Coated steel sheet and its manufacturing method
By controlling the composition and phase ratios of Al, Si, and Mg in the plating film, and using a specific chemical conversion film, the coated steel sheet achieves stable corrosion resistance and improved surface appearance, addressing the variability and defects in previous technologies.
Patent Information
- Application Number
- JP2022001320
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-01-06
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2042-01-06
AI Technical Summary
Existing hot-dip Al-Zn-Si-Mg coated steel sheets exhibit variations in corrosion resistance and surface appearance due to imbalances in the composition of the plating film, leading to uneven corrosion progression and surface defects, which are not adequately addressed by previous technologies.
The composition of the plating film is controlled to include specific ratios of Al, Si, Mg, and Co, with the Si and Mg phases managed through X-ray diffraction to stabilize corrosion resistance, and the addition of Sr to suppress surface defects, combined with a chemical conversion film containing specific resins and inorganic compounds to enhance adhesion and barrier properties.
The solution results in a coated steel sheet with consistently excellent corrosion resistance and improved surface appearance, maintaining integrity through various processing conditions and harsh environments.
Smart Images

Figure 0007564135000003 
Figure 0007564135000001 
Figure 0007564135000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a coated steel sheet having stably excellent corrosion resistance and corrosion resistance of processed parts, and a method for producing the same. [Background technology]
[0002] As a plated steel sheet used as a base for a painted steel sheet, there is a hot-dip Al-Zn plated steel sheet, typically a 55% Al-Zn plated steel sheet, which is known to have high corrosion resistance among hot-dip galvanized steel sheets, since it is possible to achieve both the sacrificial corrosion resistance of Zn and the high corrosion resistance of Al. Therefore, hot-dip Al-Zn plated steel sheets are mainly used in the field of building materials such as roofs and walls that are exposed outdoors for a long period of time, and in the field of civil engineering and construction such as guardrails, wiring and piping, and soundproof walls, due to their excellent corrosion resistance. In particular, there is an increasing demand for materials with excellent corrosion resistance and maintenance-free materials under more severe usage environments, such as acid rain caused by air pollution, spraying of deicing agents to prevent road freezing in snowy areas, and coastal area development, and the demand for hot-dip Al-Zn plated steel sheets has been increasing in recent years.
[0003] The coating of hot-dip Al-Zn coated steel sheets is composed of α-Al phases, which are areas where Al containing supersaturated Zn has solidified in the form of dendrites, and Zn-Al eutectic structures that exist in the gaps between dendrites (interdendritic structures), and is characterized by a structure in which the α-Al phases are layered in the thickness direction of the coating. This characteristic coating structure makes the corrosion progression path from the surface complex, making it difficult for corrosion to progress easily, and it is also known that hot-dip Al-Zn coated steel sheets can achieve superior corrosion resistance compared to hot-dip galvanized steel sheets with the same coating thickness.
[0004] Attempts have been made to further extend the life of such hot-dip Al-Zn coated steel sheets, and hot-dip Al-Zn-Si-Mg coated steel sheets to which Mg has been added have been put to practical use. As such a hot-dip Al-Zn-Si-Mg-plated steel sheet, for example, Patent Document 1 discloses a hot-dip Al-Zn-Si-Mg-plated steel sheet that contains an Al-Zn-Si alloy containing Mg in a plating film, the Al-Zn-Si alloy being an alloy containing 45 to 60 wt % of elemental aluminum, 37 to 46 wt % of elemental zinc, and 1.2 to 2.3 wt % of Si, and the concentration of the Mg is 1 to 5 wt %. Furthermore, Patent Document 2 discloses a hot-dip Al-Zn-Si-Mg plated steel sheet in which the plating film contains one or more of 2-10% Mg and 0.01-10% Ca to improve corrosion resistance and to enhance protective action after the base steel sheet is exposed. Furthermore, Patent Document 3 discloses a hot-dip Al-Zn-Si-Mg plated steel sheet in which a coating layer is formed containing, by mass%, 1-15% Mg, 2-15% Si, 11-25% Zn, with the balance being Al and unavoidable impurities, and the size of intermetallic compounds such as Mg2Si phase and MgZn2 phase present in the plating film is set to 10 μm or less, thereby improving the corrosion resistance of the flat plate and end faces.
[0005] The above-mentioned hot-dip Al-Zn coated steel sheet has a beautiful appearance with a spangle pattern of white metallic luster, and therefore is often used without painting, and there are strong demands for its appearance. Therefore, technologies to improve the appearance of hot-dip Al-Zn coated steel sheet have been developed. For example, Patent Document 4 discloses a hot-dip Al-Zn-Si-Mg plated steel sheet in which wrinkle-like irregular defects are suppressed by including 0.01 to 10% of Sr in the plated film. Patent Document 5 also discloses a hot-dip Al-Zn-Si-Mg plated steel sheet in which mottling defects are suppressed by including 500 to 3000 ppm of Sr in the plated film.
[0006] In addition, coated steel sheets having a chemical conversion coating, a primer coating, a top coating, etc. formed on the surface of the hot-dip Al-Zn-plated steel sheet are subjected to various processes such as 90-degree bending or 180-degree bending by press forming, roll forming, or embossing, and furthermore, long-term coating durability performance is required. In order to meet these requirements, coated steel sheets are known in which a chemical conversion coating containing chromate is formed on the hot-dip Al-Zn-plated steel sheet, a primer coating containing a chromate-based rust-preventive pigment is also formed on the primer coating, and a top coating having excellent weather resistance such as a thermosetting polyester resin coating or a fluorine-based resin coating is formed thereon. However, in recent years, the use of chromate, an environmentally hazardous substance, has come to be seen as problematic in such coated steel sheets, and there is a strong demand for the development of coated steel sheets that are chromate-free but can still have improved corrosion resistance and surface appearance. As a technique for satisfying these demands, for example, Patent Document 6 discloses a surface-treated hot-dip plated steel material in which an aluminum-zinc alloy plating layer (α) containing Al, Zn, Si and Mg with the contents of these elements adjusted is plated on the surface of a steel material, and a coating (β) containing at least one compound (A) selected from titanium compounds and zirconium compounds as a film-forming component is further formed as an upper layer thereon, in which the mass ratio of the Si-Mg phase in the aluminum-zinc alloy plating layer (α) to the total amount of Mg in the plating layer is adjusted to 3% or more. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] Patent No. 5020228 [Patent Document 2] Patent No. 5000039 [Patent Document 3] JP 2002-12959 A [Patent Document 4] Patent No. 3983932 [Patent Document 5] Special Publication No. 2011-514934 [Patent Document 6] JP 2005-169765 A Summary of the Invention [Problem to be solved by the invention]
[0008] However, the techniques disclosed in Patent Documents 1 to 3 for incorporating Mg into a plating film do not necessarily uniquely improve corrosion resistance. In the hot-dip Al-Zn-Si-Mg-plated steel sheets disclosed in Patent Documents 1 to 3, the corrosion resistance is improved only by including Mg in the plating components, but the effects of components other than the above four elements (Al, Zn, Si, Mg) and the characteristics of the metal phase and intermetallic compound phase that constitute the plating film are not taken into consideration, and it is not possible to uniformly discuss the superiority or inferiority of the corrosion resistance. Therefore, even when hot-dip Al-Zn-Si-Mg-plated steel sheets are manufactured using a plating bath composition with the same content of the above four element components, there is a problem that the corrosion resistance varies when an accelerated corrosion test is performed and the steel sheets are not necessarily superior to Al-Zn-plated steel sheets without added Mg. Similarly, in improving the appearance of the plating, wrinkle-like irregular defects cannot necessarily be eliminated by merely adding Sr to the plating film, and there have been cases where both corrosion resistance and appearance have not been achieved in the hot-dip Al-Zn-Si-Mg-plated steel sheets disclosed in Patent Documents 4 and 5. In addition, since Mg is an element that is easily oxidized, Mg contained in the plating bath may generate oxides (top dross) near the bath surface, and in the case of hot-dip plating, FeAl-based compounds (bottom dross) containing iron that are unevenly distributed in the bath or at the bottom of the plating bath over time may be generated, and these dross may adhere to the surface of the plating film, causing convex defects and impairing the appearance of the plating film surface. It is also known that when a steel sheet is plated in a molten Al-Zn-Si bath containing Mg, the Mg2Si phase, MgZn2 phase, and Si phase precipitate in addition to the α-Al phase in the plated film. However, the effect of the amount and abundance ratio of each phase on corrosion resistance has not been clarified.
[0009] Furthermore, as described above, coated steel sheets are required to have long-term coating film durability when subjected to various processes such as 90-degree bending or 180-degree bending by press forming, roll forming, embossing, etc., but the technology of Patent Document 6 does not necessarily provide stable corrosion resistance and surface appearance after processing. It goes without saying that the corrosion resistance of a coated steel sheet is affected by the corrosion resistance of the underlying plated steel sheet, and as for the surface appearance, the unevenness of wrinkle defects can vary by several tens of μm, so even if the surface is smoothed by a coating, the unevenness cannot be completely eliminated, and it is thought that an improvement in the appearance of the coated steel sheet cannot be expected. Furthermore, since the coating film is thinner at the convex parts, there is a concern that the corrosion resistance may decrease locally. Therefore, in order to obtain a coated steel sheet with excellent corrosion resistance and surface appearance, it is important to improve the corrosion resistance and surface appearance of the underlying plated steel sheet.
