Polysilazane composition and cured film thereof
A polysilazane composition with fluoropolyether and metal salt cures at room temperature, providing effective water and oil repellency and durability, overcoming the limitations of existing coatings in repelling oil-based stains and gas barrier properties for outdoor structures.
Patent Information
- Application Number
- JP2021145867
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-09-08
- Publication Date
- 2024-10-10
- Estimated Expiration
- 2041-09-08
AI Technical Summary
Existing antifouling coatings for outdoor structures, such as building exteriors and automobile bodies, face challenges in effectively repelling oil-based stains and require high-temperature processes that are not suitable for post-construction applications, while also needing to provide gas barrier properties to protect against corrosion.
A polysilazane composition containing polysilazane, fluoropolyether, and a specific metal salt, which cures at room temperature, offering excellent water and oil repellency, dirt wiping properties, and durability through phase separation and improved compatibility of components.
The composition forms a cured film with superior water and oil repellency, dirt wiping properties, and durability, suitable for outdoor use without high-temperature processing, addressing the limitations of existing coatings.
Abstract
Description
[Technical field]
[0001] The present invention relates to a polysilazane composition and a cured film thereof. [Background technology]
[0002] Building exterior walls, glass windows, car bodies, and other items that are primarily intended for outdoor use are exposed to many substances that cause dirt, such as dust and organic matter in the air. Although there are no particular problems with the performance of these structures even if they become dirty, it can lead to a decline in their design, cleanliness, and image, so anti-fouling coatings are generally applied as a countermeasure. In particular, anti-fouling coatings are essential for many public structures, such as public toilets, utility poles, roads, and bridges, as they are visible to many people for decades.
[0003] Anti-fouling coatings can be broadly divided into hydrophilic and water-repellent types, with different mechanisms of anti-fouling and different types of dirt they can prevent. Hydrophilic coatings are often used on public buildings in Japan because dirt such as sand and mud is naturally washed away by rain outdoors. However, most hydrophilic coatings have the problem of showing little anti-fouling effect against oil-based inks such as paints and color sprays. For this reason, there has been a growing demand recently, especially in urban areas, for water- and oil-repellent coatings that have a better anti-fouling effect against graffiti and other stains than hydrophilic coatings.
[0004] Materials containing fluorine atoms (fluorine-based materials) are sometimes used as water- and oil-repellent coatings. The reason for this is that the surface tension of the materials containing fluorine atoms is smaller than that of water and oil, and the materials exhibit water- and oil-repellent properties. This makes it possible to remove both water- and oil-based inks relatively easily. As an anti-soiling coating using a fluorine-based material, a method has been proposed in which a film is formed using an acrylic oligomer containing fluorine atoms using a high-frequency plasma CVD device (Patent Document 1). This method can form a coating film on the surface of a substrate that is strong and has high anti-soiling performance, but since most outdoor structures are treated with anti-soiling coatings after construction, processes that require chambers such as CVD and deposition cannot be adopted. In addition, a low-temperature curing fluoropolymer has been proposed in which a curable silane compound is modified with a fluoropolyether group (Patent Document 2).
[0005] On the other hand, in order to protect the object of application from long-term corrosion deterioration, it is necessary not only to prevent the above-mentioned contamination by solids and liquids, but also to prevent contact with water vapor and corrosive gases. It is known that the cured film obtained from polysilazane exhibits excellent gas barrier properties, heat resistance, and insulating properties, and as an example of utilizing the gas barrier properties, it has been reported that the water vapor permeability of a resin sheet intended for sealing an organic EL element can be reduced by applying polysilazane to the surface of the resin sheet to form a siliceous glass film (Patent Document 3). [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2015-003510 A [Patent Document 2] JP 2017-082194 A [Patent Document 3] International Publication No. 2018 / 174116 Summary of the Invention [Problem to be solved by the invention]
[0007] For these reasons, it is believed that a coating agent composed of polysilazane and fluoropolymer as independent components can achieve both anti-fouling and gas barrier properties by phase separation into the polysilazane layer and the fluoropolymer layer after application. There is a demand for the development of technology that contains polysilazane and fluoropolymer as independent components, has excellent compatibility, and achieves excellent anti-fouling properties by curing at room temperature of around 25°C.
[0008] The present invention has been made to solve the above problems, and an object of the present invention is to provide a polysilazane composition which has excellent compatibility between the components and which cures at room temperature of about 25° C. to give a cured film which exhibits excellent water and oil repellency, ease of wiping off dirt, and durability. [Means for solving the problem]
[0009] In order to solve the above problems, the present invention provides a polysilazane composition, comprising: (A) polysilazane, (B) an organic solvent, (C) a fluoropolyether having one or more alkoxysilyl groups in the molecule; (D) a metal salt represented by the following formula (d-1): [M a L 1 x L 2 y ] (d-1) (In the formula, M is an element selected from Groups 4 to 13 of the Periodic Table, L 1 are each independently a hydroxy group, an alkoxy group having 1 to 10 carbon atoms, or a carboxylate group having 1 to 10 carbon atoms; L 2 are each independently a group of a β-diketone or an anion or an enolate anion of a β-ketoester represented by the following formula (d-2). R d1 C(O)CHR d2 C(O)R d1 (d-2) (R in the formula d1 are each independently a hydrocarbon group having 1 to 10 carbon atoms or an alkoxy group having 1 to 10 carbon atoms, and R d2is a hydrogen atom or a methyl group.) a is the valence of M and is an integer satisfying 1≦a≦4. x is an integer satisfying 1≦x≦4, y is an integer satisfying 0≦y≦3, and x+y=a. The polysilazane composition comprises:
[0010] Such a composition is a polysilazane composition that has excellent compatibility between the components and that, when cured at room temperature of about 25° C., gives a cured film that exhibits excellent water and oil repellency, ease of wiping off dirt, and durability.
