Mud treatment agent and mud treatment method
A one-pack mud treatment agent with guar gum and magnesium oxide solidifying agent simplifies the treatment of excavation mud by promoting rapid solidification and heavy metal adsorption, addressing the complexity of conventional methods and reducing construction costs.
Patent Information
- Application Number
- JP2020169860
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-10-07
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2040-10-07
AI Technical Summary
Conventional mud treatment methods for excavation mud generated during shield construction are complicated and require multiple steps, leading to increased equipment size and complexity.
A one-pack mud treatment agent comprising powdered guar gum and magnesium oxide solidifying agent with specific particle sizes, along with iron sulfate, is used to simplify the treatment process by promoting rapid water absorption, granulation, and heavy metal adsorption, allowing for single-step solidification of excavation mud.
The one-pack mud treatment agent effectively solidifies excavation mud to a transportable hardness within one hour, reduces heavy metal elution, and simplifies the treatment process, thereby reducing construction costs and equipment size.
Smart Images

Figure 0007565555000001 
Figure 0007565555000002 
Figure 0007565555000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a mud treatment agent and a mud treatment method. [Background technology]
[0002] At work sites where shield tunneling methods (such as air bubble shield tunneling and earth pressure shield tunneling) are used, mud containing a lot of moisture (excavation mud) is generated. This type of mud is treated to give it a certain degree of hardness, as it would be difficult to transport or reclaim if left in its original state.
[0003] Conventionally, for example, natural polymers such as guar gum were added to and mixed with mud generated by the air bubble shield method to granulate the mud, and then an inorganic solidifying agent such as gypsum was added and mixed (see Patent Document 1). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2006-265885 A Summary of the Invention [Problem to be solved by the invention]
[0005] As described above, the conventional mud treatment method is divided into two steps: a step of granulating the mud by adding natural polymers, and a step of solidifying the mud by adding inorganic solidifying agents. In other words, the additives used in mud treatment (natural polymers, inorganic solidifying agents) were used separately as two agents. Thus, conventional mud treatment was complicated, and there was also the problem of the treatment equipment becoming larger.
[0006] An object of the present invention is to provide a one-pack type mud treatment agent and a mud treatment method using the same. [Means for solving the problem]
[0007] In order to solve the above problems, the mud treatment agent according to the present invention comprises: Guar gum Powdered natural polymer and powdered magnesium oxide based solidification Agent and wherein 90% by mass or more of the natural polymer passes through a 200 mesh sieve, and the magnesium oxide-based solidification Agent 90% by mass or more of the magnesium oxide solidification agent passes through a 100 mesh sieve. Agent At least 90% by mass of the composition does not pass through a 200 mesh sieve.
[0008] According to this mud treatment agent, since a highly biodegradable natural polymer is used, the environmental friendliness of the mud treatment agent can be improved. Furthermore, according to this mud treatment agent, since the particle size of the natural polymer is smaller than that of the magnesium oxide-based solidifying agent, the natural polymer can be reacted preferentially with the object to be treated rather than the magnesium oxide-based solidifying agent, and as a result, the water absorption and granulation of the object to be treated by the natural polymer can be promoted. Since the object to be treated is absorbed and granulated, the solidification ability of the magnesium oxide-based solidifying agent can be easily exerted, so that the object to be treated can be solidified even with a one-agent type. Furthermore, since the magnesium oxide-based solidifying agent adsorbs heavy metals such as arsenic, it can also suppress the elution of heavy metals from the object to be treated.
[0009] Furthermore, the mud treatment agent according to the present invention preferably contains iron sulfate, and the mass ratio of the magnesium oxide-based solidifying agent, the iron sulfate, and the natural polymer is preferably 86.5-90.5:4.5-8.5:4.5-7.0.
[0010] According to this mud treatment agent, the iron sulfate adsorbs heavy metals, so that the elution of heavy metals from the object to be treated can be further suppressed. In addition, the mud treatment agent, which becomes alkaline due to the magnesium oxide-based solidifying agent, can be neutralized by the iron sulfate.
