Soft magnetic metal flaky powder, resin composite sheet using same, and resin composite composition

The nanocrystalline soft magnetic metal flat powder with controlled properties addresses the challenge of maintaining high magnetic permeability and low core loss in resin composite sheets and molded products, ensuring effective electromagnetic noise suppression and magnetic shielding across varying temperatures.

JP7565611B2Active Publication Date: 2024-10-11MEITOYUUGEN
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2022013691
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-01-13
Publication Date
2024-10-11
Estimated Expiration
2042-01-13

AI Technical Summary

Technical Problem

Existing resin composite sheets and molded products using soft magnetic metal flat powders face challenges in maintaining high magnetic permeability and low core loss across a wide temperature range, particularly in thin-walled and flexible applications, with insufficient performance in electromagnetic noise suppression and magnetic shielding due to temperature fluctuations.

Method used

A nanocrystalline soft magnetic metal flat powder with specific particle size, aspect ratio, and crystallinity, combined with a resin composite sheet and composition, is developed to maintain high magnetic permeability and low core loss within the temperature range of -40°C to 150°C, using a controlled nanocrystallization process and optimized processing methods to adjust coercive force and particle size.

Benefits of technology

The solution provides resin composite sheets and compositions with stable magnetic permeability and low core loss across a broad temperature range, enhancing electromagnetic noise suppression and magnetic shielding performance, especially in thin-walled and flexible applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007565611000004
    Figure 0007565611000004
  • Figure 0007565611000005
    Figure 0007565611000005
  • Figure 0007565611000001
    Figure 0007565611000001
Patent Text Reader

Abstract

To provide a nanocrystalline soft magnetic metal flat powder with little change in the temperature coefficient of magnetic permeability and having high magnetic permeability and low core loss, a resin composite sheet using the material, and a resin composite composition for molding.SOLUTION: A magnetic permeability temperature coefficient Kn (n is 1, 2, 3) of nanocrystalline soft magnetic metal flat powder is expressed by the following formulas (1), (2), and (3) in the range of -40°C to 150°, and also in the range of C0≤K1≤0.20, -0.10≤K2≤0.10, and -0.15≤K3≤0.05, and higher soft magnetic properties can be obtained. K1=(μ(0°C)-μ(-40°C)) / μ(-40°C) (1). K2=(μ(85°C)-μ(-40°C)) / μ(-40°C) (2). K3=(μ(150°C)-μ(-40°C)) / μ(-40°C) (3). μ: permeability (μ': real permeability, μ": imaginary permeability), μ(0°C): permeability at 0°C.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

Detailed Description of the Invention [Technical field]

[0001] The present invention relates to a soft magnetic metal flaky powder used in noise suppression parts used as a countermeasure against unwanted electromagnetic waves in communication devices and various electronic devices, magnetic shield parts used in electromagnetic induction devices, and cores for electronic components such as inductors and reactors, and to a resin composite sheet and a resin composite composition for molding using the same. [Background technology]

[0002] Unwanted electromagnetic waves generated by communication devices and various electronic devices can cause equipment malfunctions and communication failures due to external and internal interference, and various countermeasures have been implemented, but as the types of radio waves used increase and frequencies become higher, the types of control ICs and driving frequencies become more diverse, making the problem more apparent.

[0003] In addition, as communication devices and various electronic devices become thinner and smaller, the mounting density of electronic components has increased dramatically, resulting in frequent problems caused by electromagnetic interference between components and circuit boards. To combat this, noise-suppressing electronic components and flexible magnetic sheets (resin composite sheets) are being used.

[0004] On the other hand, the effective use of electromagnetic waves is progressing, and pen input and contactless charging for mobile devices that use electromagnetic induction methods have become widespread. In addition, resin composite sheets and molded products are being used as magnetic shielding materials in combination with coil components to prevent interference with metal parts and make effective use of magnetic fields.

[0005] Soft magnetic metal flake powder is used in resin composite sheets and molded products used for electromagnetic noise suppression and magnetic shielding. This is because processing into a flake shape reduces the demagnetizing factor, increases the in-plane magnetic permeability, and allows the magnetic permeability to be maintained up to higher frequencies beyond the snake's limit. For electromagnetic noise suppression, the imaginary permeability μ'' which indicates the magnetic loss of the magnetic permeability is used, while for magnetic shielding, the real permeability μ' is used.

[0006] However, in recent years, with the progress of thinning and miniaturization of devices, the mounting space for electromagnetic noise suppression and magnetic shielding parts has become limited, and there is an increasing demand for resin composite sheets and resin composite compositions for molding using soft magnetic metal flake powders that have high magnetic permeability and low core loss, i.e., so-called high soft magnetic properties. In addition, there is a demand for core materials with high soft magnetic properties for miniaturization, loss reduction, and large current compatibility in electronic components such as inductors and reactors for boost circuits.

