Adhesive sheet
The adhesive sheet with ultraviolet absorber and active energy ray-curable adhesive addresses the issues of additional cleaning steps and laser damage by enabling damage-free, low-power laser-assisted peeling.
Patent Information
- Application Number
- JP2020090616
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-03-25
- Filing Date
- 2020-05-25
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2040-05-25
AI Technical Summary
Existing methods for temporarily fixing members using adhesive sheets require additional steps for removing the adhesive layer and cleaning the member, and high-power laser irradiation can damage the member.
An adhesive sheet containing an ultraviolet absorber and active energy ray-curable adhesive with specific light transmittance and haze values, allowing for peeling without high-power laser irradiation and eliminating the need for cleaning.
The adhesive sheet enables releasable fixation without laser-induced damage and avoids post-peeling cleaning steps, ensuring effective and damage-free removal of adherends.
Smart Images

Figure 0007566490000002 
Figure 0007566490000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a pressure-sensitive adhesive sheet. [Background technology]
[0002] When processing various members such as electronic components, it is common to temporarily fix the member to a support using an adhesive sheet, and after processing, peel the processed member from the support. For example, Patent Document 1 describes a method in which a substrate (workpiece) is processed in a state where it is temporarily fixed to a support via an adhesive layer and a separation layer, and after processing, the separation layer is destroyed by irradiating it with laser light, and the substrate together with the adhesive layer is peeled off from the support, and then the adhesive layer is removed from the substrate. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Patent No. 5875850 Summary of the Invention [Problem to be solved by the invention]
[0004] However, the above method requires a process of removing the adhesive layer from the member and cleaning the non-adhesive surface of the member, which is problematic in terms of production cost, and there is also a problem that the member may be damaged when irradiated with a high-power laser beam.
[0005] The present invention has been made to solve the above-mentioned problems in the conventional art, and an object of the present invention is to provide an adhesive sheet that can temporarily and removably fix an adherend, which does not require irradiation with high-power laser light during peeling, and which can eliminate the need for a step of cleaning the adherend after peeling. [Means for solving the problem]
[0006] The pressure-sensitive adhesive sheet of the present invention is an adhesive sheet comprising an adhesive layer containing an ultraviolet absorber and an active energy ray-curable adhesive, and the pressure-sensitive adhesive sheet has a light transmittance of 50% or less at a wavelength of 355 nm. In one embodiment, the pressure-sensitive adhesive layer has a thickness of 20 μm or less. In one embodiment, the pressure-sensitive adhesive sheet has a visible light transmittance of 50% or more. In one embodiment, the pressure-sensitive adhesive sheet has a haze value of 70% or less. In one embodiment, the active energy ray-curable pressure-sensitive adhesive further contains a photopolymerization initiator and a photosensitizer. In one embodiment, the ultraviolet absorber has a 5% weight loss temperature of 350° C. or lower. In one embodiment, the pressure-sensitive adhesive layer further comprises particles. Effect of the Invention
[0007] According to the present invention, it is possible to provide an adhesive sheet that can temporarily fix an adherend in a releasable manner, which does not require irradiation with high-power laser light during peeling, and which can eliminate the need for a step of cleaning the adherend after peeling. [Brief description of the drawings]
[0008] [Figure 1] 1(a) is a schematic cross-sectional view of a pressure-sensitive adhesive sheet according to one embodiment of the present invention, and (b) is a schematic cross-sectional view of a pressure-sensitive adhesive sheet according to another embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] A. Overview of adhesive sheets FIG. 1(a) is a schematic cross-sectional view of a pressure-sensitive adhesive sheet according to one embodiment of the present invention. The pressure-sensitive adhesive sheet 100 according to this embodiment includes a pressure-sensitive adhesive layer 10. The pressure-sensitive adhesive layer 10 includes an active energy ray-curable pressure-sensitive adhesive and an ultraviolet absorbing agent. FIG. 1(b) is a schematic cross-sectional view of a pressure-sensitive adhesive sheet according to one embodiment of the present invention. The pressure-sensitive adhesive sheet 200 according to this embodiment further includes a substrate 20, and the pressure-sensitive adhesive layer 20 is disposed on at least one side of the substrate 20. Although not shown, the pressure-sensitive adhesive sheet of the present invention may be provided with a release liner on the outside of the pressure-sensitive adhesive layer for the purpose of protecting the adhesive surface until it is used. The pressure-sensitive adhesive sheet may further include any other appropriate layers as long as the effects of the present invention can be obtained. In one embodiment, the pressure-sensitive adhesive sheet of the present invention is composed of only one pressure-sensitive adhesive layer as shown in FIG. 1(a). In another embodiment, the pressure-sensitive adhesive sheet of the present invention includes a substrate and a pressure-sensitive adhesive layer as shown in FIG. 1(b), and the pressure-sensitive adhesive layer is disposed directly on the substrate (i.e., without any other layers). In the present invention, as described below, the adhesive strength of the adhesive layer is reduced and the adhesive layer is deformed, enabling the adherend to be peeled off easily. Therefore, it is possible to construct an adhesive sheet without providing a layer other than the adhesive layer (a so-called separation layer) for separating the adherend from the adhesive sheet.
[0010] In the present invention, the adhesive layer contains an ultraviolet absorber, so that the adherend can be peeled off by irradiation with laser light. More specifically, by irradiating the adhesive layer with laser light, the adhesive layer is deformed by gas generated by decomposition of the ultraviolet absorber, and / or gas generated by decomposition of the adhesive layer due to heat generated by the ultraviolet absorber, and as a result, releasability is expressed in the part irradiated with the laser light. According to the present invention, since deformation can be generated in a minute range as described above, the adherend can be favorably peeled off even when the small adherend is processed. In addition, even if a small adherend that needs to be peeled off and a small adherend that does not need to be peeled off are temporarily fixed adjacent to each other, only the small adherend that needs to be peeled off can be peeled off, and unnecessary detachment of the small adherend can also be prevented.
[0011] Furthermore, the present invention is characterized in that the adhesive layer contains an active energy ray curable adhesive. In such an adhesive sheet of the present invention, the adhesive strength of the entire adhesive layer is reduced by irradiating active energy rays. After irradiating the entire adhesive layer of the adhesive sheet to which the adherend is attached with active energy rays to reduce the adhesive strength, the adhesive residue after peeling can be prevented by irradiating the laser light as described above. By using such an adhesive sheet, cleaning of the adherend after peeling can be omitted. In addition, by forming an adhesive layer containing an active energy ray curable adhesive, the laser output during peeling can be reduced. Since the adhesive sheet of the present invention exhibits peelability with low-output laser light, the use of the adhesive sheet can reduce damage to the adherend during peeling and prevent breakage of the adherend. Examples of active energy rays include gamma rays, ultraviolet rays, visible light, infrared rays (heat rays), radio waves, alpha rays, beta rays, electron beams, plasma flow, ionizing rays, particle beams, and the like. Preferably, ultraviolet rays.
[0012] The light transmittance of the pressure-sensitive adhesive sheet of the present invention at a wavelength of 355 nm is 50% or less. In the present invention, by reducing the light transmittance, the laser output during peeling can be reduced. Since the pressure-sensitive adhesive sheet of the present invention exhibits peelability with a low-power laser beam, the use of the pressure-sensitive adhesive sheet can reduce damage to the adherend during peeling and prevent breakage of the adherend. The light transmittance of the pressure-sensitive adhesive sheet of the present invention at a wavelength of 355 nm is preferably 40% or less, more preferably 30% or less. Within such a range, the above effect becomes more pronounced. The light transmittance of the pressure-sensitive adhesive sheet is the light transmittance in the thickness direction of the pressure-sensitive adhesive sheet, and is the light transmittance measured for all the constituent layers of the pressure-sensitive adhesive sheet. In the present invention, the light transmittance of the pressure-sensitive adhesive sheet at a wavelength of 355 nm can be controlled by adjusting the content ratio of the ultraviolet absorber contained in the pressure-sensitive adhesive layer.
