Electrode assembly, battery, battery module, battery pack and power consuming device
A hydraulic inorganic material coating on the separator surface addresses the center hole collapse issue in cylindrical batteries, enhancing safety and cycle performance by preventing deformation and dendrite growth.
Patent Information
- Application Number
- JP2023502991
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-10-20
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2041-10-20
AI Technical Summary
Cylindrical batteries face issues with center hole collapse during the charging and discharging process, leading to increased safety risks and reduced cycle life due to the partial or complete blocking of the central pore, which affects the cycling performance.
Incorporating a hydraulic inorganic material coating on the separator's surface that reacts with water to increase the separator's strength, preventing the collapse of the center pore and growth of dendrites, thereby enhancing the battery's safety and cycle performance.
The hydraulic inorganic material coating effectively suppresses the collapse of the center pore and growth of dendrites, improving the safety and extending the cycle life of the battery without adversely affecting electrochemical performance.
Smart Images

Figure 0007567101000003 
Figure 0007567101000004 
Figure 0007567101000001
Abstract
Description
[Technical field]
[0001] The present application relates to the field of battery technology, and in particular to electrode assemblies, batteries, battery modules, battery packs and power consuming devices. [Background technology]
[0002] Rechargeable batteries have the advantages of high energy density, long cycle life, reliable operating performance, no pollution, no memory effect, etc., and are therefore widely used. In recent years, with the application and popularization of rechargeable batteries in various electronic products and new energy vehicles and other industries, their safety performance has attracted more and more attention. Traditional batteries include prismatic batteries and cylindrical batteries. Compared with prismatic batteries, cylindrical batteries have the advantages of high structural stability, fewer components, and simple manufacturing process. Cylindrical batteries generally use a wound electrode assembly, where the wound electrode assembly is formed by winding a positive electrode plate, a separator, and a negative electrode plate, and a central hole is formed in the center of the wound electrode assembly. However, the central hole of a cylindrical battery is easily collapsed, and the collapse of the central hole refers to the phenomenon that the central hole is partially or completely blocked during the formation, cycle charging and discharging process of the battery. The collapse of the central pore significantly affects the cycle performance of the battery by causing the battery to be difficult to evacuate and increasing safety risks. Summary of the Invention [Problem to be solved by the invention]
[0003] The present application aims to provide an electrode assembly, a battery, a battery module, a battery pack and a power consuming device to solve the problem of the collapse of the central hole of the electrode assembly and the battery, and to improve the safety performance and cycle performance of the battery. [Means for solving the problem]
[0004] A first aspect of the present application provides an electrode assembly. The electrode assembly includes a first electrode plate, a second electrode plate having a polarity opposite to that of the first electrode plate, and a separator provided between the first electrode plate and the second electrode plate. The electrode assembly is obtained by winding the first electrode plate, the second electrode plate, and the separator. The separator includes a base film and a coating provided on at least a part of the surface of the base film. The coating includes a hydraulic inorganic material that can react with water and cure.
[0005] The present application provides a coating containing a hydraulic inorganic material on the surface of a base film, and utilizes the principle that the hydraulic inorganic material can react with water and cure, thereby significantly increasing the strength of the separator, making it difficult to deform during the formation process and the cycle charge-discharge process of the battery, effectively suppressing the collapse of the central hole and the growth of dendrites, improving the safety performance of the battery, and extending the cycle life of the battery.
[0006] In any embodiment of the present application, the hydraulic inorganic material includes at least one compound represented by Formula 1. First Oxide·a Second Oxide·b Sulfate·c Halide Formula 1 Here, 0 < a ≤ 6, 0 ≤ b ≤ 4, 0 ≤ c ≤ 4. The first oxide represents CaO or BaO. The second oxide represents Component 1, Component 2, or a combination thereof. Component 1 represents SiO 2 , Al 2 O 3 , Fe 2 O 3 or a combination of two or more of them. Component 2 represents FeO, MgO, BaO, K 2 O, Na 2 O, TiO 2 , CuO, Cr 2 O 3 , P 2 O 5 , SO 3 or a combination of two or more of them. The sulfate is CaSO 4 , MgSO 4 , BaSO 4 , SrSO4 , ZnSO 4 , Al 2 (SO 4 ) 3 , FeSO 4 , Fe 2 (SO 4 ) 3 or a combination of two or more thereof, and the halide is CaCl 2 , CaF 2 , or a combination thereof.
[0007] The compound represented by the above formula 1 can effectively inhibit the collapse of the central pore and the growth of dendrites, and has no obvious effect on the electrochemical performance of the battery.
[0008] Optionally, the weight ratio of component 1 to component 2 is (95-100):(0-5). When the weight ratio of component 1 to component 2 is within a suitable range, it is favorable for adjusting the compressive strength and hydration heat of the coating, so that the coating after reacting with water has a suitable compressive strength and does not release excessive heat after reacting with water.
[0009] In any embodiment of the present application, the hydraulic inorganic material comprises one or more of the compounds shown in Formula 1-1 to Formula 1-8: CaO·a1 SiO 2 ·b Sulfate ·c Halide Formula 1-1 CaO·a2Al 2 O 3 ·b Sulfate ·c Halide Formula 1-2 CaO·a3Fe 2 O 3 ·b Sulfate ·c Halide Formula 1-3 CaO·a4Al 2 O 3 · a5SiO 2 ·b Sulfate ·c Halide Formula 1-4 CaO·a6 Al 2 O 3 a7 Fe 2 O 3 ·b Sulfate ·c Halide Formula 1-5 BaO·a8SiO 2 ·b Sulfate·c Halide Formula 1-6 BaO·a9Al 2 O 3 ·b Sulfate·c Halide Formula 1-7 BaO·a10Al 2 O 3 ·a11SiO 2 ·b Sulfate·c Halide Formula 1-8 Here, 0 < a1 ≤ 6, 0 < a2 ≤ 6, 0 < a3 ≤ 6, 0 < a4 < 6, 0 < a5 < 6, and 0 < a4 + a5 ≤ 6, 0 < a6 < 6, 0 < a7 < 6, and 0 < a6 + a7 ≤ 6, 0 < a8 ≤ 6, 0 < a9 ≤ 6, 0 < a10 < 6, 0 < a11 < 6, and 0 < a10 + a11 ≤ 6, 0 ≤ b ≤ 4, 0 ≤ c ≤ 4. The sulfate is CaSO 4 , MgSO 4 , BaSO 4 , SrSO 4 , ZnSO 4 , Al 2 (SO 4 ) 3 , FeSO 4 , Fe 2 (SO 4 ) 3 , or a combination of two or more of them. The halide represents CaCl 2 , CaF 2 , or a combination thereof.
[0010] In any embodiment of the present application, b = 0.
[0011] In any embodiment of the present application, c = 0.
[0012] In any embodiment of the present application, b = 0 and c = 0.