[0007] Conventionally, it has been known that the magnetic permeability of a flat powder of Fe-Al-Si composition called Sendust, which is a soft magnetic metal flat powder using Fe-based alloy powder, is high, and in particular, a composition consisting of Fe and unavoidable impurities at about Al: 5.4wt% and Si: 9.6wt%, where both the crystal magnetic anisotropy and magnetostriction are zero, is excellent. For this reason, there is Patent No. 3722391 (Patent Document 1), which adjusts the composition by taking into account the surface oxidation of the flat powder. On the other hand, Patent No. 6592424 (Patent Document 2) and JP-A-2005-281783 (Patent Document 3) propose that a higher magnetic permeability can be obtained by actively adjusting the composition of Al and Si.

[0008] In addition, with regard to nanocrystalline materials that are expected to have soft magnetic properties exceeding those of sendust, nanocrystalline soft magnetic metal flat powders have been proposed in Japanese Patent No. 2702757 (Patent Document 4) and Japanese Patent Laid-Open No. 11-269509 (Patent Document 5). Furthermore, Japanese Patent Laid-Open No. 2021-111766 (Patent Document 6) proposes Fe-Al-Si-based soft magnetic metal flat powders that have little change in magnetic permeability in the temperature range in which various devices actually operate and can obtain high magnetic permeability. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] Patent No. 3722391 [Patent Document 2] Patent No. 6592424 [Patent Document 3] Patent Publication No. 2005-281783 [Patent Document 4] Patent No. 2702757 [Patent Document 5] Patent Publication No. 11-269509 [Patent Document 6] Patent Publication No. 2021-111766 Summary of the Invention [Problem to be solved by the invention]

[0010] When communication devices and various electronic devices are actually used, there are changes in the ambient temperature and heat generation, and there is a demand for performance guarantee at -40 to 150°C for automobiles and -40 to 85°C for other devices. For this reason, it is necessary to ensure stable and high electromagnetic noise suppression and magnetic shielding performance, or soft magnetic properties as a core material, at least in the temperature range of -40 to 85°C for resin composite sheets and molded products. In particular, in non-contact power supply using electromagnetic induction, heat is generated in the battery during charging and in the module due to magnetic loss in coil parts including magnetic materials, so if the performance of the magnetic shielding material decreases due to temperature rise, magnetic loss increases, which further increases the temperature and reduces performance, resulting in a vicious cycle that reduces charging efficiency.

[0011] However, soft magnetic properties including magnetic permeability are generally measured only at room temperature, and there is no description of obtaining stable magnetic permeability in the actual operating temperature range as referred to in the present invention in Patent Documents 1, 2, 3, 4, and 5. Furthermore, compared with ferrite sintered bodies used for NFC and contactless charging, or pre-cracked ferrite sheets, amorphous sheets, nanocrystalline metal sheets, etc., the magnetic permeability is insufficient and the magnetic shielding performance is insufficient.

[0012] In addition, Patent Documents 4 and 5 state that high soft magnetic properties can be obtained by using a nanocrystalline soft magnetic metal flat powder that is processed into a flat shape by crushing an Fe-based amorphous ribbon after embrittlement treatment and then nanocrystallizing it, but Patent Document 4 focuses on the coercive force and saturation magnetic flux density, and does not state anything about the magnetic permeability. In addition, the D50 average particle size is small, and the aspect ratio is also low. Patent Document 5 does not state anything about the coercive force, and it cannot be said that the magnetic permeability is sufficiently high.

[0013] Furthermore, there is a demand for resin composite sheets that have low core loss while maintaining magnetic permeability, and that have high flexibility and thin-walled products, as well as products with higher magnetic permeability and low core loss. In order to realize a thin-walled product with high flexibility, it is necessary to reduce the powder blending amount by using nanocrystalline soft magnetic metal flat powder that has high soft magnetic properties even with a small particle size. Furthermore, in order to respond to high magnetic permeability, it is necessary to significantly improve the soft magnetic properties of the nanocrystalline soft magnetic metal flat powder. However, it is difficult to achieve both of these, and it is necessary to provide a resin composite sheet that has characteristics in either flexibility or magnetic permeability by optimally nano-crystallizing the nanocrystalline soft magnetic metal flat powder, adjusting the particle size and aspect ratio, and suppressing the coercive force. In addition, there is a demand for thinning and high magnetic permeability in resin composite compositions for molding processing, and it is necessary to provide a resin composite composition that can respond to thinning by maintaining magnetic permeability and having low core loss, and a resin composite composition that has higher magnetic permeability and low core loss.

[0014] The present invention has been made to solve the above problems, and aims to provide a nanocrystalline soft magnetic metal flaky powder having a small change in the temperature coefficient of magnetic permeability within the range of -40°C to 150°C when used in a resin composite sheet or a resin composite composition molded product, and having high magnetic permeability and low core loss, as well as a resin composite sheet using this material and having high magnetic permeability and low core loss, and a resin composite composition for molding.

