Analysis method for molten slag
By measuring impedance between electrodes in molten slag to create a calibration curve, the method addresses the inaccuracy and time issues of conventional methods, enabling quick and precise slag composition analysis for improved steel refining.
Patent Information
- Application Number
- JP2024532529
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2023-07-27
- Filing Date
- 2024-03-15
- Publication Date
- 2024-10-09
- Estimated Expiration
- 2044-03-15
AI Technical Summary
Conventional methods for analyzing molten slag composition during steel refining are inaccurate and time-consuming, particularly due to the effects of heat and dust, and require sampling, which does not account for rapid changes in slag properties during the refining process.
A method that measures impedance between electrodes immersed in molten slag to quickly and accurately determine slag composition by creating a calibration curve based on reference impedance measurements, allowing for real-time estimation of basicity and iron oxide content without sampling.
Enables rapid and precise determination of molten slag composition, improving the accuracy of refining agent addition and blowing patterns, reducing manufacturing costs and preventing foaming or poor slag removal.
Smart Images

Figure 0007564513000004 
Figure 0007564513000005 
Figure 0007564513000006
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for analyzing molten slag, and more particularly to a method for analyzing molten slag that can determine the basicity and iron oxide content of the molten slag based on the relationship between the impedance between a pair of electrodes immersed in the molten slag at a predetermined temperature of the molten slag and the contents of the compositional components contained in the molten slag. [Background technology]
[0002] In the steel refining process, the main purpose of the molten steel refining step is to remove impurities such as phosphorus, silicon, and sulfur contained in the molten steel by supplying refining agents such as CaO source and oxygen to molten iron, which is the main raw material of molten steel. Generally, molten steel is refined by oxidation refining or reduction refining. For this reason, basicity is used as a measure of the basicity of molten slag in steel refining. This basicity is calculated, for example, by dividing the CaO content (%CaO) in the molten slag by the SiO 2 Content (%SiO 2 In other words, basicity can be expressed as the ratio of (%CaO) / (%SiO 2 ) can be expressed as follows.
[0003] In the process of refining molten steel, the basicity of the molten slag can be improved by adding a refining agent such as a CaO source in a predetermined amount to the molten steel, and the oxidation reaction of the molten steel can be promoted. In addition, since the dephosphorization reaction of the molten steel in the process of refining molten steel is accompanied by the reduction reaction of the iron oxide contained in the molten slag, the content of the iron oxide contained in the molten steel can be adjusted by controlling the oxygen supply rate and the height of the lance for supplying the oxygen, thereby promoting the dephosphorization reaction of the molten steel. In this way, it is necessary to determine the amount of refining agent such as CaO source to be added depending on the amount of impurities such as phosphorus, silicon, and sulfur contained in molten steel to be removed, and to add a predetermined amount of the refining agent to the molten steel. In other words, in the refining process of molten steel, it is extremely important to analyze the slag composition of the molten slag present in the furnace.
[0004] Conventionally, quantitative analysis using the intensity of fluorescent X-rays (hereinafter referred to as "fluorescent X-ray analysis") has been widely adopted for the analysis of the slag composition of molten slag. The method for quantifying the slag composition of molten slag using this fluorescent X-ray analysis is as follows. First, a part of the molten slag present in the furnace is collected (sampled), and the collected slag is transported to an analysis room to prepare an analytical sample. Then, fluorescent X-rays (primary X-rays) are irradiated onto the prepared analytical sample. Then, the intensity of the fluorescent X-rays (secondary X-rays) generated from the analytical sample is measured for each element by irradiating the analytical sample with the fluorescent X-rays (primary X-rays). Finally, the content of each element is calculated from the measured value of the fluorescent X-ray intensity using a calibration curve that shows the relationship between the fluorescent X-ray intensity of each element and the content of each element, which has been created in advance.
[0005] However, in order to quantify each component contained in molten slag with high accuracy in the X-ray fluorescence analysis, it is necessary to prepare an analytical sample. In the X-ray fluorescence analysis, it takes at least 10 minutes to prepare an analytical sample required to quantify each component contained in molten slag with high accuracy.
[0006] However, the composition of the molten slag during blowing in a converter changes with time depending on the progress of the blowing, and therefore it is extremely difficult to determine the amount of refining agent to be charged and the blowing pattern based on the analysis results of the molten slag composition obtained by performing fluorescent X-ray analysis.
[0007] Under these circumstances, rapid analysis techniques for slag composition have been proposed. For example, Patent Document 1 proposes a slag component analysis method capable of quickly and highly accurately measuring slag components generated during the refining of molten iron. That is, the slag component analysis method described in Patent Document 1 is an analysis method in which a pulsed laser is irradiated multiple times onto the surface of the slag to be analyzed to convert part of the slag into plasma, and the excitation light obtained from the plasma slag is separated to obtain an emission spectrum from which the concentration or amount ratio of a target component is derived.
[0008] Furthermore, Patent Document 2 proposes an impedance and phase angle difference measuring probe used to control the composition of slag with high precision, and a slag composition control method using the probe. That is, the slag composition control method described in Patent Document 2 is a method in which a measuring probe equipped with at least three electrodes is immersed in molten slag, impedance measurements are performed while changing the combination of electrodes, and charge transfer resistance and solution resistance are calculated separately, and the basicity of the slag and the content of iron oxide (%FeO) contained in the molten slag are obtained using a calibration curve created in advance. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] Patent No. 7111282 specification [Patent Document 2] JP 2022-110303 A Summary of the Invention [Problem to be solved by the invention]
[0010] However, the conventional techniques have the following problems to be solved. That is, the slag component analysis method described in Patent Document 1 is affected by heat and dust, so it is necessary to measure the emission spectrum obtained by dispersing the excitation light obtained from the plasmaized slag from a sufficiently distant position during the slag discharge after the end of blowing. Therefore, the slag component analysis method described in Patent Document 1 cannot be applied during blowing, which is greatly affected by heat and dust.
