Wiring Board
The wiring board's conductor layer, composed of copper crystallites with linear grain boundaries and surface features, addresses the issue of conductivity loss at high frequencies by increasing interfacial conductivity and adhesion, ensuring improved performance.
Patent Information
- Application Number
- JP2022578361
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-01-28
- Filing Date
- 2022-01-24
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2042-01-24
AI Technical Summary
Existing wiring boards experience a significant decrease in interfacial conductivity at high frequencies, which affects their performance in high-frequency applications.
The wiring board design includes a conductor layer made of a sintered body of copper crystallites with polygonal cross-sections, where adjacent crystallites are in contact along linear grain boundaries, and incorporates surface features like recesses and silica particles to enhance adhesion and conductivity.
The design significantly increases interfacial conductivity at high frequencies, reducing conductivity loss and improving adhesion between the conductor and insulating layers, thereby enhancing the board's performance across a wide frequency range.
Smart Images

Figure 0007566051000001 
Figure 0007566051000002 
Figure 0007566051000003
Abstract
Description
[Technical field]
[0001] The disclosed embodiments relate to a wiring substrate. [Background technology]
[0002] Conventionally, a wiring board having an insulating layer and a conductor layer mainly composed of copper has been known. Such a wiring board can be obtained, for example, by simultaneously firing a conductor layer material, which is made of copper powder and a metal oxide, and a glass ceramic as an insulating layer material. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2003-277852 A Summary of the Invention
[0004] The wiring board according to one aspect of the embodiment includes an insulating layer and a conductor layer laminated together. The insulating layer is made of glass ceramics. The conductor layer is a sintered body of a plurality of crystallites mainly composed of copper. The plurality of crystallites include polygonal crystallites including straight edges, and the straight edges are in contact with each other as grain boundaries. [Brief description of the drawings]
[0005] [Figure 1] FIG. 1 is a cross-sectional view showing an example of a wiring board according to an embodiment. [Diagram 2] FIG. 2 is an enlarged view of area A shown in FIG. [Diagram 3] FIG. 3 is an explanatory diagram showing a method for evaluating crystallites. [Figure 4] FIG. 4 is a diagram showing the evaluation results of a plurality of crystallites in the conductor layer. [Diagram 5] FIG. 5 is a diagram showing the relationship between frequency and interface conductivity in the wiring boards according to the examples and the reference example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0006] Hereinafter, embodiments of a wiring board disclosed in the present application will be described with reference to the accompanying drawings. Note that the present disclosure is not limited to the embodiments described below.
[0007] 1 is a cross-sectional view showing an example of a wiring board according to an embodiment of the present invention. As shown in FIG 1, a wiring board 1 according to the present embodiment has an insulating layer 20 and a conductor layer 10.
[0008] The insulating layer 20 is made of glass ceramics. The insulating layer 20 may have a first layer 21 and a second layer 22 that face each other with the conductor layer 10 sandwiched therebetween. The first layer 21 and the second layer 22 are positioned, for example, so as to sandwich both sides of the conductor layer 10 in the thickness direction.
[0009] The conductor layer 10 contains copper as a main component. Specifically, the conductor layer 10 contains 50 mass% or more of copper. The conductor layer 10 may contain 70 mass% or more, 80 mass% or more, or 90 mass% or more but less than 100 mass% (99 mass% or less) of copper.
[0010] The conductor layer 10 is a sintered body of a plurality of crystallites. Figure 2 is an enlarged view of region A shown in Figure 1. As shown in Figure 2, the conductor layer 10 includes crystallites 11 that are polygonal in cross-sectional view.
[0011] In addition, adjacent crystallites 11a, 11b are in contact with each other along the straight line of each crystallite 11 as grain boundary 12. This makes it possible to increase the interface conductivity at high frequencies, thereby making it possible to obtain a wiring board that exhibits high interface conductivity at high frequencies.
