Conductive compositions and metallized substrates and methods for their manufacture
A conductive composition combining small and large Ag particles with Mn, Fe, and Cu, and glass particles addresses the issues of adhesion and reliability in ceramic substrate circuits, providing enhanced plating resistance and conductivity under varying conditions.
Patent Information
- Application Number
- JP2020087649
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-05-29
- Filing Date
- 2020-05-19
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2040-05-19
AI Technical Summary
Existing conductive compositions for forming circuits on ceramic substrates lack sufficient adhesion, plating resistance, and reliability, particularly under varying environmental conditions, and have not been adequately evaluated for these properties.
A conductive composition comprising a combination of small and large isotropic Ag particles, along with a metal component consisting of Mn, Fe, and Cu, and glass particles, which are combined to enhance adhesion and plating resistance, ensuring high reliability and conductivity.
The composition forms a conductive part with high adhesion to ceramic substrates, exhibiting excellent electrical conductivity, electromigration resistance, and maintaining reliability under harsh conditions such as high temperature and humidity, with improved plating resistance and adhesion strength.
Smart Images

Figure 0007566488000001 
Figure 0007566488000002 
Figure 0007566488000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a conductive composition used in the electronics field for forming circuits on a ceramic substrate, a metallized substrate having a circuit formed from this composition, and a method for producing the same. [Background technology]
[0002] Conductive compositions (conductive pastes) are widely used in the electronics field because they can be easily used to form various patterns such as electrodes by printing, etc. Silver pastes, which contain silver in conductive metal powder, are used to form electrodes and circuits for electronic components, etc., and are broadly divided into resin-curing type and sintering type.
[0003] In the case of a resin-curing type conductive composition, the metal comes into contact with the resin by curing, thereby ensuring electrical conductivity, whereas in the case of a sintered type conductive composition, the metal particles are bonded together by sintering, thereby ensuring electrical conductivity.
[0004] The fired type conductive composition contains conductive metal powder such as silver, copper, nickel, palladium, gold, etc., glass powder as an inorganic binder, a vehicle, a solvent, etc. Conductive compositions are required to satisfy requirements such as adhesion to substrates, plating resistance, solder resistance, reliability, and electromigration resistance.
[0005] Plating is performed to prevent solder erosion of the electrodes, to prevent sulfurization, and to protect against corrosion. If the fired film has pores, plating solution may penetrate during plating, which may reduce the adhesive strength with the substrate. In addition, the infiltrated plating solution may evaporate and expand due to reflow, causing the electrodes to burst, resulting in reduced reliability. Therefore, a dense film must be formed to ensure plating resistance.
[0006] Silver (Ag) is stable in air and can be fired in air, but has the disadvantage of being prone to electromigration. Conductive pastes containing metal compounds such as Cu, Mn, and Sn have been disclosed to prevent Ag electromigration and to improve solder resistance.
[0007] Japanese Patent Laid-Open Publication No. 55-149356 (Patent Document 1) discloses a conductive coating material that prevents migration by mixing 1 to 100 parts by mass of Mn and / or Mn alloy powder with 100 parts by mass of Ag powder.
[0008] Japanese Patent Laid-Open Publication No. 2003-115216 (Patent Document 2) discloses a conductive paste containing a binder resin, Ag powder, and at least one metal or metal compound selected from the group consisting of Ti, Ni, In, Sn, and Sb.
[0009] However, the paint of Patent Document 1 and the paste of Patent Document 2 have not been evaluated for adhesion, solder heat resistance, plating resistance, reliability, and the like.
[0010] WO2014 / 061765 (Patent Document 3) discloses a conductive paste containing Ag powder, glass frit, an organic binder, and powder containing Cu, Sn, and Mn, and describes that the paste has excellent electromigration resistance, solder heat resistance, and adhesion.
[0011] However, this paste has not been evaluated for its plating resistance or reliability.
[0012] WO2015 / 141816 (Patent Document 4) discloses a conductive paste containing Ag powder, glass frit, an organic binder, and a powder containing Cu element and at least one metal element selected from the group consisting of V, Cr, Mn, Fe, and Co. This document describes that the inclusion of a metal powder improves the electromigration resistance, solder heat resistance, and adhesion of the conductive paste.
[0013] However, even this paste has not been evaluated for its plating resistance.
[0014] WO2017 / 141984 (Patent Document 5) discloses a conductive paste containing Ag powder, glass frit, an organic binder, and Pt-group oxides such as Cu, Sn, Mn, and ruthenium oxide. In this document, reliability tests such as high-temperature exposure and heat cycle tests are carried out.
[0015] However, even this paste has not been evaluated for its plating resistance.
[0016] Japanese Patent Laid-Open Publication No. 2018-152218 (Patent Document 6) discloses a conductive paste containing Ag powder, Bi-based glass powder, a silsesquioxane compound, and an organic vehicle. This document describes evaluations of plating resistance and solder resistance.
[0017] However, this paste has not been evaluated for reliability. [Prior art documents] [Patent documents]
[0018] [Patent Document 1] JP 55-149356 A (Claims, page 2, upper right column, line 1) [Patent Document 2] JP 2003-115216 A (Claim 1) [Patent Document 3] WO2014 / 061765 (Claim 1, paragraph
[0025] ) [Patent Document 4] WO2015 / 141816 (Claim 1, paragraph
[0009]
[0010] ) [Patent Document 5] WO2017 / 141984 (Claims, Examples) [Patent Document 6] JP 2018-152218 A (Claim 1, paragraph
[0009] ) Summary of the Invention [Problem to be solved by the invention]
[0019] Therefore, an object of the present invention is to provide a conductive composition that can form a conductive part with high adhesion to a ceramic substrate and can produce a metallized substrate that is resistant to plating and highly reliable, a metallized substrate having a conductive part formed from this composition, and a method for producing the same.
[0020] Another object of the present invention is to provide a conductive composition capable of forming a conductive portion having high adhesion to a ceramic substrate regardless of changes in the usage environment, a metallized substrate having a conductive portion formed from this composition, and methods for manufacturing the same. [Means for solving the problem]
[0021] As a result of intensive research into achieving the above-mentioned object, the present inventors have found that by combining Ag particles (A) consisting of isotropically shaped Ag small particles (A1) having a particle size of less than 1.2 μm and isotropically shaped Ag large particles (A2) having a particle size of 1.2 μm or more, metal component (B) consisting of Mn component (B1), Fe component (B2) and Cu component (B3), and glass particles (C), it is possible to form a conductive portion having high adhesion to a ceramic substrate and to produce a metallized substrate having high plating resistance and reliability, and have completed the present invention.
[0022] That is, the conductive composition of the present invention is a conductive composition containing Ag particles (A), metal components (B) and glass particles (C), the Ag particles (A) being Ag small particles (A1) and Ag large particles (A2), the Ag small particles (A1) being isotropically shaped particles with a particle size of less than 1.2 μm, the Ag large particles (A2) being isotropically shaped particles with a particle size of 1.2 μm or more, and the metal components (B) being Mn components (B1), Fe components (B2) and Cu components (B3). The Ag small particles (A1) may be spherical particles with a median particle size of 0.01 μm or more and less than 1.2 μm. The Ag large particles (A2) may be spherical particles with a median particle size of 1.2 to 20 μm. The mass ratio of the Ag small particles (A1) to the Ag large particles (A2) is about the former / latter=90 / 10 to 5 / 95. The glass particles (C) may contain bismuth-based glass particles and / or zinc-based glass particles.