[0011] Furthermore, the slag composition control method described in Patent Document 2 is a technology that can analyze the slag composition during blowing, but has several problems. First, the slag composition control method described in Patent Document 2 has difficulty in quickly analyzing the slag composition of molten slag. In this slag composition control method, due to the characteristics of impedance measurement, it is necessary to measure multiple impedances with different frequencies in a set frequency range and perform fitting to obtain the resistance value of each element in the equivalent circuit. For this reason, the slag composition control method described in Patent Document 2 spends a lot of time to obtain the resistance value of each element in the equivalent circuit.
[0012] Furthermore, the slag composition control method described in Patent Document 2 requires that the impedance of the molten slag be measured in at least three patterns by changing the combination of electrodes. Therefore, in the slag composition control method described in Patent Document 2, it is difficult to maintain the accuracy of the content of the slag composition components contained in the molten slag under the condition that the slag properties of the molten slag are likely to change during the operation of the converter.
[0013] In addition, in the slag composition control method described in Patent Document 2, the solution resistance and charge transfer resistance obtained by measuring the impedance of the molten slag vary greatly depending on the temperature change of the molten slag. Therefore, the calibration curve that must be prepared in advance and used in the slag composition control method described in Patent Document 2 must correspond to the slag temperature of the molten slag at the time of impedance measurement. However, the calibration curve used in the slag composition control method described in Patent Document 2 does not correspond to the slag temperature of the molten slag.
[0014] The present invention has been made in consideration of the above circumstances, and has an object to provide a method for analyzing molten slag that can quickly and accurately determine the basicity and iron oxide content of molten slag based on the relationship between the impedance between electrodes immersed in the molten slag and the temperature of the molten slag. [Means for solving the problem]
[0015] In order to solve the above problems, the inventors conducted various experiments and found that it is possible to accurately and quickly determine the content of the components contained in the molten slag based on the relationship between the impedance between a pair of electrodes immersed in the molten slag and the content of the components contained in the molten slag, which corresponds to the slag temperature. The present invention was made based on the above findings and is summarized as follows.
[0016] That is, the method for analyzing molten slag according to the present invention, which advantageously solves the above-mentioned problems, is a method for analyzing the compositional components of molten slag, and is characterized in that it includes a first step of measuring a reference slag temperature of a reference molten slag and a reference impedance of the reference molten slag by passing an alternating current between a pair of electrodes immersed in the reference molten slag at the reference slag temperature; a second step of creating a compositional component content calibration curve from the contents of the compositional components contained in the reference molten slag and the reference impedance measured in the first step; a third step of measuring the slag temperature of the measurement molten slag and a measured impedance by passing the alternating current between the pair of electrodes immersed in the measurement molten slag at the slag temperature; and a fourth step of estimating the contents of the compositional components contained in the measurement molten slag based on the measured impedance and the compositional component content calibration curve.
[0017] In addition, the preferred solutions of the method for analyzing molten slag according to the present invention are as follows: (a) the compositional component is iron oxide, and the compositional component content calibration curve is an iron oxide content calibration curve; (b) the compositional component is a specific compositional component necessary for calculating the basicity of the reference molten slag, and the compositional component content calibration curve is a basicity calibration curve; (c) the reference impedance and the measurement impedance are measured by passing AC currents of two selected frequencies; (d) the voltage applied between the pair of electrodes is 10 mV or more and 1.0 V or less, and the two frequencies are 10 Hz or less and 10 kHz or more; and (e) the difference in immersion potential between the pair of electrodes in the measurement molten slag is less than 50 mV. Effect of the Invention
[0018] According to the present invention, the basicity and the iron oxide content can be estimated quickly and accurately without sampling the molten slag during blowing. [Brief description of the drawings]
[0019] [Figure 1] 1 is a schematic diagram showing an overview of a molten slag analysis device used to carry out the molten slag analysis method according to this embodiment. FIG. [Diagram 2] 1 is a graph showing the behavior of the impedance of molten slag when the frequency is swept using a molten slag analysis device used to implement the molten slag analysis method of this embodiment. [Diagram 3] In the examples, the basicity of the calibration curve was estimated by performing multiple regression analysis based on the solution resistance and charge transfer resistance of the reference slag. Figure 3(a) shows the basicity at 1290 to 1310°C. Figure 3(b) shows the basicity at 1390 to 1410°C. [Figure 4]In the examples, the calibration curves are obtained by performing multiple regression analysis based on the solution resistance and charge transfer resistance of the reference slag, and the results of estimating the iron oxide content are shown. Fig. 4(a) shows the results of estimating the basicity at 1290 to 1310°C. Fig. 4(b) shows the results of estimating the basicity at 1390 to 1410°C. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0020] [First embodiment] The molten slag analysis method according to the first embodiment will be described. The molten slag analysis method according to the present embodiment includes a first step of measuring a reference slag temperature of a reference molten slag and a reference impedance of the reference molten slag by passing an AC current between a pair of electrodes immersed in the reference molten slag at the reference slag temperature, a second step of creating a composition component content calibration curve from the contents of composition components contained in the reference molten slag and the reference impedance measured in the first step, a third step of measuring the slag temperature of the measurement molten slag and a measured impedance by passing the AC current between the pair of electrodes immersed in the measurement molten slag at the slag temperature, and a fourth step of estimating the contents of composition components contained in the measurement molten slag based on the measured impedance and the composition component content calibration curve. In other words, the molten slag analysis method of this embodiment creates a component content calibration curve from the content of the component contained in the reference molten slag and the measured reference impedance, and can estimate the content of the component contained in the measurement molten slag based on the measured impedance of the measurement molten slag and the component content calibration curve. The molten slag analyzing device used in the molten slag analyzing method according to this embodiment will be described below.
[0021] <Outline of molten slag analyzer> Fig. 1 is a schematic diagram showing an overview of a molten slag analysis device used in the molten slag analysis method according to the present embodiment. As shown in Fig. 1, the molten slag analysis device 100 includes a crucible 101, a ramming material 102, and an induction melting furnace 103. Molten iron formed by melting scrap, molten pig iron, etc. is charged into the crucible 101. The crucible 101 is preferably made of a material that has low solubility in molten iron and is thermodynamically stable.
