Liquid crystal sealant

A curable resin composition with modified epoxy resins and additives addresses the issue of increased moisture permeability and reduced elasticity in (meth)acrylate resins, enhancing flexibility and maintaining display stability in liquid crystal displays.

JP7564549B2Active Publication Date: 2024-10-09KYORITSU KAGAKU SANGYO KK
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2021124171
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-07-29
Publication Date
2024-10-09
Estimated Expiration
2041-07-29

AI Technical Summary

Technical Problem

The (meth)acrylate resin with an alkylene oxide skeleton used in liquid crystal display manufacturing experiences increased moisture permeability as the modulus of elasticity decreases, compromising its flexibility.

Method used

A curable resin composition is formulated by replacing part or all of the epoxy groups of an epoxy resin with (meth)acrylic acid and/or (meth)acrylic anhydride, incorporating a photopolymerization initiator and/or a thermosetting agent, and optionally including additional curable resins, to enhance flexibility while maintaining low moisture permeability.

Benefits of technology

The composition effectively lowers the elastic modulus while suppressing moisture permeability, ensuring stable liquid crystal alignment and display characteristics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007564549000001
    Figure 0007564549000001
  • Figure 0007564549000002
    Figure 0007564549000002
  • Figure 0007564549000003
    Figure 0007564549000003
Patent Text Reader

Abstract

To provide a curable resin composition which has a high effect for reducing elastic modulus while suppressing aggravation of moisture vapor permeability.SOLUTION: A curable resin composition contains (A) an epoxy (meth)acrylate resin whose a part or all of an epoxy resin represented by formula (1) and / or an epoxy resin of the epoxy resin is modified with a (meth)acrylic acid and / or a (meth)acrylic acid anhydride, and (B) a photopolymerization initiator and / or a heat curing agent.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present invention relates to a curable resin composition. [Background technology]

[0002] In the manufacturing method of LCD elements, the dripping method is a method that allows a panel to be created by directly dripping liquid crystal into a closed loop of curable resin composition, vacuum laminating, and releasing the vacuum. This dripping method has many advantages, such as reducing the amount of liquid crystal used and shortening the time it takes to inject the liquid crystal into the panel, and is now the mainstream method for manufacturing LCD panels using large substrates. In methods that include the dripping method, a sealant and liquid crystal are applied and laminated, followed by gap clearance and alignment, and the sealant is cured, mainly by ultraviolet curing.

[0003] Patent Document 1 describes that the adhesiveness of a sealant for liquid crystal display elements and the flexibility of the cured product are improved by using a compound having an alkylene oxide skeleton introduced therein. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] International Publication No. 2018 / 116928 Summary of the Invention [Problem to be solved by the invention]

[0005] The (meth)acrylate resin having an alkylene oxide skeleton described in Patent Document 1 has a problem in that the moisture permeability decreases (i.e., the moisture permeability value increases) as the elastic modulus decreases (i.e., flexibility is improved). Therefore, an object of the present invention is to provide a curable resin composition that is highly effective in reducing the elastic modulus while suppressing the deterioration of moisture permeability. [Means for solving the problem]

[0006] The present invention relates to the following [1] to [4]. [1] (A) an epoxy resin represented by the following formula (1) and / or an epoxy (meth)acrylate resin in which part or all of the epoxy groups of the epoxy resin have been modified with (meth)acrylic acid and / or (meth)acrylic anhydride; (B) a photopolymerization initiator and / or a heat curing agent; A curable resin composition comprising: [ka] [During the ceremony, R 1 is an aliphatic hydrocarbon group having 4 to 12 carbon atoms and containing 0 to 3 unsaturated bonds, R 2 is an aliphatic hydrocarbon group having 4 to 12 carbon atoms and containing 0 to 3 unsaturated bonds. [2] The curable resin composition according to [1], wherein the epoxy resin represented by the formula (1) comprises an epoxy resin represented by the following formula (2): [ka] [3] The curable resin composition of [1] or [2] further comprising one or more curable resins selected from the group consisting of (C-1) a difunctional or higher functional epoxy resin (excluding the epoxy resin represented by formula (1)), (C-2) an epoxy (meth)acrylate resin in which some or all of the epoxy groups in the component (C-1) have been modified with (meth)acrylic acid and / or (meth)acrylic anhydride, and (C-3) other curable resins (excluding the component (A), the component (C-1), and the component (C-2)). [4] The curable resin composition according to any one of [1] to [3], which is a liquid crystal sealing agent. [Effects of the Invention]

[0007] According to the present invention, there is provided a curable resin composition that is highly effective in reducing the elastic modulus while suppressing deterioration in moisture permeability. DETAILED DESCRIPTION OF THE INVENTION

[0008] Preferred embodiments of the present invention will be described below. The term "(meth)acryloyl group" refers to an acryloyl group (CH2=CH2-C(=O)-) and / or a methacryloyl group (CH2=CH(CH3)-C(=O)-).