[0013] The visible light transmittance of the pressure-sensitive adhesive sheet of the present invention is preferably 50% or more, more preferably 60% or more, and even more preferably 70% or more.Within such a range, a pressure-sensitive adhesive sheet can be obtained that allows the adherend to be peeled off to be easily visible through the pressure-sensitive adhesive sheet when the adherend is peeled off by laser light irradiation.The higher the visible light transmittance of the pressure-sensitive adhesive sheet, the more preferable it is, and the upper limit is, for example, 95% (preferably 100%).
[0014] The haze value of the pressure-sensitive adhesive sheet of the present invention is preferably 70% or less, more preferably 65% or less.Within this range, when the adherend is peeled off by laser light irradiation, the pressure-sensitive adhesive sheet can be obtained that allows the adherend to be peeled off to be easily visible through the pressure-sensitive adhesive sheet.The lower the haze value of the pressure-sensitive adhesive sheet, the more preferable, and the lower limit is, for example, 0.1%.
[0015] The initial adhesive strength at 23°C when the adhesive sheet of the present invention is attached to a stainless steel plate is preferably 0.1N / 20mm to 15N / 20mm, more preferably 0.5N / 20mm to 10N / 20mm. Within such a range, an adhesive sheet capable of holding an adherend well can be obtained. The adhesive strength is measured in accordance with JIS Z 0237:2000. Specifically, the adhesive sheet is attached to a stainless steel plate (arithmetic mean surface roughness Ra: 50±25nm) by one reciprocation of a 2kg roller, and left at 23°C for 30 minutes, and then peeled off the adhesive sheet at a peel angle of 180° and a peel speed (pulling speed) of 300mm / min to measure. The adhesive strength of the adhesive layer changes when irradiated with active energy rays and laser light, but in this specification, the "initial adhesive strength" means the adhesive strength before irradiation with active energy rays and laser light.
[0016] In one embodiment, the adhesive sheet is attached to a silicon mirror wafer and 460 mJ / cm 2The adhesive strength at 23°C after irradiation with ultraviolet light is preferably 0.01N / 20mm to 0.3N / 20mm, and more preferably 0.02N / 20mm to 0.2N / 20mm. If the adhesive strength is within such a range, an adhesive sheet with little adhesive residue can be obtained. The ultraviolet light irradiation can be performed, for example, by using an ultraviolet light irradiation device (manufactured by Nitto Seiki Co., Ltd., product name "UM-810") to irradiate the adhesive with ultraviolet light from a high-pressure mercury lamp (characteristic wavelength: 365nm, integrated light quantity: 460mJ / cm2). 2 , Irradiation energy: 70W / cm 2 The adhesive layer is irradiated with UV light (irradiation time: 6.6 seconds).
[0017] The thickness of the pressure-sensitive adhesive sheet is preferably from 1 μm to 300 μm, and more preferably from 5 μm to 200 μm.
[0018] B.Adhesive layer The thickness of the pressure-sensitive adhesive layer is preferably 20 μm or less. If it is within this range, it is possible to further reduce the laser output during peeling, and it is possible to obtain a pressure-sensitive adhesive sheet with excellent peeling properties. The thickness of the pressure-sensitive adhesive layer is more preferably 10 μm or less, even more preferably 8 μm or less, and more preferably 1 μm to 8 μm. If it is within this range, the above effects become more pronounced.
[0019] As described above, the pressure-sensitive adhesive layer contains an active energy ray-curable pressure-sensitive adhesive and an ultraviolet absorbing agent.
[0020] (Active energy ray curable adhesive) In one embodiment, an active energy ray curable adhesive (A1) is used as the active energy ray curable adhesive, which includes a base polymer as a base material and an active energy ray reactive compound (monomer or oligomer) that can be bonded to the base polymer. In another embodiment, an active energy ray curable adhesive (A2) is used, which includes an active energy ray reactive polymer as the base polymer. Preferably, the base polymer has a functional group that can react with a photopolymerization initiator. Examples of the functional group include a hydroxyl group and a carboxyl group.
[0021] Examples of the base polymer used in the pressure sensitive adhesive (A1) include rubber-based polymers such as natural rubber, polyisobutylene rubber, styrene-butadiene rubber, styrene-isoprene-styrene block copolymer rubber, reclaimed rubber, butyl rubber, polyisobutylene rubber, and nitrile rubber (NBR); silicone-based polymers; and acrylic-based polymers. These polymers may be used alone or in combination of two or more. Among them, acrylic polymers are preferred.
[0022] Examples of the acrylic polymer include homopolymers or copolymers of hydrocarbon group-containing (meth)acrylic acid esters such as (meth)acrylic acid alkyl esters, (meth)acrylic acid cycloalkyl esters, and (meth)acrylic acid aryl esters; copolymers of the hydrocarbon group-containing (meth)acrylic acid esters and other copolymerizable monomers. Examples of the (meth)acrylic acid alkyl esters include the methyl ester, ethyl ester, propyl ester, isopropyl ester, butyl ester, isobutyl ester, s-butyl ester, t-butyl ester, pentyl ester, isopentyl ester, hexyl ester, heptyl ester, octyl ester, 2-ethylhexyl ester, isooctyl ester, nonyl ester, decyl ester, isodecyl ester, undecyl ester, dodecyl ester, i.e., lauryl ester, tridecyl ester, tetradecyl ester, hexadecyl ester, octadecyl ester, and eicosyl ester of (meth)acrylic acid. Examples of the (meth)acrylic acid cycloalkyl esters include the cyclopentyl ester and cyclohexyl ester of (meth)acrylic acid. Examples of the (meth)acrylic acid aryl ester include phenyl (meth)acrylate and benzyl (meth)acrylate. The content of the structural unit derived from the above-mentioned hydrocarbon group-containing (meth)acrylic acid ester is preferably 40 parts by weight or more, more preferably 60 parts by weight or more, based on 100 parts by weight of the base polymer.
[0023] Examples of the other copolymerizable monomers include functional group-containing monomers such as carboxy group-containing monomers, acid anhydride monomers, hydroxy group-containing monomers, glycidyl group-containing monomers, sulfonic acid group-containing monomers, phosphoric acid group-containing monomers, acrylamide, and acrylonitrile. Examples of the carboxy group-containing monomers include acrylic acid, methacrylic acid, carboxyethyl (meth)acrylate, carboxypentyl (meth)acrylate, itaconic acid, maleic acid, fumaric acid, and crotonic acid. Examples of the acid anhydride monomers include maleic anhydride and itaconic anhydride. Examples of the hydroxy group-containing monomers include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 10-hydroxydecyl (meth)acrylate, 12-hydroxylauryl (meth)acrylate, and (4-hydroxymethylcyclohexyl)methyl (meth)acrylate. Examples of the glycidyl group-containing monomer include glycidyl (meth)acrylate and methyl glycidyl (meth)acrylate. Examples of the sulfonic acid group-containing monomer include styrene sulfonic acid, allyl sulfonic acid, 2-(meth)acrylamido-2-methylpropanesulfonic acid, (meth)acrylamidopropanesulfonic acid, sulfopropyl (meth)acrylate, and (meth)acryloyloxynaphthalenesulfonic acid. Examples of the phosphoric acid group-containing monomer include 2-hydroxyethyl acryloyl phosphate. Examples of the acrylamide include N-acryloylmorpholine. These may be used alone or in combination of two or more. The content ratio of the constitutional unit derived from the above copolymerizable monomer is preferably 60 parts by weight or less, more preferably 40 parts by weight or less, based on 100 parts by weight of the base polymer.
[0024] The acrylic polymer may contain a structural unit derived from a polyfunctional monomer to form a crosslinked structure in the polymer skeleton. Examples of the polyfunctional monomer include hexanediol di(meth)acrylate, (poly)ethylene glycol di(meth)acrylate, (poly)propylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, pentaerythritol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, dipentaerythritol hexa(meth)acrylate, epoxy(meth)acrylate (i.e., polyglycidyl(meth)acrylate), polyester(meth)acrylate, and urethane(meth)acrylate. These may be used alone or in combination of two or more. The content ratio of the structural unit derived from the polyfunctional monomer is preferably 40 parts by weight or less, more preferably 30 parts by weight or less, based on 100 parts by weight of the base polymer.