[0010] In view of the above circumstances, an object of the present invention is to provide a coated steel sheet having stably excellent corrosion resistance and corrosion resistance of processed parts, and a method for producing the same. [Means for solving the problem]
[0011] As a result of investigations aimed at solving the above-mentioned problems, the present inventors have noticed that it is important not only to control the concentrations of Al, Zn, Si, and Mg when it comes to the composition of the plating film of a coated steel sheet, but also to control the concentrations of elements contained as impurities. In particular, they have found that deterioration of corrosion resistance can be effectively suppressed by appropriately controlling the Co content. In addition, it was found that the amount of precipitation of the Mg2Si and Si phases formed in the plating film increases or decreases depending on the balance of each component in the plating film and the plating film formation conditions, and that the ratio of their abundance changes, and that some phases may not precipitate depending on the balance of the compositions, and that the corrosion resistance of the coated steel sheet changes depending on the ratio of these phases, and that the corrosion resistance is stably improved especially when the Si phase is less than the Mg2Si and Si phases. However, it is known that it is very difficult to distinguish the difference between the Mg2Si and Si phases even by observing the plating film from the surface or cross section using a general method, such as a scanning electron microscope, using secondary electron images or backscattered electron images, and although it is possible to obtain microscopic information by observing using a transmission electron microscope, it was not possible to grasp the ratio of the Mg2Si and Si phases, which determines macroscopic information such as corrosion resistance and appearance.
[0012] Therefore, the inventors conducted further intensive research and as a result, they focused on X-ray diffraction method and discovered that by utilizing the intensity ratio of specific diffraction peaks of the Mg2Si phase and the Si phase, it is possible to quantitatively define the abundance ratio of the phases, and further discovered that when the Mg2Si phase and the Si phase satisfy a specific abundance ratio in the plating film, stable and excellent corrosion resistance can be achieved. In addition, the present inventors have found that by controlling the Co content and the abundance ratio of the MgSi phase and the Si phase in the plating film described above, and then controlling the Sr concentration in the plating bath, it is possible to reliably suppress the occurrence of wrinkle-like uneven defects and obtain a plated steel sheet with excellent surface appearance.
[0013] Furthermore, the inventors also investigated the chemical conversion coating and primer coating formed on the plating coating, and found that by forming the chemical conversion coating from a specific resin and a specific inorganic compound, and forming the primer coating from a specific polyester resin and an inorganic compound, the barrier properties and adhesion of the coating can be improved, and excellent post-processing corrosion resistance can be achieved even in a chromate-free system.
[0014] The present invention has been made based on the above findings, and the gist of the present invention is as follows. 1. A coated steel sheet in which a coating film is formed directly or via a chemical conversion coating on a plating film, The plating film has a composition containing 45 to 65 mass% Al, 1.0 to 4.0 mass% Si, and 1.0 to 10.0 mass% Mg, with the remainder being Zn and unavoidable impurities; the Co content in the unavoidable impurities is 0.080 mass% or less with respect to the total mass of the plating film, and the diffraction intensities of Si and MgSi in the plating film, as determined by an X-ray diffraction method, satisfy the following relationship (1), Si (111) / Mg2Si (111)≦0.8 ···(1) Si (111): Diffraction intensity of the Si (111) plane (plane spacing d = 0.3135 nm), Mg2Si (111): Diffraction intensity of the (111) plane of Mg2Si (plane spacing d = 0.3668 nm) The chemical conversion coating contains a resin component that contains 30 to 50 mass% in total of (a): an anionic polyurethane resin having an ester bond and (b): an epoxy resin having a bisphenol skeleton, the content ratio of (a) to (b) ((a):(b)) being in the range of 3:97 to 60:40 in terms of mass ratio, and an inorganic compound that contains 2 to 10 mass% of a vanadium compound, 40 to 60 mass% of a zirconium compound, and 0.5 to 5 mass% of a fluorine compound; The coating film has at least a primer coating film, and the primer coating film contains a polyester resin having a urethane bond, and an inorganic compound including a vanadium compound, a phosphate compound, and magnesium oxide.
[0015] 2. The coated steel sheet according to item 1 above, wherein the diffraction intensity of Si in the plating film as determined by an X-ray diffraction method satisfies the following relationship (2): Si(111)=0 (2) Si (111): Diffraction intensity of the Si (111) plane (plane spacing d = 0.3135 nm)
[0016] 3. The coated steel sheet according to 1 or 2 above, wherein the plating film further contains 0.01 to 1.0 mass % of Sr.
[0017] 4. The coated steel sheet according to any one of 1 to 3 above, wherein the Al content in the plating film is 50 to 60 mass %.
[0018] 5. The coated steel sheet according to any one of 1 to 4 above, wherein the Si content in the plating film is 1.0 to 3.0 mass %.
[0019] 6. The coated steel sheet according to any one of 1 to 5 above, wherein the Mg content in the plating film is 1.0 to 5.0 mass %.
[0020] 7. A method for producing a coated steel sheet in which a coating film is formed on a plating film directly or via a chemical conversion coating, comprising the steps of: The chemical conversion coating contains a resin component that contains 30 to 50 mass% in total of (a): an anionic polyurethane resin having an ester bond and (b): an epoxy resin having a bisphenol skeleton, the content ratio of (a) to (b) ((a):(b)) being in the range of 3:97 to 60:40 in terms of mass ratio, and an inorganic compound that contains 2 to 10 mass% of a vanadium compound, 40 to 60 mass% of a zirconium compound, and 0.5 to 5 mass% of a fluorine compound; The coating film has at least a primer coating film, and the primer coating film contains a polyester resin having a urethane bond, and an inorganic compound containing a vanadium compound, a phosphoric acid compound, and magnesium oxide, The method for producing a coated steel sheet includes a hot-dip galvanizing process for forming the plating film, in which a base steel sheet is immersed in a plating bath having a composition containing 45-65 mass% Al, 1.0-4.0 mass% Si, and 1.0-10.0 mass% Mg, with the balance being Zn and unavoidable impurities, and is characterized in that the Co content in the unavoidable impurities of the plating bath is controlled to 0.080 mass% or less with respect to the total mass of the plating bath. 8. The method for producing a coated steel sheet as described in 7 above, wherein the coating bath further contains 0.01 to 1.0 mass % of Sr. Effect of the Invention
[0021] According to the present invention, it is possible to provide a coated steel sheet having stably excellent corrosion resistance and corrosion resistance of processed parts, and a method for producing the same. [Brief description of the drawings]
[0022] [Figure 1] FIG. 1 is a diagram for explaining the flow of the Japanese Automotive Standard Combined Cycle Test (JASO-CCT). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0023] <Coated steel sheet> The coated steel sheet of the present invention is a coated steel sheet in which a coating film is formed on a plating film directly or via a chemical conversion film.
[0024] (Plating film) In the coated steel sheet of the present invention, the plating film has a composition containing 45 to 65 mass % Al, 1.0 to 4.0 mass % Si, 1.0 to 10.0 mass % Mg, with the balance being Zn and unavoidable impurities.
[0025] The Al content in the plating film is 45 to 65 mass%, preferably 50 to 60 mass%, in consideration of the balance between corrosion resistance and operation. This is because, if the Al content in the plating film is at least 45 mass%, dendritic solidification of Al occurs, and a plating film structure mainly composed of a dendritic solidification structure of the α-Al phase can be obtained. The dendritic solidification structure has a structure in which it is laminated in the thickness direction of the plating film, so that the corrosion progression path becomes complex, and the corrosion resistance of the plating film itself is improved. In addition, the more the α-Al phase dendrite parts are laminated, the more complex the corrosion progression path becomes, and it becomes difficult for corrosion to reach the base steel sheet, so that the corrosion resistance is improved, and therefore the Al content is preferably 50 mass% or more. On the other hand, if the Al content in the plating film exceeds 65 mass%, most of the Zn changes to a structure in which it is solid-solved in α-Al, and the dissolution reaction of the α-Al phase cannot be suppressed, and the corrosion resistance of the Al-Zn-Si-Mg-based plating is deteriorated. For this reason, the Al content in the plating film must be 65 mass % or less, and is preferably 60 mass % or less.
[0026] The Si in the plating film is added mainly for the purpose of suppressing the growth of the Fe-Al and / or Fe-Al-Si interfacial alloy layer formed at the interface with the base steel sheet and preventing the deterioration of the adhesion between the plating film and the steel sheet. In fact, when a steel sheet is immersed in an Al-Zn plating bath containing Si, Fe on the steel sheet surface reacts with Al and Si in the bath to form an Fe-Al and / or Fe-Al-Si intermetallic compound layer at the interface between the base steel sheet and the plating film. At this time, since the growth rate of the Fe-Al-Si alloy is slower than that of the Fe-Al alloy, the higher the ratio of the Fe-Al-Si alloy, the more the growth of the entire interfacial alloy layer is suppressed. Therefore, the Si content in the plating film must be 1.0 mass% or more. On the other hand, if the Si content in the plating film exceeds 4.0 mass%, not only is the effect of suppressing the growth of the interfacial alloy layer saturated, but the presence of an excess Si phase in the plating film promotes corrosion, so the Si content is set to 4.0 mass% or less. Furthermore, the Si content in the plating film is preferably 3.0 mass% or less from the viewpoint of suppressing the presence of an excessive Si phase. In addition, the Si content is preferably 1.0 to 3.0 mass% from the viewpoint of easily satisfying the relational expression (1) described later in relation to the Mg content described later.
