of (melting point + 20°C) to 650°C. The reason why the lower limit of the bath temperature is set to the melting point + 20°C is that the bath temperature needs to be at or above the solidification point in order to perform hot-dip plating, and setting the temperature at the melting point + 20°C prevents solidification due to a local drop in the bath temperature of the plating bath. On the other hand, the reason why the upper limit of the bath temperature is set to 650°C is that if the bath temperature exceeds 650°C, it becomes difficult to rapidly cool the plating film, and there is a risk that the interfacial alloy layer formed between the plating film and the steel sheet will become thick.
[0052] In addition, the temperature of the base steel sheet immersed in the coating bath (immersion sheet temperature) is not particularly limited, but from the viewpoint of ensuring the coating characteristics in continuous hot-dip coating operations and preventing changes in the bath temperature, it is preferable to control it to within ±20°C of the coating bath temperature.
[0053] Furthermore, the immersion time of the base steel sheet in the coating bath is preferably 0.5 seconds or more. This is because if it is less than 0.5 seconds, there is a risk that a sufficient coating film may not be formed on the surface of the base steel sheet. There is no particular upper limit to the immersion time, but since a longer immersion time may cause a thicker interfacial alloy layer to form between the coating film and the steel sheet, it is more preferable to set the immersion time to 8 seconds or less.
[0054] (Conversion coating) The surface-treated steel sheet of the present invention has a chemical conversion coating formed on the above-mentioned plating coating. The chemical conversion coating may be formed on at least one side of the surface-treated steel sheet, but may also be formed on both sides of the surface-treated steel sheet depending on the application and required performance.
[0055] In the surface-treated steel sheet of the present invention, the chemical conversion coating is characterized by containing at least one resin selected from epoxy resins, urethane resins, acrylic resins, acrylic silicone resins, alkyd resins, polyester resins, polyalkylene resins, amino resins, and fluororesins, and at least one metal compound selected from P compounds, Si compounds, Co compounds, Ni compounds, Zn compounds, Al compounds, Mg compounds, V compounds, Mo compounds, Zr compounds, Ti compounds, and Ca compounds. By forming the above-mentioned chemical conversion film on the plating film, it is possible to increase the affinity with the plating film, and to form the chemical conversion film uniformly on the plating film, and it is also possible to increase the rust prevention effect and barrier effect of the chemical conversion film, thereby making it possible to realize stable corrosion resistance and white rust resistance of the surface-treated steel sheet of the present invention.
[0056] Here, from the viewpoint of improving corrosion resistance, at least one resin selected from epoxy resin, urethane resin, acrylic resin, acrylic silicone resin, alkyd resin, polyester resin, polyalkylene resin, amino resin, and fluororesin is used as the resin constituting the conversion coating. From the same viewpoint, it is preferable that the resin contains at least one of urethane resin and acrylic resin. The resin constituting the conversion coating also includes an addition polymer of the above-mentioned resin.
[0057] As the epoxy resin, for example, glycidyl etherified epoxy resins such as bisphenol A type, bisphenol F type, and novolac type epoxy resins, glycidyl etherified bisphenol A type epoxy resins with added propylene oxide, ethylene oxide, or polyalkylene glycol, aliphatic epoxy resins, alicyclic epoxy resins, polyether-based epoxy resins, and the like can be used.
[0058] As the urethane resin, for example, an oil-modified polyurethane resin, an alkyd-based polyurethane resin, a polyester-based polyurethane resin, a polyether-based polyurethane resin, a polycarbonate-based polyurethane resin, or the like can be used.
[0059] Examples of the acrylic resin include polyacrylic acid and copolymers thereof, polyacrylic acid esters and copolymers thereof, polymethacrylic acid and copolymers thereof, polymethacrylic acid esters and copolymers thereof, urethane-acrylic acid copolymers (or urethane-modified acrylic resins), styrene-acrylic acid copolymers, and the like. Furthermore, these resins modified with other alkyd resins, epoxy resins, phenolic resins, and the like can be used.
[0060] The acrylic silicone resin may be, for example, a resin having hydrolyzable alkoxysilyl groups at the side chain or end of an acrylic copolymer as a base material, to which a curing agent is added, etc. In addition, when using an acrylic silicone resin, excellent weather resistance can be expected in addition to corrosion resistance.
[0061] Examples of the alkyd resin include oil-modified alkyd resins, rosin-modified alkyd resins, phenol-modified alkyd resins, styrenated alkyd resins, silicon-modified alkyd resins, acrylic-modified alkyd resins, oil-free alkyd resins, and high molecular weight oil-free alkyd resins.