[0025] The weight average molecular weight of the acrylic polymer is preferably from 100,000 to 3,000,000, and more preferably from 200,000 to 2,000,000. The weight average molecular weight can be measured by GPC (solvent: THF).
[0026] Examples of the active energy ray reactive compound that can be used in the pressure-sensitive adhesive (A1) include photoreactive monomers or oligomers having a functional group having a polymerizable carbon-carbon multiple bond, such as an acryloyl group, a methacryloyl group, a vinyl group, an allyl group, or an acetylene group. Specific examples of the photoreactive monomer include esters of (meth)acrylic acid and polyhydric alcohols such as trimethylolpropane tri(meth)acrylate, tetramethylolmethane tetra(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol monohydroxypenta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, and polyethylene glycol di(meth)acrylate; polyfunctional urethane (meth)acrylate; epoxy (meth)acrylate; oligoester (meth)acrylate, etc. Also, monomers such as methacryloylisocyanate, 2-methacryloyloxyethyl isocyanate (2-isocyanatoethyl methacrylate), and m-isopropenyl-α,α-dimethylbenzyl isocyanate may be used. Specific examples of the photoreactive oligomer include dimers to pentamers of the above-mentioned monomers, etc. The molecular weight of the photoreactive oligomer is preferably 100 to 3,000.
[0027] Furthermore, as the active energy ray reactive compound, monomers such as epoxidized butadiene, glycidyl methacrylate, acrylamide, vinyl siloxane, etc., or oligomers composed of such monomers may be used.
[0028] Furthermore, the active energy ray reactive compound may be a mixture of an organic salt such as an onium salt and a compound having multiple heterocycles in the molecule. The organic salt of the mixture is cleaved by irradiation with active energy rays (e.g., ultraviolet rays, electron beams) to generate ions, which act as initiating species to cause a ring-opening reaction of the heterocycle to form a three-dimensional network structure. Examples of the organic salt include iodonium salts, phosphonium salts, antimonium salts, sulfonium salts, and borate salts. Examples of the heterocycle in the compound having multiple heterocycles in the molecule include oxirane, oxetane, oxolane, thiirane, and aziridine.
[0029] In the above pressure-sensitive adhesive (A1), the content of the active energy ray-reactive compound is preferably 0.1 to 500 parts by weight, more preferably 5 to 300 parts by weight, and even more preferably 40 to 150 parts by weight, relative to 100 parts by weight of the base polymer.
[0030] Examples of the active energy ray reactive polymer (base polymer) contained in the pressure sensitive adhesive (A2) include polymers having functional groups with carbon-carbon multiple bonds such as acryloyl groups, methacryloyl groups, vinyl groups, allyl groups, acetylene groups, etc. Specific examples of the active energy ray reactive polymer include polymers composed of multifunctional (meth)acrylates, photocationic polymerization type polymers, cinnamoyl group-containing polymers such as polyvinyl cinnamate, diazotized amino novolac resins, polyacrylamides, etc.
[0031] In one embodiment, an active energy ray reactive polymer is used, which is constituted by introducing an active energy ray polymerizable carbon-carbon multiple bond into the side chain, main chain and / or main chain end of the acrylic polymer. For example, a method of introducing a radiation polymerizable carbon-carbon double bond into an acrylic polymer includes a method of copolymerizing a raw material monomer including a monomer having a specific functional group (first functional group) to obtain an acrylic polymer, and then subjecting a compound having a specific functional group (second functional group) capable of reacting with and bonding to the first functional group and a radiation polymerizable carbon-carbon double bond to a condensation reaction or addition reaction with the acrylic polymer while maintaining the radiation polymerizability of the carbon-carbon double bond.
[0032] Examples of combinations of the first functional group and the second functional group include a carboxy group and an epoxy group, an epoxy group and a carboxy group, a carboxy group and an aziridyl group, an aziridyl group and a carboxy group, a hydroxy group and an isocyanate group, and an isocyanate group and a hydroxy group. Among these combinations, from the viewpoint of ease of reaction tracking, a combination of a hydroxy group and an isocyanate group, or a combination of an isocyanate group and a hydroxy group is preferred. In addition, while it is technically difficult to prepare a polymer having a highly reactive isocyanate group, from the viewpoint of ease of preparation or availability of an acrylic polymer, it is more preferred that the first functional group on the acrylic polymer side is a hydroxy group and the second functional group is an isocyanate group. In this case, examples of isocyanate compounds having both a radiation-polymerizable carbon-carbon double bond and an isocyanate group as a second functional group include methacryloyl isocyanate, 2-methacryloyloxyethyl isocyanate, and m-isopropenyl-α,α-dimethylbenzyl isocyanate. Moreover, as the acrylic polymer having a first functional group, those containing structural units derived from the above-mentioned hydroxy group-containing monomers are preferable, and those containing structural units derived from ether compounds such as 2-hydroxyethyl vinyl ether, 4-hydroxybutyl vinyl ether, and diethylene glycol monovinyl ether are also preferable.
[0033] The pressure-sensitive adhesive (A2) may further contain the active energy ray-reactive compound (monomer or oligomer).
[0034] The active energy ray-curable pressure-sensitive adhesive may contain a photopolymerization initiator.
[0035] As the photopolymerization initiator, any suitable initiator can be used. As the photopolymerization initiator, for example, α-ketol-based compounds such as 4-(2-hydroxyethoxy)phenyl(2-hydroxy-2-propyl)ketone, α-hydroxy-α,α'-dimethylacetophenone, 2-methyl-2-hydroxypropiophenone, 1-hydroxycyclohexylphenylketone, etc.; acetophenone-based compounds such as methoxyacetophenone, 2,2-dimethoxy-2-phenylacetophenone, 2,2-diethoxyacetophenone, 2-methyl-1-[4-(methylthio)-phenyl]-2-morpholinopropane-1, etc.; benzoin ether-based compounds such as benzoin ethyl ether, benzoin isopropyl ether, anisoin methyl ether, etc.; ketal-based compounds such as benzyl dimethyl ketal, etc. aromatic sulfonyl chloride compounds such as 2-naphthalenesulfonyl chloride; photoactive oxime compounds such as 1-phenone-1,1-propanedione-2-(o-ethoxycarbonyl)oxime; benzophenone compounds such as benzophenone, benzoylbenzoic acid, and 3,3'-dimethyl-4-methoxybenzophenone; thioxanthone compounds such as thioxanthone, 2-chlorothioxanthone, 2-methylthioxanthone, 2,4-dimethylthioxanthone, isopropylthioxanthone, 2,4-dichlorothioxanthone, 2,4-diethylthioxanthone, and 2,4-diisopropylthioxanthone; camphorquinone; halogenated ketones; acylphosphinoxides; acylphosphonates, etc. The amount of the photopolymerization initiator used can be set to any appropriate amount.
[0036] In one embodiment, a photopolymerization initiator having a maximum absorption wavelength in the range of 400 nm or less (preferably 380 nm or less, more preferably 340 nm or less) is used. By using such a photopolymerization initiator, when the adhesive strength of the entire adhesive layer is reduced by irradiation with active energy rays, a curing reaction of the adhesive occurs favorably, and an adhesive sheet with particularly little adhesive residue can be obtained.
[0037] The photopolymerization initiator may be a commercially available product. For example, photopolymerization initiators having a maximum absorption wavelength in the range of 400 nm or less include BASF's product names "Irgacure 127", "Irgacure 369", "Irgacure 369E", "Irgacure 379", "Irgacure 379EG", "Irgacure 819", "Irgacure TOP", "Irgacure 784", "Irgacure OXE01", etc.