[0012] Here, a method for evaluating the "straight-line sides" of the crystallite 11 will be described with reference to FIG. 3. FIG. 3 is an explanatory diagram showing a method for evaluating a crystallite. As shown in FIG. 3, the crystallite 11 has a polygonal cross section. As an example, the crystallite 11 shown in FIG. 3 has an octagonal outline having sides S01 to S08. For an image of the conductor layer 10 including such a cross section, for example, a scale (or ruler) 30 is prepared and positioned along the side S01. The length of the portion of the side S01 that is along the scale (or ruler) 30 is determined to be the maximum diameter d of the crystallite 11. MAX If the length of the edge S01 is equal to or greater than 1 / 2 of the length L01, it is defined as a "straight edge". Similarly to edge S01, the other edges S02 to S08 are also evaluated as to whether they are "straight edges". In the example shown in FIG. 3, edge S01 having length L01 and edge S07 having length L07 are evaluated as "straight edges". That is, the crystallite 11 shown in FIG. 3 has two "straight edges". The longest diameter d of the crystallite 11 MAX It is preferable that the thickness is 1 μm or more and 10 μm or less.
[0013] For example, the above-mentioned evaluation is repeated for each side of each of the multiple crystallites 11 in the conductor layer 10 according to the embodiment. In this case, the multiple crystallites 11 may have 70% or more of crystallites 11 with two or more straight sides. In this way, in a wiring board 1 having a conductor layer 10 in which 70% or more of the crystallites 11 have two or more straight sides, for example, a decrease in interface conductivity at frequencies of 1 GHz to 49 GHz can be reduced. This allows the interface conductivity at high frequencies to be increased.
[0014] Fig. 4 is a diagram showing the evaluation results of a plurality of crystallites in a conductor layer. As shown in Fig. 4, the conductor layer 10 has crystallites 11 each having 0 to 5 straight sides. The total number of crystallites 11 is 7+9+24+23+21+4=88, whereas the number of crystallites 11 having two or more straight sides is 24+23+21+4=72, and the proportion of these is 72 / 88×100≒81.8%.
[0015] In this case, the wiring board 1 is cut at a location where the cross section of the conductor layer 10 is visible, and the cut surface is polished to prepare a sample for cross-section observation.
[0016] Next, the polished surface is analyzed using an electron backscattered diffraction pattern (EBSD) method. The photographing range of the sample in the thickness direction and length direction of the conductor layer 10 is set, for example, as follows. The number of crystallites 11 included in the photographing range is, for example, 50 to 100.
[0017] Thickness direction of the conductor layer 10: An image is taken of an area in which one layer of the conductor layer 10 is visible. The length direction of the conductor layer 10: A range of about 20 μm is photographed. Alternatively, the range may be 10 μm or more and 20 μm or less.
[0018] The wiring board 1 according to the embodiment may have an interface conductivity of 90% or more at a frequency of 2 GHz, for example. The wiring board 1 may have an interface conductivity of 85% or more at a frequency of 30 GHz, for example. The wiring board 1 may have an interface conductivity of 78% or more at a frequency of 49 GHz, for example. The wiring board 1 has an interface conductivity of 78% or more at a frequency range of 30 GHz or more and 49 GHz or less. In this way, according to the wiring board 1 according to the embodiment, it is possible to reduce the decrease in interface conductivity at frequencies of 2 GHz to 49 GHz, for example. This makes it possible to increase the interface conductivity at high frequencies.
[0019] The conductor layer 10 may have recesses 13, 14 on the surface along the insulating layer 20. Here, the recesses 13, 14 may have a maximum depth of, for example, 1 μm or more and 3 μm or less. The width w of the recesses 13, 14 in the direction along the insulating layer 20 may be in the range of 50% or more and 90% or less of the average thickness t of the conductor layer 10. When the conductor layer 10 has such recesses 13, 14, for example, the adhesion between the conductor layer 10 and the insulating layer 20 can be improved. The radius of curvature of the recesses 13, 14 may be 5 μm or more and 50 μm or less, particularly 10 μm or more and 30 μm or less.