[0013] In any embodiment of the present application, the hydraulic inorganic material is 2CaO·SiO 2 , 3CaO·SiO 2 , CaO·Al 2 O 3<h2 style=";text-align:left;direction:ltr">CaO2Al<h2 style=";text-align:left;direction:ltr"> 2 <h2 style=";text-align:left;direction:ltr"> O<h2 style=";text-align:left;direction:ltr"> 3 <h2 style=";text-align:left;direction:ltr"> 3CaO·Al<h2 style=";text-align:left;direction:ltr"> 2 <h2 style=";text-align:left;direction:ltr"> O<h2 style=";text-align:left;direction:ltr"> 3 <h2 style=";text-align:left;direction:ltr"> 6CaO·2Al<h2 style=";text-align:left;direction:ltr"> 2 <h2 style=";text-align:left;direction:ltr"> O<h2 style=";text-align:left;direction:ltr"> 3 <h2 style=";text-align:left;direction:ltr"> 12CaO·7Al<h2 style=";text-align:left;direction:ltr"> 2 <h2 style=";text-align:left;direction:ltr"> O<h2 style=";text-align:left;direction:ltr"> 3 <h2 style=";text-align:left;direction:ltr"> CaO·Fe<h2 style=";text-align:left;direction:ltr"> 2 <h2 style=";text-align:left;direction:ltr"> O<h2 style=";text-align:left;direction:ltr"> 3 <h2 style=";text-align:left;direction:ltr"> 、2CaO Fe<h2 style=";text-align:left;direction:ltr"> 2 <h2 style=";text-align:left;direction:ltr"> O<h2 style=";text-align:left;direction:ltr"> 3 <h2 style=";text-align:left;direction:ltr"> 2CaO·Al<h2 style=";text-align:left;direction:ltr"> 2 <h2 style=";text-align:left;direction:ltr"> O<h2 style=";text-align:left;direction:ltr"> 3 <h2 style=";text-align:left;direction:ltr"> SiO<h2 style=";text-align:left;direction:ltr"> 2 <h2 style=";text-align:left;direction:ltr"> CaO·Al<h2 style=";text-align:left;direction:ltr"> 2 <h2 style=";text-align:left;direction:ltr"> O<h2 style=";text-align:left;direction:ltr"> 3 <h2 style=";text-align:left;direction:ltr"> 2SiO<h2 style=";text-align:left;direction:ltr"> 2 <h2 style=";text-align:left;direction:ltr"> 4CaO·Al<h2 style=";text-align:left;direction:ltr"> 2 <h2 style=";text-align:left;direction:ltr"> O<h2 style=";text-align:left;direction:ltr"> 3 <h2 style=";text-align:left;direction:ltr"> ·Fe<h2 style=";text-align:left;direction:ltr"> 2 <h2 style=";text-align:left;direction:ltr"> O<h2 style=";text-align:left;direction:ltr"> 3 <h2 style=";text-align:left;direction:ltr"> 6CaO·Al<h2 style=";text-align:left;direction:ltr"> 2 <h2 style=";text-align:left;direction:ltr"> O<h2 style=";text-align:left;direction:ltr"> 3 <h2 style=";text-align:left;direction:ltr"> 2Fe<h2 style=";text-align:left;direction:ltr"> 2 <h2 style=";text-align:left;direction:ltr"> O<h2 style=";text-align:left;direction:ltr"> 3 <h2 style=";text-align:left;direction:ltr"> 3CaO·3Al<h2 style=";text-align:left;direction:ltr"> 2 <h2 style=";text-align:left;direction:ltr"> O<h2 style=";text-align:left;direction:ltr"> 3 <h2 style=";text-align:left;direction:ltr"> ·CaSO<h2 style=";text-align:left;direction:ltr"> 4 <h2 style=";text-align:left;direction:ltr"> 3CaO·3Al<h2 style=";text-align:left;direction:ltr"> 2 <h2 style=";text-align:left;direction:ltr"> O<h2 style=";text-align:left;direction:ltr"> 3 <h2 style=";text-align:left;direction:ltr"> MgSO4<h2 style=";text-align:left;direction:ltr"> 4 <h2 style=";text-align:left;direction:ltr"> 3CaO·3Al<h2 style=";text-align:left;direction:ltr"> 2 <h2 style=";text-align:left;direction:ltr"> O<h2 style=";text-align:left;direction:ltr"> 3 <h2 style=";text-align:left;direction:ltr"> ·BaSO<h2 style=";text-align:left;direction:ltr"> 4 <h2 style=";text-align:left;direction:ltr"> 3CaO·3Al<h2 style=";text-align:left;direction:ltr"> 2 <h2 style=";text-align:left;direction:ltr"> O<h2 style=";text-align:left;direction:ltr"> 3 <h2 style=";text-align:left;direction:ltr"> ·SrSO<h2 style=";text-align:left;direction:ltr"> 4 <h2 style=";text-align:left;direction:ltr"> 3CaO·3Al<h2 style=";text-align:left;direction:ltr"> 2 <h2 style=";text-align:left;direction:ltr"> O<h2 style=";text-align:left;direction:ltr"> 3 <h2 style=";text-align:left;direction:ltr"> ZnSO4<h2 style=";text-align:left;direction:ltr"> 4 <h2 style=";text-align:left;direction:ltr"> 3CaO·3Al<h2 style=";text-align:left;direction:ltr"> 2 <h2 style=";text-align:left;direction:ltr"> O<h2 style=";text-align:left;direction:ltr"> 3 <h2 style=";text-align:left;direction:ltr"> Al<h2 style=";text-align:left;direction:ltr"> 2 <h2 style=";text-align:left;direction:ltr"> (SO<h2 style=";text-align:left;direction:ltr"> 4 <h2 style=";text-align:left;direction:ltr"> )<h2 style=";text-align:left;direction:ltr"> 3 <h2 style=";text-align:left;direction:ltr"> 3CaO·3Al<h2 style=";text-align:left;direction:ltr"> 2 <h2 style=";text-align:left;direction:ltr"> O<h2 style=";text-align:left;direction:ltr"> 3 <h2 style=";text-align:left;direction:ltr"> ·FeSO<h2 style=";text-align:left;direction:ltr"> 4 <h2 style=";text-align:left;direction:ltr"> 3CaO·3Al<h2 style=";text-align:left;direction:ltr"> 2 <h2 style=";text-align:left;direction:ltr"> O<h2 style=";text-align:left;direction:ltr"> 3 <h2 style=";text-align:left;direction:ltr"> ·Fe<h2 style=";text-align:left;direction:ltr"> 2 <h2 style=";text-align:left;direction:ltr"> (SO<h2 style=";text-align:left;direction:ltr"> 4 <h2 style=";text-align:left;direction:ltr"> )<h2 style=";text-align:left;direction:ltr"> 3 <h2 style=";text-align:left;direction:ltr"> 2CaO·SiO<h2 style=";text-align:left;direction:ltr"> 2 <h2 style=";text-align:left;direction:ltr"> ·CaSO<h2 style=";text-align:left;direction:ltr"> 4 <h2 style=";text-align:left;direction:ltr"> 11CaO·7Al<h2 style=";text-align:left;direction:ltr"> 2 <h2 style=";text-align:left;direction:ltr"> O3 ·CaF 2 , 3CaO 3Al 2 O 3 ·CaF 2 , CaO 3Al 2 O 3 3CaF 2 , CaO 3Al 2 O 3 4CaF 2 , 2BaO SiO 2 , 3BaO SiO 2 , BaO Al 2 O 3 , 3BaO Al 2 O 3 , BaO 6Al 2 O 3 , BaO Al 2 O 3 SiO 2 , BaO Al 2 O 3 2SiO 2 Includes one or more of the following:
[0014] Optionally, the hydraulic inorganic material is 2CaO SiO 2 , 3CaO SiO 2 , 3CaO·Al 2 O 3 , 4CaO·Al 2 O 3 Fe 2 O 3 Includes one or more of the following:
[0015] In any embodiment of the present application, the hydraulic inorganic material is a particle with a volume particle size Dv10 of 1 μm to 10 μm. Optionally, the hydraulic inorganic material is a particle with a volume particle size Dv10 of 3 μm to 5 μm. When the volume particle size Dv10 of the hydraulic inorganic material particles is within a suitable range, the consistency of the coating is higher.
[0016] In any embodiment of the present application, the weight percentage of the hydraulic inorganic material is between 95% and 100% relative to the total weight of the coating. Optionally, the weight percentage of the hydraulic inorganic material is between 97% and 100%.
[0017] In any embodiment of the present application, the coating further comprises an additive, the additive comprising one or more of a water reducer, gypsum, pozzolan, fly ash, slag, silica sand, limestone, clay, etc. The additive may serve to adjust the compressive strength of the coating, adjust the coagulation rate of the reaction of the coating with water, and reduce the heat of hydration.
[0018] In any embodiment of the present application, the weight percentage of the additive is ≦5% relative to the total weight of the coating. Optionally, the weight percentage of the additive is ≦3%.
[0019] In any embodiment of the present application, the total thickness of the coating is 0.5 μm to 5 μm. Optionally, the total thickness of the coating is 0.5 μm to 2 μm. When the total thickness of the coating is within a suitable range, the coating has a suitable compressive strength after reacting with water and does not release excessive heat after reacting with water.
[0020] In any embodiment of the present application, the thickness of the base film is between 5 μm and 12 μm. Optionally, the thickness of the base film is between 6 μm and 7 μm.
