Steel sheets and plated steel sheets
By forming internal oxides within high-strength steel sheets, the issues of hydrogen embrittlement and liquid metal embrittlement are mitigated, enhancing plating properties and structural integrity in automotive applications.
Patent Information
- Application Number
- JP2023517129
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-04-27
- Filing Date
- 2022-03-14
- Publication Date
- 2024-10-09
- Estimated Expiration
- 2042-03-14
AI Technical Summary
High-strength steel sheets used in automotive and other applications face issues with hydrogen embrittlement cracking and liquid metal embrittlement due to hydrogen penetration and zinc intrusion during processing, which affect plating properties and structural integrity.
The formation of an internal oxidation layer with fine-grained and coarse-grained oxides within the steel sheet, along with a grain boundary oxide structure, acts as trap sites for hydrogen and zinc, preventing their penetration and enhancing plating adherence.
This approach significantly improves plating properties, hydrogen embrittlement resistance, and liquid metal embrittlement resistance by reducing hydrogen and zinc intrusion, ensuring structural integrity and adherence in corrosive environments.
Smart Images

Figure 0007564490000003 
Figure 0007564490000004 
Figure 0007564490000005
Abstract
Description
[Technical field]
[0001] The present invention relates to a steel sheet and a plated steel sheet. More specifically, the present invention relates to a high-strength steel sheet and a plated steel sheet having high plateability, LME resistance, and hydrogen embrittlement resistance. [Background technology]
[0002] In recent years, efforts have been made to increase the strength of steel sheets used in various fields such as automobiles, home appliances, and building materials. For example, in the automobile field, the use of high-strength steel sheets has been increasing in order to reduce the weight of vehicle bodies in order to improve fuel efficiency. Such high-strength steel sheets typically contain elements such as C, Si, Mn, and Al to improve the strength of the steel.
[0003] In the manufacture of high-strength steel sheets, heat treatment such as annealing is generally performed after rolling. Among the elements typically contained in high-strength steel sheets, Si, Mn, and Al, which are easily oxidized elements, may combine with oxygen in the atmosphere during the heat treatment to form a layer containing oxides near the surface of the steel sheet. Examples of the form of such a layer include a form in which an oxide containing Si, Mn, or Al is formed as a film on the outside (surface) of the steel sheet (external oxide layer), and a form in which an oxide is formed inside (surface layer) of the steel sheet (internal oxide layer).
[0004] When a plating layer (e.g., a Zn-based plating layer) is formed on the surface of a steel sheet with an outer oxide layer, the oxide exists as a film on the surface of the steel sheet, which inhibits interdiffusion between the steel components (e.g., Fe) and the plating components (e.g., Zn), affecting the adhesion between the steel and the plating, and resulting in insufficient plating (e.g., an increase in unplated areas). Therefore, from the viewpoint of improving plating, a steel sheet with an inner oxide layer is more preferable than a steel sheet with an outer oxide layer.
[0005] With regard to the internal oxidation layer, Patent Documents 1 and 2 describe a high-strength plated steel sheet having a tensile strength of 980 MPa or more, which is a plated steel sheet having a zinc-based plating layer on a base steel sheet containing C, Si, Mn, Al, etc., and which has an internal oxidation layer containing oxides of Si and / or Mn in the surface layer of the base steel sheet. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2016-130357 A [Patent Document 2] JP 2018-193614 A Summary of the Invention [Problem to be solved by the invention]
[0007] High-strength steel sheets used in automotive components and the like are sometimes used in atmospheric corrosive environments where temperature and humidity fluctuate greatly. It is known that when high-strength steel sheets are exposed to such atmospheric corrosive environments, hydrogen produced during the corrosion process penetrates into the steel. Hydrogen that penetrates into the steel segregates at the martensite grain boundaries of the steel structure, embrittling the grain boundaries and potentially causing cracks in the steel sheet. This phenomenon of cracks caused by penetrated hydrogen is called hydrogen embrittlement cracking (delayed fracture), and is often a problem when processing steel sheets. Therefore, in order to prevent hydrogen embrittlement cracking, it is effective to reduce the amount of hydrogen accumulated in the steel for steel sheets used in corrosive environments.
[0008] Furthermore, when a plated steel sheet having a Zn-based plating layer or the like provided on a high-strength steel sheet is subjected to hot stamp forming or welding, the plated steel sheet is processed at high temperatures (e.g., about 900°C), and the Zn contained in the plating layer may be processed in a molten state. In this case, the molten Zn may penetrate into the steel sheet and cause cracks inside the steel sheet. This phenomenon is called liquid metal embrittlement (LME), and it is known that the fatigue properties of the steel sheet are deteriorated due to the LME. Therefore, in order to prevent LME cracking, it is effective to suppress the penetration of Zn and other elements contained in the plating layer into the steel sheet.
[0009] Patent Documents 1 and 2 teach that controlling the average depth of the internal oxide layer to 4 μm or more and making the internal oxide layer function as a hydrogen trapping site can prevent hydrogen penetration and suppress hydrogen embrittlement. However, no consideration has been given to controlling the morphology of the oxides present in the internal oxide layer, and there is room for improvement in hydrogen embrittlement resistance. Furthermore, no consideration has been given to improving LME resistance.
[0010] In view of the above circumstances, an object of the present invention is to provide a high-strength steel sheet and a plated steel sheet having high platability, LME resistance and hydrogen embrittlement resistance. [Means for solving the problem]
[0011] The present inventors have found that, in order to solve the above problems, it is important to form oxides in the surface layer of a steel sheet, i.e., inside the steel sheet, and further to control the form of the oxides present in the surface layer of the steel sheet. More specifically, the present inventors have found that by forming an internal oxide layer, high galvanizability is ensured, and by forming a large amount of fine granular oxides present within the crystal grains of the metal structure as the form of oxides contained in the internal oxide layer, the fine granular oxides function not only as trap sites for hydrogen that can enter the steel in a corrosive environment, but also as trap sites for Zn that can enter the steel during hot stamp forming or welding, thereby obtaining high LME resistance and hydrogen embrittlement resistance, and by also forming a large amount of coarse granular oxides, the coarse granular oxides function as trap sites for hydrogen that can enter the steel in a corrosive environment. They discovered that by not only having the internal oxide layer function as a trap site for Zn that can penetrate into the steel during hot stamping or welding, but also by having the internal oxide layer function as a trap site for Zn that can penetrate into the steel during hot stamping or welding, it is possible to obtain higher LME resistance and hydrogen embrittlement resistance; by forming a large amount of grain boundary oxide present at the crystal grain boundaries of the metallographic structure, the grain boundary oxide can be made to function as an escape route for hydrogen that has penetrated into the steel, thereby obtaining higher hydrogen embrittlement resistance; and by forming a layered region (sometimes referred to as a surface depletion layer) in which the metallographic structure has a composition of low Si and high Al at half the depth of the internal oxide layer, it is possible to obtain higher LME resistance.
[0012] The present invention has been made based on the above findings, and the gist of the present invention is as follows. (1) In mass%, C: 0.05-0.40%, Si: 0.2-3.0%, Mn: 0.1-5.0%, sol.Al: 0.4-1.50%, P:0.0300% or less, S: 0.0300% or less, N: 0.0100% or less, B: 0~0.010%, Ti: 0 to 0.150%, Nb: 0 to 0.150%, V: 0~0.150%, Cr: 0-2.00%, Ni: 0-2.00%, Cu: 0-2.00%, Mo: 0-1.00%, W: 0 to 1.00%, Ca: 0-0.100%, Mg: 0~0.100%, Zr: 0 to 0.100%, Hf: 0 to 0.100%, and A steel sheet having a composition containing REM: 0 to 0.100%, with the balance being Fe and impurities, The steel sheet has an internal oxide layer on the surface thereof, the internal oxide layer including a fine granular oxide, a coarse granular oxide and a grain boundary oxide, When a cross section of the surface layer of the steel plate is observed, The number density of the fine granular oxide in the internal oxide layer is 4.0 particles / μm 2 That's all. The number density of the coarse grain oxide in the internal oxide layer is 4.0 grains / 25 μm 2 That's all. A ratio A of a length of the grain boundary oxide projected onto the surface of the steel sheet to a length of the surface of the steel sheet is 50% or more and 100% or less, a steel plate including a surface depleted layer, the surface depleted layer having a steel composition, in mass%, which does not include the fine granular oxides, the coarse granular oxides, and the grain boundary oxides at a depth half the average depth of the internal oxide layer, and which satisfies Si≦0.6% and Al≧0.05%. (2) The number density of the fine granular oxide is 4.0 to 30 particles / μm 2 The steel plate according to (1), (3) A plated steel sheet having a plating layer containing Zn on the steel sheet according to (1) or (2). (4) (3) A Zn-plated steel sheet according to the above (3), characterized in that the Al content in the plating layer is 0.3 to 1.5 mass %. Effect of the Invention
[0013] According to the present invention, it is possible to make the fine granular oxides and the coarse granular oxides present in large quantities in the surface layer of the steel sheet function as trap sites for hydrogen that penetrates in a corrosive environment, and as a result, it is possible to significantly suppress the amount of hydrogen that penetrates in a corrosive environment and significantly improve hydrogen embrittlement resistance. In addition, the fine granular oxides and the coarse granular oxides also function as trap sites for Zn that penetrates into the steel during hot stamp forming or welding, and the amount of Zn that penetrates can be significantly suppressed, and LME resistance can be significantly improved. In addition, by forming a large amount of grain boundary oxides, it is possible to make the grain boundary oxides function as escape routes for hydrogen that has penetrated into the steel, and as a result, it is possible to release the penetrated hydrogen, reduce the amount of hydrogen that accumulates in the steel, and significantly improve hydrogen embrittlement resistance. Furthermore, according to the present invention, by forming a layered region (sometimes referred to as a "surface depleted layer") in which the metal structure has a composition of low Si and high Al at half the depth of the internal oxide layer, Al inhibits the penetration of Zn into the steel grain boundaries during hot stamp forming or welding, and LME resistance can be further improved. Since the fine-grained oxide, coarse-grained oxide, grain boundary oxide and surface depleted layer are formed inside the steel sheet, when a plating layer is formed, sufficient interdiffusion between the steel components and the plating components is achieved, making it possible to obtain high plating ability. Therefore, according to the present invention, it is possible to obtain high plating ability, LME resistance and hydrogen embrittlement resistance in a high-strength steel sheet. [Brief description of the drawings]
[0014] [Figure 1] 1 shows a schematic diagram of a cross section of a steel sheet having an outer oxide layer. [Diagram 2] FIG. 1 shows a schematic diagram of a cross section of an exemplary steel plate according to the present invention. [Diagram 3] FIG. 2 shows a schematic diagram for explaining the measurement of ratio A in the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] <Steel plate> The steel plate according to the present invention comprises, in mass%, C: 0.05-0.40%, Si: 0.2-3.0%, Mn: 0.1-5.0%, sol.Al: 0.4-1.50%, P:0.0300% or less, S: 0.0300% or less, N: 0.0100% or less, B: 0~0.010%, Ti: 0 to 0.150%, Nb: 0 to 0.150%, V: 0~0.150%, Cr: 0-2.00%, Ni: 0-2.00%, Cu: 0-2.00%, Mo: 0-1.00%, W: 0 to 1.00%, Ca: 0-0.100%, Mg: 0~0.100%, Zr: 0 to 0.100%, Hf: 0 to 0.100%, and A steel sheet having a composition containing REM: 0 to 0.100%, with the balance being Fe and impurities, The steel sheet has an internal oxide layer on the surface thereof, the internal oxide layer including a fine granular oxide, a coarse granular oxide and a grain boundary oxide, When a cross section of the surface layer of the steel plate is observed, The number density of the fine granular oxide in the internal oxide layer is 4.0 particles / μm 2 That's all. The number density of the coarse grain oxide in the internal oxide layer is 4.0 grains / 25 μm 2 That's all. A ratio A of a length of the grain boundary oxide projected onto the surface of the steel sheet to a length of the surface of the steel sheet is 50% or more and 100% or less, The steel composition includes a surface depletion layer that does not include the fine granular oxides, the coarse granular oxides, and the grain boundary oxides at a depth half the average depth of the internal oxide layer and satisfies, in mass%, Si≦0.6% and Al≧0.05%.