[0011] The natural polymer but Guar gum ForFor example, the thickening and flocculation effects can be achieved even when treating materials derived from natural ground that contain sodium chloride, metal ions, cement, etc. In addition, guar gum quickly exerts its thickening and flocculation effects, making it possible to shorten the solidification time of the materials to be treated.
[0012] The magnesium oxide-based solidifying agent is preferably light-burned dolomite or light-burned magnesium. By using light-burned dolomite or light-burned magnesium, the strength of the solidified treatment object can be increased.
[0013] The mud treatment method according to the present invention includes a step of adding any one of the mud treatment agents to excavated mud generated by a shield tunneling method to solidify the excavated mud. According to the mud treatment method, the excavated mud can be solidified in one step. Effect of the Invention
[0014] According to the present invention, it is possible to provide a one-form mud treatment agent and a mud treatment method using the same. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] Hereinafter, the embodiments of the present invention will be described in detail. The following description of the constituent elements may be based on representative embodiments or specific examples, but the present invention is not limited to such embodiments. In this specification, a numerical range expressed using "~" means a range including the numerical values before and after "~" as the lower and upper limits. Furthermore, "parts" and "%" respectively indicate "parts by mass" and "% by mass" unless otherwise specified.
[0016] (Mud treatment agent) The mud treatment agent of the present embodiment contains at least a powdered natural polymer having a flocculating and thickening action, and a powdered magnesium oxide-based solidifying agent. In the mud treatment agent, the natural polymer and the magnesium oxide-based solidifying agent are premixed. In other words, the mud treatment agent of the present embodiment is a one-agent type.
[0017] When mud treatment agents are added to materials to be treated, such as excavation mud containing moisture, the fluidity of the material to be treated decreases and the material to be treated solidifies to a certain degree of hardness. For example, adding a mud treatment agent to excavation mud generated during shield construction can adjust the hardness (initial strength) of the excavation mud to a level that allows it to be transported and removed.
[0018] The hardness (initial strength) of the object treated with the mud treatment agent will vary depending on the type and condition of the object, but will be at least 150 kN / m on the cone index one hour after the addition of the mud treatment agent. 2 Above 180kN / m 2 It is preferable that the resistance is 200 kN / m or more. 2 More preferably, it is equal to or greater than this.
[0019] The amount of the mud treatment agent to be added is not particularly limited as long as it does not impair the object of the present invention. For example, the amount of the mud treatment agent to be added is 20 to 300 kg / m of the material to be treated such as mud. 3 is added in a ratio of
[0020] (natural polymer) The natural polymer mainly functions as a flocculant (thickener) that flocculates and thickens the material to be treated, such as mud containing moisture. The natural polymer absorbs moisture from the material to be treated and granulates the material to be treated. Examples of natural polymers suitable for absorbing moisture and granulating the material to be treated include natural polysaccharides, and among these, guar gum is preferable.
[0021] Guar gum is a nonionic natural polysaccharide whose main component is galactomannose. Guar gum can stably exert a flocculating effect and granulate the object to be treated, even if the object is excavated soil containing seawater (salt), metal ions, cement, etc. In addition, guar gum can quickly exert a flocculating effect and shorten the solidification time.
[0022] The natural polymer is in a powder form, and 90% by mass or more has a particle size that passes through a 200 mesh (75 μm opening) sieve.
[0023] (Magnesium oxide solidifier) Magnesium oxide solidifying agents solidify materials to be treated, such as mud, to a hardness suitable for transportation and landfill. Magnesium oxide solidifying agents adsorb heavy metals, such as arsenic, in materials to be treated, and can also suppress the elution of heavy metals. Lightly burned dolomite (CaMg(CO3)2) or lightly burned magnesium (MgO) is preferred as a magnesium oxide solidifying agent. Magnesium oxide solidifying agents are in powder form, with a particle size such that 90% by mass or more passes through a 100 mesh (149 μm opening) sieve and 90% by mass or more does not pass through a 200 mesh (75 μm opening) sieve. In other words, magnesium oxide solidifying agents Agent Of the powder, 90% by mass or more will remain on the top of a 200 mesh sieve, and only less than 10% by mass will pass through the 200 mesh sieve.