[0021] In any embodiment of the present application, the base film is one or more selected from a polyolefin porous membrane, a nonwoven fabric, and a glass fiber.
[0022] In any embodiment of the present application, the heat of hydration of the coating and water within 2 days is 300J / g-500J / g. After reacting with water, the coating has a suitable heat dissipation amount, which can, on the one hand, increase the transmission rate of active ions between the positive and negative electrodes of the battery, improve the cycle performance and rate performance of the battery, and, on the other hand, ensure that other electrochemical performances of the battery are not affected.
[0023] In any embodiment of the present application, the compressive strength of the coating after reacting with water and curing is 2500 Pa to 20000 Pa. Optionally, the compressive strength of the coating after reacting with water and curing is 2500 Pa to 10000 Pa. Because the coating after reacting with water has high compressive strength, the separator is not easily deformed during the chemical formation process and cycle charge and discharge process of the battery, and can effectively inhibit the collapse of the central hole and the growth of dendrites, improve the safety performance of the battery, and extend the cycle life of the battery.
[0024] In any embodiment of the present application, the coating is located within a region of 0 cm to L cm from the winding start end of the separator, and 10≦L≦20. The coating containing a hydraulic inorganic material is provided only within a partial region of the winding start end of the separator, thereby effectively suppressing the collapse of the central hole and the growth of dendrites, and not significantly reducing the mass energy density of the battery.
[0025] A second aspect of the present application provides a battery, the battery comprising an electrode assembly and an electrolyte, where the electrode assembly is the electrode assembly of the battery according to the first aspect of the present application, and the electrolyte comprises an electrolyte salt and water.
[0026] Since the electrolyte of the present application uses water as a solvent, after the electrolyte is infiltrated into the coating containing the hydraulic inorganic material, the hydraulic inorganic material in the coating can react with the solvent water to fully harden the coating, thereby significantly increasing the strength of the separator, so that the separator is not easily deformed during the chemical formation process and cycle charge / discharge process of the battery, and the collapse of the central hole and the growth of dendrites can be effectively inhibited, thereby improving the safety performance of the battery and extending the cycle life of the battery.
[0027] In any embodiment of the present application, the battery is a lithium ion battery, a sodium ion battery, a potassium ion battery, a zinc ion battery, a calcium ion battery, a magnesium ion battery, an aluminum ion battery, or a hybrid ion battery.
[0028] A third aspect of the present application provides a battery module including a battery of the second aspect of the present application.
[0029] A fourth aspect of the present application provides a battery pack including one of the battery module of the second aspect of the present application and the battery module of the third aspect.
[0030] A fifth aspect of the present application provides a power consuming device including at least one of the battery of the second aspect of the present application, the battery module of the third aspect, and the battery pack of the fourth aspect.
[0031] The battery modules, battery packs and power consuming devices of the present application contain a battery according to the present application and therefore have at least the same advantages as said battery. [Brief description of the drawings]
[0032] In order to more clearly describe the technical solutions in the embodiments of the present application, the following briefly describes the drawings that need to be used in the embodiments of the present application. Obviously, the drawings described below are only some embodiments of the present application, and those skilled in the art can obtain other drawings based on the drawings without spending creative labor. [Figure 1] 1A and 1B are schematic diagrams of a cylindrical battery before and after a central hole collapses. [Diagram 2] 1 is a schematic diagram of one embodiment of a power consuming device that includes a battery of the present application as a power source. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0033] Hereinafter, with appropriate reference to the drawings, embodiments specifically disclosing the electrode assembly, battery, battery module, battery pack, and power consumption device of the present application will be described in detail. However, unnecessary detailed description may be omitted. For example, detailed description of well-known matters and duplicated description of structures that are actually the same may be omitted. This is to avoid the following description from becoming unnecessarily redundant and to allow those skilled in the art to easily understand. Note that the drawings and the following description are provided to allow those skilled in the art to fully understand the present application, and are not intended to limit the subject matter described in the claims.
[0034] The "ranges" disclosed in this application are defined in the form of lower and upper limits, where a given range is defined by selecting one lower limit and one upper limit, and the selected lower and upper limits define the boundaries of the particular range. Such defined ranges may be inclusive or exclusive of the end values, and any combination is possible, i.e., any combination of any lower limit and any upper limit can form a range. For example, if ranges of 60-120 and 80-110 are recited for a particular parameter, it is understood that ranges of 60-110 and 80-120 are also contemplated. It is noted that if minimum range values 1 and 2 are recited, and maximum range values 3, 4, and 5 are recited, then ranges of 1-3, 1-4, 1-5, 2-3, 2-4, and 2-5 are all contemplated. In this application, unless otherwise specified, a numerical range "a to b" represents a shorthand representation of any combination of real numbers from a to b, where a and b are both real numbers. For example, a numerical range of "0-5" is meant herein to enumerate all real numbers between "0-5," and "0-5" is merely a shorthand for combinations of these numerical values. Note that expressing a parameter as an integer ≧2 is equivalent to disclosing that the parameter is, for example, the integers 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0035] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution, and such technical solution should be considered to be included in the content disclosed in the present application.
[0036] Unless otherwise stated, all technical features and optional technical features of the present application can be combined with each other to form a new technical solution, and such technical solution should be considered to be included in the content disclosed in the present application.
[0037] Unless otherwise stated, all steps in the present application may be performed sequentially or randomly, and are preferably performed sequentially. For example, the method includes steps (a) and (b) to mean that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method mentioned above further includes step (c) to mean that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), may include steps (a), (c) and (b), may include steps (c), (a) and (b), etc.
[0038] Unless otherwise specified, the terms "comprise" and "comprises" referred to in this application may be open ended or closed ended. For example, the terms "comprise" and "comprises" may further include or include other ingredients not listed, or may include or include only the listed ingredients.
[0039] Unless otherwise stated, in this application, the term "or" is inclusive. For example, the term "A or B" means "A, B, or both A and B." More specifically, any of the following conditions satisfy "A or B": A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); and A and B are both true (or exist).
[0040] FIG. 1 is a schematic diagram of a cylindrical battery before and after the central hole collapses. As shown in FIG. 1, the center of the cylindrical battery has a central hole, and the central hole is easily collapsed during the formation and cycle charge / discharge process of the battery. After the central hole collapses, the internal gap of the battery increases (for example, the gap between the positive and negative plates increases), which makes it easy for dendrites to grow, affecting the safety of the battery and reducing the cycle life of the battery. The collapse of the central hole is affected by factors such as the gas generation rate of the battery formation, the coating weight of the electrode plate, the thickness of the current collector, and the repulsion rate of the electrode plate. Generally, the larger the coating weight of the electrode plate and the higher the gas generation rate of the battery formation, the more easily the central hole collapses, and the thinner the thickness of the current collector and the higher the repulsion rate of the electrode plate, the more easily the central hole collapses. Therefore, the effect of suppressing the collapse of the central hole can be achieved by increasing the resistance of the electrode plate and separator in the partial region of the central hole and making the central hole less likely to deform. In the prior art, the hardness of the separator can be increased to a certain extent by providing a ceramic coating on the surface of the separator base film, but the hardness of the separator is still low and the effect of effectively suppressing the collapse of the central hole cannot be achieved.
[0041] In view of the above problems, the inventors have made improvements to the structure of the separator and proposed an electrode assembly and a battery that can effectively suppress the collapse of the central hole.
[0042] Electrode Assembly and Battery The battery of the present application includes a case, an electrode assembly, end caps, and an electrolyte, the electrode assembly is disposed in the case, the end caps are disposed on the case, and the electrolyte permeates the electrode assembly and serves to conduct active ions between the positive electrode and the negative electrode. The electrolyte includes an electrolyte salt and water, and the type of the electrolyte salt is not specifically limited and may be selected according to actual needs. The material of the case is not specifically limited and may be, for example, a hard plastic case, an aluminum case, a steel case, etc.
