Structural member design method, steel plate manufacturing method, tailored blank manufacturing method, structural member manufacturing method, and structural member
By selectively removing aluminum plating and intermetallic compound layers in high-risk fracture areas through numerical simulation, the method addresses the inefficiencies of existing methods, improving structural integrity and tool life in tailored blanks for hot stamping.
Patent Information
- Application Number
- JP2023540383
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-08-03
- Filing Date
- 2022-08-03
- Publication Date
- 2024-10-09
- Estimated Expiration
- 2042-08-03
AI Technical Summary
Existing methods for removing aluminum plating in tailored blanks for hot stamping take too much time and reduce the strength of welded portions, leading to potential breakage and reduced tool life.
A method for designing structural members that involves performing numerical simulation to identify high-risk fracture areas and selectively removing the aluminum plating and intermetallic compound layers only in these areas, while maintaining the strength of the welded portions by exposing the base steel plate.
This approach reduces the time required for plating removal, enhances the structural integrity of the welded portions, and extends tool life by maintaining strength in high-load regions.
Smart Images

Figure 0007564494000002 
Figure 0007564494000003 
Figure 0007564494000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for designing a structural member, a method for manufacturing a steel plate, a method for manufacturing a tailored blank, a method for manufacturing a structural member, and a structural member. This application claims priority based on Japanese Patent Application No. 2021-127370, filed on August 3, 2021, the contents of which are incorporated herein by reference. [Background technology]
[0002] In recent years, in order to protect the global environment by reducing CO2 gas emissions, the weight reduction of automobile bodies has become an urgent issue in the automotive field. To solve this issue, the application of high-strength steel sheets is being actively considered. The strength of steel sheets (plated steel sheets) is becoming increasingly high.
[0003] Hot pressing (hereinafter sometimes referred to as "hot stamping") has attracted attention as one of the technologies for forming automotive components. In hot stamping, a steel sheet is heated to a high temperature and press-formed at a temperature range above the Ar3 transformation temperature. Furthermore, in hot stamping, the press-formed steel sheet is rapidly cooled by removing heat using a die, and transformation occurs simultaneously with forming under the application of press pressure. Through the above process, hot stamping is a technology that can manufacture hot press-formed products (hereinafter sometimes referred to as "hot stamped products") that have high strength and excellent shape fixability.
[0004] In addition, to improve the yield and functionality of press-formed automotive parts, tailored blanks, in which at least two steel sheets are butted together at their end faces and joined by laser welding, plasma welding, or the like, are used as press materials. In tailored blanks, multiple steel sheets are joined according to the purpose, so that the thickness and strength of one part can be freely changed. As a result, the use of tailored blanks can improve the functionality of automotive parts and reduce the number of parts in automotive parts. In addition, hot stamping of tailored blanks can produce high-strength press-formed parts in which the thickness, strength, etc. can be freely changed.
[0005] When a tailored blank is used as a press material to form an automotive component by hot stamping, the tailored blank is heated, for example, to a temperature range of 800° C. to 1000° C. For this reason, a plated steel sheet that is plated with aluminum such as Al-Si, which has a higher plating boiling point than Zn-based plating, is often used for a tailored blank for hot stamping.
[0006] When aluminum-plated steel sheets are butt-welded, the aluminum concentration in the weld increases, and the hardenability decreases, resulting in a problem of reduced strength of the weld.
[0007] To solve this problem, there is a technique for removing the aluminum plating from the area of the aluminum-plated steel sheet that will be butt-welded. US Patent No. 5,399,633 discloses a method in which one or more of the sheet metal pieces includes a coating material layer and a weld notch, and where at least a portion of the coating material layer is removed from the edge region prior to welding such that the weld joint is substantially free of the constituents of the coating material layer. Patent Document 2 discloses a technology in which a plate is formed from a steel substrate and a precoating, the precoating being in contact with the substrate and being formed from an intermetallic alloy layer on which a metal alloy layer is placed, and on at least one precoated surface of the plate, one zone is free of the metal alloy layer, and the zone is located around the plate. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] Japanese Patent No. 6034490 [Patent Document 2] Japanese Patent No. 5237263 Summary of the Invention [Problem to be solved by the invention]
[0009] The techniques described in Patent Documents 1 and 2 have a problem in that the aluminum plating is removed from the entire area to be welded, and therefore the process of removing the aluminum plating takes a long time.
[0010] The present invention has been made in consideration of the above problems, and has an object to provide a method for designing a structural component, a method for manufacturing a steel plate, a method for manufacturing a tailored blank, a method for manufacturing a structural component, and a structural component, which can suppress breakage of the structural component, shorten the time required for removing the aluminum plating, and extend the life of a tool. [Means for solving the problem]
[0011] In order to solve the above problems, the present invention proposes the following means. (1) The method for designing a structural member according to the first aspect of the present invention comprises the steps of: A method for designing a structural member obtained by forming a tailored blank, comprising the steps of: The tailored blank has a linear weld formed by butt-welding two or more steel plates, The steel sheet before butt welding has an exposed portion where the base steel sheet is exposed at a part of the joined end portion to be butt-welded of the plated steel sheet having an intermetallic compound layer and an aluminum plating layer provided on a surface of the base steel sheet in this order from the base steel sheet side, a weld setting process for performing a collision analysis by a numerical simulation on an analysis model of the structural member, and setting a position of the weld so that a fracture index of a first region, which is at least a part of a region in an extension direction of the weld, is equal to or greater than a specified value, and the fracture index of all remaining regions other than the first region in the weld is less than the specified value; The method includes a removal region setting step of setting, after the weld portion setting step, a region in the welded end portion that includes a portion corresponding to the first region, as a removal region in which the exposed portion is to be formed. (2) Aspect 2 of the present invention is a design method for a structural member according to aspect 1, The structural member includes a flange portion to be joined to another member, The first region may be located in the flange portion. (3) The method for producing a steel sheet according to the third aspect of the present invention is as follows: A method for manufacturing a steel plate used in the manufacture of a structural member designed by the structural member design method of embodiment 1 or 2, providing a plated steel sheet having the intermetallic compound layer and the aluminum plating layer provided on a surface of the base steel sheet in this order from the base steel sheet side; a removal process for forming an exposed portion in which the base steel sheet is exposed by removing a part of the aluminum plating layer and the intermetallic compound layer in the removal region, a first plating portion in which the intermetallic compound layer and the aluminum plating layer remain on the surface of the base steel sheet in this order from the base steel sheet side, and a second plating portion in which the intermetallic compound layer and the aluminum plating layer remain on the surface of the base steel sheet, In the removal process, the aluminum plating layer and a portion of the intermetallic compound layer are removed so that in a first direction that is perpendicular to the thickness direction of the plated steel sheet and that runs from the center of the plated steel sheet toward one edge of the plated steel sheet in a planar view, the first plating portion, the exposed portion, the second plating portion, and the edge of the plated steel sheet are arranged in this order on one surface of the base steel sheet, and so that in the first direction, at least the first plating portion, the exposed portion, and the edge of the plated steel sheet are arranged in this order on the other surface of the base steel sheet. (4) A method for producing a steel plate according to a fourth aspect of the present invention is a method for producing a steel plate used for producing a structural member designed by the design method for a structural member according to the first or second aspect, providing a plated steel sheet having the intermetallic compound layer and the aluminum plating layer provided on a surface of the base steel sheet in this order from the base steel sheet side; a removal process for forming an exposed portion in which the base steel sheet is exposed by removing a part of the aluminum plating layer and the intermetallic compound layer in the removal region, and a first plating portion in which the intermetallic compound layer and the aluminum plating layer remain in this order from the base steel sheet side on a surface of the base steel sheet, In the removal process, the aluminum plating layer and a portion of the intermetallic compound layer are removed so that in a first direction that is perpendicular to the thickness direction of the plated steel sheet and that runs from the center of the plated steel sheet toward one edge of the plated steel sheet in a planar view, the first plating portion, the exposed portion, and the edge of the plated steel sheet are arranged in this order on one surface of the base steel sheet, and so that in the first direction, at least the first plating portion, the exposed portion, and the edge of the plated steel sheet are arranged in this order on the other surface of the base steel sheet. (5) The method for manufacturing a tailored blank according to the fifth aspect of the present invention includes a step of butt-welding the steel plate manufactured by the method for manufacturing a steel plate according to the third or fourth aspect. (6) A method for manufacturing a structural component according to a sixth aspect of the present invention includes a step of hot pressing a tailored blank manufactured by the method for manufacturing a tailored blank according to the fifth aspect. (7Aspects of the present invention of 7 Structural members teeth , A structural member having a linear weld formed therein, The structural member comprises two or more steel members joined by the welds, The steel member is A base material; A plating layer provided on a surface of the base material; Equipped with The steel member includes an exposed portion in which the base material is exposed in an area adjacent to the weld portion along the weld portion, The exposed portion is partially present in the extension direction of the weld portion, The exposed portion is present in a portion of the structural member corresponding to an assumed breakage portion. R . ( 8 Aspects of the present invention of 8 Structural members teeth , A structural member having a linear weld formed therein, The structural member comprises two or more steel members joined by the welds, The steel member is A base material; A plating layer provided on a surface of the base material; Equipped with The steel member includes an exposed portion in which the base material is exposed in an area adjacent to the weld portion along the weld portion, The exposed portion is partially present in the extension direction of the weld portion, The structural member is A top plate portion, A pair of vertical wall portions bent and connected to the end portions of the top plate portion; a first ridge portion connecting the top plate portion and the vertical wall portion; A pair of flange portions bent and connected to the ends of the vertical wall portion; a second ridge portion connecting the vertical wall portion and the flange portion; having The exposed portion is present in a portion other than the vertical wall portion. R . ( 9 Aspects of the present invention 9 The aspect 8 In the structural members of The exposed portion may be present only in the flange portion. Effect of the Invention