[0038] In one embodiment, the active energy ray-curable pressure-sensitive adhesive may contain a photosensitizer.
[0039] In one embodiment, the photosensitizer may be used in combination with the photopolymerization initiator. The photosensitizer can generate radicals from the photopolymerization initiator by transferring the energy obtained by absorbing light to the photopolymerization initiator, so that polymerization can proceed with light on the long wavelength side where the photopolymerization initiator itself does not have an absorption peak. Therefore, by including a photosensitizer, it is possible to increase the difference between the absorption wavelength of the ultraviolet absorber and the wavelength at which radicals can be generated from the photopolymerization initiator. As a result, the photopolymerization of the adhesive layer and the peeling by the ultraviolet absorber can be performed without affecting each other. In one embodiment, 2,2-dimethoxy-1,2-diphenylethan-1-one (for example, BASF, product name "Irgacure 651") as a photopolymerization initiator and a photosensitizer are used in combination. Examples of such photosensitizers include "UVS-581" (trade name, manufactured by Kawasaki Chemical Industries, Ltd.), 9,10-diethoxyanthracene (for example, "UVS1101" (trade name, manufactured by Kawasaki Chemical Industries, Ltd.), and the like.
[0040] Other examples of the photosensitizer include 9,10-dibutoxyanthracene (e.g., Kawasaki Chemical Industries, Ltd., product name "UVS-1331"), 2-isopropylthioxanthone, benzophenone, thioxanthone derivatives, 4,4'-bis(dimethylamino)benzophenone, etc. Examples of thioxanthone derivatives include ethoxycarbonylthioxanthone, isopropylthioxanthone, etc.
[0041] The content of the photosensitizer is preferably 0.01 to 2 parts by weight, and more preferably 0.5 to 2 parts by weight, relative to 100 parts by weight of the base polymer.
[0042] Preferably, the active energy ray-curable pressure-sensitive adhesive contains a crosslinking agent, such as an isocyanate-based crosslinking agent, an epoxy-based crosslinking agent, an oxazoline-based crosslinking agent, an aziridine-based crosslinking agent, a melamine-based crosslinking agent, a peroxide-based crosslinking agent, a urea-based crosslinking agent, a metal alkoxide-based crosslinking agent, a metal chelate-based crosslinking agent, a metal salt-based crosslinking agent, a carbodiimide-based crosslinking agent, or an amine-based crosslinking agent.
[0043] When the pressure-sensitive adhesive layer has a single layer configuration, the content of the crosslinking agent is preferably 0.5 to 10 parts by weight, more preferably 1 to 8 parts by weight, based on 100 parts by weight of the base polymer of the pressure-sensitive adhesive.
[0044] In one embodiment, an isocyanate-based crosslinking agent is preferably used. The isocyanate-based crosslinking agent is preferred because it can react with various functional groups. Specific examples of the isocyanate-based crosslinking agent include lower aliphatic polyisocyanates such as butylene diisocyanate and hexamethylene diisocyanate; alicyclic isocyanates such as cyclopentylene diisocyanate, cyclohexylene diisocyanate and isophorone diisocyanate; aromatic isocyanates such as 2,4-tolylene diisocyanate, 4,4'-diphenylmethane diisocyanate and xylylene diisocyanate; and isocyanate adducts such as trimethylolpropane / tolylene diisocyanate trimer adduct (manufactured by Nippon Polyurethane Industry Co., Ltd., product name "Coronate L"), trimethylolpropane / hexamethylene diisocyanate trimer adduct (manufactured by Nippon Polyurethane Industry Co., Ltd., product name "Coronate HL"), and isocyanurate of hexamethylene diisocyanate (manufactured by Nippon Polyurethane Industry Co., Ltd., product name "Coronate HX"). Preferably, a crosslinking agent having three or more isocyanate groups is used.
[0045] The active energy ray curable pressure sensitive adhesive may further contain any suitable additive as necessary, such as an active energy ray polymerization accelerator, a radical scavenger, a tackifier, a plasticizer (e.g., a trimellitic acid ester plasticizer, a pyromellitic acid ester plasticizer, etc.), a pigment, a dye, a filler, an antiaging agent, a conductive material, an antistatic agent, an ultraviolet absorbing agent, a light stabilizer, a release regulator, a softener, a surfactant, a flame retardant, an antioxidant, etc.
[0046] (UV absorber) Any suitable ultraviolet absorber may be used as the ultraviolet absorber, so long as it is a compound that absorbs ultraviolet light (for example, wavelength 355 nm). Examples of ultraviolet absorbers include benzotriazole-based ultraviolet absorbers, benzophenone-based ultraviolet absorbers, triazine-based ultraviolet absorbers, salicylate-based ultraviolet absorbers, and cyanoacrylate-based ultraviolet absorbers. Among them, triazine-based ultraviolet absorbers or benzotriazole-based ultraviolet absorbers are preferred, and triazine-based ultraviolet absorbers are particularly preferred. In particular, when an acrylic adhesive is used as the adhesive A, a triazine-based ultraviolet absorber can be preferably used because of its high compatibility with the base polymer of the acrylic adhesive. The triazine-based ultraviolet absorber is more preferably composed of a compound having a hydroxyl group, and is particularly preferably an ultraviolet absorber composed of a hydroxyphenyltriazine-based compound (hydroxyphenyltriazine-based ultraviolet absorber).
[0047] Examples of hydroxyphenyltriazine-based ultraviolet absorbers include a reaction product of 2-(4,6-bis(2,4-dimethylphenyl)-1,3,5-triazin-2-yl)-5-hydroxyphenyl with [(C10-C16 (mainly C12-C13) alkyloxy)methyl]oxirane (trade name "TINUVIN 400", manufactured by BASF), 2-[4,6-bis(2,4-dimethylphenyl)-1,3,5-triazin-2-yl]-5-[3-(dodecyloxy)-2-hydroxypropoxy]phenol), a reaction product of 2-(2,4-dihydroxyphenyl)-4,6-bis-(2,4-dimethylphenyl)-1,3,5-triazine with (2-ethylhexyl)-glycidic acid ester (trade name "TINUVIN 405" manufactured by BASF), 2,4-bis(2-hydroxy-4-butoxyphenyl)-6-(2,4-dibutoxyphenyl)-1,3,5-triazine (trade name "TINUVIN 460" manufactured by BASF), 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5-[(hexyl)oxy]-phenol (trade name "TINUVIN 1577" manufactured by BASF), 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5-[2-(2-ethylhexanoyloxy)ethoxy]-phenol (trade name "ADEKA STAB LA-46" manufactured by ADEKA Corporation), 2-(2-hydroxy-4-[1-octyloxycarbonylethoxy]phenyl)-4,6-bis(4-phenylphenyl)-1,3,5-triazine (trade name "TINUVIN 479" manufactured by BASF), and TINUVIN 477 manufactured by BASF.