[0023] The present invention also includes a method for producing the conductive composition, in which at least one selected from the group consisting of the Mn component (B1), the Fe component (B2), and the Cu component (B3) is added in the form of a liquid composition.
[0024] The present invention also includes a method for producing a metallized substrate, the method including a step of adhering the conductive composition to a ceramic substrate, and a step of firing the conductive composition adhered to the ceramic substrate to form a conductive portion. In the firing step, the conductive composition may be fired in air.
[0025] The present invention also includes a metallized substrate obtained by the above-mentioned manufacturing method. The ceramic substrate may be an alumina substrate, an alumina-zirconia substrate, an aluminum nitride substrate, a silicon nitride substrate, or a silicon carbide substrate.
[0026] In the present application, the term "metal component" is used to include both simple metals and metal compounds, including Mn, Fe, and Cu components. Effect of the Invention
[0027] In the present invention, Ag particles (A) consisting of isotropic Ag small particles (A1) with a particle size of less than 1.2 μm and isotropic Ag large particles (A2) with a particle size of 1.2 μm or more, metal components (B) consisting of Mn components (B1), Fe components (B2) and Cu components (B3), and glass particles (C) are combined, so that a conductive part with high adhesion to a ceramic substrate can be formed, and a metallized substrate with high plating resistance and reliability can be manufactured. In particular, a conductive part with high adhesion to a ceramic substrate can be formed regardless of changes in the usage environment. Furthermore, the metallized substrate exhibits excellent conductivity and electromigration resistance, and can maintain high adhesion to a ceramic substrate even under harsh conditions such as high temperature and high humidity, rapid temperature changes, and long-term exposure to high temperatures, and can manufacture a highly reliable metallized substrate. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0028] [Ag particles (A)] The conductive composition of the present invention contains Ag particles (A) as a conductive component. The Ag particles (A) are a combination of isotropically shaped Ag small particles (A1) having a particle size of less than 1.2 μm and isotropically shaped Ag large particles (A2) having a particle size of 1.2 μm or more. The Ag particles (A) impart conductivity, and by combining the Ag small particles (A1) and the Ag large particles (A2), the Ag particles can form a close-packed structure, thereby forming a denser film.
[0029] (Ag small particles (A1)) The shape of the Ag small particles (A1) is isotropic from the viewpoint of improving plating resistance and reliability. Examples of isotropic shapes include spherical (true spherical or nearly spherical) and regular polyhedral (regular hexahedral or cubic, regular octahedral, etc.). Among these, spherical is particularly preferred from the viewpoint of improving adhesion to ceramic substrates.
[0030] In the present application, the term "spherical" is used to include both a perfect sphere and an approximately sphere. In a sphere, the ratio of the major axis to the minor axis is, for example, 1 to 2, preferably 1 to 1.5, more preferably 1 to 1.3, even more preferably 1 to 1.2, and most preferably 1 to 1.1. In addition, an isotropic shape also includes an approximately isotropic shape.
[0031] The particle size (particle size distribution) of the Ag small particles (A1) may be in the range of less than 1.2 μm, for example, in the range of 0.01 μm or more and less than 1.2 μm. The median particle size (D50) of the Ag small particles (A1) is, for example, 0.05 μm or more and less than 1.2 μm, preferably 0.1 to 1 μm, more preferably 0.2 to 0.8 μm, more preferably 0.3 to 0.7 μm, more preferably 0.4 to 0.6 μm, and most preferably about 0.45 to 0.55 μm. If the particle size of the Ag small particles (A1) is too small, it may be difficult to fill the gaps of the Ag large particles (A2), and conversely, if it is too large, it may be difficult to penetrate into the gaps.
[0032] The 10 volume % particle size (D10) of the Ag small particles (A1) may be 0.01 μm or more (e.g., 0.01 to 0.49 μm), for example, 0.1 μm or more (e.g., 0.1 to 0.45 μm), preferably 0.2 μm or more, more preferably 0.3 μm or more, and most preferably 0.4 μm or more (e.g., 0.4 to 0.43 μm). If D10 is too small, it may be difficult to efficiently fill the gaps between the Ag large particles (A2).
[0033] The 90 volume % particle size (D90) of the Ag small particles (A1) may be 1.19 μm or less (e.g., 0.5 to 1.19 μm), for example, 1.18 μm or less, preferably 1.17 μm or less, more preferably 1.15 μm or less, and most preferably 1.12 μm or less (e.g., 1 to 1.12 μm). If D90 is too large, it may be difficult to efficiently fill the gaps between the Ag large particles (A2).
[0034] In this application, the particle size distribution and median particle size of particles (including other particles described later) refer to the particle size distribution and median particle size (volume basis) measured using a laser diffraction scattering type particle size distribution measuring device.
[0035] (Ag large particles (A2)) The shape of the Ag large particles (A2) is also isotropic from the viewpoint of improving plating resistance and reliability, and is the same as that of the Ag small particles (A1), including the preferred embodiment.
[0036] The particle size (particle size distribution) of the Ag large particles (A2) may be in the range of 1.2 μm or more, for example, 1.2 to 20 μm, preferably 1.2 to 15 μm, more preferably 1.2 to 10 μm, and most preferably about 1.2 to 8 μm. The median particle size (D50) of the Ag large particles (A2) is, for example, 1.2 to 20 μm, preferably 1.3 to 10 μm, more preferably 1.5 to 5 μm, more preferably 1.7 to 3 μm, more preferably 1.8 to 2.5 μm, and most preferably about 1.9 to 2.2 μm. If the particle size of the Ag large particles (A2) is too small, there is a risk that the adhesion to the ceramic substrate will decrease, and conversely, if the particle size is too large, there is a risk that the adhesion will also decrease.
[0037] The 10 volume % particle size (D10) of the Ag large particles (A2) may be 1.21 μm or more (e.g., 1.21 to 1.9 μm), for example, 1.22 μm or more (e.g., 1.22 to 1.8 μm), preferably 1.23 μm or more, more preferably 1.24 μm or more, and most preferably 1.25 μm or more (e.g., 1.25 to 1.5 μm). If D10 is too small, there is a risk of reduced adhesion to the ceramic substrate.
[0038] The 90 volume % particle size (D90) of the Ag large particles (A2) may be 10 μm or less (e.g., 2 to 10 μm), for example, 8 μm or less, preferably 5 μm or less, more preferably 3.5 μm or less, and most preferably 3.3 μm or less (e.g., 2.5 to 3.3 μm). If D90 is too large, there is a risk of reduced adhesion to the ceramic substrate.
[0039] (Characteristics of Ag particles (A)) The mass ratio of the Ag small particles (A1) to the Ag large particles (A2) can be selected from the range of about the former / latter = 99 / 1 to 1 / 99 (e.g., 95 / 5 to 10 / 90), for example, about 90 / 10 to 5 / 95 (e.g., 90 / 10 to 10 / 90), preferably about 90 / 10 to 20 / 80 (e.g., 80 / 20 to 10 / 90), more preferably about 70 / 30 to 20 / 80, and most preferably about 50 / 50 to 30 / 70. If the proportion of the Ag small particles (A1) is too small, the denseness of the fired body may decrease, and conversely, if it is too large, the adhesion to the ceramic substrate may decrease.