[0011] In the present invention, the component (A) is preferably perhydropolysilazane.
[0012] Such a polysilazane composition can improve the effects of the present invention.
[0013] In the present invention, M in the component (D) is preferably an element selected from Groups 4, 12, and 13 of the periodic table.
[0014] Such a component (D) can improve the immobilization efficiency of the component (C) and thereby provide better dirt wiping properties.
[0015] In the present invention, the blending amount of the component (D) is preferably 5 to 200 parts by mass per 100 parts by mass of the component (A).
[0016] Such a polysilazane composition can further improve the effects of the present invention.
[0017] In the present invention, the blending amount of the component (C) is preferably 0.1 to 1 part by mass per 100 parts by mass of the total of the components (A) and (B).
[0018] Such a polysilazane composition can further improve the effects of the present invention.
[0019] In the present invention, the polysilazane composition may further contain an amine compound (E).
[0020] Such a polysilazane composition can improve the curability.
[0021] The present invention also provides a cured film obtained by curing the polysilazane composition.
[0022] Such a cured film exhibits excellent water and oil repellency, ease of wiping off dirt, and durability, and is therefore useful as a cured film with excellent antifouling properties. Effect of the Invention
[0023] According to the present invention, a polysilazane composition containing a fluoropolyether having one or more alkoxysilyl groups in the molecule and a specific metal salt has excellent compatibility with each other, and can provide a cured film that exhibits excellent water and oil repellency, dirt wiping property, and durability by curing at room temperature of about 25°C. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0024] As described above, there has been a demand for the development of a polysilazane composition which has excellent compatibility between the components and which cures at room temperature of about 25°C to give a cured film which exhibits excellent water and oil repellency, ease of wiping off dirt, and durability.
[0025] Therefore, the present inventors have conducted extensive research into the above-mentioned problems and have found that a polysilazane composition containing an appropriate combination of a fluoropolyether and a metal salt has excellent solution compatibility and stability, and the cured film has excellent water and oil repellency and ease of wiping off dirt, thereby completing the present invention.
[0026] That is, the present invention is a polysilazane composition, (A) polysilazane, (B) an organic solvent, (C) a fluoropolyether having one or more alkoxysilyl groups in the molecule; (D) a metal salt represented by the following formula (d-1): [M a L 1 x L 2 y ] (d-1) (In the formula, M is an element selected from Groups 4 to 13 of the Periodic Table, L 1 are each independently a hydroxy group, an alkoxy group having 1 to 10 carbon atoms, or a carboxylate group having 1 to 10 carbon atoms; L 2 are each independently a group of a β-diketone or an anion or an enolate anion of a β-ketoester represented by the following formula (d-2). R d1 C(O)CHR d2 C(O)R d1 (d-2) (R in the formula d1 are each independently a hydrocarbon group having 1 to 10 carbon atoms or an alkoxy group having 1 to 10 carbon atoms, and R d2 is a hydrogen atom or a methyl group.) a is the valence of M and is an integer satisfying 1≦a≦4. x is an integer satisfying 1≦x≦4, y is an integer satisfying 0≦y≦3, and x+y=a. The polysilazane composition comprises:
[0027] The following describes the embodiments of the present invention, but these are presented as examples, and it goes without saying that the present invention is not limited to these and various modifications are possible.
[0028] <Polysilazane Composition> The present invention relates to a polysilazane composition comprising (A) polysilazane, (B) an organic solvent, (C) a fluoropolyether having one or more alkoxysilyl groups in the molecule, and (D) a metal salt, and may further comprise (E) an amine compound, etc. Each component will be described in detail below.
[0029] <(A) Polysilazane> The polysilazane (A) constituting the polysilazane composition of the present invention forms a glassy cured film by curing. The polysilazane is not particularly limited, but examples thereof include perhydropolysilazane, which is an inorganic polysilazane, or modified polysilazanes such as methylpolysilazane, dimethylpolysilazane, phenylpolysilazane, and vinylpolysilazane, which are organic polysilazanes; crosslinked polysilazanes chemically crosslinked with compounds such as hydrocarbon compounds having reactive groups such as hydroxyl groups, vinyl groups, amino groups, and silyl groups that chemically react with polysilazane to generate crosslinked structures, cyclic saturated hydrocarbon compounds, cyclic unsaturated hydrocarbon compounds, saturated heterocyclic compounds, unsaturated heterocyclic compounds, and silicone compounds. The polysilazane can be arbitrarily selected from one type alone, a mixture of polysilazanes selected from two or more types, or a polysilazane copolymer consisting of two or more types of polysilazane structures, and it is preferable that one molecule contains at least one hydrogen atom directly bonded to a silicon atom, and perhydropolysilazane is more preferable.