[0043] It should be noted that the battery of the present application may be a lithium ion battery, a sodium ion battery, a potassium ion battery, a zinc ion battery, a calcium ion battery, a magnesium ion battery, an aluminum ion battery, or a hybrid ion battery. In the present application, the term "hybrid ion battery" refers to a battery in which a desorption reaction of two or more active ions occurs between the positive and negative electrodes of the battery, and the electrolyte of the hybrid ion battery usually contains two or more active ions, such as two or more of lithium ions, sodium ions, potassium ions, zinc ions, calcium ions, magnesium ions, and aluminum ions. For example, the hybrid ion battery may include a lithium sodium hybrid ion battery, a sodium zinc hybrid ion battery, a sodium potassium hybrid ion battery, etc.
[0044] The electrode assembly of the present application includes a first electrode plate, a second electrode plate having an opposite polarity to the first electrode plate, and a separator provided between the first electrode plate and the second electrode plate, and the electrode assembly is obtained by winding the first electrode plate, the second electrode plate, and the separator, and the separator includes a base film and a coating provided on at least a portion of a surface of the base film, and the coating includes a hydraulic inorganic material that can react with water to harden.
[0045] The inventors unexpectedly discovered that by providing a coating containing a hydraulic inorganic material on the surface of a base film and utilizing the principle that the hydraulic inorganic material can react with water and harden, the strength of the separator can be significantly increased and the separator is less likely to deform during the battery formation process and cycle charge / discharge process, thereby effectively inhibiting the collapse of the central hole and the growth of dendrites, improving the safety performance of the battery, and extending the cycle life of the battery.
[0046] Since the electrolyte of this application uses water as a solvent, after the coating containing the hydraulic inorganic material is infiltrated with the electrolyte, the hydraulic inorganic material in the coating can react with water, which is the solvent, to fully cure the coating, thereby significantly increasing the strength of the separator. Therefore, in the battery formation process and the cycle charge-discharge process, the separator is not easily deformed, effectively suppressing the collapse of the central hole and the growth of dendrites, improving the safety performance of the battery, and extending the cycle life of the battery.
[0047] The electrode assembly of this application is a wound electrode assembly, and the end face shape of the electrode assembly is not specifically limited and may be selected according to actual needs. For example, the end face of the electrode assembly may be a regular shape such as circular, elliptical, rectangular, etc., or the end face of the electrode assembly may be an irregular shape.
[0048] In some embodiments, the hydraulic inorganic material contains at least one compound represented by Formula 1.
[0049] First Oxide·a Second Oxide·b Sulfate·c Halide Formula 1 In Formula 1, 0 < a ≤ 6, 0 ≤ b ≤ 4, 0 ≤ c ≤ 4. The first oxide represents CaO or BaO, the second oxide represents Component 1, Component 2, or a combination thereof. Component 1 represents SiO 2 、Al 2 O 3 、Fe 2 O 3、 or a combination of two or more of them. Component 2 represents FeO, MgO, BaO, K 2 O, Na 2 O, TiO 2 、CuO、Cr 2 O 3 、P 2 O 5 、SO 3、 or a combination of two or more of them. The sulfate is CaSO 4 、MgSO 4 、BaSO 4 、SrSO 4, ZnSO 4 , Al 2 (SO 4 ) 3 , FeSO 4 , Fe 2 (SO 4 ) 3 , or a combination of two or more thereof, and the halide represents CaCl 2 , CaF 2 , or a combination thereof.
[0050] The product of the reaction between the compound represented by Formula 1 and water contains one or more of a gel, a hydrate, Ca(OH) 2 , etc., and the compound represented by Formula 1 has an appropriate compressive strength after reacting with water and does not release excessive heat after reacting with water. Therefore, the compound represented by Formula 1 can effectively suppress the collapse of the central hole and the growth of dendrites, and has no obvious influence on the electrochemical performance of the battery.
[0051] In some embodiments, the weight ratio of Component 1 to Component 2 is (95 - 100):(0 - 5). When the weight ratio of Component 1 to Component 2 is within an appropriate range, it is advantageous for adjusting the compressive strength and heat of hydration of the coating, giving the coating an appropriate compressive strength after reacting with water and not releasing excessive heat after reacting with water.
[0052] In some embodiments, the second oxide represents only Component 1.
[0053] In some embodiments, b = 0.
[0054] In some embodiments, 0 < b ≤ 4. When the sulfate content is appropriate, it is advantageous for adjusting the compressive strength and heat of hydration of the coating, giving the coating an appropriate compressive strength after reacting with water and not releasing excessive heat after reacting with water.
[0055] In some embodiments, c = 0.
[0056] In some embodiments, 0 < c ≤ 4. When the halide content is appropriate, it is advantageous for adjusting the compressive strength and heat of hydration of the coating, such that the coating after reacting with water has an appropriate compressive strength and does not release excessive heat after reacting with water.
[0057] In some embodiments, b = 0 and c = 0.
[0058] The compound represented by Formula 1 may be produced by a general method in the art. For example, it may be produced by a high-temperature solid-phase reaction method. An exemplary production method is as follows. A Ca source or Ba source, an M1 element precursor, an optional SO 3 , and an optional halogen precursor are uniformly mixed according to a certain molar ratio, and then subjected to high-temperature firing to obtain the compound represented by Formula 1. M1 is one or more selected from Si, Al, Fe, K, Na, Mg, Ba, Ti, Cu, Cr, Sr, Zn, etc. Optionally, the firing temperature is 800 °C to 1600 °C.
[0059] As an example, the Ca source includes, but is not limited to, one or more of CaO, CaCO 3 , Ca(OH) 2 . As an example, the Ba source includes, but is not limited to, one or more of BaO, BaCO 3 , Ba(OH) 2 . As an example, the M1 element precursor includes, but is not limited to, one or more of an oxide, a hydroxide compound, a sulfate compound, a hydrochloride compound, a nitrate compound, a carbonate compound, and an acetate compound of the M1 element. For example, the M1 element precursor is SiO 2 , Al(OH) 3 , Al 2 O 3 , Fe 2 O 3 , FeO, K 2 O, Na 2 O, MgO, BaO, TiO 2 , CuO, Cr 2 O 3, SrO, ZnO. By way of example, the halogen precursor may include one or more of ammonium fluoride, hydrogen fluoride, ammonium chloride, and hydrogen chloride.
[0060] In some embodiments, the hydraulic inorganic material comprises a compound represented by formula 1-1, where sulfate, halide are as defined herein.
[0061] CaO·a1 SiO 2 ·b Sulfate ·c Halide Formula 1-1 In Equation 1-1, 0 <a1≦6、0≦b≦4、0≦c≦4である。
[0062] Optionally, 0 <a1≦3、b=0、c=0である。
[0063] Optionally, 0 <a1≦3、0<b≦4、c=0である。
[0064] Optionally, 0 <a1≦3、b=0、0<c≦4である。
[0065] In some embodiments, the hydraulic inorganic material comprises a compound of formula 1-2, where sulfate, halide are as defined herein.
[0066] CaO·a2Al 2 O 3 ·b Sulfate ·c Halide Formula 1-2 In Equation 1-2, 0 <a2≦6、0≦b≦4、0≦c≦4である。
[0067] Optionally, 0 <a2≦3、b=0、c=0である。
[0068] Optionally, 0 <a2≦3、0<b≦4、c=0である。
[0069] Optionally, 0 <a2≦3、b=0、0<c≦4である。
[0070] In some embodiments, the hydraulic inorganic material contains a compound represented by Formula 1-3, and the sulfate and halide are as defined herein.
[0071] CaO·a3 Fe 2 O 3 ·b Sulfate·c Halide Formula 1-3 In Formula 1-3, 0 < a3 ≤ 6, 0 ≤ b ≤ 4, and 0 ≤ c ≤ 4.
[0072] Optionally, 0 < a3 ≤ 3, b = 0, and c = 0.
[0073] Optionally, 0 < a3 ≤ 3, 0 < b ≤ 4, and c = 0.
[0074] Optionally, 0 < a3 ≤ 3, b = 0, and 0 < c ≤ 4.
[0075] In some embodiments, the hydraulic inorganic material contains a compound represented by Formula 1-4, and the sulfate and halide are as defined herein.
[0076] CaO·a4 Al 2 O 3 ·a5 SiO 2 ·b Sulfate·c Halide Formula 1-4 In Formula 1-4, 0 < a4 < 6, 0 < a5 < 6, and 0 < a4 + a5 ≤ 6, 0 ≤ b ≤ 4, and 0 ≤ c ≤ 4.