[0009] "(A) an epoxy resin represented by the following formula (1) and / or an epoxy (meth)acrylate resin in which part or all of the epoxy groups of the epoxy resin have been modified with (meth)acrylic acid and / or (meth)acrylic anhydride" is also referred to as "component (A)." The same applies to "(B) a photopolymerization initiator and / or a thermosetting agent," etc.

[0010] [Curable resin composition] The curable resin composition contains (A) an epoxy resin represented by the following formula (1) and / or an epoxy (meth)acrylate resin in which some or all of the epoxy groups of the epoxy resin have been modified with (meth)acrylic acid and / or (meth)acrylic anhydride, and (B) a photopolymerization initiator and / or a heat curing agent.

[0011] [ka]

[0012] [During the ceremony, R 1 is an aliphatic hydrocarbon group having 4 to 12 carbon atoms and containing 0 to 3 unsaturated bonds, R 2 is an aliphatic hydrocarbon group having 4 to 12 carbon atoms and containing 0 to 3 unsaturated bonds.

[0013] The curable resin composition is inhibited from deteriorating in moisture permeability, i.e., the curable resin composition has a small moisture permeability value. Furthermore, the curable resin composition is highly effective in reducing the elastic modulus, i.e., the curable resin composition has a smaller elastic modulus value.

[0014] <(A) An epoxy resin represented by formula (1) and / or an epoxy (meth)acrylate resin in which some or all of the epoxy groups of the epoxy resin have been modified with (meth)acrylic acid and / or (meth)acrylic anhydride> Examples of the component (A) include "(A-1) an epoxy resin represented by formula (1)," "(A-2) an epoxy (meth)acrylate resin in which some or all of the epoxy groups in the component (A-1) have been modified with (meth)acrylic acid and / or (meth)acrylic anhydride," and "a combination of the component (A-1) and the component (A-2)."

[0015] <(A-1) Epoxy resin represented by formula (1)> The component (A-1) is a curable component of the curable resin composition, and is also a raw material for the component (A-2) described below.

[0016] In formula (1), R 1 is a divalent aliphatic hydrocarbon group having 4 to 12 carbon atoms and containing 0 to 3 unsaturated bonds, and R 2 is a monovalent aliphatic hydrocarbon group having 4 to 12 carbon atoms and containing 0 to 3 unsaturated bonds. In this specification, "unsaturated bond" means an ethylenically unsaturated bond (C=C) and / or an acetylenically unsaturated bond (C≡C), and an ethylenically unsaturated bond is preferred. Furthermore, the aliphatic hydrocarbon group may be either linear or branched, but is preferably linear.

[0017] R 1 The number of unsaturated bonds contained in R is preferably 0 or 1. 1 is preferably an alkylene group having 4 to 12 carbon atoms or an alkenylene group having 4 to 12 carbon atoms.

[0018] R 2 The number of unsaturated bonds contained in R is preferably 0 to 2. 2 is particularly preferably an alkyl group having 4 to 12 carbon atoms, an alkenyl group having 4 to 12 carbon atoms, or an alkadienyl group having 4 to 12 carbon atoms.

[0019] Specific preferred examples of the component (A-1) include epoxy resins represented by the following formulas (2) to (11).

[0020] [ka] [ka]

[0021] The component (A-1) preferably contains one or more epoxy resins selected from the group consisting of epoxy resins represented by formula (2) to formula (11), and particularly preferably contains an epoxy resin represented by formula (2).

[0022] <(A-2) Epoxy (meth)acrylate resin in which part or all of the epoxy groups of the epoxy resin represented by formula (1) have been modified with (meth)acrylic acid and / or (meth)acrylic anhydride> Component (A-2) is a curable component of the curable resin composition. Here, the epoxy resin represented by formula (1), which is the raw material for component (A-2), is as described above. The epoxy (meth)acrylate resin is not particularly limited in proportion, as long as at least a portion of the epoxy groups in the epoxy resin represented by formula (1) are modified with (meth)acrylic acid and / or (meth)acrylic anhydride. Furthermore, the epoxy resin represented by formula (1), which is the raw material for component (A-2), including preferred embodiments, is as described above for component (A-1).

[0023] <Preferred Embodiments of Component (A)> From the viewpoint of further suppressing deterioration of moisture permeability, it is preferable that component (A) contains component (A-1). Also, from the viewpoint of further enhancing the effect of reducing elastic modulus, it is preferable that component (A) contains component (A-2). Furthermore, from the viewpoint of efficiently achieving both suppression of deterioration in moisture permeability and a low elastic modulus, it is preferable that component (A) contains an epoxy resin represented by formula (2) and / or an epoxy (meth)acrylate resin in which some or all of the epoxy groups of the epoxy resin represented by formula (2) have been modified with (meth)acrylic acid and / or (meth)acrylic anhydride. When component (A) contains an epoxy resin represented by formula (2), it may further contain one or more epoxy resins selected from the group consisting of epoxy resins represented by formulas (3) to (11). Furthermore, when component (A) contains an epoxy (meth)acrylate resin in which some or all of the epoxy groups of an epoxy resin represented by formula (2) have been modified with (meth)acrylic acid and / or (meth)acrylic anhydride, it may further contain an epoxy (meth)acrylate resin in which some or all of the epoxy groups of one or more epoxy resins selected from the group consisting of epoxy resins represented by formulas (3) to (11) have been modified with (meth)acrylic acid and / or (meth)acrylic anhydride.