[0016] In the manufacture of high-strength steel sheets, after rolling (typically hot rolling and cold rolling) a steel billet adjusted to a predetermined composition, annealing is generally performed for the purpose of obtaining a desired structure, etc. In this annealing, components in the steel sheet that are relatively easily oxidized (e.g., Si, Mn, Al) combine with oxygen in the annealing atmosphere to form a layer containing oxides near the surface of the steel sheet. For example, as in the steel sheet 1 shown in FIG. 1, an outer oxide layer 2 is formed in a film shape on the surface of the base steel 3 (i.e., outside the base steel 3). When the outer oxide layer 2 is formed in a film shape on the surface of the base steel 3, when a plating layer (e.g., a zinc-based plating layer) is formed, the outer oxide layer 2 inhibits interdiffusion between the plating components (e.g., Zn, Al) and the steel components (e.g., Fe), so that the adhesion between the steel and the plating cannot be sufficiently ensured, and unplated parts where no plating layer is formed may occur.
[0017] In contrast, as illustrated in FIG. 2, the steel sheet 11 according to the present invention does not form an outer oxide layer 2 on the surface of the base steel 3 as in the steel sheet 1 shown in FIG. 1, but has fine granular oxides 12, coarse granular oxides 15, and grain boundary oxides 13 inside the base steel 14. Therefore, when a coating layer is formed on the surface of the steel sheet 11, the steel sheet 11 according to the present invention in which the oxides 12, coarse granular oxides 15, and grain boundary oxides 13 are formed inside the base steel 14 allows sufficient interdiffusion between the coating components and the steel components, and can obtain high coating properties, compared to the steel sheet 1 having the outer oxide layer 2 as shown in FIG. 1. Therefore, the present inventors have found that, from the viewpoint of obtaining high coating properties, it is effective to form oxides inside the steel sheet by controlling the conditions during the annealing treatment. The term "high coating properties", when used with respect to a steel sheet, indicates that a coating layer can be formed with little (for example, 5.0 area % or less) or no uncoated parts (parts on which a coating layer is not formed) when the steel sheet is subjected to a coating treatment. Furthermore, the term "high platability" when used in reference to a plated steel sheet refers to a plated steel sheet having very little (e.g., 5.0% by area or less) or no unplated areas. From the viewpoint of the above-mentioned platability, the steel sheet 11 according to this embodiment preferably has a smaller outer oxide layer, but may have an outer oxide layer as long as high platability is obtained.
[0018] Moreover, high-strength steel sheets used in atmospheric environments, particularly high-strength steel sheets for automobiles, are repeatedly exposed to various environments with different temperatures and humidity. Such environments are called atmospheric corrosive environments, and it is known that hydrogen is generated during the corrosion process in such atmospheric corrosive environments. This hydrogen penetrates deeper than the surface layer region in the steel and segregates at the martensite grain boundaries of the steel sheet structure, embrittling the grain boundaries and causing hydrogen embrittlement cracking (delayed fracture) in the steel sheet. Since martensite is a hard structure, it is highly sensitive to hydrogen and is prone to hydrogen embrittlement cracking. Such cracking can be a problem during processing of the steel sheet. Therefore, in order to prevent hydrogen embrittlement cracking, it is effective to reduce the amount of hydrogen stored in the steel, more specifically, the amount of hydrogen stored at a position deeper than the surface layer region of the steel sheet, in high-strength steel sheets used in atmospheric corrosive environments. The present inventors have found that by controlling the morphology of the oxides present in the surface layer of a steel sheet, more specifically, by causing "fine granular oxides" having a particle size and number density in a predetermined range as oxides to be present, the fine granular oxides function as trap sites for hydrogen that penetrates in a corrosive environment in the surface layer region of the steel sheet, making it possible to reduce the amount of hydrogen accumulation in the steel sheet used in a corrosive environment; and by causing "coarse granular oxides" having a particle size and number density in a predetermined range as oxides to be present, the coarse granular oxides function as trap sites for hydrogen that penetrates in a corrosive environment in the surface layer region of the steel sheet, making it possible to further reduce the amount of hydrogen accumulation in the steel sheet used in a corrosive environment; and by causing "grain boundary oxides" present in a predetermined ratio to coexist, the grain boundary oxides function as an escape route for the penetrated hydrogen, making it possible to reduce the amount of hydrogen accumulation in the steel sheet used in a corrosive environment by not only suppressing the penetration of hydrogen but also promoting the release of the penetrated hydrogen out of the system. The term "high hydrogen embrittlement resistance" refers to a state in which the amount of hydrogen accumulated in the steel sheet and plated steel sheet is reduced so that hydrogen embrittlement cracking can be sufficiently suppressed.
[0019] The present inventors conducted a detailed analysis of the relationship between the form of oxides and their effectiveness as hydrogen trapping sites, and found that it is effective to have a large amount of fine granular oxides 12 dispersed in a granular form and spaced apart from each other on the surface layer of the base steel 14, as shown in FIG. 2. In addition, it was found that it is more effective to have a large amount of coarse granular oxides 15 dispersed in a granular form and spaced apart from each other on the surface layer of the base steel 14. Without being bound by a particular theory, it is believed that the trapping function of oxides in steel sheets against invaded hydrogen is positively correlated with the surface area of the oxides. That is, it is believed that by dispersing a large amount of fine oxides in a discrete manner on the surface layer of the steel sheet, the surface area of the oxides on the surface layer of the steel sheet increases, improving the hydrogen trapping function. Furthermore, when hydrogen is excessively invaded and the fine oxides cannot trap it, the coarse oxides have a relatively large capacity and can trap a large amount of hydrogen, so that the excessively invaded hydrogen can also be trapped, and the hydrogen trapping function is further improved. Therefore, the inventors have found that, from the viewpoint of obtaining high hydrogen embrittlement resistance, it is important to control the conditions during manufacturing of the steel sheet, particularly during annealing, so that a large amount of fine granular oxides and coarse granular oxides that function as trap sites for hydrogen that penetrates when placed in a corrosive environment are present. Note that, since the metal structure of the surface layer of a steel sheet is typically composed of a metal structure that is softer than that of the interior of the steel sheet (for example, at the 1 / 8 or 1 / 4 position of the sheet thickness), hydrogen embrittlement cracking does not pose a particular problem even if hydrogen is present in the surface layer of the steel sheet.
[0020] In addition, the present inventors conducted a detailed analysis of the relationship between the form of oxides and their effectiveness as a hydrogen escape route, and found that it is effective to have a large amount of grain boundary oxide 13 present at the grain boundaries in the surface layer of the base steel 14, as shown in FIG. 2. It was found that the presence of a large amount of grain boundary oxide 13 ensures a route for hydrogen in the steel to leave the system, and makes it possible to efficiently release hydrogen that has entered the steel to the outside of the system along the grain boundaries. It was also found that if the grain boundary oxide exists at a deeper position in the steel sheet, more hydrogen can be released from the inside of the steel sheet to the outside, and the amount of hydrogen accumulated in the steel sheet can be further reduced. Therefore, by having the above-mentioned granular oxide and the grain boundary oxide coexist, it is possible to significantly improve hydrogen embrittlement resistance.
[0021] On the other hand, when a plated steel sheet having a Zn-containing plating layer provided on the surface of the steel sheet is subjected to hot stamp forming or welding, the temperature during processing becomes high, and the Zn contained in the plating layer may melt. When Zn melts, the molten Zn penetrates into the steel, and when processing is performed in this state, liquid metal embrittlement (LME) cracks occur inside the steel sheet, and the fatigue properties of the steel sheet may deteriorate due to the LME. The present inventors have found that when the above-mentioned fine granular oxide and coarse granular oxide have a desired number density, they contribute not only to improving hydrogen embrittlement resistance but also to improving LME resistance. More specifically, they have found that the fine granular oxide and coarse granular oxide function as trap sites for Zn that tries to penetrate into the steel during processing at high temperatures. As a result, for example, Zn that tries to penetrate into the steel during hot stamp forming is captured by the fine granular oxide and coarse granular oxide on the surface layer of the steel sheet, and the penetration of Zn into the grain boundaries is suitably suppressed. Therefore, it was found that in order to improve not only the above-mentioned hydrogen penetration resistance but also the LME resistance, it is important to have a large amount of fine granular oxide and coarse granular oxide.
[0022] In addition, the fine-grained oxide, the coarse-grained oxide, and the grain boundary oxide are formed by the oxidation of relatively easily oxidized components (e.g., Si, Mn, Al) in the steel sheet, and therefore the composition of the steel (in other words, the metal structure) around the oxide is deficient in these easily oxidized component elements compared to the original base material of the steel sheet. This region where the elements of the steel composition are deficient compared to the original base material of the steel sheet is also called a "depleted region". The layered "depleted region" is also called a "depleted layer", and the one present in the surface layer of the steel sheet is also called a "surface depleted layer". In the depleted region, among the elements that are easily oxidized, Si is relatively easily oxidized and Al is relatively difficult to oxidize, so that Si can be present at a low concentration and Al at a high concentration. The present inventors have also discovered that when such a depleted region in which the composition of the steel is low in Si and high in Al is present within a desired range, it also contributes to improving LME resistance. More specifically, in addition to the granular oxides and coarse granular oxides that function as Zn trap sites, the presence of Al in the composition of the steel surrounding the granular oxides and grain boundary oxides has been found to inhibit the penetration of Zn into the grain boundaries of the steel during high-temperature processing, and that the higher the concentration of Si in the steel composition, the more likely LME cracking occurs, and that LME can be suppressed by keeping the concentration of Si as low as possible. As a result, for example, the penetration of Zn into the grain boundaries of the steel during hot stamp forming is inhibited by Al in the steel composition, and the penetration of Zn into the grain boundaries is suitably suppressed, and LME is less likely to occur because the concentration of Si, which is prone to cause LME, is low. Therefore, it has been found that in order to improve LME resistance, it is important to have a depleted region where Si is low in concentration and Al is high in concentration.
[0023] The depletion region where Si is low in concentration and Al is high in concentration may overlap with the region where fine-grained oxides, coarse-grained oxides and the grain boundary oxides are distributed, that is, it may be formed inside the base steel, not like the outer oxide layer 2 on the surface of the base steel 3 in Fig. 1. Therefore, when a coating layer is formed on the surface of a steel sheet, the steel sheet according to the present invention having a depletion region, more specifically a surface depletion layer, formed inside the base steel allows sufficient interdiffusion between the coating components and the steel components, and enables high galvanic properties to be obtained, compared to the steel sheet 1 having the outer oxide layer 2 as shown in Fig. 1.
[0024] The steel plate according to the present invention will be described in detail below. The thickness of the steel plate according to the present invention is not particularly limited, but may be, for example, 0.1 to 3.2 mm.
[0025] [Steel plate composition] The composition of the steel sheet according to the present invention will be described. Unless otherwise specified, "%" regarding the content of an element means "mass%". In the numerical range of the composition, a numerical range expressed with "~" means a range including the numerical values written before and after "~" as the lower and upper limits, unless otherwise specified.
