How to make an inductor
The blasting method for forming recesses and vias in inductors minimizes molten and solidified material, ensuring stable electrical connections and improved workability in inductor manufacturing.
Patent Information
- Application Number
- JP2020126343
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-07-27
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2040-07-27
AI Technical Summary
The formation of vias in inductors using conventional methods results in a large amount of molten and solidified magnetic particles, leading to instability in forming a plating layer, which hinders electrical connectivity and deteriorates the conductive wire.
A method involving a blasting process to form recesses in the magnetic layer, followed by precise abrasive particle injection to create vias, ensuring minimal molten and solidified material, and subsequent plating to stabilize the conductive connection.
The method allows for the production of inductors with improved workability and stable electrical connections, reducing the risk of conductive wire deterioration and enabling precise via formation.
Smart Images

Figure 0007565721000003 
Figure 0007565721000004 
Figure 0007565721000005
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for manufacturing an inductor. [Background technology]
[0002] Conventionally, inductors have been known that include wiring and a magnetic layer that covers the wiring (see, for example, Patent Document 1 below). The magnetic layer in Patent Document 1 contains magnetic particles. The inductor in Patent Document 1 further includes a slit. The slit is formed in the magnetic layer between two wirings. The slit is formed by a laser. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2019-186365 A Summary of the Invention [Problem to be solved by the invention]
[0004] However, in order to electrically connect the wiring to an external device, a via may be formed in the inductor and a plating layer may be formed inside the via The via penetrates from the surface of the inductor toward the wiring.
[0005] However, when a via is formed by the method of Patent Document 1, a large amount of molten and solidified magnetic particles remains on the inner circumferential surface of the via due to irradiation of the magnetic layer with a laser. This causes a problem in that a plating layer cannot be stably formed inside the via due to the large amount of molten and solidified material.
[0006] The present invention produces inductors with reduced melt solidification. [Means for solving the problem]
[0007] The present invention (1) includes a method for manufacturing an inductor, comprising: a first step of producing a magnetic laminate including wiring; and a magnetic layer having the wiring embedded therein and containing magnetic particles, the magnetic layer having a first main surface spaced apart on one side of the thickness direction from the wiring, and a second main surface spaced apart from the first main surface and located on the opposite side of the first main surface from the wiring; and a second step of, after the first step, forming a recess in the magnetic layer by a blasting method, the recess being recessed from the first main surface toward the second main surface.
[0008] In this method, the recesses are formed by blasting, so there is little melted and solidified magnetic particle in the recesses, making it possible to manufacture an inductor having recesses that are easy to process.
[0009] The present invention (2) includes the method for manufacturing an inductor described in (1), wherein the second step includes a third step of arranging a resist having an opening corresponding to the recess on the first main surface, and a fourth step of spraying abrasive particles toward the first main surface exposed through the opening.
[0010] In this method, the abrasive particles are jetted toward the first main surface exposed through the opening, so that recesses of the desired shape can be reliably formed.
[0011] The present invention (3) includes a method for manufacturing an inductor as described in (1) or (2), in which in the first step, a magnetic laminate is produced including wiring having a conductor and an insulating film arranged on the circumferential surface of the conductor, and in the second step, a via corresponding to the recess and having an inner circumferential surface extending from the first main surface to the insulating film is formed in the magnetic layer so that one surface in the thickness direction of the insulating film is exposed.
[0012] In this method, a via is formed corresponding to the recess, and by providing a conductive member in the via, the wiring and an external device can be electrically connected. Meanwhile, since the insulating film covers the conductor before providing the conductive member, deterioration and damage of the conductor can be suppressed.
[0013] The present invention (4) includes the method for manufacturing an inductor described in (3), in which one thickness-wise edge of the inner circumferential surface has a longest length D1 and a shortest length D2 in a planar direction perpendicular to the thickness direction, and the ratio (D1 / D2) of the longest length D1 to the shortest length D2 is 10 or less.
[0014] In this method, the ratio (D1 / D2) is small, at 10 or less, so that the conductive member can be formed stably.
[0015] The present invention (5) includes the method for manufacturing an inductor according to (3) or (4), further comprising the step of filling the vias with a processing stability layer.
[0016] In this method, the via is filled with the processing stability layer, so that the processing stability of the via can be improved.
[0017] The present invention (6) includes a method for manufacturing an inductor as described in (5), further comprising a step of forming a through hole penetrating the processing stability layer and the insulating film in a thickness direction so that one thickness-wise side of the conductor is exposed.
[0018] In this method, the through hole exposes one surface of the conductor in the thickness direction, so that the conductor can be electrically connected to an external device via the through hole.
[0019] Furthermore, even if a conductive member is provided so as to fill the through-holes, the process stabilizing layer can ensure insulation between the conductive member and the magnetic layer.
[0020] The present invention (7) includes the method for manufacturing an inductor according to (6), in which the through hole is formed by laser processing.
[0021] In this method, the through holes are formed by laser processing, so that the through holes can be formed with high precision.
[0022] The present invention (8) includes the method for manufacturing an inductor described in (1) or (2), in which in the first step, the magnetic laminate is produced having a plurality of the wirings arranged at intervals in a direction perpendicular to the extension direction of the wirings and the thickness direction, and in the second step, a slit corresponding to the recess is formed between the plurality of the wirings.
[0023] In this method, the slits are formed between a plurality of wirings, so that crosstalk between the plurality of wirings can be suppressed. Effect of the Invention
[0024] The manufacturing method of the present invention can manufacture an inductor with a small amount of melted and solidified material. [Brief description of the drawings]
[0025] [Figure 1] 1A to 1E are cross-sectional views for explaining a first embodiment of a method for manufacturing an inductor of the present invention. FIG. 1A shows a step of preparing a magnetic laminate. FIG. 1B shows a step of forming a resist. FIG. 1C shows a step of forming a via. FIG. 1D shows a step of removing the resist. FIG. 1E shows a mode of use in which a conductive member is formed in a via. [Diagram 2] Figures 2A and 2B are plan views corresponding to Figures 1A and 1D, respectively. Figure 2A shows a magnetic laminate. Figure 2B shows an inductor. [Diagram 3] FIG. 3 is an enlarged view of the inductor shown in FIG. 1D. [Figure 4] FIG. 4 is an image-processed view of an SEM photograph of the inductor of Example 1 corresponding to FIG. [Diagram 5] FIG. 5 is an enlarged cross-sectional view of the inductor shown in FIG. 1D taken along a first direction. [Figure 6] FIG. 6 is an image-processed view of an SEM photograph of the inductor of Comparative Example 1. In FIG. [Figure 7] FIG. 7 shows a modification of the inductor shown in FIG. 2B. [Figure 8] FIG. 8 shows a modification of the inductor shown in FIG. 2B. [Figure 9] FIG. 9 shows a modification of the inductor shown in FIG. 1D. [Figure 10] Figures 10A and 10B correspond to Figures 1D and 1E, respectively. Figure 10A shows a modified example of the inductor. Figure 10B shows an inductor further including a conductive member. [Figure 11] FIG. 11 shows a modification of the inductor shown in FIG. 1D. [Figure 12] FIG. 12 shows a modification of the inductor shown in FIG. 1D. [Figure 13] FIG. 13 is a cross-sectional view of an inductor obtained by the second embodiment of the inductor manufacturing method of the present invention. [Figure 14] FIG. 14 is a cross-sectional view of an inductor obtained by the third embodiment of the inductor manufacturing method of the present invention. [Figure 15] 15A and 15B show an inductor obtained by a fourth embodiment of the inductor manufacturing method of the present invention, where Fig. 15A is a plan view and Fig. 15B is a cross-sectional view. [Figure 16] Fig. 16A to Fig. 16F are cross-sectional views of the fifth embodiment. Fig. 16A shows a process of preparing a magnetic laminate. Fig. 16B shows a process of forming a processing stability layer and a second processing stability layer. Fig. 16C shows a process of forming a via and a slit. Fig. 16D shows a process of forming a new processing stability layer. Fig. 16E shows a process of forming a through hole. Fig. 16F shows a usage mode in which a conductive member is formed in a through hole. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0026] A first embodiment of a method for manufacturing an inductor according to the present invention will be described with reference to FIGS.