[0077] Optionally, 0 < a4 ≤ 2, 0 < a5 ≤ 2, and 0 < a4 + a5 ≤ 3, b = 0, and c = 0.
[0078] Optionally, 0 < a4 ≤ 2, 0 < a5 ≤ 2, and 0 < a4 + a5 ≤ 3, 0 < b ≤ 4, and c = 0.
[0079] Optionally, 0 < a4 ≤ 2, 0 < a5 ≤ 2, and 0 < a4 + a5 ≤ 3, b = 0, and 0 < c ≤ 4.
[0080] In some embodiments, the hydraulic inorganic material contains a compound represented by Formula 1-5, and the sulfate and halide are as defined herein.
[0081] CaO·a6Al 2 O 3 ·a7Fe 2 O 3 ·b sulfate·c halide Formula 1-5 In Formula 1-5, 0 < a6 < 6, 0 < a7 < 6, and 0 < a6 + a7 ≤ 6, 0 ≤ b ≤ 4, 0 ≤ c ≤ 4.
[0082] Optionally, 0 < a6 ≤ 2, 0 < a7 ≤ 2, and 0 < a6 + a7 ≤ 3, b = 0, c = 0.
[0083] Optionally, 0 < a6 ≤ 2, 0 < a7 ≤ 2, and 0 < a6 + a7 ≤ 3, 0 ≤ b ≤ 4, c = 0.
[0084] Optionally, 0 < a6 ≤ 2, 0 < a7 ≤ 2, and 0 < a6 + a7 ≤ 3, b = 0, 0 < c ≤ 4.
[0085] In some embodiments, the hydraulic inorganic material contains a compound represented by Formula 1-6, and the sulfate and halide are as defined herein.
[0086] BaO·a8SiO 2 ·b sulfate·c halide Formula 1-6 In Formula 1-6, 0 < a8 ≤ 6, 0 ≤ b ≤ 4, 0 ≤ c ≤ 4.
[0087] Optionally, 0 < a8 ≤ 3, b = 0, c = 0.
[0088] Optionally, 0 < a8 ≤ 3, 0 ≤ b ≤ 4, c = 0.
[0089] Optionally, 0 < a8 ≤ 3, b = 0, 0 < c ≤ 4.
[0090] In some embodiments, the hydraulic inorganic material contains a compound represented by Formula 1-7, and the sulfate and halide are as defined herein.
[0091] BaO·a9 Al 2 O 3 ·b sulfate·c halide Formula 1-7 In Formula 1-7, 0 < a9 ≤ 6, 0 ≤ b ≤ 4, and 0 ≤ c ≤ 4.
[0092] Optionally, 0 < a9 ≤ 6, b = 0, and c = 0.
[0093] Optionally, 0 < a9 ≤ 6, 0 < b ≤ 4, and c = 0.
[0094] Optionally, 0 < a9 ≤ 6, b = 0, and 0 < c ≤ 4.
[0095] In some embodiments, the hydraulic inorganic material contains a compound represented by Formula 1-8, and the sulfate and halide are as defined herein.
[0096] BaO·a10 Al 2 O 3 ·a11 SiO 2 ·b sulfate·c halide Formula 1-8 In Formula 1-8, 0 < a10 < 6, 0 < a11 < 6, and 0 < a10 + a11 ≤ 6, 0 ≤ b ≤ 4, and 0 ≤ c ≤ 4.
[0097] Optionally, 0 < a10 ≤ 2, 0 < a11 ≤ 2, and 0 < a10 + a11 ≤ 3, b = 0, and c = 0.
[0098] Optionally, 0 < a10 ≤ 2, 0 < a11 ≤ 2, and 0 < a10 + a11 ≤ 3, 0 < b ≤ 4, and c = 0.
[0099] Optionally, 0 < a10 ≤ 2, 0 < a11 ≤ 2, and 0 < a10 + a11 ≤ 3, b = 0, and 0 < c ≤ 4.
[0100] In some embodiments, the hydraulic inorganic material comprises two or more of the compounds shown in formula 1-1 to formula 1-8, which is favorable for adjusting the compressive strength and heat of hydration of the coating, so that the coating has a suitable compressive strength after reacting with water, and does not release excessive heat after reacting with water.
[0101] In some embodiments, for example, the hydraulic inorganic material is 2CaO SiO 2 , 3CaO SiO 2 , CaO·Al 2 O 3 , CaO 2Al 2 O 3 , 3CaO·Al 2 O 3 , 6CaO 2Al 2 O 3 , 12CaO 7Al 2 O 3 , CaO·Fe 2 O 3 , 2CaO Fe 2 O 3 , 2CaO·Al 2 O 3 SiO 2 , CaO·Al 2 O 3 2SiO 2 , 4CaO·Al 2 O 3 Fe 2 O 3 , 6CaO·Al 2 O 3 2Fe 2 O 3 , 3CaO 3Al 2 O 3 ·CaSO 4 , 3CaO 3Al 2 O 3 MgSO 4 , 3CaO 3Al 2 O 3 ·BaSO 4 , 3CaO 3Al 2 O 3 SrSO 4 , 3CaO 3Al 2 O 3 ZnSO4 , 3CaO 3Al 2 O 3 ·Al 2 (SO 4 ) 3 , 3CaO 3Al 2 O 3 FeSO 4 , 3CaO 3Al 2 O 3 Fe 2 (SO 4 ) 3 , 2CaO SiO 2 ·CaSO 4 , 11CaO 7Al 2 O 3 ·CaF 2 , 3CaO 3Al 2 O 3 ·CaF 2 , CaO 3Al 2 O 3 3CaF 2 , CaO 3Al 2 O 3 4CaF 2 , 2BaO SiO 2 , 3BaO SiO 2 , BaO Al 2 O 3 , 3BaO Al 2 O 3 , BaO 6Al 2 O 3 , BaO Al 2 O 3 SiO 2 , BaO Al 2 O 3 2SiO 2 Includes one or more of the following:
[0102] Optionally, the hydraulic inorganic material is 2CaO SiO 2 , 3CaO SiO 2 , 3CaO·Al 2 O 3 , 4CaO·Al 2 O 3 Fe 2 O 3 Includes one or more of the following:
[0103] In some embodiments, the hydraulic inorganic material is a particle having a volume particle size Dv10 of 1 μm to 10 μm. For example, the hydraulic inorganic material particle has a volume particle size Dv10 of 1 μm, 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, or any range of values. Optionally, the hydraulic inorganic material is a particle having a volume particle size Dv10 of 3 μm to 5 μm. When the hydraulic inorganic material particle has a volume particle size Dv10 within a suitable range, the conformity of the coating is higher.
[0104] In some embodiments, the weight percentage of the hydraulic inorganic material is between 95% and 100% relative to the total weight of the coating. Optionally, the weight percentage of the hydraulic inorganic material is between 97% and 100%.
[0105] In some embodiments, the coating further includes an additive, which can adjust the compressive strength of the coating, adjust the coagulation rate of the reaction between the coating and water, and reduce the heat of hydration. For example, the additive can include, but is not limited to, one or more of water-reducing admixture, gypsum, pozzolan, fly ash, slag, silica sand, limestone, and clay. Here, the gypsum can include one or more of natural dihydrate gypsum, anhydrite, hemihydrate gypsum, phosphorus gypsum, and desulfurization gypsum. The type of the additive is not specifically limited and can be selected according to actual needs, for example, the water-reducing admixture can be a polycarboxylic acid water-reducing admixture. These additives can be used alone or in combination of two or more. The mass percentage of the additive is ≦5% based on the total mass of the coating. For example, the mass percentage of the additive is ≦4.5%, ≦4%, ≦3.5%, ≦3%, ≦2.5%, ≦2%, ≦1.5%, ≦1%, ≦0.5%, or 0%.
[0106] In some embodiments, the thickness of the base film is 5 μm to 12 μm. Optionally, the thickness of the base film is 6 μm to 7 μm. When the thickness of the base film is within an appropriate range, the separator can have sufficient compressive strength and also have high ionic conductivity.