[0015] The present invention aims to solve the problems associated with the above-mentioned conventional soft magnetic metal flaky powder, the resin composite sheet using said material, and the resin composite composition for molding. [Means for solving the problem]

[0016] According to the present invention, there is provided a nanocrystalline soft magnetic metal flaky powder in which the nanocrystalline particles have a particle size of 5 nm to less than 30 nm, a crystallinity of 65% to less than 95%, and further, the aspect ratio of the powder having a particle size near the average particle size D50 is less than 20 to 80, and the coercive force is less than 20 A / m to 150 A / m. The nanocrystalline soft magnetic metal flaky powder is characterized in that the temperature coefficient of magnetic permeability Kn (n is 1, 2, 3) of a resin composite sheet or a molded resin composite composition using the nanocrystalline soft magnetic metal flaky powder is represented by the following formulas (1), (2), and (3) in the range of -40°C to 150°C or less, and is in the ranges of 0≦K1≦0.20, -0.10≦K2≦0.10, and -0.15≦K3≦0.05. K1=(μ(0℃)-μ(-40℃)) / μ(-40℃) (1) K2=(μ(85℃)-μ(-40℃)) / μ(-40℃) (2) K3=(μ(150℃)-μ(-40℃)) / μ(-40℃) (3) μ: Magnetic permeability (μ': Real magnetic permeability, μ”: Imaginary magnetic permeability), μ(0℃): Magnetic permeability at 0℃

[0017] Furthermore, according to the present invention, there is obtained a nanocrystalline soft magnetic metal flaked powder, characterized in that the nanocrystalline soft magnetic metal flaked powder has an average particle size D50 of 20 μm to less than 40 μm, an average thickness around the D50 average particle size of less than 0.2 μm to 1.5 μm, and a resin composite sheet using the nanocrystalline soft magnetic metal flaked powder has a coercive force of 20 A / m to less than 100 A / m.

[0018] Furthermore, according to the present invention, there is obtained a nanocrystalline soft magnetic metal flaked powder, characterized in that the nanocrystalline soft magnetic metal flaked powder has an average particle size D50 of 40 μm to less than 100 μm, an average thickness around the D50 average particle size of 1.5 μm to less than 5 μm, and a resin composite sheet using the nanocrystalline soft magnetic metal flaked powder has a coercive force of 20 A / m to less than 80 A / m.

[0019] According to the present invention, the core loss is 50kW / m when measured under the conditions of Bm and frequency of 50mT-100kHz using three stacked ring-shaped samples made of the nanocrystalline soft magnetic metal flaky powder and resin, the coercive force is 20A / m to less than 100A / m, and the samples are 20mm in outer diameter, 10mm in inner diameter, and 0.15mm in thickness. 3 ~300kW / m 3 A resin composite sheet is obtained, characterized in that the resin composite sheet has a thickness of less than 100 μm.

[0020] According to the present invention, a core loss of 100 kW / m2 was measured under the conditions of Bm and frequency of 50 mT-100 kHz using a molded product made of the nanocrystalline soft magnetic metal flake powder and resin, with an outer diameter of 12.8 mm, an inner diameter of 7.5 mm, and a thickness of 5 mm. 3 ~600kW / m 3 The resin composite composition for molding is obtained, characterized in that the viscosity of the resin composite is less than 1000 MPa. Effect of the Invention

[0021] The present invention provides a nanocrystalline soft magnetic metal flaky powder having a small change in the temperature coefficient of magnetic permeability within the range of -40°C to 150°C when used in a resin composite sheet or a resin composite composition molded product, and having high magnetic permeability and low core loss, as well as a resin composite sheet using the material and having high magnetic permeability and low core loss, and a resin composite composition for molding. [Brief description of the drawings]

[0022] [Figure 1] This figure shows a method for calculating the degree of crystallinity by profile fitting using the bcc Fe(110) peak near 2θ=45° obtained by orienting nanocrystalline metal flake powder parallel to the measurement surface and measuring it with a Cu tube using XRD. [Diagram 2] 1 is a graph showing the temperature dependence of magnetic permeability of resin composite sheets using flat soft magnetic metal powders of Examples 4 and 9 and Comparative Examples 10 and 11. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0023] The best mode of the present invention will now be described in detail.

[0024] The amorphous alloys that are the raw material for nanocrystalline soft magnetic metal flake powder can be produced by quenching methods such as the single roll method, twin roll method, and melt spin method. do.

[0025] The amorphous alloy is an Fe-based alloy, and for example, an alloy having an Fe-Si-B-Nb-Cu composition or an Fe-Si-BP-Cu composition can be used. If necessary, it may contain trace components such as Cr, W, Ta, Hf, Ti, Ni, and C, but is not particularly limited as long as a nanocrystalline phase can be obtained by crystallization treatment.

[0026] When using a metal foil strip obtained by a single roll method, a twin roll method, a melt spin method, or the like, it is difficult to pulverize the metal foil strip to obtain a raw material for flattening as it is. In addition, in order to obtain a raw material powder having the desired processability, the metal foil strip is embrittled at a temperature exceeding 200°C and below the nanocrystallization temperature in air or nitrogen gas atmosphere, inert gas atmosphere, or vacuum, and then pulverized with a ball mill, vibration mill, pin mill, hammer mill, or the like to obtain a raw material powder for flattening of a predetermined particle size. However, if embrittlement has progressed during the manufacturing process of the metal foil strip, embrittlement is not particularly necessary, and the metal foil strip may be pulverized as it is. In addition, if the metal foil strip can be flattened, embrittlement and pulverization can be omitted.