[0062] The polyester resin is a polycondensate synthesized by dehydration condensation of a polycarboxylic acid and a polyalcohol to form an ester bond, and examples of the polycarboxylic acid include terephthalic acid and 2,6-naphthalenedicarboxylic acid, and examples of the polyalcohol include ethylene glycol, 1,3-propanediol, 1,4-butanediol, and 1,4-cyclohexanedimethanol. Specific examples of the polyester include polyethylene terephthalate, polytrimethylene terephthalate, polyethylene naphthalate, and polybutylene naphthalate. These polyester resins modified with acrylic may also be used.
[0063] Examples of the polyalkylene resin include ethylene-based copolymers such as ethylene-acrylic acid copolymers, ethylene-methacrylic acid copolymers, and carboxyl-modified polyolefin resins, ethylene-unsaturated carboxylic acid copolymers, and ethylene-based ionomers. Furthermore, these resins modified with other alkyd resins, epoxy resins, phenolic resins, and the like can be used.
[0064] The amino resin is a thermosetting resin produced by the reaction of an amine or amide compound with an aldehyde, and examples of the resin include melamine resin, guanamine resin, and thiourea resin, with melamine resin being preferred from the viewpoints of corrosion resistance, weather resistance, adhesion, etc. The melamine resin is not particularly limited, but examples thereof include butylated melamine resin, methylated melamine resin, and aqueous melamine resin.
[0065] Examples of the fluororesin include fluoroolefin polymers and copolymers of fluoroolefin with alkyl vinyl ether, cycloalkyl vinyl ether, carboxylic acid-modified vinyl ester, hydroxyalkyl allyl ether, tetrafluoropropyl vinyl ether, etc. When these fluororesins are used, not only corrosion resistance but also excellent weather resistance and excellent hydrophobicity can be expected.
[0066] Furthermore, in order to improve corrosion resistance and workability, it is particularly preferable to use a curing agent for the resin constituting the chemical conversion coating. As the curing agent, amino resins such as urea resins (butylated urea resins, etc.), melamine resins (butylated melamine resins, butyl etherified melamine resins, etc.), butylated urea-melamine resins, and benzoguanamine resins, blocked isocyanates, oxazoline compounds, and phenolic resins can be appropriately used.
[0067] The metal compound constituting the chemical conversion coating is at least one selected from the group consisting of P compounds, Si compounds, Co compounds, Ni compounds, Zn compounds, Al compounds, Mg compounds, V compounds, Mo compounds, Zr compounds, Ti compounds, and Ca compounds. From the same viewpoint, it is preferable that the metal compound contains at least one of P compounds, Si compounds, and V compounds.
[0068] The P compound contained in the chemical conversion coating can improve corrosion resistance and sweat resistance. The P compound is a compound containing P, and can contain, for example, one or more selected from inorganic phosphoric acid, organic phosphoric acid, and salts thereof.
[0069] The inorganic phosphoric acid, organic phosphoric acid, and salts thereof are not particularly limited and any compound can be used. For example, the inorganic phosphoric acid is preferably one or more selected from phosphoric acid, primary phosphate, secondary phosphate, tertiary phosphate, pyrophosphoric acid, pyrophosphate, tripolyphosphoric acid, tripolyphosphate, phosphorous acid, phosphite, hypophosphorous acid, and hypophosphite. The organic phosphoric acid is preferably phosphonic acid (phosphonic acid compound). The phosphonic acid is preferably one or more selected from nitrilotrismethylenephosphonic acid, phosphonobutanetricarboxylic acid, methyldiphosphonic acid, methylenephosphonic acid, and ethylidenediphosphonic acid. When the P compound is a salt, the salt is preferably a salt of an element of Groups 1 to 13 in the periodic table, more preferably a metal salt, and is preferably one or more selected from alkali metal salts and alkaline earth metal salts.
[0070] When the chemical conversion treatment solution containing the above-mentioned P compound is applied to a plated steel sheet, the surface of the plated film is etched by the action of the P compound, and a concentrated layer containing Al, Zn, Si, and Mg, which are the constituent elements of the plated film, is formed on the plated film side of the chemical conversion film. The formation of the concentrated layer strengthens the bond between the chemical conversion film and the plated film surface, improving the adhesion of the chemical conversion film. The concentration of the P compound in the chemical conversion treatment solution is not particularly limited, but can be 0.25% by mass to 5% by mass. If the concentration of the P compound is less than 0.25% by mass, the etching effect is insufficient, the adhesion to the plating interface is reduced, and not only the corrosion resistance of the flat surface is reduced, but also the corrosion resistance and sweat resistance of defective parts, cut end faces, and damaged parts of the plating and film caused by processing may be reduced. From the same viewpoint, the concentration of the P compound is preferably 0.35% by mass or more, more preferably 0.50% by mass or more. On the other hand, if the concentration of the P compound exceeds 5% by mass, not only the life of the chemical conversion treatment solution is shortened, but also the appearance of the film when formed is likely to be non-uniform, and the amount of P eluted from the chemical conversion film increases, which may reduce the resistance to blackening. From the same viewpoint, the concentration of the P compound is preferably 3.5% by mass or less, more preferably 2.5% by mass or less. Regarding the content of the P compound in the chemical conversion coating, for example, a chemical conversion treatment solution containing a P compound at a concentration of 0.25% by mass to 5% by mass is applied and dried, so that the amount of P attached in the chemical conversion coating after drying is 5 to 100 mg / m 2 It can be said that:
[0071] The Si compound is a component that becomes a framework for forming a chemical conversion coating together with the resin, and can enhance affinity with the plating coating to form a uniform chemical conversion coating. The Si compound is a compound containing Si, and preferably contains one or more selected from, for example, silica, trialkoxysilane, tetraalkoxysilane, and a silane coupling agent.