[0040] The median particle size (D50) of the Ag particles (A) is, for example, about 0.1 to 10 μm, preferably about 0.3 to 5 μm, more preferably about 0.5 to 3 μm, and most preferably about 1 to 2 μm. If the particle size of the Ag particles (A) is too small, there is a risk that the adhesion to the ceramic substrate may decrease, and conversely, if the particle size is too large, there is a similar risk that the adhesion may decrease.
[0041] The proportion of the Ag particles (A) in the conductive composition can be selected from the range of about 10 to 99 mass%, for example, about 30 to 98 mass%, preferably 50 to 95 mass%, more preferably 70 to 93 mass%, and most preferably about 80 to 90 mass%. If the proportion of the Ag particles (A) is too small, the conductivity may decrease, and conversely, if it is too large, the adhesion to the ceramic substrate may decrease.
[0042] [Metal component (B)] The metal component (B) is a combination of a Mn component (B1), an Fe component (B2), and a Cu component (B3). In the present invention, the conductive composition contains this metal component (B), which can improve the denseness and electromigration resistance of the sintered body, and can improve the reliability of the conductive part, which is the sintered body. Furthermore, it is preferable that at least one of the Mn component (B1), the Fe component (B2), and the Cu component (B3) is an organometallic compound (particularly, a metal carboxylate) in terms of ease of viscosity adjustment during composition preparation and improved reliability.
[0043] (Mn component (B1)) The Mn component (B1) includes simple Mn, inorganic Mn compounds, and organic Mn compounds.
[0044] Examples of inorganic Mn compounds include Mn oxides such as manganese dioxide, manganese boride, inorganic acid Mn salts such as manganese carbonate, manganese phosphate, manganese borate, manganese sulfate, and manganese nitrate, and Mn halides such as manganese chloride. These inorganic Mn compounds can be used alone or in combination. Among these, manganese dioxide, manganese carbonate, and manganese phosphate are preferred.
[0045] Examples of shapes of Mn simple substance and inorganic Mn compounds include spherical (true spherical or nearly spherical), ellipsoidal (elliptical sphere), polyhedral (polygonal pyramid, polygonal column such as cube or rectangular parallelepiped, etc.), rod or stick, fibrous, acicular, irregular, etc. Among these, granular shapes such as spherical, ellipsoidal, polyhedral, and irregular shapes are preferred from the viewpoint of improving adhesion to the ceramic substrate, and isotropic shapes (particularly spherical) such as spheres and regular polyhedral (regular hexahedron, cube, regular octahedron, etc.) are particularly preferred.
[0046] The median particle size (D50) of particles formed of simple Mn and inorganic Mn compounds is, for example, about 0.1 to 10 μm, preferably about 0.3 to 5 μm, more preferably about 0.5 to 3 μm, and most preferably about 0.8 to 2 μm. If the particle size is too small, the economic efficiency decreases and dispersibility in the conductive composition may also decrease. Conversely, if the particle size is too large, the printability and uniformity of the fired film decrease, and when printing with a mesh screen, it may cause mesh clogging.
[0047] The organic Mn compound may be a Mn carboxylate such as manganese formate, manganese acetate, manganese oxalate, manganese butyrate, manganese caproate, manganese octoate, manganese neodecanoate, manganese stearate, or manganese naphthenate. The organic Mn compound may be a Mn-based metal soap (for example, a higher fatty acid Mn salt such as manganese octoate, manganese neodecanoate, or manganese stearate). These organic Mn compounds may be used alone or in combination of two or more. Of these, C carboxylates such as manganese octoate are preferred. 4-24 Saturated fatty acid manganese is preferred. Organic Mn compounds (especially C 4-24 The saturated fatty acid Mn salt may be used in the form of a liquid composition. The liquid composition may be a hydrocarbon solution, such as a petroleum-based hydrocarbon solution (e.g., a mineral spirits solution).
[0048] The Mn component (B1) is preferably an inorganic Mn compound or an organic Mn compound, and more preferably a Mn oxide such as manganese dioxide, or a C compound such as manganese octylate. 6-18 Saturated fatty acid Mn salts are more preferred, C 6-12 Saturated fatty acid Mn salts are most preferred.
[0049] The ratio of the Mn component (B1) is, in terms of Mn element (as the ratio of Mn element), for example, 0.01 to 1 part by mass, preferably 0.03 to 0.5 parts by mass, more preferably 0.1 to 0.3 parts by mass (for example, 0.15 to 0.25 parts by mass), and most preferably about 0.2 to 0.3 parts by mass, relative to 100 parts by mass of the Ag particles (A). The ratio of the Mn component (B1) in the metal component (B) is, in terms of Mn element, for example, 3 to 20% by mass, preferably 5 to 15% by mass, and more preferably about 7.5 to 10% by mass. If the ratio of the Mn component (B1) is too low, the denseness of the fired body may decrease, and conversely, if it is too high, the electrical conductivity may decrease.
[0050] (Fe component (B2)) The Fe component (B2) includes simple Fe, inorganic Fe compounds, and organic Fe compounds.
[0051] Examples of inorganic Fe compounds include Fe oxides such as iron(II) oxide, iron(III) oxide (iron trioxide), and triiron tetroxide; iron boride; iron hydroxide; iron sulfide; inorganic acid Fe salts such as iron carbonate, iron phosphate, iron borate, iron sulfate, and iron nitrate; and Fe halides such as iron chloride. These inorganic Fe compounds can be used alone or in combination of two or more. Of these, iron(II) oxide, iron(III) oxide, triiron tetroxide, and iron phosphate are preferred.
[0052] The forms of the Fe element and the inorganic Fe compound, including the preferred embodiments, are the same as those of the Mn element and the inorganic Mn compound.
[0053] The median particle size (D50) of particles formed of simple Fe and inorganic Fe compounds is, for example, about 0.1 to 10 μm, preferably about 0.3 to 5 μm, more preferably about 0.5 to 3 μm, and most preferably about 0.8 to 2 μm. If the particle size is too small, the economic efficiency may decrease and the dispersibility in the conductive composition may also decrease. Conversely, if the particle size is too large, the printability and uniformity of the fired film may decrease, and when printing with a mesh screen, it may cause clogging of the mesh.
[0054] Examples of the organic Fe compounds include Fe carboxylates such as iron formate, iron acetate, iron oxalate, iron butyrate, iron caproate, iron octoate, iron neodecanoate, iron stearate, and iron naphthenate; and metal complexes such as acetylacetone metal complex (ferric nursem). Examples of the organic Fe compounds include Fe-based metal soaps (for example, higher fatty acid Fe salts such as iron octoate, iron neodecanoate, and iron stearate). These organic Fe compounds can be used alone or in combination of two or more. Of these, C ions such as iron octoate are preferred. 4-24 Saturated fatty acid Fe salts are preferred. Organic Fe compounds (especially C 4-24 The saturated fatty acid Fe salt may be used in the form of a liquid composition. The liquid composition may be a hydrocarbon solution such as a petroleum-based hydrocarbon solution (e.g., a mineral spirit solution).
[0055] The Fe component (B2) is preferably an inorganic Fe compound or an Fe carboxylate, and more preferably iron oxide, C 6-18 Saturated fatty acid Fe salts are more preferred, and iron(II) oxide is most preferred.