[0030] From the viewpoint of solubility in an organic solvent, which is the component (B) described below, and workability during application, the polysilazane preferably has a weight-average molecular weight in the range of 100 to 100,000,000, preferably 1,000 to 1,000,000, and more preferably 2,000 to 500,000. A weight-average molecular weight of 100 or more is preferable because it has low volatility and there is no risk of the film quality of the coating film deteriorating due to the volatilization of the organic solvent and the volatilization of the polysilazane itself during the curing process, while a weight-average molecular weight of 100,000,000 or less is preferable because it has high solubility in an organic solvent.
[0031] The weight average molecular weight referred to in this specification refers to a value obtained by gel permeation chromatography (GPC) measured under the following conditions using polystyrene as a standard substance. [Measurement conditions] Developing solvent: Tetrahydrofuran (THF) Flow rate: 0.35mL / min Detector: Differential refractive index detector Column: TSKguardcolumn SuperMP(HZ)-M TSKgel SuperMultipore HZ-M (4.6mmI.D.×15cm,4μm×4) (All manufactured by Tosoh Corporation) Column temperature: 40℃ Sample injection volume: 20 μL (THF solution with a concentration of 0.5% by mass)
[0032] <(B) Organic solvent> The polysilazane used in the present invention is diluted with an organic solvent in order to improve workability during application and storage stability. The organic solvent is not particularly limited as long as it dissolves the polysilazane (A), the fluoropolyether (C) having one or more alkoxysilyl groups in the molecule, and the metal salt (D).For example, saturated aliphatic hydrocarbons such as n-pentane, isopentane, n-hexane, isohexane, n-heptane, isoheptane, n-octane, isooctane, n-nonane, isononane, n-decane, and isodecane; unsaturated aliphatic hydrocarbons such as 1-octene, 1-nonene, 1-decene, 1-dodecene, and β-myrcene; saturated alicyclic hydrocarbons such as cyclopentane, cyclohexane, methylcyclohexane, dimethylcyclohexane, ethylcyclohexane, and decahydronaphthalene; and unsaturated alicyclic hydrocarbons such as cyclohexene. Saturated alicyclic hydrocarbons, terpene compounds such as p-menthane, d-limonene, l-limonene, and dipentene, aromatic hydrocarbons such as benzene, toluene, xylene, trifluoromethylbenzene, bis(trifluoromethyl)benzene, ethylbenzene, diethylbenzene, trimethylbenzene, triethylbenzene, and tetrahydronaphthalene, acetone, methyl ethyl ketone, diethyl ketone, methyl isobutyl ketone, di-n-butyl ketone, diisobutyl ketone, cyclopentanone, and cyclohexanone. , ketone compounds such as diacetone alcohol; ester compounds such as n-propyl acetate, isopropyl acetate, n-butyl acetate, isobutyl acetate, isoamyl acetate, ethyl acetoacetate, and ethyl caproate; alkyl ether compounds such as diethyl ether, di-n-propyl ether, di-n-butyl ether, di-n-pentyl ether, di-n-hexyl ether, and tert-butyl methyl ether; aryl ether compounds such as anisole and diphenyl ether; glycol ether compounds such as bis(2-methoxyethyl)ether, bis(2-ethoxyethyl)ether, and bis(2-butoxyethyl)ether; and fluorous solvents such as tetradecafluorohexane, hexadecafluoropentane, octadecafluorooctane, eicosafluorononane, octafluorocyclopentene, tetradecafluoromethylcyclohexane, octadecafluorodecahydronaphthalene, hexafluorobenzene, octafluorotoluene, and hexafluoroisopropyl methyl ether.
[0033] From the viewpoints of workability during application and storage stability of polysilazane, the dilution ratio is preferably within the range of 100 to 100,000 parts by mass, and more preferably 400 to 10,000 parts by mass, of the organic solvent (B) per 100 parts by mass of the polysilazane (A).
[0034] The (B) organic solvents may be used alone or in combination of two or more kinds.
[0035] The water content in the polysilazane composition of the present invention is preferably 500 ppm or less, more preferably 300 ppm or less. If the water content is 500 ppm or less, polysilazane and the contained water do not react with each other, so there is no risk of heat generation, hydrogen gas or ammonia gas generation, and there is no risk of thickening or gelation. Therefore, it is preferable that the water content in the (B) organic solvent is controlled so that the water content in the polysilazane composition of the present invention is within the above range.
[0036] <(C) Alkoxysilyl Group-Containing Fluoropolyether> (C) fluoropolyether having one or more alkoxysilyl groups in the molecule (alkoxysilyl group-containing fluoropolyether) plays a role of imparting water and oil repellency and antifouling properties to the cured film obtained from the polysilazane composition of the present invention by adding it to the polysilazane composition of the present invention. Specifically, in the curing process of the polysilazane composition of the present invention, the alkoxysilyl group is condensed, and the alkoxysilyl group-containing fluoropolyether (C) is bonded to the polysilazane (A), thereby obtaining a cured film that exerts the effects of the present invention.