[0012] According to the above aspects of the present invention, it is possible to provide a design method for a structural member having a flange portion, a manufacturing method for a steel plate, a manufacturing method for a tailored blank, and a manufacturing method for a structural member having a flange portion, which can suppress breakage of the structural member having a flange portion, can shorten the time required for removing the aluminum plating, and can extend the life of tools. [Brief description of the drawings]
[0013] [Figure 1] FIG. 2 is a perspective view showing an example of a structural member. [Diagram 2] FIG. 2 is a cross-sectional view of the structural member of FIG. 1 taken along line AA. [Diagram 3] 1 is a flowchart of a structural member design method according to the present disclosure. [Figure 4] FIG. 11 is an explanatory diagram for explaining a collision analysis. [Diagram 5] FIG. 13 is a diagram showing the results of a collision analysis. [Figure 6] FIG. 13 is a schematic diagram for explaining a removal region. [Figure 7] 1 is a schematic cross-sectional view showing an example of an end portion having an exposed portion of a base steel sheet and a second plated portion in a steel sheet used in a flange structural member of the present disclosure. FIG. [Figure 8] 1 is a flowchart of a method for manufacturing a steel plate and a method for manufacturing a tailored blank according to the present disclosure. [Figure 9] FIG. 4 is a cross-sectional view illustrating a bottom forming step in the steel plate manufacturing method of the present disclosure. [Figure 10] FIG. 4 is a cross-sectional view illustrating a bottom forming step in the steel plate manufacturing method of the present disclosure. [Figure 11] FIG. 4 is a cross-sectional view illustrating a bottom forming step in the steel plate manufacturing method of the present disclosure. [Figure 12] FIG. 2 is a cross-sectional view illustrating a cutting step in the manufacturing method of the steel plate according to the present disclosure. [Figure 13] FIG. 2 is a cross-sectional view illustrating a cutting step in the manufacturing method of the steel plate according to the present disclosure. [Figure 14]FIG. 2 is a cross-sectional view illustrating a cutting step in the manufacturing method of the steel plate according to the present disclosure. [Figure 15] FIG. 2 is a cross-sectional schematic diagram of a tailored blank of the present disclosure. [Figure 16] 2 is a cross-sectional view of the structural member of FIG. 1 taken along line BB. [Figure 17] FIG. 2 is an explanatory diagram of a removal region in the first embodiment. [Figure 18] FIG. 13 is a diagram showing the analysis results of Example 2. [Figure 19] FIG. 11 is an explanatory diagram of a removal region in the second embodiment. [Figure 20] FIG. 13 is an explanatory diagram of a removal region in Comparative Example 1. [Figure 21] FIG. 13 is a diagram showing the relationship between the height from the bottom end of the vehicle and the intrusion amount in an example and a comparative example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] As a result of intensive research by the present inventors, it was found that in a structural member obtained by forming a tailored blank, a tensile force is not applied over the entire area of the linear welded portion during a collision. Therefore, there is a region in the structural member that does not require removal of the aluminum plating layer and the intermetallic compound layer. In the present disclosure, a numerical simulation is used to perform a collision analysis of a structural member obtained by forming a tailored blank, and the structural member is designed so that a portion in the welded portion that is at high risk of breaking due to the application of a tensile force or local bending deformation is only a first region, which is at least a part of the region in the extension direction of the welded portion. By designing the structural member in this manner, the range in which the aluminum plating layer and the intermetallic compound layer are removed can be limited to the first region. This allows the strength of the welded portion to be maintained in the first region where the load is high. Since the aluminum plating layer and the intermetallic compound layer do not need to be removed in the region where the load is low, the processing time required for removing the aluminum plating layer and the intermetallic compound layer can be shortened, and the life of the tool can be extended.
[0015] <Design method for structural members> Hereinafter, a design method for a structural member according to the present disclosure will be described with reference to the drawings. The structural member of the present disclosure is, for example, a structural member for an automobile, and examples thereof include a B-pillar, a bumper, and a side sill. An example of the structural member of the present disclosure is shown in FIG. 1 and FIG. 2, but the structural member of the present disclosure is not limited to the shape shown in FIG. 1 and FIG. 2. FIG. 1 is a perspective view of the structural member. FIG. 2 is a cross-sectional view of the structural member 10 of FIG. 1 along line AA. The structural member 10 of FIG. 1 and FIG. 2 is a B-pillar including a member (steel member) 10A, a member (steel member) 10B, and a linear weld 150 connecting the member 10A and the member 10B. The structural member 10 will be described later. The structural member 10 includes at least a flange portion 1, a first ridge portion 2, a vertical wall portion 3, a second ridge portion 4, and a top plate portion 5. The member 10A and the member 10B may have the same tensile strength and thickness, or may have different properties. The structural member 10 is obtained by hot stamping a tailored blank. Moreover, the tailored blank used in the structural member 10 has a linear weld formed by butt welding two or more steel plates (steel plates for butt welding). The steel plate used in manufacturing the tailored blank (steel plate before butt welding) has an exposed portion where the base steel plate is exposed at a part of the end (joined end to be butt welded) of the plated steel plate on which an intermetallic compound layer and an aluminum plating layer are provided from the base steel plate side on the surface of the base steel plate. The steel plate used in the tailored blank of the present disclosure will be described later. A design method for a structural member will be described below. In this specification, the meaning of the term "process" includes not only an independent process but also a process that cannot be clearly distinguished from other processes as long as the intended purpose of the process is achieved.
[0016] A structural member design method S10 of the present disclosure will be described with reference to Fig. 3. Fig. 3 is a flowchart of the structural member design method of the present disclosure. The structural member design method S10 of the present disclosure includes a weld setting step S5 for performing a collision analysis by numerical simulation on an analysis model of the structural member 10, and setting the position of the weld so that the fracture index of a first region, which is at least a part of the region in the extension direction of the weld 150, is equal to or greater than a specified value and the fracture index of all remaining regions other than the first region in the weld 150 is less than the specified value, and a removal region setting step for setting, after the weld setting step S5, a region in the welded end including a portion corresponding to the first region as a removal region in which an exposed portion is to be formed. For example, in the case where only the flange portion is the first region, the structural member design method S10 includes a weld setting step S5 for performing a collision analysis by numerical simulation on the structural member 10, and setting the position of the weld 150 so that the fracture index of the flange portion 1 of the structural member 10 in the weld 150 is equal to or greater than a specified value and the fracture index of the portion of the structural member 10 other than the flange portion 1 in the weld 150 is less than the specified value, and a removal region setting step S6 for setting, after the weld setting step S5, a region in which the fracture index is equal to or greater than the specified value in the collision analysis and which includes at least an end of the plated steel sheet corresponding to the region in which the weld is formed, as a removal region in which the aluminum plating layer and the intermetallic compound layer are removed. Hereinafter, an example will be described in which the first region is only the flange portion 1, but the present invention is not limited to this. The first region may be located in, for example, one or more of the flange portion 1, the first ridge portion 2, the second ridge portion 4, and the top plate portion 5. The first region can be set as appropriate. The first region is preferably located only in the flange portion 1. If the first region from which the plating layer is to be removed is located in the flange portion 1, it is possible to prevent the welded portion 150 in the flange portion 1 that is joined to another member from breaking early. Therefore, when a load is applied, it is possible to maintain the connection to the other member as much as possible. This can improve the load-bearing performance of a member such as an automobile frame member that has a structure in which another member is joined at the flange portion of a structural member.
[0017] (Welding section setting process) In the weld setting process S5, first, a collision analysis is performed on the structural member 10 (S1). Specifically, a collision analysis is performed by numerical simulation on an analytical model of the structural member 10. The collision analysis will be described with reference to FIG. 4. FIG. 4(a) shows the positional relationship between the structural member 10 and the collision barrier, and FIG. 4(b) shows the direction of the bending moment and tensile force at the time of collision. In the example of FIG. 4, the part where the collision barrier collides becomes an energy absorption area, and the part is subjected to large deformation. Specifically, the top plate part 5 and the vertical wall part 3 of the collision part are subjected to bending deformation and crushing deformation. At this time, the flange part 1 is generally arranged on the outside of the bending, so tensile strain is generated. On the other hand, the upper side of the structural member 10 is subjected to a bending moment due to the intrusion of the collision barrier. Therefore, the flange part 1 located on the upper side is arranged on the outside of the bending, like the flange part 1 located on the lower side of the structural member 10, so tensile strain is generated. Therefore, the flange part 1 is subjected to tensile strain over the entire length. Therefore, the risk of fracture is high regardless of the position of the weld part. On the other hand, if there is a weld in a position where bending deformation occurs in a part other than the flange part 1 (for example, the top plate part 5), the risk of fracture increases. This fracture can be avoided by changing the position of the weld. In order to understand the risk of fracture in parts other than the first region (here, the flange part 1), a crash analysis is performed.
[0018] In the crash analysis S1, a crash analysis is performed by a numerical simulation on an analytical model of a structural member. The numerical simulation is not particularly limited, and for example, a finite element method, a difference method, a boundary element method, etc. can be used. The crash analysis is performed, for example, using software such as LS-DYNA (registered trademark), and the analysis of the fracture index can be performed using NSafe (registered trademark)-MAT. FIG. 5 is a diagram showing the results of the crash analysis. As shown in FIG. 5, by performing the crash analysis, it is possible to identify a part with a high fracture index (a part with a high fracture risk). Examples of the fracture index include strain, stress, and a plate thickness reduction rate. As the fracture index, strain is preferable.
[0019] The conditions used in the collision analysis (collision direction, collision speed, tensile strength of the structural member, etc.) are not particularly limited and can be set appropriately depending on the application of the structural member. For example, in the case of the structural member 10, a full car model is used to perform an analysis of a side collision.