[0056] The proportion of the Fe component (B2) is, in terms of Fe element (as the proportion of Fe element), for example, 0.01 to 1 part by mass, preferably 0.03 to 0.5 parts by mass, more preferably 0.1 to 0.3 parts by mass (for example, 0.15 to 0.25 parts by mass), and most preferably about 0.13 to 0.2 parts by mass, relative to 100 parts by mass of the Ag particles (A). The proportion of the Fe component (B2) in the metal component (B) is, in terms of Fe element, for example, 3 to 15% by mass, preferably 4 to 10% by mass, and more preferably about 5 to 8% by mass. If the proportion of the Fe component (B2) is too small, the denseness of the fired body may decrease, and conversely, if it is too large, the electrical conductivity may decrease.
[0057] (Cu component (B3)) The Cu component (B3) includes simple Cu, inorganic Cu compounds, and organic Cu compounds.
[0058] Examples of inorganic Cu compounds include Cu oxides such as copper oxide, copper hydroxide, copper sulfide, inorganic acid Cu salts such as copper carbonate, copper phosphate, copper borate, copper sulfate, and copper nitrate, and Cu halides such as copper chloride. These inorganic Cu compounds can be used alone or in combination. Among these, copper oxide, copper carbonate, and copper phosphate are preferred.
[0059] The forms of the Cu element and the inorganic Cu compound, including the preferred embodiments, are the same as those of the Mn element and the inorganic Mn compound.
[0060] The median particle size (D50) of particles formed of simple Cu and inorganic Cu compounds is, for example, about 0.1 to 10 μm, preferably about 0.5 to 5 μm, and more preferably about 1 to 3 μm. If the particle size is too small, the economic efficiency may decrease and the dispersibility in the conductive composition may also decrease. Conversely, if the particle size is too large, the printability and uniformity of the fired film may decrease, and when printing with a mesh screen, it may cause mesh clogging.
[0061] Examples of organic Cu compounds include Cu carboxylates such as copper formate, copper acetate, copper oxalate, copper butyrate, copper caproate, copper octylate, copper neodecanoate, and copper naphthenate; and metal complexes such as acetylacetone metal complex (nacem copper). Examples of organic Cu compounds include Cu-based metal soaps (e.g., higher fatty acid Cu salts such as copper neodecanoate and copper naphthenate). These organic Cu compounds can be used alone or in combination of two or more. Among these, cyclic fatty acid Cu salts such as copper naphthenate (e.g., C salts of cyclopentane, cyclohexane, etc.) are preferred. 4-8 C such as copper salts of fatty acids with cycloalkane carboxylic acids, copper neodecanoate, etc. 4-24 Saturated fatty acid Cu salts are preferred. The organic Cu compounds (particularly cyclic fatty acid Cu salts) may be used in the form of a liquid composition. The liquid composition may be a hydrocarbon solution such as a petroleum-based hydrocarbon solution (e.g., a mineral spirit solution).
[0062] As the Cu component (B3), Cu alone, inorganic Cu compounds, and Cu carboxylates are preferred, copper alone, copper oxide, and a mineral spirit solution of cyclic fatty acid copper are more preferred, and a combination of Cu alone with copper oxide and / or Cu carboxylates is particularly preferred. Of these, copper oxide is particularly preferred, and a combination of Cu alone with copper oxide is most preferred.
[0063] When simple Cu is combined with copper oxide and / or a Cu carboxylate (particularly copper oxide), the ratio of the former / the latter, calculated in terms of Cu element (as the ratio of Cu element), is about 50 / 1 to 1 / 1, preferably 30 / 1 to 3 / 1, more preferably 20 / 1 to 5 / 1, and most preferably 15 / 1 to 8 / 1.
[0064] The proportion of the Cu component (B3) can be selected from a range of about 0.01 to 5 parts by mass (for example, 0.1 to 5 parts by mass) relative to 100 parts by mass of the Ag particles (A) in terms of Cu element (as the proportion of Cu element), and is, for example, about 0.5 to 5 parts by mass, preferably about 1 to 4 parts by mass, more preferably about 1.5 to 3 parts by mass, and most preferably about 2 to 2.5 parts by mass. The proportion of the Cu component (B3) in the metal component (B) is, for example, about 70 to 90% by mass, preferably about 80 to 88% by mass, and more preferably about 83 to 86% by mass, in terms of Cu element. If the proportion of the Cu component (B3) is too small, the denseness of the fired body may decrease, and conversely, if it is too large, the electrical conductivity may decrease.
[0065] (Preferred embodiment of metal component (B)) From the viewpoint of improving reliability, the metal component (B) preferably contains an organometallic compound (i.e., an organic Mn compound, an organic Fe compound, or an organic Cu compound), and any of the Mn component (B1), the Fe component (B2), and the Cu component (B3) may contain an organometallic compound. Among them, it is preferable that one or two of the Mn component (B1), the Fe component (B2), and the Cu component (B3) are organometallic compounds (particularly, metal carboxylates), and it is particularly preferable that only one is an organometallic compound. Furthermore, it is preferable that at least the Mn component (B1) or the Fe component (B2) is an organometallic compound, it is more preferable that at least the Mn component (B1) is an organometallic compound, and it is particularly preferable that only the Mn component (B1) is an organometallic compound. In particular, in the present invention, when the organometallic compound is blended in the form of a liquid composition, reliability can be further improved.
[0066] Mn component (B1) is an organometallic compound (especially C 6-12In the case where the Fe component (B2) is a saturated fatty acid Mn salt, the Fe component (B2) is preferably an inorganic Fe compound and / or an organic Fe compound, more preferably an iron oxide and / or an Fe carboxylate, and more preferably Fe 2 O 3 is particularly preferred. The Cu component (B3) may be a Cu simple substance, an inorganic Cu compound, or 4-8 At least one selected from fatty acid Cu salts having a cycloalkane ring is preferred, copper oxide is more preferred, and a combination of Cu alone and copper oxide is particularly preferred.
[0067] The Fe component (B2) is an organometallic compound (especially C 6-12 In the case where the Mn component (B1) is an inorganic Mn compound and an organic Mn compound, it is preferable that the Mn component (B1) is at least one selected from inorganic Mn compounds and organic Mn compounds, more preferably manganese oxide and / or a Mn carboxylate, and more preferably manganese oxide or C 6-12 Saturated fatty acid Mn salts are particularly preferred. The Cu component (B3) is preferably at least one selected from the group consisting of Cu simple substance, inorganic Cu compounds, and cyclic fatty acid Cu salts. 4-8 A fatty acid Cu salt having a cycloalkane ring is more preferred, and Cu alone is particularly preferred.
[0068] The Cu component (B3) is an organometallic compound (especially C 4-8 In the case where the Mn component (B1) contains a fatty acid Cu salt having a cycloalkane ring, the Mn component (B1) is preferably an inorganic Mn compound and / or an organic Mn compound, more preferably manganese oxide and / or a carboxylate Mn salt, and more preferably manganese oxide or C 6-12 Saturated fatty acid Mn salts are particularly preferred. The Fe component (B2) is preferably an inorganic Fe compound and / or an organic Fe compound, more preferably an iron oxide and / or an Fe carboxylate, and more preferably Fe 2 O 3 or C 6-12 Saturated fatty acid Fe salts are more preferred, Fe 2 O 3 is particularly preferred.