[0024] Component (A) is commercially available or can be prepared according to known methods. For example, commercially available epoxy resins represented by formula (1) include NC-514 and NC-514S manufactured by Cardrite Co., Ltd. Here, NC-514 and NC-514S manufactured by Cardrite Co., Ltd. are mixtures of epoxy resins represented by formula (1), containing an epoxy resin represented by formula (2) as the main component and one or more epoxy resins selected from the group consisting of epoxy resins represented by formulas (3) to (11). The component (A) may be one type or a combination of two or more types.

[0025] <(B) Photopolymerization initiator and / or heat curing agent> The photopolymerization initiator is a component that can convert the curable resin composition into a photopolymerizable and curable composition. The heat curing agent is a component that can convert the curable resin composition into a heat curable composition. The photopolymerization initiator and / or heat curing agent can be appropriately selected depending on the type of curable resin contained in the curable resin composition and the desired curing conditions (energy ray curing and / or heat curing). Therefore, examples of component (B) include photopolymerization initiators, heat curing agents, and combinations of photopolymerization initiators and heat curing agents.

[0026] <Photopolymerization initiator> The photopolymerization initiator may be a radical polymerization initiator, an anionic polymerization initiator, and / or a cationic polymerization initiator.

[0027] Examples of radical polymerization initiators include benzoins, acetophenones, benzophenones, thioxanthones, α-acyloxime esters, phenylglyoxylates, benzils, azo compounds, diphenyl sulfide compounds, acylphosphine oxide compounds, benzoin ethers, anthraquinones, and organic peroxides. Radical polymerization initiators are preferably those that have low solubility in liquid crystals and have reactive groups that do not gasify upon exposure to light. Furthermore, as a radical polymerization initiator, a polymerization initiator that is a mixture of a polyether compound having a dialkylaminobenzoyl group and a polyether compound having a group in which one hydrogen atom has been removed from thioxanthone, as described in JP 2020-076794, is preferred. A polymerization initiator that is a mixture of a compound obtained by reacting a compound having at least two epoxy groups with dimethylaminobenzoic acid and a compound obtained by reacting a compound having at least two epoxy groups with hydroxythioxanthone is particularly preferred.

[0028] Examples of the anionic polymerization initiator include imidazoles, amines, phosphines, organic metal salts, metal chlorides, and organic peroxides.

[0029] Examples of the cationic polymerization initiator include onium salts, iron allene complexes, titanocene complexes, arylsilanol aluminum complexes, Lewis acid compounds, Bronsted acid compounds, benzylsulfonium salts, thiophenium salts, thioranium salts, benzylammonium, pyridinium salts, hydrazinium salts, carboxylic acid esters, sulfonic acid esters, amine imides, sulfone compounds, sulfonic acid esters, sulfonimides, disulfonyldiazomethanes, and amines.

[0030] The photopolymerization initiator is commercially available or can be prepared according to known methods. The photopolymerization initiator may be one type or a combination of two or more types.

[0031] <Thermal hardener> The heat curing agent is not particularly limited, and examples thereof include amine-based heat curing agents such as organic acid dihydrazide compounds, amine adducts, imidazole and its derivatives, dicyandiamide, aromatic amines, epoxy-modified polyamines, and polyaminoureas. Preferred examples include organic acid dihydrazides such as VDH (1,3-bis(hydrazinocarboethyl)-5-isopropylhydantoin), ADH (adipic acid dihydrazide), UDH (7,11-octadecadiene-1,18-dicarbohydrazide), and LDH (octadecane-1,18-dicarboxylic acid dihydrazide); polyamine-based compounds sold by ADEKA Corporation as ADEKA Hardener EH-5030S, etc.; and amine adducts sold by Ajinomoto Fine-Techno Co., Inc. as Amicure PN-23, Amicure PN-30, Amicure MY-24, Amicure MY-H, etc. The heat curing agent may be one type or a combination of two or more types.

[0032] <Other ingredients> The curable resin composition may contain a curable resin other than the component (A) (component (C)) and / or a component other than the component (C) (component (D)) depending on the purpose, as long as the effects of the present invention are not impaired. Examples of the component (D) include a silane coupling agent, a polymerization inhibitor, an organic filler, and an inorganic filler. Note that the components (C) and (D) are not the components (A) and (B) described above.

[0033] <<Curable resin other than component (A) (component (C))>> Examples of the component (C) include (C-1) difunctional or higher functional epoxy resins (excluding epoxy resins represented by formula (1)), (C-2) epoxy (meth)acrylate resins in which some or all of the epoxy groups in the component (C-1) have been modified with (meth)acrylic acid and / or (meth)acrylic anhydride, and (C-3) other curable resins (excluding the components (A), (C-1), and (C-2)).