[0026] (C: 0.05~0.40%) C (carbon) is an important element for ensuring the strength of steel. If the C content is insufficient, sufficient strength may not be ensured. Furthermore, if the C content is insufficient, the desired internal oxide and / or surface depletion layer morphology may not be obtained. Therefore, the C content is 0.05% or more, preferably 0.07% or more, more preferably 0.10% or more, and even more preferably 0.12% or more. On the other hand, if the C content is excessive, weldability may decrease. Therefore, the C content is 0.40% or less, preferably 0.35% or less, and more preferably 0.30% or less.
[0027] (Si: 0.2 to 3.0%) Si (silicon) is an element effective in improving the strength of steel. If the Si content is insufficient, sufficient strength may not be ensured. Furthermore, desired oxides, particularly fine granular oxides, coarse granular oxides, grain boundary oxides, and / or surface depletion layers may not be sufficiently formed inside the steel sheet. Therefore, the Si content is 0.2% or more, preferably 0.3% or more, more preferably 0.5% or more, and even more preferably 1.0% or more. On the other hand, if the Si content is excessive, it may cause deterioration of the surface properties. Furthermore, it may cause coarsening of the granular oxides. Therefore, the Si content is 3.0% or less, preferably 2.5% or less, and more preferably 2.0% or less.
[0028] (Mn: 0.1-5.0%) Mn (manganese) is an element effective in improving the strength of steel by obtaining a hard structure. If the Mn content is insufficient, sufficient strength may not be ensured. Furthermore, desired oxides, particularly fine granular oxides, coarse granular oxides, grain boundary oxides, and / or surface depletion layers may not be sufficiently formed inside the steel sheet. Therefore, the Mn content is 0.1% or more, preferably 0.5% or more, more preferably 1.0% or more, and even more preferably 1.5% or more. On the other hand, if the Mn content is excessive, the metal structure may become non-uniform due to Mn segregation, and the workability may decrease. Furthermore, the granular oxides may become coarse. Therefore, the Mn content is 5.0% or less, preferably 4.5% or less, more preferably 4.0% or less, and even more preferably 3.5% or less.
[0029] (sol.Al:0.4~1.50%) Al (aluminum) is an element that acts as a deoxidizing element. If the Al content is insufficient, there is a risk that the effect of deoxidization cannot be sufficiently ensured. Furthermore, there is a risk that the desired oxides, particularly the fine granular oxides, the coarse granular oxides, the grain boundary oxides and / or the surface depletion layer, are not sufficiently generated inside the steel sheet. The Al content may be 0.4% or more, but in order to obtain a sufficient desired effect, the fine granular oxides, the coarse granular oxides, the grain boundary oxides and the surface depletion layer, the Al content is 0.5% or more, preferably 0.6% or more, more preferably 0.7% or more. On the other hand, if the Al content is excessive, there is a risk that the workability is reduced and the surface properties are deteriorated. Furthermore, there is a risk that the granular oxides are coarsened. Therefore, the Al content is 1.50% or less, preferably 1.20% or less, more preferably 0.80% or less. The Al content means the content of so-called acid-soluble Al (sol.Al).
[0030] (P:0.0300% or less) P (phosphorus) is an impurity generally contained in steel. If the P content exceeds 0.0300%, the weldability may be reduced. Therefore, the P content is 0.0300% or less, preferably 0.0200% or less, more preferably 0.0100% or less, and further preferably 0.0050% or less. The lower limit of the P content is not particularly limited, but from the viewpoint of manufacturing costs, the P content may be more than 0% or 0.0001% or more.
[0031] (S:0.0300% or less) S (sulfur) is an impurity generally contained in steel. If the S content exceeds 0.0300%, the weldability is reduced, and furthermore, the amount of MnS precipitated increases, which may reduce workability such as bendability. Therefore, the S content is 0.0300% or less, preferably 0.0100% or less, more preferably 0.0050% or less, and further preferably 0.0020% or less. The lower limit of the S content is not particularly limited, but from the viewpoint of desulfurization costs, the S content may be more than 0% or 0.0001% or more.
[0032] (N:0.0100% or less) N (nitrogen) is an impurity generally contained in steel. If the N content exceeds 0.0100%, the weldability may be reduced. Therefore, the N content is 0.0100% or less, preferably 0.0080% or less, more preferably 0.0050% or less, and further preferably 0.0030% or less. There is no particular lower limit for the N content, but from the viewpoint of manufacturing costs, the N content may be more than 0% or 0.0010% or more.
[0033] (B: 0~0.010%) Since B (boron) is an element that improves hardenability and contributes to improving strength, and also segregates at grain boundaries to strengthen the grain boundaries and improve toughness, it may be contained as necessary. Therefore, the B content is 0% or more, preferably 0.001% or more, more preferably 0.002% or more, and even more preferably 0.003% or more. On the other hand, from the viewpoint of ensuring sufficient toughness and weldability, the B content is 0.010% or less, preferably 0.008% or less, and more preferably 0.006% or less.
[0034] (Ti: 0 to 0.150%) Ti (titanium) is an element that precipitates as TiC during cooling of steel and contributes to improving strength, so it may be contained as necessary. Therefore, the Ti content is 0% or more, preferably 0.001% or more, more preferably 0.003% or more, even more preferably 0.005% or more, and even more preferably 0.010% or more. On the other hand, if it is contained excessively, coarse TiN may be generated and toughness may be impaired, so the Ti content is 0.150% or less, preferably 0.100% or less, and more preferably 0.050% or less.
[0035] (Nb: 0~0.150%) Since Nb (niobium) is an element that contributes to improving strength through improving hardenability, it may be contained as necessary. Therefore, the Nb content is 0% or more, preferably 0.010% or more, more preferably 0.020% or more, and even more preferably 0.030% or more. On the other hand, from the viewpoint of ensuring sufficient toughness and weldability, the Nb content is 0.150% or less, preferably 0.100% or less, and more preferably 0.060% or less.
[0036] (V:0~0.150%) V (vanadium) is an element that contributes to improving strength through improving hardenability, so it may be contained as necessary. Therefore, the V content is 0% or more, preferably 0.010% or more, more preferably 0.020% or more, and even more preferably 0.030% or more. On the other hand, from the viewpoint of ensuring sufficient toughness and weldability, the V content is 0.150% or less, preferably 0.100% or less, and more preferably 0.060% or less.
[0037] (Cr:0~2.00%) Cr (chromium) is effective in increasing the hardenability of steel and increasing its strength, so it may be contained as necessary. Therefore, the Cr content is 0% or more, preferably 0.10% or more, more preferably 0.20% or more, even more preferably 0.50% or more, and even more preferably 0.80% or more. On the other hand, if it is contained in excess, a large amount of Cr carbide is formed, which may adversely impair the hardenability, so the Cr content is 2.00% or less, preferably 1.80% or less, and more preferably 1.50% or less.
[0038] (Ni: 0-2.00%) Ni (nickel) is effective in increasing the hardenability of steel and increasing the strength of steel, so it may be contained as necessary. Therefore, the Ni content is 0% or more, preferably 0.10% or more, more preferably 0.20% or more, even more preferably 0.50% or more, and even more preferably 0.80% or more. On the other hand, since excessive addition of Ni leads to an increase in cost, the Ni content is 2.00% or less, preferably 1.80% or less, and more preferably 1.50% or less.
[0039] (Cu: 0-2.00%) Cu (copper) is effective in increasing the hardenability of steel and increasing the strength of steel, so it may be contained as necessary. Therefore, the Cu content is 0% or more, preferably 0.10% or more, more preferably 0.20% or more, even more preferably 0.50% or more, and even more preferably 0.80% or more. On the other hand, from the viewpoint of suppressing a decrease in toughness, cracking of the slab after casting, and a decrease in weldability, the Cu content is 2.00% or less, preferably 1.80% or less, and more preferably 1.50% or less.
[0040] (Mo:0~1.00%) Mo (molybdenum) is effective in increasing the hardenability of steel and increasing the strength of steel, so it may be contained as necessary. Therefore, the Mo content is 0% or more, preferably 0.10% or more, more preferably 0.20% or more, and even more preferably 0.30% or more. On the other hand, from the viewpoint of suppressing the deterioration of toughness and weldability, the Mo content is 1.00% or less, preferably 0.90% or less, and more preferably 0.80% or less.
[0041] (W:0~1.00%) W (tungsten) is effective in increasing the hardenability of steel and increasing the strength of steel, so it may be contained as necessary. Therefore, the W content is 0% or more, preferably 0.10% or more, more preferably 0.20% or more, and even more preferably 0.30% or more. On the other hand, from the viewpoint of suppressing the deterioration of toughness and weldability, the W content is 1.00% or less, preferably 0.90% or less, and more preferably 0.80% or less.
[0042] (Ca: 0~0.100%) Ca (calcium) is an element that contributes to inclusion control, particularly to finely dispersing inclusions, and has the effect of increasing toughness, so it may be contained as necessary. Therefore, the Ca content is 0% or more, preferably 0.001% or more, more preferably 0.005% or more, even more preferably 0.010% or more, and even more preferably 0.020% or more. On the other hand, if it is contained excessively, deterioration of surface properties may become apparent, so the Ca content is 0.100% or less, preferably 0.080% or less, and more preferably 0.050% or less.
[0043] (Mg: 0~0.100%) Mg (magnesium) is an element that contributes to inclusion control, particularly to finely dispersing inclusions, and has the effect of increasing toughness, so it may be contained as necessary. Therefore, the Mg content is 0% or more, preferably 0.001% or more, more preferably 0.003% or more, and even more preferably 0.010% or more. On the other hand, if it is contained excessively, deterioration of surface properties may become apparent, so the Mg content is 0.100% or less, preferably 0.090% or less, and more preferably 0.080% or less.
[0044] (Zr: 0~0.100%) Zr (zirconium) is an element that contributes to inclusion control, particularly to finely dispersing inclusions, and has the effect of increasing toughness, so it may be contained as necessary. Therefore, the Zr content is 0% or more, preferably 0.001% or more, more preferably 0.005% or more, and even more preferably 0.010% or more. On the other hand, if it is contained excessively, deterioration of surface properties may become apparent, so the Zr content is 0.100% or less, preferably 0.050% or less, and more preferably 0.030% or less.
[0045] (Hf:0~0.100%) Hf (hafnium) is an element that contributes to inclusion control, particularly to finely dispersing inclusions, and has the effect of increasing toughness, so it may be contained as necessary. Therefore, the Hf content is 0% or more, preferably 0.001% or more, more preferably 0.005% or more, and even more preferably 0.010% or more. On the other hand, if it is contained excessively, deterioration of surface properties may become apparent, so the Hf content is 0.100% or less, preferably 0.050% or less, and more preferably 0.030% or less.
[0046] (REM:0~0.100%) REM (rare earth elements) are elements that contribute to inclusion control, particularly to finely dispersing inclusions, and have the effect of increasing toughness, and may be contained as necessary. Therefore, the REM content is 0% or more, preferably 0.001% or more, more preferably 0.005% or more, and even more preferably 0.010% or more. On the other hand, if contained excessively, deterioration of surface properties may become apparent, so the REM content is 0.100% or less, preferably 0.050% or less, and more preferably 0.030% or less. REM is an abbreviation for Rare Earth Metal, and refers to elements belonging to the lanthanoid series. REM is usually added as misch metal.
[0047] The balance of the steel sheet according to the present invention other than the above-mentioned composition is composed of Fe and impurities. Here, the impurities refer to components that are mixed in due to various factors in the manufacturing process, including raw materials such as ores and scraps, during industrial production of the steel sheet, and are allowed to be contained within a range that does not adversely affect the properties of the steel sheet according to the present invention.
[0048] In the present invention, the composition of the steel sheet may be analyzed by an elemental analysis method known to those skilled in the art, for example, inductively coupled plasma mass spectrometry (ICP-MS). However, C and S may be measured by a combustion-infrared absorption method, and N may be measured by an inert gas fusion-thermal conductivity method. These analyses may be performed on samples taken from the steel sheet by a method conforming to JIS G0417:1999.