[0027] The manufacturing method of the inductor 1 includes a first step and a second step. In this manufacturing method, the first step and the second step are carried out in this order.
[0028] 1A and 2A, in the first step, a magnetic laminate 20 is produced. The magnetic laminate 20 is an inductor 1 in which a via 10 (described later, see FIGS. 1C and 2B) has not yet been formed.
[0029] The magnetic laminate 20 has a predetermined thickness and is generally plate-shaped. The magnetic laminate 20 is long in a first direction perpendicular to the thickness direction. The magnetic laminate 20 has a rectangular shape in a plan view. As shown in FIG. 1A , the magnetic laminate 20 has one side 11 and the other side 12. The one side 11 is disposed opposite the other side 12 on one side in the thickness direction with a gap therebetween. The magnetic laminate 20 has wiring 2 and a magnetic layer 3.
[0030] As shown in FIG. 2A, the wiring 2 extends along the first direction. The shape, dimensions, configuration, material, and formulation (filling rate, content ratio, etc.) of the wiring 2 are described in, for example, JP 2019-220618 A. Preferably, as shown in FIG. 1A, the wiring 2 has a substantially circular shape in a cross section along the thickness direction and the second direction. The second direction is perpendicular to the thickness direction and the first direction. The wiring 2 includes an outer peripheral surface 14 in the cross section. The wiring 2 preferably includes a conductor wire 4 and an insulating film 5 that covers the peripheral surface of the conductor wire 4.
[0031] The magnetic layer 3 has the same outer shape as the magnetic laminate 20 in plan view. The magnetic layer 3 has a sheet shape extending in the first direction. In addition, the magnetic layer 3 has the wiring 2 embedded therein in cross-sectional view. The material of the magnetic layer 3 is a magnetic composition containing a binder and magnetic particles. The magnetic particles are preferably soft magnetic particles from the viewpoint of increasing the inductance of the inductor 1. The magnetic composition and the method of forming the magnetic layer 3 are described in detail, for example, in JP-A-2019-165221 and JP-A-2019-165222. The magnetic layer 3 has a first main surface 6 as an example of a first main surface, a second main surface 7 as an example of a second main surface, and an outer surface 8.
[0032] 1A, the first main surface 6 forms one surface in the thickness direction of the magnetic layer 3. The first main surface 6 is also one surface 11 of the magnetic laminate 20. The first main surface 6 is disposed on one side in the thickness direction with a gap therebetween with respect to the wiring 2. The first main surface 6 includes a curved surface corresponding to the wiring 2.
[0033] The second main surface 7 forms the other surface in the thickness direction of the magnetic layer 3. The second main surface 7 is also the other surface 12 of the magnetic laminate 20. The second main surface 7 is spaced apart from the first main surface 6 on the other side in the thickness direction. The second main surface 7 is disposed on the opposite side of the first main surface 6 with respect to the wiring 2. The second main surface 7 includes a curved surface corresponding to the wiring 2.
[0034] 1A and 2A, the outer surfaces 8 are two side surfaces of the magnetic layer 3 that face each other at an interval in the second direction. The outer surfaces 8 connect both end edges of the first main surface 6 in the second direction to both end edges of the second main surface 7.
[0035] A method for producing the magnetic laminate 20 is described in detail in, for example, JP-A-2019-165221 and JP-A-2019-165222.
[0036] As shown in FIGS. 1B to 1D, in the second step, vias 10 as an example of recesses are formed in the magnetic layer 3. The second step is performed after the first step. A blasting method is used to form the vias 10. The blasting method includes a third step, a fourth step, and a fifth step.
[0037] As shown in FIG. 1B, in the third step, a resist 21 is placed on the first main surface 6. The resist 21 has an opening 22 corresponding to the via 10. The opening 22 penetrates the resist 21 in the thickness direction. The resist 21 is made of a material that is not easily damaged by collision with abrasive particles, which will be described next. The material of the resist 21 is not particularly limited. A commercially available product can be used as the resist 21, and for example, a commercially available "dry film resist for sandblasting" can also be used. The resist 21 is formed through a photolithography process.
[0038] 1C, in the fourth step, abrasive particles are jetted toward the first main surface 6 exposed through the opening 22. An abrasive particle jetting device (not shown) is used to jet the abrasive particles.
[0039] Although not shown, the abrasive particle injection device includes, for example, an introduction section, an extension section, a flow straightening section, a collection section, and an injection nozzle, arranged in this order in the direction of the flow of the abrasive particles. The introduction section is connected to an abrasive particle tank and a gas tank. The extension section diffuses the abrasive particles inside. The flow straightening section straightens the flow of the abrasive particles. The collection section increases the flow pressure while gathering the abrasive particles. The injection nozzle includes multiple nozzles. Each of the multiple nozzles is a substantially circular hole. The injection nozzle injects the abrasive particles from the multiple nozzles while keeping the abrasive particles uniform. The configuration and use conditions of the abrasive particle injection device are described, for example, in JP 2015-199131 A. A commercially available product can be used as the abrasive particle injection device.
[0040] Specifically, examples of the material of the abrasive grain include alumina, glass beads, silicon carbide, silicon nitride, zirconia, and stainless steel. The nozzle diameter is, for example, 0.1 μm or more, preferably 0.5 μm or more, and, for example, 10000 μm or less, preferably 5000 μm or less. The median diameter of the abrasive grain is, for example, 0.1 μm or more, preferably 0.5 μm or more, and, for example, 1000 μm or less, preferably 100 μm or less. The ejection pressure of the abrasive grain is, for example, 0.01 MPa or more, preferably 0.05 MPa or more, and, for example, 10 MPa or less, preferably 5 MPa or less.
[0041] In a fourth step, the first main surface 6 exposed from the opening 22 is ground, and a via 10 is formed in the magnetic layer 3 .
[0042] 1D, in the fifth step, the resist 21 is removed. Specifically, the resist 21 is peeled off from the first main surface 6.
[0043] As a result, an inductor 1 including the wiring 2, the magnetic layer 3, and the via 10 is obtained.