[0022] The crucible 101 may be a MgO crucible, a C crucible, a CaO crucible, or an Al 2 O 3 A crucible 101 can be used. The shape of the crucible 101 is not particularly limited, but may be cylindrical. When the crucible 101 is cylindrical, its cross-sectional area is 0.005 to 0.030 m 2 For example, 0.018 m 2 may be also possible.
[0023] The ramming material 102 is a refractory material. The ramming material 102 covers the side wall and the bottom surface of the crucible 101, and is attached to the inner wall of the induction melting furnace 103. The thickness of the ramming material 102 is preferably 100 to 150 mm in terms of heat resistance and durability. The induction melting furnace 103 is a crucible-type low-frequency induction furnace. The induction melting furnace 103 can hold molten iron while maintaining a high temperature. An induction heater may be provided on the side wall of the induction melting furnace 103.
[0024] Furthermore, the molten slag analyzing apparatus 100 is provided with a pair of electrodes 104 for passing an AC current through the molten slag 200 placed in the crucible 101. The pair of electrodes 104 is provided for measuring the impedance of the molten slag 200. The upper ends of the pair of electrodes 104 penetrate the crucible 101 and the heat insulating board 108 and protrude to the outside of the molten slag analyzing apparatus 100. The lower ends of the electrodes 104 are immersed in the molten slag 200 in order to measure the impedance of the molten slag 200 present inside the crucible 101. The electrode 104 is preferably a platinum electrode, but instead of a platinum electrode, an electrode made of a material that is chemically stable and has a small overvoltage, such as tungsten, a zirconia-based refractory, or a magnesia-based refractory, may be used. The electrode 104 may be in the form of a rod or a plate.
[0025] In the molten slag analyzing apparatus 100, a pair of electrodes 104 is formed by an electrode 104L installed on the left side and an electrode 104R installed on the right side. The inter-electrode distance formed between the electrodes 104L and 104R is preferably 5 to 500 mm. Such an inter-electrode distance can be appropriately changed depending on the analysis conditions of the molten slag 200 adopted by the molten slag analyzing method of this embodiment.
[0026] Furthermore, the electrodes 104L and 104R are provided with a temperature sensor 105 for measuring the slag temperature of the molten slag 200. By providing the electrode 104 with the temperature sensor 105, it is possible to measure the slag temperature of the molten slag 200 and the impedance of the molten slag 200 associated with the slag temperature, which is preferable. The temperature sensor 105 may be disposed between the electrodes 104L and 104R. That is, if the temperature sensor 105 is disposed near the wall surface of the crucible 101, rather than near the electrodes 104L and 104R, there is a concern that the impedance measurement temperature may be deviated from the impedance measurement temperature. For this reason, the temperature sensor 105 is preferably disposed near the electrodes 104L and 104R for measuring the impedance measurement temperature. The electrode 104 and the temperature sensor 105 may be configured as a probe attached to a substrate, and the probe may be attached to a converter sublance. Here, the slag temperature of the molten slag 200 is an important index when determining the amount of refining agent such as a CaO source to be added to the molten steel when controlling the basicity of the molten slag 200.
[0027] Electrode 104L attached to induction melting furnace 103 is connected to the negative electrode of potentiostat 106 installed outside induction melting furnace 103 via conductor 107. Electrode 104R attached to induction melting furnace 103 is connected to the positive electrode of potentiostat 106 installed outside induction melting furnace 103 via conductor 107. In this way, both electrodes consisting of electrode 104R and electrode 104L forming a pair of electrodes are connected to potentiostat 106 installed outside induction melting furnace 103 to form an electric circuit that is an equivalent circuit.
[0028] The upper surfaces of the MgO crucible 101, the ramming material 102, and the induction melting furnace 103 included in the molten slag analysis device 100 are covered with a heat insulating board 108. The heat insulating board 108 covers the upper surfaces of the crucible 101, the ramming material 102, and the induction melting furnace 103, and serves to maintain the slag temperature of the molten slag 200 charged in the crucible 101. The heat insulating board 108 is not particularly limited as long as it is made of a material having heat insulating properties. Next, each step included in the molten slag analysis method according to this embodiment using such a molten slag analysis apparatus 100 will be described.
[0029] <First step: Measuring the slag temperature and impedance of the reference molten slag> The method for analyzing molten slag in this embodiment includes a first step of measuring a reference slag temperature of a reference molten slag and a reference impedance of the reference molten slag by passing an alternating current between a pair of electrodes immersed in the reference molten slag at the reference slag temperature. That is, the first step is to measure the reference slag temperature T ref and the reference impedance Z ref This is the process of measuring the reference impedance Z of the reference molten slag. ref is the reference slag temperature T ref The reference impedance Z of the reference molten slag is ref is measured in order to create a calibration curve showing the relationship between the content of each of the constituent elements contained in the reference molten slag.
[0030] In the first step of the method for analyzing molten slag according to the present embodiment, the reference impedance Z ref is measured by passing an AC current between a pair of electrodes 104 immersed in the reference molten slag. A reference impedance Z ref It serves as an electrode for measuring Here, the reference molten slag is a known molten slag in which the content of the compositional components contained in the reference molten slag is already known. In other words, the reference molten slag is a molten slag that is determined by the content of the compositional components contained in the reference molten slag and the reference impedance Z ref This refers to a molten slag 200 used to create a composition component content calibration curve showing the relationship between the above and the molten slag 200, which is separate from the measurement molten slag that is the subject of measurement in the third step described below.
[0031] Using the molten slag analyzing apparatus 100 shown in FIG. 1, a crucible 101 is prepared by, for example, placing a CaO-SiO 2 A -FeO-based molten slag 200 is formed as a reference molten slag. Specifically, a ramming material 102 is embedded in the outer wall of a C crucible, and then, using an induction melting furnace 103, industrial pure iron is heated and melted to obtain molten iron. The molten iron may be produced by adjusting the phosphorus concentration of phosphorus contained in the molten iron to fall within a predetermined range.
[0032] The molten slag 200 that can be applied to the molten slag analysis method according to the present embodiment is CaO-SiO 2 -Not limited to FeO-based molten slag, but also CaO-SiO 2 -MgO-FeO system, CaO-SiO 2 -Al 2 O 3 -FeO system, CaO-SiO 2 -MgO-Al 2 O 3 -FeO-based molten slag may also be used.