[0049] [surface] In the present invention, the "surface layer" of a steel sheet means a region from the surface of the steel sheet (the interface between the steel sheet and the plating layer in the case of a plated steel sheet) to a predetermined depth in the sheet thickness direction, and the "predetermined depth" is typically 50 μm or less.
[0050] As illustrated in FIG. 2, the steel sheet 11 according to the present invention contains fine oxides 12, coarse granular oxides 15, and grain boundary oxides 13 in the surface layer of the steel sheet 11. Preferably, the fine granular oxides 12, coarse granular oxides 15, and grain boundary oxides 13 are present only in the surface layer of the steel sheet 11. The fine granular oxides 12, coarse granular oxides 15, and grain boundary oxides 13 are present inside the base steel 14 (i.e., as internal oxides), which allows the steel sheet 11 to have high galvanic properties compared to the case in which the outer oxide layer 2 is present on the surface of the base steel 3 shown in FIG. 1. This is considered to occur because, when a plating (e.g., a Zn-based plating) is formed on the surface of the steel sheet, oxides that can inhibit interdiffusion between plating components and steel components are generated inside the steel sheet, not outside. Therefore, the steel sheet and plated steel sheet according to the present invention, which contain granular oxides and grain boundary oxides in the surface layer of the steel sheet, i.e., inside the steel sheet, have high galvanic properties.
[0051] 2, the surface layer of the steel sheet 11 according to the present invention includes a surface depleted layer in addition to the fine granular oxide 12, coarse granular oxide 15, and grain boundary oxide 13. This surface depleted layer is a region in which the elements of the steel composition around the fine granular oxide 12, coarse granular oxide 15, and grain boundary oxide 13 are depleted compared to the original steel sheet base material due to the formation of the fine granular oxide 12, coarse granular oxide 15, and grain boundary oxide 13, and exists so as to overlap with the region in which the fine granular oxide 12, coarse granular oxide 15, and grain boundary oxide 13 are distributed. In other words, the surface depleted layer exists inside the base steel 14, like the fine granular oxide 12, coarse granular oxide 15, and grain boundary oxide 13, and therefore the steel sheet and plated steel sheet including the fine granular oxide 12, coarse granular oxide 15, grain boundary oxide 13, and the surface depleted layer also have high galvanizability.
[0052] [Fine-grained oxide and coarse-grained oxide] In the present invention, the term "granular oxide" refers to oxides dispersed in a granular shape within steel crystal grains or on grain boundaries. In addition, "granular" refers to oxides that are present apart from one another in the steel matrix, and for example, refers to an aspect ratio (maximum line length (major axis) crossing the granular oxide / maximum line length (minor axis) crossing the oxide perpendicular to the major axis) of 1.0 to 5.0. "Dispersed in a granular shape" refers to oxide particles that are not arranged according to a specific rule (for example, linearly) but are arranged randomly. In reality, granular oxides are typically present three-dimensionally in a spherical or nearly spherical shape in the surface layer of the steel sheet, and therefore, when a cross section of the surface layer of the steel sheet is observed, the granular oxides are typically observed in a circular or nearly circular shape. In FIG. 2, a fine granular oxide 12 and a coarse granular oxide 15 that appear to be nearly circular are shown as examples. In Fig. 2, as a typical example of a steel sheet 11, a coarse granular oxide 15 is shown below a fine granular oxide 12. This is thought to be because the grain size of the granular oxide becomes larger and tends to grow more easily toward the inside of the steel sheet. Near the surface of the steel sheet, the diffusion rate of oxygen from the atmosphere into the inside of the steel sheet is fast, so the granular oxide is less likely to coarsen, whereas the diffusion rate of oxygen is slower as the distance from the surface of the steel sheet toward the inside of the steel sheet increases, so the granular oxide tends to coarsen. However, there are also cases where the coarse granular oxide 15 is formed near the surface of the base steel 14.
[0053] (particle size) In the present invention, the particle size of the granular oxide is 20 nm or more and 600 nm or less. Within this range, the particle size of the "fine" granular oxide is 20 nm or more and 100 nm or less, and the particle size of the "coarse" granular oxide is 150 nm or more and 600 nm or less. The reason for setting the upper limit of the particle size of the fine granular oxide (100 nm) and the lower limit of the particle size of the coarse granular oxide (150 nm) is to avoid a case where it becomes difficult to distinguish between fine granular oxide and coarse granular oxide from the viewpoint of measurement accuracy. By controlling the particle size within such a range, it is possible to disperse fine granular oxide and coarse granular oxide in the surface layer of the steel sheet, and the fine granular oxide and the coarse granular oxide function well as hydrogen trapping sites that suppress hydrogen penetration in a corrosive environment, and further function well as Zn trapping sites that may penetrate when a plated steel sheet having a plating layer formed on the steel sheet is subjected to hot stamp forming or welding processing. On the other hand, if the particle size exceeds 600 nm, the number of granular oxide particles may decrease, and the desired number density may not be obtained. The lower limit of the particle size of the granular oxide is 20 nm or more. The finer the granular oxide, the higher the specific surface area and the higher the reactivity as a trapping site, but the amount of hydrogen and / or Zn that can be trapped per particle decreases, and hydrogen and / or Zn cannot be sufficiently trapped, and the oxide may not function sufficiently as a hydrogen trapping site and / or a Zn trapping site.
[0054] (Number density of fine granular oxide) In the present invention, the number density of the fine granular oxide is 4.0 pieces / μm 2 That is all. By controlling the number density within this range, it is possible to disperse a large amount of fine granular oxides in the surface layer of the steel sheet, and the fine granular oxides function well as hydrogen trapping sites that suppress hydrogen penetration in a corrosive environment, and further function well as Zn trapping sites that can penetrate when a plated steel sheet having a plating layer formed on the steel sheet is subjected to hot stamp forming or welding. On the other hand, when the number density is 4.0 particles / μm 2If it is less than 1.0, the number density of hydrogen trapping sites and / or Zn trapping sites is insufficient, and the fine granular oxides do not function adequately as hydrogen trapping sites and / or Zn trapping sites, and there is a risk that good hydrogen embrittlement resistance and / or LME resistance cannot be obtained. In contrast, there is a risk that external oxidation is promoted and good plating properties cannot be obtained. The number density of the fine granular oxides is preferably 6.0 pieces / μm 2 More preferably, 8.0 particles / μm 2 More preferably, 10.0 particles / μm 2 The fine granular oxide is preferable in terms of functioning as a hydrogen trapping site and / or a Zn trapping site, but the granular oxide may become the starting point of LME cracking, and the fine granular oxide is preferable in terms of functioning as a hydrogen trapping site and / or a Zn trapping site ... may become the starting point of LME cracking, and the fine granular oxide may become the starting point of LME cracking, and the fine granular oxide may become the starting point of LME cracking. 2 Since there is a risk of the LME resistance decreasing if the number density of the fine granular oxide exceeds 100 particles / μm 2 Below, 90 pieces / μm 2 Below, 80 pieces / μm 2 Below, 70 pieces / μm 2 Below, 60 pieces / μm 2 Below, 50 pieces / μm 2 Below, 40 pieces / μm 2 Below, 30 pieces / μm 2 Below, 25 pieces / μm 2 Below, 20 pieces / μm 2 It may be the following.
[0055] The particle size and number density of the fine granular oxide are measured by a scanning electron microscope (SEM). The specific measurement is as follows. The cross section of the surface layer of the steel sheet is observed by SEM to obtain an SEM image containing the fine granular oxide. A total of 10 regions of 1.0 μm (depth direction) × 1.0 μm (width direction) are selected as observation regions from the SEM image. The observation position of each region is 1.0 μm from the steel sheet surface to 1.5 μm in the depth direction (direction perpendicular to the steel sheet surface), and 1.0 μm at any position in the above SEM image in the width direction (direction parallel to the steel sheet surface). Next, an SEM image of each of the regions selected as described above is extracted and binarized to separate the oxide portion from the steel portion. The area of the granular oxide portion is calculated from each binarized image, and the particle size (nm) of the granular oxide is calculated as the diameter of a circle having the same area as the calculated area, i.e., the circle equivalent diameter. Particles with a particle size in the range of 20 nm to 100 nm are defined as fine granular oxides. Furthermore, the number of fine granular oxides in each binarized image is counted. The average number of fine granular oxides in the total of the 10 regions thus calculated is taken as the number density of the fine granular oxides (particles / μm 2 In addition, when only a part of a granular oxide is observed in the observation area, that is, when the entire outline of a granular oxide is not within the observation area, it is not counted.
[0056] (Number density of coarse grain oxide) The number density of the coarse-grained oxide was 4.0 pieces / 25 μm. 2 That is all. By controlling the number density within this range, it is possible to disperse a large amount of coarse fine grain type oxides in the surface layer of the steel sheet, and the coarse grain type oxides function well as hydrogen trapping sites that suppress hydrogen penetration in a corrosive environment, and further function well as Zn trapping sites that can penetrate when a plated steel sheet having a plating layer formed on the steel sheet is subjected to hot stamp forming or welding. On the other hand, when the number density is 4.0 particles / 25 μm 2If it is less than 100 μm, the number density of hydrogen trapping sites and / or Zn trapping sites is insufficient, and the coarse grain type oxides do not function adequately as hydrogen trapping sites and / or Zn trapping sites, and there is a risk that good hydrogen embrittlement resistance and / or LME resistance cannot be obtained. In contrast, there is a risk that external oxidation is promoted and good plating properties cannot be obtained. The number density of the coarse grain type oxides is preferably 6.0 pieces / 25 μm 2 More preferably, 8.0 pieces / 25μm 2 More preferably, 10.0 pieces / 25 μm 2 The larger the amount of coarse grain oxide, the better from the viewpoint of functioning as a hydrogen trapping site and / or a Zn trapping site. However, the coarse grain oxide may become the starting point of LME cracking, and the number of 50 grains / 25 μm is not sufficient. 2 Since there is a risk of the LME resistance decreasing if the number density of the coarse grain type oxide exceeds 50 pieces / 25μm 2 Below, 40 pieces / 25μm 2 Below, 30 pieces / 25μm 2 Below, 25 pieces / 25μm 2 Below, 20 pieces / 25μm 2 It may be the following.
[0057] The particle size and number density of the coarse-grained oxides are measured by a scanning electron microscope (SEM). The specific measurement is as follows. The cross section of the surface layer of the steel sheet is observed by SEM to obtain an SEM image containing the coarse-grained oxides. A total of 10 regions of 5.0 μm (depth direction) × 5.0 μm (width direction) are selected as observation regions from the SEM image. The observation position of each region is 5.0 μm from the steel sheet surface to 8.0 μm in the depth direction (direction perpendicular to the steel sheet surface), and 5.0 μm at any position in the SEM image in the width direction (direction parallel to the steel sheet surface). Next, an SEM image of each of the regions selected as described above is extracted and binarized to separate the oxide portion from the steel portion. The area of the granular oxide portion is calculated from each binarized image, and the particle size (nm) of the granular oxide is calculated as the diameter of a circle having the same area as the calculated area, i.e., the circle equivalent diameter. Particles with a particle size in the range of 150 nm to 600 nm are defined as coarse granular oxides. Furthermore, the number of coarse granular oxides in each binarized image is counted. The average number of coarse granular oxides in the total of the 10 regions thus calculated is taken as the number density of the coarse granular oxides (particles / 25 μm 2 In addition, when only a part of a granular oxide is observed in the observation area, that is, when the entire outline of a granular oxide is not within the observation area, it is not counted.