[0020] After performing the collision analysis (S1), in the welded portion 150, a portion other than the first region where the fracture index is large is extracted (S2). Next, it is confirmed whether the fracture index of all the portions extracted in S2 is less than a specified value. That is, it is confirmed whether the region where the fracture index is equal to or greater than the specified value (sometimes referred to as a fracture assumed portion) is only the first region (here, the flange portion 1) of the welded portion 150 (S3). Here, the specified value is, for example, a threshold value at which fracture occurs in the fracture index. In the welded portion 150, if there is a region where the fracture index is equal to or greater than the specified value in all remaining regions other than the first region, the position of the welded portion 150 is changed (S4), and the collision analysis is performed again (S1). In the case where the region where the fracture index is equal to or greater than the specified value is only the first region of the welded portion 150, a removal region setting step S6 is performed. There is no particular limitation on the way in which the position of the welded portion 150 is changed. For example, in the case where a door hinge mounting portion is provided, the position can be changed so that the welded portion 150 does not enter the door hinge mounting portion.
[0021] In the removal area setting step S6, the end area of the steel plate (steel plate for butt welding) where the fracture index becomes equal to or greater than a specified value in the collision analysis after the weld setting step S5 and corresponds to the area (high load area) where the weld 150 is to be formed is set as the removal area where the aluminum plating layer and the intermetallic compound layer are to be removed. In other words, in the removal area setting step S6, the area including at least the part corresponding to the first area in the joined end is set as the removal area where the exposed part is to be formed. FIG. 6 is a schematic diagram for explaining the removal area 170. Here, the high load area is the first area 180. The steel plate 120 to be the member 10A and the steel plate 110 to be the member 10B are set to have the shape of the structural member 10 by hot press forming, and the planned welding position 160 is set to the position of the weld 150 set in the weld setting step S5. The end 110a of the steel plate 110 and the end 120a of the steel plate 120 along the planned welding position 160 are the joined end 130 to be butt-welded. The removal region 170 includes a high-stress region. The longitudinal length L1 of the removal region is preferably three times or less than the longitudinal length of the high-stress region. More preferably, it is twice or less than the longitudinal length of the high-stress region. The removal region 170 may be equal to the length of the high-stress region. That is, the removal region may be only the high-stress region. The length W1 of the removal region in a direction perpendicular to the longitudinal direction is preferably longer than the width of the region where the weld 150 is to be formed (the length in a direction perpendicular to the longitudinal direction of the weld). Since the aluminum plating layer and the intermetallic compound layer 16 are not removed except for the removal region, the mass productivity of the steel plate used for the structural member 10 is improved.
[0022] <Steel plate> Next, a description will be given of the steel plate 110 and the steel plate 120 in Fig. 6. The steel plates (steel plates for butt welding) 110 and 120 of the present disclosure are steel plates that are butt-welded with another steel plate to form a tailored blank. In this specification, a numerical range expressed using "to" means a range that includes the numerical values before and after "to" as the lower and upper limits. In this specification, the content of a component (element), for example, the content of C (carbon), may be expressed as "C content." The contents of other elements may also be expressed in a similar manner.
[0023] In the present disclosure, the terms "base steel sheet," "intermetallic compound layer," and "aluminum plating layer" will be explained in "Definition of the scope of the base steel sheet, intermetallic compound layer, and aluminum plating layer" described later in the first embodiment. In the present disclosure, the term "cross section" of a steel plate (steel plate for butt welding) refers to a cross section cut in the thickness (plate thickness) direction of the steel plate. Specifically, in Fig. 7, the thickness direction of the steel plate 100 is Z, and the longitudinal direction of the exposed portion 22 (direction perpendicular to the display surface of Fig. 7) is X. Then, the directions perpendicular to the directions Z and X are each referred to as Y. In this case, the cross section refers to a cross section cut along the YZ plane.
[0024] In the present disclosure, the term "thickness direction" refers to the direction in which the sheet thickness at the center of the sheet width of the steel sheet is measured. In the present disclosure, the term "plating thickness" means the length in the thickness direction of the steel sheet from the surface of the first plated portion or the second plated portion to the base steel sheet. In the present disclosure, the term "end face of a steel plate" means a face of a steel plate that is exposed in a direction perpendicular to the thickness direction. In this disclosure, the term "edge of a steel plate" means a portion adjacent to the end face of the steel plate. In the present disclosure, the term "edge of a steel plate" means a region located on the periphery of a steel plate, the region ranging from the end face of the steel plate to within 20% of the opposing width of the steel plate (i.e., the length from edge to edge of the opposing steel plates). The steel plate of the present disclosure forms a tailored blank by butt-welding an end surface at an end portion to an end surface of another steel plate. Here, the embodiment of the two steel plates to be butt-welded may adopt any one of the following embodiments.
[0025] The steel sheet used in the structural member of the present disclosure has a base steel sheet, an intermetallic compound layer, and an aluminum plating layer. The steel sheet of the present disclosure has a first plating portion on the surface of the base steel sheet, in which an intermetallic compound layer and an aluminum plating layer are provided in this order from the base steel sheet side. The steel sheet of the present disclosure also has an exposed portion in which the base steel sheet is exposed in the removal area 170 set in the removal area setting step S6. The steel sheet of the present disclosure also has a second plating portion on the surface of the base steel sheet, in which an intermetallic compound layer and an aluminum plating layer are provided in this order from the base steel sheet side in the removal area 170 set in the removal area setting step S6.
[0026] Here, the direction perpendicular to the thickness direction of the steel sheet and extending from the first plating portion to one edge of the steel sheet (Y direction) is defined as the first direction (first orientation). In the steel sheet of the present disclosure, in the first direction, the first plating portion, exposed portion, second plating portion, and edge of the steel sheet are arranged in this order on at least one surface of the base steel sheet. Also, in the steel sheet of the present disclosure, in the first direction, at least the first plating portion, exposed portion, and edge of the steel sheet are arranged in this order on the other surface of the base steel sheet. In addition, in the first direction, the first plated portion, the exposed portion, the second plated portion, and the edge of the steel plate may be arranged in this order on the other surface of the base steel plate. The steel plate of the present disclosure is formed into a tailored blank by butt-welding an end face of the steel plate to an end face of another steel plate. The shape of the other steel plate is not particularly limited.
[0027] FIG. 7 is an example of a steel sheet used as the steel sheets 110 and 120 used in FIG. 6. FIG. 7 is a schematic cross-sectional view showing an example of an end portion in which a first plating portion, an exposed portion of a base steel sheet, and a second plating portion having an intermetallic compound layer and an aluminum plating layer are provided on one surface of the steel sheet of the present disclosure, and the first plating portion and the exposed portion are provided on the other surface. That is, FIG. 7 shows an embodiment in which a steel sheet has a first plating portion, an exposed portion, and a second plating portion on one surface, and an intermetallic compound layer and an aluminum plating layer are provided in the second plating portion. In addition, the first plating portion and the exposed portion are provided at the end portion on the other surface of the steel sheet shown in FIG. 7, but the second plating portion is not provided, and the exposed portion is extended to the edge of the steel sheet.
[0028] In FIG. 7, 100 denotes a steel sheet, 12 denotes a base steel sheet, 14 denotes an aluminum plating layer, 16 denotes an intermetallic compound layer, 22 denotes an exposed portion, 24 denotes a second plating portion, and 26 denotes a first plating portion. Additionally, 100A indicates an edge of the steel sheet 100. 100B indicates an edge of the first plating portion 26 on the boundary between the first plating portion 26 and the exposed portion 22. 100C indicates an edge of the second plating portion 24 on the boundary between the second plating portion 24 and the exposed portion 22.
[0029] The steel sheet 100 of the present disclosure has a base steel sheet 12, an intermetallic compound layer 16, and an aluminum plating layer 14. The steel sheet 100 of the present disclosure has a first plating portion 26 in which the intermetallic compound layer 16 and the aluminum plating layer 14 are provided, in that order, from the base steel sheet 12 side, on the surface of the base steel sheet 12. The steel sheet 100 of the present disclosure also has an exposed portion 22 in which the base steel sheet 12 is exposed in the removed region. The steel sheet 100 of the present disclosure also has a second plating portion 24 in which the intermetallic compound layer 16 and the aluminum plating layer 14 are provided, on the surface of the base steel sheet 12. Here, a first direction F1 is a direction perpendicular to the thickness direction of the steel sheet 100 and extending from the first plated portion 26 toward one edge 100A of the steel sheet 100. In the steel sheet 100 of the present disclosure, in the first direction F1, the first plated portion 26, the exposed portion 22, the second plated portion 24, and the edge 100A of the steel sheet 100 are arranged on the same plane in the following order: first plated portion 26, exposed portion 22, second plated portion 24, and edge 100A of the steel sheet 100.
[0030] The exposed portion 22 is formed in the region between an edge 100B of the first plating portion 26 and an edge 100C of the boundary between the second plating portion 24 and the exposed portion 22. The exposed portion 22 is formed between the first plating portion 26 and the second plating portion 24. The second plating portion 24 is formed in an area including the edge 100A of the steel sheet 100. In the first direction F1, the edge 100A of the steel sheet 100 and the second plating portion 24 are adjacent to each other. The second plating portion 24 is formed in an area between the edge 100A of the steel sheet 100 and an edge 100C at the boundary between the second plating portion 24 and the exposed portion 22.
[0031] The above-mentioned second plating portion 24, exposed portion 22 and first plating portion 26 are formed on one surface of the end portion of the steel plate 100, and the exposed portion 22 and first plating portion 26 are formed on the other surface of the end portion.
[0032] 7 , in the steel sheet 100 of the present disclosure, at the end of the steel sheet 100, the thickness of the base steel sheet 12 at the exposed portion 22 where the base steel sheet 12 is exposed may be the same as the thickness of the base steel sheet 12 at the first plated portion 26. Also, in the steel sheet 100 of the present disclosure, at the end of the steel sheet 100, the thickness of the base steel sheet 12 at the exposed portion 22 where the base steel sheet 12 is exposed may be smaller than the thickness of the base steel sheet 12 at the first plated portion 26.
[0033] Although the steel sheets according to the present disclosure have been described above with reference to FIG. 7, the steel sheets according to the present disclosure are not limited thereto.