[0048] Examples of benzotriazole-based ultraviolet absorbers (benzotriazole-based compounds) include 2-(2-hydroxy-5-tert-butylphenyl)-2H-benzotriazole (trade name "TINUVIN PS", manufactured by BASF), an ester compound of benzenepropanoic acid and 3-(2H-benzotriazol-2-yl)-5-(1,1-dimethylethyl)-4-hydroxy (C7-9 side chain and linear alkyl) (trade name "TINUVIN 384-2", manufactured by BASF), a mixture of octyl 3-[3-tert-butyl-4-hydroxy-5-(5-chloro-2H-benzotriazol-2-yl)phenyl]propionate and 2-ethylhexyl-3-[3-tert-butyl-4-hydroxy-5-(5-chloro-2H-benzotriazol-2-yl)phenyl]propionate (trade name "TINUVIN 109, manufactured by BASF), 2-(2H-benzotriazol-2-yl)-4,6-bis(1-methyl-1-phenylethyl)phenol (trade name "TINUVIN 900", manufactured by BASF), 2-(2H-benzotriazol-2-yl)-6-(1-methyl-1-phenylethyl)-4-(1,1,3,3-tetramethylbutyl)phenol (trade name "TINUVIN 928", manufactured by BASF), reaction product of methyl 3-(3-(2H-benzotriazol-2-yl)-5-tert-butyl-4-hydroxyphenyl)propionate / polyethylene glycol 300 (trade name "TINUVIN 1130", manufactured by BASF), 2-(2H-benzotriazol-2-yl)-p-cresol (trade name "TINUVIN P", manufactured by BASF), 2-(2H-benzotriazol-2-yl)-4,6-bis(1-methyl-1-phenylethyl)phenol (trade name "TINUVIN 234", manufactured by BASF), 2-[5-chloro-2H-benzotriazol-2-yl]-4-methyl-6-(tert-butyl)phenol (trade name "TINUVIN 326", manufactured by BASF), 2-(2H-benzotriazol-2-yl)-4,6-di-tert-pentylphenol (trade name "TINUVIN 328", manufactured by BASF), 2-(2H-benzotriazol-2-yl)-4-(1,1,3,3-tetramethylbutyl)phenol (trade name "TINUVIN 329", manufactured by BASF), 2,2'-methylenebis[6-(2H-benzotriazol-2-yl)-4-(1,1,3,3-tetramethylbutyl)phenol] (trade name "TINUVIN 360", manufactured by BASF), reaction product of methyl 3-(3-(2H-benzotriazol-2-yl)-5-tert-butyl-4-hydroxyphenyl)propionate with polyethylene glycol 300 (trade name "TINUVIN 213", manufactured by BASF), 2-(2H-benzotriazol-2-yl)-6-dodecyl-4-methylphenol (trade name "TINUVIN 571", manufactured by BASF), 2-[2-hydroxy-3-(3,4,5,6-tetrahydrophthalimido-methyl)-5-methylphenyl]benzotriazole (trade name "Sumisorb 250" manufactured by Sumitomo Chemical Co., Ltd.), 2-(3-tert-butyl-2-hydroxy-5-methylphenyl)-5-chloro-2H-benzotriazole (trade name "SEESORB 703" manufactured by Shipro Chemical Co., Ltd.), 2-(2H-benzotriazol-2-yl)-4-methyl-6-(3,4,5,6-tetrahydrophthalimidylmethyl)phenol (trade name "SEESORB 706" manufactured by Shipro Chemical Co., Ltd.), 2-(4-benzoyloxy-2-hydroxyphenyl)-5-chloro-2H-benzotriazole (trade name "SEESORB 7012BA" manufactured by Shipro Chemical Co., Ltd.), 2-tert-butyl-6-(5-chloro-2H-benzotriazol-2-yl)-4-methylphenol (trade name "KEMISORB 73" manufactured by Chemipro Chemicals), 2,2'-methylenebis[6-(2H-benzotriazol-2-yl)-4-tert-octylphenol] (trade name "ADK STAB LA-31" manufactured by ADEKA Corporation), 2-(2H-benzotriazol-2-yl)-p-cellulose (trade name "ADK STAB LA-32" manufactured by ADEKA Corporation), 2-(5-chloro-2H-benzotriazol-2-yl)-6-tert-butyl-4-methylphenol (trade name "ADK STAB LA-36" manufactured by ADEKA Corporation), etc.
[0049] The ultraviolet absorber may be a dye or a pigment. Examples of pigments include azo, phthalocyanine, anthraquinone, lake, perylene, perinone, quinacridone, thioindigo, dioxandine, isoindolinone, and quinophthalone pigments. Examples of dyes include azo, phthalocyanine, anthraquinone, carbonyl, indigo, quinoneimine, methine, quinoline, and nitro dyes.
[0050] The molecular weight of the compound constituting the ultraviolet absorber is preferably from 100 to 1500, more preferably from 200 to 1200, and even more preferably from 200 to 1000. Within such a range, a pressure-sensitive adhesive sheet capable of forming a better deformed portion upon irradiation with laser light can be obtained.
[0051] The maximum absorption wavelength of the ultraviolet absorber is preferably 300 nm to 450 nm, more preferably 320 nm to 400 nm, and further preferably 330 nm to 380 nm. The difference between the maximum absorption wavelength of the ultraviolet absorber and the maximum absorption wavelength of the photopolymerization initiator is preferably 10 nm or more, and more preferably 25 nm or more.
[0052] The 5% weight loss temperature of the ultraviolet absorber is preferably 350°C or less, more preferably 330°C or less. The lower limit of the 5% weight loss temperature of the ultraviolet absorber is, for example, 100°C. Within this range, a pressure-sensitive adhesive sheet capable of forming a better deformed portion by laser light irradiation can be obtained. The 5% weight loss temperature of the ultraviolet absorber means the temperature at which the weight of the ultraviolet absorber when heated is reduced by 5% by weight relative to the weight before heating. The 5% weight loss temperature is measured using a differential thermal analyzer under the measurement conditions of a heating temperature of 10°C / min, an air atmosphere, and a flow rate of 25 ml / min.
[0053] The content of the ultraviolet absorber is preferably 1 to 50 parts by weight, more preferably 5 to 20 parts by weight, relative to 100 parts by weight of the base polymer in the adhesive layer. Within such a range, when the adhesive strength of the entire adhesive layer is satisfactorily reduced by irradiation with active energy rays, the adhesive layer is cured satisfactorily, and an adhesive sheet exhibiting good releasability by irradiation with laser light can be obtained.
[0054] (particle) The pressure-sensitive adhesive layer may further contain any suitable additive. In one embodiment, the pressure-sensitive adhesive layer further contains particles. If the pressure-sensitive adhesive layer contains particles, it is possible to prevent the adherend (e.g., chip) from being excessively embedded in the pressure-sensitive adhesive layer, and as a result, it is possible to obtain a pressure-sensitive adhesive sheet that exhibits good releasability. In particular, when the pressure-sensitive adhesive layer is thick, such an effect is remarkable.
[0055] The particles may be inorganic particles or organic particles. Examples of inorganic particles include silica particles, titanium particles, alumina particles, and zirconia particles. Examples of organic particles include melamine-based resin particles and acrylic-based resin particles.
[0056] The average particle size of the particles is preferably 5 nm to 1 μm, and more preferably 10 nm to 500 nm. If the average particle size is too small, the effect of adding the particles may be reduced. If the average particle size is too large, the pressure-sensitive adhesive surface may become uneven, and sufficient adhesive strength may not be obtained. The average particle size of the particles is the number average particle size measured by a laser diffraction method.
[0057] The content of the particles is preferably 0.5 to 10 parts by weight, more preferably 1 to 5 parts by weight, based on 100 parts by weight of the base polymer in the adhesive layer. If the content of the particles is too low, the effect of adding the particles may be reduced. If the content of the particles is too high, unevenness may be formed on the adhesive surface, and sufficient adhesive strength may not be obtained.
[0058] C. Base material The substrate may be made of any suitable resin. Examples of the resin include polyolefin resins such as polyethylene resins, polypropylene resins, polybutene resins, and polymethylpentene resins, polyurethane resins, polyester resins, polyimide resins, polyether ketone resins, polystyrene resins, polyvinyl chloride resins, polyvinylidene chloride resins, fluorine resins, silicon resins, cellulose resins, and ionomer resins. Among these, polyolefin resins are preferred.
[0059] The thickness of the substrate is preferably from 2 μm to 300 μm, more preferably from 2 μm to 100 μm, and further preferably from 2 μm to 50 μm.
[0060] The light transmittance of the substrate at a wavelength of 355 nm is preferably 70% or more, more preferably 80% or more, even more preferably 90% or more, and particularly preferably 95% or more. The upper limit of the total light transmittance of the substrate is, for example, 98% (preferably 99%).