[0069] Among these combinations, the Mn component (B1) is an organometallic compound (especially C6-12 The most preferred combination is that the Fe component (B1) is an inorganic Fe compound (particularly, iron oxide), and the Cu component (B3) is an inorganic Cu compound (particularly, a combination of elemental Cu and copper oxide).
[0070] (Proportion of metal component (B)) The ratio of the metal component (B) can be selected from the range of about 0.1 to 10 parts by mass relative to 100 parts by mass of the Ag particles (A) in terms of metal elements (as the total ratio of Mn, Fe and Cu elements), and is, for example, about 0.5 to 5 parts by mass, preferably 0.7 to 4.5 parts by mass (e.g., 1 to 4 parts by mass), more preferably 0.8 to 3.7 parts by mass (e.g., 2 to 3.5 parts by mass), and most preferably about 2.5 to 3 parts by mass. If the ratio of the metal component (B) is too low, the denseness of the fired body may decrease, and conversely, if it is too high, the electrical conductivity may decrease.
[0071] Glass particles (C) The glass particles (glass powder) (C) need only function as a sintering aid, and conventional glass particles used for electrical conductors can be used.
[0072] The composition of the glass constituting the glass particles (C) is not particularly limited, but may be, for example, a glass having the composition formula SiO 2 -B 2 O 3 -R 2 Borosilicate glass (silica-based glass) represented by the formula AlO (wherein R represents an alkali metal such as K or Na) 2 O 3 -SiO 2 -M.O.R. 2 O (wherein M represents an element other than Al and Si, and R is the same as above), aluminosilicate glass represented by the composition formula Al 2 O 3 -SiO 2 -B 2 O 3 -M.O.R. 2 O (wherein M represents an element other than Al, Si, and B, and R is the same as above), 2 O 3 -MO-B2 O 3 (wherein M represents an element other than Bi and B), bismuth-based glass represented by the formula: ZnO-SiO 2 -B 2 O 3 -R 2 Examples of the glass include zinc-based glass represented by O (wherein R is the same as above). These glasses can be used alone or in combination of two or more. Among these, bismuth-based glass and / or zinc-based glass are preferred from the viewpoint of improving plating resistance, and bismuth-based glass is particularly preferred. Glass particles having these glass compositions can also be used alone or in combination of two or more.
[0073] The softening point (or melting point) of the glass particles (C) is preferably lower than the firing temperature of the conductive composition. The softening point of the glass particles is, for example, about 400 to 800° C., preferably about 420 to 780° C., more preferably about 450 to 750° C., more preferably about 460 to 600° C., and most preferably about 470 to 550° C. If the softening point is too low, the strength of the fired body may decrease, and conversely, if it is too high, the melt flowability may decrease, and the function as a binder may decrease.
[0074] The shape of the glass particles (C), including the preferred embodiment, is the same as that of the small Ag particles (A1).
[0075] The median particle size (D50) of the glass particles (C) is, for example, about 0.1 to 20 μm, preferably about 0.5 to 10 μm, and more preferably about 1 to 5 μm. If the particle size is too small, the economic efficiency may decrease and the dispersibility in the composition may also decrease. Conversely, if the particle size is too large, the printability and uniformity of the fired film may decrease, and when printing with a mesh screen, it may cause mesh clogging.
[0076] The proportion of the glass particles (C) can be selected from the range of about 0.05 to 15 parts by mass relative to 100 parts by mass of the Ag particles (A), and is, for example, about 0.1 to 10 parts by mass, preferably 0.5 to 8 parts by mass, more preferably 1 to 5 parts by mass, and most preferably about 2 to 4 parts by mass. If the proportion of the glass particles (C) is too small, the function as a sintering aid may decrease, and the effect of improving plating resistance may also decrease, while conversely, if it is too large, the electrical conductivity may decrease.
[0077] [Resin component (D)] The conductive composition of the present invention may further contain a resin component (D) as an organic binder. The resin component (D) is not particularly limited, and examples thereof include thermoplastic resins (olefin resins, vinyl resins, acrylic resins, styrene resins, polyether resins, polyester resins, polyamide resins, cellulose derivatives, etc.), thermosetting resins (thermosetting acrylic resins, epoxy resins, phenolic resins, unsaturated polyester resins, polyurethane resins, etc.). These resin components can be used alone or in combination of two or more. Among these resin components, resins that are easily burned off during the firing process and have a low ash content, such as acrylic resins (polymethyl methacrylate, polybutyl methacrylate, etc.), cellulose derivatives (nitrocellulose, ethyl cellulose, butyl cellulose, cellulose acetate, etc.), polyethers (polyoxymethylene, etc.), rubbers (polybutadiene, polyisoprene, etc.), etc. are commonly used, and cellulose derivatives such as ethyl cellulose are preferred.
[0078] The proportion of the resin component (D) is, for example, about 0.1 to 5 parts by mass, preferably about 0.3 to 3 parts by mass, more preferably about 0.5 to 2 parts by mass, and most preferably about 0.8 to 1.5 parts by mass, relative to 100 parts by mass of the Ag particles (A). If the proportion of the resin component (D) is too small, the handleability of the conductive composition may decrease, whereas if it is too large, the denseness of the fired body may decrease.
[0079] [Organic solvent (E)] The conductive composition of the present invention may further contain an organic solvent (E). The organic solvent (E) is not particularly limited, and may be an organic compound that imparts appropriate viscosity to the conductive composition (particularly a paste-like composition) and can be easily volatilized by drying treatment after the conductive composition is applied to a substrate, and may be a high-boiling organic solvent.
[0080] Examples of such organic solvents include aromatic hydrocarbons (paraxylene, ethylbenzene, trimethylbenzene, naphthalene, cumene, indene, etc.), aliphatic hydrocarbons (hexane, heptane, octane, nonane, etc.), esters (ethyl lactate, texanol, etc.), ketones (isophorone, etc.), amides (dimethylformamide, etc.), aliphatic alcohols (ethanol, isopropanol, butanol, octanol, 2-ethylhexanol, decanol, diacetone alcohol, etc.), cellosolves (methyl cellosolve, ethyl cellosolve, etc.), cellosolve acetates (ethyl cellosolve acetate, butyl cellosolve acetate, etc.), carbitols (carbitol, methyl carbitol, ethyl carbitol, ethyl carbitol, etc.), and the like. Examples of suitable organic solvents include carbitol acetates (ethyl carbitol acetate, butyl carbitol acetate), aliphatic polyhydric alcohols (ethylene glycol, diethylene glycol, dipropylene glycol, butanediol, triethylene glycol, glycerin, etc.), alicyclic alcohols (e.g., cycloalkanols such as cyclohexanol; terpene alcohols (monoterpene alcohols, etc.) such as α-terpineol and dihydroterpineol), aromatic alcohols (metacresol, etc.), aromatic carboxylic acid esters (dibutyl phthalate, dioctyl phthalate, etc.), and nitrogen-containing heterocyclic compounds (dimethylimidazole, dimethylimidazolidinone, etc.). These organic solvents can be used alone or in combination of two or more.