[0024] (Effect of particle size difference) In this way, by adjusting the particle size of the natural polymer to be smaller than the particle size of the magnesium oxide-based solidifying agent, even if the magnesium oxide-based solidifying agent and the natural polymer are added in a premixed state to the material to be treated, the natural polymer will react preferentially with the material to be treated over the magnesium oxide-based solidifying agent.
[0025] In order to verify the effect due to the difference in particle size, the present inventors carried out the following experiment regarding the order of adding reagents. In this experiment, a simulated soil for verifying particle size, which was a mixture of the following, was used as the treatment object. <Simulated soil> Sandy soil: 1050g Earthenware (crushed to less than 2mm): 600g Water: 350g
[0026] In this experiment, the following reagents were used as mud treatment agents. Hereinafter, for example, the description "200 mesh" means that 90% or more by mass of the target has a particle size that passes through a 200 mesh (75 μm opening) sieve. The same applies to "100 mesh" and "60 mesh." <Mud treatment agent> Natural polymer, small particle size (Guar gum, 200 mesh): 0.6g Ferrous sulfate (ferrous sulfate tetrahydrate): 3.4g Magnesium oxide solidifier, large particle size (lightly burnt magnesium, 60 mesh): 26g
[0027] The formulations of the simulated soil and mud treatment agents are shown in Table 1.
[0028] [Table 1]
[0029] In this experiment, the following two samples were created. Sample 1: A sample in which the reagents were added to the simulated soil in the following order: natural polymer, iron sulfate, and magnesium oxide solidifying agent. Sample 2: A sample in which magnesium oxide-based solidifying agent, ferrous sulfate, and natural polymer were added to the simulated soil in that order and mixed.
[0030] The cone index was measured for Sample 1 and Sample 2 1 hour and 24 hours after the final addition of the reagent. The cone index was measured in accordance with JIS A 1228 "Test method for cone index of compacted soil." The results are shown in Table 2.
[0031] [Table 2]
[0032] Generally, if a sample in which a natural polymer is added first is compared with a sample in which a magnesium oxide-based solidifying agent is added first, the Cone Index of the former should be higher. This is because adding the natural polymer first allows the natural polymer to absorb the moisture of the material to be treated, improving the granulation effect of the material to be treated.
[0033] However, as shown in Table 2, there is no significant difference in the Cone Index between Sample 1, in which the natural polymer was added first, and Sample 2, in which the magnesium oxide-based solidifying agent was added first. This is thought to be because the particle size of the natural polymer was sufficiently smaller than that of the magnesium oxide-based solidifying agent, improving the reactivity of the natural polymer and allowing the granulation effect to be achieved even when the natural polymer was added later.
[0034] As can be seen from this experiment, by making the particle size of the natural polymer much smaller than that of the magnesium oxide-based solidifying agent, the water absorption and granulation effects are exerted and the simulated soil is solidified even when the natural polymer is added later. Therefore, even with a one-agent type mud treatment agent in which such a natural polymer and magnesium oxide-based solidifying agent are premixed, it is believed that the water absorption and granulation effects of the natural polymer and the solidification action of the magnesium oxide-based solidifying agent can rapidly solidify the object to be treated.
[0035] (Ferrous Sulfate) The mud treatment agent preferably contains powdered iron sulfate so as to suppress the elution of heavy metals such as arsenic contained in the object to be treated. In other words, iron sulfate is preferably premixed into the mud treatment agent. By blending iron sulfate into the mud treatment agent, heavy metals such as arsenic in the object to be treated are adsorbed by the iron sulfate and insolubilized, so that the elution of heavy metals from the object to be treated can be suppressed. The arsenic elution test result of the object to be treated is preferably 0.01 mg / L or less due to insolubilization. In addition, iron sulfate also contributes to neutralizing the mud treatment agent, which is alkaline due to the magnesium oxide-based solidifying agent.