[0072] The silica is not particularly limited and any silica can be used. For example, at least one of wet silica and dry silica can be used. For example, Snowtex O, C, N, S, 20, OS, OXS, NS, etc. manufactured by Nissan Chemical Industries, Ltd. can be suitably used as colloidal silica, which is a type of wet silica. For example, AEROSIL 50, 130, 200, 300, 380, etc. manufactured by Nippon Aerosil Co., Ltd. can be suitably used as the dry silica.
[0073] The trialkoxysilane is not particularly limited and any trialkoxysilane can be used. For example, it is preferable to use a trialkoxysilane represented by the general formula: R1Si(OR2)3 (wherein R1 is hydrogen or an alkyl group having 1 to 5 carbon atoms, and R2 is the same or different alkyl group having 1 to 5 carbon atoms). Examples of such trialkoxysilane include trimethoxysilane, triethoxysilane, and methyltriethoxysilane.
[0074] The tetraalkoxysilane is not particularly limited and any tetraalkoxysilane can be used. For example, it is preferable to use a tetraalkoxysilane represented by the general formula: Si(OR)4 (wherein R is the same or different alkyl group having 1 to 5 carbon atoms). Examples of such tetraalkoxysilane include tetramethoxysilane, tetraethoxysilane, and tetrapropoxysilane.
[0075] The silane coupling agent is not particularly limited and any one can be used. For example, γ-glycidoxypropyl trimethoxysilane, γ-glycidoxypropyl methyl diethoxysilane, γ-glycidoxypropyl triethoxysilane, γ-aminopropyl trimethoxysilane, γ-aminopropyl methyl diethoxysilane, γ-aminopropyl triethoxysilane, γ-methacryloxypropyl trimethoxysilane, γ-methacryloxypropyl triethoxysilane, γ-mercaptopropyl methyl dimethoxysilane, γ-mercaptopropyl trimethoxysilane, vinyl triethoxysilane, γ-isocyanate propyl triethoxysilane, etc. can be mentioned.
[0076] By incorporating the Si compound in the chemical conversion film, the Si compound undergoes dehydration condensation to form an amorphous chemical conversion film having siloxane bonds that have a high barrier effect of shielding corrosion factors. In addition, by bonding with the above-mentioned resin, a chemical conversion film with higher barrier properties is formed. Furthermore, in a corrosive environment, dense and stable corrosion products are formed in defective parts or damaged parts of the plating or film caused by processing, etc., and the combined effect with the plating film also has the effect of suppressing corrosion of the base steel sheet. From the viewpoint of a high effect of forming a stable corrosion product, it is preferable to use at least one of colloidal silica and dry silica as the Si compound.
[0077] The concentration of the Si compound in the chemical conversion treatment liquid for forming the chemical conversion coating is 0.2% by mass to 9.5% by mass. If the concentration of the Si compound in the chemical conversion treatment liquid is 0.2% by mass or more, a barrier effect due to siloxane bonds can be obtained, and as a result, in addition to the corrosion resistance of flat surfaces, the corrosion resistance of defective parts, cut parts, and parts damaged due to processing, etc., and sweat resistance are improved. Furthermore, if the concentration of the Si compound is 9.5% by mass or less, the life of the chemical conversion treatment liquid can be extended. By applying and drying a chemical conversion treatment liquid with a Si compound concentration of 0.2% by mass to 9.5% by mass, the Si adhesion amount in the chemical conversion coating after drying can be 2 to 95 mg / m 2 It can be said that:
[0078] The Co compound and the Ni compound contained in the chemical conversion coating can improve the blackening resistance. This is believed to be because Co and Ni have the effect of delaying the elution of water-soluble components from the coating in a corrosive environment. In addition, the Co and Ni are elements that are less likely to be oxidized than Al, Zn, Si, Mg, and the like. Therefore, by concentrating (forming a concentrated layer) at least one of the Co compound and the Ni compound at the interface between the chemical conversion coating and the plating coating, the concentrated layer becomes a barrier against corrosion, and as a result, the blackening resistance can be improved.