[0044] As shown in FIG. 2B, the vias 10 are provided in the magnetic layer 3 corresponding to both ends of the wiring 2 in the first direction. Each of the two vias 10 has a substantially circular shape in a plan view. As shown in FIGS. 3 to 5, the vias 10 penetrate from one surface 11 of the inductor 1 toward the wiring 2. The vias 10 expose one thickness direction surface 34 of the insulating film 5. The one thickness direction surface 34 is a portion of the outer peripheral surface 14 of the wiring 2 that is located on one thickness direction side from the center. The via 10 has an inner peripheral surface 9 and a bottom surface 17.
[0045] The inner circumferential surface 9 faces the inside of the via 10 in the magnetic layer 3. As shown in FIG. 2B, the inner circumferential surface 9 has an endless shape in plan view (same meaning as when viewed from the thickness direction, the same applies below). Specifically, the inner circumferential surface 9 has a substantially annular shape in plan view. As shown in FIGS. 3 to 5, the inner circumferential surface 9 has a tapered surface 27 in which the opening cross-sectional area of the via 10 increases toward the one surface 11. Specifically, the inner circumferential surface 9 is made of the tapered surface 27. The inner circumferential surface 9 has a step 13. The number of steps 13 per one via 10 is, for example, one.
[0046] The bottom surface 17 faces the via 10. The bottom surface 17 is a part of the outer peripheral surface 14 of the wiring 2. The bottom surface 17 is also one thickness direction surface 34 of the wiring 2. The bottom surface 17 is continuous with an edge (a second edge E2 described later) on the other thickness direction side of the inner peripheral surface 9. As shown in FIG. 2B, the bottom surface 17 has a substantially circular shape in a plan view. As shown in FIGS. 3 and 4, the bottom surface 17 has a substantially arc shape in a cross section along the second direction. As shown in FIG. 5, the bottom surface 17 has a flat shape in a cross section along the first direction. The maximum height roughness Rz of the bottom surface 17 is, for example, 10 μm or less, preferably 1 μm or less, more preferably 0.1 μm or less, and for example, 0.000001 μm or more. In the one thickness direction surface 34, a portion covered by the magnetic layer 3 is a covering portion 18. The maximum height roughness Rz of the covering portion 18 is, for example, 10 μm or less, preferably 1 μm or less, more preferably 0.1 μm or less, and for example, 0.000001 μm or more. The ratio of the maximum height roughness Rz of the bottom surface 17 to the maximum height Rz of the covering portion 18 is, for example, less than 2, preferably 1.5 or less, more preferably 1.1 or less, and for example, 1 or more. If the ratio is below the above-mentioned upper limit, the bottom surface 17 of the via 10 is prevented from being excessively rough compared to the covering portion 18. Therefore, the conductive member 19 can be formed more reliably by the via 10.
[0047] The magnetic layer 3 may be a single layer or multiple layers. When the magnetic layer 3 is multiple layers, it includes, for example, a first layer 15 in which the wiring 2 is embedded, and two second layers 16. Each of the two second layers 16 is disposed on one surface and the other surface in the thickness direction of the first layer 15. The type and / or ratio of magnetic particles in the second layer 16 is different from those in the first layer 15.
[0048] In addition, in this inductor 1, the upper limit of the percentage of the molten and solidified material M is, for example, 10% or less, preferably 7.5%, more preferably 5%, even more preferably 2.5%, particularly preferably 1%, even more preferably 0.1%, or even more preferably 0.01%, and most preferably the percentage of the molten and solidified material M is 0%.
[0049] The percentage of the molten solidified material M is determined by the following method.
[0050] First, as shown in Figures 3 to 5, in a cross section across the via 10, a first point P1 and a second point P2 are defined, each located 50 μm apart on one side and the other side in the direction in which the first main surface 6 extends, based on a first edge E1 on one side of the thickness direction of the inner surface 9, and a third point P3 and a fourth point P4 are defined, each located 50 μm apart on one side and the other side in the direction in which the first main surface 6 extends, based on a second edge E2 on the other side of the thickness direction of the inner surface 9.
[0051] The cross section across the via 10 may be a cross section along the second direction as shown in FIGS. 3 and 4, or a cross section along the first direction as shown in FIG.
[0052] The first edge E1 is an angle formed by the inner circumferential surface 9 and the first main surface 6. In a cross section along the second direction, the direction in which the first main surface 6 extends is the tangent direction at the first edge E1 if the first main surface 6 is a curved surface as shown in Figures 3 and 4. On the other hand, in a cross section along the first direction, the direction in which the first main surface 6 extends is the direction along the first main surface 6, that is, the first direction, if the first main surface 6 is a flat surface as shown in Figure 5.
[0053] The second edge E2 is an angle formed by the inner circumferential surface 9 and the outer circumferential surface 14 of the wiring 2. The direction serving as a reference when determining the third point P3 and the fourth point P4 with respect to the second edge E2 is the same as the direction serving as a reference when determining the first point P1 and the second point P2. Therefore, the first line segment L1 connecting the first point P1 and the second point P2 and the second line segment L2 connecting the third point P3 and the fourth point P4 are parallel to each other. This forms a quadrangle with the first point P1, the second point P2, the third point P3, and the fourth point P4 as vertices. The quadrangle is a quadrilateral with two sides (the first line segment L1 and the second line segment L2) parallel to each other, that is, a parallelogram.
[0054] Next, the area S0 of the quadrilateral is obtained.
[0055] Next, the area S1 of the molten and solidified material M located inside the rectangle is obtained. The molten and solidified material M is a solid material formed by melting, agglomerating, and solidifying magnetic particles as shown in FIG. 6 when forming the via 10 by the manufacturing method described later. For example, the molten and solidified material M can be defined as follows. The periphery of 10 unmelted magnetic particles is obtained by observing a cross-sectional SEM image, and the average value is calculated. The area of 10 unmelted magnetic particles is also obtained by observing a cross-sectional SEM image, and the average value is calculated. An object having a periphery and area larger than the average periphery and area of the magnetic particles described above, respectively, is a molten and solidified material.
[0056] Then, the percentage (S1 / S0 x 100) of the area S1 of the molten solidified material to the area S0 of the rectangle is calculated.
[0057] If the percentage of the molten solidified material M is equal to or less than the above upper limit, a conductive member 19, which will be described later, can be stably formed inside the via 10, as shown in FIG. 1E.
[0058] Next, the use of inductor 1 will be described.
[0059] 1E, the conductive member 19 is formed in the via 10 by, for example, plating, specifically, electroless plating and / or electrolytic plating. Preferably, the conductive member 19 is formed by electroless plating and electrolytic plating. In this case, a desmear (cleaning and roughening) step is performed, then electroless plating is performed, followed by disposing, exposing and developing a photosensitive dry film resist to form a plating resist, then electrolytic plating is performed using the plating resist, and then the plating resist is removed.
[0060] Before forming the conductive member 19, the insulating film 5 in the via 10 is peeled off. The insulating film 5 can be peeled off by various methods, for example, by laser processing or blasting. Furthermore, a seed layer (not shown) is formed before electrolytic plating. The conductive member 19 is formed by deposition from the bottom surface 17 of the via 10. The conductive member 19 is deposited on one side in the thickness direction along the inner circumferential surface 9. The conductive member 19 is also formed on one surface 11 around the via 10. Examples of materials for the conductive member 19 include conductors such as copper.