[0027] The plating film contains 1.0 to 10.0 mass % of Mg. By including Mg in the plating film, the above-mentioned Si can be present in the form of an intermetallic compound of Mg2Si phase, and the promotion of corrosion can be suppressed. Furthermore, when Mg is contained in the plating film, an intermetallic compound, MgZn2 phase, is also formed in the plating film, and the effect of further improving corrosion resistance is obtained. When the Mg content in the plating film is less than 1.0 mass%, Mg is used for solid solution in the α-Al phase, which is the main phase, rather than for the formation of the intermetallic compounds (Mg2Si, MgZn2), and sufficient corrosion resistance cannot be ensured. On the other hand, when the Mg content in the plating film is high, the effect of improving corrosion resistance is saturated, and in addition, the α-Al phase becomes brittle, resulting in a decrease in workability, so the content is set to 10.0 mass% or less. Furthermore, the Mg content in the plating film is preferably set to 5.0 mass% or less from the viewpoints of suppressing the generation of dross during plating formation and facilitating plating bath management. In addition, from the viewpoint of easily satisfying the relational expression (1) described later in relation to the Si content, the Mg content is preferably 3.0 mass%, and in consideration of compatibility with dross suppression, the Mg content is more preferably 3.0 to 5.0 mass%.
[0028] The plating film contains Zn and unavoidable impurities. Among these, the unavoidable impurities contain Fe. This Fe is inevitably contained in the plating film as a result of dissolution of the steel sheet or bath-immersed equipment into the plating bath, and as a result of being supplied by diffusion from the base steel sheet during the formation of the interface alloy layer. The Fe content in the plating film is usually about 0.3 to 2.0 mass%. Other unavoidable impurities include Cr, Ni, Cu, Co, W, etc. These elements are inevitably contained in the plating film due to the fact that they are dissolved in the plating bath from the WC-based or Co-Cr-W-based thermal spray coating applied to the base steel sheet or the bath-immersing equipment made of stainless steel, that they are contained as impurities in the metal ingots that are the raw materials for the plating bath, and that they are produced using pots or bath-immersing equipment that were used in the production of plated steel sheets to which these elements were intentionally added.
[0029] The coated steel sheet of the present invention is characterized in that the Co content in the unavoidable impurities is 0.080 mass% or less with respect to the total mass of the plating film. Since Co contained in the plating film may deteriorate the corrosion resistance of the coated steel sheet, the deterioration of the corrosion resistance can be suppressed by appropriately controlling the contents of Al, Zn, Si and Mg in the plating film described above and further reducing the Co content as an unavoidable impurity. From the same viewpoint, the Co content in the unavoidable impurities is preferably 0.020 mass% or less with respect to the total mass of the plating film, more preferably 0.001 mass% or less, and most preferably 0 mass%.
[0030] Co contained in the plating film is mainly present as a solid solution element in α-Al. When Co is contained in a concentration exceeding the solid solubility limit, it may precipitate as Fe-Co-Al compounds or Fe-Co-Al-Si compounds in the alloy layer formed at the base steel / plating interface. In addition, although the mechanism by which the corrosion resistance deteriorates due to the inclusion of Co as an impurity is uncertain, it is hypothesized that the corrosion rate increases due to a decrease in the barrier properties of the α-Al phase in which Co is dissolved, and that the corrosion rate increases due to Co-containing compounds functioning as a cathode in a corrosive environment and forming a local battery with the surrounding solidified structure.
[0031] Furthermore, the total content of unavoidable impurities in the plating film is not particularly limited, but if contained in excess, it may affect various properties of the plated steel sheet, so it is preferable that the total content be 5.0 mass% or less.
[0032] In addition, in the coated steel sheet of the present invention, the diffraction intensities of Si and Mg2Si in the plating film, as determined by an X-ray diffraction method, are required to satisfy the following relationship (1): Si (111) / Mg2Si (111)≦0.8 ···(1) Si (111): Diffraction intensity of the Si (111) plane (interplanar spacing d = 0.3135 nm), Mg2Si (111): Diffraction intensity of the Mg2Si (111) plane (interplanar spacing d = 0.3668 nm)
[0033] As described above, in the present invention, it is important to control the ratio of the Mg2Si phase and the Si phase that are generated in the plating film due to the inclusion of Mg and Si to a specific ratio. Although the effects of these on corrosion resistance are still under investigation and many points remain unclear, the following mechanism is assumed.
[0034] When a coated steel sheet is exposed to a corrosive environment, the above-mentioned intermetallic compounds dissolve preferentially over the α-Al phase, resulting in a Mg-rich environment in the vicinity of the formed corrosion products. It is presumed that in such a Mg-rich environment, the formed corrosion products are less likely to decompose, and as a result, the protective effect of the plating film is enhanced. In addition, the protective effect of the plating film is more reliably expressed when the Si in the plating film exists as the Mg2Si phase rather than the Si phase, so it is considered effective to reduce the ratio of the Si phase to the Mg2Si phase.
[0035] The abundance ratio of Si and Mg2Si in the plating film is required to satisfy the relationship (1): Si (111) / Mg2Si (111)≦0.8 using the diffraction peak intensity obtained by X-ray diffraction. However, if the abundance ratio of Si and Mg2Si in the plating film does not satisfy the relationship (1), that is, Si (111) / Mg2Si (111)>0.8, the Si phase present in the plating film increases, and the above-mentioned Mg-rich environment cannot be obtained in the vicinity of the corrosion product, making it difficult to obtain the protective effect of the plating film. From the same viewpoint, the abundance ratio of Si to Mg2Si (Si (111) / Mg2Si (111)) is preferably 0.5 or less, more preferably 0.3 or less, and particularly preferably 0.2 or less.
[0036] Here, in the above relationship (1), Si (111) is the diffraction intensity of the Si (111) plane (planar spacing d=0.3135 nm), and Mg2Si (111) is the diffraction intensity of the Mg2Si (111) plane (planar spacing d=0.3668 nm). The method for measuring Si(111) and Mg2Si(111) by X-ray diffraction involves mechanically scraping off a portion of the plating film, powdering it, and performing X-ray diffraction on the powdered state (powder X-ray diffraction measurement method). The diffraction intensity is measured by measuring the diffraction peak intensity of Si corresponding to the interplanar spacing d=0.3135 nm and the diffraction peak intensity of Mg2Si corresponding to the interplanar spacing d=0.3668 nm, and calculating the ratio between these to obtain Si(111) / Mg2Si(111). The amount of the plating film required for carrying out the powder X-ray diffraction measurement (amount of the plating film to be scraped off) is 0.1 g or more, preferably 0.3 g or more, from the viewpoint of accurately measuring Si(111) and Mg2Si(111). When the plating film is scraped off, steel sheet components other than the plating film may be contained in the powder, but these intermetallic compound phases are contained only in the plating film and do not affect the above-mentioned peak intensity. Furthermore, the plating film is powdered and X-ray diffraction is carried out because, when X-ray diffraction is carried out on the plating film formed on the plated steel sheet, it is affected by the plane orientation of the plating film solidification structure, making it difficult to calculate the correct phase ratio.
[0037] In addition, in the coated steel sheet of the present invention, since the concentrations of Al, Zn, Si, Mg, and Co as an unavoidable impurity described above can be controlled and corrosion resistance can be more stably improved, it is preferable that the diffraction intensity of Si in the plating film, as determined by an X-ray diffraction method, satisfies the following relationship (2): Si(111)=0 (2) Si (111): Diffraction intensity of the Si (111) plane (planar spacing d=0.3135 nm) In general, it is known that in the dissolution reaction of an Al alloy in an aqueous solution, the presence of a Si phase as a cathode site promotes the dissolution of the surrounding α-Al phase. Therefore, reducing the amount of Si phase is also effective in terms of suppressing the dissolution of the α-Al phase. Among these, a coating in which no Si phase exists, as shown in relationship (2) (the diffraction peak intensity of the Si(111) is set to zero) is the most excellent in terms of stabilizing corrosion resistance. The method for measuring the diffraction peak intensity of the Si (111) plane by X-ray diffraction is as described above.
[0038] Here, the method for satisfying the above-mentioned relationship (1) or relationship (2) is not particularly limited. For example, in order to satisfy the relationship (1) or relationship (2), the abundance ratio of Si and Mg2Si (diffraction intensity of Si(111) and Mg2Si(111)) can be controlled by adjusting the balance of the Si content, Mg content, and Al content in the plating film. The balance of the Si content, Mg content, and Al content in the plating film does not necessarily satisfy the relationship (1) or relationship (2) by setting the content ratio of Si, Mg content, and Al to a constant content ratio, and it is necessary to change the content ratio of Mg and Al depending on the Si content (mass%), for example. In addition to adjusting the balance of the Si content, the Mg content, and the Al content in the plating film, the diffraction intensities of Si(111) and MgSi(111) can be controlled so as to satisfy the relationship (1) or (2) by adjusting the conditions for forming the plating film (e.g., the cooling conditions after plating).