[0028] The flattening process is not particularly limited, but can be carried out in the presence of distilled water or an organic solvent using an attritor, ball mill, vibration mill, etc. As the organic solvent, toluene, hexane, alcohol, ethylene glycol, etc. can be used, and the atmosphere inside the device can be adjusted during processing. Stearic acid, etc. can also be added as a flattening aid.

[0029] After the flattening process, the amorphous alloy flat powder is heat-treated in a nitrogen gas atmosphere, an inert gas atmosphere, or in a vacuum at a temperature above the crystallization temperature to generate a nanocrystalline phase. The heat treatment device and conditions are not particularly limited as long as the flat powder breaks down and becomes smaller in diameter due to the volumetric shrinkage associated with nanocrystallization, and the desired crystal grain size and degree of crystallinity can be achieved.

[0030] The aspect ratio of the nanocrystalline soft magnetic metal flat powder in the powder having an average particle size of about D50 is preferably 20 to less than 80, and the coercive force is preferably 20A / m to less than 150A / m. If the aspect ratio is less than 20, the demagnetizing factor becomes large, and if it is 80 or more, the processability decreases. However, even if the aspect ratio is less than 20 to 80, if the proportion of fine powder increases, the coercive force becomes 150A / m or more, and the magnetic permeability of the resin composite sheet and molded product decreases. For this reason, the coercive force may be adjusted by removing the fine powder by air classification or the like.

[0031] The average particle diameter D50 of the nanocrystalline soft magnetic metal flat powder was measured using R4 with HELOS / BR-multi manufactured by Sympatec. Flat powders with a particle diameter range of ±10% of the obtained average particle diameter D50 were extracted by air classification, embedded in epoxy resin and mirror polished to obtain a sample for thickness measurement. The aspect ratio is expressed as diameter / thickness because the flat powder is generally disc-shaped, but the diameter is the value of the average particle diameter D50, and the thickness of the flat powder was measured with a scanning electron microscope to obtain the aspect ratio. The aspect ratio may also be obtained by embedding a resin composite sheet or molded product in epoxy resin, measuring the average length and thickness with a scanning electron microscope, and correcting the length to the diameter.

[0032] The magnetic permeability was measured in a thermostatic chamber at a temperature range of -40°C to 150°C using an impedance analyzer E4991B, a magnetic material test fixture 16454A, and a heat resistance test kit manufactured by Keysight Corporation. The measurement samples used were products obtained by molding a resin composite sheet and a resin composite composition. The measurement sample for the resin composite sheet was made by punching a ring-shaped sample having an outer diameter of 20 mm and an inner diameter of 10 mm from a sheet having a thickness of 0.15 mm. The molded product used was a sample having an outer diameter of 20 mm, an inner diameter of 20 mm, and a thickness of 0.6 mm. The shape of the sample for measuring the magnetic permeability is not particularly limited as long as the magnetic permeability can be measured. Furthermore, the measurement may be performed in the state of the resin composite sheet or the molded product, or in the state of powder, using a vibration sample magnetometer (VSM), a BH analyzer, an LCR meter, or the like.

[0033] The coercive force was measured using an automatic coercive force meter K-HC1000 manufactured by Tohoku Special Steel Co., Ltd., with an applied magnetic field of 148 kA / m. Approximately 10 mg of the flat powder was covered with non-magnetic tape to prevent scattering, and used as a measurement sample. A sample for magnetic permeability measurement was used to measure the coercive force of the resin composite sheet and the molded product of the resin composite composition. Coercive force may also be measured using a vibrating sample magnetometer (VSM), BH analyzer, etc.

[0034] The crystal grain size of the nanocrystalline particles of the nanocrystalline soft magnetic metal flat powder is desirably 5 nm to less than 30 nm, and more preferably 5 nm to less than 25 nm. If the crystal grain size is less than 5 nm, the nanocrystalline particle growth is insufficient, resulting in poor soft magnetic properties, and if it is 30 nm or more, the responsiveness of the crystal grains to an AC magnetic field decreases, resulting in poor soft magnetic properties. In addition, the crystallinity is desirably less than 65% to less than 95%, and more preferably less than 65% to less than 90%. If the crystallinity is less than 65%, the crystal grains are insufficiently generated, and if it is 95% or more, the crystal grains become coarse, resulting in poor soft magnetic properties.