[0034] <(C-1) Difunctional or higher epoxy resin (excluding epoxy resins represented by formula (1))>> The component (C-1) is not particularly limited as long as it is an epoxy resin other than that represented by formula (1), and examples thereof include bisphenol A-type epoxy resins, bisphenol F-type epoxy resins, bisphenol S-type epoxy resins, phenol novolac-type epoxy resins, cresol novolac-type epoxy resins, bisphenol A novolac-type epoxy resins, bisphenol F novolac-type epoxy resins, alicyclic epoxy resins, aliphatic linear epoxy resins, glycidyl ester-type epoxy resins, glycidyl amine-type epoxy resins, hydantoin-type epoxy resins, isocyanurate-type epoxy resins, and phenol novolac-type epoxy resins having a triphenolmethane skeleton. Other examples include glycidyl ethers of difunctional or higher phenols, glycidyl ethers of difunctional or higher alcohols, and their halides and hydrogenated derivatives. Examples of trifunctional and tetrafunctional epoxy resins include the epoxy resins described in JP 2012-077202 A. The number of epoxy functionalities of the component (C-1) is not particularly limited, but is preferably 2 to 4. The component (C-1) is preferably an epoxy resin having a bisphenol structure, and is particularly preferably at least one selected from the group consisting of bisphenol A type epoxy resins and bisphenol F type epoxy resins. The component (C-1) may be one type or a combination of two or more types.

[0035] <(C-2) Epoxy (meth)acrylate resin> The component (C-2) is an epoxy (meth)acrylate resin in which some or all of the epoxy groups in the component (C-1) have been modified with (meth)acrylic acid and / or (meth)acrylic anhydride. That is, the component (C-2) has both epoxy groups and (meth)acryloyl groups in the resin, or has no epoxy groups and (meth)acryloyl groups in the resin. Here, the component (C-1), including preferred examples, is as described above. The component (C-2) is particularly preferably an epoxy (meth)acrylate resin in which some of the epoxy groups of a difunctional epoxy resin have been modified with (meth)acrylic acid and / or (meth)acrylic anhydride. The component (C-2) may be one type or a combination of two or more types.

[0036] <(C-3) Other curable resins> The component (C-3) is not particularly limited as long as it is a curable resin other than the components (A), (C-1), and (C-2). Examples include conventional resins having unsaturated groups and / or epoxy groups, resins having one epoxy group, and resins having neither unsaturated groups nor epoxy groups, which are used as the base resin of curable resin compositions. Here, "unsaturated groups" refers to ethylenically unsaturated groups and / or acetylenically unsaturated groups. The component (C-3) is appropriately selected from cationic polymerizable resins, radically polymerizable resins, and / or anionic polymerizable resins depending on the type of polymerization initiator and / or thermosetting agent contained in the curable resin composition.

[0037] Examples of resins having an unsaturated group include (meth)acrylate compounds, aliphatic acrylamide compounds, alicyclic acrylamide compounds, aromatic acrylamide compounds, N-substituted acrylamide compounds, and diene polymers (e.g., polybutadiene polymers, polyisoprene polymers, etc.). The functionality of the (meth)acrylate compound can be monofunctional, difunctional, or polyfunctional (e.g., trifunctional or higher), and is preferably difunctional or trifunctional or higher.

[0038] The bifunctional (meth)acrylate compound is preferably one or more compounds selected from the group consisting of tricyclodecane dimethanol di(meth)acrylate, dimethylol dicyclopentane di(meth)acrylate, EO-modified 1,6-hexanediol di(meth)acrylate, EO-modified bisphenol A di(meth)acrylate, PO-modified bisphenol A di(meth)acrylate, polyester di(meth)acrylate (e.g., ARONIX M-6100, manufactured by Toa Gosei Co., Ltd.), polyethylene glycol di(meth)acrylate (e.g., 4G, manufactured by Shin-Nakamura Chemical Co., Ltd.), and silicon di(meth)acrylate (e.g., EBECRYL 350, manufactured by Daicel-Allnex Corporation). Here, "EO" means ethylene oxide, and "PO" means propylene oxide.

[0039] The tri- or higher functional polyfunctional (meth)acrylate compound is preferably one or more compounds selected from EO-modified glycerol tri(meth)acrylate (trifunctional), PO-modified glycerol tri(meth)acrylate (trifunctional), pentaerythritol tri(meth)acrylate (trifunctional), dipentaerythritol hexa(meth)acrylate (hexafunctional), and pentaerythritol tetra(meth)acrylate (tetrafunctional).