[0020] The average thickness t of the conductor layer 10 is obtained by, for example, averaging the thicknesses of the conductor layer 10 measured at each point (a total of five points) when an observed region (e.g., a length of 50 μm) is divided into four equal parts in the longitudinal direction. The thickness of each point of the conductor layer 10 is the length in the direction perpendicular to the longitudinal direction of the conductor layer 10. The average thickness t of the conductor layer 10 can be, for example, 5 μm or more and 15 μm or less, and further 6.5 μm or more and 10 μm or less.
[0021] The conductor layer 10 may have the recess 13 or the recess 14 on only one of the two surfaces facing the insulating layer 20, or may have the recesses 13 and 14 on both surfaces of the conductor layer 10 facing the insulating layer 20. The conductor layer 10 may have a plurality of recesses 13 and / or recesses 14.
[0022] In addition to the relatively large recesses 13 and 14, the conductor layer 10 may have a plurality of uneven portions 10A (in FIG. 2, the position of the recess is designated as the concave portion 10a, and the position of the protrusion adjacent thereto is designated as the convex portion 10b) having a smaller width. Here, even if the conductor layer 10 has the uneven portions 10A, it is preferable that the difference between the maximum thickness tmax and the minimum thickness tmin of the conductor layer 10 is 1 μm or more and 3 μm or less. When the conductor layer 10 has the uneven portions 10A, for example, the adhesion between the conductor layer 10 and the insulating layer 20 can be improved. Also, the variation in the interface conductivity can be reduced.
[0023] The conductor layer 10 may have silica particles on its surface. In other words, in this wiring board 1, silica is present on the surface of the conductor layer 10 in a particulate state. Here, the surface of the conductor layer 10 refers to the vicinity of the interface between the insulating layer 20 and the conductor layer 10 when the conductor layer 10 is formed on the surface of the insulating layer 20. The vicinity of the interface includes a small width range from the surface of the conductor layer 10 to the inside of the conductor layer 10. The small width range is within 1 μm from the surface of the conductor layer 10. The presence of silica particles on the surface of the conductor layer 10 can further increase the adhesion between the conductor layer 10 and the insulating layer 20, for example. The silica particles may be present over the entire surface of the conductor layer 10 facing the insulating layer 20, or may be present on a part of the surface of the conductor layer 10. When a plurality of silica particles are present on the surface of the conductor layer 10, these silica particles may be present as individual particles isolated from each other.
[0024] The reason why the adhesion between the insulating layer 20 and the conductor layer 10 is enhanced by the presence of silica particles on the surface of the conductor layer 10 or near the interface between the insulating layer 20 and the conductor layer 10 is considered to be due to the fact that the shrinkage behavior of the metal material (e.g., copper) used in the conductor layer 10 during firing is similar to the shrinkage behavior of the silica particles. In this case, the reason why the shrinkage behavior of the metal material used in the conductor layer 10 during firing is similar to the shrinkage behavior of the silica particles is considered to be that the size of the silica particles is small. For example, silica particles larger than the silica particles having a size described below have a wide particle size distribution based on the size. In addition, there is an increase in heat capacity due to the size. These factors are factors that change the sintering behavior and adhesion. In addition, when a glass powder of a complex oxide is used instead of the silica particles of a small size, the glass powder contains multiple components, so the temperature range at which the glass powder becomes molten is wider than that of the silica particles of a small size. For example, the melting temperature of the glass powder may start at a lower temperature than that of the silica particles of a small size. In addition, the glass powder often has a wide particle size distribution. When glass powder having these properties is used, the glass powder is likely to aggregate and move during firing in the print pattern that will become the conductor layer 10. As a result, when the conductor layer 10 is formed, the metal particles are likely to grow and voids are likely to occur in the conductor layer 10. This is because the glass powder is likely to diffuse from the print pattern to the area that will become the insulating layer 20. When fine silica particles are used, the range of temperatures at which the conductor layer 10 becomes molten is narrower than that of glass powder because of the single composition. As a result, the conductor layer 10 becomes dense, and the recesses 13 and 14 with a gentle shape are likely to be formed on the surface along the insulating layer 20. The particle size of the silica particles should preferably be 10 nm or more and 80 nm or less. Among these, the average particle size should preferably be 30 nm. The ratio of the integrated amount of the lower limit of 20 nm and the upper limit of 40 nm should preferably be 70% or more.