[0079] By using a chemical conversion treatment solution containing the Co compound, Co can be contained in the chemical conversion coating and incorporated into the concentrated layer. As the Co compound, a cobalt salt is preferably used. As the cobalt salt, one or more selected from cobalt sulfate, cobalt carbonate, and cobalt chloride are more preferably used. In addition, by using a chemical conversion treatment solution containing the Ni compound, Ni can be contained in the chemical conversion coating and incorporated into the concentrated layer. As the Ni compound, a nickel salt is preferably used. As the nickel salt, it is more preferable to use one or more selected from nickel sulfate, nickel carbonate, and nickel chloride.
[0080] The concentration of the Co compound and / or Ni compound in the chemical conversion treatment liquid is not particularly limited, but can be 0.25 mass% to 5 mass% in total. If the concentration of the Co compound and / or Ni compound is less than 0.25 mass%, the interface thickened layer becomes nonuniform, and not only the corrosion resistance of the flat portion decreases, but also the corrosion resistance of the plating or film damaged portion caused by defects, cut end faces, processing, etc. may decrease. From the same viewpoint, it is preferably 0.5 mass% or more, more preferably 0.75 mass% or more. On the other hand, if the concentration of the Co compound and / or Ni compound exceeds 5 mass%, the appearance of the formed film is likely to become nonuniform, and the corrosion resistance may decrease. From the same viewpoint, it is preferably 4.0 mass% or less, more preferably 3.0 mass% or less. By applying and drying the chemical conversion treatment liquid having a total concentration of the Co compound and / or Ni compound of 0.25 mass% to 5 mass%, the total adhesion amount of Co and Ni in the chemical conversion film after drying is 5 to 100 mg / m 2 It can be said that:
[0081] The Al compound, the Zn compound, and the Mg compound are contained in the chemical conversion treatment solution, so that a concentrated layer containing at least one of Al, Zn, and Mg can be formed on the plating film side of the chemical conversion film. The formed concentrated layer can improve corrosion resistance. The Al compound, the Zn compound, and the Mg compound are not particularly limited as long as they are compounds containing Al, Zn, and Mg, respectively, but are preferably inorganic compounds, and are preferably salts, chlorides, oxides, or hydroxides.
[0082] The Al compound may be, for example, one or more selected from aluminum sulfate, aluminum carbonate, aluminum chloride, aluminum oxide, and aluminum hydroxide. The Zn compound may be, for example, one or more selected from zinc sulfate, zinc carbonate, zinc chloride, zinc oxide, and zinc hydroxide. The Mg compound may be, for example, one or more selected from magnesium sulfate, magnesium carbonate, magnesium chloride, magnesium oxide, and magnesium hydroxide.
[0083] The total concentration of the Al compound, Zn compound and / or Mg compound in the chemical conversion treatment solution for forming the chemical conversion coating is preferably 0.25% by mass to 5% by mass. If the total concentration is 0.25% by mass or more, the concentrated layer can be formed more effectively, and as a result, the corrosion resistance can be further improved. On the other hand, if the total concentration is 5% by mass or less, the appearance of the chemical conversion coating becomes more uniform, and the corrosion resistance of flat parts, defective parts, and damaged parts of the plating or coating caused by processing, etc. is further improved.
[0084] The V compound contained in the chemical conversion coating allows the V to be appropriately dissolved in a corrosive environment and to bond with zinc ions and other plating components that also dissolve in a corrosive environment to form a dense protective coating. The formed protective coating can further increase corrosion resistance not only to the flat surface of the steel sheet, but also to defects, damaged areas of the plating coating caused by processing, corrosion that progresses from the cut end surface to the flat surface, and the like.
[0085] The V compound is a compound containing V, and examples thereof include one or more selected from sodium metavanadate, vanadyl sulfate, and vanadium acetylacetonate.
[0086] The V compound in the chemical conversion treatment solution for forming the chemical conversion coating is preferably 0.05% by mass to 4% by mass. If the concentration of the V compound is 0.05% by mass or more, it is easy to dissolve in a corrosive environment to form a protective coating, and the corrosion resistance of defective parts, cut end faces, and damaged parts of the plating coating caused by processing is improved. On the other hand, if the concentration of the V compound exceeds 4% by mass, the appearance of the formed chemical conversion coating is likely to be non-uniform, and the resistance to blackening is also reduced.
[0087] The Mo compound, when contained in the chemical conversion coating, can enhance the blackening resistance of the surface-treated steel sheet. The Mo compound is a compound containing Mo, and can be obtained by adding one or both of molybdic acid and a molybdate to the chemical conversion treatment solution. The molybdate may be, for example, one or more selected from sodium molybdate, potassium molybdate, magnesium molybdate, and zinc molybdate.
[0088] The concentration of the Mo compound in the chemical conversion treatment solution for forming the chemical conversion coating is preferably 0.01% by mass to 3% by mass. If the concentration of the Mo compound is 0.01% by mass or more, the generation of oxygen-deficient zinc oxide is further suppressed, and blackening resistance can be further improved. On the other hand, if the concentration of the Mo compound is 3% by mass or less, the life of the chemical conversion treatment solution is further extended and corrosion resistance can be further improved.