[0040] Further, examples of resins having unsaturated groups include epoxy resins modified with a modifying compound in which all of the epoxy groups of the epoxy resin have unsaturated groups (excluding (meth)acrylic acid and acrylic anhydride). Resins having one epoxy group include aromatic epoxy resins and aliphatic epoxy resins. Examples of resins having neither an unsaturated group nor an epoxy group include modified epoxy resins in which all of the epoxy groups of an epoxy resin have been modified with a modifying compound having no unsaturated groups, and urethane resins formed from a hydroxyl group-containing compound and an isocyanate group-containing compound. The component (C-3) may be one type or a combination of two or more types.

[0041] The component (C) may be one type or a combination of two or more types. For example, the component (C) may be a combination of one or more types of component (C-1) and one or more types of component (C-2).

[0042] <<Other ingredients other than ingredient (C) (ingredient (D))>> Examples of the component (D) include a silane coupling agent, a polymerization inhibitor, an organic filler, and an inorganic filler.

[0043] <Silane coupling agents> Examples of silane coupling agents include silane compounds having one or more reactive functional groups selected from the group consisting of epoxy groups, alkenyl groups (e.g., vinyl groups), (meth)acryloyl groups, primary or secondary amino groups, mercapto groups, isocyanato groups, ureido groups, and halogen atoms, or alkyl groups substituted with such groups, and one or more alkoxy groups, and may also have unsubstituted alkyl groups. The reactive functional groups may be bonded to the silicon atoms of the silane compounds as alkyl groups substituted with the reactive functional groups.

[0044] Specific examples of the silane coupling agent include silane compounds having an epoxy group and an alkoxy group, and optionally having an alkyl group, such as 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, and 3-glycidoxypropyltriethoxysilane; silane compounds having an alkenyl group and an alkoxy group, and optionally having an alkyl group, such as vinyltrimethoxysilane and p-styryltrimethoxysilane; silane compounds having a (meth)acrylic group and an alkoxy group, and optionally having an alkyl group, such as 3-methacryloxypropylmethyldimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropylmethyldiethoxysilane, 3-methacryloxypropyltriethoxysilane, and 3-acryloxypropyltrimethoxysilane; N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane, N-2-(acrilicoxypropyl)-3-aminopropylmethyldimethoxysilane, Examples of suitable silane compounds include silane compounds having a primary or secondary amino group and an alkoxy group, and optionally an alkyl group, such as N-(aminoethyl)-3-aminopropyltrimethoxysilane, N-2-(aminoethyl)-3-aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-triethoxysilyl-N-(1,3-dimethyl-butylidene)propylamine, and N-phenyl-3-aminopropyltrimethoxysilane; and silane compounds having one or more groups selected from the group consisting of mercapto groups, isocyanato groups, ureido groups, and halogen atoms, and one or more alkoxy groups, and optionally an alkyl group, such as 3-ureidopropyltriethoxysilane, 3-chloropropyltrimethoxysilane, 3-mercaptopropylmethyldimethoxysilane, 3-mercaptopropyltrimethoxysilane, bis(triethoxysilylpropyl)tetrasulfide, and 3-isocyanatopropyltriethoxysilane. The silane coupling agent may be one type or a combination of two or more types.

[0045] Examples of inorganic fillers include calcium carbonate, magnesium carbonate, barium sulfate, magnesium sulfate, aluminum silicate, titanium oxide, alumina, zinc oxide, silicon dioxide (precipitated silica, fumed silica (fumed silica), etc.), kaolin, talc, glass beads, sericite activated clay, aluminum hydroxide, asbestos powder, copper oxide, copper hydroxide, iron oxide, lead oxide, magnesium oxide, tin oxide, carbon, mica, smectite, carbon black, bentonite, aluminum nitride, and silicon nitride. The inorganic fillers may be used alone or in combination of two or more.

[0046] Examples of organic fillers include acrylic particles, polymethyl methacrylate, polystyrene (polystyrene beads), copolymers obtained by copolymerizing the monomers constituting these (i.e., methyl methacrylate or styrene) with other monomers, polyethylene particles, polysiloxane resin particles, polyamide particles, polyester fine particles, polyurethane fine particles, and rubber fine particles (acrylic rubber particles, isoprene rubber particles). The organic filler may have a core-shell structure. The organic filler may be one type or a combination of two or more types.

[0047] The average particle size of the inorganic filler and the organic filler is not particularly limited, but is preferably 0.01 μm to 10 μm, and particularly preferably 1 μm to 5 μm. The average particle size of the inorganic filler and the organic filler can be measured using a laser diffraction particle size distribution analyzer.

[0048] Examples of the polymerization inhibitor include hydroquinone, paramethoxyphenol, and 2,6-di-t-butyl-4-cresol. Components other than those mentioned above can be appropriately selected from known components used in curable resin compositions.

[0049] The component (D) may be one type or a combination of two or more types. For example, the component (D) may be a combination of one or more silane coupling agents and one or more polymerization inhibitors.