[0036] There are two types of ferrous sulfate: ferrous sulfate (I) and ferric sulfate (II). Ferrous sulfate is easy to obtain and safe enough to be used as a food additive, so it is suitable for use in mud treatment agents. There are various hydrates of ferrous sulfate with different numbers of water of hydration, and the more water of hydration there is, the higher the water solubility. The ferrous sulfate used in mud treatment agents is not limited by the water of hydration, but ferrous sulfate monohydrate, for example, is preferred because of its ease of availability.
[0037] The pH of the object to be treated to which the mud treatment agent has been added is preferably 7 to 11. Therefore, the present inventors created samples of mud treatment agents with different blends of ferrous sulfate in order to study the blending of ferrous sulfate that lowers the pH of the mud treatment agent that has become alkaline due to the magnesium oxide-based solidifying agent.
[0038] The ferrous sulfate used in the mud treatment agent was ferrous sulfate monohydrate. The following light-burned magnesium oxide solidification agents (1) to (4) were used. (1) Light-burned magnesium A (200 mesh) (2) Light-burned magnesium B (100 mesh) (3) Light-burned magnesium C (200 mesh) (4) Light-burned magnesium D (60 mesh)
[0039] The following mud treatment agent samples were prepared using the iron sulfate and magnesium oxide solidifying agents described above. Sample 1: Light-burned magnesium A Sample 2: Light-burned magnesium B Sample 3: Light-burned magnesium C Sample 4: Light-burned magnesium D Sample 5: Light-burned magnesium B and ferrous sulfate mixed in a mass ratio of 100:5.26 Sample 6: Light-burned magnesium B and ferrous sulfate mixed in a mass ratio of 100:6.38 Sample 7: Light-burned magnesium B and ferrous sulfate mixed in a mass ratio of 100:7.53 Sample 8: Light-burned magnesium B and ferrous sulfate mixed in a mass ratio of 100:8.70
[0040] In Table 3, 30 g of each mud treatment agent sample was added to 2000 g of simulated soil and mixed, and the pH of the simulated soil was measured according to JIS K0102 12.1 "Glass electrode method." The composition of the simulated soil was the same as that in Table 1.
[0041] [Table 3]
[0042] As shown in Table 3, differences in particle size of magnesium oxide-based solidifying agent did not have a significant effect on pH. Also, while the pH of the sample containing only magnesium oxide-based solidifying agent exceeded 11, the pH of the sample containing 5.26 or more iron sulfate per 100 magnesium oxide-based solidifying agent by mass ratio was 11 or less.
[0043] (Mass ratio of magnesium oxide solidifier to iron sulfide) The mass ratio of the magnesium oxide-based solidifying agent to iron sulfide in the mud treatment agent is preferably 5.20 to 10.00 iron sulfide per 100 parts of magnesium oxide-based solidifying agent. When the mass ratio of the magnesium oxide-based solidifying agent to iron sulfide is within this range, the pH of the material to be treated can be adjusted to 7 to 11, and iron sulfide can be prevented from interfering with the solidifying action of the magnesium oxide-based solidifying agent.
[0044] (Mud treatment agent blend ratio) The mass ratio of the magnesium oxide-based solidifying agent, iron sulfate, and natural polymer in the mud treatment agent is preferably 86.5-90.5:4.5-8.5:4.5-7.0. When the blending ratio in the mud treatment agent is within the above range, the material to be treated can be quickly solidified by the water absorption and granulation action of the natural polymer and the solidification action of the magnesium oxide-based solidifying agent, the iron sulfate is prevented from interfering with the solidification action of the magnesium oxide-based solidifying agent, and the pH of the material to be treated to which the mud treatment agent has been added can be adjusted to 7-11.
[0045] The object to be treated with the mud treatment agent of this embodiment is not limited to excavated mud generated by the shield construction method, but may be waste soil generated at other construction sites, etc.