[0037] (C) The alkoxysilyl group-containing fluoropolyether may have a divalent linear fluoropolyether group represented by the following formula (c-1) in the molecule. -(CF2O) p (CF2CF2O) q (CF2CF2CF2O) r (CF2CF2CF2CF2O) s - (c-1)
[0038] The values of p, q, r, and s above are 19 It is a value obtained from the integral ratio of F NMR, p is an integer of 1 or more, preferably 1 to 80, more preferably 3 to 30, q is an integer of 1 or more, preferably 1 to 80, more preferably 3 to 30, r is an integer of 0 or more, preferably 0 to 20, more preferably 0 to 5, and s is an integer of 0 or more, preferably 0 to 20, more preferably 0 to 5, and each repeating unit may be bonded randomly.
[0039] The alkoxysilyl group in the above fluoropolyether can be represented by the following formula (c-2). -Si(OR c1 ) m R c2 n (c-2) In the formula, m is an integer satisfying 1≦m≦3, n is an integer satisfying 0≦n≦2, and m+n=3, and it is preferable that m is 3 and n is 0.
[0040] OR c1 represents an alkoxy group bonded directly to a silicon atom, and OR c1 The oxygen atom of the above is directly bonded to a silicon atom to form an alkoxysilyl group.
[0041] R c1 Examples of the alkyl group include hydrocarbon groups such as a methyl group, an ethyl group, a propyl group, a butyl group, a vinyl group, a cyclohexyl group, and a phenyl group; ether bond-containing hydrocarbon groups such as a methoxymethyl group, a benzyloxymethyl group, and a methoxyethoxymethyl group; and thioether bond-containing hydrocarbon groups such as a methylthiomethyl group. Of these, a methyl group is preferred.
[0042] R c2is a group other than an alkoxy group, and examples thereof include hydrocarbon groups such as a methyl group, an ethyl group, a propyl group, a butyl group, a vinyl group, a cyclohexyl group, and a phenyl group; ether bond-containing hydrocarbon groups such as a methoxymethyl group, a benzyloxymethyl group, and a methoxyethoxymethyl group; and thioether bond-containing hydrocarbon groups such as a methylthiomethyl group. Of these, a methyl group is preferred.
[0043] The divalent linear fluoropolyether group represented by (c-1) and the alkoxysilyl group represented by (c-2) are linked via a linking group. The linking group improves the solubility of the alkoxysilyl group-containing fluoropolyether (C) in the organic solvent (B), thereby enhancing the compatibility with the polysilazane composition of the present invention.
[0044] As long as the divalent linear fluoropolyether group represented by (c-1) above and the alkoxysilyl group represented by (c-2) above are covalently linked via a molecular chain consisting of a divalent or higher linking group, the structure of the molecular chain of the divalent or higher linking group is not particularly limited.
[0045] By using a trivalent or higher linking group to increase the number of alkoxysilyl groups contained, the effects of the present invention can be improved.
[0046] In order to avoid a decrease in the compatibility of the fluoropolyether with the polysilazane composition of the present invention due to the increase in molecular weight of the fluoropolyether resulting from intramolecular condensation of the alkoxysilyl group, the valence of the linking group is preferably 2 to 10, more preferably 2 to 5.
[0047] The above-mentioned linking group may be one which is mediated by one or more types of structures selected from an ether bond, an amide bond, an ester bond, and a siloxane bond.
[0048] The linking group links (c-1) and (c-2) via it, and may contain a branched or cyclic structure, and the number of atoms derived from the linking group is preferably 2 to 50, and more preferably 4 to 30. When the number of atoms is 50 or less, the amount of fluorine atoms per weight contained in the additive (C) component does not decrease, and therefore the antifouling performance does not decrease.
[0049] Examples of the linking group include -CF2CH2O(CH2)3-.
[0050] The (C) alkoxysilyl group-containing fluoropolyethers may be used alone or in combination of two or more kinds.
[0051] The blending amount of (C) alkoxysilyl group-containing fluoropolyether is preferably 0.1 to 1 part by mass, and more preferably 0.2 to 0.6 parts by mass, per 100 parts by mass of the total of (A) polysilazane and (B) organic solvent.
[0052] Examples of (C) alkoxysilyl group-containing fluoropolyethers include KY-1281 (manufactured by Shin-Etsu Chemical Co., Ltd.) (a solution of alkoxysilyl group-containing fluoropolyether dissolved in MEK with an active ingredient concentration of 20% by mass) and compounds of the following formula CB. [ka]
[0053] <(D) Metal salt> The (D) metal salt improves the fixation efficiency of the (C) component in the cured product obtained from the polysilazane composition of the present invention, thereby exerting an effect of exhibiting stain wiping property, which is evaluated as the wipeability of oil-based pens, etc.
[0054] The (D) metal salt is a metal salt represented by the following formula (d-1). [M a L 1 x L 2 y ] (d-1) (In the formula, M is an element selected from Groups 4 to 13 of the Periodic Table, L 1 are each independently a hydroxy group, an alkoxy group having 1 to 10 carbon atoms, or a carboxylate group having 1 to 10 carbon atoms; L 2 are each independently a group of a β-diketone or an anion or an enolate anion of a β-ketoester represented by the following formula (d-2). R d1 C(O)CHR d2 C(O)R d1 (d-2) (R in the formula d1 are each independently a hydrocarbon group having 1 to 10 carbon atoms or an alkoxy group having 1 to 10 carbon atoms, and R d2 is a hydrogen atom or a methyl group.) a is the valence of M and is an integer satisfying 1≦a≦4. x is an integer satisfying 1≦x≦4, y is an integer satisfying 0≦y≦3, and x+y=a.