[0050] <Content of each ingredient> In the curable resin composition, the content of each component is preferably as follows: When the curable resin composition does not contain the component (C), "100 parts by mass of the total of the component (A) and the component (C)" means "100 parts by mass of the component (A)." The content of component (A) is preferably 10 to 100 parts by mass, and particularly preferably 30 to 90 parts by mass, per 100 parts by mass of the combined total of components (A) and (C). Furthermore, when component (A) includes component (A-1), the content of the epoxy resin represented by formula (2) per 100 parts by mass of component (A-1) is preferably 5 to 80 parts by mass, and particularly preferably 10 to 60 parts by mass. Furthermore, in the above case, the total content of the epoxy resins represented by formula (2) to formula (11) per 100 parts by mass of component (A-1) is preferably 5 to 100 parts by mass, particularly preferably 10 to 80 parts by mass, and even more preferably 15 to 60 parts by mass. When component (A) contains component (A-2), the content of the epoxy (meth)acrylate resin of the epoxy resin represented by formula (2) per 100 parts by mass of component (A-2) is preferably 5 to 80 parts by mass, and particularly preferably 10 to 60 parts by mass. Furthermore, in the above case, the total content of the epoxy (meth)acrylate resin of the epoxy resin represented by formula (2) to the epoxy (meth)acrylate resin of the epoxy resin represented by formula (11) per 100 parts by mass of component (A-2) is preferably 5 to 100 parts by mass, particularly preferably 10 to 80 parts by mass, and even more preferably 15 to 60 parts by mass. The content of the photopolymerization initiator is preferably 0.1 to 10 parts by mass, and particularly preferably 0.5 to 5 parts by mass, per 100 parts by mass of the total of the components (A) and (C). The content of the heat curing agent is preferably 5 to 50 parts by mass, and particularly preferably 10 to 40 parts by mass, per 100 parts by mass of the total of the components (A) and (C). The content of the component (C) is preferably the same as the content of the component (A) described above.

[0051] The total amount of the components (A), (B), and (C) relative to 100 parts by mass of the curable resin composition is preferably 50 to 100 parts by mass, and particularly preferably 60 to 100 parts by mass. When the curable resin composition does not contain the component (C), the term "the total amount of the components (A), (B), and (C)" refers to "the total amount of the components (A) and (B)."

[0052] <Method for preparing curable resin composition> The curable resin composition can be produced by mixing the components.

[0053] <Curing method> The curable resin composition can be cured by irradiation with energy rays such as ultraviolet rays and by applying heat, or by applying heat before, after, or simultaneously with irradiation with energy rays such as ultraviolet rays. Thus, the curable resin composition is a photo- (energy ray) curable, heat-curable, or energy ray and heat-curable composition.

[0054] <Application> The curable resin composition has reduced solubility in liquid crystal and can prevent contamination of the liquid crystal. Therefore, the curable resin composition can be used as a liquid crystal sealant (such as a liquid crystal sealant for display elements and a liquid crystal sealant for light control) and a sealant for various flexible displays such as organic EL displays.

[0055] A cured product of the curable resin composition is used to seal a liquid crystal display. Therefore, the present invention also covers a liquid crystal display sealed with the curable resin composition. Examples of a method for producing a liquid crystal display include a step of applying the curable resin composition to one of two transparent substrates with electrodes using a dispenser to form a pattern of the curable resin composition, a step of dropping liquid crystal onto the entire frame of the transparent substrate and immediately laminating the other transparent substrate, and a step of curing the composition by irradiating the seal pattern portion with light such as ultraviolet light, heating the curable resin composition, or applying heat before, after, or simultaneously with irradiating the seal pattern portion with energy rays such as ultraviolet light. [Example]

[0056] Next, specific embodiments of the present invention will be described in more detail with reference to examples, but the present invention is not limited to these examples.

[0057] 1. Manufacturing example (1) Partially methacrylated bisphenol A type epoxy resin 340.0 g of bisphenol A epoxy resin (EXA-850CRP, manufactured by DIC Corporation), 86.1 g of methacrylic acid (manufactured by Tokyo Chemical Industry Co., Ltd.), and 524 mg of triphenylphosphine (manufactured by Tokyo Chemical Industry Co., Ltd.) were mixed and stirred at 100-110°C. The reaction solution was subjected to acid value titration with aqueous sodium hydroxide solution (0.01 N) to calculate the amount of remaining methacrylic acid. The reaction rate was calculated from the amount of methacrylic acid initially added and the amount of remaining methacrylic acid. The reaction was continued with heating and stirring until the reaction rate reached 99.9% or higher. 418.0 g of a pale yellow, transparent, viscous partially methacrylated bisphenol A epoxy resin was obtained. The epoxy equivalent of the resulting resin was 470 g / eq.

[0058] (2) Partially methacrylated resin 1 108.0 g of epoxy resin (NC-514S, manufactured by Cardrite Co., Ltd.), 10.8 g of methacrylic acid (manufactured by Tokyo Chemical Industry Co., Ltd.), and 65.6 mg of triphenylphosphine (manufactured by Tokyo Chemical Industry Co., Ltd.) were mixed and stirred at 100-110°C. The reaction solution was subjected to acid value titration with aqueous sodium hydroxide solution (0.01 N) to calculate the amount of remaining methacrylic acid. The reaction rate was calculated from the amount of methacrylic acid initially added and the amount of remaining methacrylic acid. The reaction was continued with heating and stirring until the reaction rate reached 99.9% or higher. 114.0 g of partially methacrylated resin 1 was obtained. The epoxy equivalent of the resulting resin was 968 g / eq.