[0058] [Grain boundary oxide] In the present invention, the term "granular oxide" refers to an oxide that exists along the grain boundaries of steel, and does not include oxides that exist within the grains of steel. In reality, the grain boundary oxide exists in a planar form along the grain boundaries in the surface layer of the steel sheet, so that when a cross section of the surface layer of the steel sheet is observed, the grain boundary oxide is observed in a linear form. In Figs. 2 and 3, a grain boundary oxide 13 that appears linear is shown as an example. In Figs. 2 and 3, the grain boundary oxide 13 is shown below the fine grain oxide 12 and the coarse grain oxide 15 as a typical example of the steel sheet 11, but the grain boundary oxide 13 may also be formed near the surface of the base steel 14.
[0059] (Ratio A) In the present invention, the "ratio A" refers to the ratio of "the length of the grain boundary oxide projected on the surface of the steel sheet: L (= L1 + L2 + L3 + L4)" to "the length of the surface of the steel sheet: L0" in the observed image when the cross section of the surface layer of the steel sheet 11 is observed as shown in FIG. 3. In the present invention, the ratio A is 50% or more and 100% or less. By controlling the ratio A within such a range, a large amount of grain boundary oxide 13 can be present in the surface layer of the steel sheet, and the grain boundary oxide 13 functions well as an escape route for hydrogen that has penetrated into the steel. On the other hand, if the ratio A is less than 50%, there is not a sufficient amount of grain boundary oxide 13 as an escape route for hydrogen, and the amount of hydrogen accumulation in the steel cannot be sufficiently reduced, and there is a risk that good hydrogen embrittlement resistance cannot be obtained. In comparison, external oxidation is promoted, and there is a risk that good platability cannot be obtained. The ratio A is preferably 60% or more, more preferably 70% or more, even more preferably 80% or more, still more preferably 90% or more, and most preferably 100%.
[0060] The ratio A is determined by observing a cross section of the surface layer of the steel sheet 11 as shown in FIG. 3. The specific measurement method is as follows. The cross section of the surface layer of the steel sheet 11 is observed by SEM. The observation position is a randomly selected position. The length L0 of the surface (i.e., the width of the SEM image) is measured from the observed SEM image. The length L0 is 100 μm or more (for example, 100 μm, 150 μm, or 200 μm), and the depth to be measured is a region from the surface of the steel sheet to 50 μm. Next, the position of the grain boundary oxide 13 is identified from the SEM image, and the identified grain boundary oxide 13 is projected onto the surface of the steel sheet 11 (on the interface between the steel sheet 11 and the plating layer in the case of a plated steel sheet), and the length L (= L1 + L2 + L3 + L4) of the grain boundary oxide 13 within the field of view is determined. Based on the L0 and L thus determined, the ratio A (%) = 100 × L / L0 in the present invention is determined. It should be noted that in FIG. 3, the fine grain oxide 12 and the coarse grain oxide 15 are omitted for the sake of explanation.
[0061] [Depth D] In the present invention, the "depth D" refers to the distance from the surface of the steel sheet 11 (the interface between the steel sheet and the plating layer in the case of a plated steel sheet) to the farthest position where the grain boundary oxide 13 exists, when proceeding from the surface of the steel sheet 11 (the interface between the steel sheet and the plating layer in the case of a plated steel sheet) in the sheet thickness direction of the steel sheet 11 (the direction perpendicular to the surface of the steel sheet), as shown in FIG. 3. As described above, the grain boundary oxide can function as an escape route for hydrogen that has penetrated into the steel sheet. Therefore, if the depth D of the grain boundary oxide is large, hydrogen can be released from a deeper position in the steel sheet to the outside of the system, and the above function is more preferably exerted. In the steel sheet according to the present invention, the depth D of the grain boundary oxide is preferably 3.0 μm or more, more preferably 5.0 μm or more, and even more preferably 7.0 μm or more. There is no particular limit to the upper limit of the depth D, but the depth D is substantially 50.0 μm or less. The depth D may be obtained from the same image as the SEM image (surface length L0) in which the above-mentioned ratio A is measured.
[0062] (depth of internal oxide layer) In the steel sheet according to the present invention, the internal oxide layer is a layer formed inside the steel sheet, and includes the fine granular oxide 12, the coarse granular oxide 15, and the grain boundary oxide 13. Therefore, the "internal oxide layer" is a continuous region from the surface of the steel sheet to the furthest position where any of the fine granular oxide 12, the coarse granular oxide 15, and the grain boundary oxide 13 exists. Therefore, the "depth of the internal oxide layer" refers to the distance from the surface of the steel sheet 11 to the furthest position where any of the fine granular oxide 12, the coarse granular oxide 15, and the grain boundary oxide 13 exists, when proceeding from the surface of the steel sheet 11 (the interface between the steel sheet and the coating layer in the case of a coated steel sheet) in the thickness direction of the steel sheet 11 (the direction perpendicular to the surface of the steel sheet), as shown as "Rn" in FIG. 2. However, the surface of an actual steel sheet is uneven, and the positions of the fine granular oxide 12, the coarse granular oxide 15, and the grain boundary oxide 13, which are the furthest from the steel sheet surface, vary depending on which location (point) on the steel sheet surface is selected. Therefore, 10 observation areas are selected, and the average value of the results measured at those 10 points is taken as the "average depth of the internal oxide layer" (sometimes referred to as "R"). FIG. 2 shows, as an example, a case in which the grain boundary oxide 13 is located at the deepest position. As described above, the fine granular oxide 12 and the coarse granular oxide 15 function as trap sites for hydrogen that penetrates in a corrosive environment, and the grain boundary oxide 13 can function as an escape route for hydrogen that has penetrated into the steel sheet. Therefore, the larger the average depth R of the internal oxide layer, the more hydrogen can be trapped in the surface region of the steel sheet, and the more hydrogen can be discharged outside the system. In the steel sheet according to the present invention, the lower limit of the average depth R of the internal oxide layer is not particularly limited, but if it is too shallow, the fine granular oxides 15, the coarse granular oxides 15, and the grain boundary oxides 13 may not be sufficiently dispersed, so that the lower limit is 8 μm or more, preferably 10 μm or more, more preferably 15 μm or more, and even more preferably 20 μm or more. The upper limit of the average depth R is not particularly limited, but is substantially 100 μm or less.
[0063] The depth R is determined by observing a cross section of the surface layer of the steel sheet 11, as shown in FIG. 2. The specific measurement method is as follows. The cross section of the surface layer of the steel sheet 11 is observed by SEM. Ten randomly selected observation positions are used. The length L0 of the surface (i.e., the width of the SEM image) is measured from the observed SEM image. The length L0 is 100 μm or more (e.g., 100 μm, 150 μm, or 200 μm), and the depth to be measured is the region from the surface of the steel sheet to 100 μm. Next, the positions of the fine granular oxide 12, the coarse granular oxide 15, and the grain boundary oxide 13 are identified from the SEM image, and one of the fine granular oxide 12, the coarse granular oxide 15, and the grain boundary oxide 13 that is located at the farthest position from the surface of the steel sheet is selected from the identified fine granular oxide 12, the coarse granular oxide 15, and the grain boundary oxide 13. The distance from the surface of the steel sheet 11 to the farthest position where the fine granular oxide 12, the coarse granular oxide 15, or the grain boundary oxide 13 is located is calculated as the depth Rn. The average value of Rn measured at 10 points is calculated as the "average depth of the internal oxide layer" (sometimes referred to as "R").
[0064] [Oxide composition] In the present invention, the granular oxide and the grain boundary oxide (hereinafter, simply referred to as oxide) contain, in addition to oxygen, one or more of the elements contained in the steel sheet described above, and typically have a composition containing Si, O, and Fe, and may further contain Mn and / or Al. The oxide may contain elements (e.g., Cr) that may be contained in the steel sheet described above.
[0065] [Surface depletion layer] In the present invention, the fine-grained oxides, the coarse-grained oxides and the grain boundary oxides are formed by the oxidation of relatively easily oxidized components (e.g., Si, Mn, Al) in the steel sheet, and therefore the composition of the steel (in other words, the metal structure) around the oxides is depleted in these easily oxidized component elements compared to the original base material of the steel sheet. This region where the elements of the steel composition are depleted compared to the original base material of the steel sheet is also called a "deficient region". The layered "deficient region" is also called a "deficient layer", and the one present in the surface layer of the steel sheet is also called a "surface depleted layer". In the depleted region, among the elements that are easily oxidized, Si is relatively easily oxidized and Al is relatively difficult to oxidize, so that Si can be present at a low concentration and Al at a high concentration. If the depleted region where the composition of the steel is low Si and high Al exists within a desired range, it also contributes to improving LME resistance. Although not wishing to be bound by a particular theory, the reason for this is thought to be that in addition to the granular oxides that function as Zn trap sites, the presence of Al in the composition of the steel surrounding the granular oxides and grain boundary oxides inhibits the intrusion of Zn into the grain boundaries of the steel during high-temperature processing, and since the higher the concentration of Si in the steel composition, the more likely LME cracking occurs, LME can be suppressed by keeping the concentration of Si as low as possible. As a result, the intrusion of Zn into the grain boundaries of the steel during hot stamp forming and welding is inhibited by Al in the steel composition, and the intrusion of Zn into the grain boundaries is suitably suppressed, and since the concentration of Si, which is prone to cause LME, is low, LME is less likely to occur, and LME resistance can be improved.
[0066] In the present invention, the surface depletion layer, which is low in Si and high in Al, satisfies, in mass %, Si≦0.6% and Al≧0.05% in the composition of the steel (in other words, metal structure) that does not contain fine granular oxides, coarse granular oxides, and grain boundary oxides at a depth of 1 / 2 the average depth of the internal oxide layer. If the Si content exceeds 0.6%, LME cracking is likely to occur. Therefore, Si≦0.6%. The lower limit of Si is not particularly limited and may be 0% or more. Furthermore, Al inhibits the penetration of Zn into the steel grain boundaries that attempt to penetrate into the steel during high-temperature processing. If the Al content is less than 0.05%, the penetration of Zn into the steel grain boundaries may not be sufficiently inhibited. Therefore, Al≧0.05%. The more Al, the higher the function of inhibiting the penetration of Zn into the steel grain boundaries is, which is preferable, but if the Al concentration is too high, the effect is saturated, so the upper limit of Al may be 1.2% or less or 1.0% or less. The Si and Al concentrations are those in a steel composition that does not include fine-grained oxides, coarse-grained oxides, and grain boundary oxides in the internal oxide layer, and are those measured at a depth that is half the average depth R of the internal oxide layer. The base point for the average depth of the internal oxide layer is the steel sheet surface (the interface between the steel sheet and the plating layer in the case of a plated steel sheet), but if these have irregularities, the base point is the average line of the 10 surfaces or interfaces where the average depth of the internal oxide layer was calculated. The element concentrations are measured by EDS (Energy Dispersed Spectroscopy).
[0067] The surface depleted layer may overlap with the region where fine-granular oxides, coarse-granular oxides and grain boundary oxides are distributed, and is present in the surface layer of the steel sheet, i.e., formed inside the base steel material. Therefore, when a coating layer is formed on the surface of the steel sheet, the steel sheet according to the present invention, which has a depleted region, more specifically a surface depleted layer, formed inside the base steel material, allows sufficient interdiffusion between the coating components and the steel components and enables high coating properties to be obtained, compared to a steel sheet having an outer oxide layer.
[0068] <Plated steel sheets> The plated steel sheet according to the present invention has a plating layer containing Zn on the above-mentioned steel sheet according to the present invention. This plating layer may be formed on one side or both sides of the steel sheet. Examples of the plating layer containing Zn include a hot-dip galvanized layer, a galvannealed hot-dip galvanized layer, an electric galvanized layer, and an electric alloy galvanized layer. More specifically, examples of the plating type that can be used include Zn-0.2%Al (GI), Zn-(0.3 to 1.5)%Al, Zn-4.5%Al, Zn-0.09%Al-10%Fe (GA), Zn-1.5%Al-1.5%Mg, Zn-11%Al-3%Mg-0.2%Si, Zn-11%Ni, and Zn-15%Mg.