[0034] <Base material steel plate> An aluminum plating layer 14 is provided on the surface of the base steel sheet 12. The base steel sheet 12 is not particularly limited as long as it is obtained by a normal method including a hot rolling process, a cold rolling process, a plating process, etc. The base steel sheet may be either a hot rolled steel sheet or a cold rolled steel sheet. The thickness of the base steel sheet 12 may be any thickness depending on the purpose, and is not particularly limited. For example, the thickness of the base steel sheet 12 may be 0.8 mm or more, or may be 1 mm or more, as the overall thickness of the plated steel sheet after the aluminum plating layer 14 is provided (the steel sheet before the exposed portion 22, etc. are formed). The thickness of the base steel sheet 12 may be 4 mm or less, or may be 3 mm or less.
[0035] For the base steel plate 12, it is preferable to use a steel plate formed to have high mechanical strength (for example, various properties related to mechanical deformation and destruction such as tensile strength, yield point, elongation, reduction in area, hardness, impact value, fatigue strength, etc.). Specifically, a steel plate having a tensile strength of 400 to 2700 MPa, which is currently easily available, is exemplified, but is not limited to this. The plate thickness is, for example, 0.7 mm to 3.2 mm. Note that a steel plate having low mechanical strength may be used as the base steel plate 12. Specifically, it is 1300 MPa class, 1200 MPa class, 1000 MPa class, 600 MPa class, 500 MPa class, etc. For example, in the case of a B-pillar of an automobile, a steel plate with high tensile strength is used from the upper part to the center where deformation is to be prevented, and a steel plate with lower tensile strength is used for the lower part which is an energy absorbing part. For the upper part to the center part, it is preferable to use a steel plate of 1500 to 2700 MPa class, which is currently easily available. The lower part is desirably made of a steel plate with a tensile strength of 500 MPa to 1800 MPa, and more preferably of 600 MPa to 1300 MPa. The thickness of the steel plate for the B-pillar is desirably 1.4 mm to 2.6 mm for the upper part and 1.0 mm to 1.6 mm for the lower part.
[0036] An example of a preferable chemical composition of the base steel sheet 12 is, for example, the following chemical composition. The base steel plate 12 contains, by mass%, C: 0.02% to 0.58%, Mn: 0.20% to 3.00%, Al: 0.005% to 0.06%, P: 0.03% or less, S: 0.010% or less, N: 0.010% or less, Ti: 0% to 0.20%, Nb: 0% to 0.20%, V: 0% to 1.0%, W: 0% to 1.0%, and Cr: 0% to 1.0%. It has a chemical composition of Mo: 0% to 1.0%, Cu: 0% to 1.0%, Ni: 0% to 1.0%, B: 0% to 0.0100%, Mg: 0% to 0.05%, Ca: 0% to 0.05%, REM: 0% to 0.05%, Sn: 0% to 0.5%, Bi: 0% to 0.05%, Si: 0% to 2.00%, and the balance: Fe and impurities. In the following description, "%" indicating the content of a component (element) means "mass %".
[0037] (C: 0.02% to 0.58%) C is an important element that enhances the hardenability of the base steel plate 12 and mainly determines the strength after hardening. Furthermore, C is an element that lowers the A3 point and promotes lowering the hardening temperature. If the C content is less than 0.02%, the effect may not be sufficient. Therefore, the C content is preferably 0.02% or more. On the other hand, if the C content exceeds 0.58%, the toughness of the hardened portion deteriorates significantly. Therefore, the C content is preferably 0.58% or less. Preferably, the C content is 0.45% or less.
[0038] (Mn: 0.20% to 3.00%) Mn is a very effective element for improving the hardenability of the base steel plate 12 and stably ensuring strength after quenching. If the Mn content is less than 0.20%, the effect may not be sufficient. Therefore, the Mn content should be 0.20% or more. Preferably, the Mn content is 0.80% or more. On the other hand, if the Mn content exceeds 3.00%, not only will the effect saturate, but it may become difficult to ensure stable strength after quenching. Therefore, the Mn content should be 3.00% or less. Preferably, the Mn content is 2.40% or less.
[0039] (Al: 0.005% to 0.06%) Al functions as a deoxidizing element and has the effect of improving the soundness of the base steel sheet 12. If the Al content is less than 0.005%, it may be difficult to obtain the above-mentioned effect. Therefore, the Al content is preferably 0.005% or more. On the other hand, if the Al content exceeds 0.06%, the above-mentioned effect saturates and becomes disadvantageous in terms of cost. Therefore, the Al content is preferably 0.06% or less. Preferably, the Al content is 0.05% or less. Also, it is preferable that the Al content is 0.01% or more.
[0040] (P:0.03% or less) P is an element contained as an impurity. If P is contained in excess, the toughness of the base steel plate 12 is likely to decrease. Therefore, the P content is preferably 0.03% or less. More preferably, the P content is 0.01% or less. There is no particular need to specify a lower limit for the P content, but from the viewpoint of cost, the lower limit is preferably 0.0002%.
[0041] (S:0.010% or less) S is an element contained as an impurity. S forms MnS and has the effect of embrittling the base steel sheet 12. Therefore, the S content is preferably 0.010% or less. More preferably, the S content is 0.004% or less. There is no particular need to specify a lower limit for the S content, but from the viewpoint of cost, the lower limit is preferably set to 0.0002%.
[0042] (N:0.010% or less) N is an element contained as an impurity in the base steel sheet 12. Furthermore, N is an element that forms inclusions in the base steel sheet 12 and deteriorates toughness after hot press forming. Therefore, the N content is preferably 0.010% or less, more preferably 0.008% or less, and further preferably 0.005% or less. There is no particular need to specify a lower limit for the N content, but from the viewpoint of cost, the lower limit is preferably 0.0002%.
[0043] (Ti:0%~0.20%, Nb:0%~0.20%, V:0%~1.0%, W:0%~1.0%) Ti, Nb, V, and W are elements that promote the mutual diffusion of Fe and Al in the aluminum plating layer and the base steel sheet 12. Therefore, at least one or more of Ti, Nb, V, and W may be contained in the base steel sheet 12. However, when 1) the Ti content and Nb content exceed 0.20%, or 2) the V content and W content exceed 1.0%, the effect of the above action is saturated and it becomes disadvantageous in terms of cost. Therefore, the Ti content and Nb content are preferably 0.20% or less, and the V content and W content are preferably 1.0% or less. The Ti content and Nb content are preferably 0.15% or less, and the V content and W content are preferably 0.5% or less. In order to obtain the effect of the above action more reliably, it is preferable to set the lower limit of the Ti content and Nb content to 0.01%, and the lower limit of the V content and W content to 0.1%.
[0044] (Cr:0%~1.0%, Mo:0%~1.0%, Cu:0%~1.0%, Ni:0%~1.0%, B:0%~0.0100%) Cr, Mo, Cu, Ni, and B are elements that are effective in improving the hardenability of the base steel sheet 12 and stably ensuring the strength after hardening. Therefore, one or more of these elements may be contained in the base steel sheet 12. However, even if the contents of Cr, Mo, Cu, and Ni exceed 1.0% and the amount of B exceeds 0.0100%, the above effects are saturated and it is disadvantageous in terms of cost. Therefore, the contents of Cr, Mo, Cu, and Ni are preferably 1.0% or less. In addition, the amount of B is preferably 0.0100% or less, and preferably 0.0080% or less. To obtain the above effects more reliably, it is preferable to satisfy either the contents of Cr, Mo, Cu, and Ni being 0.1% or more and the content of B being 0.0010% or more.
[0045] (Ca:0%~0.05%, Mg:0%~0.05%, REM:0%~0.05%) Ca, Mg, and REM have the effect of refining the morphology of inclusions in steel and preventing the occurrence of cracks due to the inclusions during hot press forming. Therefore, one or more of these elements may be contained in the base steel sheet 12. However, if they are added in excess, the effect of refining the morphology of inclusions in the base steel sheet 12 becomes saturated and only leads to an increase in costs. Therefore, the Ca content is set to 0.05% or less, the Mg content is set to 0.05% or less, and the REM content is set to 0.05% or less. To more reliably obtain the effects of the above actions, it is preferable to satisfy any one of the following: the Ca content is 0.0005% or more, the Mg content is 0.0005% or more, and the REM content is 0.0005% or more.
[0046] Here, REM refers to 17 elements, namely, Sc, Y, and lanthanoids, and the content of the REM refers to the total content of these elements. In the case of lanthanoids, they are industrially added to the base steel sheet 12 in the form of misch metal.
[0047] (Sn: 0%~0.5%) Sn is an element that improves the corrosion resistance of the exposed portion 22. Therefore, Sn may be contained in the base steel plate 12. However, if the base steel plate 12 contains Sn in an amount exceeding 0.5%, it will lead to embrittlement of the base steel plate 12. Therefore, the Sn content is set to 0.5% or less. Preferably, the Sn content is set to 0.3% or less. To more reliably obtain the effects of the above action, it is preferable that the Sn content is set to 0.02% or more. More preferably, the Sn content is set to 0.04% or more.
[0048] (Bi: 0% to 0.05%) Bi is an element that acts as a solidification nucleus during the solidification process of molten steel, and reduces the secondary arm spacing of dendrites, thereby suppressing the segregation of Mn and other elements that segregate within the secondary arm spacing of dendrites. Therefore, Bi may be contained in the base steel plate 12. In particular, for steel plates that often contain a large amount of Mn, such as steel plates for hot pressing, Bi is effective in suppressing the deterioration of toughness caused by the segregation of Mn. Therefore, it is preferable for such steel types to contain Bi. However, even if the base steel sheet 12 contains Bi at a content exceeding 0.05%, the effect of the above-mentioned action saturates and costs increase. Therefore, the Bi content is set to 0.05% or less. Preferably, the Bi content is set to 0.02% or less. To more reliably obtain the effect of the above-mentioned action, it is preferable that the Bi content be 0.0002% or more. More preferably, the Bi content is 0.0005% or more.