[0059] (3) Partially methacrylated resin 2 60.4 g of hexanediol diglycidyl ether (EX-212, Nagase ChemteX Corporation), 17.2 g of methacrylic acid (Tokyo Chemical Industry Co., Ltd.), and 104.9 mg of triphenylphosphine (Tokyo Chemical Industry Co., Ltd.) were mixed and stirred at 100-110°C. The reaction solution was subjected to acid value titration with aqueous sodium hydroxide (0.01 N) to calculate the amount of remaining methacrylic acid. The reaction rate was calculated from the amount of methacrylic acid initially added and the amount of remaining methacrylic acid. The reaction was continued with heating and stirring until the reaction rate reached 99.9% or higher. 72.2 g of partially methacrylated resin 2 was obtained. The epoxy equivalent of the resulting resin was 403 g / eq.

[0060] (4) Partially methacrylated resin 3 80.4 g of polyethylene glycol diglycidyl ether (EX-830, Nagase ChemteX Corporation), 12.9 g of methacrylic acid (Tokyo Chemical Industry Co., Ltd.), and 78.7 mg of triphenylphosphine (Tokyo Chemical Industry Co., Ltd.) were mixed and stirred at 100-110°C. The reaction solution was subjected to acid value titration with aqueous sodium hydroxide (0.01 N) to calculate the amount of remaining methacrylic acid. The reaction rate was calculated from the amount of methacrylic acid initially added and the amount of remaining methacrylic acid. The reaction was continued with heating and stirring until the reaction rate reached 99.9% or higher. 89.5 g of partially methacrylated resin 3 was obtained. The epoxy equivalent of the resulting resin was 663 g / eq.

[0061] (5) Photopolymerization initiator 1 26.8 g (0.1 epoxy equivalents) of polyethylene glycol diglycidyl ether (EX-830, Nagase ChemteX Corporation), 16.5 g (0.1 equivalents) of 4-dimethylaminobenzoic acid, 3.71 g (0.02 equivalents) of benzyltrimethylammonium chloride, and 25 g of MIBK (methyl isobutyl ketone) were placed in a flask and stirred at 110°C for 24 hours using an oil bath. The reaction mixture was cooled to room temperature, dissolved in 50 g of chloroform, and washed six times with 100 ml of water. The solvent in the organic phase was distilled off under reduced pressure, yielding 35.3 g of photopolymerization initiator 1.

[0062] (6) Photopolymerization initiator 2 26.8 g (0.1 epoxy equivalent) of polyethylene glycol diglycidyl ether (EX-830, Nagase ChemteX Corporation), 22.83 g (0.1 equivalent) of 2-hydroxy-9H-thioxanthen-9-one, 3.71 g (0.02 equivalent) of benzyltrimethylammonium chloride, and 40 g of MIBK were placed in a flask and stirred at 110°C for 72 hours using an oil bath. The reaction mixture was cooled to room temperature, dissolved in 50 g of chloroform, and washed six times with 100 ml of water. The solvent in the organic phase was distilled off under reduced pressure, yielding 36.2 g of photopolymerization initiator 2.

[0063] 2. Preparation of curable resin composition The components shown in the table were mixed in the amounts (parts by mass) shown in the table below, and then thoroughly kneaded using a three-roll mill (C-4 3 / 4 × 10, manufactured by Inoue Seisakusho Co., Ltd.) to prepare curable resin compositions for the examples and comparative examples.

[0064] 3. Evaluation The curable resin compositions of the Examples and Comparative Examples were evaluated by the following tests.

[0065] (1) Moisture permeability The resin composition was sandwiched between 100 mm x 100 mm, 0.1 mm thick PET (polyethylene terephthalate) films so that the diameter was 3.6 mm to 3.8 mm and the thickness was 0.28 mm to 0.32 mm, and the 100 mW / cm 2 UV irradiation intensity of 1500mJ / cm on both sides 2 The sample was irradiated with light energy at 1000 W / cm² and then thermally cured in a hot air oven at 120°C for 1 hour to prepare a sample for moisture permeability measurement. The moisture permeability was measured in accordance with JIS K0208:1976 using a constant temperature and humidity chamber at 65°C / 95% and calculated from the weight change using the moisture permeability cup method. From the viewpoint of suppressing deterioration of moisture permeability, the smaller the moisture permeability value, the better.

[0066] (2) Storage modulus The mixture was poured into a mold 5 cm long, 5 mm wide, and 0.5 mm thick, and then irradiated with ultraviolet light (UV irradiation device: UVX-01224S1, manufactured by Ushio Inc., 100 mW / cm 2 / 365nm for 30 seconds) with an integrated light intensity of 3000mJ / cm2 The composition was then cured by irradiation with light at 1000 W at 1000 W at 1000 W at 12 ...