[0061] D. Manufacturing method of adhesive sheet The pressure-sensitive adhesive sheet can be produced by any suitable method. The pressure-sensitive adhesive sheet can be obtained, for example, by coating the pressure-sensitive adhesive on a substrate or a release liner. Various methods can be adopted as the coating method, such as bar coater coating, air knife coating, gravure coating, gravure reverse coating, reverse roll coating, lip coating, die coating, dip coating, offset printing, flexographic printing, and screen printing. In addition, a method of forming a pressure-sensitive adhesive layer on a release liner and then laminating it to a substrate can also be adopted.
[0062] E. How to use the adhesive sheet The pressure-sensitive adhesive sheet of the present invention can be used when temporarily fixing any suitable workpiece (e.g., electronic parts) when processing the workpiece. Examples of the method of using the pressure-sensitive adhesive sheet of the present invention include (i) attaching and fixing the workpiece to an adhesive sheet, (ii) processing the workpiece, (iii) irradiating the entire pressure-sensitive adhesive layer of the pressure-sensitive adhesive sheet with active energy rays (e.g., ultraviolet rays) to reduce the adhesive strength of the pressure-sensitive adhesive sheet, and (iv) irradiating the desired location for release with laser light to release the workpiece. According to this method, the workpiece can be released by natural drop. In addition, when multiple workpieces are temporarily fixed, it is also possible to release only a part of them. By using the pressure-sensitive adhesive sheet of the present invention, the adhesive strength can be reduced to the extent that the workpiece can naturally drop, so that even very small workpieces (e.g., 50 μm square) can be individually released. EXAMPLES
[0063] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. Test and evaluation methods in the examples are as follows. Furthermore, unless otherwise specified, "parts" and "%" are by weight.
[0064] (1) Peelability The PET separator of the adhesive sheet was peeled off, and the sheet was attached to a large slide glass (manufactured by Matsunami Glass, product name "S9111") using a hand roller. After that, the PET separator on the other side was peeled off, and a 100 μm square silicon chip was attached to the adhesive surface. Using an ultraviolet irradiation device (manufactured by Nitto Seiki, product name "UM-810"), ultraviolet light from a high-pressure mercury lamp (specific wavelength: 365 nm, cumulative light amount: 350 mJ / cm ) was applied from the side of the slide glass. 2 ) was irradiated over the entire surface. A laser beam with a wavelength of 355 nm was irradiated only at the target component position from the large slide glass side with an irradiation area of 80 μmφ and outputs of 0.3 W, 0.2 W, 0.1 W, and 0.05 W (1 plus per chip). If the component fell naturally, it was judged as a pass (◯), and if it did not fall naturally, it was judged as a fail (×).
[0065] (2) Damage to the substrate After the above operation (1), the appearance of the peeled silicon chip was observed under a microscope. If there was no visible damage, it was rated as pass (◯), and if there was damage, it was rated as fail (×).
[0066] (3) Contamination After the above operation (1), the surface of the peeled silicon chip was observed under a microscope to check for the presence or absence of contamination due to decomposition components of the adhesive layer. If there was no contamination, it was judged as pass (◯), and if there was contamination, it was judged as fail (×).
[0067] (4) Light transmittance at wavelength 355nm The PET separator of the adhesive sheet was peeled off, and the sheet was attached to a large glass slide (manufactured by Matsunami Glass, product name "S9111") using a hand roller, and the measurement was performed with the PET separator on the other side peeled off. Specifically, a spectrophotometer (product name "Spectrophotometer U-4100", manufactured by Hitachi High-Tech Science) was used to measure the transmittance of the adhesive sheet itself at a wavelength of 355 nm for the adhesive sheet on the large glass slide.
[0068] (5)Visible light transmittance The PET separator of the adhesive sheet was peeled off, and the sheet was attached to a large slide glass (manufactured by Matsunami Glass, product name "S9111") using a hand roller, and the measurement was performed with the PET separator on the other side peeled off. Specifically, a spectrophotometer (product name "Spectrophotometer U-4100", manufactured by Hitachi High-Tech Science) was used to measure the light transmittance over the wavelength range of 280 nm to 800 nm for the adhesive sheet on the glass. The obtained measured values were used to calculate the visible light transmittance based on the calculation method of JIS R 3106:1998.
[0069] (6) Haze value A haze meter (trade name "HAZE METER HM-150", manufactured by Murakami Color Research Laboratory) was used to measure the haze value by setting a large glass slide (manufactured by Matsunami Glass, trade name "S9111") so that the incident light was perpendicular to the surface of the glass slide. The PET separator of the adhesive sheet was then peeled off, and the sheet was attached to the large glass slide after the haze value measurement using a hand roller, and the haze value was measured again with the PET separator on the other side peeled off. The haze value of the adhesive sheet was determined by subtracting the haze value of the glass slide alone from the obtained haze value.
[0070] (7) 5% weight loss temperature of ultraviolet absorber The 5% weight loss temperature of the ultraviolet absorber was measured using a differential thermal analyzer (manufactured by TA Instruments, product name "Discovery TGA") under measurement conditions of a temperature rise rate of 10°C / min, in an air atmosphere, and at a flow rate of 25 ml / min.
[0071] [Production Example 1] Preparation of Acrylic Polymer I A monomer composition was prepared by mixing 90 parts by weight of lauryl methacrylate and 10 parts by weight of 2-hydroxyethyl methacrylate. Next, nitrogen was introduced into a reaction vessel equipped with a nitrogen inlet tube, a thermometer, and a stirrer, and 43 parts by weight of toluene, 100 parts by weight of the monomer composition, and 0.2 parts by weight of azoisobutylnitrile (AIBN) were charged under a nitrogen atmosphere and stirred at 60° C. for 4 hours. Thereafter, the mixture was cooled to room temperature, and 9 parts by weight of 2-methacryloyloxyethyl isocyanate was added and reacted to add an NCO group to the side chain terminal OH group of 2-hydroxyethyl acrylate in the copolymer, thereby obtaining an acrylic polymer solution I containing an acrylic polymer I having a weight average molecular weight of 1,000,000 and a carbon-carbon double bond at the end.
[0072] [Production Example 2] Preparation of Acrylic Polymer II A monomer composition was prepared by mixing 100 parts by weight of 2-methoxyethyl acrylate, 27 parts by weight of acryloylmorpholine, and 22 parts by weight of 2-hydroxyethyl acrylate. Next, nitrogen was introduced into a reaction vessel equipped with a nitrogen inlet tube, a thermometer, and a stirrer, and 500 parts by weight of toluene, 149 parts by weight of the monomer composition, and 0.3 parts by weight of benzoyl peroxide (BPO) were charged under a nitrogen atmosphere and stirred for 5 hours at 60° C. Thereafter, the mixture was cooled to room temperature, and 24 parts by weight of 2-methacryloyloxyethyl isocyanate was added and reacted to add an NCO group to the terminal OH group of the side chain of 2-hydroxyethyl acrylate in the copolymer, thereby obtaining an acrylic polymer solution II containing an acrylic polymer II having a weight average molecular weight of 1,000,000 and a carbon-carbon double bond at the terminal.
[0073] [Production Example 3] Preparation of Acrylic Polymer III A monomer composition was prepared by mixing 70 parts by weight of methyl acrylate, 30 parts by weight of 2-hydroxyethyl acrylate, and 10 parts by weight of acrylic acid. Next, nitrogen was introduced into a reaction vessel equipped with a nitrogen inlet tube, a thermometer, and a stirrer, and 165 parts by weight of toluene, 110 parts by weight of the monomer composition, and 0.2 parts by weight of benzoyl peroxide (BPO) were charged under a nitrogen atmosphere and stirred at 60°C for 4 hours to obtain an acrylic polymer solution III containing an acrylic polymer III having a weight average molecular weight of 1,000,000.