[0089] The Zr compound and the Ti compound contained in the chemical conversion coating can prevent the chemical conversion coating from becoming porous and can densify the coating, which makes it difficult for corrosive factors to permeate the chemical conversion coating and improves corrosion resistance.
[0090] The Zr compound is a compound containing Zr, and for example, one or more selected from zirconyl acetate, zirconyl sulfate, potassium zirconyl carbonate, sodium zirconyl carbonate, and ammonium zirconyl carbonate can be used. Among these, organic titanium chelate compounds are preferred because they densify the film when the chemical conversion treatment liquid is dried to form the film, thereby obtaining better corrosion resistance.
[0091] The Ti compound is a compound containing Ti, and for example, one or more selected from titanium sulfate, titanium chloride, titanium hydroxide, titanium acetylacetonate, titanium octylene glycolate, and titanium ethylacetoacetate can be used.
[0092] The concentration of the Zr compound and / or Ti compound in the chemical conversion treatment solution for forming the chemical conversion coating is preferably 0.2% by mass to 20% by mass in total. If the total concentration of the Zr compound and / or Ti compound is 0.2% by mass or more, the effect of inhibiting the permeation of corrosion factors is enhanced, and the corrosion resistance of not only the flat surface corrosion resistance but also the corrosion resistance of defective parts, cut end faces, and parts of the plating film damaged by processing can be further improved. On the other hand, if the total concentration of the Zr compound and / or Ti compound is 20% by mass or less, the life of the chemical conversion treatment solution can be further extended.
[0093] The Ca compound contained in the chemical conversion coating can exert an effect of reducing the corrosion rate.
[0094] The Ca compound is a compound containing Ca, and examples of the Ca compound include Ca oxide, Ca nitrate, Ca sulfate, and intermetallic compounds containing Ca. More specifically, examples of the Ca compound include CaO, CaCO3, Ca(OH)2, Ca(NO3)2·4H2O, and CaSO4·2H2O. The content of the Ca compound in the chemical conversion coating is not particularly limited.
[0095] The chemical conversion coating may contain various known components commonly used in the coating field, as necessary, such as various surface conditioners, such as leveling agents and antifoaming agents, various additives, such as dispersants, anti-settling agents, ultraviolet absorbers, light stabilizers, silane coupling agents and titanate coupling agents, various pigments, such as color pigments, extender pigments and luster materials, curing catalysts, organic solvents and lubricants.
[0096] In the surface-treated steel sheet of the present invention, it is preferable that the chemical conversion coating does not contain harmful components such as hexavalent chromium, trivalent chromium, fluorine, etc. This is because the chemical conversion treatment solution for forming the chemical conversion coating does not contain these harmful components, resulting in high safety and low environmental impact.
[0097] The coating weight of the chemical conversion coating is not particularly limited. For example, from the viewpoint of preventing peeling of the chemical conversion coating while more reliably securing corrosion resistance, the coating weight of the chemical conversion coating is set to 0.1 to 3.0 g / m 2 It is preferable to set the thickness to 0.5 to 2.5 g / m 2 It is more preferable that the coating weight of the chemical conversion coating is 0.1 g / m 2 By setting the coating weight at 3.0 g / m or more, corrosion resistance can be more reliably ensured, and the coating weight of the chemical conversion film is 3.0 g / m or more. 2 By setting the temperature below 100° C., cracking and peeling of the chemical conversion coating can be prevented. The coating weight of the chemical conversion coating may be determined by a method appropriately selected from existing techniques, such as a method of subjecting the coating to fluorescent X-ray analysis to measure the amount of an element present in the coating whose content is known in advance.
[0098] The method for forming the chemical conversion coating is not particularly limited, and can be appropriately selected according to the required performance, manufacturing equipment, etc. For example, the chemical conversion coating can be formed by continuously applying a chemical conversion treatment solution onto the plating film using a roll coater or the like, and then drying at a peak metal temperature (PMT) of about 60 to 200°C using hot air or induction heating. In addition to the roll coater, known methods such as airless spray, electrostatic spray, and curtain flow coater can be appropriately used to apply the chemical conversion treatment solution. Furthermore, the chemical conversion coating may be either a single-layer film or a multi-layer film as long as it contains the resin and the metal compound, and is not particularly limited.
[0099] In addition, in the surface-treated steel sheet of the present invention, a paint film can be formed on the chemical conversion film, if necessary.