[0061] [Effects of the first embodiment]
[0062] In this method, since the vias 10 are formed by a blasting method, the amount of molten and solidified material M of the magnetic particles is small in the vias 10. Specifically, the percentage of the molten and solidified material M is, for example, 10% or less. Therefore, the inductor 1 having the vias 10 with excellent workability can be manufactured.
[0063] In contrast, when the vias 10 are formed by a laser, a large amount of molten and solidified material M of the magnetic particles is produced, as shown in Fig. 6. Specifically, the percentage of the molten and solidified material M exceeds, for example, 10%. As a result, it is not possible to manufacture an inductor 1 having a via 10 with excellent workability.
[0064] Furthermore, in the second step of this method, abrasive particles are blasted toward the first main surface 6 exposed through the openings 22 of the resist 21, so that the vias 10 having the desired shape can be formed with high precision.
[0065] Furthermore, in this method, by providing a conductive member 19 in the via 10 as shown in Fig. 1E, the wiring 2 can be electrically connected to an external device. Meanwhile, in the inductor 1 before providing the conductive member 19 in the via 10 as shown in Fig. 1D, the insulating film 5 covers the conductive wire 4, so that deterioration and damage of the conductive wire 4 can be suppressed.
[0066] [Modification of the first embodiment]
[0067] In the modified example, the same components and steps as those in the first embodiment are denoted by the same reference numerals, and detailed description thereof will be omitted. In addition, the modified example can achieve the same effects as those in the first embodiment, unless otherwise specified. Furthermore, the first embodiment and the modified example can be appropriately combined.
[0068] In the first embodiment, the inner circumferential surface 9 has an endless shape in a plan view, but as shown in Fig. 7, the inner circumferential surface 9 has an ended shape. In this modification, the slit 40 as an example of a recess has two inner circumferential surfaces 9.
[0069] The slit 40 extends along the wiring 2 in a planar view. The slit 40 overlaps with the wiring 2 in a planar view. Specifically, the slit 40 is included in the wiring 2 in a planar view. The slit 40 has two inner circumferential surfaces 9. The two inner circumferential surfaces 9 face each other in the second direction. Each of the two inner circumferential surfaces 9 has a straight shape along the first direction in a planar view. Each of the two inner circumferential surfaces 9 has an end shape in a planar view, specifically, has both ends 29 in the first direction.
[0070] Therefore, it is proposed to form the slit 40 having an inner peripheral surface 9 having an end shape using a dicing saw (not shown). The dicing saw includes, for example, a blade and a moving device. The blade is disk-shaped. The blade is rotatable. The moving device is capable of moving the blade in the thickness direction and the first direction. To form the slit 40 with the dicing saw, the blade is moved to one side in the thickness direction while being in contact with one side of the first main surface 6 in the thickness direction until the peripheral surface of the blade comes into contact with the insulating film 5. Then, the blade is moved along the first direction. As a result, the slit 40 having two inner peripheral surfaces 9 is formed.
[0071] However, in this tentative plan, the rotating blade deforms the magnetic particles in the magnetic layer 3. For example, when the magnetic particles come into contact with the rotating blade along the thickness direction and are caught in the blade, they may be torn (or stretched) in the thickness direction and may further recombine, eventually producing a molten solidified material M.
[0072] On the other hand, in this method, a blasting method using abrasive particles is adopted instead of a dicing saw, so that the generation of the above-mentioned melt-solidified material M is suppressed.
[0073] The shape of the via 10 is not limited to a substantially circular shape in plan view. As shown in FIG. 8, for example, the via 10 has a substantially rectangular shape in plan view. In this modification, the via 10 is long in the first direction in plan view. The via 10 has a maximum length D1 and a minimum length D2 in plan view. In this modification, the maximum length D1 is the distance between two opposing vertices in the rectangular shape of the via 10. The minimum length D2 is the length of the via 10 in the second direction. The upper limit of the ratio (D1 / D2) of the maximum length D1 to the minimum length D2 is, for example, 10, preferably 5, more preferably 3, and even more preferably 2. The lower limit of the ratio is, for example, 1.1, preferably 1.2. In the circular shape of the via 10 shown in FIG. 2B, the maximum length D1 and the minimum length D2 are the same. If the ratio (D1 / D2) is small, such as 10 or less, the conductive member 19 can be stably formed in the via 10.
[0074] As shown in FIG. 9, the inner circumferential surface 9 may be a flat surface in a cross-sectional view.
[0075] In another modified example, as shown in FIG. 10A, the inner circumferential surface 9 has a tapered surface 27 and a second tapered surface .
[0076] The opening cross-sectional area of the via 10 increases with increasing distance from the tapered surface 27 to the one surface 11. The tapered surface 27 extends from the second edge E2 toward one side in the thickness direction.
[0077] On the other hand, the opening cross-sectional area of the via 10 becomes smaller as the second tapered surface 28 approaches the one surface 11. The second tapered surface 28 reaches from the first end edge E1 to one edge in the thickness direction of the tapered surface 27. On this inner circumferential surface 9, the tapered surface 27 and the second tapered surface 28 are arranged in order toward one thickness direction side.
[0078] In the second direction, the distance between one thickness direction edges of the two second tapered surfaces 28 is the distance between the two first edges E1. In the second direction, the distance between the two first edges E1 is shorter than the distance between the other thickness direction edges E3 of the two second tapered surfaces 28. The ratio of the distance between the two other edges E3 to the distance between the two first edges E1 is, for example, 1.1 or more, preferably 1.2 or more, more preferably 1.5 or less, and is, for example, 3 or less.
[0079] In the second direction, the distance between the other thickness direction edges of the two tapered surfaces 27 is the distance between the two E2. In the second direction, the distance between the two second edges E2 is shorter than the distance between the two other thickness direction edges E3. The ratio of the distance between the two other edges E3 to the distance between the two second edges E2 is, for example, 1.1 or more, preferably 1.2 or more, more preferably 1.5 or less, and is, for example, 3 or less.
[0080] To form the via 10, for example, the opening 22 of the resist 21 shown in Fig. 1B is narrowed. Specifically, the diameter of the opening 22 is, for example, 300 µm or less, preferably 200 µm or less.
[0081] Then, in the fourth step, the abrasive particles pass through the narrow opening 22 and collide with the first main surface 6 of the magnetic layer 3 to grind the magnetic layer 3, but the abrasive particles tend to remain on the other side of the periphery of the opening 22 in the thickness direction of the magnetic layer 3. These abrasive particles flow back upstream in the injection direction. At this time, the abrasive particles form the inner circumferential surface 9 on a substantially arc-shaped trajectory. Therefore, the abrasive particles form the inner circumferential surface 9 having the second tapered surface 28 and the tapered surface 27.
[0082] As shown in FIG. 10B, when the conductive member 19 is provided in the via 10, the conductive member 19 comes into contact with the tapered surface 27 and the second tapered surface .
[0083] In this inductor 1, the conductive member 19 can be prevented from falling off from the via 10 due to the anchor effect.
[0084] As shown in FIG. 11, the inner circumferential surface 9 may not include the tapered surface 27 and may include only the second tapered surface .