[0049] (Si:0%~2.00%) Si is a solid solution strengthening element and can be effectively utilized when it is contained up to 2.00%. However, if the base steel sheet 12 contains more than 2.00% Si, there is a concern that defects in galvanizing properties may occur. Therefore, when the base steel sheet 12 contains Si, the Si content is preferably 2.00% or less. The preferred upper limit is 1.40% or less, and more preferably 1.00% or less. The lower limit is not particularly limited, but in order to more reliably obtain the effects of the above action, the lower limit is preferably 0.01%.
[0050] (Remainder) The balance is Fe and impurities. Here, examples of the impurities include components contained in raw materials such as ores and scraps, or components that are mixed into the steel sheet during the manufacturing process. The impurities refer to components that are not intentionally contained in the steel sheet.
[0051] <Aluminum plating layer> The aluminum plating layer 14 is formed on both sides of the base steel sheet 12. There is no particular limitation on the method for forming the aluminum plating layer 14. For example, the aluminum plating layer 14 may be formed on both sides of the base steel sheet 12 by a hot-dip plating method (a method in which the base steel sheet 12 is immersed in a molten metal bath mainly containing aluminum to form an aluminum plating layer).
[0052] Here, the aluminum plating layer 14 is a plating layer mainly containing aluminum, and may contain 50% by mass or more of aluminum. Depending on the purpose, the aluminum plating layer 14 may contain elements other than aluminum (e.g., Si, etc.), and may contain impurities that are mixed in during the manufacturing process, etc. Specifically, the aluminum plating layer 14 may have a chemical composition that contains, for example, 5% to 12% by mass of Si (silicon), with the balance being aluminum and impurities. Alternatively, the aluminum plating layer 14 may have a chemical composition that contains, for example, 5% to 12% by mass of Si (silicon) and 2% to 4% by mass of Fe (iron), with the balance being aluminum and impurities. When the aluminum plating layer 14 contains Si within the above range, deterioration in workability and corrosion resistance can be suppressed, and the thickness of the intermetallic compound layer can be reduced.
[0053] The thickness of the aluminum plating layer 14 in the first plating portion 26 is not particularly limited, but may be, for example, an average thickness of 8 μm (micrometers) or more, and preferably 15 μm or more. Also, the thickness of the aluminum plating layer 14 in the first plating portion 26 may be, for example, an average thickness of 50 μm or less, preferably 40 μm or less, more preferably 35 μm or less, and even more preferably 30 μm or less. The thickness of the aluminum plating layer 14 represents the average thickness in the first plating portion 26 of the steel sheet 100.
[0054] The aluminum plating layer 14 prevents corrosion of the base steel sheet 12. Furthermore, the aluminum plating layer 14 prevents the generation of scale (iron compounds) due to oxidation of the surface of the base steel sheet 12 even if the base steel sheet 12 is heated to a high temperature when the base steel sheet 12 is processed by hot press forming. Furthermore, the aluminum plating layer 14 has a higher boiling point and melting point than plating coatings made of organic materials and plating coatings made of other metal materials (e.g., zinc-based materials). Therefore, the coating does not evaporate when a hot-press-formed product is formed by hot press forming, providing a high surface protection effect. The aluminum plating layer 14 can be alloyed with iron (Fe) in the base steel sheet 12 by heating during hot-dip plating.
[0055] <Intermetallic compound layer> The intermetallic compound layer 16 is a layer formed at the boundary between the base steel sheet 12 and the aluminum plating layer 14 when aluminum plating is provided on the base steel sheet 12. Specifically, the intermetallic compound layer 16 is formed by a reaction between iron (Fe) of the base steel sheet 12 and metal containing aluminum (Al) in a molten metal bath mainly containing aluminum. The intermetallic compound layer 16 is mainly composed of Fe x Al y (x and y each represent 1 or more). When the aluminum plating layer contains Si (silicon), the intermetallic compound layer 16 is formed of Fe x Al y and Fe x Al y S z (x, y, z each represent 1 or more)
[0056] The thickness of the intermetallic compound layer 16 in the first plating portion 26 is not particularly limited, but may be, for example, an average thickness of 1 μm or more, preferably 3 μm or more, and more preferably 4 μm or more. The thickness of the intermetallic compound layer 16 in the first plating portion 26 may be, for example, an average thickness of 10 μm or less, and preferably 8 μm or less. The thickness of the intermetallic compound layer 16 refers to the average thickness in the first plating portion 26. The thickness of the intermetallic compound layer 16 can be controlled by the temperature and immersion time of the molten metal bath mainly containing aluminum.
[0057] Here, the base steel sheet 12, the intermetallic compound layer 16, and the aluminum plating layer 14 are confirmed, and the thicknesses of the intermetallic compound layer 16 and the aluminum plating layer 14 are measured by the following method.
[0058] The steel plate 100 is cut so that the cross section thereof is exposed, and the cross section of the steel plate 100 is polished. The orientation of the exposed cross section of the steel plate 100 is not particularly limited. However, the cross section of the steel plate 100 is preferably a cross section perpendicular to the longitudinal direction of the exposed portion 22. The polished cross section of the steel sheet 100 is linearly analyzed from the surface of the steel sheet 100 to the base steel sheet 12 by an electron probe microanalyser (FE-EPMA) to measure the aluminum concentration and iron concentration. The aluminum concentration and iron concentration are preferably average values of three measurements. The measurement conditions are an acceleration voltage of 15 kV, a beam diameter of about 100 nm, an irradiation time per point of 1000 ms, and a measurement pitch of 60 nm. The measurement distance may be any distance that allows the thickness of the plating layer to be measured, and for example, the measurement distance is about 30 μm to 80 μm in the thickness direction from the surface of the steel sheet 100 to the base steel sheet 12. It is preferable to measure the thickness of the base steel sheet 12 using an optical microscope with a scale.
[0059] <Definition of the range of base steel sheet, intermetallic compound layer, and aluminum plating layer> As a measurement value of the aluminum concentration in a cross section of steel sheet 100 (plated steel sheet), a region where the aluminum (Al) concentration is less than 0.06 mass% is determined to be base steel sheet 12, and a region where the aluminum concentration is 0.06 mass% or more is determined to be intermetallic compound layer 16 or aluminum plating layer 14. Furthermore, of the intermetallic compound layer 16 and the aluminum plating layer 14, a region where the iron (Fe) concentration is more than 4 mass% is determined to be intermetallic compound layer 16, and a region where the iron concentration is 4 mass% or less is determined to be aluminum plating layer 14. The thickness of the intermetallic compound layer 16 is defined as the distance from the boundary between the base steel sheet 12 and the intermetallic compound layer 16 to the boundary between the intermetallic compound layer 16 and the aluminum plating layer 14. The thickness of the aluminum plating layer 14 is defined as the distance from the boundary between the intermetallic compound layer 16 and the aluminum plating layer 14 to the surface of the aluminum plating layer 14.
[0060] The thickness of the aluminum plating layer 14 and the thickness of the intermetallic compound layer 16 are measured by linear analysis from the surface of the steel sheet 100 to the surface of the base steel sheet 12 (the boundary between the base steel sheet 12 and the intermetallic compound layer 16) as follows. For example, when measuring the thickness of the first plating portion 26, the thickness of the aluminum plating layer 14 is measured at five positions obtained by dividing the entire length of the first plating portion 26 in the third direction (the same applies to the definition of the entire length below) in the longitudinal direction of the exposed portion 22 (for example, the X direction in FIG. 1, hereinafter referred to as the third direction) into six equal parts, and the average of the measured values is taken as the thickness of the aluminum plating layer 14. Here, the measurement position of the thickness in the first direction is a position that is half the width of the first plating portion 26 in each of the five cross-sectional views (hereinafter, the thickness measurement is performed in the same manner). The width of the first plating portion 26 refers to the distance between the edges of the first plating portion 26 in the first direction F1, and hereinafter, is also simply referred to as the width of the first plating portion 26. The distinction between the aluminum plating layer 14, the intermetallic compound layer 16, and the base steel sheet 12 when measuring the thickness is determined according to the above-mentioned criteria. When the exposed portion 22 is extended on a curve, the thickness may be measured at positions that divide the entire length along the curve into six equal parts. Similarly, when measuring the thickness of the intermetallic compound layer 16, the thickness of the intermetallic compound layer 16 is measured at five positions obtained by dividing the entire length of the intermetallic compound layer 16 (the same applies to the definition of the entire length below) into six equal parts in the third direction, and the average of the measured values is defined as the thickness of the intermetallic compound layer 16. When measuring the thickness of the intermetallic compound layer 16 of the first plating portion 26, the measurement is performed at a position that is 1 / 2 the width of the first plating portion 26, as in the case of measuring the thickness of the aluminum plating layer 14. Furthermore, the distinction between the aluminum plating layer 14, the intermetallic compound layer 16, and the base steel sheet 12 during thickness measurement is determined according to the criteria described above.
[0061] <Exposed part> 7, steel sheet 100 has exposed portions 22 on both sides of the end in removal area 170. On the side where second plating portion 24 is provided, exposed portion 22 is provided between first plating portion 26 and second plating portion 24 at the end of removal area 170. On the side where second plating portion 24 is not provided, exposed portion 22 is provided between first plating portion 26 and edge 100A of steel sheet 100 at the end of removal area 170. 7, when the second plating portion 24 is formed, the exposed portion 22 is formed in the range from the edge 100C of the boundary between the second plating portion 24 and the exposed portion 22 to the edge 100B of the first plating portion 26. When the second plating portion 24 is not formed, the exposed portion 22 is formed in the range from the edge 100A of the steel sheet 100 to the edge 100B of the first plating portion 26.