[0081] Among these organic solvents, from the viewpoint of the fluidity of the conductive composition, aliphatic diol monocarboxylates such as texanol (2,2,4-trimethylpentane-1,3-diol monoisobutyrate), aliphatic alcohols such as octanol, alicyclic alcohols such as terpineol, carbitols such as butyl carbitol, and carbitol acetates such as butyl carbitol acetate are preferred, and a combination of the aliphatic diol monocarboxylates and the carbitol acetates is particularly preferred. When the aliphatic diol monocarboxylates and the carbitol acetates are combined, the mass ratio of the two is the former / the latter=99 / 1 to 10 / 90, preferably 90 / 10 to 30 / 70, and more preferably 80 / 20 to 50 / 50 (particularly 75 / 25 to 60 / 40). Furthermore, from the viewpoint of improving reliability, the organic solvent is preferably a hydrocarbon such as a petroleum-based hydrocarbon (or mineral spirits) such as an aromatic hydrocarbon or an aliphatic hydrocarbon.
[0082] The ratio of the organic solvent (E) can be selected from the range of about 0.01 to 50 parts by mass relative to 100 parts by mass of Ag particles (A), and is, for example, about 1 to 30 parts by mass, preferably 3 to 20 parts by mass, more preferably 5 to 15 parts by mass, and most preferably about 8 to 13 parts by mass. When the organic solvent (E) contains a petroleum-based hydrocarbon, the ratio of the petroleum-based hydrocarbon is, for example, 0.01 to 30 parts by mass, preferably 0.05 to 20 parts by mass, more preferably 0.1 to 10 parts by mass, more preferably 0.5 to 5 parts by mass, and most preferably 1 to 3 parts by mass relative to 100 parts by mass of Ag particles (A). If the ratio of the organic solvent (E) is too small, the viscosity of the conductive composition may increase, and the handling property and reliability may decrease, and conversely, if it is too large, the denseness of the fired body may decrease.
[0083] [Other metal-containing components (F)] The conductive composition of the present invention may further contain a metal-containing component (other metal-containing component) (F) other than the Ag particles (A), the metal component (B), and the glass particles (C).
[0084] Examples of the other metal-containing component (F) include metal components (metal elements, metal compounds) of metal elements selected from the group consisting of Pd, Al, Ni, Mo, W, Pt, Au, Co, Ti, Zr, Sn, etc., Ag compounds, alloys or composite metal compounds of two or more metal elements selected from the above group and Ag, Mn, Fe, Cu, etc.
[0085] The shapes of the other metal-containing components, including the preferred embodiments, are the same as those of the Ag small particles (A1).
[0086] The particle size of the particles formed by the other metal-containing component (F) is not particularly limited and can be selected from the range of about 0.5 to 30 μm as the median particle size (D50), and the median particle size is, for example, about 1 to 10 μm, preferably about 1 to 4 μm, and more preferably about 1.5 to 3 μm (particularly about 1.5 to 2.5 μm). If the median particle size is too small, there is a risk that the adhesion to the ceramic substrate will decrease, and conversely, if it is too large, there is a similar risk that the adhesion will decrease.
[0087] The proportion of the other metal-containing component (F), calculated as the metal element, may be about 5 parts by mass or less (for example, 0.01 to 5 parts by mass) per 100 parts by mass of the Ag particles (A).
[0088] [Conventional additives] The conductive composition of the present invention may further contain conventional additives within a range that does not impair the effects of the present invention. Examples of conventional additives include curing agents (such as curing agents for acrylic resins), colorants (such as dyes and pigments), hue improvers, dye fixing agents, gloss imparting agents, metal corrosion inhibitors, stabilizers (such as antioxidants and ultraviolet absorbers), surfactants or dispersants (such as anionic surfactants, cationic surfactants, nonionic surfactants, and amphoteric surfactants), dispersion stabilizers, viscosity modifiers or rheology modifiers, moisturizing agents, thixotropic agents, leveling agents, defoamers, bactericides, and fillers. These other components can be used alone or in combination of two or more. The total ratio of conventional additives can be selected depending on the type of component, and is usually about 10 parts by mass or less (for example, 0.01 to 10 parts by mass) relative to 100 parts by mass of Ag particles (A).
[0089] [Method of preparing conductive composition] The conductive composition (or conductive paste) of the present invention can be prepared by mixing the components using a conventional mixer to uniformly disperse the components, or by using a device with a grinding function (e.g., a three-roll mill, a mortar, a mill, etc.). The components can be added in one batch and mixed, or in separate batches and mixed.
[0090] In the present invention, from the viewpoint of improving plating resistance, it is preferable to add at least one selected from the group consisting of the Mn component (B1), the Fe component (B2) and the Cu component (B3) in the form of a liquid composition.
[0091] [Metallized substrate and its manufacturing method] The metallized substrate (ceramic substrate with conductive portion such as a wiring circuit board) of the present invention is obtained through an adhesion step of adhering the conductive composition to a ceramic substrate, and a firing step of firing the conductive composition adhered to the ceramic substrate to form a conductive portion.
[0092] In the present invention, in terms of improving reliability, when the metal component (B) contains an organometallic compound, the organometallic compound may be added in the form of a liquid composition, it is more preferable to add at least one selected from the group consisting of the Mn component (B1), the Fe component (B2) and the Cu component (B3) in the form of a liquid composition, and it is particularly preferable to add at least the Mn component (B1) in the form of a liquid composition.
[0093] In the adhesion process, the method of adhering the conductive composition can be selected depending on the type of metallized substrate. In the case of surface metallized substrates and through-hole wall metallized substrates, the conductive composition may be applied to the surface of the substrate or the inner walls of the through holes (through holes). In the case of via-filled substrates, the conductive composition may be filled into the front and back through holes (via filling).
[0094] As a method for forming a coating film using a conductive composition, a conventional coating method, such as a flow coating method, a dispenser coating method, a spin coating method, a spray coating method, a screen printing method, a flexographic printing method, a casting method, a bar coating method, a curtain coating method, a roll coating method, a gravure coating method, a dipping method, a slit method, a photolithography method, an inkjet method, etc., can be used. In the coating method, a pattern may be formed (drawn) with the coating film, and a pattern (sintered film, metal film, sintered body layer, conductor layer) can be formed by drying the formed pattern (drawn pattern). The drawing method (or printing method) for drawing a pattern (coating layer) is not particularly limited as long as it is a printing method capable of forming a pattern, and examples thereof include a screen printing method, an inkjet printing method, an intaglio printing method (e.g., a gravure printing method, etc.), an offset printing method, an intaglio offset printing method, and a flexographic printing method. Among these, a screen printing method is preferred.
[0095] Examples of materials for the ceramic substrate include metal oxides (alumina or aluminum oxide, zirconia, sapphire, ferrite, zinc oxide, niobium oxide, mullite, beryllia, etc.), silicon oxides (quartz, silicon dioxide, etc.), metal nitrides (aluminum nitride, titanium nitride, etc.), silicon nitride, boron nitride, carbon nitride, metal carbides (titanium carbide, tungsten carbide, etc.), silicon carbide, boron carbide, metal double oxides [metal titanates (barium titanate, strontium titanate, lead titanate, niobium titanate, calcium titanate, magnesium titanate, etc.), metal zirconates (barium zirconate, calcium zirconate, lead zirconate, etc.)], etc. These ceramics can be used alone or in combination of two or more.