[0085] The shape of the wiring 2 is not limited. As shown in Fig. 12, the shape of the wiring 2 may be a substantially rectangular cross section. The other surface in the thickness direction of the wiring 2 contacts the insulating layer 23. The insulating layer 23 extends in the second direction. Examples of materials for the insulating layer 23 include insulating resins such as polyimide.
[0086] Moreover, the inductor 1 of this modified example includes a plurality of (specifically, two) wirings 2. The plurality of wirings 2 are adjacent to each other with a gap therebetween. The plurality of wirings 2 are parallel to each other.
[0087] Although not shown, the blasting method of the second step can also be performed without using the resist 21. Preferably, the resist 21 is used. Specifically, abrasive particles are sprayed onto the first main surface 6 exposed from the opening 22 of the resist 21. This ensures that the via 10 having a shape corresponding to the opening 22 is formed.
[0088] Although not shown, the vias 10 can be provided on both the one surface 11 and the other surface 12 .
[0089] Although not shown, the via 10 can also be provided in the magnetic layer 3 only at one end of the wiring 2 in the first direction.
[0090] [Second embodiment]
[0091] In the second embodiment, the same components and steps as those in the first embodiment are given the same reference numerals, and detailed description thereof will be omitted. In addition, the second embodiment can achieve the same effects as those in the first embodiment, except as otherwise specified. Furthermore, the first embodiment and the second embodiment can be appropriately combined.
[0092] 13, in addition to the first and second steps of the first embodiment, the second embodiment further includes a step of filling the vias 10 with a process stabilizing layer 24. The second embodiment also includes a step of arranging a second process stabilizing layer 25 on the second main surface 7. This second embodiment includes a step of providing the process stabilizing layer 24 and the second process stabilizing layer 25 on the inductor 1. This step is performed after the second step.
[0093] To provide the inductor 1 with the process stabilizing layer 24 and the second process stabilizing layer 25, two process stabilizing sheets 26 are prepared as shown by the imaginary lines in FIG. 13. The material of each of the two process stabilizing sheets 26 includes a thermosetting resin composition. The thermosetting resin composition includes a thermosetting resin as an essential component. The thermosetting resin includes a base agent, a curing agent, and a curing accelerator.
[0094] Examples of the base resin include epoxy resins and silicone resins, and preferably epoxy resins. Examples of the epoxy resin include bifunctional epoxy resins such as bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol S type epoxy resins, modified bisphenol A type epoxy resins, modified bisphenol F type epoxy resins, modified bisphenol S type epoxy resins, and biphenyl type epoxy resins, and polyfunctional epoxy resins having three or more functional groups such as phenol novolac type epoxy resins, cresol novolac type epoxy resins, trishydroxyphenylmethane type epoxy resins, tetraphenylolethane type epoxy resins, and dicyclopentadiene type epoxy resins. These epoxy resins can be used alone or in combination of two or more kinds. Preferably, bifunctional epoxy resins are used, and more preferably, bisphenol A type epoxy resins are used. The lower limit of the epoxy equivalent of the epoxy resin is, for example, 10 g / eq., and the upper limit is, for example, 1,000 g / eq.
[0095] As the curing agent, if the main agent is an epoxy resin, phenol resin, isocyanate resin, etc. can be mentioned. As the phenol resin, for example, phenol novolac resin, cresol novolac resin, phenol aralkyl resin, phenol biphenylene resin, dicyclopentadiene type phenol resin, resol resin, etc. can be mentioned. These can be used alone or in combination of two or more. As the phenol resin, preferably, phenol novolac resin, phenol biphenylene resin can be mentioned. If the main agent is an epoxy resin and the curing agent is a phenol resin, the lower limit of the total of hydroxyl groups in the phenol resin relative to 1 equivalent of epoxy groups in the epoxy resin is, for example, 0.7 equivalents, preferably 0.9 equivalents, and the upper limit is, for example, 1.5 equivalents, preferably 1.2 equivalents. Specifically, the lower limit of the number of parts by mass of the curing agent is, for example, 1 part by mass, or, for example, 50 parts by mass, relative to 100 parts by mass of the main agent.
[0096] The curing accelerator is a catalyst (thermosetting catalyst) (preferably an epoxy resin curing accelerator) that accelerates the curing of the base agent, and examples thereof include organic phosphorus compounds, such as imidazole compounds such as 2-phenyl-4-methyl-5-hydroxymethylimidazole (2P4MHZ). The lower limit of the number of parts by mass of the curing accelerator is, for example, 0.05 parts by mass, and the upper limit is, for example, 5 parts by mass, relative to 100 parts by mass of the base agent.
[0097] Furthermore, the thermosetting resin composition may contain, for example, particles as an optional component. The particles are dispersed in the thermosetting resin. The particles are, for example, at least one type selected from the group consisting of first particles and second particles.
[0098] The first particles have, for example, a substantially spherical shape. The lower limit of the median diameter of the first particles is, for example, 1 μm, preferably 5 μm, and the upper limit of the median diameter of the first particles is, for example, 250 μm, preferably 200 μm. The median diameter of the first particles is determined by a laser diffraction particle size distribution measuring device. The median diameter of the first particles can also be determined, for example, by binarization processing based on cross-sectional observation.
[0099] The material of the first particles is not particularly limited. Examples of the material of the first particles include metals, inorganic compounds, and organic compounds, and in order to increase the thermal expansion coefficient, metals and inorganic compounds are preferable.
[0100] The metal is contained in the thermosetting resin composition when the processing stabilizing layer 24 is made to function as an inductance improving layer. Examples of the metal include the magnetic materials exemplified in the magnetic layer 3, preferably an organic iron compound containing iron as the first metal element, and more preferably carbonyl iron.
[0101] The inorganic compound is contained in the thermosetting resin composition when the processing stabilizing layer 24 functions as a thermal expansion coefficient suppressing layer. Examples of the inorganic compound include inorganic fillers, specifically, silica, alumina, and the like, and preferably, silica.
[0102] Specifically, the first particles are preferably spherical silica, and are preferably spherical carbonyl iron.
[0103] The second particles have, for example, a substantially flat shape. The substantially flat shape includes a substantially plate shape.
[0104] The lower limit of the flattening ratio (flatness) of the second particles is, for example, 8, or preferably 15, and the upper limit is, for example, 500, or preferably 450. The flattening ratio of the second particles is calculated by the same method as the flattening ratio of the magnetic particles in the magnetic layer 3 described above.
[0105] The lower limit of the median diameter of the second particles is, for example, 1 μm, preferably 5 μm, and the upper limit of the median diameter of the second particles is, for example, 250 μm, preferably 200 μm. The median diameter of the second particles is determined in the same manner as that of the first particles.
[0106] The lower limit of the average thickness of the second particles is, for example, 0.1 μm, preferably 0.2 μm, and the upper limit is, for example, 3.0 μm, preferably 2.5 μm.
[0107] The material of the second particles is, for example, an inorganic compound. Examples of the inorganic compound include thermally conductive compounds such as boron nitride. Therefore, the inorganic compound is preferably included in the thermosetting resin composition when the processing stabilizing layer 24 functions as a thermal conductivity improving layer.