[0062] The width of the exposed portion 22 in the first direction F1 (the distance from the second plating portion 24 to the first plating portion 26 in the first direction F1; hereinafter, simply referred to as the width of the exposed portion 22) may be, for example, 0.1 mm or more on average. By making the width of the exposed portion 22 0.1 mm or more, it is possible to prevent aluminum from remaining at the end of the welded portion when welding the tailored blank. The width of the exposed portion 22 may be 5.0 mm or less on average. By making the width of the exposed portion 22 5.0 mm or less, it is possible to suppress deterioration of corrosion resistance after painting. When the butt welding is laser welding, the width of the exposed portion 22 is preferably 0.5 mm or more, and the width of the exposed portion 22 is preferably 1.5 mm or less. When the butt welding is plasma welding, the width of the exposed portion 22 is preferably 1.0 mm or more, and the width of the exposed portion 22 is preferably 4.0 mm or less. That is, it is preferable to make the width of the exposed portion 22 0.1 mm or more and the width of the exposed portion 22 5.0 mm or less (average). The width of exposed portion 22 is determined by, for example, measuring the width of exposed portion 22 from five cross sections obtained by dividing the entire length of exposed portion 22 in the third direction (X direction) into six equal parts using a microscope and a scale, and taking the average value (the same method of measuring the width is used below).
[0063] <2nd Plating Department> Similar to exposed portion 22, second plating portion 24 is formed at the end of the removal region, where exposed portion 22 is provided. Second plating portion 24 is preferably provided on at least one side of the end portion located around the periphery of steel sheet 100, closer to the edge of steel sheet 100 than exposed portion 22, in an area including edge 100A of steel sheet 100. In other words, second plating portion 24 is preferably provided along edge 100A of steel sheet 100, at the end of the removal region.
[0064] The second plating portion 24 is preferably formed in a region including the edge of the steel sheet 100 so that it is included in the weld after butt welding. To achieve this state, the second plating portion 24 is provided along the edge of the steel sheet 100 on at least one side of the end of the steel sheet 100.
[0065] In the first direction F1, it is preferable that (all of) the second plating portion 24 is present in a range of 0.9 mm from the edge 100A of the steel sheet 100. If the second plating portion 24 is present in this range, the second plating portion 24 is more likely to be included in the welded portion after butt welding. In addition, by setting the area in which the second plating portion 24 is present in this range, at least the area more than 0.9 mm from the edge 100A of the steel sheet 100 toward the first plating portion becomes the exposed portion 22. This makes it possible to make at least the surface between the weld metal and the weld heat affected zone after butt welding a region in which hard intermetallic compounds are not generated. In this way, by specifying the width of the second plating portion 24 and the position of the exposed portion 22, it is possible to supply Al required for improving the corrosion resistance of the weld metal after painting to the weld metal, and to prevent the generation of intermetallic compounds that reduce fatigue strength at the boundary between the weld metal and the weld heat affected zone. The second plating portion 24 is preferably located within 0.5 mm from the edge 100A of the steel sheet 100, more preferably within 0.4 mm from the edge 100A of the steel sheet 100, and even more preferably within 0.3 mm from the edge 100A of the steel sheet 100. For example, the width of the second plating portion 24 is preferably set according to the width of the welded portion 150 in the tailored blank after butt welding. The width of the welded portion 150 is, for example, 0.4 mm to 6 mm. When the width of the welded portion 150 is 0.4 mm, the width of the second plating portion 24 is preferably 0.04 mm or more and less than 0.2 mm, and the sum of the width of the second plating portion 24 and the width of the exposed portion 22 is preferably 0.5 mm or more. When the width of the welded portion 150 is 1 mm, the width of the second plating portion 24 is preferably 0.3 mm or less, and the sum of the width of the second plating portion 24 and the width of the exposed portion 22 is preferably 0.8 mm or more. When the width of the welded portion is 2 mm, the width of the second plating portion 24 is preferably 0.8 mm or less, and the sum of the width of the second plating portion 24 and the width of the exposed portion 22 is preferably 1.3 mm or more. When the width of the welded portion 150 is 6 mm, the width of the second plated portion 24 is preferably 0.9 mm or less, and the sum of the width of the second plated portion 24 and the width of the exposed portion 22 is preferably 3.3 mm or more. The width of the welded portion 150 varies depending on the welding method. For this reason, for example, when the butt welding is laser welding, the width of the second plated portion 24 is preferably 0.05 mm or more, and the width of the second plated portion 24 is preferably 0.40 mm or less. When used in plasma welding, the width of the second plated portion 24 is preferably 0.10 mm or more, and the width of the second plated portion 24 is preferably 0.60 mm or less.
[0066] Here, the width of exposed portion 22 is the average value of measurements of the width of exposed portion 22 at five locations, and the width of second plated portion 24 is the average value of measurements of the width of second plated portion 24 at five locations. The measurement locations of exposed portion 22 and second plated portion 24 are five positions in the longitudinal direction of exposed portion 22, which divide the entire length of exposed portion 22 in the X direction into six equal parts. The method for measuring the width of exposed portion 22 and the width of second plating portion 24 is as follows. Five measurement samples including a cross section (e.g., a cross section along the first direction F1 in a plan view of the steel sheet 100) at which the entire width of the exposed portion 22 and the second plating portion 24 formed at the end of the steel sheet 100 can be observed are taken. The measurement samples are taken from five positions obtained by dividing the length of the exposed portion 22 formed in the direction along the end edge 100A of the steel sheet 100 into six equal parts. Next, the steel sheet 100 is cut so that the cross section is exposed. Thereafter, the cut measurement samples are embedded in resin, polished, and the cross section is magnified under a microscope. Then, for each sample, the width of the exposed portion 22, which is the distance from the second plating portion 24 to the first plating portion 26, is measured. In addition, the distance between both ends of the second plating portion 24 is measured for each sample. In the case of FIG. 7, the width w1 of the removed region is the sum of the width of the second plating portion 24 and the width of the exposed portion 22.
[0067] <Steel sheet manufacturing method> Next, an example of a manufacturing method of the steel plate according to the present disclosure will be described. The manufactured steel plate is a steel plate used for manufacturing a structural member designed by the above-mentioned design method. Fig. 8 is a flowchart showing a manufacturing method S11 of the tailored blank according to the present disclosure.
[0068] First, in the manufacturing method S11 for manufacturing a steel sheet (steel sheet for butt welding), a plated steel sheet manufacturing step S12 is performed. In the plated steel sheet manufacturing step S12, a plated steel sheet 101 shown in Fig. 9 is manufactured. In the plated steel sheet manufacturing step S12, a plated steel sheet 101 is manufactured by a known method, in which an intermetallic compound layer 16 and an aluminum plating layer 14 are provided on each surface of a base steel sheet 12 in this order from the base steel sheet 12 side. In the plated steel sheet 101, the exposed portion 22 and the second plating portion 24 are not formed compared to the steel sheet 100 described above. Here, the thickness of the plated steel sheet 101 is taken as t μm. The thickness of the plated steel sheet 101 is equal to the thickness of the steel sheet 100 in the first plating portion 26. When the plated steel sheet manufacturing process S12 is completed, the process proceeds to a removal process S14 in step S14. The removal process S14 is a process of mechanically removing the aluminum plating layer 14 and the intermetallic compound layer 16. In the removal process S14, a part of the aluminum plating layer 14 and the intermetallic compound layer 16 may be removed so that the first plating portion 26, the exposed portion 22, the second plating portion 24, and the edge 100C of the plated steel sheet 101 are arranged in this order on one surface of the base steel sheet 12 in a first direction F1 that is perpendicular to the thickness direction of the plated steel sheet 101 and extends from the center of the plated steel sheet 101 toward one edge of the plated steel sheet 101 in a plan view, and at least the first plating portion 26, the exposed portion 22, and the edge 100C of the plated steel sheet are arranged in this order on the other surface of the base steel sheet 12 in the first direction F1.
[0069] Next, in the removing step S14, a bottom portion forming step S15 is performed. 10 , in the bottom forming step S15, the plated steel sheet 101 is cut to deform a part of the plated steel sheet 101, thereby forming a bottom region R2 on the surface of the base steel sheet 12 of the plated steel sheet 101. The bottom region R2 is formed on an edge of the base steel sheet 12. When cutting the plated steel sheet 101, the plated steel sheet 101 may be cut so as to have the shape of the structural member 10. Here, a first direction F1 is defined. The first direction F1 is perpendicular to the thickness direction of the plated steel sheet 101, and is a direction from the center of the plated steel sheet 101 toward one edge of the plated steel sheet 101 in a plan view. This first direction F1 coincides with the first direction F1 of the steel sheet 100 when the plated steel sheet 101 is processed to become the steel sheet 100. The lower region R2 referred to here means a region of the aluminum plating layer 14 and the intermetallic compound layer 16 located on the inner side of the base steel sheet 12 in the thickness direction from a virtual plane T1 obtained by extending the surface of a portion (e.g., the exposed portion 22) of the base steel sheet 12 that is not deformed when cut in the first direction F1. Note that the virtual plane T1 becomes a virtual line when viewed in a cross section perpendicular to the thickness direction.
[0070] In this example, in the bottom forming step S15, the plated steel sheet 101 is cut by a mechanical method called shearing (shearing), to form a bottom region R2 in the plated steel sheet 101. Note that instead of the shearing, a blanking (punching) process may be used to form the bottom region R2 in the plated steel sheet 101. The mechanical method referred to here means a method in which a tool is brought into direct contact with the plated steel sheet 101, and the plated steel sheet 101 is processed by the tool in contact. Specifically, in the bottom forming step S15, as shown in Fig. 9, the plated steel sheet 101 is placed on an upper surface 401a of a support table 401 of a shearing device 400. The upper surface 401a is flat and arranged along a horizontal plane. At this time, the plated steel sheet 101 is arranged so that an end portion thereof protrudes from the support table 401.
[0071] The blade portion 402 of the shearing device 400 is disposed above the upper surface 401a of the support table 401 at a fixed distance S from the support table 401 along the upper surface 401a. 10, the plated steel sheet 101 is cut in the thickness direction of the plated steel sheet 101 by moving the blade portion 402 downward, and the end portion of the plated steel sheet 101 is cut off. At this time, a bottom region R2, which is a sag, is formed on the first surface 101A of the plated steel sheet 101. A protruding portion 38, which is a burr, is formed on the lower surface of the plated steel sheet 101. Here, the deepest bottom depth of the bottom region R2 is defined as x (μm). The bottom depth x indicates the (maximum value of) the distance from the imaginary plane T1 to the surface of the base steel sheet 12 in the bottom region R2. The bottom depth x can be measured by a known laser profile meter or the like.