[0107] In some embodiments, the porosity of the base film is 30% to 50%. Optionally, the porosity of the base film is 35% to 50%. When the porosity of the base film is within an appropriate range, the separator can have sufficient compressive strength and also have high ionic conductivity.
[0108] In some embodiments, the type of the base film is not particularly limited, and any well-known porous structure film having good chemical stability and mechanical stability may be selected. Optionally, the base film is one or more selected from polyolefin porous membrane, nonwoven fabric, and glass fiber. The base film may be a single layer film or a multi-layer composite film. When the base film is a multi-layer composite film, the materials of each layer are the same or different. For example, the material of the base film may be one or more selected from polyethylene, polypropylene, polyimide, polyvinylidene fluoride, vinylidene fluoride-hexafluoropropylene copolymer, polyamide, and polyethylene terephthalate.
[0109] The base film has two opposing surfaces in the thickness direction, and the coating is provided on either or both of the two surfaces of the base film.
[0110] In some embodiments, the total thickness of the coating is between 0.5 μm and 5 μm. In this application, the term "total thickness of the coating" refers to the sum of the thicknesses of the coatings applied on the two surfaces of the base film. When the coating is applied on any one of the two surfaces of the base film, the thickness of the coating is the total thickness of the coating, and when the coating is applied on both of the two surfaces of the base film, the sum of the thicknesses of the coating is the total thickness of the coating.
[0111] For example, the total thickness of the coating is in a range of any numerical value, such as 0.5 μm, 1.0 μm, 1.5 μm, 2.0 μm, 2.5 μm, 3.0 μm, 3.5 μm, 4.0 μm, 4.5 μm, 5.0 μm, or more. Optionally, the total thickness of the coating is 0.5 μm to 2 μm. When the total thickness of the coating is within the appropriate range, the coating after reacting with water has an appropriate compressive strength and does not release excessive heat after reacting with water.
[0112] In some embodiments, the heat of hydration of the coating with water within two days is between 300 J / g and 500 J / g, for example, the heat of hydration of the coating with water within two days is in the range of 300 J / g, 310 J / g, 320 J / g, 330 J / g, 340 J / g, 350 J / g, 360 J / g, 370 J / g, 380 J / g, 390 J / g, 400 J / g, 410 J / g, 420 J / g, 430 J / g, 440 J / g, 450 J / g, 460 J / g, 470 J / g, 480 J / g, 490 J / g, 500 J / g, or any value greater than or equal to ...500 J / g. By adjusting the composition, thickness, etc. of the coating, the coating can have a suitable heat dissipation amount after reacting with water, which can, on the one hand, increase the transmission rate of active ions between the positive and negative electrodes of the battery, improve the cycle performance and rate performance of the battery, and, on the other hand, ensure that other electrochemical performances of the battery are not affected.
[0113] In some embodiments, the compressive strength of the coating after reacting with water and curing is between 2500 Pa and 20000 Pa. For example, the compressive strength of the coating after reacting with water and curing may be in the range of any value between 2500 Pa, 3000 Pa, 4000 Pa, 5000 Pa, 6000 Pa, 7000 Pa, 8000 Pa, 9000 Pa, 10000 Pa, 11000 Pa, 12000 Pa, 13000 Pa, 14000 Pa, 15000 Pa, 16000 Pa, 17000 Pa, 18000 Pa, 19000 Pa, 20000 Pa, or greater. Optionally, the compressive strength of the coating after reacting with water and curing is 2500 Pa to 18000 Pa, 2500 Pa to 16000 Pa, 2500 Pa to 14000 Pa, 2500 Pa to 12000 Pa, 2500 Pa to 10000 Pa, 2500 Pa to 9000 Pa, 2500 Pa to 8000 Pa, 2500 Pa to 7000 Pa, 2500 Pa to 6000 Pa, or 2500 Pa to 5000 Pa. By adjusting the composition, thickness, etc. of the coating, the coating after reacting with water can have high compressive strength, so that the separator is not easily deformed during the chemical formation process and cycle charge and discharge process of the battery, and the collapse of the central hole and the growth of dendrites can be effectively suppressed, thereby improving the safety performance of the battery and extending the cycle life of the battery.
[0114] The heat of hydration has a meaning known in the art and can be measured by adopting instruments and methods known in the art. For example, a TAM Air heat-activated microcalorimeter (obtained from TA Instruments, USA) is used to measure the heat of hydration of the coating. An exemplary test method is as follows: a freshly manufactured separator is taken for testing, the coating is sampled in any one area of the separator (e.g., powder is sampled by using a doctor blade), the mass of all the collected samples is weighed, all the collected samples are placed in an ampoule, a measured amount of water is collected by a syringe in an electric mixer, the electric mixer is inserted into the ampoule, and the electric mixer together with the ampoule is placed in the measuring position of the microthermometer, and finally the water in the syringe is injected into the ampoule, and stirring and recording are started, and the total heat release during the test period is obtained. Here, the test period is 48 hours, and the test temperature is room temperature.
[0115] Compressive strength has a meaning known in the art and can be measured using equipment and methods known in the art. During testing, the separator sample can be taken directly from a freshly manufactured separator or can be obtained from a battery.
[0116] When a newly manufactured separator is taken for testing, an exemplary test method is as follows: A newly manufactured single-sided coated separator sample is taken for testing; if it is a double-sided coated separator, the coating on one side may be wiped off first, the separator is placed in deionized water, the coating is fully reacted with water to harden, the separator is taken out of the deionized water, and after being fully dried, it is placed in a compressive strength measuring device (e.g., YN-200-400 microcomputer compressive strength measuring device) for testing, and the breaking load when the separator is broken is obtained. Optionally, the loading speed is 0.4MPa / s to 0.6MPa / s.
[0117] When the separator is taken from the battery, an exemplary test method is as follows: After the battery is fully discharged, the separator is removed, and the area where the winding start end is sufficiently hardened is sampled for testing. If the separator is double-sided coated, the coating on one side may be wiped off first, and the separator is placed in an oven to thoroughly dry (e.g., 45°C, 30 min), and after removing excess electrolyte, it is further placed in a compressive strength measuring device (e.g., YN-200-400 microcomputer compressive strength measuring device) for testing, and the breaking load when the separator is broken is obtained. Optionally, the loading speed is 0.4MPa / s to 0.6MPa / s.
[0118] The compressive strength of the coating after reacting with water and curing was calculated according to the formula p=P / A, where p represents the compressive strength of the sample, P represents the breaking load of the sample, and A represents the area of the sample.
[0119] In some embodiments, the coating is located within a region of 0 cm to L cm from the winding start end of the separator, and 10≦L≦20. The coating containing a hydraulic inorganic material is provided only within a partial region of the winding start end of the separator, so that the collapse of the central hole and the growth of dendrites can be effectively suppressed and the mass energy density of the battery is not significantly reduced. Therefore, the electrode assembly of the present application can have high safety performance and high energy density at the same time.
[0120] The separator may be manufactured by a method commonly used in the art. An exemplary manufacturing method is as follows: A hydraulic inorganic material and optional additives are dissolved in an organic solvent, thoroughly stirred and mixed to form a uniform coating slurry, and the coating slurry is applied to the surface of a base film, and then dried to obtain a separator. Here, the type of the organic solvent is not specifically limited and may be selected according to actual needs. For example, the organic solvent is selected from dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, etc.
[0121] In some embodiments, the pH of the electrolyte is between 5 and 9. Optionally, the pH of the electrolyte is 7.
[0122] In some embodiments, the concentration of the electrolyte salt may be between 0.5 mol / L and 2.0 mol / L. Optionally, the concentration of the electrolyte salt is 1.0 mol / L.