[0055] Here, M is a metal element that is the center of the metal salt, and is not particularly limited as long as it is an element selected from Groups 4 to 13 of the periodic table, but is preferably an element selected from Groups 4, 12, and 13 of the periodic table. Specific examples include Ti, Zr, V, Nb, Cr, Mo, Mn, Tc, Fe, Ru, Co, Rh, Ir, Ni, Pd, Pt, Cu, Ag, Au, Zn, Cd, Al, Ga, and In, of which Ti, Zr, Zn, Al, Ga, and In are preferred, and of which Zn or Al is more preferred.
[0056] L 1 The role of this compound is to improve the compatibility of the component (D) with the polysilazane composition of the present invention.
[0057] L 1are monovalent anions and are, independently of each other, a hydroxy group, an alkoxy group having 1 to 10 carbon atoms, or a carboxylate group having 1 to 10 carbon atoms. Examples of such an anion include alkoxy groups such as a hydroxy group, a methoxy group, an ethoxy group, a propoxy group, a butoxy group, a pentoxy group, a hexoxy group, a heptoxy group, an octoxy group, a nonoxy group, and a decoxy group, and carboxylate groups such as a methanoate group, an ethanoate group, a propanoate group, a butanoate group, a pentanoate group, a hexanoate group, a heptanoate group, an octanoate group, a nonanoate group, a decanoate group, and a 2-ethylhexanoate group. Of these, a butoxy group or a 2-ethylhexanoate group is preferred.
[0058] L 2 In the polysilazane composition of the present invention, it plays a role in improving the storage stability of the component (D).
[0059] L 2 are monovalent anions, each independently a group of a β-diketone or β-ketoester anion or an enolate anion, as represented by the following formula (d-2). R d1 C(O)CHR d2 C(O)R d1 (d-2)
[0060] R in the formula d1 are each independently a hydrocarbon group having 1 to 10 carbon atoms or an alkoxy group having 1 to 10 carbon atoms, and examples thereof include hydrocarbon groups such as a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, a hexyl group, a heptyl group, an octyl group, a nonyl group, and a decyl group, and alkoxy groups such as a methoxy group, an ethoxy group, a propoxy group, a butoxy group, a pentoxy group, a hexoxy group, a heptoxy group, an octoxy group, a nonoxy group, and a decoxy group, and of these, an ethoxy group is preferred.
[0061] R in the formula d2 is a hydrogen atom or a methyl group, and is preferably a hydrogen atom.
[0062] a is the valence of M and is an integer satisfying 1≦a≦4. x is an integer satisfying 1≦x≦4, y is an integer satisfying 0≦y≦3, and x+y=a.
[0063] (D) Examples of metal salts include aluminum di-n-butoxy monoethylacetoacetate (Hope Pharmaceutical's Kerope EB-2), aluminum mono-n-butoxy diethylacetoacetate (Hope Pharmaceutical's Kerope ACS-2), zinc bis(2-ethylhexanoate) (Hope Pharmaceutical's 22% Octope Zn), titanium(IV) tetrabutoxide, monomer (Fujifilm Wako Pure Chemical Industries), and zirconium di-n-butoxy diethylacetoacetate (Hope Pharmaceutical).
[0064] (D) The metal salts may be used alone or in combination of two or more kinds.
[0065] The blending amount of the (D) metal salt is preferably from 5 to 200 parts by mass, and more preferably from 20 to 100 parts by mass, per 100 parts by mass of the (A) polysilazane.
[0066] <(E) Amine Compound> The polysilazane composition of the present invention may further contain an amine compound for the purpose of improving the curing reaction rate.
[0067] The structure of the amine compound is not particularly limited as long as it can serve as a catalyst for a curing reaction when left standing at room temperature or irradiated with UV light. Examples of suitable amine compounds include aliphatic amines such as methylamine, dimethylamine, trimethylamine, ethylamine, diethylamine, triethylamine, ethylenediamine, and tetramethylethylenediamine; alkoxysilyl-containing aliphatic amines such as 3-aminopropyltriethoxysilane and N-2-(aminoethyl)-3-aminopropyltrimethoxysilane; and aliphatic aminoalkoxyamines such as ethanolamine, N-methylethanolamine, and N,N-dimethylethanolamine. Examples of the amine compounds include aliphatic amino ethers such as 2-methoxyethylamine, bis(2-aminoethyl)ether, 1,4-butanediol bis(2-aminoethyl)ether, bis[2-(2-aminoethoxy)ethyl]ether, and triethylene glycol bis(2-aminoethyl)ether, aromatic amines such as aniline, phenylethylamine, and toluidine, and heterocyclic amines such as pyrrolidine, piperidine, piperazine, pyrrole, pyrazole, imidazole, pyridine, pyridazine, pyrimidine, pyrazine, diazabicyclononene, and diazabicycloundecene. The amine compounds may be used alone or in combination of two or more.