[0072] By adjusting the material of the plated steel sheet 101, the interval S, etc., the protrusion 38 is formed, and at the same time, the lower surface of the plated steel sheet 101 may be deformed as shown by the two-dot chain line in Fig. 10, forming a bottom region R3. Note that the two-dot chain line represents the shape of the lower surface of the plated steel sheet 101. In this case, in the bottom forming step S15, a bottom region R2 is formed on the upper surface of the plated steel sheet 101, and a bottom region R3 is formed on the lower surface of the plated steel sheet 101. For example, it is considered that the bottom region R3 is formed when the material forming the plated steel sheet 101 is pulled toward the protruding portion 38 due to the rigidity of the plated steel sheet 101 when the protruding portion 38 is formed. When the bottom portion forming step S15 is completed, the process proceeds to step S17.
[0073] Next, in a cutting step (removal step) S17, a part of the base steel sheet 12 and the intermetallic compound layer 16 in the removal region 170 of the plated steel sheet 101 is cut using a cutting process, which is a mechanical method, to form the exposed portion 22 and the second plated portion 24, thereby manufacturing the steel sheet 100. In the present disclosure, an end mill is used for the cutting process, and the aluminum plating layer 14 and the intermetallic compound layer 16 that are present at least outside the plated steel sheet 101 in the thickness direction relative to the imaginary plane T1 and that are in the removal region 170 are cut and removed by the end mill. The blade of the end mill that rotates around an axis is brought into direct contact with the plated steel sheet 101 to cut the plated steel sheet 101. In the cutting process S17, for example, a cutting tool, an end mill, a metal saw, etc. are used in addition to an end mill. In the removing step, the aluminum plating layer 14 and the intermetallic compound layer 16 may be removed by grinding. For grinding, a whetstone, a grinder, etc. are used.
[0074] In the cutting step S17, a region R5 is cut from the edge of the plated steel sheet 101 in the direction opposite to the first direction F1 to a transgressing position P beyond the low region R2. The transgressing position P is a position that will become the edge 100B of the first plating portion 26 in a later step, and the range between the low region R2 and the transgressing position P becomes the exposed portion 22. At this time, the depth to which the region R5 of the plated steel sheet 101 is cut is constant. This reduces the manufacturing cost required for cutting. Note that the aluminum plating layer 14 and the intermetallic compound layer 16 on the low region R2 within the region R5 do not need to be cut. The depth to which the plated steel sheet 101 is cut is less than the sum of the thickness a of the aluminum plating layer 14, the thickness b of the intermetallic compound layer 16, and the bottom depth x. That is, the cutting is performed so as to leave at least a part of the intermetallic compound layer 16 and the aluminum plating layer 14 located in the bottom region R2. The above cutting forms the exposed portion 22 and the second plating portion 24, and similarly, the base steel sheet 12 and the intermetallic compound layer 16 in the range of the removal region 170 are removed from the other surface to form the exposed portion 22, thereby producing the steel sheet 100.
[0075] In the manufacturing method of the steel sheet of the present disclosure, the exposed portion 22 and the second plating portion 24 may be formed in the removed region 170 as follows. 11, the plated steel sheet 101 is placed on an upper surface 420a of a support stand 420. A bottom region R7 is formed on the upper surface of the plated steel sheet 101 by using a mechanical method in which an end portion of the plated steel sheet 101 is pressed in the thickness direction of the plated steel sheet 101 with a pressing member 425 such as a pressure roll. The bottom region R7 is formed on the edge of the plated steel sheet 101. Note that the pressing direction by the pressing member 425 may be inclined with respect to the thickness direction. In the lower region R7, the deepest recessed portion is located at the edge of the plated steel sheet 101. Next, a cutting step S17 is performed to produce a steel plate 102 having an exposed portion 22 and a second plating portion 42 formed thereon, as shown in FIG.
[0076] Furthermore, in the manufacturing method of the present disclosure, only the exposed portion 22 may be formed in the removal region 170. That is, in the removal step S14, a part of the aluminum plating layer 14 and the intermetallic compound layer 16 may be removed so that in a first direction F1 that is perpendicular to the thickness direction of the plated steel sheet 101 and extends from the center of the plated steel sheet 101 toward one edge of the plated steel sheet 101 in a plan view, the first plating portion 26, the exposed portion 22, and an edge 100C of the plated steel sheet 101 are arranged in this order on one surface of the base steel sheet 12, and at least the first plating portion 26, the exposed portion 22, and an edge 100C of the plated steel sheet 101 are arranged in this order on the other surface of the base steel sheet 12 in the first direction F1. In this example, a laser processing method, which is not a mechanical method, is used. As shown in Fig. 13, a laser processing device 430 irradiates an end of the plated steel sheet 101 with laser light L7 along the thickness direction of the plated steel sheet 101. As a result, the end of the plated steel sheet 101 is cut off, but no bottom region is formed in the plated steel sheet 101. Thereafter, by cutting using an end mill or the like in the same manner as above, a steel sheet 103 in which only the exposed portion 22 is formed in the removal region 170 is obtained as shown in Fig. 14.
[0077] <Manufacturing method of tailored blanks> The manufacturing method of the tailored blank of the present disclosure includes a step of butt-welding the steel plates of the present disclosure by a known method. Specifically, as shown in Fig. 6, the ends of the steel plates 110 and 120 with exposed portions are arranged in a butt-welded state, and the steel plates 110 and 120 are butt-welded, for example, using a known laser welding device (not shown). This forms a weld 150, and the tailored blank 300 of Fig. 15 is obtained. The weld 150 is formed at a position set in the weld setting step S5.
[0078] <Manufacturing methods for structural components> The manufacturing method of the structural member of the present disclosure includes a step of hot pressing the tailored blank 300 manufactured as described above. By hot pressing, it is possible to obtain the structural member 10 shaped into the structure shown in Figs. 1 and 2, for example.
[0079] <Structural components> A structural member 10 of the present disclosure will be described. FIG. 16 is a cross-sectional view of the structural member 10 of FIG. 1 along the line BB. The structural member 10 of the present disclosure is a structural member 10 in which a linear weld 150 is formed. The structural member 10 includes two or more steel members 10A, 10B joined by a weld 150. The structural member 10 includes a top plate portion 5, a pair of vertical wall portions 3 that are bent and connected from an end of the top plate portion 5, a first ridge portion 2 that connects the top plate portion 5 and the vertical wall portion 3, a pair of flange portions 1 that are bent and connected from an end of the vertical wall portion 3, and a second ridge portion 4 that connects the vertical wall portion 3 and the flange portion 1. The steel members 10A, 10B include a base material 12A and a plating layer 36 provided on the surface of the base material 12A. In the structural member 10 of the present disclosure, the plating layer 36 is, for example, an intermetallic compound layer. The steel members 10A, 10B have exposed portions 22 where the base material 12A is exposed, in adjacent regions along the welded portion 150. The exposed portions 22 exist partially in the direction in which the welded portion 150 extends.
[0080] The exposed portion 22 is present in a portion of the structural member 10 corresponding to the assumed fracture portion. The assumed fracture portion is a portion of the weld where stress is most concentrated when a load is applied to the structural member 10 under a specific load input condition. The assumed fracture portion may be determined empirically as a portion where stress is likely to concentrate, such as a flange portion, or may be an area where the fracture index is equal to or greater than a specified value in a crash analysis. The following methods are available for identifying the assumed fracture portion of the structural member 10 in a crash analysis. For example, three-dimensional shape data of the structural member 10 is obtained using a three-dimensional scanner or from CAD data, and a structural model with a weld is created based on the shape data and the mechanical properties of the material. A crash analysis is performed on the obtained structural model under a specific load input condition under a condition where no exposed portion is formed, and an area with a high fracture index is identified. The fracture index is preferably strain. When the mesh size of the structural model is large, even if a large strain occurs locally in the mesh, the strain is distributed to the mesh area, so the larger the mesh size, the smaller the equivalent plastic strain at which fracture occurs tends to be. The threshold value of the equivalent plastic strain when determining the assumed fracture portion can be set to 5 to 20% for an analysis with a mesh size of 1 mm to 4 mm, for example. Specifically, when the mesh size of the structure model is 2 mm, the region where the equivalent plastic strain is 10% or more can be determined as the assumed fracture portion.
[0081] It is preferable that the exposed portion 22 is present in a portion other than the vertical wall portion 3. By having the exposed portion 22 in a portion other than the vertical wall portion 3, it is possible to reduce the area from which the aluminum plating layer and the intermetallic compound layer are removed while maintaining the strength of the portion with a high risk of fracture. It is preferable that the exposed portion 22 is present in one or more of the flange portion 1, the first ridge portion 2, the second ridge portion 4, and the top plate portion 5. It is preferable that the exposed portion 22 is present in the top plate portion 5, the flange portion 1, or the top plate portion 5 and the flange portion 1. It is particularly preferable that the exposed portion 22 is present only in the flange portion 1. By having the exposed portion 22 only in the flange portion 22, it is possible to suppress fracture of the flange portion 1 to which another member is connected, and it is possible to improve the load-bearing performance of the structural member 10.
[0082] As described above, the structural component design method, steel plate manufacturing method, tailored blank manufacturing method, structural component manufacturing method, and structural component disclosed herein can suppress breakage of the structural component and shorten the time required for removing the aluminum plating.
[0083] The technical scope of the present invention is not limited to the above-mentioned embodiment, and various modifications can be made without departing from the spirit of the present invention. In the above example, the second plating portion is formed by forming the lower region, but the second plating portion may be formed without forming the lower region by removing a part of the aluminum plating using a laser.
[0084] In a plan view of the structural member 10, it is preferable that the angle between the longitudinal direction of the structural member 10 and the weld line of the flange portion is 80° or less. When the angle between the longitudinal direction of the structural member 10 and the weld line of the flange portion is 80° or less, the exposed portion 22 of the flange portion 1 may not be present.