[0108] Specifically, the second particles are preferably flat-shaped boron nitride particles.
[0109] The thermosetting resin composition may contain a single type of the first particles and a single type of the second particles, or may contain both of them.
[0110] The lower limit of the number of parts by mass of the particles (first particles and / or second particles) relative to 100 parts by mass of the thermosetting resin is, for example, 10 parts by mass, preferably 50 parts by mass, and the upper limit is, for example, 2,000 parts by mass, preferably 1,500 parts by mass. The lower limit of the content ratio of the particles in the cured product is, for example, 10% by mass, and the upper limit is, for example, 90% by mass. When both the first particles and the second particles are contained in the thermosetting resin composition, the lower limit of the number of parts by mass of the second particles relative to 100 parts by mass of the first particles is, for example, 30 parts by mass, and the upper limit is, for example, 300 parts by mass.
[0111] Since particles are an optional component in a thermosetting resin composition, the thermosetting resin composition does not necessarily need to contain particles.
[0112] On the other hand, the material of each of the two processing stabilizing sheets 26 may further contain a thermoplastic resin. The lower limit of the number of parts by mass of the thermoplastic resin relative to 100 parts by mass of the thermosetting resin is, for example, 1 part by mass, and the upper limit is, for example, 100 parts by mass.
[0113] Next, the two process stabilizing sheets 26 and the inductor 1 are pressed from both sides in the thickness direction. After that, they are heated to bring the two process stabilizing sheets 26 to the C stage. As a result, the process stabilizing layer 24 and the second process stabilizing layer 25 are provided on the inductor 1.
[0114] The process stabilizing layer 24 is disposed on the first main surface 6 of the magnetic layer 3, the inner peripheral surface 9 of the via 10, and one surface 34 in the thickness direction of the insulating film 5. That is, at least a part of the process stabilizing layer 24 is filled in the via 10. The process stabilizing layer 24 improves the surface processability of the first main surface 6 of the magnetic layer 3 and the surface processability of the inner peripheral surface 9 of the via 10 and the via 10. Furthermore, the process stabilizing layer 24 is also an insulating layer that can ensure insulation between the conductive member 19 and the magnetic layer 3 when the conductive member 19 is disposed in the through hole 30 described later (see FIG. 14 and the third embodiment). Furthermore, the process stabilizing layer 24 is also a corrosion suppressing layer that suppresses corrosion of the magnetic particles in the magnetic layer 3 in the desmear process. The lower limit of the thickness of the process stabilizing layer 24 is, for example, 1 μm, preferably 10 μm, and the upper limit is, for example, 1,000 μm, preferably 100 μm. The lower limit of the ratio of the thickness of the process stabilizing layer 24 to the thickness of the inductor 1 is, for example, 0.001, preferably 0.005, more preferably 0.01, and the upper limit is, for example, 0.5, preferably 0.3, more preferably 0.1. The thickness of the process stabilizing layer 24 is the shortest length between the first main surface 6 and one surface of the process stabilizing layer 24 in the thickness direction.
[0115] The second process-stabilizing layer 25 is disposed on the second main surface 7 of the magnetic layer 3. That is, the second process-stabilizing layer 25 is disposed on the other surface 12 of the inductor 1. The second process-stabilizing layer 25 improves the surface processability of the other surface 12 of the inductor 1. The lower limit of the thickness of the second process-stabilizing layer 25 is, for example, 1 μm, preferably 10 μm, and the upper limit is, for example, 1,000 μm, preferably 100 μm. The lower limit of the ratio of the thickness of the second process-stabilizing layer 25 to the thickness of the inductor 1 is, for example, 0.001, preferably 0.005, more preferably 0.01, and the upper limit is, for example, 0.5, preferably 0.3, more preferably 0.1. The thickness of the second process-stabilizing layer 25 is the shortest length between the second main surface 7 and the other surface in the thickness direction of the second process-stabilizing layer 25.
[0116] [Effects of the second embodiment]
[0117] In the second embodiment, a part of the processing stabilizing layer 24 is filled in the via 10, thereby improving the processing stability of the via 10. Specifically, the stability during the next processing (third embodiment described later) of the via 10 can be improved.
[0118] [Third embodiment]
[0119] In the third embodiment, the same components and steps as those in the first and second embodiments are given the same reference numerals, and detailed description thereof will be omitted. Furthermore, the third embodiment can achieve the same effects as those in the first and second embodiments, unless otherwise specified. Furthermore, the first to third embodiments can be appropriately combined.
[0120] As shown in FIG. 14, the third embodiment further includes a step of forming a through hole 30 in addition to the steps of the second embodiment.
[0121] The through hole 30 penetrates the process stabilizing layer 24 and the insulating film 5 in the thickness direction. One thickness direction surface 34 of the conductive wire 4 is exposed from the through hole 30. For example, one thickness direction surface 34 of the conductive wire 4 is exposed from the process stabilizing layer 24 and a part of the insulating film 5.
[0122] The processing stabilizing layer 24 obtained in the third embodiment includes a first covering portion 31 and a second covering portion 32. The first covering portion 31 conforms to and covers the first main surface 6. The first covering portion 31 is located on one surface in the thickness direction of the first main surface 6. The second covering portion 32 conforms to and covers the inner circumferential surface 9. The second covering portion 32 overlaps with the inner circumferential surface 9 when projected in the second direction (or the first direction). The second covering portion 32 is aligned along the thickness direction. The other end surface in the thickness direction of the second covering portion 32 contacts the protruding end portion 35 of the insulating film 5 from one side in the thickness direction. The other end surface in the thickness direction of the second covering portion 32 is a surface of the second covering portion 32 located on the opposite side of the first covering portion 31. The protruding end portion 35 is a part of the insulating film 5. The protruding end portion 35 has a substantially annular shape in a plan view. The annular shape of the protruding end portion 35 is not depicted in FIG. 14. The protruding end portion 35 exposes, at its inner side, a part of one thickness direction surface 34 of the conductive wire 4. The inner surface of the protruding end portion 35 and the inner surface of the second covering portion 32 are flush with each other.
[0123] As a result, the protruding end 35 of the insulating film 5 and the second covering portion 32 of the process stabilizing layer 24 expose one thickness direction surface 34 of the conductive wire 4 toward one thickness direction side.
[0124] The through hole 30 is defined by the second covering portion 32 of the processing stabilizing layer 24, the protruding end portion 35 of the insulating film 5, and one surface 34 of the conductive wire 4 in the thickness direction.
[0125] To form the through holes 30, the processing stabilizing layer 24 of the second embodiment is, for example, perforated. Examples of perforation methods include laser processing, drilling, and blasting, and preferably include laser processing and drilling, and more preferably include laser processing. Laser processing can form the through holes 30 in the processing stabilizing layer 24 with high precision. On the other hand, the blasting method may not be able to cut the processing stabilizing layer 24 quickly, and may not be able to form the through holes 30 efficiently.
[0126] [Effects of the third embodiment]
[0127] In the third embodiment, the through hole 30 exposes one thickness direction surface 34 of the conductor 4, so that by arranging a conductive member 19 shown by an imaginary line in the through hole 30, the conductor 4 can be electrically connected to an external device.