[0039] In the coated steel sheet of the present invention, the plating film preferably contains 0.01 to 1.0 mass % of Sr. When the plating film contains Sr, the occurrence of surface defects such as wrinkle-like irregularities can be more reliably suppressed, and good surface appearance can be achieved. The wrinkle-like defect is a wrinkle-like uneven defect formed on the surface of the plating film, and is observed as a whitish streak on the surface of the plating film. Such wrinkle-like defects are likely to occur when a large amount of Mg is added to the plating film. Therefore, in the hot-dip plated steel sheet, by adding Sr to the plating film, Sr is oxidized preferentially over Mg in the surface layer of the plating film, and the oxidation reaction of Mg is suppressed, thereby making it possible to suppress the occurrence of the wrinkle-like defect.
[0040] In addition, since the plating film can improve the stability of corrosion products and retard the progress of corrosion like Mg, it is preferable that the plating film further contains one or more selected from Cr, Mn, V, Mo, Ti, Ca, Sb, and B in a total amount of 0.01 to 10 mass%. The reason why the total content of the above-mentioned components is set to 0.01 to 10 mass% is that a sufficient corrosion retardation effect can be obtained and the effect does not saturate.
[0041] From the viewpoint of satisfying various characteristics, the coating weight of the plating film is set to 45 to 120 g / m2 per side. 2 It is preferable that the coating weight of the plating film is 45 g / m 2 In the above cases, sufficient corrosion resistance is obtained for applications requiring long-term corrosion resistance, such as building materials, and the coating weight of the plating film is 120 g / m 2 This is because, in the following cases, it is possible to realize excellent corrosion resistance while suppressing the occurrence of plating cracks during processing. From the same viewpoint, the coating weight of the plating film is 45 to 100 g / m 2 It is more preferable that:
[0042] The coating weight of the plating film can be derived, for example, by a method in which a specific area of the plating film is dissolved and peeled off with a mixed solution of hydrochloric acid and hexamethylenetetramine as specified in JIS H 0401: 2013, and the coating weight is calculated from the difference in the weight of the steel sheet before and after peeling. To determine the coating weight per side using this method, the plating surface of the non-target side is sealed with tape so as not to be exposed, and then the above-mentioned dissolution is carried out.
[0043] The composition of the plating film can be confirmed, for example, by immersing the plating film in hydrochloric acid or the like to dissolve it, and subjecting the solution to ICP emission spectrometry, atomic absorption spectrometry, etc. This method is merely one example, and any method that can accurately quantify the composition of the plating film may be used, and is not particularly limited.
[0044] The plating film on the coated steel sheet obtained according to the present invention has a composition substantially equivalent to that of the plating bath as a whole, and therefore the composition of the plating film can be controlled with high precision by controlling the composition of the plating bath.
[0045] Furthermore, the base steel sheet constituting the coated steel sheet of the present invention is not particularly limited, and cold-rolled steel sheet, hot-rolled steel sheet, etc. can be used as appropriate depending on the required performance and specifications.
[0046] Furthermore, the method for obtaining the base steel sheet is not particularly limited. For example, in the case of the hot-rolled steel sheet, one that has been subjected to a hot rolling process and a pickling process can be used, and in the case of the cold-rolled steel sheet, it can be manufactured by further adding a cold rolling process. Furthermore, in order to obtain the properties of the steel sheet, it is also possible to pass through a recrystallization annealing process or the like before the hot-dip plating process.
[0047] The conditions for forming the plating film when producing the coated steel sheet of the present invention are not particularly limited to a hot-dip galvanizing process in which the base steel sheet is immersed in a plating bath. The hot-dip galvanizing process can be carried out, for example, by cleaning, heating, and immersing the base steel sheet in a plating bath in a continuous hot-dip galvanizing facility. In the heating process of the steel sheet, recrystallization annealing or the like is carried out to control the structure of the base steel sheet itself, and heating in a reducing atmosphere such as a nitrogen-hydrogen atmosphere is effective in preventing oxidation of the steel sheet and reducing a small amount of oxide film present on the surface.
[0048] As for the plating bath used in the hot-dip plating process, as described above, the composition of the plating film as a whole is approximately the same as the composition of the plating bath, and therefore a plating bath having a composition containing 45 to 65 mass% Al, 1.0 to 4.0 mass% Si, and 1.0 to 10.0 mass% Mg, with the balance being Zn and unavoidable impurities, can be used.
[0049] In the hot-dip coating process, the Co content in the inevitable impurities of the coating bath needs to be controlled to 0.080 mass% or less with respect to the total mass of the coating bath. Since the Co contained in the coating film may deteriorate the corrosion resistance of the coated steel sheet as described above, the Al, Zn, Si, and Mg contents in the coating bath are appropriately controlled, and the Co content as an inevitable impurity is further reduced, whereby deterioration of the corrosion resistance can be suppressed. Furthermore, the content of Co as an unavoidable impurity in the coating bath needs to be controlled to 0.080 mass% or less, more preferably 0.020 mass% or less, and even more preferably 0.001 mass% or less, based on the total mass of the coating bath. If the Co content in the coating bath is 0.080 mass% or less, the produced coated steel sheet can have sufficiently excellent corrosion resistance, but if it is 0.020 mass% or less, it can have even better corrosion resistance, and if it is 0.001 mass% or less, it can have particularly excellent corrosion resistance. Thus, since the lower the Co content in the coating bath, the better the corrosion resistance of the coated steel sheet. There is no particular lower limit for the Co content, and it is most preferable that the Co content in the coating bath is 0%.
[0050] Here, the means for reducing the Co content in the plating bath is not particularly limited. For example, since it is effective to prevent the elution of a Co-Cr-W based thermal spray coating applied to a bath-immersed device into the plating bath, it is preferable to use a thermal spray coating that does not contain Co.
[0051] As another means for reducing the Co content in the plating bath, it is preferable to use a metal block having a low Co content among impurities as a raw material for the plating bath. Furthermore, it is also effective not to use pots or bath-immersed equipment used in the production of plated steel sheets to which Co is intentionally added in the production of coated steel sheets, since this can prevent metal lumps containing Co adhering to the pots or bath-immersed equipment from dissolving and being mixed into the plating bath.
[0052] Furthermore, the bath temperature of the plating bath is not particularly limited, but is preferably in the range of (melting point + 20°C) to 650°C. The reason why the lower limit of the bath temperature is set to the melting point + 20°C is that the bath temperature needs to be at or above the solidification point in order to perform hot-dip plating, and setting the temperature at the melting point + 20°C prevents solidification due to a local drop in the bath temperature of the plating bath. On the other hand, the reason why the upper limit of the bath temperature is set to 650°C is that if the bath temperature exceeds 650°C, it becomes difficult to rapidly cool the plating film, and there is a risk that the interfacial alloy layer formed between the plating film and the steel sheet will become thick.
[0053] In addition, the temperature of the base steel sheet immersed in the coating bath (immersion sheet temperature) is not particularly limited, but from the viewpoint of ensuring the coating characteristics in continuous hot-dip coating operations and preventing changes in the bath temperature, it is preferable to control it to within ±20°C of the coating bath temperature.
[0054] Furthermore, the immersion time of the steel sheet in the plating bath is 0.5 seconds or more. This is because if it is less than 0.5 seconds, there is a risk that a sufficient plating film may not be formed on the surface of the base steel sheet. There is no particular upper limit to the immersion time, but since a longer immersion time may cause the interfacial alloy layer formed between the plating film and the steel sheet to become thick, it is preferable to set it to 8 seconds or less.
[0055] (Conversion coating) The coated steel sheet of the present invention can have a chemical conversion coating formed on the above-mentioned plating coating. The chemical conversion coating may be formed on at least one side of the coated steel sheet, and may also be formed on both sides of the coated steel sheet depending on the application and required performance.
[0056] The coated steel sheet of the present invention is characterized in that the chemical conversion coating contains a resin component that contains 30 to 50 mass% in total of (a): an anionic polyurethane resin having an ester bond and (b): an epoxy resin having a bisphenol skeleton, the content ratio of (a):(b) being within a range of 3:97 to 60:40 in terms of mass ratio, and inorganic compounds that include 2 to 10 mass% of a vanadium compound, 40 to 60 mass% of a zirconium compound, and 0.5 to 5 mass% of a fluorine compound. By forming the above-mentioned chemical conversion film on the plating film, it is possible to increase the strength and adhesion of the chemical conversion film while improving the corrosion resistance.
[0057] Here, the resin components constituting the chemical conversion coating include (a): an anionic polyurethane resin having an ester bond and (b): an epoxy resin having a bisphenol skeleton.
[0058] The (a) anionic polyurethane resin having an ester bond may be a resin obtained by copolymerizing a reaction product of a polyester polyol with a diisocyanate or polyisocyanate having two or more isocyanate groups with a dimethylol alkyl acid. A chemical conversion treatment liquid can be obtained by dispersing the reaction product in a liquid such as water by a known method.