[0068] The amount of the amine compound is preferably from 1 to 20 parts by mass, and more preferably from 5 to 10 parts by mass, per 100 parts by mass of the polysilazane (A).
[0069] <Other additives> The polysilazane composition of the present invention may contain additives other than those mentioned above depending on the purpose. For example, inorganic fillers such as silica, alumina, and titania may be added as additives to improve the properties (coating strength, heat resistance) of the cured film. For example, ultraviolet absorbers such as benzophenone compounds and / or light stabilizers such as hindered amine compounds may be added as additives to improve weather resistance.
[0070] <Cured film> In the present invention, the polysilazane composition can be cured to form a cured film. Such a cured film exhibits excellent water and oil repellency, dirt wiping property, and durability, and is therefore useful as a cured film with excellent antifouling properties.
[0071] <Method of producing polysilazane composition> The polysilazane composition of the present invention may be produced by any method without limitation. For example, a polysilazane composition in which each component is suitably dissolved can be obtained by adding the components (C) and (D) and, optionally, the component (E) to a solution obtained by mixing the components (A) and (B), and then, for example, shaking and stirring the mixture.
[0072] <Method of forming a cured film> The method for forming a cured film using the polysilazane composition of the present invention is not particularly limited, and examples thereof include a method including a coating step of coating the polysilazane composition on a substrate, a solvent volatilization step of volatilizing and removing the organic solvent from the coating film coated on the substrate, and a curing step of curing the polysilazane composition components other than the organic solvent.
[0073] (Coating process) Examples of methods for applying the polysilazane composition of the present invention to a substrate include roll coating methods using a direct gravure coater, a chamber doctor coater, an offset gravure coater, a reverse kiss coater, a reverse roll coater, a slot die, a lip coater, an air doctor coater, a single roll kiss coater, a positive rotation roll coater, a blade coater, an impregnation coater, an MB coater, an MB reverse coater, a knife coater, a bar coater, etc., spin coating methods, dispensing methods, dipping methods, spraying methods, transfer methods, slit coating methods, etc.
[0074] The thickness of the coating film varies depending on the purpose of the cured film, but the cured film thickness is preferably 10 to 100,000 nm, and more preferably 100 to 10,000 nm.
[0075] Before applying the polysilazane composition, the substrate may be subjected to a surface modification treatment. The surface modification treatment is mainly performed for the purpose of improving the adhesion between the substrate and the polysilazane, and is realized by decomposing and removing organic matter attached to the substrate surface, or by forming chemical reaction points on the substrate surface. Examples of the surface modification treatment method include argon plasma treatment, oxygen plasma treatment, ozone treatment, UV irradiation treatment, and xenon excimer light irradiation treatment, and are used depending on the type of substrate.
[0076] (Solvent evaporation process) Following the coating step, the process proceeds to a solvent evaporation step in which the organic solvent is evaporated from the coating film formed on the substrate. The solvent evaporation step may be performed at a temperature at which the substrate does not deteriorate, and is preferably performed at, for example, 20 to 300°C. Within this range, the organic solvent evaporates quickly and the process can proceed to the curing step. If the temperature of the solvent evaporation step is 300°C or less, there is no risk of the evaporated solvent igniting, and this is preferable.
[0077] For the above reasons, the boiling point of the (B) organic solvent used in the present invention under atmospheric pressure (1013 hPa) is preferably 25 to 300° C., and more preferably 25 to 150° C. If it is within this range, the organic solvent will not remain in the cured film, and handling properties will be good.
[0078] (hardening process) After the solvent evaporation process, the process proceeds to hardening the fluoropolymer (component (C)) and metal salt (component (D))-containing polysilazane. There are no particular restrictions on the hardening process for the fluoropolymer and metal salt-containing polysilazane as long as the hardening reaction proceeds, but it is necessary to select an appropriate method that does not alter the base material. Examples of hardening methods include leaving the material at rest under constant temperature and humidity, atmospheric pressure plasma treatment, low-temperature plasma treatment, UV treatment, and excimer light treatment. EXAMPLES
[0079] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to the following examples. The weight average molecular weight refers to the value obtained by gel permeation chromatography (GPC) using polystyrene as a standard substance as described above.
[0080] (A) Polysilazane (Synthesis example) Synthesis of polysilazane (A) Dehydrated pyridine (4,500 g) was cooled to -10°C under a nitrogen atmosphere, and dichlorosilane (64 L) was blown in, followed by stirring at -10°C for 1 hour. Ammonia (216 L) was blown in, and the mixture was stirred for 12 hours while returning to 25°C. The resulting solid was filtered off, and di-n-dibutyl ether (1,000 g) was added to the filtrate. The pyridine in the liquid was distilled off under reduced pressure while azeotroping with di-n-butyl ether, and when the distillate reached 4,500 g, di-n-butyl ether (1,000 g) was further added. Subsequently, pyridine was distilled off under reduced pressure while azeotroping with di-n-butyl ether to obtain a di-n-butyl ether solution of perhydropolysilazane. The weight-average molecular weight of this perhydropolysilazane was 6,100. Thereafter, di-n-butyl ether was added so that the amount of polysilazane was 2.5 parts by mass when the entire solution was 100 parts by mass. In the following examples and comparative examples, this solution was used assuming that it contained 2.5 parts by mass of perhydropolysilazane as component (A) and 97.5 parts by mass of di-n-butyl ether as component (B-1). When 1,3-bis(trifluoromethyl)benzene was contained as component (B-2), it was used assuming that it contained 2.5 parts by mass of component (A), 47.5 parts by mass of component (B-1), and 50 parts by mass of component (B-2).