[0128] In this method, if the through-holes 30 are formed by laser processing, the through-holes 30 can be formed with high precision.
[0129] Furthermore, if the processing stabilizing layer 24 is an insulating layer, the processing stabilizing layer 24 can be interposed between the conductive member 19 and the magnetic layer 3, thereby improving the insulation between them.
[0130] [Fourth embodiment]
[0131] In the fourth embodiment, the same components and steps as those in the first to third embodiments are given the same reference numerals, and detailed description thereof will be omitted. Furthermore, the third embodiment can achieve the same effects as those in the first to third embodiments, unless otherwise specified. Furthermore, the first to fourth embodiments can be appropriately combined.
[0132] As shown in FIG. 15, the slits 40 may be arranged so as to be shifted from the wirings 2 in a plan view.
[0133] In plan view, the slit 40 penetrates in the thickness direction through the second layer 16 (the second layer 16A on one side) disposed on one side of the first layer 15 in the thickness direction. However, the slit 40 does not penetrate the first layer 15. The slit 40 has an inner peripheral surface 9 and a bottom surface 17. The inner peripheral surface 9 of the slit 40 is shifted to one side in the thickness direction of the wiring 2 when projected in the second direction. In cross-sectional view, the bottom surface 17 of the slit 40 is not common to the outer peripheral surface 14 of the wiring 2, but is spaced apart. Although not depicted in FIG. 15, in plan view, the slit 40 is parallel to the multiple wirings 2.
[0134] [Effects of the fourth embodiment]
[0135] According to the fourth embodiment, since the slits 40 are formed between the plurality of wirings 2, crosstalk between the plurality of wirings 2 can be suppressed.
[0136] [Modification of the fourth embodiment]
[0137] In the modified example, the same members and steps as those in the fourth embodiment are denoted by the same reference numerals, and detailed description thereof will be omitted. In addition, the modified example can achieve the same effects as those in the fourth embodiment, except as otherwise specified. Furthermore, the fourth embodiment and the modified example can be appropriately combined.
[0138] Although not shown, the slit 40 may overlap the wiring 2 when projected in the second direction.
[0139] Although not shown, the slits 40 may penetrate in the thickness direction of the magnetic layer 3. In this modification, the slits 40 have, for example, a perforated shape in a plan view.
[0140] [Fifth embodiment]
[0141] In the fifth embodiment, the same components and steps as those in the first to fourth embodiments are given the same reference numerals, and detailed description thereof will be omitted. Furthermore, the fourth embodiment can achieve the same effects as those in the first to fourth embodiments, unless otherwise specified. Furthermore, the first to fifth embodiments can be appropriately combined.
[0142] As shown in FIGS. 16A to 16F, a via 10, a through hole 30, and a slit 40 can also be formed.
[0143] 16A, in this method, first, a magnetic laminate 20 is produced. The magnetic laminate 20 includes a plurality of wirings 2.
[0144] Subsequently, as shown in FIG. 16B, a processing stabilizing layer 24 and a second processing stabilizing layer 25 are provided on the magnetic laminate 20.
[0145] The processing stabilizing layer 24 is disposed in the first layer 15 disposed on one side in the thickness direction of the magnetic layer 3. That is, the processing stabilizing layer 24 is disposed on the first main surface 6.
[0146] The second work-stabilizing layer 25 is disposed in the first layer 16 disposed on the other thickness-wise side of the magnetic layer 3. That is, the second work-stabilizing layer 25 is disposed on the second main surface .
[0147] 16C, the vias 10 and the slits 40 are formed by blasting. The vias 10 and the slits 40 are also formed in the process stability layer 24.
[0148] 16D, the vias 10 and the slits 40 are filled with the processing stabilizing layer 24. The material of the processing stabilizing layer 24 used in the vias 10 and the slits 40 and the material of the processing stabilizing layer 24 disposed on the first main surface 6 are, for example, the same.
[0149] 16E, through holes 30 are formed so as to expose the conductive wires 4. The through holes 30 are formed by, for example, laser processing or a blasting method.
[0150] 16F, conductive members 19 are formed in through holes 30. When conductive members 19 are formed by electroless plating and electrolytic plating, a desmear (cleaning and roughening) step is carried out in advance.
[0151] The inductor 1 has a plurality of wirings 2, a magnetic layer 3, a processing stability layer 24, a second processing stability layer 25, and a conductive member 19. The inductor 1 further has a through hole 30. The slit 40 is filled with the processing stability layer 24. The via 10 is filled with the conductive member 19.
[0152] [Effects of the Fifth Embodiment]
[0153] Even after the desmear process for cleaning and roughening the through-holes 30, the process stabilizing layer 24 can prevent the chemical solution used in the desmear process from contacting the magnetic layer 3. Therefore, deterioration in the function of the magnetic layer 3 caused by contact with the chemical solution can be suppressed.
[0154] Moreover, the inductor 1 can be manufactured, which includes the through hole 30 including the via 10, the process stabilizing layer 24 filled in the slit 40, and the second process stabilizing layer 25.
[0155] Furthermore, since the inductor 1 has the process stabilizing layer 24 disposed on the first principal surface 6 and the process stabilizing layer 25 disposed on the second principal surface 7, warping to one side or the other in the thickness direction can be suppressed. EXAMPLES
[0156] The present invention will be described in more detail below with reference to examples and comparative examples. The present invention is not limited to the examples and comparative examples. The specific numerical values of the blending ratio (content ratio), physical property values, parameters, etc. used in the following description can be replaced with the upper limit (a numerical value defined as "not more than" or "less than") or lower limit (a numerical value defined as "not less than" or "exceeding") of the corresponding blending ratio (content ratio), physical property values, parameters, etc. described in the above "Form for carrying out the invention".
[0157] Example 1 [Example corresponding to the first embodiment] As shown in Figures 1A and 2A, first, a magnetic laminate 20 was produced. Specifically, a plurality of wirings 2 with a radius of 115 μm were covered with a magnetic layer 3 consisting of a first magnetic sheet with a thickness of 100 μm and a second magnetic sheet with a thickness of 125 μm.
[0158] The first magnetic sheet contains 61.5% by volume of spherical magnetic powder, 9.6% by volume of cresol novolac epoxy resin (base material), 9.6% by volume of phenolic resin (hardener), 0.5% by volume of polyether phosphate ester (dispersant), 0.3% by volume of imidazole compound (hardener), and 18.5% by volume of thermoplastic resin (carboxyl group-containing acrylic acid ester copolymer). The second magnetic sheet contains 55% by volume of flat Fe-Si alloy magnetic particles, 11.0% by volume of cresol novolac epoxy resin (base material), 11.0% by volume of phenolic resin (hardener), 0.4% by volume of polyether phosphate ester (dispersant), 0.4% by volume of imidazole compound (hardener), and 21.2% by volume of thermoplastic resin (carboxyl group-containing acrylic acid ester copolymer).
[0159] 1B, a resist 21 was formed on the first main surface 6 of the insulating film 5. An opening 22 was formed in the resist 21 through a photolithography process. The opening 22 had a circular shape in a plan view. The diameter of the opening 22 was 250 μm.