[0100] <Method of manufacturing surface-treated steel sheet> The method for producing a surface-treated steel sheet of the present invention is a method for producing a surface-treated steel sheet comprising a plating film and a chemical conversion film formed on the plating film. In the manufacturing method of the present invention, the chemical conversion coating contains at least one resin selected from the group consisting of epoxy resins, urethane resins, acrylic resins, acrylic silicone resins, alkyd resins, polyester resins, polyalkylene resins, amino resins, and fluororesins, and at least one metal compound selected from the group consisting of P compounds, Si compounds, Co compounds, Ni compounds, Zn compounds, Al compounds, Mg compounds, V compounds, Mo compounds, Zr compounds, Ti compounds, and Ca compounds, The formation of the plating film includes a hot-dip galvanizing process in which a base steel sheet is immersed in a plating bath having a composition containing 45-65 mass% Al, 1.0-4.0 mass% Si, and 1.0-10.0 mass% Mg, with the balance being Zn and unavoidable impurities, and the Co content in the unavoidable impurities of the plating bath is controlled to 0.080 mass% or less.
[0101] As described above, Co contained in the plating film may deteriorate the corrosion resistance of the surface-treated steel sheet. Therefore, by appropriately controlling the contents of Al, Zn, Si, and Mg in the plating bath and further reducing the content of Co as an unavoidable impurity, deterioration of corrosion resistance can be suppressed.
[0102] The conditions for the hot dip galvanizing process are the same as those explained in the description of the plating film of the surface-treated steel sheet of the present invention. The structure of the chemical conversion coating is also the same as that described for the chemical conversion coating of the surface-treated steel sheet of the present invention. EXAMPLES
[0103] (Sample 1-134) (1) A cold-rolled steel sheet having a thickness of 0.8 mm, produced by a conventional method, was used as a base steel sheet, and annealing and plating processes were performed using a hot-dip plating simulator manufactured by Rhesca Corporation to produce samples of hot-dip plated steel sheets having the plating film conditions shown in Tables 2 and 3. The composition of the coating bath used in the production of hot-dip galvanized steel sheets was changed in various ranges of Al: 5-75 mass%, Si: 0.0-4.5 mass%, Mg: 0-10 mass%, and Co: 0.000-0.120 mass% so as to obtain the composition of the coating film of each sample shown in Tables 2 and 3. The bath temperature of the coating bath was controlled to 450°C for Al: 5 mass%, 480°C for Al: 15 mass%, 590°C for Al: 30-60 mass%, and 630°C for Al: over 60 mass%, so that the plating immersion sheet temperature of the base steel sheet was the same as the plating bath temperature. Furthermore, in the case of Al: 30-60 mass%, the plating process was performed under the condition that the sheet temperature was cooled to a temperature range of 520-500°C in 3 seconds. In addition, the coating weight of the plating film was 85±5 g / m on one side for samples 1 to 104 and 117 to 134. 2 , 50±5g / m per side for samples 105-106 2 , Samples 107 to 108 are 100±5g / m per side 2 , Samples 109-110 are 125 g / m per side 2 ±5g / m2 , Samples 111 to 116 are 70±5g / m per side 2 , was controlled so that
[0104] (2) Then, a chemical conversion coating was formed on the plating film of each sample of hot-dip plated steel sheet prepared by using a bar coater, and the plated film was dried in a hot air furnace (heating rate: 60°C / s, PMT: 120°C) to prepare each sample of surface-treated steel sheet shown in Tables 2 and 3. The chemical conversion treatment solutions were prepared by dissolving each component in water as a solvent to prepare surface treatment solutions A to F. The types of each component (resin, metal compound) contained in the surface treatment solutions are as follows. (resin) Urethane resin: Superflex 130, Superflex 126 (Dai-ichi Kogyo Seiyaku Co., Ltd.) Acrylic resin: Boncoat EC-740EF (DIC Corporation) (metal compound) P compound: Aluminum dihydrogen tripolyphosphate Silicon compounds: Silica V compound: Sodium metavanadate Mo Compounds: Molybdic Acid Zr compound: Potassium zirconyl carbonate The compositions of the prepared chemical conversion treatment solutions A to F and the adhesion weights of the formed chemical conversion coatings are shown in Table 1. The concentration of each component in Table 1 of this specification is the concentration (mass %) of the solid content.
[0105] [Table 1]
[0106] (evaluation) The following evaluations were carried out on each sample of the hot-dip plated steel sheet and the surface-treated steel sheet obtained as described above. The evaluation results are shown in Tables 2 and 3.