[0025] Furthermore, the conductor layer 10 may have uneven portions 10A on both sides facing the insulating layer 20, in addition to the recesses 13 and 14. By having portions forming uneven portions 10A in addition to the recesses 13 and 14 on both sides of the conductor layer 10 facing the insulating layer 20, i.e., the surfaces of the conductor layer 10 facing the first layer 21 and the second layer 22 of the insulating layer 20, it is possible to further increase the adhesion between the conductor layer 10 and the insulating layer 20, for example.
[0026] Furthermore, the conductor layer 10 may be located on the surface of the wiring board 1 that is exposed to the outside. In this case, the conductor layer 10 may be located on one side of the wiring board 1 or on both sides of the wiring board 1.
[0027] [Example] Specifically, wiring boards were fabricated and the difference in interface conductivity was evaluated.
[0028] First, a mixture of 40 wt% alumina particles and 60 wt% borosilicate glass was prepared as the material for the insulating layer. This mixture is a glass ceramic raw material with a firing temperature of 900°C to 1000°C. In addition, 20 parts by mass of isobutyl methacrylate resin and dibutyl phthalate were used as an organic binder for 100 parts by mass of the glass ceramic raw material, and a green sheet with a thickness of 100 μm was produced by doctor blade molding.
[0029] In addition, copper powder with an average particle size of 2 μm and silica particles with an average particle size of 20 nm were prepared as raw materials for the conductor layer. The ratio of the cumulative amount of silica particles with a lower limit of 10 nm and an upper limit of 30 nm was 70% or more. The amount of silica particles added was 1 part by mass per 100 parts by mass of copper powder. In addition, isobutyl methacrylate resin and a mixed solvent of butyl carbitol acetate and dibutyl phthalate were used as the organic binder. Five parts by mass of isobutyl methacrylate resin was added to 100 parts by mass of copper powder, and a mixed solvent of butyl carbitol acetate and dibutyl phthalate was further added to prepare a conductor paste containing copper powder and silica particles.
[0030] A conductive paste was printed on both surfaces of the prepared green sheet in a specified area and then fired. The firing was performed in a reducing atmosphere using a hydrogen-nitrogen mixed gas, with a maximum temperature of 930°C and a holding time of 2 hours. Multiple green sheets were stacked to a thickness of 500 μm.
[0031] On the other hand, the wiring board according to the reference example was produced in the same manner as the wiring board according to the above-mentioned example, except that the average particle size of the silica particles was set to 1 μm.
[0032] The interface conductivity was measured using the wiring boards fabricated as described above. The interface conductivity was measured by the dielectric cylinder resonator method described below. The measurement sample used was a 50 mm diameter sample with the conductor layer 10 formed over almost the entire surface of both sides.
[0033] The method for measuring interfacial conductivity using the dielectric cylinder resonator method is a method for measuring the conductivity at the interface between a conductor and an insulating layer, i.e., at the conductor interface, by attaching an insulating layer having a conductor formed therein to both end faces or one end face of a dielectric cylinder made of a dielectric material with known relative dielectric constant and dielectric loss in a predetermined relationship to form a dielectric resonator.
[0034] The principle of this measurement method is that when an electromagnetic resonator is constructed by sandwiching a conductor plate (usually a conductor plate having a diameter D about three times the diameter d of the dielectric cylinder) that is large enough to ignore the edge effect, parallel to both end faces of a dielectric cylinder having a predetermined dimensional ratio (height h / diameter d), the high-frequency current flowing in the conductor plate due to the TEomn resonance mode (hereinafter referred to as the TEomn mode) is distributed only on the short-circuit surface, i.e., the opposing surface between the dielectric and the conductor.
[0035] In a dielectric resonator, the high-frequency current flowing in the conductor due to the TEomn mode (m = 1, 2, 3..., n = 1, 2, 3...) is distributed only at the interface between the conductor and the dielectric substrate in contact with the dielectric cylinder. By utilizing this, the interfacial conductivity can be calculated from the resonant frequency f0, unloaded Q, and Qu of the measured TEomn mode (m = 1, 2, 3..., n = 1, 2, 3...). The interfacial conductivity was measured in the frequency range from 2 GHz to 49 GHz. The results are shown in Figure 5.