[0046] (Mud treatment method using mud treatment agent) The mud treatment method of the present embodiment includes a step (kneading step) of adding the mud treatment agent to excavated mud (treatment object) generated by a shield method such as an air bubble shield method, and mixing and stirring the excavated mud (treatment object) to which the mud treatment agent has been added using a backhoe, etc. By this treatment step, the excavated mud, which is the treatment object, is solidified to a predetermined hardness or higher, and if the treatment object contains arsenic, the arsenic in the treatment object is insolubilized by this treatment step.
[0047] After the mud treatment agent of this embodiment is added to the object to be treated such as soil and sand, the process of kneading the object to be treated (kneading process) can be simplified to one time. In other words, the object to be treated can be treated in one process. The object to be treated such as soil and sand to which the mud treatment agent of this embodiment is added develops strength (hardness) to a degree that allows it to be carried out in a short time (for example, about 1 hour). Therefore, the time from when the object to be treated is treated with the mud treatment agent to when it is carried out can be significantly shortened compared to the conventional technology (two-component type mud treatment agent), and the space for temporarily storing the object to be treated with the mud treatment agent (treated object) until it is carried out can be reduced. Therefore, by using the mud treatment agent of this embodiment, the construction costs can be kept low overall. EXAMPLES
[0048] The present invention will be described in more detail below with reference to examples, although the present invention is not limited to these examples in any way.
[0049] (Preparation of imitation soil) The following model soils 1 and 2 with different arsenic contents were prepared. The arsenic elution test result for model soil 1 was 0.051 mg / L, and the arsenic elution test result for model soil 2 was 0.039 mg / L. The method for the arsenic elution test will be described later.
[0050] <Simulated soil 1> Sandy soil: 1050g Earthenware (crushed to less than 2mm): 600g Water: 350g Arsenic reagent (Fujifilm Wako Pure Chemical Industries, Ltd.: As1000): 3.3cc
[0051] <Simulated soil 2> Sandy soil: 1050g Earthenware (crushed to less than 2mm): 600g Water: 350g Arsenic reagent (Fujifilm Wako Pure Chemical Industries, Ltd.: As1000): 2.2cc
[0052] (Reagents used in mud treatment) The following reagents were used for the soil treatment: (1) Light-burned magnesium, small particle size (200 mesh) (2) Light-burned magnesium, large particle size (100 mesh) (3) Guar gum, small particle size (200 mesh) (4) Guar gum, large particle size (100 mesh) (5) Ferrous sulfate monohydrate
[0053] <Example 1> 27.0 g of light-burned magnesium (large particle size), 1.5 g of ferrous sulfate monohydrate, and 1.5 g of guar gum (small particle size) were mixed in advance to obtain 30 g of mud treatment agent. This mud treatment agent was added to 2000 g of simulated soil 1 and mixed to obtain the mud of Example 1.
[0054] <Example 2> The mud of Example 2 was prepared in the same manner as in Example 1, except that 26.1 g of light-burned magnesium (large particle size), 2.4 g of ferrous sulfate monohydrate, and 1.5 g of guar gum (small particle size) were premixed to obtain 30 g of a mud treatment agent.
[0055] <Example 3> The mud of Example 3 was prepared in the same manner as in Example 1, except that 26.7 g of light-burned magnesium (large particle size), 1.5 g of ferrous sulfate monohydrate, and 1.8 g of guar gum (small particle size) were premixed to obtain 30 g of a mud treatment agent.
[0056] <Example 4> The mud of Example 4 was prepared in the same manner as in Example 1, except that 26.4 g of light-burned magnesium (large particle size), 2.1 g of ferrous sulfate monohydrate, and 1.5 g of guar gum (small particle size) were premixed to obtain 30 g of a mud treatment agent.
[0057] <Example 5> 27.0 g of light-burned magnesium (large particle size), 1.5 g of ferrous sulfate monohydrate, and 1.5 g of guar gum (small particle size) were mixed in advance to obtain 30 g of a mud treatment agent. This mud treatment agent was added to 2000 g of simulated soil 2 and mixed to obtain the mud of Example 5.