[0107] (1) Plating film (composition, coating weight, X-ray diffraction intensity) For each sample of hot-dip galvanized steel sheet, a 100 mm diameter cut was made, the non-measurement surface was sealed with tape, and the plating was dissolved and peeled off with a mixture of hydrochloric acid and hexamethylenetetramine as specified in JIS H 0401: 2013, and the adhesion weight of the plating film was calculated from the difference in mass of the sample before and after peeling. The calculated adhesion weights of the plating film obtained are shown in Tables 2 and 3. The stripper solution was then filtered, and the filtrate and solid content were analyzed. Specifically, the filtrate was analyzed by ICP atomic emission spectrometry to quantify the components other than insoluble Si. The solids were dried and incinerated in a 650°C heating furnace, and then melted by adding sodium carbonate and sodium tetraborate. The molten material was then dissolved in hydrochloric acid, and the solution was analyzed by ICP emission spectroscopy to quantify the insoluble silicon. The silicon concentration in the plating film was calculated by adding the soluble silicon concentration obtained by filtrate analysis to the insoluble silicon concentration obtained by solid content analysis. The compositions of the plating film obtained as a result of calculation are shown in Tables 2 and 3. In addition, each sample was sheared to a size of 100 mm x 100 mm, and the plating film on the surface to be evaluated was mechanically scraped off until the base steel sheet was revealed. The resulting powder was thoroughly mixed, and 0.3 g was taken out and a qualitative analysis of the above powder was performed using an X-ray diffraction apparatus (Rigaku Corporation, "SmartLab") under the following conditions: X-ray used: Cu-Kα (wavelength = 1.54178 Å), Kβ ray removal: Ni filter, tube voltage: 40 kV, tube current: 30 mA, scanning speed: 4° / min, sampling interval: 0.020°, divergence slit: 2 / 3°, solar slit: 5°, detector: high-speed one-dimensional detector (D / teX Ultra). The diffraction intensity (cps) was calculated by subtracting the base intensity from each peak intensity, and the diffraction intensity of the Si (111) plane (plane spacing d = 0.3135 nm) and the diffraction intensity of the Mg2Si (111) plane (plane spacing d = 0.3668 nm) were measured. The measurement results are shown in Tables 2 and 3.
[0108] (2) Corrosion resistance evaluation For each sample of hot-dip plated steel sheet and surface-treated steel sheet, after shearing to a size of 120 mm x 120 mm, a range of 10 mm from each edge of the evaluation target surface and the end face and non-evaluation target surface of the sample were sealed with tape to expose the evaluation target surface in a size of 100 mm x 100 mm, which was used as the evaluation sample. Three identical evaluation samples were prepared. Accelerated corrosion tests were carried out on the three evaluation samples prepared as described above, with the cycle shown in Figure 1. The accelerated corrosion tests were started from wetting and continued for 300 cycles, after which the corrosion weight loss of each sample was measured by the methods described in JIS Z 2383 and ISO 8407, and evaluated according to the following criteria. The evaluation results are shown in Tables 2 and 3. ◎: The corrosion loss of all three samples was 30 g / m 2 below ○: The corrosion loss of all three samples was 50 g / m 2 below ×: Corrosion loss of one or more samples is 50 g / m 2 Over
[0109] (3) White rust resistance For each sample of hot-dip plated steel sheet and surface-treated steel sheet, after shearing to a size of 120 mm x 120 mm, a range of 10 mm from each edge of the surface to be evaluated, as well as the end faces of the sample and the surfaces not to be evaluated, were sealed with tape to expose the surface to be evaluated in a size of 100 mm x 100 mm, and these were used as evaluation samples. The above evaluation samples were subjected to a salt spray test according to JIS Z 2371 for 90 hours and evaluated according to the following criteria. The evaluation results are shown in Tables 2 and 3. ◎: No white rust on the plate ○: White rust occurs on less than 10% of the flat surface area ×: White rust occurs on 10% or more of the flat plate area
[0110] (4) Surface appearance For each sample of hot-dip plated steel sheet, the surface of the plating film was visually observed. The observation results were evaluated according to the following criteria. The evaluation results are shown in Tables 2 and 3. ◎: No wrinkle defects were observed ○: Wrinkle defects were observed only within 50 mm from the edge ×: Wrinkle defects were observed outside the range of 50 mm from the edge.
[0111] (5) Processability Each hot-dip galvanized steel sheet sample was sheared to a size of 70 mm x 150 mm, and then eight sheets of the same thickness were sandwiched inside and bent 180° (8T bend). Cellophane tape (registered trademark) was firmly attached to the outer surface of the bent part after bending, and then peeled off. The surface condition of the plating film on the outer surface of the bent part and the presence or absence of adhesion (peeling) of the plating film on the surface of the tape used were visually observed, and the workability was evaluated according to the following criteria. The evaluation results are shown in Tables 2 and 3. ○: No cracks or peeling were observed in the plating film. △: There are cracks in the plating film, but no peeling is observed. ×: Both cracks and peeling were observed in the plating film.
[0112] (5) Bath stability During hot-dip plating, the state of the plating bath surface was visually inspected and compared with the plating bath surface (bath surface free of Mg-containing oxide) used in manufacturing hot-dip Al-Zn-plated steel sheets. Evaluation was performed according to the following criteria, and the evaluation results are shown in Tables 2 and 3. ◯: Similar to hot-dip Al-Zn plating bath (55% Al by mass, balance Zn-1.6% by mass bath) △: There is more white oxide than in the hot-dip Al-Zn plating bath (55% Al by mass, balance Zn-1.6% by mass bath). ×: Black oxide formation is observed in the plating bath.