[0074] [Production Example 4] Preparation of Acrylic Polymer IV A monomer composition was prepared by mixing 70 parts by weight of ethyl acrylate, 30 parts by weight of 2-hydroxyethyl acrylate, 5 parts by weight of methyl methacrylate acrylate, and 4 parts by weight of hydroxyethyl acrylate. Next, nitrogen was introduced into a reaction vessel equipped with a nitrogen inlet tube, a thermometer, and a stirrer, and 295 parts by weight of toluene, 109 parts by weight of the monomer composition, and 0.2 parts by weight of benzoyl peroxide (BPO) were charged under a nitrogen atmosphere and stirred at 60°C for 4 hours to obtain an acrylic polymer solution IV containing an acrylic polymer IV having a weight average molecular weight of 500,000.
[0075] [Production Example 5] Preparation of Acrylic Polymer V A monomer composition was prepared by mixing 100 parts by weight of 2-hydroxyethyl acrylate and 4 parts by weight of hydroxyethyl acrylate. Next, nitrogen was introduced into a reaction vessel equipped with a nitrogen inlet tube, a thermometer, and a stirrer, and 163 parts by weight of toluene, 104 parts by weight of the monomer composition, and 0.2 parts by weight of azoisobutyronitrile (AIBN) were charged under a nitrogen atmosphere and stirred at 60°C for 4 hours to obtain an acrylic polymer solution V containing an acrylic polymer V having a weight average molecular weight of 550,000.
[0076] [Example 1] (Preparation of Adhesive) To an acrylic polymer solution I containing 100 parts by weight of acrylic polymer I, 5 parts by weight of a crosslinker (manufactured by Nippon Polyurethane Industry Co., Ltd., product name "Coronate L"), 3 parts by weight of a photopolymerization initiator (manufactured by IGM Resins BV, product name "Omnirad369"), and 1 part by weight of an ultraviolet absorber (manufactured by BASF Japan, product name "Tinuvin 477"; 5% weight loss temperature of ultraviolet absorber: 320.2°C) were added to obtain an adhesive (1). (Adhesive sheet) The above-mentioned pressure-sensitive adhesive (1) was applied to the silicone-treated surface of a PET separator (thickness: 38 μm), and then heated at 130° C. for 2 minutes to form a pressure-sensitive adhesive layer with a thickness of 5 μm. A PET separator was laminated onto the adhesive layer using a hand roller to obtain an adhesive sheet with a separator.
[0077] [Example 2] A separator-attached pressure-sensitive adhesive sheet was obtained in the same manner as in Example 1, except that the blended amount of the ultraviolet absorber (manufactured by BASF Japan, product name "Tinuvin 477") was changed to 5 parts by weight.
[0078] [Example 3] A separator-attached pressure-sensitive adhesive sheet was obtained in the same manner as in Example 1, except that the blended amount of the ultraviolet absorber (manufactured by BASF Japan, product name "Tinuvin 477") was changed to 20 parts by weight.
[0079] [Example 4] An adhesive sheet with a separator was obtained in the same manner as in Example 1, except that 5 parts by weight of an ultraviolet absorber (manufactured by BASF Japan, product name "Tinuvin 477") was used instead of 1 part by weight of an ultraviolet absorber (manufactured by Chemipro Chemical, product name "KEMISORB111", 5% weight loss temperature of ultraviolet absorber: 153.6°C).
[0080] [Example 5] An adhesive sheet with a separator was obtained in the same manner as in Example 1, except that 5 parts by weight of an ultraviolet absorber (manufactured by BASF Japan, product name "Tinuvin 477") was used instead of 1 part by weight of an ultraviolet absorber (manufactured by Chemipro Chemical, product name "KEMISORB111", 5% weight loss temperature of ultraviolet absorber: 153.6°C) and the thickness of the adhesive layer was 10 μm.
[0081] [Example 6] The adhesive contains silica particles (manufactured by Admatec Co., Ltd., product name "YA050C", average particle size: 10 nm, specific surface area: 300 m 2 A separator-attached pressure-sensitive adhesive sheet was obtained in the same manner as in Example 5, except that 3 parts by weight of 1000 g / g was further added.
[0082] [Example 7] The adhesive contains silica particles (manufactured by Admatec Co., Ltd., product name "SO-C1", average particle size: 200 nm to 400 nm, specific surface area: 10 m 2 / g~300m 2 A separator-attached pressure-sensitive adhesive sheet was obtained in the same manner as in Example 5, except that 3 parts by weight of 1000 g / g was further added.
[0083] [Example 8] An adhesive sheet with a separator was obtained in the same manner as in Example 1, except that 5 parts by weight of an ultraviolet absorber (manufactured by BASF Japan, product name "Tinuvin 477") was used instead of 1 part by weight of an ultraviolet absorber (manufactured by Tokushiki, product name "9155YELLOW", 5% weight loss temperature of ultraviolet absorber: 277.6°C).
[0084] [Example 9] An adhesive sheet with a separator was obtained in the same manner as in Example 1, except that 5 parts by weight of an ultraviolet absorber (manufactured by BASF Japan, product name "Tinuvin 477") was used instead of 1 part by weight of an ultraviolet absorber (manufactured by TOKUSHIKI, product name "9156BLUE", 5% weight loss temperature of ultraviolet absorber: 330.9°C).
[0085] [Example 10] An adhesive sheet with a separator was obtained in the same manner as in Example 1, except that 5 parts by weight of an ultraviolet absorber (manufactured by BASF Japan, product name "Tinuvin 477") was used instead of 1 part by weight of an ultraviolet absorber (manufactured by TOKUSHIKI, product name "9157GREEN", 5% weight loss temperature of ultraviolet absorber: 311.1°C).
[0086] [Example 11] (Preparation of Adhesive) To an acrylic polymer solution II containing 100 parts by weight of acrylic polymer II, 3 parts by weight of a crosslinker (manufactured by Nippon Polyurethane Industry, product name "Coronate L"), 3 parts by weight of a photopolymerization initiator (manufactured by IGM Resins BV, product name "Omnirad369"), and 5 parts by weight of an ultraviolet absorber (manufactured by BASF Japan, product name "Tinuvin 477", 5% weight loss temperature of ultraviolet absorber: 320.2°C) were added to obtain an adhesive (2). (Preparation of adhesive sheet) The above-mentioned pressure-sensitive adhesive (2) was applied to the silicone-treated surface of a PET separator (thickness: 38 μm), and then heated at 130° C. for 2 minutes to form a pressure-sensitive adhesive layer with a thickness of 5 μm. A PET separator was laminated onto the adhesive layer using a hand roller to obtain an adhesive sheet with a separator.
[0087] [Example 12] An adhesive sheet with a separator was obtained in the same manner as in Example 11, except that the amount of ultraviolet absorber (manufactured by BASF Japan, product name "Tinuvin 477") was 20 parts by weight and the thickness of the adhesive layer was 10 μm.
[0088] [Example 13] An adhesive sheet with a separator was obtained in the same manner as in Example 11, except that 20 parts by weight of an ultraviolet absorber (manufactured by BASF Japan, product name "Tinuvin 384-2", 5% weight loss temperature of ultraviolet absorber: 264.4°C) was used instead of 5 parts by weight of an ultraviolet absorber (manufactured by BASF Japan, product name "Tinuvin 477").
[0089] [Example 14] (Preparation of Adhesive) To an acrylic polymer solution III containing 100 parts by weight of acrylic polymer III, 60 parts by weight of a urethane acrylate-based multifunctional oligomer (manufactured by Nippon Synthetic Chemical Industry, product name "UV-1700TL"), 1 part by weight of a crosslinking agent (manufactured by Nippon Polyurethane Industry, product name "Coronate L"), 1 part by weight of a melamine resin (manufactured by DIC, product name "Amidea J-820-60N"), 3 parts by weight of a photopolymerization initiator (manufactured by IGM Resins BV, product name "Omnirad369"), and 5 parts by weight of an ultraviolet absorber (manufactured by BASF Japan, product name "Tinuvin 477", 5% weight loss temperature of ultraviolet absorber: 320.2°C) were added to obtain an adhesive (3). (Preparation of adhesive sheet) The above-mentioned pressure-sensitive adhesive (3) was applied to the silicone-treated surface of a PET separator (thickness: 38 μm), and then heated at 130° C. for 2 minutes to form a pressure-sensitive adhesive layer with a thickness of 5 μm. A PET separator was laminated onto the adhesive layer using a hand roller to obtain an adhesive sheet with a separator.