[0035] The crystal grain size of the nanocrystalline particles was determined by orienting the nanocrystalline metal flat powder so that the plane of the powder was roughly parallel to the measurement surface, and the results of XRD measurement using a Cu tube on a powder X-ray diffractometer MiniFlex600 manufactured by Rigaku were used to determine the crystallinity using the peak of bcc Fe (110) near 2θ = 45 ° according to the Sherrer formula. The crystallinity was calculated from the XRD measurement results by the profile fitting method using the SmartLab Studio II applied analysis package manufactured by Rigaku. For the calculation, the area of ​​the diffraction peak before and after nanocrystallization of bcc Fe (110) was used, as shown in Figure 1. Since it is difficult to measure the crystallinity precisely, the apparent crystallinity obtained simply from the XRD measurement results was used as the crystallinity. The sample for XRD measurement does not need to be a powder, and it is sufficient to set the sheet and molded product in a folder so that the plane of the nanocrystalline metal flat powder is roughly parallel to the measurement surface.

[0036] The nanocrystalline soft magnetic metal flat powder desirably has an average particle diameter D50 of 20 μm to less than 40 μm. If it is less than 20 μm, the amount of fine powder with high coercive force increases, making it difficult to obtain a sufficiently high magnetic permeability. If it is 40 μm or more, the flexibility of the resin composite sheet decreases. In addition, it is desirable that the average thickness near the average particle diameter D50 is less than 0.2 μm to 1.5 μm. If it is less than 0.2 μm, the specific surface area becomes too high, resulting in reduced processability, and if it is 1.5 μm or more, the aspect ratio becomes small, and the magnetic permeability decreases due to an increase in the demagnetizing field coefficient. It is desirable that the coercive force of the resin composite sheet using the nanocrystalline soft magnetic metal flat powder is less than 20 A / m to 100 A / m. If the coercive force is 100 A / m or more, the magnetic permeability decreases.

[0037] The nanocrystalline soft magnetic metal flat powder preferably has an average particle diameter D50 of 40 μm to less than 100 μm. If it is less than 40 μm, the requirement for particularly high magnetic permeability cannot be met, and if it is more than 100 μm, the processability decreases. Furthermore, the coarse flat powder contains internal cracks, which become magnetic gaps and lead to a decrease in soft magnetism, so they may be removed by air classification or mechanical sieving. In addition, it is preferable that the average thickness near the D50 average particle diameter is less than 1.5 μm to 5 μm. If it is less than 1.5 μm, the amount of fine powder with high coercive force increases, and if it is 5 μm or more, the demagnetizing field coefficient increases and the magnetic permeability decreases. It is preferable that the coercive force of the resin composite sheet using the nanocrystalline soft magnetic metal flat powder is less than 20 A / m to 80 A / m. If it is 80 A / m or more, the magnetic permeability decreases.

[0038] Furthermore, the bulk density / true density is preferably in the range of 0.034 to 0.076. If it is less than 0.034, the flattening will progress too much, making handling difficult, and the amount of over-pulverized fine powder will increase and the contour will become uneven, resulting in high coercive force and low magnetic permeability. On the other hand, if it exceeds 0.076, the flattening will be insufficient and the magnetic permeability will decrease. The bulk density was measured based on JIS Z2504. The true density was measured using AccuPyc1330 manufactured by Shimadzu Corporation.

[0039] The resin composite sheet is prepared by mixing nanocrystalline soft magnetic metal flaky powder and polymeric material in a predetermined ratio, forming it into an ink-like form using various known methods, and then producing a sheet-like product by doctor coating, comma coating, screen printing, etc., which may be further compressed with various rolls or presses. It may also be produced by kneading with a kneader or the like and then rolling it, and then compressing it with a press, but the method for producing the resin composite sheet is not limited to these. When producing the sheet, a magnetic field is applied to control the orientation of the nanocrystalline soft magnetic metal flaky powder, thereby increasing the magnetic permeability.

[0040] As the polymer resin, polyurethane, acrylic, silicon, epoxy, chlorinated polyethylene, chloroprene rubber, etc. can be used alone or in combination, but there is no particular limitation, and it is desirable that the resin has a heat resistance of 150°C. There is also no particular limitation on the thermoplasticity and thermosetting properties. In addition, various surface treatments using coupling agents, dispersants, rust inhibitors, etc., and various additives such as antioxidants, pigments, non-magnetic fillers, and thermally conductive fillers can be added as necessary within a range that does not impair the object of the present invention.

[0041] The resin composite sheet preferably has a coercive force of 20 A / m to less than 100 A / m, more preferably less than 80 A / m. If the coercive force is 100 A / m or more, the magnetic permeability decreases. Also, if the core loss is less than 50 kW / m 3 ~300kW / m 3 It is preferable that it is less than 200 kW / m 3 It is more preferable that the core loss is less than 300 kW / m 3If the content exceeds this amount, when the powder is used in the magnetic parts of various electronic components, magnetic loss increases, resulting in a decrease in component performance. Furthermore, when the powder is used as a magnetic shielding material for contactless charging, the decrease in charging efficiency due to magnetic loss and the associated heat generation become major problems. The content of the nanocrystalline soft magnetic metal flake powder is desirably less than 35 vol% to 65 vol% of the total solid content. More desirably, it is less than 40 vol% to 55 vol%. If the content is less than 35 vol%, the magnetic permeability will be low even if the coercive force is less than 100 A / m, and if the content is 65 vol% or more, it will be difficult to form the powder into a sheet, and the magnetic permeability will decrease.