[0085] In addition, within the scope of the invention, the components in the above-described embodiments may be replaced with well-known components, and the above-described modified examples may be combined as appropriate. EXAMPLES
[0086] Next, an embodiment of the present invention will be described, but the conditions in the embodiment are merely an example of conditions adopted to confirm the feasibility and effects of the present invention, and the present invention is not limited to this example of conditions. Various conditions can be adopted in the present invention as long as they do not deviate from the gist of the present invention and achieve the object of the present invention.
[0087] (Welding Design) The crash analysis was performed using LS-DYNA (registered trademark), and the fracture index analysis was performed using NSafe (registered trademark)-MAT. A crash analysis was performed on the shape of the B-pillar in FIG. 1, and the position of the weld was determined so that the fracture index (strain) of the first region in the weld was equal to or greater than the fracture threshold, and the fracture index (strain) of the region other than the first region was less than the fracture threshold. The crash analysis was performed using a full car model, with the barrier being an IIHS side impact honeycomb barrier, the bogie weight being 1500 kg, and the collision speed being 50 km / h. The tensile strength of the member A was 2000 MPa, and the plate thickness was 2.2 mm. The tensile strength of the member B was 1300 MPa, and the plate thickness was 1.6 mm.
[0088] Example 1 In Example 1, the first region was the flange portion only. For two plated steel sheets (aluminum plating layer 30 μm, intermetallic compound layer 8 μm) formed as shown in Fig. 17, the aluminum plating layer and the intermetallic compound layer in the portion that would become only the flange portion, which has a high risk of fracture, were cut off by a length of 25 mm on one side (total of upper and lower surfaces: 100 mm), and analysis was performed.
[0089] Example 2 In Example 2, the first region was the flange portion, the ridge portion, and the top plate portion. The welded portion was determined so that the fracture index of the flange portion, the ridge portion, and the top plate portion was high, as shown in Fig. 18. For two plated steel sheets (aluminum plating layer 30 μm, intermetallic compound layer 8 μm) formed as shown in Fig. 19, the aluminum plating layer and the intermetallic compound layer in the flange portion, ridge portion, and top plate portion, which are at high risk of fracture, were cut off by 380 mm in total from the upper and lower surfaces, and analysis was performed.
[0090] Comparative Example 1 For two plated steel sheets (aluminum plating layer 30 μm, intermetallic compound layer 8 μm) formed as shown in Figure 20, an analysis was performed assuming that the aluminum plating layer and intermetallic compound layer were cut away over the entire area where the weld was to be formed (a total of 700 mm on the top and bottom surfaces).
[0091] Comparative Example 2 An analysis was performed on two plated steel sheets with the same shape as in Figure 17, assuming that no cutting was performed.
[0092] (Intrusion amount analysis) Crash analysis was performed under the conditions of Examples 1 and 2 and Comparative Examples 1 and 2, and evaluation was performed based on the intrusion amount at five points with different heights from the bottom end of the vehicle. The crash analysis was performed using LS-DYNA, and the fracture index analysis was performed using NSafe-MAT. The crash analysis was performed using a full car model, with the barrier being an IIHS side impact honeycomb barrier, the bogie weight being 1500 kg, and the crash speed being 50 km / h. Component A had a tensile strength of 2000 MPa and a plate thickness of 2.2 mm. Component B had a tensile strength of 1300 MPa and a plate thickness of 1.6 mm. The results are shown in Figure 21. In Examples 1 and 2, like Comparative Example 1 in which the entire area was removed, there was no breakage in the structural member and the amount of penetration was suppressed. On the other hand, in Comparative Example 2 in which no cutting was performed, breakage occurred.
[0093] (Work time and tool life) The machining time and tool life were determined for the example and comparative example with a scanning speed of 6 m / min, a rotation speed of 40,000 rpm, a tool diameter of φ6 mm, an end R of 0.5 mm, and a machining length of 300 m. The results are shown in Table 1. In Table 1, "-" indicates that no machining was performed.
[0094] [Table 1]
[0095] As shown in Table 1, in Example 1, since the machining range was limited to the flange portion only, the machining time was short and the tool life was also long. Moreover, in Example 2, in which the flange portion, top plate portion, and ridge portion were cut, the tool life was shorter than that of Example 1, but longer than that of Comparative Example 1. From the above results, it was confirmed that by using the design method for a structural member disclosed herein, it is possible to suppress breakage of the structural member and to shorten the time required for removing the aluminum plating. [Explanation of symbols]
[0096] REFERENCE SIGNS LIST 1 flange portion, 2 first ridge portion, 3 vertical wall portion, second ridge portion, 5 top plate portion, 10 structural member, 12 base steel plate, 14 aluminum plating layer, 16 intermetallic compound layer, 22 exposed portion, 26 first plating portion, 42 second plating portion
Claims
1. A method for designing a structural member obtained by forming a tailored blank, comprising the steps of: The tailored blank has a linear weld portion formed by butt-welding two or more steel plates, The steel sheet before butt welding has an exposed portion where the base steel sheet is exposed at a part of the joined end portion to be butt-welded of the plated steel sheet having an intermetallic compound layer and an aluminum plating layer provided on a surface of the base steel sheet in this order from the base steel sheet side, a weld setting process for performing a collision analysis by a numerical simulation on an analysis model of the structural member, and setting a position of the weld so that a fracture index of a first region, which is at least a part of a region in an extension direction of the weld, is equal to or greater than a specified value, and the fracture index of all remaining regions other than the first region in the weld is less than the specified value; a removal area setting step of setting a region including a portion corresponding to the first region at the welded end portion as a removal area in which the exposed portion is to be formed, after the welded portion setting step; A method for designing a structural member comprising:
2. The structural member includes a flange portion to be joined to another member, The method for designing a structural member according to claim 1 , wherein the first region is located in a flange portion.
3. A method for manufacturing a steel plate used in manufacturing a structural member designed by the structural member design method according to claim 1 or 2, providing a plated steel sheet having the intermetallic compound layer and the aluminum plating layer provided on a surface of the base steel sheet in this order from the base steel sheet side; a removal process for forming an exposed portion in which the base steel sheet is exposed by removing a part of the aluminum plating layer and the intermetallic compound layer in the removal region, a first plating portion in which the intermetallic compound layer and the aluminum plating layer remain on the surface of the base steel sheet in this order from the base steel sheet side, and a second plating portion in which the intermetallic compound layer and the aluminum plating layer remain on the surface of the base steel sheet, A method for manufacturing a steel sheet, in which the removing step removes a portion of the aluminum plating layer and the intermetallic compound layer so that, in a first direction that is perpendicular to the thickness direction of the plated steel sheet and extends from the center of the plated steel sheet toward one edge of the plated steel sheet in a plan view, the first plating portion, the exposed portion, the second plating portion, and the edge of the plated steel sheet are arranged in this order on one surface of the base steel sheet, and so that, in the first direction, at least the first plating portion, the exposed portion, and the edge of the plated steel sheet are arranged in this order on the other surface of the base steel sheet.
4. A method for manufacturing a steel plate used in manufacturing a structural member designed by the structural member design method according to claim 1 or 2, providing a plated steel sheet having the intermetallic compound layer and the aluminum plating layer provided on a surface of the base steel sheet in this order from the base steel sheet side; a removal process for forming an exposed portion in which the base steel sheet is exposed by removing a part of the aluminum plating layer and the intermetallic compound layer in the removal region, and a first plating portion in which the intermetallic compound layer and the aluminum plating layer remain in this order from the base steel sheet side on a surface of the base steel sheet, A method for manufacturing a steel sheet, in which the removing step involves removing a portion of the aluminum plating layer and the intermetallic compound layer so that, in a first direction that is perpendicular to the thickness direction of the plated steel sheet and extends from the center of the plated steel sheet toward one edge of the plated steel sheet in a planar view, the first plating portion, the exposed portion, and the edge of the plated steel sheet are arranged in this order on one surface of the base steel sheet, and so that, in the first direction, at least the first plating portion, the exposed portion, and the edge of the plated steel sheet are arranged in this order on the other surface of the base steel sheet.
5. A method for manufacturing a tailored blank, comprising a step of butt-welding a steel plate manufactured by the method for manufacturing a steel plate according to claim 4.
6. A method for manufacturing a structural member, comprising a step of hot pressing a tailored blank manufactured by the method for manufacturing a tailored blank according to claim 5.
7. A structural member having a linear weld formed therein, The structural member comprises two or more steel members joined by the welds, The steel member is A base material; A plating layer provided on a surface of the base material; Equipped with The steel member includes an exposed portion in which the base material is exposed in an area adjacent to the weld portion along the weld portion, The exposed portion is partially present in the extension direction of the weld portion, The exposed portion is present in a portion of the structural member corresponding to an assumed breakage portion.
8. A structural member having a linear weld formed therein, The structural member comprises two or more steel members joined by the welds, The steel member is A base material; A plating layer provided on a surface of the base material; Equipped with The steel member includes an exposed portion in which the base material is exposed in an area adjacent to the weld portion along the weld portion, The exposed portion is partially present in the extension direction of the weld portion, The structural member is A top plate portion, A pair of vertical wall portions bent and connected to the end portions of the top plate portion; a first ridge portion connecting the top plate portion and the vertical wall portion; A pair of flange portions bent and connected to the ends of the vertical wall portion; a second ridge portion connecting the vertical wall portion and the flange portion; having A structural member, wherein the exposed portion is present in a portion other than the vertical wall portion.
9. The structural member of claim 8 , wherein said exposed portions are only in said flange portions.
Citation Information
Patent Citations
Disposer
JP1977037263A
Fiber padding producing apparatus
JP1985034490A
Press forming method of dissimilar material tailored blank excellent in formability
JP2001001062A
Welding method of forming raw material using high-strength steel plate, laser welding apparatus, forming raw material obtained by method, forming method, and formed article
JP2009000721A
Prediction method of fracture strain of weld, prediction system, and manufacturing method of member with weld
JP2015087349A