[0096] Among these ceramic substrates, from the viewpoint of high reliability in the electrical and electronic fields, an alumina substrate, an alumina-zirconia substrate, an aluminum nitride substrate, a silicon nitride substrate, and a silicon carbide substrate are preferred, an alumina substrate, an aluminum nitride substrate, and a silicon nitride substrate are more preferred, and an alumina substrate is most preferred.
[0097] The thickness of the ceramic substrate may be appropriately selected depending on the application, and may be, for example, about 0.001 to 10 mm, preferably 0.01 to 5 mm, and more preferably 0.05 to 3 mm (particularly 0.1 to 1 mm).
[0098] The firing atmosphere is preferably air. The firing temperature may be any temperature higher than the softening point of the glass particles in the conductive composition, and is, for example, about 600 to 1100° C., preferably about 700 to 1000° C., and more preferably about 800 to 950° C. The firing time is, for example, about 1 minute to 3 hours, preferably about 10 minutes to 2 hours, and more preferably about 30 minutes to 1.5 hours.
[0099] The firing may be carried out using a batch furnace or a belt conveying type tunnel furnace.
[0100] The metallized substrate of the present invention has excellent electrical conductivity, and the resistivity of the conductive portion may be 3 μΩ·cm or less (for example, 1 to 3 μΩ·cm). EXAMPLES
[0101] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. In the following examples, the materials used in the examples, the evaluation substrates obtained in the examples, and the evaluation methods of the obtained substrates are shown below.
[0102] [Materials used] (Ag particles) Ag particle a: spherical, particle size distribution (D10~D90) 0.42~1.24μm, 10% particle size (D10) 0.42μm, center particle size (D50) 0.5μm, 90% particle size (D90) 1.24μm, maximum particle size 4.63μm, specific surface area 1.3m 2 / g Ag particle b: spherical, particle size distribution (D10~D90) 1.2~3.1μm, 10% particle size (D10) 1.2μm, center particle size (D50) 2μm, 90% particle size (D90) 3.1μm, maximum particle size 7.8μm, specific surface area 0.4m 2 / g Ag particle c: flake-shaped, central particle size (D50): approx. 6 μm Ag particles: flake-shaped, median particle size (D50): approx. 1.1 μm, specific surface area: 1.6 m 2 / g
[0103] (Metal Components) Copper (Cu) particles: spherical, center particle diameter (D50) 3μm Copper oxide (CuO) particles: purity 3N, average particle size approximately 1μm Cu naphthenate: Copper naphthenate solution in mineral spirits, Cu content 8% by mass Iron oxide (Fe 2 O 3 ) Particles: Purity 2N, average particle size approximately 1μm Fe octylate: Ferrous octylate mineral spirits solution, Fe content 6% by mass Manganese oxide (MnO) particles: purity 3N, average particle size approximately 1μm Mn octylate: Manganese(II) octylate solution in mineral spirits, Mn content 8% by mass
[0104] (glass particles) Bismuth-based glass particles: composition Bi 2 O 3 -ZnO-B 2 O 3 , softening temperature 488℃ Zinc-based glass particles: composition ZnO-SiO 2 -B 2 O 3 -R 2 O, softening temperature 575℃ Silica-based glass particles: composition SiO 2 -B 2 O 3 -R 2 O, softening temperature 780℃.
[0105] (Resin component) Ethyl cellulose: "STD20" manufactured by The Dow Chemical Company.
[0106] [Preparation of evaluation board] Conductive pastes of Examples 1 to 17 and Comparative Examples 1 to 15 were prepared with the compositions shown in Tables 1 to 6. The pastes were prepared by mixing an organic vehicle in which 10% by mass of ethyl cellulose was dissolved in a mixed solvent of Texanol / Butyl Carbitol Acetate = 55 / 35 (mass ratio) with the inorganic components shown in Tables 1 to 6. At that time, the solid content concentration of the inorganic components in the conductive paste was adjusted to 87% by mass. Then, using the prepared paste, electrodes were formed by screen printing on an alumina substrate of 3 inches x 3 inches x 0.635 mm thick, and the electrodes were fired at 900°C in air to prepare an evaluation substrate.
[0107] [Resistivity] The resistivity was calculated from the surface resistance measured by a four-probe method and the film thickness. Ten samples of the conductive films obtained in the examples and comparative examples were measured, and the average value was calculated.
[0108] [Plating resistance, initial adhesive strength] After electroless plating (Ni / Pd / Au), the adhesion was evaluated on the 2 mm square pad pattern. A tin-plated soft copper wire (peel wire) was soldered along the surface of the 2 mm square pad.
[0109] The soft copper wire was bent vertically upward at the end of the pad, fixed to a tensile tester, and pulled up until the pad peeled off from the board. The highest load when the pad peeled off from the board was recorded as the peel strength (peel strength of 2mm square pattern) and was taken as the initial adhesive strength. A peel strength of 3.0kgf or more means that the peel strength per 1mm square pattern is 0.75kgf or more, and if the electrode peeled off just by lifting the copper wire, it was taken as 0kgf.
[0110] [Initial judgment] The results of the above plating resistance evaluation test (initial adhesive strength) were initially judged and ranked according to the following criteria.
[0111] Rank A: Initial adhesive strength is 3.0 kgf or more. Rank B: Initial adhesive strength is 2.0kgf or more and less than 3.0kgf Rank C: The initial adhesive strength is less than 2.0 kgf.
[0112] For the substrates that passed the initial judgment, the following reliability evaluation was carried out to evaluate the adhesive strength.
[0113] [Constant temperature and humidity test] In the constant temperature and humidity test, the sample was left in a constant temperature and humidity chamber at a temperature of 85° C. and a relative humidity of 85% RH for 1000 hours, after which the adhesion (bonding strength) of the fired film was measured and rated according to the following criteria.
[0114] ◎: 2.5kgf or more ○: 2.0kgf or more and less than 2.5kgf ×: Less than 2.0kgf.
[0115] [Heat cycle test] The adhesive strength after 1000 cycles of -40°C / 125°C was measured and rated according to the following criteria.
[0116] ◎: 2.5kgf or more ○: 2.0kgf or more and less than 2.5kgf ×: Less than 2.0kgf.
[0117] [Heat aging test] After 1000 hours in an oven at 170°C, the adhesive strength was measured and rated according to the following criteria.
[0118] ◎: 2.5kgf or more ○: 2.0kgf or more and less than 2.5kgf ×: Less than 2.0kgf.
[0119] [Overall Judgment] The results of the above evaluation tests were comprehensively judged and ranked according to the following criteria.
[0120] Rank A: All reliability tests are ◎ or 〇 (passed) Rank B: All reliability tests are ○ (passed) Rank C: There is an × in the reliability test, or the initial judgment is Rank C (failed).
[0121] Tables 1 to 6 also show the evaluation results of the evaluation substrates obtained in Examples 1 to 17 and Comparative Examples 1 to 15.
[0122] [Table 1]
[0123] [Table 2]
[0124] [Table 3]
[0125] [Table 4]
[0126] [Table 5]
[0127] [Table 6]
[0128] The details of the ratios (mass %) shown in Tables 1 to 6 are as follows.
[0129] The "ratio of metal component (B) to Ag particles (A)" means the ratio (mass %) of metal component (B) to Ag particles (A) (i.e., the total amount of Ag particles a and Ag particles b) in terms of metal element (parts by mass of metal element contained in metal component (B) per 100 parts by mass of the total amount of Ag particles a and Ag particles b).