[0069] [Composition of plating layer] The composition of the components contained in the Zn-containing plating layer of the present invention will be described. Unless otherwise specified, "%" regarding the content of an element means "mass%". In the numerical range of the composition of the plating layer, the numerical range expressed by "~" means a range including the numerical values written before and after "~" as the lower and upper limits, unless otherwise specified.
[0070] (Al: 0-60.0%) Since Al is an element that improves the corrosion resistance of the coating layer by being contained together with Zn or alloyed with Zn, it may be contained as necessary. Therefore, the Al content may be 0%. In order to form a coating layer containing Zn and Al, the Al content is preferably 0.01% or more, and may be, for example, 0.1% or more, 0.3% or more, 0.5% or more, 1.0% or more, or 3.0% or more. On the other hand, since the effect of improving the corrosion resistance is saturated when it exceeds 60.0%, the Al content is preferably 60.0% or less, and may be, for example, 55.0% or less, 50.0% or less, 40.0% or less, 30.0% or less, 20.0% or less, 10.0% or less, or 5.0% or less. Although the detailed mechanism is unknown, when the Al in the coating layer is in the range of 0.3 to 1.5%, the penetration speed of Zn into the steel grain boundary is significantly reduced due to the effect of Al, and it is possible to improve the LME resistance. Therefore, from the viewpoint of improving LME resistance, the Al content in the coating layer is preferably 0.3 to 1.5%.
[0071] (Mg: 0-15.0%) Mg is an element that improves the corrosion resistance of the plating layer by being contained together with Zn and Al or alloyed with them, so it may be contained as necessary. Therefore, the Mg content may be 0%. In order to form a plating layer containing Zn, Al, and Mg, the Mg content is preferably 0.01% or more, and may be, for example, 0.1% or more, 0.5% or more, 1.0% or more, or 3.0% or more. On the other hand, if it exceeds 15.0%, Mg does not completely dissolve in the plating bath and floats as an oxide, and when zinc plating is performed with this plating bath, the oxide adheres to the plating surface layer, causing poor appearance, or there is a risk of non-plated parts occurring, so the Mg content is preferably 15.0% or less, and may be, for example, 10.0% or less, 5.0% or less.
[0072] (Fe: 0-15.0%) When a Zn-containing plating layer is formed on a steel sheet and then the plated steel sheet is heat-treated, Fe can be diffused from the steel sheet and contained in the plating layer. Therefore, in a state where no heat treatment is performed, Fe is not contained in the plating layer, and the Fe content may be 0%. The Fe content may be 1.0% or more, 2.0% or more, 3.0% or more, 4.0% or more, or 5.0% or more. On the other hand, the Fe content may be 15.0% or less, and may be, for example, 12.0% or less, 10.0% or less, 8.0% or less, or 6.0% or less.
[0073] (Si: 0-3.0%) Since Si is an element that further improves corrosion resistance when contained in a Zn-containing plating layer, particularly a Zn-Al-Mg plating layer, it may be contained as necessary. Therefore, the Si content may be 0%. From the viewpoint of improving corrosion resistance, the Si content may be, for example, 0.005% or more, 0.01% or more, 0.05% or more, 0.1% or more, or 0.5% or more. In addition, the Si content may be 3.0% or less, 2.5% or less, 2.0% or less, 1.5% or less, or 1.2% or less.
[0074] The basic composition of the plating layer is as described above. Furthermore, the plating layer may optionally contain one or more of Sb: 0-0.50%, Pb: 0-0.50%, Cu: 0-1.00%, Sn: 0-1.00%, Ti: 0-1.00%, Sr: 0-0.50%, Cr: 0-1.00%, Ni: 0-1.00%, and Mn: 0-1.00%. Although not particularly limited, from the viewpoint of fully exerting the action and function of the above basic components constituting the plating layer, the total content of these optional added elements is preferably 5.00% or less, more preferably 2.00% or less.
[0075] The remainder of the plating layer other than the above components is composed of Zn and impurities. The impurities in the plating layer refer to components that are mixed in due to various factors in the manufacturing process, including raw materials, when the plating layer is manufactured, and are not components that are intentionally added to the plating layer. The plating layer may contain trace amounts of elements other than the basic components and optional added components described above as impurities within a range that does not impair the effects of the present invention.
[0076] The component composition of the plating layer can be determined by dissolving the plating layer in an acid solution containing an inhibitor that suppresses corrosion of the steel sheet, and measuring the resulting solution by ICP (inductively coupled plasma) emission spectroscopy.
[0077] The thickness of the plating layer may be, for example, 3 to 50 μm. The coating weight of the plating layer is not particularly limited, but is, for example, 10 to 170 g / m per side. 2 In the present invention, the coating weight of the plating layer is determined by dissolving the plating layer in an acid solution to which an inhibitor that suppresses corrosion of the base steel has been added, and measuring the change in weight before and after dissolution of the plating.
[0078] [Tensile strength] The steel sheet and plated steel sheet according to the present invention preferably have high strength, specifically, a tensile strength of 440 MPa or more. For example, the tensile strength may be 500 MPa or more, 600 MPa or more, 700 MPa or more, or 800 MPa or more. The upper limit of the tensile strength is not particularly limited, but may be, for example, 2000 MPa or less from the viewpoint of ensuring toughness. The tensile strength may be measured in accordance with JIS Z 2241 (2011) by taking a JIS No. 5 tensile test piece with the longitudinal direction perpendicular to the rolling direction.
[0079] The steel sheet and plated steel sheet according to the present invention have high strength and high galvanizability, LME resistance, and hydrogen embrittlement resistance, and therefore can be suitably used in a wide range of fields such as automobiles, home appliances, and building materials, but are particularly preferably used in the automobile field. Steel sheets used for automobiles are usually plated (typically Zn-based plating), so when the steel sheet according to the present invention is used as an automobile steel sheet, the effect of the present invention of having high galvanizability is suitably exhibited. Furthermore, steel sheets and plated steel sheets used for automobiles are often hot stamped, in which case hydrogen embrittlement cracking and LME cracking can become significant problems. Therefore, when the steel sheet and plated steel sheet according to the present invention are used as an automobile steel sheet, the effect of the present invention of having high hydrogen embrittlement resistance and LME resistance is suitably exhibited.
[0080] <Steel sheet manufacturing method> A preferred method for producing the steel plate according to the present invention will be described below. The following description is intended to exemplify a characteristic method for producing the steel plate according to the present invention, and is not intended to limit the steel plate to one produced by the production method described below.
[0081] The steel sheet according to the present invention can be obtained, for example, by carrying out a casting process in which molten steel with an adjusted composition is cast to form a steel slab, a hot rolling process in which the steel slab is hot rolled to obtain a hot rolled steel sheet, a coiling process in which the hot rolled steel sheet is coiled, a cold rolling process in which the coiled hot rolled steel sheet is cold rolled to obtain a cold rolled steel sheet, a pretreatment process in which the cold rolled steel sheet is brush ground, and an annealing process in which the pretreated cold rolled steel sheet is annealed. Alternatively, the cold rolling process may be carried out directly after the hot rolling process without coiling, after which the cold rolling process is carried out after pickling.
[0082] [Casting process] The conditions for the casting process are not particularly limited. For example, after melting in a blast furnace or an electric furnace, various secondary smelting processes may be carried out, and then casting may be carried out by a method such as ordinary continuous casting or casting by an ingot method.
[0083] [Hot rolling process] The cast steel slab as described above can be hot-rolled to obtain a hot-rolled steel sheet. The hot rolling step is performed by hot-rolling the cast steel slab directly or after cooling it once and then reheating it. When reheating is performed, the heating temperature of the steel slab may be, for example, 1100°C to 1250°C. In the hot rolling step, rough rolling and finish rolling are usually performed. The temperature and reduction of each rolling step may be appropriately changed depending on the desired metal structure and plate thickness. For example, the finishing temperature of the finish rolling may be 900 to 1050°C, and the reduction of the finish rolling may be 10 to 50%.
[0084] [Winding process] The hot-rolled steel sheet can be coiled at a predetermined temperature. The coiling temperature may be appropriately changed depending on the desired metal structure, etc., and may be, for example, 500 to 800°C. The hot-rolled steel sheet may be recoiled before or after coiling and subjected to a predetermined heat treatment. Alternatively, the coiling step may be omitted, and the hot-rolled steel sheet may be pickled after the hot-rolling step and then subjected to the cold-rolling step described below.
[0085] [Cold rolling process] After the hot-rolled steel sheet is subjected to pickling or the like, the hot-rolled steel sheet is cold-rolled to obtain a cold-rolled steel sheet. The rolling reduction in the cold rolling may be appropriately changed depending on the desired metal structure and sheet thickness, and may be, for example, 20 to 80%. After the cold rolling process, the steel sheet may be cooled to room temperature, for example, by air cooling.
[0086] [Pretreatment process] In order to obtain a large amount of fine granular oxide, coarse granular oxide and grain boundary oxide in the surface layer of the finally obtained steel sheet, and further to obtain a surface depleted layer, it is effective to perform a predetermined pretreatment process before annealing the cold-rolled steel sheet. The pretreatment process introduces a large amount of dislocations into the surface of the cold-rolled steel sheet. Since oxygen and the like diffuse faster at grain boundaries than in grains, introducing a large amount of dislocations into the surface of the cold-rolled steel sheet can form many paths as in the case of grain boundaries. Therefore, oxygen is more likely to diffuse (penetrate) into the inside of the steel along these dislocations during annealing, and the diffusion rate of Si and Al is also improved, so that it is possible to promote the formation of fine granular oxide, coarse granular oxide and grain boundary oxide by oxygen bonding with Si and / or Al inside the steel. In addition, the promotion of the formation of such internal oxides also promotes the reduction of the surrounding Si and Al concentrations, so that the formation of a surface depleted layer having a desired composition can also be promoted. Therefore, when such a pretreatment step is performed, the desired fine granular oxide, coarse granular oxide, grain boundary oxide, and surface depletion layer are easily formed in the annealing step described later. The pretreatment step includes grinding the surface of the cold-rolled steel sheet with a heavy-duty grinding brush (brush grinding treatment). As the heavy-duty grinding brush, D-100 manufactured by HOTANI CORP. may be used. When grinding, it is preferable to apply a 1.0 to 5.0% NaOH aqueous solution to the steel sheet surface. The brush reduction is preferably 0.5 to 10.0 mm, more preferably 5.0 to 10.0 mm, and the rotation speed is preferably 100 to 1000 rpm. By performing the brush grinding treatment under such conditions of the coating solution, brush reduction, and rotation speed, it is possible to efficiently form the fine granular oxide, coarse granular oxide, grain boundary oxide, and surface depletion layer on the surface layer of the steel sheet in the annealing step described later.
[0087] [Annealing process] The cold-rolled steel sheet that has been subjected to the above pretreatment step is then annealed. The annealing is preferably performed under tension of, for example, 0.1 to 30.0 MPa. Applying tension during annealing makes it possible to more effectively introduce strain into the steel sheet, which in turn promotes dislocations in the metal structure of the steel sheet, and oxygen easily penetrates into the steel along the dislocations, which makes it easier for oxides to be generated inside the steel sheet. As a result, this is advantageous for increasing the number density of granular oxides, increasing the ratio of grain boundary oxides, and forming a surface depleted layer.