[0059] Examples of the polyester polyol include polyesters obtained by a dehydration condensation reaction between a glycol component and an acid component such as an ester-forming derivative of a hydroxyl carboxylic acid, polyesters obtained by a ring-opening polymerization reaction of a cyclic ester compound such as ε-caprolactone, and copolymer polyesters thereof. Examples of the polyisocyanate include aromatic polyisocyanates, aliphatic polyisocyanates, and alicyclic polyisocyanates. Examples of the aromatic polyisocyanate include 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, m-xylylene diisocyanate, diphenylmethane diisocyanate, 2,4-diphenylmethane diisocyanate, 2,2-diphenylmethane diisocyanate, triphenylmethane triisocyanate, polymethylene polyphenyl polyisocyanate, naphthalene diisocyanate, and derivatives thereof (e.g., prepolymers obtained by reaction with polyols, modified polyisocyanates such as carbodiimide compounds of diphenylmethane diisocyanate, etc.).
[0060] When the polyester polyol is reacted with the diisocyanate or polyisocyanate to synthesize urethane, the anionic polyurethane resin having the ester bond (a) can be obtained by, for example, copolymerizing a dimethylol alkyl acid and self-emulsifying it to be water-soluble (water-dispersed). In this case, examples of the dimethylol alkyl acid include dimethylol alkyl acids having 2 to 6 carbon atoms, more specifically, dimethylol ethanoic acid, dimethylol propanoic acid, dimethylol butanoic acid, dimethylol heptanoic acid, and dimethylol hexanoic acid.
[0061] In addition, the epoxy resin having a bisphenol skeleton (b) may be a known epoxy resin. Examples include bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol AD type epoxy resin, and bisphenol S type epoxy resin. These epoxy resins can be obtained by reacting a bisphenol compound such as bisphenol A, bisphenol F, bisphenol AD, or bisphenol S with epichlorohydrin in the presence of an alkali catalyst. Among them, component [A] preferably contains a bisphenol A type epoxy resin or a bisphenol F type epoxy resin, and more preferably contains a bisphenol A type epoxy resin. The epoxy resin having a bisphenol skeleton (b) can be dispersed in a liquid such as water by a known method to obtain a chemical conversion treatment liquid.
[0062] The resin component acts as a binder for the chemical conversion coating, and the (a) anionic polyurethane resin having ester bonds that constitutes the binder is flexible and therefore has the effect of making the chemical conversion coating less likely to be destroyed (peeled off) when processed, and the (b) epoxy resin having a bisphenol skeleton has the effect of improving adhesion to the underlying zinc-based plated steel sheet and the upper primer coating film. The resin components are contained in the chemical conversion coating in a total amount of 30 to 50% by mass. If the content of the resin components is less than 30% by mass, the binder effect of the chemical conversion coating is reduced, and if it exceeds 50% by mass, the functions of the inorganic components described below, such as the inhibitor action, are reduced. From the same viewpoint, the content of the resin components in the chemical conversion coating is preferably 35 to 45% by mass.
[0063] Furthermore, the resin component must have a content ratio ((a):(b)) of the (a) anionic polyurethane resin having an ester bond and the (b) epoxy resin having a bisphenol skeleton in the range of 3:97 to 60:40 by mass. If the (a):(b) is outside the above range, the flexibility and adhesion of the chemical conversion coating film will decrease, and sufficient corrosion resistance will not be obtained. From the same viewpoint, the (a):(b) is preferably 10:90 to 55:45.
[0064] The resin component may contain resins (other resin components) other than the above-mentioned (a) anionic polyurethane resin having an ester bond and (b) epoxy resin having a bisphenol skeleton, depending on the required performance. The other resin components are not particularly limited, and may be, for example, at least one selected from acrylic resin, acrylic silicone resin, alkyd resin, polyester resin, polyalkylene resin, amino resin, and fluororesin, or a combination of two or more selected therefrom. When the resin component contains other resins, the total content of the (a) anionic polyurethane resin having an ester bond and the (b) epoxy resin having a bisphenol skeleton is preferably 50% by mass or more, and more preferably 75% by mass or more, in order to more reliably prevent a decrease in flexibility and obtain adhesion as a chemical treatment film.
[0065] The chemical conversion coating contains, as inorganic compounds, 2 to 10 mass % of a vanadium compound, 40 to 60 mass % of a zirconium compound, and 0.5 to 5 mass % of a fluorine compound. By including these compounds, the corrosion resistance of the chemical conversion coating can be improved.
[0066] The vanadium compound is added to a chemical conversion solution and acts as a rust inhibitor. When the vanadium compound is contained in the chemical conversion film, the vanadium compound is appropriately dissolved in a corrosive environment and combines with zinc ions and other plating components that also dissolve in a corrosive environment to form a dense protective film. The formed protective film can further increase corrosion resistance not only to the flat surface of the steel sheet, but also to defects, damaged areas of the plating film caused by processing, corrosion that progresses from the cut end surface to the flat surface, and the like. Examples of the vanadium compound include vanadium pentoxide, metavanadic acid, ammonium metavanadate, vanadium oxytrichloride, vanadium trioxide, vanadium dioxide, magnesium vanadate, vanadyl acetylacetonate, vanadium acetylacetonate, etc. Among these, it is particularly desirable to use a tetravalent vanadium compound or a tetravalent vanadium compound obtained by reduction or oxidation.
[0067] The content of the vanadium compound in the chemical conversion coating is 2 to 10 mass %. If the content of the vanadium compound in the chemical conversion coating is less than 2 mass %, the inhibitor effect is insufficient, resulting in a decrease in corrosion resistance, whereas if the content of the vanadium compound exceeds 10 mass %, the moisture resistance of the chemical conversion coating is decreased.
[0068] The zirconium compound is contained in the chemical conversion coating, and is expected to improve the strength and corrosion resistance of the chemical conversion coating through its reaction with the plating metal and its coexistence with a resin component. Furthermore, the zirconium compound itself contributes to the formation of a dense chemical conversion coating, and because of its excellent covering properties, a barrier effect can be expected. Examples of the zirconium compound include neutral salts of zirconium sulfate, zirconium carbonate, zirconium nitrate, zirconium lactate, zirconium acetate, zirconium chloride, and the like.
[0069] The content of the zirconium compound in the chemical conversion coating is 40 to 60 mass %. If the content of the zirconium compound in the chemical conversion coating is less than 40 mass %, the strength and corrosion resistance of the chemical conversion coating will decrease, whereas if the content of the zirconium compound exceeds 60 mass %, the chemical conversion coating will become embrittled, causing damage or peeling of the chemical conversion coating when subjected to severe processing.
[0070] The fluorine compound is contained in the chemical conversion coating and acts as an adhesive agent for the plating coating, thereby making it possible to improve the corrosion resistance of the chemical conversion coating. As the fluorine compound, for example, fluoride salts such as ammonium salts, sodium salts, potassium salts, or fluorine compounds such as ferrous fluoride, ferric fluoride, etc. Among these, it is preferable to use fluoride salts such as ammonium fluoride, sodium fluoride, and potassium fluoride.
[0071] Furthermore, the content of the fluorine compound in the chemical conversion coating is 0.5 to 5 mass %. If the content of the fluorine compound in the chemical conversion coating is less than 0.5 mass %, sufficient adhesion cannot be obtained at the processed portion, and if the content of the fluorine compound exceeds 5 mass %, the moisture resistance of the chemical conversion coating decreases.
[0072] The coating weight of the chemical conversion coating is not particularly limited. For example, from the viewpoint of improving the adhesion of the chemical conversion coating while more reliably ensuring corrosion resistance, the coating weight of the chemical conversion coating is set to 0.025 to 0.5 g / m. 2 It is preferable that the coating weight of the chemical conversion coating is 0.025 g / m 2 By setting the coating weight at 0.5 g / m or more, corrosion resistance can be more reliably ensured, and the coating weight of the chemical conversion film is 0.5 g / m or more. 2 By setting the following, peeling of the chemical conversion coating can be suppressed. The coating weight of the chemical conversion coating may be determined by a method appropriately selected from existing techniques, such as a method of subjecting the coating to fluorescent X-ray analysis to measure the amount of an element present in the coating whose content is known in advance.
[0073] The method for forming the chemical conversion coating is not particularly limited, and can be appropriately selected according to the required performance, manufacturing equipment, etc. For example, the chemical conversion coating can be formed by continuously applying a chemical conversion treatment solution onto the plating film using a roll coater or the like, and then drying at a peak metal temperature (PMT) of about 60 to 200°C using hot air or induction heating. In addition to the roll coater, known methods such as airless spray, electrostatic spray, and curtain flow coater can be appropriately used to apply the chemical conversion treatment solution. Furthermore, the chemical conversion coating may be either a single-layer film or a multi-layer film as long as it contains the resin and the metal compound, and is not particularly limited.
[0074] (Paint film) As described above, the coated steel sheet of the present invention has a coating film formed directly or via a chemical conversion coating on a plating film, and the coating film has at least a primer coating film.