[0123] In some embodiments, for example, the electrolyte salt may be Li 2 SO 4 , LiNO 3 , LiCl, LiCF 3 SO 3 , Na 2 SO 4 , NaNO 3 , NaCl, NaCF 3 SO 3 , K 2 SO 4 , KNO 3 , KCl, KCF 3 SO 3 , ZnSO 4 , Zn(NO 3 ) 2 , ZnCl 2 , Zn(CF 3 SO 3 ) 2 , Ca(NO 3 ) 2 , CaCl 2 , Ca(CF 3 SO 3 ) 2 , MgSO 4 , Mg(NO 3 ) 2 , MgCl 2 , Mg(CF 3 SO 3 ) 2 , Sr(NO 3 ) 2 , SrCl 2 , Sr(CF 3 SO 3 ) 2 , Ba(NO 3 ) 2 , BaCl 2 , Ba(CF 3 SO 3 )2 , Al 2 (SO 4 ) 3 , Al(NO 3 ) 3 , AlCl 3 , Al(CF 3 SO 3 ) 3 This includes, but is not limited to, one or more of:
[0124] In some embodiments, the electrolyte solution optionally further includes additives, for example, additives that may include an anode film-forming additive, a cathode film-forming additive, or additives that may improve some performance of the battery, such as additives that improve the overcharge performance of the battery, additives that improve the high temperature performance of the battery, additives that improve the low temperature performance of the battery, etc.
[0125] In some embodiments, the first plate is a positive plate and the second plate is a negative plate. In some embodiments, the first plate is a negative plate and the second plate is a positive plate.
[0126] The positive electrode plate may include a positive electrode current collector and a positive electrode film layer provided on at least one surface of the positive electrode current collector. For example, the positive electrode current collector has two surfaces facing each other in the thickness direction, and the positive electrode film layer is provided on either one or both of the two surfaces of the positive electrode current collector.
[0127] The positive electrode membrane layer typically includes a positive electrode active material, an optional conductive agent, and an optional adhesive, and is typically obtained after applying a positive electrode slurry to a positive electrode current collector, drying, and cold pressing. The positive electrode slurry is typically formed by dispersing the positive electrode active material, the optional conductive agent, the optional adhesive, and any other components in a solvent and stirring the mixture uniformly. The solvent may be, but is not limited to, deionized water, N-methylpyrrolidone (NMP), etc. For example, the adhesive used in the positive electrode membrane layer includes one or more of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, fluorine-containing acrylate resin, styrene butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA) and carboxymethyl chitosan (CMCS). For example, the conductive agent used in the positive electrode membrane layer includes one or more of superconducting carbon, conductive graphite, acetylene black, carbon black, ketjen black, carbon spots, carbon nanotubes, graphene, and carbon nanofibers.
[0128] The positive electrode current collector may adopt a metal foil sheet or a composite current collector. As an example of the metal foil sheet, the positive electrode current collector may adopt an aluminum foil. The composite current collector may include a polymeric material base layer and a metal material layer formed on at least one surface of the polymeric material base layer. As an example, the metal material may be one or more selected from aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy. As an example, the polymeric material base layer may be selected from polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.
[0129] The negative electrode plate may include a negative electrode current collector and a negative electrode film provided on at least one surface of the negative electrode current collector. For example, the negative electrode current collector has two surfaces facing each other in a thickness direction thereof, and the negative electrode film is provided on one or both of the two surfaces of the negative electrode current collector.
[0130] The negative electrode membrane layer typically includes a negative electrode active material, an optional adhesive, an optional conductive agent, and other optional auxiliary agents, and is typically obtained after applying a negative electrode slurry to a negative electrode current collector, drying, and cold pressing. The negative electrode slurry is typically formed by dispersing the negative electrode active material, the optional conductive agent, the optional adhesive, and any other components in a solvent and stirring the mixture uniformly. The solvent may be, but is not limited to, deionized water, N-methylpyrrolidone (NMP), etc. For example, the adhesive used in the negative electrode film layer includes one or more of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, fluorine-containing acrylate resin, styrene butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA) and carboxymethyl chitosan (CMCS). For example, the conductive agent used in the negative electrode film layer includes one or more of superconducting carbon, conductive graphite, acetylene black, carbon black, ketjen black, carbon spots, carbon nanotubes, graphene, and carbon nanofibers. For example, other auxiliary agents used in the negative electrode membrane layer include thickeners, such as sodium carboxymethylcellulose (CMC-Na).
[0131] The negative electrode current collector may be a metal foil sheet or a composite current collector. An example of the metal foil sheet may be copper foil. The composite current collector may include a polymeric material base layer and a metal material layer formed on at least one surface of the polymeric material base layer. For example, the metal material may be one or more selected from copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy. For example, the polymeric material base layer may be selected from polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.
[0132] The positive electrode active material and the negative electrode active material may be materials known in the art that are used in lithium ion batteries, sodium ion batteries, potassium ion batteries, zinc ion batteries, calcium ion batteries, magnesium ion batteries, aluminum ion batteries, or hybrid ion batteries.
[0133] The positive electrode active material is selected from materials having an active ion (e.g., lithium ion, sodium ion, potassium ion, zinc ion, calcium ion, magnesium ion, aluminum ion, etc.) storage potential lower than the oxygen evolution potential of water, while the negative electrode active material is selected from materials having an active ion (e.g., lithium ion, sodium ion, potassium ion, zinc ion, calcium ion, magnesium ion, aluminum ion, etc.) storage potential higher than the oxygen evolution potential of water.
[0134] As examples, the positive electrode active material includes one or more of a transition metal oxide material, a polyanion material (e.g., an olivine structure, a NASICON structure, a maricite structure, a pyrophosphate, a fluorophosphate, a sulfate, etc.), a Prussian blue material, an organic polymer material, and a modified compound of each. x MO 2(M is a transition metal, preferably one or more selected from Mn, Fe, Ni, Co, V, Cu, and Cr, and 0 < x ≤ 1), and may include, but is not limited to, one or more of manganese-based oxides, vanadium-based oxides, and their respective modified compounds. Examples of the organic polymer material may include, but are not limited to, poly(2,2,6,6-tetramethylpiperidineoxy-4-vinyl ether) (PTVE). This application is not limited to these materials, and other conventionally known materials that can be used as the positive electrode active material of the battery may also be used. These positive electrode active materials may be used alone or in combination of two or more.
[0135] Optionally, the modified compound of each of the above positive electrode active materials may be one obtained by doping modification of the positive electrode active material, one obtained by surface coating modification, or one obtained by simultaneously performing doping modification and surface coating modification.
[0136] As an example, the negative electrode active material includes one or more of artificial graphite, natural graphite, soft carbon, hard carbon, activated carbon, transition metal oxides, and organic polymer materials. Examples of the organic polymer material may include, but are not limited to, polyimide (PI), quinone, for example, poly(2-vinylanthraquinone) (PVAQ). However, this application is not limited to these materials, and other conventionally known materials that can be used as the negative electrode active material of the battery may also be used. These negative electrode active materials may be used alone or in combination of two or more.
[0137] Battery module and battery pack In some embodiments of this application, the battery according to this application can be assembled into a battery module. The number of batteries included in the battery module may be plural, and the specific number can be adjusted based on the application and capacity of the battery module.
[0138] In the battery module, the batteries may be arranged in sequence along the length of the battery module, or may be arranged in any other manner. The batteries may be secured together by fasteners.
[0139] Optionally, the battery module may further include a housing having an accommodation space for accommodating a plurality of batteries.
[0140] In some embodiments of the present application, the above battery modules can be further assembled into a battery pack, and the number of battery modules included in the battery pack can be adjusted based on the application and capacity of the battery pack.
[0141] Optionally, the battery pack may further include a battery case and a plurality of battery modules disposed in the battery case. The battery case includes an upper case and a lower case, and the upper case is disposed on the lower case as a lid to form a sealed space for accommodating the battery modules. The plurality of battery modules may be disposed in the battery case according to any manner.
[0142] power consumption equipment An embodiment of the present application further provides a power consuming device, including at least one of the battery, battery module, and battery pack of the present application. The battery, battery module, or battery pack may be used as a power source for the power consuming device, or may be used as an energy storage unit for the power consuming device. The power consuming device may be, but is not limited to, a mobile device (e.g., mobile phone, laptop, etc.), an electric vehicle (e.g., pure electric vehicle, hybrid electric vehicle, plug-in hybrid electric vehicle, electric bicycle, electric scooter, electric golf cart, electric truck, etc.), an electric train, a ship and satellite, an energy storage system, etc.
[0143] The power consuming device may be a battery, a battery module or a battery pack depending on the needs of the usage.