[0033] Furthermore, in the system of the molten slag analyzer 100, a flux is poured onto the upper surface of the molten iron to form a reference molten slag as molten slag 200 on the upper surface of the molten iron. The amount of flux to be poured can be appropriately determined depending on the inner volume of the crucible 101, the total amount of molten iron, and the like. The amount of flux to be poured may be, for example, 10 to 30 kg / t of molten iron, preferably 15 to 25 kg / t of molten iron, and more preferably 20 kg / t of molten iron.
[0034] The composition of the flux is not particularly limited as long as it contains a composition that can form the reference molten slag. The composition of the flux is, for example, CaO, SiO 2 , FeO, MgO, etc. The flux contains CaO, SiO 2 In the case where FeO and MgO are contained, the content is, for example, 22.5 (% CaO), 28.0 (% SiO 2 ), 42.5 (% FeO), and 7.0 (% MgO).
[0035] After the flux is poured onto the top surface of the molten iron, the molten steel temperature of the molten iron present inside the crucible 101 is maintained in the range of 1200 to 1700°C. By pouring the flux into the molten iron and maintaining the molten steel temperature, reference molten slag and molten iron are formed in the system of the molten slag analyzer 100. Thereafter, the opening of the induction melting furnace 103 is blocked with an insulating boat 108, and the inside of the induction melting furnace 103 is maintained in the range of 1300 to 1600°C, preferably 1250 to 1500°C, more preferably 1290 to 1310°C or 1390 to 1410°C.
[0036] A pair of electrodes 104 are immersed in the reference molten slag formed in the system of the molten slag analyzing apparatus 100. In the molten slag analyzing apparatus 100, the electrode 104L installed on the left side and the electrode 104R installed on the right side form a pair of electrodes 104. It is preferable that the electrochemical properties of the electrodes 104L and 104R are the same. Therefore, the electrodes 104L and 104R may be the same or may be different as long as they have the same electrochemical properties. The distance between the two electrodes 104L and 104R is not particularly limited as long as the two electrodes 104 do not come into contact with each other and the reference impedance of the reference molten slag can be measured accurately, and may be 5 to 50 mm, preferably 10 mm.
[0037] In the first step, the temperature sensor 105 first detects the reference slag temperature T ref The reference impedance Z of the reference molten slag is measured by passing an AC current between the pair of electrodes 104 formed of the electrodes 104R and 104L immersed in the reference molten slag. ref is measured.
[0038] Next, the reference slag temperature T ref The reference impedance of the reference molten slag is measured by passing an AC current between a pair of electrodes 104 immersed in the reference molten slag. The current value of the AC current passed between the pair of electrodes 104 is determined based on the CaO content (%CaO) and SiO 2 Content (%SiO 2 ), the iron oxide content (%FeO), the concentrations of impurities such as phosphorus, silicon, and sulfur, and the physical properties of the slag. Therefore, the above current value is determined at the time when the applied voltage between the pair of electrodes 104 is set.
[0039] The voltage applied between the pair of electrodes 104 is determined based on the CaO content (%CaO) in the reference molten slag, SiO 2 Content (%SiO 2 ), the iron oxide content (%FeO), and the concentration of impurities such as phosphorus, silicon, and sulfur are taken into consideration to accurately calculate the reference impedance Z ref There are no particular limitations as long as the voltage can be measured. The voltage applied between the pair of electrodes 104 may be 5.0 mV to 5.0 V or less. If the voltage applied between the pair of electrodes 104 is 5.0 mV or more, the effect of noise on frequency response is small, which is preferable. If the voltage applied between the pair of electrodes 104 is 5.0 V or less, the state of the electrode surfaces of the pair of electrodes 104 can be maintained, which is preferable.
[0040] Two types of frequencies are used to apply a voltage between the pair of electrodes 104. The two types of frequencies are set on the high frequency side and the low frequency side. The higher frequency of the two frequencies is the reference impedance Z ref The solution resistance R sol The lower frequency of the two frequencies is set to calculate the reference impedance Z ref The charge transfer resistance R ct The frequency difference between the high frequency side frequency and the low frequency side frequency constituting the two kinds of frequencies is not particularly limited as long as they are two different kinds of frequencies. The frequency used to apply the voltage between the pair of electrodes 104 may be generated by a variable signal generator (not shown) that is a sweep signal generator provided in the potentiostat 106 .
[0041] In the first step of the method for analyzing molten slag according to the present embodiment, the reference slag temperature T ref The measurement was performed at the reference slag temperature T ref For example, the possible temperature range of the slag temperature of the reference molten slag is set to 1200 to 1500 °C, and the reference slag temperature T ref (T ref 1 , T ref 2 , T ref 3 T ref n ) may be measured multiple times.
[0042] In the first step, the reference impedance Z ref The measurement is performed at the reference slag temperature T ref (T ref 1 , T ref 2 , T ref 3 T ref n In the first step of the method for analyzing molten slag according to the present embodiment, the reference molten slag temperature T ref (T ref 1 , T ref 2 , T ref 3 T ref n ) can take on a range of temperatures, measure the reference slug temperature over the entire range, and calculate the reference impedance Z ref (Z ref 1 , Z ref 2 , Z ref 3 Z ref n ) can be measured.
[0043] Thus, in the first step, the reference slag temperature T ref In all ranges assumed for the reference molten slag, the reference slag temperature T ref Measurement of and reference impedance Z ref By performing all of the measurements, the reference slag temperature T ref and the reference impedance Z ref The relationship can be obtained with high accuracy.
[0044] <Second step: A step of preparing a calibration curve of the composition component content based on the reference impedance> The method for analyzing molten slag according to this embodiment includes a second step of creating a calibration curve of the content of the compositional components contained in the reference molten slag and the reference impedance measured in the first step. In the second step, the reference impedance Z of the reference molten slag measured at a pair of electrodes 104 formed by electrodes 104R and 104L is ref Based on this, the combined resistance of the reference molten slag is calculated. Here, the combined resistance of the reference molten slag is the solution resistance R of the reference molten slag. sol and the charge transfer resistance R ct The solution resistance R of the reference molten slag is calculated from the combined resistance of the reference molten slag. sol and the charge transfer resistance of the reference molten slag R ct and can be calculated separately.