[0160] 1C, vias 10 were formed by blasting. The inner peripheral surface 9 of via 10 has a tapered surface 27.
[0161] The conditions for the blasting method are described below.
[0162] Nozzle diameter: 2mm Abrasive material: Alumina Median diameter of abrasive particles: 14μm Injection speed: 0.4MPa
[0163] Subsequently, the resist 21 was peeled off from the first main surface 6, as shown in FIG. 1D.
[0164] In this way, the inductor 1 was manufactured.
[0165] Example 2 [Example corresponding to the second embodiment] As shown in FIG. 13, the inductor 1 of the first embodiment was provided with a process stabilizing layer 24 and a second process stabilizing layer 25. As shown in FIG.
[0166] Specifically, first, two processing stabilizing sheets 26 were prepared as shown by the imaginary lines in FIG. 13. The processing stabilizing sheet 26 was formed by applying and drying a varnish containing 935 parts by mass of spherical silica particles (first particles), 100 parts by mass of bisphenol A type epoxy resin (main agent of thermosetting resin), 106 parts by mass of phenol resin (hardening agent), 4 parts by mass of an imidazole compound (hardening accelerator), and 10 parts by mass of cyclohexene (solvent). The content of silica particles in the processing stabilizing sheet 26 was 55% by volume. The thickness of the processing stabilizing sheet 26 was 40 μm. The processing stabilizing sheet 26 was in the B stage.
[0167] The two process stabilizing sheets 26 and the inductor 1 were pressed from both sides in the thickness direction. After that, the process stabilizing sheets 26 were brought to the C stage.
[0168] Example 3 [Example corresponding to the third embodiment] As shown in FIG. 14, a through hole 30 was formed in the processing stabilizing layer 24 of Example 2.
[0169] Specifically, the through-holes 30 were formed in the process stabilizing layer 24 by laser processing.
[0170] Thereafter, a desmear process was carried out, and then, as shown in Fig. 1E, a seed layer (not shown) was formed in the through hole 30 by electroless copper plating, and then the conductive member 19 was formed by electrolytic copper plating. The conductive member 19 could be formed smoothly.
[0171] Example 4 Except for changing the diameter of the opening 22 to 100 μm, the processing was performed in the same manner as in Example 1. As shown in FIG.
[0172] Comparative Example 1 Except for changing the blasting method to laser processing, the treatment was the same as in Example 1. The conductor 4 was exposed by the laser processing. Furthermore, an attempt was made to form the conductive member 19 by electrolytic copper plating. However, the formation of the conductive member 19 was defective.
[0173] Example 5 [Example corresponding to the fourth embodiment] 15, the process was the same as in Example 1, except that slits 40 were formed instead of the vias 10 and the number of wirings 2 was changed to two. The slits 40 penetrated the first layer 15.
[0174] Comparative Example 2
[0175] The same treatment as in Example 5 was carried out, except that cutting using a dicing saw was used instead of the blasting method.
[0176] evaluation SEM observation, ratio of molten solidified material M, and formation of conductive material Cross-sectional SEM observation was carried out for each of the Examples to Comparative Examples. A processed SEM image along the second direction of Example 1 is shown in Fig. 4. A processed SEM image along the first direction of Comparative Example 1 is shown in Fig. 6.
[0177] Additionally, the percentage of the molten solidified material M was calculated. The results are shown in Tables 1 and 2.
[0178] In addition, the conductive member 19 on the bottom surface 17 and the inner peripheral surface 17 of the via 10 was observed from the cross-sectional SEM image, and the formation of the conductive member 19 was evaluated according to the following criteria.
[0179] [Good] The conductive member 19 was not formed via the molten and solidified material M. [Defective] The conductive member 19 was formed via the molten and solidified material M.
[0180] [Table 1]
[0181] [Table 2] [Explanation of symbols]
[0182] 1 Inductor 2 Wiring 3 magnetic layer 4 conductors 5. Insulating film 6 First main surface 7 Second main surface 9 Inner surface 10 Via (an example of a recess) 11 One side 20 Magnetic laminate 21 Resist 22 Opening 24 Processing stable layer 30 Through hole 34 One side 40 Slit (an example of a recess)
Claims
1. a first step of producing a magnetic laminate including a wiring, and a magnetic layer having the wiring embedded therein and containing magnetic particles, the magnetic layer having a first main surface disposed on one side of the wiring in a thickness direction and spaced apart from the wiring, and a second main surface disposed on the opposite side of the wiring and spaced apart from the first main surface; a second step of forming a recess in the magnetic layer by a blasting method, the recess being recessed from the first main surface toward the second main surface after the first step; Equipped with The second step comprises: a third step of placing a resist having an opening corresponding to the recess on the first main surface; and a fourth step of jetting abrasive particles toward the first main surface exposed through the opening. The median diameter of the abrasive particles is 100 μm or less, In the first step, the magnetic laminate is prepared, the magnetic laminate including a plurality of the wirings arranged at intervals in a first direction in which the wirings extend and in a second direction perpendicular to the thickness direction; In the second step, a slit corresponding to the recess is formed between the plurality of wirings, A method for manufacturing an inductor, characterized in that the entire inner surface of the slit, when projected in a second direction, is shifted to one side in the thickness direction relative to the wiring.
2. a first step of producing a magnetic laminate including a wiring, and a magnetic layer having the wiring embedded therein and containing magnetic particles, the magnetic layer having a first main surface disposed on one side of the wiring in a thickness direction and spaced apart from the wiring, and a second main surface disposed on the opposite side of the wiring and spaced apart from the first main surface; a second step of forming a recess in the magnetic layer by a blasting method, the recess being recessed from the first main surface toward the second main surface after the first step; Equipped with In the first step, a magnetic laminate including wiring is produced, the wiring including a conductor and an insulating film disposed on a peripheral surface of the conductor, A method for manufacturing an inductor, characterized in that in the second step, a via corresponding to the recess and having an inner surface extending from the first main surface to the insulating film is formed in the magnetic layer so that one thickness direction side of the insulating film is exposed.
3. The second step comprises: a third step of placing a resist having an opening corresponding to the recess on the first main surface; The method for manufacturing an inductor according to claim 2 , further comprising a fourth step of blasting abrasive particles toward the first main surface exposed through the opening.
4. The one edge in the thickness direction of the inner circumferential surface has a maximum length D1 and a minimum length D2 in a surface direction perpendicular to the thickness direction, 4. The method for manufacturing an inductor according to claim 2, wherein a ratio (D1 / D2) of the longest length D1 to the shortest length D2 is 10 or less.
5. The method for manufacturing an inductor according to claim 4 , further comprising the step of filling the vias with a process stability layer.
6. 6. The method for manufacturing an inductor according to claim 5, further comprising the step of forming a through hole penetrating said processing stability layer and said insulating film in a thickness direction such that one thickness direction surface of said conductor is exposed.
7. The method for manufacturing an inductor according to claim 6, wherein the through hole is formed by laser processing.
Citation Information
Patent Citations
JP1974022594A
Inductor and method of manufacturing the same
JP2002083732A
Method for manufacturing electronic component
JP2002134344A
Flat magnetic element
JP2003332163A
Magnetic induction element and manufacturing method thereof
JP2007214348A