[0081] (B) Organic solvent (B-1): Di-n-butyl ether (Kanto Chemical) (B-2): 1,3-bis(trifluoromethyl)benzene (Tokyo Chemical Industry Co., Ltd.)
[0082] (C) Fluoropolyether having one or more alkoxysilyl groups in the molecule Treatment liquid (C-1): KY-1281 (manufactured by Shin-Etsu Chemical Co., Ltd.) (a solution containing alkoxysilyl-containing fluoropolyether dissolved in MEK with an active ingredient concentration of 20% by mass)
[0083] Treatment solution (C-2): A solution with an active ingredient concentration of 20% by mass, in which the CB synthesized below is dissolved in the component (B-2).
[0084] Synthesis of precursor (CA) Fomblin D2 (Solvay) (50 g), 30 wt% sodium hydroxide aqueous solution (6 g), and tetrabutylammonium hydrogen sulfate (0.4 g) were placed in a 100 mL three-neck flask. Allyl bromide (12 g) was added while stirring, and the mixture was heated at an internal temperature of 50°C for 24 hours. 2.4 M hydrochloric acid (12 g), 1,3-bis(trifluoromethyl)benzene (40 g), and pure water (40 g) were added, and after shaking, the organic layer and the aqueous layer were separated. The organic layer was washed four times with pure water (40 g). Activated carbon (Shirasagi P) (Osaka Gas Chemical) (0.4 g) and Kyoward 2200 (Kyowa Chemical Industry) (0.4 g) were added to the organic layer, and the mixture was stirred at room temperature for 1 hour. The mixture was filtered and the solvent was distilled off under reduced pressure to obtain the precursor (CA) as a colorless, transparent liquid with a yield of 85%.
[0085] Synthesis of the active ingredient (CB) of the treatment liquid (C-2) The CA (10 g), 1,3-bis(trifluoromethyl)benzene (20 g), and platinum catalyst (CAT-PL-50T, manufactured by Shin-Etsu Chemical Co., Ltd.) (0.015 g) were added to a 100 mL three-neck flask, and the mixture was heated to an internal temperature of 60°C, after which trimethoxysilane (03-MS, manufactured by Shin-Etsu Chemical Co., Ltd.) (1.5 g) was added dropwise. After heating and stirring at an internal temperature of 60°C for 5 hours, activated carbon (0.5 g) was added and the mixture was stirred for 1 hour while returning to room temperature. The mixture was filtered and the solvent was distilled off under reduced pressure to obtain the active ingredient (CB) as a colorless, transparent liquid with a yield of 97%. [ka]
[0086] Preparation of treatment solution (C-2) The CB synthesized above was dissolved in component (B-2) to prepare a solution with an active ingredient concentration of 20 mass %.
[0087] Comparative fluoropolyether Treatment liquid (C-3): A solution containing a polyether group-containing fluoropolyether having no alkoxysilyl group dissolved in component (B-2), with an active ingredient concentration of 20% by mass.
[0088] Preparation of treatment solution (C-3) Fluorolink PEG45 (manufactured by Solvay) (a polyether group-containing fluoropolyether) was dissolved in component (B-2) to prepare a solution with an active ingredient concentration of 20% by mass.
[0089] (D) Metal salts (D-1): Aluminum di-n-butoxy monoethylacetoacetate (Hope Pharmaceuticals, Kerope EB-2) (D-2): Aluminum mono-n-butoxy diethylacetoacetate (Hope Pharmaceuticals, Kerope ACS-2) (D-3): Zinc bis(2-ethylhexanoate) (Hope Pharmaceuticals, 22% Octope Zn) (D-4): Titanium(IV) tetrabutoxide, monomer (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) (D-5): Zirconium di-n-butoxy diethylacetoacetate (Hope Pharmaceuticals)
[0090] Comparative metal salts (D-6): Aluminum acetylacetonate (Kanto Chemical) (D-7): Zinc chloride (Kanto Chemical)
[0091] (E) Amine compounds 3-Aminopropyltriethoxysilane (KBE-903 manufactured by Shin-Etsu Chemical Co., Ltd.)
[0092] [Examples 1 to 12, Comparative Examples 1 to 6] (1) Compatibility evaluation The polysilazane compositions were prepared by adding the above-prepared components (C) and (D), and optionally the components (B-2) and (E) to a solution prepared by mixing the components (A) and (B-1) prepared in the above Synthesis Example in the ratios shown in Table 1 or Table 2, and shaking and stirring the container for 10 seconds. The appearance immediately after preparation was visually observed, and in Table 1 or Table 2, those that were transparent were marked with an ◯, and those in which the components were not compatible and insoluble matter was observed were marked with an ×.