[0075] In the present invention, the primer coating film contains a polyester resin having a urethane bond, and an inorganic compound including a vanadium compound, a phosphate compound, and magnesium oxide. The primer coating film contains the polyester resin having a urethane bond and the inorganic compound, and therefore the adhesion of the coating film can be increased and the corrosion resistance can be improved.
[0076] The primer coating contains a polyester resin having a urethane bond as a main component. The polyester resin having a urethane bond is flexible and strong, so that the primer coating is less likely to crack when processed, and has a high affinity with a chemical conversion coating containing a urethane resin, so that the primer coating can particularly contribute to improving the corrosion resistance of processed parts. The term "main component" used herein means the component that is contained in the greatest amount among all the components in the primer coating film.
[0077] The polyester resin having a urethane bond may be a known resin such as a resin obtained by reacting a polyester polyol with a diisocyanate or polyisocyanate having two or more isocyanate groups. Also usable is a resin obtained by reacting the polyester polyol with the diisocyanate or polyisocyanate in an excess hydroxyl group state (urethane-modified polyester resin) with a blocked polyisocyanate.
[0078] The polyester polyol can be obtained by a known method utilizing a dehydration condensation reaction between a polyhydric alcohol component and a polybasic acid component. The polyhydric alcohol includes glycol and trihydric or higher polyhydric alcohol. Examples of the glycol include ethylene glycol, propylene glycol, diethylene glycol, triethylene glycol, tetraethylene glycol, dipropylene glycol, polyethylene glycol, polypropylene glycol, neopentyl glycol, hexylene glycol, 1,3-butanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 2-butyl-2-ethyl-1,3-propanediol, methylpropanediol, cyclohexanedimethanol, 3,3-diethyl-1,5-pentanediol, etc. Examples of the trihydric or higher polyhydric alcohol include glycerin, trimethylolethane, trimethylolpropane, pentaerythritol, dipentaerythritol, etc. These polyhydric alcohols can be used alone or in combination of two or more. The polybasic acid is usually a polyvalent carboxylic acid, but can be used in combination with a monovalent fatty acid if necessary. Examples of the polybasic acid include phthalic acid, tetrahydrophthalic acid, hexahydrophthalic acid, 4-methylhexahydrophthalic acid, bicyclo[2,2,1]heptane-2,3-dicarboxylic acid, trimellitic acid, adipic acid, sebacic acid, succinic acid, azelaic acid, fumaric acid, maleic acid, itaconic acid, pyromellitic acid, dimer acid, and the like, and their acid anhydrides, as well as 1,4-cyclohexanedicarboxylic acid, isophthalic acid, tetrahydroisophthalic acid, hexahydroisophthalic acid, hexahydroterephthalic acid, and the like. These polybasic acids can be used alone or in combination of two or more.
[0079] Examples of the polyisocyanate include aliphatic diisocyanates such as hexamethylene diisocyanate, trimethylhexamethylene diisocyanate, and dimer acid diisocyanate, aromatic diisocyanates such as xylylene diisocyanate (XDI), metaxylylene diisocyanate, tolylene diisocyanate (TDI), and 4,4-diphenylmethane diisocyanate (MDI), and further cyclic aliphatic diisocyanates such as isophorone diisocyanate, hydrogenated XDI, hydrogenated TDI, and hydrogenated MDI, as well as adducts, biurets, and isocyanurates thereof. These polyisocyanates can be used alone or in combination of two or more.
[0080] In addition, the hydroxyl value of the polyester resin having a urethane bond is not particularly limited, but from the viewpoints of solvent resistance, processability, etc., it is preferably 5 to 120 mgKOH / g, more preferably 7 to 100 mgKOH / g, and even more preferably 10 to 80 mgKOH / g. Furthermore, the number average molecular weight of the polyester resin having a urethane bond is preferably from 500 to 15,000, more preferably from 700 to 12,000, and even more preferably from 800 to 10,000, from the viewpoints of solvent resistance, processability, and the like.
[0081] The content of the polyester resin having a urethane bond in the primer coating is preferably 40 to 88% by mass. If the content of the polyester resin having a urethane bond is less than 40% by mass, the binder function of the primer coating may be reduced, whereas if the content of the polyester resin having a urethane bond exceeds 88% by mass, the inorganic functions described below, such as the inhibitor action, may be reduced.
[0082] Vanadium compounds, which are one of the inorganic compounds, act as inhibitors. Examples of the vanadium compounds include vanadium pentoxide, metavanadic acid, ammonium metavanadate, vanadium oxytrichloride, vanadium trioxide, vanadium dioxide, magnesium vanadate, vanadyl acetylacetonate, vanadium acetylacetonate, etc. In particular, among these, it is desirable to use a tetravalent vanadium compound or a tetravalent vanadium compound obtained by reduction or oxidation. The vanadium compound added to the primer coating may be the same or different from the vanadium compound added to the chemical conversion coating. It is believed that vanadate ions, which are gradually dissolved by moisture entering from the outside, react with ions on the surface of the zinc-based plated steel sheet to form a passive film with good adhesion, protecting the exposed metal parts and exerting a rust-preventing effect.
[0083] The content of the vanadium compound in the primer coating is not particularly limited, but is preferably 4 to 20 mass% from the viewpoint of achieving both corrosion resistance and moisture resistance. If the content of the vanadium compound is less than 4 mass%, the inhibitor effect may decrease, leading to a decrease in corrosion resistance, whereas if the content of the vanadium compound is more than 20 mass%, the moisture resistance of the primer coating may decrease.
[0084] Phosphate compounds, which are one of the inorganic compounds, also act as inhibitors. Examples of the phosphate compounds include phosphoric acid, ammonium salts of phosphoric acid, alkali metal salts of phosphoric acid, and alkaline earth metal salts of phosphoric acid. In particular, alkali metal salts of phosphoric acid, such as calcium phosphate, are preferably used.
[0085] The content of the phosphate compound in the primer coating is not particularly limited, but is preferably 4 to 20 mass% from the viewpoint of achieving both corrosion resistance and moisture resistance. If the content of the phosphate compound is less than 4 mass%, the inhibitor effect may decrease, leading to a decrease in corrosion resistance, whereas if the content of the phosphate compound is more than 20 mass%, the moisture resistance of the primer coating may decrease.
[0086] Magnesium oxide, which is one of the inorganic compounds, produces a product containing Mg during initial corrosion, and as a sparingly soluble magnesium salt, it has the effect of stabilizing the material and improving corrosion resistance.
[0087] The content of the magnesium oxide in the primer coating is not particularly limited, but is preferably 4 to 20% by mass from the viewpoint of achieving both corrosion resistance and corrosion resistance of the processed part. If the content of the magnesium oxide is less than 4% by mass, the above effect may decrease, leading to a risk of a decrease in corrosion resistance, whereas if the content of the magnesium oxide is more than 20% by mass, the flexibility of the primer coating may decrease, leading to a decrease in the corrosion resistance of the processed part.
[0088] The primer coating film may also contain components other than the above-mentioned polyester resin having a urethane bond and inorganic compound. For example, a crosslinking agent used in forming a primer coating film can be mentioned. The crosslinking agent reacts with the polyester resin having the urethane bond to form a crosslinked coating film, and examples thereof include oxazoline compounds, epoxy compounds, melamine compounds, isocyanate compounds, carbodiimide compounds, silane coupling compounds, etc., and it is also possible to use two or more crosslinking agents in combination. Among them, from the viewpoint of the corrosion resistance of the processed part of the obtained coated steel plate, a blocked polyisocyanate compound or the like can be preferably used. Examples of the blocked polyisocyanate include those in which the isocyanate group of a polyisocyanate compound is blocked with, for example, alcohols such as butanol, oximes such as methyl ethyl ketoxime, lactams such as ε-caprolactams, diketones such as acetoacetic acid diester, imidazoles such as 2-ethylimidazole, or phenols such as m-cresol.
[0089] Furthermore, the primer coating film may contain various known components that are commonly used in the coating field, if necessary, such as various surface conditioners, such as leveling agents and defoamers, various additives, such as dispersants, anti-settling agents, ultraviolet absorbers, light stabilizers, silane coupling agents and titanate coupling agents, various pigments, such as coloring pigments and extender pigments, luster materials, curing catalysts, organic solvents, etc.
[0090] The thickness of the primer coating film is preferably 1.5 μm or more, because by making the thickness of the primer coating film 1.5 μm or more, it is possible to more reliably obtain the effect of improving corrosion resistance and the effect of improving adhesion with the chemical conversion coating film and the top coating film formed on the primer coating film.
[0091] The method for forming the primer coating film is not particularly limited. In addition, as for the method for applying the coating composition constituting the primer coating film, the coating composition can be preferably applied by a method such as roll coater coating or curtain flow coating. After applying the coating composition, the primer coating film can be obtained by baking the coating composition by a heating means such as hot air heating, infrared heating, or induction heating. The baking treatment is usually performed at a maximum plate temperature of about 180 to 270°C for about 30 seconds to 3 minutes in this temperature range.
[0092] In addition, with regard to the coating film constituting the coated steel plate of the present invention, it is preferable that a top coating film is further formed on the primer coating film. The topcoat coating film can impart beauty to the coated steel sheet, such as color, gloss, and surface condition, and can also improve various performance properties, such as processability, weather resistance, chemical resistance, stain resistance, water resistance, and corrosion resistance.