[0090] [Example 15] (Preparation of Adhesive) To an acrylic polymer solution I containing 100 parts by weight of acrylic polymer I, 5 parts by weight of a crosslinker (manufactured by Nippon Polyurethane Industry Co., Ltd., product name "Coronate L"), 3 parts by weight of a photopolymerization initiator (manufactured by BASF, product name "Irgacure 651"), and 5 parts by weight of an ultraviolet absorber (manufactured by BASF Japan, product name "Tinuvin 477", 5% weight loss temperature of ultraviolet absorber: 320.2°C) were added to obtain an adhesive (4). (Adhesive sheet) The above-mentioned pressure-sensitive adhesive (4) was applied to the silicone-treated surface of a PET separator (thickness: 38 μm), and then heated at 130° C. for 2 minutes to form a pressure-sensitive adhesive layer with a thickness of 5 μm. A PET separator was laminated onto the adhesive layer using a hand roller to obtain an adhesive sheet with a separator.
[0091] [Example 16] An adhesive sheet with a separator was obtained in the same manner as in Example 15, except that 1 part by weight of a photosensitizer (manufactured by Kawasaki Chemical Industries, Ltd., product name "UVS-581") was further added to the adhesive.
[0092] [Example 17] An adhesive sheet with a separator was obtained in the same manner as in Example 15, except that 1 part by weight of a photosensitizer (manufactured by Kawasaki Chemical Industries, Ltd., product name "UVS-1101") was further added to the adhesive.
[0093] [Example 18] An adhesive sheet with a separator was obtained in the same manner as in Example 11, except that 5 parts by weight of an ultraviolet absorber (manufactured by BASF Japan, product name "Tinuvin 477") was replaced with 5 parts by weight of an ultraviolet absorber (manufactured by BASF Japan, product name "Tinuvin 405").
[0094] [Example 19] An adhesive sheet with a separator was obtained in the same manner as in Example 11, except that 5 parts by weight of an ultraviolet absorber (manufactured by BASF Japan, product name "Tinuvin 477") was replaced with 5 parts by weight of an ultraviolet absorber (manufactured by BASF Japan, product name "Tinuvin 928", 5% weight loss temperature of ultraviolet absorber: 227.6°C).
[0095] [Comparative Example 1] A separator-attached pressure-sensitive adhesive sheet was obtained in the same manner as in Example 1, except that the blended amount of the ultraviolet absorber (manufactured by BASF Japan, product name "Tinuvin 477") was 0.5 parts by weight.
[0096] [Comparative Example 2] A separator-attached pressure-sensitive adhesive sheet was obtained in the same manner as in Example 1, except that no photopolymerization initiator was added and the amount of ultraviolet absorber (manufactured by BASF Japan, product name "Tinuvin 477") added was 5 parts by weight.
[0097] [Comparative Example 3] (Preparation of Adhesive) To an acrylic polymer solution IV containing 100 parts by weight of acrylic polymer IV, 5 parts by weight of a crosslinker (manufactured by Nippon Polyurethane Industry, product name "Coronate L"), 10 parts by weight of a phenolic resin (manufactured by Sumitomo Bakelite, product name "Sumilite Resin PR12603"), and 20 parts by weight of an ultraviolet absorber (manufactured by BASF Japan, product name "Tinuvin 477") were added to obtain an adhesive (4). (Preparation of adhesive sheet) The above-mentioned pressure-sensitive adhesive (4) was applied to the silicone-treated surface of a PET separator (thickness: 38 μm), and then heated at 130° C. for 2 minutes to form a pressure-sensitive adhesive layer with a thickness of 5 μm. A PET separator was laminated onto the adhesive layer using a hand roller to obtain an adhesive sheet with a separator.
[0098] [Comparative Example 4] (Preparation of Adhesive) To an acrylic polymer solution V containing 100 parts by weight of acrylic polymer V, 4 parts by weight of a crosslinker (manufactured by Nippon Polyurethane Industry, product name "Coronate HX") and 20 parts by weight of an ultraviolet absorber (manufactured by BASF Japan, product name "Tinuvin 477") were added to obtain a pressure-sensitive adhesive (5). (Preparation of adhesive sheet) The above-mentioned pressure-sensitive adhesive (5) was applied to the silicone-treated surface of a PET separator (thickness: 38 μm), and then heated at 130° C. for 2 minutes to form a pressure-sensitive adhesive layer with a thickness of 5 μm. A PET separator was laminated onto the adhesive layer using a hand roller to obtain an adhesive sheet with a separator.
[0099] [Table 1]
[0100] As is clear from Table 1, when the light transmittance of the adhesive sheet at a wavelength of 355 nm is 50% or less, excellent peelability is exhibited by irradiation with low-power (0.2 W or less) laser light. In addition, by forming an adhesive layer containing an active energy ray curable adhesive, contamination of the silicon chip can be prevented. When the adhesive sheet of the embodiment is used, cleaning of the peeled silicon chip is not required. In addition, the adhesive sheet of the embodiment has a high visible light transmittance, and is advantageous in that the silicon chip can be clearly seen through the adhesive sheet when the adherend is peeled off by irradiation with laser light. [Explanation of symbols]
[0101] 10 Adhesive layer 20 Base material 100, 200 Adhesive Sheet
Claims
1. A pressure-sensitive adhesive sheet having a pressure-sensitive adhesive layer containing an ultraviolet absorber and an active energy ray-curable pressure-sensitive adhesive, the ultraviolet absorber is a triazine-based ultraviolet absorber or a benzotriazole-based ultraviolet absorber, The pressure-sensitive adhesive sheet has a light transmittance of 50% or less at a wavelength of 355 nm, The adhesive sheet was attached to a silicon mirror wafer, and 460 mJ / cm 2 The adhesive strength at 23°C after irradiation with ultraviolet light is 0.01N / 20mm to 0.3N / 20mm, the active energy ray-curable pressure-sensitive adhesive contains a base polymer, and the content of the ultraviolet absorber is 1 part by weight to 50 parts by weight per 100 parts by weight of the base polymer in the pressure-sensitive adhesive layer; Adhesive sheet.
2. The pressure-sensitive adhesive sheet according to claim 1 , wherein the pressure-sensitive adhesive layer has a thickness of 20 μm or less.
3. The pressure-sensitive adhesive sheet according to claim 1 or 2, which has a visible light transmittance of 50% or more.
4. The pressure-sensitive adhesive sheet according to claim 1 , which has a haze value of 70% or less.
5. The pressure-sensitive adhesive sheet according to claim 1 , wherein the active energy ray-curable pressure-sensitive adhesive further comprises a photopolymerization initiator and a photosensitizer.
6. The pressure-sensitive adhesive sheet according to claim 1 , wherein the ultraviolet absorber has a 5% weight loss temperature of 350° C. or lower.
7. The pressure-sensitive adhesive sheet according to claim 1 , wherein the pressure-sensitive adhesive layer further comprises particles.
8. The pressure-sensitive adhesive sheet according to claim 1 , wherein the active energy ray-curable pressure-sensitive adhesive comprises an acrylic polymer.
9. The pressure-sensitive adhesive sheet according to claim 8, wherein the active energy ray-curable pressure-sensitive adhesive comprises an active energy ray-reactive polymer configured by introducing an active energy ray-polymerizable carbon-carbon multiple bond into a side chain, a main chain and / or a main chain end of an acrylic polymer.
Citation Information
Patent Citations
Ultraviolet curing adhesive
CN105111998A
Ultraviolet-cured pressure-sensitive adhesive and preparation method therefor
CN106398554A
Sealing cover for IC package and forming method thereof
JP1983075850A
Production of tacky adhesive tape
JP1998110140A
Adhesive composition and adhesion method therewith, and peeling method after adhesion
JP2014101496A