[0058] <Example 6> The mud of Example 6 was prepared in the same manner as in Example 5, except that 26.1 g of light-burned magnesium (large particle size), 2.4 g of ferrous sulfate monohydrate, and 1.5 g of guar gum (small particle size) were premixed to obtain 30 g of a mud treatment agent.
[0059] <Example 7> The mud of Example 7 was prepared in the same manner as in Example 5, except that 26.7 g of light-burned magnesium (large particle size), 1.5 g of ferrous sulfate monohydrate, and 1.8 g of guar gum (small particle size) were premixed to obtain 30 g of a mud treatment agent.
[0060] <Example 8> The mud of Example 8 was prepared in the same manner as in Example 5, except that 26.4 g of light-burned magnesium (large particle size), 2.1 g of ferrous sulfate monohydrate, and 1.5 g of guar gum (small particle size) were premixed to obtain 30 g of a mud treatment agent.
[0061] <Comparative Example 1> The mud of Comparative Example 1 was prepared in the same manner as in Example 1, except that 27.0 g of light-burned magnesium (large particle size), 1.5 g of ferrous sulfate monohydrate, and 1.5 g of guar gum (large particle size) were premixed to obtain 30 g of a mud treatment agent.
[0062] <Comparative Example 2> The mud of Comparative Example 2 was prepared in the same manner as in Example 1, except that 27.0 g of light-burned magnesium oxide (small particle size), 1.5 g of ferrous sulfate monohydrate, and 1.5 g of guar gum (small particle size) were premixed to obtain 30 g of a mud treatment agent.
[0063] <Comparative Example 3> The mud of Comparative Example 3 was prepared in the same manner as in Example 1, except that 27.0 g of light-burned magnesium (small particle size), 1.5 g of ferrous sulfate monohydrate, and 1.5 g of guar gum (large particle size) were premixed to obtain 30 g of a mud treatment agent.
[0064] <Comparative Example 4> The mud of Comparative Example 4 was prepared in the same manner as in Example 1, except that 26.1 g of light-burned magnesium (large particle size), 2.4 g of ferrous sulfate monohydrate, and 1.5 g of guar gum (large particle size) were premixed to obtain 30 g of a mud treatment agent.
[0065] <Comparative Example 5> The mud of Comparative Example 5 was prepared in the same manner as in Example 1, except that 26.1 g of light-burned magnesium oxide (small particle size), 2.4 g of ferrous sulfate monohydrate, and 1.5 g of guar gum (small particle size) were premixed to obtain 30 g of a mud treatment agent.
[0066] <Comparative Example 6> The mud of Comparative Example 6 was prepared in the same manner as in Example 1, except that 26.1 g of light-burned magnesium (small particle size), 2.4 g of ferrous sulfate monohydrate, and 1.5 g of guar gum (large particle size) were premixed to obtain 30 g of a mud treatment agent.
[0067] <Comparative Example 7> The mud of Comparative Example 7 was prepared in the same manner as in Example 1, except that 26.7 g of light-burned magnesium (large particle size), 1.5 g of ferrous sulfate monohydrate, and 1.8 g of guar gum (large particle size) were premixed to obtain 30 g of a mud treatment agent.
[0068] <Comparative Example 8> The mud of Comparative Example 8 was prepared in the same manner as in Example 1, except that 26.7 g of light-burned magnesium oxide (small particle size), 1.5 g of ferrous sulfate monohydrate, and 1.8 g of guar gum (small particle size) were premixed to obtain 30 g of a mud treatment agent.
[0069] <Comparative Example 9> The mud of Comparative Example 9 was prepared in the same manner as in Example 1, except that 26.7 g of light-burned magnesium (small particle size), 1.5 g of ferrous sulfate monohydrate, and 1.8 g of guar gum (large particle size) were premixed to obtain 30 g of a mud treatment agent.