[0042] The core loss was measured for the resin composite sheet and the molded product of the resin composite composition using a BH analyzer SY-8219 manufactured by Iwasaki Electric Co., Ltd. and a high-speed bipolar power supply HSA4041 manufactured by NF Corporation. The measurement sample for the resin composite sheet was made by punching out a ring-shaped sample with an outer diameter of 20 mm and an inner diameter of 10 mm from a sheet with a thickness of 0.15 mm, stacking three of these, sandwiching them between non-magnetic resin plates, and winding a wire rod with a diameter of 0.26 mm on the secondary winding. The primary side had 19 turns and the secondary side had 5 turns. The molded products were prepared as follows: a sample with an outer diameter of 20 mm and an inner diameter of 10 mm and a thickness of 0.6 mm, and a sample with an outer diameter of 12.8 mm and an inner diameter of 7.5 mm and a thickness of 5 mm. The sample with an outer diameter of 20 mm had 19 turns on the primary side and 5 turns on the secondary side, and the sample with an outer diameter of 12.8 mm had 15 turns on the primary side and 5 turns on the secondary side to prepare the measurement samples. The measurements were carried out at room temperature of 25°C, with Bm and frequency of 50mT-100kHz.

[0043] The resin composite composition is obtained by mixing nanocrystalline soft magnetic metal flaky powder with a polymer resin and kneading it with a kneader or a twin-screw kneader, but is not limited to these and can be produced by various known methods. The content of the nanocrystalline soft magnetic metal flaky powder relative to the total solid content is desirably 35 vol% to less than 65 vol%, and more desirably 40 vol% to less than 60 vol%. If it is less than 35 vol%, the magnetic permeability of the molded product will be low, and if it is 65 vol% or more, molding will be difficult and the magnetic permeability will decrease. In addition, the core loss will be 100 kW / m 3~600kW / m 3 It is preferable that it is less than 400 kW / m 3 More preferably, it is less than

[0044] The resin composite composition can be molded into various shapes using, but not limited to, an extrusion molding machine, an extrusion molding machine, a compression molding machine, etc. During molding, a magnetic field may be applied to orient the flat powder. EXAMPLES

[0045] The present invention will now be described in more detail with reference to examples.

[0046] Examples 1 to 12 and Comparative Examples 1-4 and 6-9 The nanocrystalline soft magnetic metal flake powder used in the present study was prepared using Fe 20 μm thick powder produced by the single roll method. 83.3 S 7.7 B 2.0 Nb 5.7 Cu 1.3 An amorphous ribbon having a composition of (wt%) was used as the starting material. This was then subjected to the annealing in an Ar atmosphere in Examples 1 to 5 and Comparative Example. 1~4 The temperature was 420°C, and Examples 6 to 12 and Comparative Example 6~9 Each was embrittlement treated at 220℃ for 1 hour, then crushed to 74μm or less in a ball mill. The crushed powder was then flattened under wet conditions using ethanol in an attritor. It was then nanocrystallized at 560℃ for 1 hour in an Ar atmosphere.

[0047] Examples 1 to 12 and Comparative Examples 1 to 4, Comparative Examples 6 to 9The nanocrystalline soft magnetic metal flat powder obtained was mixed and dispersed in a resin solution diluted with toluene with a thermosetting acrylic rubber-based mixed resin with a heat resistance of 150°C so that the total solid content was 50 vol%. This paint was applied to a thickness of 0.05 mm using a comma coater, and after magnetic field orientation, it was dried at 50°C to remove the solvent. Six dried sheets were stacked and hot pressed at 150°C with a pressure of 10 MPa to obtain a resin composite sheet for performance evaluation with a thickness of 0.15 mm. Next, it was punched into a doughnut shape with an outer diameter of 20 mm and an inner diameter of 10 mm, and the magnetic permeability, coercive force, and core loss were measured. The real part (μ') of the magnetic permeability at each temperature was measured at 1 MHz, and the imaginary part (μ'') was measured at 10 MHz.

[0048] In Comparative Examples 5 and 10, Fe was prepared by gas atomization. 84.8 Al 5.6 S 9.6 In Comparative Example 11, the alloy powder was made of Fe 84.0 Al 7.0 S 9.0 The starting material was an alloy powder with a composition of (wt%), which was flattened in an attritor under wet conditions using ethanol, and then heat-treated in an Ar atmosphere at 700°C for 1 hour. A resin composite sheet was made using this flat powder and a thermosetting acrylic rubber-based mixed resin with a heat resistance of 150°C, and the magnetic permeability, coercivity, and core loss were measured. The real part (μ') of the magnetic permeability at each temperature was measured at 1 MHz, and the imaginary part (μ'') was measured at 10 MHz.