[0130] The "proportion of metal component (B) in the inorganic components" means the proportion (mass %) of metal component (B) in terms of metal element relative to the total amount of Ag particles (A), metal component (B), and glass particles (C) in terms of metal elements.
[0131] The "proportion of Mn component (B1) in metal component (B)" means the proportion (mass%) of Mn component (B1) calculated as a metal element relative to metal component (B) (i.e., the total amount of Mn component (B1), Fe component (B2) and Cu component (B3) calculated as a metal element). The same applies to the proportions of Fe component (B2) and Cu component (B3).
[0132] "The ratio of glass particles (C) to Ag particles (A)" means the parts by mass of glass particles (C) relative to 100 parts by mass of Ag particles (A).
[0133] The "proportion of glass particles (C) in the inorganic component" means the proportion (mass%) of glass particles (C) to the total amount of Ag particles (A), metal component (B), and glass particles (C) calculated as metal elements.
[0134] As is clear from the results of Tables 1 and 2, when the material contained small Ag particles (A1) and large Ag particles (A2) and also contained all three components, Mn component (B1), Fe component (B2), and Cu component (B3), excellent plating resistance (adhesion) was obtained in the initial plating resistance and reliability evaluation (Examples 1 to 3). Among them, the properties of Examples 1 and 2, in which the ratio of small Ag particles (A1) in the Ag particles exceeds 5 mass%, were excellent, and Example 1 was the most excellent.
[0135] The results of Example 1, which had the best balance of properties, are shown not only in Table 1 but also in Tables 3, 5 and 6 for comparison.
[0136] On the other hand, when the alloy contained all three components, Mn (B1), Fe (B2), and Cu (B3) (and one of the components was a metal carboxylate), but only one of small Ag particles (A1) and large Ag particles (A2), the initial plating resistance was judged to be B or higher, but the alloy failed the reliability evaluation (Comparative Examples 1 to 7).
[0137] Comparative Examples 8 and 9 are also examples containing only one of small Ag particles (A1) and large Ag particles (A2), and containing all three components, Mn (B1), Fe (B2), and Cu (B3), but no carboxylate metal salt. Similarly, although the initial plating resistance test was passed, the reliability test was failed. Comparative Examples 8 and 9 have a similar composition to the paste disclosed in Patent Document 4.
[0138] Tables 3 and 4 show examples (Examples 4 to 9) in which the combination of the Mn component (B1), Fe component (B2), and Cu component (B3) was changed from Example 1, which gave good results in Table 1. All of these examples are examples in which at least one of the three metal components contains a metal carboxylate, and all of the examples showed excellent plating resistance (adhesion) in the initial plating resistance evaluation and reliability evaluation. Among them, Example 1, which contains one type of manganese octylate, was excellent.
[0139] On the other hand, even when the Ag small particles (A1) and the Ag large particles (A2) were included, Comparative Examples 10 and 11, which contained only two of the Mn component (B1), Fe component (B2), and Cu component (B3), passed the initial plating resistance test, but failed the reliability test. Comparative Example 12 failed the plating resistance test because the electrodes did not adhere at all. Furthermore, Comparative Examples 13 to 15, which contained only one of the Mn component (B1), Fe component (B2), and Cu component (B3), also failed the plating resistance test because the electrodes did not adhere at all.
[0140] As is clear from the results in Table 5, the results of Examples 10 and 11 in which the ratio (total amount) of the three metal components to the Ag particles was changed compared to Example 1 show that the ratio is preferably about 0.5 to 5.0 mass%.
[0141] In addition, in Examples 12 and 13 in which the distribution ratio of the Mn compound (B1), the Fe compound (B2), and the Cu compound (B3) was changed from that of Example 1, the same results as in Example 1 were obtained, but in terms of reliability, Example 1 was the best.
[0142] As is clear from the results in Table 6, compared to Example 1, Example 14, which uses zinc-based glass particles, and Example 15, which uses silica-based glass particles, also obtained results equivalent to those of Example 1, but the bismuth-based glass and zinc-based glass were particularly excellent.
[0143] Furthermore, in Examples 16 and 17 in which the amount of glass particles was reduced and increased compared to Example 1, results equivalent to those of Example 1 were obtained. However, in Example 16 in which the amount of glass particles was reduced, the adhesive strength after the heat aging test was slightly decreased, and in Example 17 in which the amount of glass particles was increased, the adhesive strength after the heat cycle test was slightly decreased. [Industrial Applicability]
[0144] The conductive composition of the present invention can be used for circuit boards, electronic components, thermal substrates, substrates for LED packages, substrates for semiconductors, thin film circuit substrates, substrates for resistors, etc., and can be particularly effectively used as a composition for forming conductive parts such as electrodes in wiring circuit boards.
Claims
1. A conductive composition comprising Ag particles (A), a metal component (B) and glass particles (C), the Ag particles (A) are small Ag particles (A1) and large Ag particles (A2); a mass ratio of the small Ag particles (A1) to the large Ag particles (A2) is 99 / 1 to 30 / 70; the small Ag particles (A1) are spherical or regular polyhedral particles having a maximum particle size of less than 1.2 μm, and the large Ag particles (A2) are spherical or regular polyhedral particles having a minimum particle size of 1.2 μm or more, In the small Ag particles (A1) and the large Ag particles (A2), the ratio of the major axis to the minor axis of the spherical particles is 1 to 2; The Ag small particles (A1) have a median particle size (D50) of 0.4 μm or more, The metal component (B) is a Mn component (B1), an Fe component (B2) and a Cu component (B3), and The conductive composition, wherein at least one selected from the group consisting of the Mn component (B1), the Fe component (B2) and the Cu component (B3) is an organometallic compound.
2. 2. The conductive composition according to claim 1, wherein the large Ag particles (A2) are spherical particles having a median particle size (D50) of 1.3 to 10 μm.
3. 3. The conductive composition according to claim 1, wherein a mass ratio of the small Ag particles (A1) to the large Ag particles (A2) is 90 / 10 to 30 / 70.
4. 4. The conductive composition according to claim 1, wherein the glass particles (C) contain bismuth-based glass particles and / or zinc-based glass particles.
5. The method for producing a conductive composition according to any one of claims 1 to 4, wherein at least one selected from the group consisting of the Mn component (B1), the Fe component (B2), and the Cu component (B3) is added in the form of a liquid composition.
6. A method for producing a metallized substrate, comprising: an attachment step of attaching the conductive composition according to any one of claims 1 to 4 to a ceramic substrate; and a firing step of firing the conductive composition attached to the ceramic substrate to form a conductive portion.
7. The method according to claim 6, wherein the conductive composition is fired in air in the firing step.
8. A metallized substrate obtained by the method according to claim 6 or 7.
9. 9. The metallized substrate according to claim 8, wherein the ceramic substrate is an alumina substrate, an alumina-zirconia substrate, an aluminum nitride substrate, a silicon nitride substrate or a silicon carbide substrate.
Citation Information
Patent Citations
Electrically conductive coating
JP1980149356A
Conductive composition
JP1997092028A
Conductive paste
JP2003115216A
Silver paste and electronic element
JP2018055883A
Conductive paste, chip electronic component and method for producing the same