[0070] <Comparative Example 10> The mud of Comparative Example 10 was prepared in the same manner as in Example 1, except that 26.4 g of light-burned magnesium (large particle size), 2.1 g of ferrous sulfate monohydrate, and 1.5 g of guar gum (large particle size) were premixed to obtain 30 g of a mud treatment agent.
[0071] <Comparative Example 11> The mud of Comparative Example 11 was prepared in the same manner as in Example 1, except that 26.4 g of light-burned magnesium oxide (small particle size), 2.1 g of ferrous sulfate monohydrate, and 1.5 g of guar gum (small particle size) were premixed to obtain 30 g of a mud treatment agent.
[0072] <Comparative Example 12> The mud of Comparative Example 12 was prepared in the same manner as in Example 1, except that 26.4 g of light-burned magnesium oxide (small particle size), 2.1 g of ferrous sulfate monohydrate, and 1.5 g of guar gum (large particle size) were premixed to obtain 30 g of a mud treatment agent.
[0073] <Comparative Example 13> The mud of Comparative Example 13 was prepared in the same manner as in Example 5, except that 27.0 g of light-burned magnesium (large particle size), 1.5 g of ferrous sulfate monohydrate, and 1.5 g of guar gum (large particle size) were premixed to obtain 30 g of a mud treatment agent.
[0074] <Comparative Example 14> The mud of Comparative Example 14 was prepared in the same manner as in Example 5, except that 27.0 g of light-burned magnesium oxide (small particle size), 1.5 g of ferrous sulfate monohydrate, and 1.5 g of guar gum (small particle size) were premixed to obtain 30 g of a mud treatment agent.
[0075] <Comparative Example 15> The mud of Comparative Example 15 was prepared in the same manner as in Example 5, except that 27.0 g of light-burned magnesium (small particle size), 1.5 g of ferrous sulfate monohydrate, and 1.5 g of guar gum (large particle size) were premixed to obtain 30 g of a mud treatment agent.
[0076] <Comparative Example 16> The mud of Comparative Example 16 was prepared in the same manner as in Example 5, except that 26.1 g of light-burned magnesium (large particle size), 2.4 g of ferrous sulfate monohydrate, and 1.5 g of guar gum (large particle size) were premixed to obtain 30 g of a mud treatment agent.
[0077] <Comparative Example 17> The mud of Comparative Example 17 was prepared in the same manner as in Example 5, except that 26.1 g of light-burned magnesium oxide (small particle size), 2.4 g of ferrous sulfate monohydrate, and 1.5 g of guar gum (small particle size) were premixed to obtain 30 g of a mud treatment agent.
[0078] <Comparative Example 18> The mud of Comparative Example 18 was prepared in the same manner as in Example 5, except that 26.1 g of light-burned magnesium oxide (small particle size), 2.4 g of ferrous sulfate monohydrate, and 1.5 g of guar gum (large particle size) were premixed to obtain 30 g of a mud treatment agent.
[0079] <Comparative Example 19> The mud of Comparative Example 19 was prepared in the same manner as in Example 5, except that 26.7 g of light-burned magnesium (large particle size), 1.5 g of ferrous sulfate monohydrate, and 1.8 g of guar gum (large particle size) were premixed to obtain 30 g of a mud treatment agent.
[0080] <Comparative Example 20> The mud of Comparative Example 20 was prepared in the same manner as in Example 5, except that 26.7 g of light-burned magnesium oxide (small particle size), 1.5 g of ferrous sulfate monohydrate, and 1.8 g of guar gum (small particle size) were premixed to obtain 30 g of a mud treatment agent.
[0081] <Comparative Example 21> The mud of Comparative Example 21 was prepared in the same manner as in Example 5, except that 26.7 g of light-burned magnesium (small particle size), 1.5 g of ferrous sulfate monohydrate, and 1.8 g of guar gum (large particle size) were premixed to obtain 30 g of a mud treatment agent.
[0082] <Comparative Example 22> The mud of Comparative Example 22 was prepared in the same manner as in Example 5, except that 26.4 g of light-burned magnesium (large particle size), 2.1 g of ferrous sulfate monohydrate, and 1.5 g of guar gum (large particle size) were premixed to obtain 30 g of a mud treatment agent.