[0036] 5 is a diagram showing the relationship between frequency and interface conductivity in the wiring boards according to the examples and the reference example, where a solid line 51 represents the measurement result of the wiring board according to the example, and a dashed line 52 represents the measurement result of the wiring board according to the reference example.
[0037] As shown in Fig. 5, the wiring board according to the embodiment had a higher interfacial conductivity than the wiring board according to the reference example over the entire measured frequency range. In particular, the wiring board according to the reference example showed a significant decrease in interfacial conductivity in the frequency range of 30 to 48 GHz, while the wiring board according to the embodiment showed a small decrease in interfacial conductivity. This makes it clear that the wiring board according to the embodiment can increase the interfacial conductivity at high frequencies.
[0038] In addition, when the interfacial conductivity of an organic substrate using copper foil as a conductor layer was measured, the interfacial conductivity was found to be 99%, 81%, and 61% at frequencies of 2 GHz, 30 GHz, and 49 GHz, respectively, and the decrease in interfacial conductivity was particularly large in the frequency range of 30 to 48 GHz.
[0039] As described above, the wiring board 1 according to the embodiment includes an insulating layer 20 and a conductor layer 10 laminated together. The insulating layer 20 is made of glass ceramics. The conductor layer 10 is a sintered body of a plurality of crystallites 11 containing copper as a main component. The plurality of crystallites 11 include polygonal crystallites 11 including straight sides, and the straight sides are in contact with each other as grain boundaries 12. This can increase the interface conductivity at high frequencies.
[0040] Further advantages and other aspects may readily occur to those skilled in the art. Thus, the disclosure in its broader aspects is not limited to the specific details and representative embodiments shown and described above. Accordingly, various modifications may be made without departing from the spirit or scope of the general inventive concept as defined by the appended claims and equivalents thereof. [Explanation of symbols]
[0041] 1. Wiring board 10 Conductor layer 11 Crystal 12 Grain boundaries 13,14 Recess 20 Insulating layer 21 1st layer 22 2nd layer
Claims
1. An insulating layer; A conductor layer is laminated, the insulating layer is made of glass ceramics; the conductor layer is a sintered body of a plurality of crystallites containing copper as a main component, The plurality of crystallites include polygonal crystallites having straight edges, and the edges are in contact with each other as grain boundaries, the conductor layer has a plurality of silica particles; The silica particles have a single composition and are isolated from each other. Wiring board.
2. The plurality of crystallites include crystallites having two or more sides in a number ratio of 70% or more. The wiring board according to claim 1 .
3. the conductor layer has a recess on a surface along the insulating layer, The recess has a width in a direction along the insulating layer that is 50% or more of the average thickness of the conductor layer. The wiring board according to claim 1 .
4. The conductor layer is sandwiched between the insulating layers and has projections and recesses on both sides along the insulating layers. The wiring board according to any one of claims 1 to 3.
5. 5. The wiring board according to claim 1, wherein the conductor layer contains copper as a metal component, and the copper content is 80% by mass or more and 99% by mass or less.
6. 6. The wiring board according to claim 1, wherein the conductor layer has an interface conductivity of 78% or more in a frequency range of 30 GHz or more and 49 GHz or less.
7. 7. The wiring board according to claim 1, wherein the silica particles are present near the interface between the conductor layer and the insulating layer.
8. 8. The wiring board according to claim 1, wherein the silica particles have an average particle size of 10 nm or more and 80 nm or less.
9. 9. The wiring board according to claim 1, wherein the silica particles have an average particle size of 30 nm, and the ratio of the integrated amount of the lower limit of 20 nm to the upper limit of 40 nm is 70% or more.
Citation Information
Patent Citations
Multilayer ceramic circuit board
JP2000244123A
Thick film paste and ceramic circuit board
JP2001202823A
Copper metallized composition and ceramic wiring board
JP2003277852A
Multilayer ceramic substrate
WO2017187753A1