[0049] Table 1 shows Examples 1 to 5 and Comparative Example 1~5 In Examples 1 to 5, the flexibility of the resin composite sheet was emphasized, and the flattening conditions were adjusted so that the nanocrystalline metal flat powder had an average particle size of less than 20 μm to 40 μm and an average thickness of less than 0.2 to 1.5 μm, and flattened powder with a predetermined bulk density / true density was obtained after nanocrystallization. Furthermore, in the flattening process, the flattening conditions such as the slurry concentration and the collision energy of the grinding media were optimized so that the coercive force after nanocrystallization was minimized, the generation of fine powder was suppressed, and the contour of the flattened powder was smooth. At the same time, controlled moderate microcracks were introduced into the surface of the flattened powder.

[0050] Table 2 shows Examples 6 to 12 and Comparative Example. 6~11 In Examples 6 to 12, the magnetic permeability of the resin composite sheet was emphasized, and the flattening conditions were adjusted so that the average particle size of the nanocrystalline soft magnetic metal flat powder was less than 40 μm to 100 μm, the average thickness was less than 1.5 to 5 μm, and flat powder with a predetermined bulk density / true density was obtained after nanocrystallization. Furthermore, in the flattening process, the flattening conditions such as the slurry concentration and the collision energy of the grinding media were optimized so that the coercive force after the nanocrystallization process was minimized, the generation of fine powder was suppressed, and the outline of the flat powder was smooth. At the same time, moderate microcracks were introduced into the surface of the flat powder. In Examples 8 to 10, 5 wt% of fine powder with high coercive force and coarse flat powder with internal cracks that become magnetic gaps and affect the soft magnetic properties were removed by air classification.

[0051] Table 3 shows Examples 13 and 14 and Comparative Examples 12 and 13. Examples 13 and 14 and Comparative Examples 12 and 13 respectively use the nanocrystalline soft magnetic metal flaky powder of Example 4 and the Fe of Comparative Example 10. 84.8 Al 5.6 S 9.6 A soft magnetic metal flat powder having a composition of 10 ...

[0052] [Table 1]

[0053] [Table 2]

[0054] [Table 3]

[0055] From Table 1, in all of Examples 1 to 5, the temperature coefficients K of real (1 MHz) and imaginary permeability (10 MHz) satisfy 0≦K1≦0.20, −0.10≦K2≦0.10, and −0.15≦K3≦0.05 in the range of −40° C. to 150° C., and the effect of the measurement temperature on the permeability is minor. 1~4 The Fe alloy produced by the gas atomization method in Comparative Example 5 has higher real and imaginary permeabilities at 0° C. and has lower core loss than the Fe alloy produced by the gas atomization method in Comparative Example 5. 84.8 Al 5.6 S 9.6 In the case of the flat metal powder using alloy powder of (wt%) composition, the magnetic permeability is maximum at 0°C, and there is a significant drop in the magnetic permeability at 85°C and 150°C. Furthermore, the magnetic permeability at 0°C is significantly insufficient, and the core loss is high.

[0056] From Table 2, in all of Examples 6 to 12, the temperature coefficients K of real (1 MHz) and imaginary permeability (10 MHz) satisfy 0≦K1≦0.20, -0.10≦K2≦0.10, and -0.15≦K3≦0.05 in the range of -40°C to 150°C, and the effect of the measurement temperature on the permeability is minor. In addition, they have significantly higher real and imaginary permeabilities at 0°C than Comparative Examples 6 to 9, and have low core loss. In particular, Examples 8 to 10, in which fine powder and coarse flat powder were removed by air classification, show extremely high permeability values. Fe produced by the gas atomization method in Comparative Example 10 84.8 Al 5.6 S 9.6 In the case of the flat metal powder using the alloy powder of the composition (wt%), the magnetic permeability is maximum at 0°C, and drops significantly at 85°C and 150°C. Furthermore, the magnetic permeability at 0°C is insufficient, and the core loss is high. 84.0 Al 7.0 S 9.0In the case of the flat metal powder using an alloy powder of (wt%) composition, the temperature dependence of the magnetic permeability is smaller than that of Comparative Example 10, but the decrease in magnetic permeability becomes significant above 85°C, the magnetic permeability at 0°C is also insufficient, and the core loss is high.

[0057] As shown in Fig. 2, the real permeability (1 MHz) of Examples 4 and 9 shows a maximum value near 0°C, but the temperature change of the permeability is smaller and the value is higher than that of Comparative Examples 10 and 11. In particular, Example 9 has a significantly high permeability in the temperature range of -40°C to 150°C. Furthermore, despite the small particle size, Example 10 has a higher permeability than Comparative Examples 10 and 11, and the amount of flat powder to be mixed can be reduced to achieve the same permeability, making it possible to reduce the thickness of the resin composite sheet and improve its flexibility.