[0045] The solution resistance R of the reference molten slag is calculated from the combined resistance of the reference molten slag. sol and the charge transfer resistance R ct and are calculated as follows: Usually, when measuring the impedance of molten slag, the combined resistance of the molten slag is measured at multiple measurement points while gradually shifting the frequency to obtain an impedance measurement curve. The impedance measurement results of the molten slag can be represented by a graph with the horizontal axis representing the real component of the combined resistance of the molten slag and the vertical axis representing the imaginary component of the combined resistance of the molten slag. The locus showing the impedance measurement results of the molten slag shown on the graph forms a semicircle. Two points are formed where this semicircle touches the horizontal axis representing the real component of the combined resistance of the molten slag. The solution resistance value R of the reference molten slag is calculated from one point where the semicircle is tangent to the horizontal axis. sol The solution resistance R of the reference molten slag can be calculated from the other point. sol and the charge transfer resistance R ct In other words, the points that touch the horizontal axis are the solution resistance R of the reference molten slag. sol and the solution resistance of the reference molten slag R sol +Charge transfer resistance R ct It becomes. From such a technical viewpoint, the method for analyzing molten slag according to the present embodiment can calculate the solution resistance R by subtraction if the resistance values of two points where the semicircle is tangent to the horizontal axis showing the real component of the combined resistance of the molten slag are known. sol +Charge transfer resistance R ct It was found that it is possible to calculate That is, in the method for analyzing molten slag according to the present embodiment, for example, plots at the halfway position of the semicircle are not required, so the solution resistance R of the reference molten slag is obtained by measuring the impedance of the molten slag only by the frequency tangent to the horizontal axis. sol and the solution resistance of the reference molten slag R sol +Charge transfer resistance R ct The measurement time can be shortened. Thus, in the second step, the combined resistance of the reference molten slag is calculated by multiplying the solution resistance R sol and the charge transfer resistance R ct can be separated and rapidly calculated.
[0046] Specifically, the reference impedance Z of the reference molten slag ref The solution resistance of the reference molten slag R is calculated from the combined resistance of the reference molten slag and sol and the charge transfer resistance R ct In order to calculate these resistances, it is necessary to create a Nyquist plot of the reference molten slag. Then, the combined resistance of the reference molten slag is calculated from the created Nyquist plot of the reference molten slag and the following relational expression (1). Here, the Nyquist plot is an impedance spectrum plotted on a complex plane, and is generally plotted to draw a semicircle around a solid line. A Nyquist plot curve can be obtained by multiple Nyquist plots based on a large amount of experimental data to draw the semicircle. That is, in order to obtain a Nyquist plot curve, a number of reference impedances Z ref and the combined resistance of the reference molten slag, generate numerous Nyquist plots, and perform fitting on these numerous Nyquist plots, which requires a lot of work.
[0047]
number
[0048] 2 is a graph showing the behavior of the impedance of the molten slag when the frequency is swept using a molten slag analyzer used in the molten slag analysis method according to the present embodiment. In FIG. 2, the horizontal axis shows the real component of the impedance, and the vertical axis shows the imaginary component of the impedance. As shown in Figure 2, the intersection point P 1 , P 2 Among them, the intersection point P located farther from the origin (0,0) 2 (R sol +R ct , 0) is the combined resistance R of the reference molten slag. sol +R ct On the other hand, the intersection point P 1 , P 2 Among them, the intersection point P located closer to the origin (0,0) 1 (R sol , 0) is the solution resistance R of the reference molten slag. sol Corresponds to.
[0049] That is, the reference impedance Z of the reference molten slag ref From the combined resistance of the reference molten slag 210 and the reference molten slag 210, the solution resistance R sol and the charge transfer resistance R ctIn order to separate and calculate the above, it is not necessary to have a very large number of Nyquist plots that form a Nyquist plot curve. 1 , P 2 It is necessary to calculate only the horizontal axis value. That is, at the two points where the plot converges on the horizontal axis, R sol , and R sol +R ct Therefore, it is sufficient to measure only the points that converge on the respective real axes, and the solution resistance R can be determined by impedance measurements at only two frequencies without performing numerous Nyquist plots to create Nyquist plot curves. sol and the charge transfer resistance R ct It is possible to obtain: In other words, the method for analyzing molten slag according to this embodiment can quickly and accurately determine the solution resistance R by measuring the impedance at two frequencies. sol and the charge transfer resistance R ct It is possible to obtain:
[0050] Here, the reason why only one semicircle appears in the impedance outline shown in Figure 2 is that the pair of electrodes 104 equipped in the molten slag analyzing apparatus 100 are made of the same material so that their electrochemical properties are equivalent, and the semicircles overlap to appear as a single semicircle. In other words, in the method for analyzing molten slag according to this embodiment, the aim is to make it easier to interpret the Nyquist diagram by selecting electrodes with similar electrochemical properties. The solution resistance of the reference molten slag R sol is the liquid resistance of the molten slag between the pair of electrodes 104 and depends on the inter-electrode distance formed between the pair of electrodes 104. The charge transfer resistance R of the reference molten slag c is the transfer resistance of the charge that moves with the electrode reaction in the electrode 104, and is not dependent on the inter-electrode distance formed between the pair of electrodes 104.
[0051] In the second step, the solution resistance R of the reference molten slagsol and charge transfer resistance R c A composition content calibration curve is created based on the above. The composition content calibration curve can be created by multiple regression analysis. Specifically, the content of the composition contained in the reference molten slag, which is already known or has been prepared in advance, is used as the objective variable, and the solution resistance R sol and charge transfer resistance R c A calibration curve of the composition component contents can be created from a regression equation obtained by multiple regression using the above as explanatory variables. The compositional component content calibration curve covers all the compositional components contained in the reference molten slag and the measurement molten slag, and includes CaO, SiO 2 , FeO, Al 2 O 3 , MgO, MnO, P 2 O 5 , silicon, sulfur, etc.