[0088] From the viewpoint of generating a large amount of granular oxides of a desired size and a large amount of grain boundary oxides, the holding temperature in the annealing step is preferably 750°C to 900°C. If the holding temperature in the annealing step is less than 750°C, the grain boundary oxides may not be generated in a sufficient amount, and the hydrogen embrittlement resistance may be insufficient. On the other hand, if the holding temperature in the annealing step is more than 900°C, the granular oxides may become coarse, and the desired granular oxides, grain boundary oxides and / or surface depletion layer may not be obtained, and the hydrogen embrittlement resistance and / or LME resistance may be insufficient. The heating rate to the above holding temperature is not particularly limited, but may be 1 to 10°C / sec. The heating may be performed in two stages, with a first heating rate of 1 to 10°C / sec and a second heating rate of 1 to 10°C / sec different from the first heating rate.
[0089] The holding time at the holding temperature in the annealing step is preferably 50 to 300 seconds, more preferably 55 to 120 seconds. If the holding time is less than 50 seconds, there is a risk that a sufficiently large amount of granular oxides and / or grain boundary oxides are not generated, and the LME resistance and / or hydrogen embrittlement resistance may be insufficient. On the other hand, if the holding time is more than 300 seconds, there is a risk that external oxidation proceeds while internal oxidation does not proceed, and the platability, hydrogen embrittlement resistance and / or LME resistance may be insufficient.
[0090] During the temperature increase and holding (isothermal) in the annealing process, humidification is performed from the viewpoint of generating the desired fine granular oxide, coarse granular oxide, grain boundary oxide, and surface depletion layer. The atmosphere has a dew point of -20 to 10°C, preferably -10 to 5°C, and 1 to 15 vol% H2. If the dew point is too low, an outer oxide layer may be formed on the surface of the steel sheet, and an inner oxide layer may not be sufficiently formed, resulting in insufficient galvanization, hydrogen embrittlement resistance, and LME resistance. On the other hand, if the dew point is too high, the granular oxide may become coarse, and the desired granular oxide, grain boundary oxide, and / or surface depletion layer may not be obtained.
[0091] The temperature at which humidification is started during the temperature rise is preferably less than 600° C. If humidification is started at a temperature exceeding 600° C., the internal oxide layer and / or the surface depletion layer may not be sufficiently formed before the holding temperature is reached.
[0092] Furthermore, when performing the annealing process, it is effective to remove the internal oxide layer of the steel sheet, particularly before the brush grinding process. An internal oxide layer may be formed on the surface layer of the steel sheet during the above-mentioned rolling process, particularly the hot rolling process. Since such an internal oxide layer formed in the rolling process may hinder the formation of fine-grained oxides, coarse-grained oxides, grain boundary oxides and / or surface depletion layers in the annealing process and may promote the formation of an external oxide layer, it is preferable to remove the internal oxide layer by pickling or the like before annealing. More specifically, the depth of the internal oxide layer of the cold-rolled steel sheet when performing the annealing process is preferably 0.5 μm or less, preferably 0.3 μm or less, more preferably 0.2 μm or less, and even more preferably 0.1 μm or less.
[0093] By carrying out the above-mentioned steps, it is possible to obtain a steel sheet having a surface depleted layer formed and containing sufficiently large amounts of granular oxides and grain boundary oxides in the surface layer of the steel sheet.
[0094] <Method of manufacturing plated steel sheets> A preferred method for producing the plated steel sheet according to the present invention will be described below. The following description is intended to exemplify a characteristic method for producing the plated steel sheet according to the present invention, but is not intended to limit the plated steel sheet to one produced by the production method described below.
[0095] The plated steel sheet according to the present invention can be obtained by carrying out a plating treatment step of forming a plating layer containing Zn on the steel sheet produced as described above.
[0096] [Plating process] The plating process may be carried out according to a method known to those skilled in the art. The plating process may be carried out, for example, by hot-dip plating or by electroplating. Preferably, the plating process is carried out by hot-dip plating. The conditions of the plating process may be appropriately set in consideration of the component composition, thickness, and coating weight of the desired plating layer. After the plating process, an alloying process may be carried out. Typically, the conditions of the plating process may be set so as to form a plating layer containing Al: 0-60.0%, Mg: 0-15.0%, Fe: 0-15%, Ni: 0-20%, and Si: 0-3%, with the balance being Zn and impurities. More specifically, the conditions of the plating process may be appropriately set to form, for example, Zn-0.2%Al (GI), Zn-0.8%Al, Zn-4.5%Al, Zn-0.09%Al-10%Fe (GA), Zn-1.5%Al-1.5%Mg, or Zn-11%Al-3%Mg-0.2%Si, Zn-11%Ni, or Zn-15%Mg. From the viewpoint of improving LME resistance, the Al content in the plating layer is preferably 0.3 to 1.5%. EXAMPLES
[0097] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples in any way.
[0098] Example 1: Examples and comparative examples of steel sheets (Preparation of steel plate samples) The molten steel with the adjusted composition was cast to form a steel slab, which was hot-rolled, pickled, and then cold-rolled to obtain a cold-rolled steel sheet. The cold-rolled steel sheet was then air-cooled to room temperature, and pickled to remove the internal oxide layer formed by rolling to the depth (μm) of the internal oxide layer before annealing shown in Table 1. Samples were then taken from each cold-rolled steel sheet according to a method conforming to JIS G0417:1999, and the composition of the steel sheet was analyzed by ICP-MS or the like. The measured composition of the steel sheet is shown in Table 1. The thickness of all the steel sheets used was 1.6 mm.
[0099] Next, a 2.0% aqueous solution of NaOH was applied to some of the cold-rolled steel sheets, and a pretreatment was performed by brush grinding using a heavy-duty grinding brush (D-100 manufactured by Hotani Co., Ltd.) at a brush reduction of 2.0 mm and a rotation speed of 600 rpm. Thereafter, annealing was performed at the dew point, holding temperature, and holding time shown in Table 1 to prepare each steel sheet sample. In all steel sheet samples, the heating rate during annealing was 6.0°C / sec up to 500°C, and 2.0°C / sec from 500°C to the holding temperature. In the above annealing treatment, some of the cold-rolled steel sheets were annealed under a tension of 30.0 MPa, and the other cold-rolled steel sheets were annealed without tension. Table 1 shows the presence or absence of pretreatment and the conditions of the annealing treatment (with or without tension, humidification zone, dew point (°C), hydrogen concentration (vol%), humidification start temperature (°C) in the heating process, holding temperature (°C), and holding time (sec)). For each steel plate sample, a JIS No. 5 tensile test piece was taken with the longitudinal direction perpendicular to the rolling direction, and a tensile test was conducted in accordance with JIS Z 2241 (2011). As a result, the tensile strength of No. 1 was less than 440 MPa, and the rest were 440 MPa or more.
[0100] (Analysis of the surface layer of steel plate samples: Number density of fine granular oxide) Each steel plate sample prepared as described above was cut into 25 mm x 15 mm, the cut samples were embedded in resin and mirror polished, and 10 areas of 1.0 μm x 1.0 μm were observed on the cross section of each steel plate sample by SEM. The observation positions were 1.0 μm from the steel plate surface in the depth direction (direction perpendicular to the surface of the steel plate) to 0.2 to 1.2 μm, and 1.0 μm at any position on the SEM image in the width direction (direction parallel to the surface of the steel plate). The SEM images of each region of each obtained steel plate sample were binarized, the area of the granular oxide portion was calculated from the binarized image, and the particle size (nm) of the granular oxide was calculated as the diameter of a circle having an area equal to the area, i.e., the circle equivalent diameter, and those within the particle size range of 20 to 100 nm were defined as fine granular oxides. Furthermore, the number of fine granular oxides in the SEM image was counted. The average number of fine granular oxide particles in the binarized images at 10 locations thus obtained was taken as the number density of fine granular oxide particles. 2 ) are shown in Table 1.
[0101] (Analysis of the surface layer of steel plate samples: Number density of coarse-grained oxide) Each steel plate sample prepared as described above was cut into 25 mm x 15 mm, the cut samples were embedded in resin and mirror polished, and 10 areas of 5.0 μm x 5.0 μm were observed on the cross section of each steel plate sample by SEM. The observation positions were 5.0 μm from the steel plate surface in the depth direction (direction perpendicular to the surface of the steel plate) to 0.2 to 8.0 μm, and in the width direction (direction parallel to the surface of the steel plate), 5.0 μm at any position on the SEM image. The SEM images of each region of each steel plate sample obtained were binarized, the area of the granular oxide portion was calculated from the binarized image, and the particle diameter (nm) of the granular oxide was calculated as the diameter of a circle having an area equal to the area, i.e., the circle equivalent diameter, and those within the particle diameter range of 150 to 600 nm were regarded as coarse granular oxides. Furthermore, the number of fine granular oxides in the SEM images was counted. The average number of coarse granular oxide particles in the binarized images at 10 locations thus obtained was taken as the number density of the coarse granular oxide particles. 2 ) are shown in Table 1.
[0102] (Analysis of the surface layer of steel plate sample: ratio A of grain boundary type oxide) In addition, the ratio A of each steel sheet sample was measured from the cross-sectional observation of the embedded sample. Specifically, the position of the grain boundary oxide was identified in a 150 μm wide (= L0) SEM image, the identified grain boundary oxide was projected onto the surface of the steel sheet, and the length L of the grain boundary oxide within the field of view was determined. Based on the L0 and L thus determined, the ratio A (%) = 100 × L / L0 was calculated. The ratio A (%) of the granular oxide for each steel sheet sample is shown in Table 1. In addition, the depth D of the identified grain boundary oxide was measured from the same SEM image.
[0103] (Analysis of the surface layer of steel plate samples: surface depletion layer) In order to evaluate the surface depletion layer of each steel sheet sample, the composition of the steel structure that does not contain oxides was analyzed at a depth of half the average depth of the internal oxide layer calculated from the cross-sectional SEM image of the steel sheet using TEM-EDS. The cases where Si≦0.6% and Al≧0.05% were satisfied were marked with "○", and the cases where Si≦0.6% and Al≧0.05% were not satisfied were marked with "×".
[0104] (Platability evaluation) Each steel sheet sample was plated, and the area ratio of the unplated part on the surface of the plated steel sheet was measured to evaluate the plateability. Specifically, a 1 mm × 1 mm area on the surface of each plated steel sheet sample on which a plated layer was formed was observed under an optical microscope after being plated with hot-dip Zn-0.2% Al (bath temperature 450 to 470°C). The observed image was used to distinguish between the part on which the plated layer was formed (plated part) and the part on which the plated layer was not formed (unplated part), and the area ratio of the unplated part (area of the unplated part / area of the observed image) was calculated to evaluate the plateability according to the following criteria. The results are shown in Table 1. Grade A: Area ratio of plated area is 95% or more (area ratio of unplated area is 5.0% or less) Grade B: Area ratio of plated area is 90% or more but less than 95% (area ratio of unplated area is 5.0% or more but less than 10%)
[0105] (Composition analysis of plating layer) The composition of the plating layer was determined by immersing a sample cut to 30 mm x 30 mm in a 10% hydrochloric acid solution containing an inhibitor (Ibit, manufactured by Asahi Chemical Industry Co., Ltd.), pickling the plating layer to remove it, and then performing ICP analysis of the plating components dissolved in the solution.