[0067] The obtained cured test pieces were measured using a dynamic viscoelasticity measuring device (DMA, Seiko Instruments Inc., DMS6100) in a tensile deformation mode at a frequency of 1.0 Hz while increasing the temperature at a rate of 2°C / min in the range of 25°C to 200°C. From the obtained results, the storage modulus value at each temperature was extracted.

[0068] (3) NI point change Each sealant of the examples and comparative examples was poured into a mold with a diameter of 5 mm and a thickness of 0.5 mm, and ultraviolet rays were irradiated at an integrated light intensity of 3,000 mJ / cm. 2 The sealant was cured by irradiating with UV light to obtain a photocured product. Approximately 0.1 g of the photocured product was placed in an ampoule, and liquid crystal (MLC-6609, manufactured by Merck) was added in an amount 10 times the amount of the photocured product. The ampoule was placed in a 120°C oven for 1 hour, and then left to cool at room temperature until the temperature returned to room temperature (25°C). The liquid crystal portion was removed and filtered through a 0.2 μm filter to obtain a liquid crystal sample for evaluation.

[0069] The NI point was measured using a differential scanning calorimeter (DSC, PerkinElmer, PYRIS6) by sealing 10 mg of the liquid crystal sample for evaluation in an aluminum sample pan and heating at a rate of 5°C / min. Note that the blank was obtained by sealing 10 mg of the liquid crystal in an aluminum sample pan and measuring at a rate of 5°C / min.

[0070] The difference between the endothermic peak top (phase transition temperature) TB of the blank and the endothermic peak top (phase transition temperature) TE of the liquid crystal for evaluation; TE-TB, was defined as the NI point change.

[0071] The NI point (Nematic-Isotropic point), which is the phase transition temperature of liquid crystal, is determined by the mixture composition of each component of the liquid crystal, and is a unique value for each blend. It is generally known that the NI point changes when some impurity (other component) is mixed into these liquid crystals. From the perspective of suppressing the elution of components contained in the sealant into the liquid crystal, ensuring stable alignment of the liquid crystal, and improving display characteristics, the smaller the absolute value of the NI point change, the better.

[0072] [Table 1]

[0073] The components in Table 1 are as follows: 1. Curable resin (component (A) and component (C)) (1) Component (A) Partially methacrylated resin 1 (see Production Example (2)) NC-514S (Cardright) (2)(C) component Partially methacrylated bisphenol A epoxy resin (see Production Example (1)) Partially methacrylated resin 2 (see Production Example (3)) Partially methacrylated resin 3 (see Production Example (4)) EX-212 (hexanediol diglycidyl ether, manufactured by Nagase ChemteX Corporation) EX-830 (polyethylene glycol diglycidyl ether, manufactured by Nagase ChemteX Corporation) 2. Photopolymerization initiator (component (B)) Photopolymerization initiator 1 (see Production Example (5)) Photopolymerization initiator 2 (see Production Example (6)) 3. Heat curing agent (component (B)) EH-5030S (Polyamine compound, manufactured by ADEKA Corporation, active hydrogen equivalent: 105g / eq.)

Claims

1. (A) an epoxy resin represented by the following formula (1) and / or an epoxy (meth)acrylate resin in which a part or all of the epoxy groups of the epoxy resin have been modified with (meth)acrylic acid and / or (meth)acrylic anhydride; (B) a photopolymerization initiator and / or a heat curing agent; A liquid crystal sealant comprising: 【Chemistry 5】 [During the ceremony, R 1 is an aliphatic hydrocarbon group having 4 to 12 carbon atoms and containing 0 to 3 unsaturated bonds, R 2 is an aliphatic hydrocarbon group having 4 to 12 carbon atoms and containing 0 to 3 unsaturated bonds.

2. The liquid crystal sealant according to claim 1 , wherein the epoxy resin represented by the formula (1) includes an epoxy resin represented by the following formula (2): 【Chemistry 6】

3. The liquid crystal sealant according to claim 1 or 2 further comprises one or more additional curable resins selected from the group consisting of (C-1) a difunctional or higher epoxy resin (excluding the epoxy resin represented by formula (1)), (C-2) an epoxy (meth)acrylate resin in which part or all of the epoxy groups of the component (C-1) are modified with (meth)acrylic acid and / or (meth)acrylic anhydride), and (C-3) other curable resins (excluding the component (A), the component (C-1), and the component (C-2)).

Citation Information

Patent Citations

  • Resin composition, covering film and flexible printed circuit

    CN107663369A

  • Mold compositions with high adhesion to metal substrates

    US20070299154A1

  • Preparation and Characterization of Cardanol Based Vinyl Ester Resins as Cross-linker Units

    US20200361842A1

  • Sealing agent for liquid crystal display elements, vertically conducting material and liquid crystal display element

    WO2018116928A1