[0113] [Table 2]
[0114] [Table 3]
[0115] The results in Tables 2 and 3 show that the samples of the present invention are excellent in terms of corrosion resistance, white rust resistance, surface appearance, workability, and bath stability in a well-balanced manner compared to the samples of the comparative examples. Moreover, it can be seen from the results in Table 3 that the samples subjected to the chemical conversion treatments A to D exhibited particularly excellent white rust resistance. [Industrial Applicability]
[0116] According to the present invention, it is possible to provide a surface-treated steel sheet having stably excellent corrosion resistance and white rust resistance, and a method for producing the same.
Claims
1. A surface-treated steel sheet comprising a plating film and a chemical conversion film formed on the plating film, The plating film has a composition containing 45 to 65 mass% Al, 1.0 to 4.0 mass% Si, and 1.0 to 10.0 mass% Mg, with the remainder being Zn and unavoidable impurities; The Co content in the unavoidable impurities is 0.080 mass% or less with respect to the total mass of the plating film, The Si and Mg in the plating film 2 The diffraction intensity of Si as determined by an X-ray diffraction method satisfies the following relationship (1): Si(111) / Mg 2 Si (111)≦0.8...(1) Si (111): Diffraction intensity of the Si (111) plane (plane spacing d = 0.3135 nm), Mg 2 Si(111):Mg 2 Diffraction intensity of Si (111) plane (plane spacing d = 0.3668 nm) The chemical conversion coating film is a surface-treated steel sheet characterized in that it contains at least one resin selected from the group consisting of epoxy resins, urethane resins, acrylic resins, acrylic silicone resins, alkyd resins, polyester resins, polyalkylene resins, amino resins, and fluororesins, and at least one metal compound selected from the group consisting of P compounds, Si compounds, Co compounds, Ni compounds, Zn compounds, Al compounds, Mg compounds, V compounds, Mo compounds, Zr compounds, Ti compounds, and Ca compounds.
2. 2. The surface-treated steel sheet according to claim 1, wherein a diffraction intensity of Si in the plating film, as determined by an X-ray diffraction method, satisfies the following relationship (2): Si (111)=0...(2) Si (111): Diffraction intensity of the Si (111) plane (plane spacing d = 0.3135 nm)
3. The surface-treated steel sheet according to claim 1 or 2, wherein the plating film further contains Sr: 0.01 to 1.0 mass %.
4. The surface-treated steel sheet according to any one of claims 1 to 3, characterized in that the Al content in the plating film is 50 to 60 mass%.
5. The surface-treated steel sheet according to any one of claims 1 to 4, characterized in that the Si content in the plating film is 1.0 to 3.0 mass%.
6. The surface-treated steel sheet according to any one of claims 1 to 5, characterized in that the Mg content in the plating film is 1.0 to 5.0 mass%.
7. A method for producing a surface-treated steel sheet having a plating film and a chemical conversion film formed on the plating film, comprising: The chemical conversion coating contains at least one resin selected from the group consisting of epoxy resins, urethane resins, acrylic resins, acrylic silicone resins, alkyd resins, polyester resins, polyalkylene resins, amino resins, and fluororesins, and at least one metal compound selected from the group consisting of P compounds, Si compounds, Co compounds, Ni compounds, Zn compounds, Al compounds, Mg compounds, V compounds, Mo compounds, Zr compounds, Ti compounds, and Ca compounds, The method for producing a surface-treated steel sheet includes a hot-dip galvanizing process for forming the plating film, in which a base steel sheet is immersed in a plating bath having a composition containing 45 to 65 mass% Al, 1.0 to 4.0 mass% Si, and 1.0 to 10.0 mass% Mg, with the remainder consisting of Zn and unavoidable impurities, and is characterized in that the diffraction intensity of Si and Mg2Si in the plating film by X-ray diffraction method satisfies the following relationship (1) by controlling the Co content in the unavoidable impurities of the plating bath to 0.080 mass% or less with respect to the total mass of the plating bath. Si (111) / Mg 2 Si (111)≦0.8 ... (1) Si (111): Diffraction intensity of the Si (111) plane (plane spacing d = 0.3135 nm), Mg 2 Si (111): Diffraction intensity of the (111) plane of Mg 2 Si (plane spacing d = 0.3668 nm)
8. The method for producing a surface-treated steel sheet according to claim 7, characterized in that the coating bath further contains 0.01 to 1.0 mass% Sr.
Citation Information
Patent Citations
Method for plating surface of steel with Al-Zn-Mg-Si alloy plating layer in continuous hot-dipping manner
CN105483594A
JP1975000039A
JP1975020228A
Electric fan
JP1982051093A
Access method of memory unit
JP1985055591A