[0083] <Comparative Example 23> The mud of Comparative Example 23 was prepared in the same manner as in Example 5, except that 26.4 g of light-burned magnesium oxide (small particle size), 2.1 g of ferrous sulfate monohydrate, and 1.5 g of guar gum (small particle size) were premixed to obtain 30 g of a mud treatment agent.
[0084] <Comparative Example 24> The mud of Comparative Example 24 was prepared in the same manner as in Example 5, except that 26.4 g of light-burned magnesium oxide (small particle size), 2.1 g of ferrous sulfate monohydrate, and 1.5 g of guar gum (large particle size) were premixed to obtain 30 g of a mud treatment agent.
[0085] (Arsenic leaching test) The arsenic elution test for the examples and comparative examples was performed in accordance with JIS K0102 61.2 "Hydride generation atomic absorption spectrometry" using the arsenic measurement kit "MQuant Arsenic Test". The arsenic measurement range by this test method is 0.005 to 0.5 mg / L. In light of environmental standards, it is preferable that the arsenic elution test result of the treatment target after treatment with the mud treatment agent is less than 0.1 mg / L.
[0086] (Corn Index) The cone index in the examples and comparative examples was measured in accordance with JIS A 1228 "Cone index test method for compacted soil". The cone index was measured 1 hour and 24 hours after the mud treatment agent was added to the simulated soil. If the cone index was 150KN / m 2 A pass was achieved when the test was over 100%.
[0087] The results of the experiment on model soil 1 are shown in Table 4, and the results of the experiment on model soil 2 are shown in Table 5.
[0088] [Table 4]
[0089] [Table 5]
[0090] As can be seen from Tables 4 and 5, the results of the arsenic elution tests in all Examples and Comparative Examples were below the lower limit of quantification of 0.005 mg / L, which was significantly lower than the arsenic elution test result of 0.051 mg / L for model soil 1 and 0.039 mg / L for model soil 2, and met the environmental standard. This is believed to be due to the arsenic adsorption effect of ferrous sulfate monohydrate.
[0091] In Examples 1 to 8, the cone index 1 hour after addition of the mud treatment agent was 150KN / m 2 and thus sufficiently solidified the simulated soil 1 and the simulated soil 2. On the other hand, in Comparative Examples 1 to 24, in which the particle size of the guar gum was equal to or larger than the particle size of the polymer, the cone index 1 hour after the addition of the mud treatment agent did not meet the pass standard.
Claims
1. The present invention comprises a powdered natural polymer and a powdered magnesium oxide-based solidifying agent, 90% by mass or more of the natural polymer passes through a 200 mesh sieve; 90% by mass or more of the magnesium oxide-based solidifying agent passes through a 100 mesh sieve, A mud treatment agent in which 90% by mass or more of the magnesium oxide-based solidifying agent does not pass through a 200 mesh sieve, A mud treatment agent, characterized in that the natural polymer is guar gum.
2. Contains ferrous sulfate, 2. The mud treatment agent according to claim 1, wherein a mass ratio of the magnesium oxide-based solidifying agent, the iron sulfate, and the natural polymer is 86.5-90.5:4.5-8.5:4.5-7.
0.
3. 3. The mud treatment agent according to claim 1, wherein the magnesium oxide solidifying agent is light-burned dolomite or light-burned magnesium.
4. A mud treatment method comprising the step of adding the mud treatment agent according to any one of claims 1 to 3 to excavated mud generated by a shield construction method, thereby solidifying the excavated mud.
Citation Information
Patent Citations
Neutral inorganic composite material for dehydration, solidification and modification of high water content sludge
CN101955345A
Method and apparatus for treating muddy water
JP1981076292A
Coagulant for sludge treatment and sludge treating method
JP1998337575A
Agent and method for solidifying sludge
JP2002282894A
Treating method of construction sludge generated in cellular shield construction method
JP2006265885A