[0093] The configuration of the topcoat coating film is not particularly limited, and the material, thickness, etc. can be appropriately selected depending on the required performance. For example, the topcoat film can be formed using a polyester resin paint, a silicon polyester resin paint, a polyurethane resin paint, an acrylic resin paint, a fluororesin paint, or the like. Furthermore, the topcoat coating film may contain appropriate amounts of titanium oxide, red iron oxide, mica, carbon black or other various coloring pigments; metallic pigments such as aluminum powder and mica; extender pigments consisting of carbonates, sulfates, etc.; various fine particles such as silica fine particles, nylon resin beads, acrylic resin beads, etc.; curing catalysts such as p-toluenesulfonic acid and dibutyltin dilaurate; wax; and other additives.
[0094] From the viewpoint of achieving both good appearance and workability, the thickness of the topcoat film is preferably 5 to 30 μm. When the thickness of the topcoat film is 5 μm or more, it is possible to more reliably stabilize the color appearance, and when the thickness of the topcoat film is 30 μm or less, it is possible to more reliably suppress the decrease in workability (the occurrence of cracks in the topcoat film).
[0095] The method of applying the coating composition for forming the topcoat coating film is not particularly limited. For example, the coating composition can be applied by a method such as roll coater coating or curtain flow coating. After applying the coating composition, the topcoat coating film can be formed by baking using a heating means such as hot air heating, infrared heating, or induction heating. The baking treatment is usually performed at a maximum plate temperature of about 180 to 270°C for about 30 seconds to 3 minutes in this temperature range.
[0096] <Manufacturing method for coated steel sheets> The method for producing a coated steel sheet of the present invention is a method for producing a coated steel sheet in which a coating film is formed on a plating film directly or via a chemical conversion film. In the manufacturing method of the present invention, the chemical conversion coating comprises a resin component containing 30 to 50 mass% in total of (a): an anionic polyurethane resin having an ester bond and (b): an epoxy resin having a bisphenol skeleton, the content ratio of (a):(b) being within a range of 3:97 to 60:40 by mass, and inorganic compounds including 2 to 10 mass% of a vanadium compound, 40 to 60 mass% of a zirconium compound, and 0.5 to 5 mass% of a fluorine compound; The coating film has at least a primer coating film, and the primer coating film contains a polyester resin having a urethane bond, and an inorganic compound containing a vanadium compound, a phosphoric acid compound, and magnesium oxide, The formation of the plating film includes a hot-dip galvanizing process in which a base steel sheet is immersed in a plating bath having a composition containing 45-65 mass% Al, 1.0-4.0 mass% Si, and 1.0-10.0 mass% Mg, with the balance being Zn and unavoidable impurities, and the Co content in the unavoidable impurities of the plating bath is controlled to 0.080 mass% or less.
[0097] As described above, Co contained in the plating film may deteriorate the corrosion resistance of the coated steel sheet. Therefore, by appropriately controlling the contents of Al, Zn, Si, and Mg in the plating bath and further reducing the content of Co as an unavoidable impurity, deterioration of corrosion resistance can be suppressed.
[0098] The conditions for the hot-dip galvanizing process are the same as those explained in the description of the plating film of the coated steel sheet of the present invention. The configurations of the chemical conversion film and the paint film are also the same as those explained for the chemical conversion film of the coated steel sheet of the present invention. EXAMPLES
[0099] (Samples 1-55) A cold-rolled steel sheet having a thickness of 0.8 mm produced by conventional methods was used as the base steel sheet, and annealing and plating processes were performed using a hot-dip plating simulator manufactured by Rhesca Corporation to produce hot-dip plated steel sheet samples 1 to 55 under the conditions shown in Table 1. The composition of the plating bath used in the production of hot-dip galvanized steel sheets was changed in various ranges of Al: 5-75 mass%, Si: 0.0-4.5 mass%, Mg: 0-10 mass%, and Co: 0.000-0.120 mass% so as to obtain the composition of the plating film of each sample shown in Table 2. The bath temperature of the plating bath was controlled to 450°C for Al: 5 mass%, 480°C for Al: 15 mass%, 590°C for Al: 30-60 mass%, and 630°C for Al: over 60 mass%, so that the plating immersion sheet temperature of the base steel sheet was the same as the plating bath temperature. Furthermore, in the case of Al: 30-60 mass%, the plating process was performed under the condition that the sheet temperature was cooled to a temperature range of 520-500°C in 3 seconds. In addition, the coating weight of the plating film was 85±5g / m per side for samples 1 to 52. 2 , and sample 53 is 50±5g / m per side 2 , and sample 54 is 100±5g / m per side 2 , Sample 55 is 125±5g / m per side 2 It was controlled so that
[0100] (2) After that, the coating of each sample of hot-dip galvanized steel sheet prepared was coated with the chemical conversion treatment solution shown in Table 1 using a bar coater, and then dried in a hot air drying furnace (achieved sheet temperature: 90°C) to obtain a coating weight of 0.1 g / m 2 A chemical conversion coating was formed. The chemical conversion treatment liquid used was prepared by dissolving each component in water as a solvent, and had a pH of 8 to 10. The types of each component (resin component, inorganic compound) contained in the chemical conversion treatment liquid are as follows: (Resin component) Resin A: (a) an anionic polyurethane resin having an ester bond (Superflex 210 manufactured by Daiichi Kogyo Seiyaku Co., Ltd.) and (b) an epoxy resin having a bisphenol skeleton (Yukarejin RE-1050 manufactured by Yoshimura Oil Chemical Co., Ltd.) mixed in a mass ratio of (a):(b) = 50:50. Resin B: Acrylic resin (DIC Corporation "Boncoat EC-740EF") (Inorganic compound) Vanadium compounds: Organic vanadium compounds chelated with acetylacetone. Zirconium Compounds: Ammonium Zirconium Carbonate Fluorine compounds: Ammonium fluoride
[0101] (3) Then, a primer paint was applied onto the chemical conversion coating film formed as described above using a bar coater, and baking was performed under conditions of a steel plate temperature of 230°C and a baking time of 35 seconds, thereby forming a primer coating film having the component composition shown in Table 1. Thereafter, a topcoat paint composition was applied onto the primer coating film formed as described above using a bar coater, and baking was performed under conditions of a steel plate temperature of 230°C to 260°C and a baking time of 40 seconds, thereby forming a topcoat coating film having the resin conditions and film thickness shown in Table 1, and each sample coated steel plate was produced. The primer coating was obtained by mixing the components and then stirring for about 1 hour in a ball mill. The following resin components and inorganic compounds were used to compose the primer coating film. (Resin component) Resin α: A urethane-modified polyester resin (obtained by reacting 455 parts by mass of polyester resin and 45 parts by mass of isophorone diisocyanate, having a resin acid value of 3, a number average molecular weight of 5,600, and a hydroxyl value of 36) cured with a blocked isocyanate was used. The polyester resin to be urethane-modified was prepared under the following conditions: 320 parts by mass of isophthalic acid, 200 parts by mass of adipic acid, 60 parts by mass of trimethylolpropane, and 420 parts by mass of cyclohexanedimethanenol were charged into a flask equipped with a stirrer, a distillation column, a water separator, a cooling tube, and a thermometer, and the mixture was heated and stirred, and the temperature was raised from 160°C to 230°C at a constant rate over 4 hours while distilling off the generated condensed water outside the system. After the temperature reached 230°C, 20 parts by mass of xylene was gradually added, and the condensation reaction was continued while maintaining the temperature at 230°C. The reaction was terminated when the acid value became 5 or less, and the mixture was cooled to 100°C, and then 120 parts by mass of Solvesso 100 (trade name, high-boiling aromatic hydrocarbon solvent, manufactured by Exxon Mobil Corp.) and 100 parts by mass of butyl cellosolve were added to obtain a polyester resin solution. Resin β: urethane-cured polyester resin ("Evaclad 4900" manufactured by Kansai Paint Co., Ltd.) (Inorganic compound) Vanadium Compounds: Magnesium Vanadate Phosphate Compounds: Calcium Phosphate Magnesium oxide compounds: Magnesium oxide In addition, the resins used in the topcoat coating shown in Table 1 were the following paints. Resin I: Melamine-cured polyester paint (BASF Japan Ltd. "Precolor HD0030HR") Resin II: Organosol-based baking-type fluororesin paint with a mass ratio of polyvinylidene fluoride and acrylic resin of 80:20 (BASF Japan Ltd. "Precolor No. 8800HR")
[0102] [Table 1]
[0103] (evaluation) The following evaluations were carried out on each of the coated steel sheet samples obtained as described above. The evaluation results are shown in Table 2.