[0052] In the second step, the compositional component contained in the reference molten slag may be iron oxide, and the compositional component content calibration curve may be an iron oxide content calibration curve. That is, in the second step, focusing on iron oxide required for removing phosphorus contained in the molten iron by a dephosphorization reaction, an iron oxide content calibration curve is created as a compositional component content calibration curve of the reference molten slag used to estimate its content.
[0053] In the second step, the compositional components may be specific compositional components necessary for calculating the basicity of the reference molten slag, and the compositional component content calibration curve may be a basicity calibration curve. That is, the second step includes calculating the content of CaO, SiO 2 Focusing on the contents of, a basicity calibration curve is created as a calibration curve of the content of the compositional components of the reference molten slag used to calculate a predetermined basicity defined from these contents.
[0054] The basicity can be appropriately set according to the compositional components contained in the reference molten slag. 2In the case of a molten slag of the SiO-FeO system, the basicity of the reference molten slag may be a basicity B1 defined by the following relational expression (2): 2 The basicity B1 can be calculated by dividing the basicity B1 by the mass% of the actual converter. The basicity B1 is the most important index in an actual converter. In other words, the method for analyzing molten slag according to the present embodiment has a technical significance in that it can estimate the basicity B1, which is the most important index in an actual converter, with high accuracy.
[0055]
number
[0056] The reference molten slag is, for example, CaO-SiO 2 -MgO-Al 2 O 3 The reference molten slag 210 may be a -FeO-based molten slag 200. The basicity of the reference molten slag may be a basicity B2 defined by the following relational expression (3). The basicity B2 is determined by the mass percentage of CaO, the mass percentage of MgO, and the mass percentage of Al contained in the reference molten slag 210. 2 O 3 The sum of the mass% of SiO 2 It can be calculated by dividing the mass % by the mass %.
[0057]
number
[0058] <Third step: Step of measuring the slag temperature and impedance of the molten slag for measurement> The method for analyzing molten slag in this embodiment includes a third step of measuring the slag temperature of the molten slag to be measured and the measurement impedance by passing an alternating current between a pair of electrodes immersed in the molten slag to be measured at the slag temperature. That is, in the third step, the slag temperature T and the measured impedance Z of the molten slag for measurement are measured in the same manner as in the first and second steps. Furthermore, in the same manner as in the first and second steps, the solution resistance R of the molten slag for measurement is calculated based on the measured impedance Z. sol and charge transfer resistance R c are separated and calculated. The space between a pair of electrodes 104 immersed in the molten slag for measurement functions as a measurement electrode for measuring the measurement impedance Z.
[0059] <Fourth step: A step of estimating the compositional component contents of the molten slag for measurement based on the calibration curve> The method for analyzing molten slag according to the present embodiment includes a fourth step of estimating the content of the compositional components contained in the molten slag for measurement based on the measured impedance and the compositional component content calibration curve. That is, the fourth step is to estimate the solution resistance R of the molten slag for measurement calculated from the measured impedance Z measured at the slag temperature T of the molten slag for measurement based on the composition content calibration curve created in the second step. sol and charge transfer resistance R c This is a process of estimating the contents of the composition components corresponding to the above.
[0060] Here, when the composition content calibration curve created in the second step is an iron oxide content calibration curve, the content of iron oxide contained in the molten slag for measurement corresponding to the slag temperature T of the molten slag for measurement can be estimated. When the composition content calibration curve created in the second step is a basicity calibration curve, the content of CaO, SiO 2 The basicity of the molten slag for measurement can be estimated from the content.
[0061] Based on the iron oxide content and basicity of the molten slag for measurement estimated in the fourth step, an appropriate amount of refining agent to be added to the molten steel can be determined. By adding an appropriate amount of refining agent to the molten steel, it is possible to suppress an increase in production costs associated with adding excess quicklime to the molten steel. Furthermore, by adding an appropriate amount of refining agent to the molten steel, it is possible to prevent foaming at the end of phosphorus blowing, poor slag removal during the process, and the progression of multiple phosphorus reactions during decarburization blowing. In addition, the blowing pattern can be determined based on the iron oxide content and basicity of the measurement molten slag estimated in the fourth step.
[0062] In this way, the method for analyzing molten slag according to the present embodiment includes the first to fourth steps, and therefore the reference slag temperature T ref , reference impedance Z ref Solution resistance R based on sol and charge transfer resistance R c The compositional component content calibration curve can be created by calculating the above, and the compositional component contents of the molten slag to be measured can be estimated quickly and accurately by utilizing the calibration curve.
[0063] As described above, according to the first embodiment of the present invention, the basicity and the iron oxide content can be estimated quickly and accurately without sampling the molten slag during blowing.
[0064] [Second embodiment] The molten slag analysis method according to the second embodiment will be described. The molten slag analysis method according to this embodiment is characterized in that in the molten slag analysis method according to the above embodiment, the voltage applied between the pair of electrodes is 10 mV or more and 1.0 V or less, and the two kinds of frequencies are 10 Hz or less and 10 kHz or more. Below, the characteristic features of the molten slag analysis method according to this embodiment will be described.
[0065] In the method for analyzing molten slag according to this embodiment, the voltage applied between the pair of electrodes 104 is 10 mV or more and 1.0 V or less. If the voltage applied between the pair of electrodes 104 is 10 mV or more, it is preferable because the effect of noise does not appear in the frequency response when applying a voltage between the pair of electrodes. If the voltage applied between the pair of electrodes is 1.0 V or less, it is preferable because the surface state of the pair of electrodes does not change.
[0066] Furthermore, in the method for analyzing molten slag according to this embodiment, the two frequencies when applying a voltage between the pair of electrodes are 10 Hz or less and 10 kHz or more. That is, by setting the two frequencies when applying a voltage between the pair of electrodes to a low-frequency frequency of 10 Hz or less and a high-frequency frequency of 10 kHz or more, the reference impedance Z ref and the measured impedance Z can be measured with high accuracy, and the measured impedance Z ref Based on the solution resistance R of the molten slag for measurement sol and charge transfer resistance R c This is preferable because it is possible to obtain the value with high accuracy.