[0106] (LME resistance evaluation) Each 100×100 mm plated steel sheet sample was subjected to spot welding. Two pieces were prepared by cutting into a size of 50 mm×100 mm, and the two Zn-based plated steel sheet samples were spot-welded using a dome radius type welding electrode with a tip diameter of 8 mm at an impact angle of 3°, a pressure of 3.5 kN, a clearance of 0.3 mm, a current time of 0.5 seconds (20 cycles, power frequency of 50 Hz), and a current of 7 kA to obtain welded members. The welded parts were polished in cross section, and then observed with an optical microscope to measure the length of the LME cracks that occurred in the cross section of the welded parts, and evaluated as follows. The results are shown in Table 1. All plating types in Table 1 were GA, and the plating types in Table 2 were as shown in Table 2. Rating AAA: No LME cracks Rating AA: LME crack length 0μm to 100μm Rating A: LME crack length over 100μm to 200μm Rating B: LME crack length over 200 μm
[0107] (Evaluation of hydrogen embrittlement resistance) Each plated steel sheet sample of 50mm x 100mm was treated with zinc phosphate using a zinc phosphate-based chemical conversion treatment solution (Surfdyne SD5350 series: manufactured by Nippon Paint Industrial Coating Co., Ltd.), and then electrocoated (PN110 Powernics Gray: manufactured by Nippon Paint Industrial Coating Co., Ltd.) to a thickness of 20μm, and baked at a baking temperature of 150℃ for 20 minutes to form a coating film on the plated steel sheet sample. The sample was then cut to 30 x 100mm to expose the iron end surface. After that, the sample was subjected to a complex cyclic corrosion test according to JASO (M609-91) while being subjected to a stress load using a bending jig so that the stress of the bent part was 800MPa. Hydrogen embrittlement resistance was evaluated according to the following criteria, and the results are shown in Table 1. Rating AA: No cracks up to 230 cycles Rating A: Cracks occur within 140 to 230 cycles Rating B: Cracks occur within 140 cycles
[0108] [Table 1]
[0109] Example 2: Examples and comparative examples of plated steel sheets (Preparation of plated steel sheet samples) Each steel sheet sample of Example 1 was cut to a size of 100 mm × 200 mm, and then a plating process was carried out to form the plating types shown in Table 2, thereby producing plated steel sheet samples of Example 2. In Table 2, plating type a means "galvannealed steel sheet (GA)", plating type b means "hot-dip Zn-0.2% Al plated steel sheet (GI)", and plating type c means "hot-dip Zn-(0.3-1.5)% Al plated steel sheet (Al content is shown in Table 2)". In the hot-dip galvanizing process, the cut samples were immersed in a hot-dip galvanizing bath at 440°C for 3 seconds. After immersion, the samples were pulled out at 100 mm / s, and the coating weight was reduced to 50 g / m by N2 wiping gas. 2 For plating type a, alloying treatment was then carried out at 500°C.
[0110] For the plated steel sheet samples obtained for Example 2, the evaluation items, i.e., the number density of fine granular oxides and coarse granular oxides, the ratio A of grain boundary oxides, the surface depletion layer, and galvanizability, were evaluated using the same evaluation methods as in Example 1, except for hydrogen embrittlement resistance, and it was confirmed that results equivalent to those of Example 1 were obtained. The tensile strength was slightly reduced by the plating treatment in some cases, but as in Example 1, the tensile strength of No. 1 was less than 440 MPa, and the other samples were 440 MPa or more. Regarding LME resistance, when the Al content of plating type c was 0.3 to 1.5 mass%, LME resistance was improved. The results are shown in Table 2.
[0111] (Evaluation of hydrogen embrittlement resistance of plated steel sheets) Each plated steel sheet sample of 50mm x 100mm was treated with zinc phosphate using a zinc phosphate-based chemical conversion treatment solution (Surfdyne SD5350 series: manufactured by Nippon Paint Industrial Coating Co., Ltd.), and then electrocoated (PN110 Powernics Gray: manufactured by Nippon Paint Industrial Coating Co., Ltd.) to a thickness of 20μm. The plated steel sheet sample was baked at a baking temperature of 150℃ for 20 minutes to form a coating film on the plated steel sheet sample. The sample was then cut to 30 x 100mm to expose the iron end surface. The sample was then subjected to a cyclic corrosion test according to JASO (M609-91) while being subjected to a stress load of 800MPa using a bending jig. Hydrogen embrittlement resistance was evaluated according to the following criteria, and the results are shown in Table 2. Rating AA: No cracks up to 180 cycles Rating A: Cracks occur within 90 to 180 cycles Rating B: Cracks occur within 90 cycles
[0112] [Table 2]
[0113] In this example, a high-strength steel sheet or plated steel sheet having a tensile strength of 440 MPa or more, a grade of A for galvanizability, a grade of AA or A for hydrogen embrittlement resistance, and a grade of AAA, AA, or A for LME resistance was evaluated as having high galvanizability, hydrogen embrittlement resistance, and LME resistance. Throughout Examples 1 and 2, Samples Nos. 2 to 8 and 23 to 36 had high galvanizability, LME resistance, and hydrogen embrittlement resistance because the steel sheet composition, the number density of fine granular oxides and coarse granular oxides, the ratio A of grain boundary oxides, and the surface depleted layer all satisfied the ranges of the present invention. Sample No. 1 had an insufficient C content, and therefore not only was it unable to obtain sufficient strength, but it was also unable to obtain the desired fine granular oxides, coarse granular oxides, grain boundary oxides, and surface depleted layer, and therefore did not obtain high galvanizability, hydrogen embrittlement resistance, and LME resistance. In sample No. 9, the dew point during annealing was low, and an internal oxide layer was not formed sufficiently, and an external oxide layer was formed, so high galvanic properties, hydrogen embrittlement resistance, and LME resistance were not obtained. In sample No. 10, the dew point during annealing was high, and the granular oxides became coarse, and the desired granular oxides and grain boundary oxides were not obtained, so high galvanic properties, hydrogen embrittlement resistance, and LME resistance were not obtained. In sample No. 11, the holding temperature during annealing was high, and the granular oxides became coarse, and the desired granular oxides and grain boundary oxides were not obtained, so high hydrogen embrittlement resistance and LME resistance were not obtained. In sample No. 12, the holding temperature during annealing was low, and a grain boundary oxide layer was not formed sufficiently, so high hydrogen embrittlement resistance was not obtained. In sample No. 13, the holding time during annealing was short, and a grain boundary oxide layer was not formed sufficiently, so high hydrogen embrittlement resistance was not obtained. Sample No. 14 had a long holding time during annealing, so an internal oxide layer was not formed sufficiently, but an external oxide layer was formed, and high galvanizability, hydrogen embrittlement resistance, and LME resistance were not obtained. Samples No. 15 and No. 17 had excessive amounts of Si and Mn, so the desired internal oxide layer was not formed, but an external oxide layer was formed, and high galvanizability, hydrogen embrittlement resistance, and LME resistance were not obtained. Samples No. 16 and No. 18 had insufficient amounts of Si and Mn, so an internal oxide layer was not formed sufficiently, but an external oxide layer was formed, and high galvanizability, hydrogen embrittlement resistance, and LME resistance were not obtained.In sample No. 19, the amount of Al was excessive, and the internal oxide layer was not sufficiently formed, but the external oxide layer was formed, so high galvanizability, hydrogen embrittlement resistance, and LME resistance were not obtained. In sample No. 20, the amount of Al was insufficient, and the surface depletion layer and internal oxide layer were not sufficiently formed, so high hydrogen embrittlement resistance and LME resistance were not obtained. In sample No. 21, humidification was performed only during the annealing temperature rise, and the humidification time was short, so the coarse grain type oxide and grain boundary type oxide layers were not sufficiently formed, and high hydrogen embrittlement resistance and LME resistance were not obtained. In sample No. 22, the internal oxide layer was thick before annealing, and the internal oxide layer was not sufficiently formed after annealing, and the external oxide layer was formed, so high galvanizability, hydrogen embrittlement resistance, and LME resistance were not obtained. In sample No. 37, tension was not applied to the steel sheet during annealing, so the internal oxide layer was not sufficiently formed, and high hydrogen embrittlement resistance and LME resistance were not obtained. Sample No. 38 did not undergo brush grinding before annealing, so an adequate internal oxide layer was not formed, and high hydrogen embrittlement resistance and LME resistance were not obtained. Sample No. 39 had a humidification start temperature of 600°C or higher, so an adequate internal oxide layer was not formed, and an external oxide layer was formed, and high plateability, hydrogen embrittlement resistance, and LME resistance were not obtained.
[0114] In the examples of the invention, fine-grained oxides, coarse-grained oxides and grain boundary oxide layers were confirmed at a predetermined number density or ratio, and it was also confirmed by EDS that a predetermined surface depleted layer was obtained. Therefore, high galvanizability, hydrogen embrittlement resistance and LME resistance were obtained. On the other hand, in the comparative examples, an internal oxide layer and / or a surface depleted layer was not properly formed near the steel sheet surface. Therefore, at least one of the following was confirmed: poor galvanizability, penetration of a large amount of hydrogen, and poor LME resistance. [Industrial Applicability]
[0115] According to the present invention, it is possible to provide a high-strength steel sheet and plated steel sheet having high galvanizability, LME resistance and hydrogen embrittlement resistance, and the steel sheet and plated steel sheet can be suitably used for applications such as automobiles, home appliances, building materials, and the like, particularly for automobiles, and are expected to have high collision safety and long life as automotive steel sheets and automotive plated steel sheets. Therefore, the present invention can be said to be an invention of extremely high industrial value. [Explanation of symbols]
[0116] 1 steel plate 2. Outer oxide layer 3 Base steel 11 Steel plate 12 Fine granular oxide 13 Intergranular oxides 14 Base steel 15 Coarse grained oxide
Claims
1. In mass percent, C: 0.05-0.40%, Si: 0.2-3.0%, Mn: 0.1 to 5.0%, sol. Al: 0.4 to 1.50%, P: 0.0300% or less, S: 0.0300% or less, N: 0.0100% or less, B: 0 to 0.010%, Ti: 0 to 0.150%, Nb: 0 to 0.150%, V: 0 to 0.150%, Cr: 0-2.00%, Ni: 0-2.00%, Cu: 0-2.00%, Mo: 0-1.00%, W: 0-1.00%, Ca: 0-0.100%, Mg: 0-0.100%, Zr: 0 to 0.100%, Hf: 0 to 0.100%, and A steel sheet having a composition containing REM: 0 to 0.100%, with the balance being Fe and impurities, The steel sheet has an internal oxide layer on the surface thereof, the internal oxide layer including a fine granular oxide, a coarse granular oxide, and a grain boundary oxide, When observing a cross section of the surface layer of the steel plate, The number density of the fine granular oxide in the internal oxide layer is 4.0 particles / μm 2 That's all. The number density of the coarse grain oxide in the internal oxide layer is 4.0 grains / 25 μm 2 That's all. a ratio A of a length of the grain boundary oxide projected onto the surface of the steel sheet to a length of the surface of the steel sheet is 50% or more and 100% or less, a steel plate including a surface depleted layer, the surface depleted layer having a steel composition, at a depth half the average depth of the internal oxide layer, that does not include the fine granular oxides, the coarse granular oxides, and the grain boundary oxides and that satisfies, in mass%, Si≦0.6% and Al≧0.05%.
2. The number density of the fine grain oxide is 4.0 to 30 grains / μm 2 The steel sheet according to claim 1 .
3. A plated steel sheet having a plating layer containing Zn on the steel sheet according to claim 1 or 2.
4. 4. The Zn-plated steel sheet according to claim 3, wherein the Al content in the plating layer is 0.3 to 1.5 mass %.
Citation Information
Patent Citations
Hot-dip galvannealed steel sheet and method for producing the same
JP2011117040A
High-strength hot-dip galvanized steel plate and method for manufacturing the same
JP2011219779A
High-strength plated steel sheet, as well as method for producing the same
JP2016130357A
High strength plating steel sheet excellent in plating property, processability and delayed fracture resistance, and manufacturing method therefor
JP2018193614A
Method for producing high-strength hot-dip galvanized steel sheet, and high-strength hot-dip galvanized steel sheet