[0104] (1) Plating film (composition, coating weight, X-ray diffraction intensity) For each sample of hot-dip galvanized steel sheet, a 100 mm diameter was punched out, the non-measurement surface was sealed with tape, and the plating was then dissolved and stripped off using a mixture of hydrochloric acid and hexamethylenetetramine as specified in JIS H 0401: 2013, and the adhesion weight of the plating film was calculated from the difference in mass of the sample before and after stripping. The calculated adhesion weights of the plating film obtained are shown in Table 2. The stripper solution was then filtered, and the filtrate and solid content were analyzed. Specifically, the filtrate was analyzed by ICP atomic emission spectrometry to quantify the components other than insoluble Si. The solids were dried and incinerated in a 650°C heating furnace, and then melted by adding sodium carbonate and sodium tetraborate. The molten material was then dissolved in hydrochloric acid, and the solution was analyzed by ICP emission spectroscopy to quantify the insoluble silicon. The silicon concentration in the plating film was calculated by adding the soluble silicon concentration obtained by filtrate analysis to the insoluble silicon concentration obtained by solid content analysis. The composition of the plating film obtained as a result of calculation is shown in Table 2. In addition, each sample was sheared to a size of 100 mm x 100 mm, and the plating film on the surface to be evaluated was mechanically scraped off until the base steel sheet was revealed. The resulting powder was thoroughly mixed, and 0.3 g was taken out and qualitative analysis of the above powder was performed using an X-ray diffraction apparatus (Rigaku Corporation, "SmartLab") under the following conditions: X-ray used: Cu-Kα (wavelength = 1.54178 Å), Kβ ray removal: Ni filter, tube voltage: 40 kV, tube current: 30 mA, scanning speed: 4° / min, sampling interval: 0.020°, divergence slit: 2 / 3°, solar slit: 5°, detector: high-speed one-dimensional detector (D / teX Ultra). The diffraction intensity (cps) was calculated by subtracting the base intensity from each peak intensity, and the diffraction intensity of the Si (111) plane (plane spacing d = 0.3135 nm) and the Mg2Si (111) plane (plane spacing d = 0.3668 nm) were measured. The measurement results are shown in Table 2.
[0105] (2) Corrosion resistance evaluation Each coated steel sheet sample was sheared to a size of 120 mm x 120 mm, and the area of 10 mm from each edge of the surface to be evaluated, as well as the end faces and non-evaluation surfaces of the sample, were sealed with tape to expose the surface to be evaluated in a size of 100 mm x 100 mm, which was used as the evaluation sample. Three identical evaluation samples were prepared. An accelerated corrosion test was carried out on all three evaluation samples prepared as described above, following the cycle shown in Figure 1. The accelerated corrosion test started with wetting, and the sample was taken out every 20 cycles, washed with water, dried, and then visually inspected to see if there was any red rust on the sheared edge of one side that was not sealed with tape. The number of cycles at which red rust was observed was evaluated according to the following criteria. The evaluation results are shown in Table 2. ◎: Number of cycles in which red rust occurred on three samples ≥ 600 cycles ○: 600 cycles > Number of cycles in which red rust appeared on 3 samples ≧ 500 cycles ×: Number of cycles in which red rust occurred in at least one sample <500 cycles
[0106] (3) Appearance after painting The surface of each of the coated steel sheet samples was visually observed. The observation results were evaluated according to the following criteria. The evaluation results are shown in Table 2. ◎: No wrinkle defects were observed ○: Wrinkle defects were observed only within 50 mm from the edge ×: Wrinkle defects were observed outside the range of 50 mm from the edge.
[0107] (4) Workability after painting Each coated steel plate sample was sheared to a size of 70 mm x 150 mm, and then eight plates of the same thickness were sandwiched inside and bent 180° (8T bend). Cellophane tape (registered trademark) was firmly attached to the outer surface of the bent part after bending, and then peeled off. The surface condition of the coating film on the outer surface of the bent part and the presence or absence of adhesion (peeling) of the coating film on the surface of the tape used were visually observed, and the processability was evaluated according to the following criteria. The evaluation results are shown in Table 2. ○: No cracks or peeling were observed in the plating film. △: There are cracks in the plating film, but no peeling is observed. ×: Both cracks and peeling were observed in the plating film.
[0108] (5) Bath stability During hot-dip plating, the condition of the plating bath surface was visually inspected and compared with the plating bath surface (bath surface free of Mg-containing oxide) used in manufacturing hot-dip Al-Zn-plated steel sheets. Evaluation was performed according to the following criteria, and the evaluation results are shown in Table 2. ◯: Similar to hot-dip Al-Zn plating bath (55% Al by mass, balance Zn-1.6% by mass bath) △: There is more white oxide than in the hot-dip Al-Zn plating bath (55% Al by mass, balance Zn-1.6% by mass bath). ×: Black oxide formation is observed in the plating bath.
[0109] [Table 2]
[0110] The results in Table 2 show that the samples of the present invention are excellent in terms of a good balance of corrosion resistance, appearance after painting, workability after painting, and bath stability, compared to the samples of the comparative examples. [Industrial Applicability]
[0111] According to the present invention, it is possible to provide a coated steel sheet having stably excellent corrosion resistance and corrosion resistance of processed parts, and a method for producing the same.
Claims
1. A coated steel sheet having a coating film formed directly or via a chemical conversion coating on a plating film, The plating film has a composition containing 45 to 65 mass% Al, 1.0 to 4.0 mass% Si, and 1.0 to 10.0 mass% Mg, with the remainder being Zn and unavoidable impurities; The Co content in the unavoidable impurities is 0.080 mass% or less with respect to the total mass of the plating film, The Si and Mg in the plating film 2 The diffraction intensity of Si as determined by an X-ray diffraction method satisfies the following relationship (1): Si(111) / Mg 2 Si (111)≦0.8 ・・・(1) Si (111): Diffraction intensity of the Si (111) plane (plane spacing d = 0.3135 nm), Mg 2 Si(111):Mg 2 Diffraction intensity of Si (111) plane (plane spacing d = 0.3668 nm) The chemical conversion coating contains a resin component containing 30 to 50 mass% in total of (a): an anionic polyurethane resin having an ester bond and (b): an epoxy resin having a bisphenol skeleton, the content ratio of (a) to (b) ((a):(b)) being in the range of 3:97 to 60:40 in terms of mass ratio, and an inorganic compound containing 2 to 10 mass% of a vanadium compound, 40 to 60 mass% of a zirconium compound, and 0.5 to 5 mass% of a fluorine compound; The coating film has at least a primer coating film, and the primer coating film contains a polyester resin having a urethane bond, and an inorganic compound including a vanadium compound, a phosphate compound, and magnesium oxide.
2. 2. The coated steel sheet according to claim 1, wherein a diffraction intensity of Si in the plating film, as determined by an X-ray diffraction method, satisfies the following relationship (2): Si (111)=0...(2) Si (111): Diffraction intensity of the Si (111) plane (plane spacing d = 0.3135 nm)
3. The coated steel sheet according to claim 1 or 2, wherein the plating film further contains Sr: 0.01 to 1.0 mass %.
4. The coated steel sheet according to any one of claims 1 to 3, characterized in that the Al content in the plating film is 50 to 60 mass%.
5. The coated steel sheet according to any one of claims 1 to 4, characterized in that the Si content in the plating film is 1.0 to 3.0 mass%.
6. The coated steel sheet according to any one of claims 1 to 5, characterized in that the Mg content in the plating film is 1.0 to 5.0 mass%.
7. A method for producing a coated steel sheet in which a coating film is formed on a plating film directly or via a chemical conversion coating, comprising the steps of: The chemical conversion coating contains a resin component containing 30 to 50 mass% in total of (a): an anionic polyurethane resin having an ester bond and (b): an epoxy resin having a bisphenol skeleton, the content ratio of (a) to (b) ((a):(b)) being in the range of 3:97 to 60:40 in terms of mass ratio, and an inorganic compound containing 2 to 10 mass% of a vanadium compound, 40 to 60 mass% of a zirconium compound, and 0.5 to 5 mass% of a fluorine compound; The coating film has at least a primer coating film, and the primer coating film contains a polyester resin having a urethane bond, and an inorganic compound containing a vanadium compound, a phosphoric acid compound, and magnesium oxide, The method for producing a coated steel sheet includes a hot-dip coating process in which a base steel sheet is immersed in a coating bath containing 45 to 65 mass% Al, 1.0 to 4.0 mass% Si, and 1.0 to 10.0 mass% Mg, with the remainder consisting of Zn and unavoidable impurities, and is characterized in that the diffraction intensity of Si and Mg2Si in the coating, as measured by an X-ray diffraction method, satisfies the following relationship (1) by controlling the Co content in the unavoidable impurities of the coating bath to 0.080 mass% or less with respect to the total mass of the coating bath. Si (111) / Mg 2 Si (111)≦0.8 ... (1) Si (111): Diffraction intensity of the Si (111) plane (plane spacing d = 0.3135 nm), Mg 2 Si (111): Diffraction intensity of the (111) plane of Mg 2 Si (plane spacing d = 0.3668 nm)
8. The method for producing a coated steel sheet according to claim 7, characterized in that the plating bath further contains 0.01 to 1.0 mass% Sr.
Citation Information
Patent Citations
Method for plating surface of steel with Al-Zn-Mg-Si alloy plating layer in continuous hot-dipping manner
CN105483594A
JP1975000039A
JP1975020228A
Access method of memory unit
JP1985055591A
Steel sheet plated with al based metal with corrosion resistance in plated part and end face
JP2002012959A