[0067] In the method for analyzing molten slag according to the present embodiment, two frequencies are set when applying a voltage between a pair of electrodes: a low frequency and a high frequency. The low frequency may be set to 0.1 Hz or more and 10 Hz or less. The high frequency may be set to 10 kHz or more and 100 kHz or less.
[0068] In this way, the method for analyzing molten slag according to the present embodiment focuses on the voltage applied between a pair of electrodes and two types of frequencies when applying the voltage between the electrodes, and calculates the reference impedance Z ref The measured impedance Z can be measured with high accuracy. ref Based on the measured impedance Z, the solution resistance R of the reference molten slag and the measured impedance Z sol and charge transfer resistance R cIt is possible to accurately calculate the content of the compositional components and create a calibration curve for the compositional components, and the content of the compositional components contained in the molten slag to be measured can be estimated using the calibration curve.
[0069] As described above, according to the second embodiment of the invention, by setting the applied voltage between a pair of electrodes and two types of frequencies, the reference impedance and the measured impedance can be accurately measured, and the basicity and iron oxide content of the molten slag can be accurately estimated.
[0070] [Third embodiment] The molten slag analysis method according to the third embodiment will be described. The molten slag analysis method according to this embodiment is characterized in that the difference in immersion potential between the pair of electrodes in the molten slag to be measured is less than 50 mV in the molten slag analysis method according to the above embodiment. The characteristic parts included in the molten slag analysis method according to this embodiment will be described below.
[0071] In the method for analyzing a molten slag according to the present embodiment, the difference in immersion potential in the molten slag to be measured is less than 50 mV. The difference in immersion potential in the molten slag to be measured is the potential difference measured between a pair of electrodes 104. If the difference in immersion potential in the molten slag to be measured is less than 50 mV, it can be considered that the electrochemical properties of the electrode 104R and the electrode 104L constituting the pair of electrodes 104 are substantially identical. In other words, since the electrochemical properties of the electrode 104R and the electrode 104L constituting the pair of electrodes 104 are substantially identical, it can be considered that the electrodes 104R and 104L constituting the pair of electrodes 104 are made of the same material.
[0072] Since the pair of electrodes 104 are made of the same material, in the second step included in the method for analyzing molten slag according to this embodiment, the reference impedance Z ref The solution resistance R of the reference molten slag calculated from sol and charge transfer resistance R cis used to calculate the solution resistance R of the reference molten slag, and only one Nyquist curve is formed from the semicircle. sol and charge transfer resistance R c This is preferable because it makes the Nyquist curve used in calculating the Nyquist curve clear and improves the accuracy of the analysis of the Nyquist curve.
[0073] On the other hand, if the difference in immersion potential in the molten slag to be measured is 50 mV or more, the electrochemical properties of the electrode 104R and the electrode 104L constituting the pair of electrodes 104 cannot be regarded as being substantially the same. For this reason, since the pair of electrodes 104 cannot be regarded as being made of the same material, in the second step included in the method for analyzing molten slag according to this embodiment, the reference impedance Z ref The solution resistance R of the reference molten slag calculated from sol and charge transfer resistance R c is used to calculate the solution resistance R of the reference molten slag, and the Nyquist curve formed by the semicircle is not the only one. sol and charge transfer resistance R c This is not preferable because the Nyquist curve used in calculating the Nyquist curve becomes unclear and the accuracy of the analysis of the Nyquist curve does not improve.
[0074] In this manner, in the method for analyzing molten slag according to the present embodiment, the difference in immersion potential in the molten slag to be measured is set to less than 50 mV, so that the electrochemical properties of the electrodes 104R and 104L constituting the pair of electrodes 104 are set to be substantially the same. sol and charge transfer resistance R c By improving the accuracy of the analysis of the Nyquist curve used in calculating the above, the accuracy of the composition component content calibration curve is improved.
[0075] As described above, according to the third embodiment of the present invention, the solution resistance R of the reference molten slag sol and charge transfer resistance R cBy improving the accuracy of the analysis of the Nyquist curve used in calculating the basicity and iron oxide content of the molten slag, it is possible to estimate the basicity and iron oxide content of the molten slag with great accuracy.
[0076] [Other embodiments] Although the present invention has been described above with reference to the embodiments, the present invention is not limited to the above-mentioned embodiments. Various modifications that can be understood by those skilled in the art can be made to the configuration and details of the present invention within the technical scope of the present invention. In addition, systems or devices that combine the separate features included in each embodiment in any way are also included in the technical scope of the present invention. EXAMPLES
[0077] The effects of the present invention will be specifically described below based on examples, but the present invention is not limited to these examples.
[0078] (Example 1) The slag composition of the molten slag present in the converter during blowing was analyzed by adopting the method for analyzing the molten slag composition according to the present invention. Specifically, a sublance was installed in an induction melting furnace equipped with a magnesium oxide crucible and a ramming material, and a probe equipped with two platinum electrodes and a temperature sensor for measuring the temperature of the molten slag was installed. The distance between the platinum electrodes was set to 10 mm.
[0079] Next, the sublance with the probe attached was lowered during blowing in the converter to immerse the platinum electrode and temperature sensor in the molten slag, and the temperature and impedance of the molten slag were measured. The impedance measurement of the molten slag was performed under the conditions of an applied voltage of 1.0 V and a measurement frequency of 10 kHz and 1.0 Hz. Here, a basicity calibration curve was prepared, which shows the relationship between the impedance of the molten slag obtained in advance and the basicity of the molten slag calculated from the content of each composition component contained in the molten slag. Based on the basicity calibration curve, the basicity of the molten slag calculated from the composition components contained in the molten slag was calculated from the measured impedance value.
[0080] Furthermore, an iron oxide calibration curve was prepared, which shows the relationship between the impedance of the molten slag obtained in advance and the iron oxide content in the molten slag calculated from the content of each composition component in the molten slag. Based on the iron oxide calibration curve, the iron oxide content in the molten slag was calculated from the measured impedance value.