[0093] (2) Evaluation of water contact angle and hexadecane contact angle (coating process) Of the polysilazane compositions prepared in the above evaluation (1), those that were evaluated as ◯ in (1) were spin-coated (rotation speed: 1000 rpm, rotation time: 10 seconds) onto a slide glass. (Solvent evaporation process and hardening process) The polysilazane composition thus applied was allowed to stand for 24 hours in an environment at a temperature of 24° C. and a relative humidity of 40%. The contact angles of water or hexadecane with the cured films prepared above were measured using a contact angle meter Dropmaster DMo-701 (manufactured by Kyowa Interface Science). The measured contact angle values are shown in Table 1 or Table 2.
[0094] (3) Evaluation of oil-based pen wiping properties A curved line 5 cm long was drawn on the cured film prepared in the evaluation of (2) above using an oil-based pen (Pentel Pen N50, manufactured by Pentel). The drawn curve was wiped off with Kay Dry (manufactured by Nippon Paper Crecia). Those that could be wiped off completely within 3 wipes were given a ◯, and those that required 4 wipes or more or could not be wiped off were given a ×, as shown in Tables 1 and 2.
[0095] (4) Evaluation of wear resistance The surface of the cured film prepared in the evaluation of (2) above was abraded using Tribogear (manufactured by Shinto Scientific Co., Ltd.) under the following conditions. Thereafter, the water contact angle was measured in the same manner as in the evaluation of (2) above. Those with a water contact angle of 90° or more were marked with an ◯, and those with a water contact angle of less than 90° were marked with an ×, as shown in Tables 1 and 2. [Wear conditions] Friction material: Bencot Super CN (made by Asahi Kasei) Contact area: 3.0cm x 2.8cm Load: 500g Rubbing distance (one way): 30mm Scraping speed: 3,600 mm / min Number of trips: 100
[0096] [Table 1] In the table, the unit of each component is parts by mass.
[0097] [Table 2] In the table, the unit of each component is parts by mass.
[0098] In all evaluation items, Examples 1 to 12 had evaluation results equal to or higher than those of the comparative examples. In Comparative Examples 3 and 4, the metal salt (D) was used, which had a structure outside the scope of the present invention, and therefore the metal salt did not dissolve. The fluoropolyether used in Comparative Example 6 did not contain an alkoxysilyl group, and therefore did not exhibit oil-based pen wiping properties and abrasion resistance. From the results of Comparative Examples 1, 2, 5, and 6, when at least one of the components (C) and (D) in the polysilazane composition of the present invention was missing, the oil-based pen wiping properties and abrasion resistance were not exhibited.
[0099] [Industrial Applicability] The polysilazane composition of the present invention is useful as an antifouling coating composition, and can form a cured film having excellent composition stability and excellent water / oil repellency and antifouling properties at room temperature. Therefore, it is useful for forming the above-mentioned cured film on a substrate having low heat resistance or in an outdoor coating environment where heating is difficult.
[0100] The present invention is not limited to the above-described embodiment. The above-described embodiment is merely an example, and anything that has substantially the same configuration as the technical idea described in the claims of the present invention and exhibits similar effects is included in the technical scope of the present invention.
Claims
1. 1. A polysilazane composition comprising: (A) polysilazane, (B) an organic solvent, (C) a fluoropolyether having one or more alkoxysilyl groups in the molecule; (D) a metal salt represented by the following formula (d-1): [M a L 1 x L 2 y ] (d-1) (In the formula, M is an element selected from Groups 4 to 13 of the Periodic Table, L 1 are each independently a hydroxy group, an alkoxy group having 1 to 10 carbon atoms, or a carboxylate group having 1 to 10 carbon atoms; L 2 are each independently a group of a β-diketone or an anion or an enolate anion of a β-ketoester represented by the following formula (d-2). R d1 C(O)CHR d2 C(O)R d1 (d-2) (In the formula R d1 are each independently a hydrocarbon group having 1 to 10 carbon atoms or an alkoxy group having 1 to 10 carbon atoms; R d2 is a hydrogen atom or a methyl group.) a is the valence of M and is an integer satisfying 1≦a≦4. x is an integer satisfying 1≦x≦4, y is an integer satisfying 0≦y≦3, and x+y=a. A polysilazane composition comprising:
2. 2. The polysilazane composition according to claim 1, wherein the component (A) is a perhydropolysilazane.
3. 3. The polysilazane composition according to claim 1, wherein M in component (D) is an element selected from Groups 4, 12, and 13 of the Periodic Table.
4. 4. The polysilazane composition according to claim 1, wherein the blending amount of the component (D) is 5 to 200 parts by mass per 100 parts by mass of the component (A).
5. The polysilazane composition according to any one of claims 1 to 4, wherein the blending amount of the component (C) is 0.1 to 1 part by mass per 100 parts by mass of the total of the components (A) and (B).
6. The polysilazane composition according to any one of claims 1 to 5, further comprising (E) an amine compound.
7. A cured film obtained by curing the polysilazane composition according to any one of claims 1 to 6.
Citation Information
Patent Citations
Coating composition and coating method
JP1989221466A
Method for producing modified silica film, coating liquid, and modified silica film
JP2014213317A
Laminate
JP2015003510A
Perfluoro(POLY)ether group-containing silane compound
JP2017082194A
Sheet for sealing
WO2018174116A1
Cited By
Coating film, electronic device, moving body, and coating liquid
JP2026086331A