[0058] From Table 3, in both Examples 13 and 14, the temperature coefficient K of real (1 MHz) and imaginary permeability (10 MHz) satisfies 0≦K1≦0.20, -0.10≦K2≦0.10, -0.15≦K3≦0.05 in the range of -40 ° C to 150 ° C, and the effect of the measurement temperature on the permeability is minor. In addition, it has a higher real and imaginary permeability at 0 ° C than Comparative Example 12, and even in Example 14, which has a large powder blending amount, it has better molding processability than Comparative Example 12. Therefore, it is easy to make the molded product thinner. Comparative Example 12 shows a maximum permeability at 0 ° C, and the permeability drops significantly with increasing temperature. Comparative Example 13 could not be molded because the powder blending amount was too large, and it was not possible to measure. The core loss is lower in Shape 1 than Shape 2 in the highly oriented nanocrystalline soft magnetic metal flat powder and Shape 2, which is randomly oriented, but Examples 13 and 14 show values ​​significantly lower than Comparative Example 12.

Claims

1. A nanocrystalline soft magnetic metal flat powder having an Fe-Si-B-Nb-Cu composition or an Fe-Si-B-P-Cu composition, in which the particle size of the nanocrystalline particles is 5 nm to less than 30 nm and the crystallinity is 65% to less than 95%, and the aspect ratio of the powder having a particle size around the average particle size D50 is 20 to less than 80, the bulk density / true density is 0.034 to 0.076, and the coercive force is 20 A / m to less than 150 A / m. Furthermore, the temperature coefficient Kn (n is 1, 2, 3) of the magnetic permeability of a resin composite sheet or a molded product of a resin composite composition using the nanocrystalline soft magnetic metal flat powder is represented by the following formulas (1), (2), and (3) in the range of -40 ° C. to 150 ° C. or less, and is in the range of 0 ≦ K1 ≦ 0.20, -0.10 ≦ K2 ≦ 0.10, and -0.15 ≦ K3 ≦ 0.

05. K1=(μ(0℃)−μ(−40℃)) / μ(−40℃) (1) K2=(μ(85℃)−μ(−40℃)) / μ(−40℃) (2) K3=(μ(150℃)−μ(−40℃)) / μ(−40℃) (3) μ: magnetic permeability (μ': real magnetic permeability, μ”: imaginary magnetic permeability), μ (0℃): magnetic permeability at 0℃

2. The nanocrystalline soft magnetic metal flaky powder according to claim 1, characterized in that the average particle diameter D50 is less than 20 μm to 40 μm, the average thickness around the D50 average particle diameter is less than 0.2 μm to 1.5 μm, and the coercive force of a resin composite sheet using the nanocrystalline soft magnetic metal flaky powder is 20 A / m to less than 100 A / m.

3. The nanocrystalline soft magnetic metal flaky powder according to claim 1, characterized in that the average particle diameter D50 is less than 40 μm to 100 μm, the average thickness around the D50 average particle diameter is less than 1.5 μm to 5 μm, and the coercive force of a resin composite sheet using the nanocrystalline soft magnetic metal flaky powder is less than 20 A / m to 80 A / m.

4. A method for producing a nanocrystalline soft magnetic metal flaky powder according to any one of claims 1 to 3, A step of subjecting a raw material Fe-based amorphous alloy foil strip to an embrittlement treatment at a temperature equal to or lower than a nanocrystallization temperature; A step of pulverizing the embrittlement treatment to obtain a raw material powder for flattening; A step of performing a flattening process in the presence of distilled water or an organic solvent, and introducing microcracks into the surface of the raw material powder for flattening during the flattening process; This method for producing nanocrystalline soft magnetic metal flat powder is characterized by the steps of: heat-treating the flat powder obtained after the flattening process at a temperature equal to or higher than the crystallization temperature in a nitrogen gas atmosphere, an inert gas atmosphere, or in vacuum to generate a nanocrystalline phase; and causing the flat powder to self-break and become smaller in diameter due to the volumetric shrinkage associated with nanocrystallization.

5. A resin composite sheet comprising the nanocrystalline soft magnetic metal flaky powder according to any one of claims 1 to 3 and a resin, the coercive force being 20 A / m to less than 100 A / m, and further comprising three stacked ring-shaped samples each having an outer diameter of 20 mm, an inner diameter of 10 mm, and a thickness of 0.15 mm, as a measurement sample of the resin composite sheet. When the measurement sample is measured under the conditions of Bm and a frequency of 50 mT-100 kHz, the core loss is 50 to 300 kW / m 3 A resin composite sheet, characterized in that

6. A product made of the nanocrystalline soft magnetic metal flaky powder according to any one of claims 1 to 3 and a resin, and molded to an outer diameter of 12.8 mm, an inner diameter of 7.5 mm, and a thickness of 5 mm, is used, and the core loss measured under the conditions of Bm and frequency of 50 mT-100 kHz is 100 to 600 kW / m 3 A resin composite composition for molding, characterized in that:

Citation Information

Patent Citations

  • Flat nano-crystal soft magnetic powder excellent in noise inhibiting effect, and its production

    JP1999269509A

  • Soft magnetic resin composition, its manufacturing method and molded body

    JP2003209010A

  • Soft magnetic powder for noise suppression, production method therefor and noise suppression sheet using the same

    JP2005281783A

  • Flame-retardant noise suppressing sheet

    JP2009059753A

  • Soft magnetic alloy and magnetic part

    JP2016094652A