[0081] Comparative Example 1 X-ray fluorescence analysis was used to analyze the composition of the molten slag present in the converter during blowing. Specifically, the molten slag was sampled at the same time as the impedance measurement of the molten slag performed in Example 1, and the collected sample was processed into an analytical specimen, after which the slag composition of the molten slag was analyzed by X-ray fluorescence analysis.
[0082] In the fluorescent X-ray analysis method, a prepared analysis sample is irradiated with fluorescent X-rays (primary X-rays). By irradiating the analysis sample with fluorescent X-rays (primary X-rays), the intensity of the fluorescent X-rays (secondary X-rays) generated from the analysis sample is measured for each element. Then, using a calibration curve that shows the relationship between the fluorescent X-ray intensity of each element and the content of each element, which was created in advance, the content of each element was determined from the measured value of the fluorescent X-ray intensity. Based on the content of each element contained in the molten slag calculated from the measured value of the fluorescent X-ray intensity, the basicity and iron oxide content of the molten slag were determined.
[0083] Fig. 3 shows the analysis results of the basicity of the molten slag measured in Example 1 and Comparative Example 1. Specifically, Fig. 3(a) is a graph showing a comparison between Example 1, in which the basicity of the molten slag at a temperature of 1290 to 1310°C was calculated using the method for analyzing the molten slag composition according to the present invention, and Comparative Example 1, in which the basicity was calculated using the fluorescent X-ray analysis method. Fig. 3(b) is a graph showing a comparison between Example 1, in which the basicity of the molten slag at a temperature of 1390 to 1410°C was calculated using the method for analyzing the molten slag composition according to the present invention, and Comparative Example 1, in which the basicity was calculated using the fluorescent X-ray analysis method (the fluorescent X-ray analysis result is referred to as actual result).
[0084] According to Figures 3(a)-(b), the regression coefficient R calculated from these graphs 2 The regression coefficients R 2 This shows that the method for analyzing the composition of molten slag according to the present invention can estimate the basicity of molten slag with extremely high accuracy.
[0085] Fig. 4 shows the analysis results of the iron oxide content of the molten slag measured in Example 1 and Comparative Example 1. Specifically, Fig. 4(a) is a graph comparing the iron oxide content of molten slag at a temperature of 1290 to 1310°C calculated using the molten slag composition analysis method according to the present invention in Example 1 with that calculated using fluorescent X-ray analysis in Comparative Example 1. FIG. 4(b) is a graph showing a comparison between Example 1 of the invention in which the iron oxide content of molten slag having a temperature of 1390 to 1410°C was calculated using the method for analyzing the molten slag composition according to the present invention and Comparative Example 1 in which the iron oxide content was calculated using a fluorescent X-ray analysis method.
[0086] According to Figures 4(a)-(b), the regression coefficient R calculated from these graphs 2 were found to be 0.9520 and 0.9699, respectively. These regression coefficients R 2 This shows that the method for analyzing the composition of molten slag according to the present invention can estimate the iron oxide content of the iron oxide contained in the molten slag with extremely high accuracy.
[0087] In addition, in the method for analyzing molten slag according to the present invention, the time from immersion of the platinum electrode in the molten slag to deriving the estimated values of the basicity and iron oxide content of the molten slag was within 60 seconds. On the other hand, in the X-ray fluorescence analysis method employed in Comparative Example 1, the analysis of the slag composition of the molten slag present in the converter during blowing required more than 10 minutes for sampling the molten slag and processing the collected sample for analysis. From the above, it has been confirmed that the method for analyzing molten slag according to the present invention is a technique that can analyze the basicity and iron oxide content of molten slag quickly and with high accuracy. [Industrial Applicability]
[0088] According to the method for analyzing molten slag of the present invention, the basicity and iron oxide content can be estimated quickly and accurately without sampling the molten slag during blowing, which contributes to the related development of the iron and steel industry and is extremely useful industrially. [Explanation of symbols]
[0089] 100 Molten Slag Analyzer 101 Crucible 102 Ramming material 103 Induction melting furnace 104 Electrode 104R electrode (right side) 104L electrode (left side) 105 Temperature Sensor 106 Potentiostat 107 Conductor 108 Insulation Board 200 Molten Slag
Claims
1. A method for analyzing the composition of a molten slag, comprising the steps of: A first step of measuring a reference slag temperature of a reference molten slag and a reference impedance of the reference molten slag by passing an alternating current between a pair of electrodes immersed in the reference molten slag at the reference slag temperature; A second step of preparing a calibration curve of the content of the compositional components contained in the reference molten slag and the reference impedance measured in the first step; a third step of measuring a slag temperature of the molten slag to be measured and a measurement impedance by passing the AC current between the pair of electrodes immersed in the molten slag to be measured at the slag temperature; A method for analyzing molten slag, comprising a fourth step of estimating the content of the compositional components contained in the molten slag for measurement based on the measured impedance and the compositional component content calibration curve.
2. 2. The method for analyzing molten slag according to claim 1, wherein the composition component is iron oxide, and the composition component content calibration curve is an iron oxide content calibration curve.
3. The compositional components are specific compositional components necessary for calculating the basicity of the reference molten slag, The method for analyzing molten slag according to claim 1, characterized in that the composition component content calibration curve is a basicity calibration curve.
4. A method for analyzing molten slag described in any one of claims 1 to 3, characterized in that the reference impedance and the measured impedance are measured by passing alternating currents of two selected frequencies.
5. The voltage applied between the pair of electrodes is 10 mV or more and 1.0 V or less, The method for analyzing molten slag according to claim 4, characterized in that the two types of frequencies are 10 Hz or less and 10 kHz or more.
6. A method for analyzing molten slag according to any one of claims 1 to 3, characterized in that the difference in immersion potential between the pair of electrodes in the molten slag to be measured is less than 50 mV.
Citation Information
Patent Citations
Visualization device
JP2022099837A
Gas supply device
JP2025091919A
Device and Method for Processing Image Using Neural Network
KR102695997B1
Probe for measuring impedance and phase angle difference, and method for controlling slag composition in converter using the same
JP2022110303A
Slag component analysis method, slag basicity analysis method, and molten iron refining method
JP7111282B1
Cited By
Scrap material production equipment and scrap material production method
WO2026163935A1