[0144] 2 is a schematic diagram of an example power consuming device, such as a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle, that may employ a battery pack or battery module to meet the high power and high energy density needs of the power consuming device.
[0145] As another example, the power consuming device may be a mobile phone, a tablet computer, a laptop, etc. The power consuming device is generally required to be thin and lightweight, and may employ a battery as a power source.
[0146] Working Example The following examples are provided to more specifically describe the contents disclosed in this application, and these examples are used for illustrative purposes only. This is because it is obvious to those skilled in the art that various modifications and changes can be made within the scope of the contents disclosed in this application. Unless otherwise stated, all parts, percentages, and ratios reported in the following examples are all based on weight, and all reagents used in the examples are all commercially available or obtained by conventional synthesis, and can be used directly without treatment, and the equipment used in the examples can be commercially available.
[0147] Example 1 Positive electrode plate manufacturing Cathode active material Na 0.44 MnO 2 The conductive agent carbon black and adhesive PVA were thoroughly mixed in an appropriate amount of deionized water in a mass ratio of 96:2:2 to form a uniform positive electrode slurry. The positive electrode slurry was then applied to two surfaces of a positive electrode current collector aluminum foil, and after drying and cold pressing, a positive electrode plate was obtained.
[0148] Negative plate manufacturing The negative electrode active material hard carbon, the conductive agent carbon black, and the adhesive PVA were thoroughly mixed in a mass ratio of 95:2.5:2.5 with an appropriate amount of deionized water and stirred to form a uniform negative electrode slurry. The negative electrode slurry was applied to two surfaces of a negative electrode current collector copper foil, and after drying and cold pressing, a negative electrode plate was obtained.
[0149] Separator manufacturing 3CaO SiO 2 (Dv10 is 4.7μm) was dissolved in dimethyl carbonate to obtain a coating slurry, a gravure roll was immersed in the slurry, and the slurry was filled into the recesses on the surface of the gravure roll as the gravure roll rotated, the slurry on the surface of the gravure roll was scraped off with a doctor blade, leaving only the slurry in the recesses, the gravure roll was rotated to a contact position with a base film (a porous polyethylene film with a thickness of 7μm), and the slurry in the recesses was transferred to one surface of the base film by the action of a press roll. Here, the coating length of the slurry was about 10μm, and the coating thickness was 5μm.
[0150] Electrolyte production Na 2 SO 4 was dissolved uniformly in deionized water to obtain an electrolyte solution with a pH of 7. 2 SO 4 The concentration was 1 mol / L.
[0151] Battery manufacturing The positive electrode plate, separator, and negative electrode plate manufactured as above were sequentially stacked and wound to obtain a wound electrode assembly. The wound electrode assembly was then placed in an aluminum case, and after processes such as end cap welding, electrolyte injection, packaging, standing, and chemical formation, a cylindrical battery was obtained.
[0152] Example 2-19 and Comparative Example 1-2 The manufacturing method of the battery is similar to that of Example 1, except that the manufacturing parameters of the separator are adjusted, and the specific details are as shown in Table 1.
[0153] [Table 1]
[0154] Performance test part (1) Coating hydration heat test A newly manufactured separator was taken for testing, powder was collected from the coating in one area of the separator, and the mass of all the collected samples was weighed, all the collected samples were placed in an ampoule, and a measured amount of water was collected with a syringe in the electric mixer, and then the electric mixer was inserted into the ampoule, and the electric mixer together with the ampoule was placed at the measurement position of the microthermometer, and finally the water in the syringe was injected into the ampoule, and stirring and recording were started, and the total heat release during the test period was obtained. The heat of hydration of the coating (J / g) = total heat release (J) / mass of the sample (g). Here, the test period was 48 hours, the test temperature was room temperature, and the microthermometer was a TAM Air 8-channel microthermometer.
[0155] (2) Coating compression strength test After the battery was fully discharged, the separator was removed and the area where the winding start end was sufficiently hardened was sampled for testing, the separator was placed in a 45°C oven for 30 minutes to dry, and excess electrolyte was removed. Then, the separator was placed in the center position of the lower platen of the YN-200-400 microcomputer compressive strength measuring device, the device was started, and a load was applied continuously at a constant speed until the separator was broken, and the breaking load was recorded. Here, the load speed was 0.4MPa / s to 0.6MPa / s.
[0156] The compressive strength of the coating was calculated according to the formula p=P / A, where p represents the compressive strength of the sample, P represents the breaking load of the sample, and A represents the area of the sample.
[0157] (3) Battery internal temperature test The temperature change inside the battery was monitored by attaching a temperature-sensing cord to the outer surface of the wound electrode assembly, and the maximum temperature inside the battery was recorded. The temperature detector was a KSD301 temperature sensor.
[0158] (4) Rate performance test At 25°C, the battery was charged at a constant current of 1 / 3C up to 2.0V, followed by constant voltage charging until the current reached 0.05C. After leaving the battery stationary for 5 minutes, it was discharged at a constant current of 4C down to 0.5V, and the discharge capacity at 4C rate was recorded.
[0159] (5) Cycle performance test At 25°C, the battery was charged at a constant current of 1 / 3C to 2.0V, and then charged at a constant voltage of 0.05C, at which point the current was fully charged and the charge capacity at this point was recorded as the charge capacity of the first cycle, and after leaving the battery to stand for 5 minutes, it was discharged at a constant current of 4C to 0.5V, which was one cycle charge-discharge process and the discharge capacity at this point was recorded as the discharge capacity of the first cycle. The battery was subjected to cycle charge-discharge testing according to the above method, and the discharge capacity after each cycle was recorded.
[0160] The capacity retention rate (%) of the battery at 500 cycles=discharge capacity at 500th cycle / discharge capacity at 1st cycle×100%.
[0161] Table 2 shows the performance test results of Examples 1-19 and Comparative Examples 1-2.
[0162] [Table 2]
[0163] As can be seen from the test results in Table 2, after the coating containing the hydraulic inorganic material of the present application is infiltrated with the electrolyte, the hydraulic inorganic material in the coating can react with the solvent water to fully harden the coating, thereby significantly increasing the tensile strength of the separator, so that the separator is not easily deformed during the chemical formation process and cycle charge / discharge process of the battery, and can effectively inhibit the collapse of the central hole and the growth of dendrites, thereby improving the safety performance and cycle performance of the battery. After the coating containing the hydraulic inorganic material of the present application is infiltrated with the electrolyte, a suitable amount of heat can also be released, thereby increasing the transmission rate of active ions between the positive and negative electrodes of the battery, and improving the rate performance of the battery.
[0164] In Comparative Example 2, by providing an alumina ceramic coating on the surface of the base film, the compressive strength of the separator can be increased to a certain extent, but the compressive strength of the separator is still low, the collapse of the central hole cannot be effectively suppressed, and the improvement effect on the battery cycle performance is small.
[0165] The above content is merely a specific embodiment of the present application, but the scope of protection of the present application is not limited thereto, and a person skilled in the art can easily think of various equivalent modifications and replacements within the technical scope disclosed in the present application, and all of these modifications and replacements belong to the scope of protection of the present application. Therefore, the scope of protection of the present application should be based on the scope of protection of the claims.
Claims
1. 1. An electrode assembly comprising: A first electrode plate; a second plate of opposite polarity to the first plate; a separator provided between the first electrode plate and the second electrode plate; Where: The electrode assembly is obtained by winding a first electrode plate, a second electrode plate, and a separator; the separator includes a base film and a coating provided on at least a portion of a surface of the base film, the coating includes a hydraulic inorganic material that can react with water to harden, the coating is located within a region of 0 cm to L cm from a winding start end of the separator, and 10≦L≦20; The hydraulic inorganic material comprises at least one compound represented by formula 1: First oxide a Second oxide b Sulfate c Halide Formula 1 Where: 0<a≦6, 0≦b≦4, and 0≦c≦4; The first oxide represents CaO or BaO; The second oxide comprises component 1, which is SiO 2 , Al 2 O 3 , Fe 2 O 3 , or a combination of two or more thereof; Sulfate represents CaSO4, MgSO4, BaSO4, SrSO4, ZnSO4, Al2(SO4)3, FeSO4, Fe2(SO4)3, or a combination of two or more thereof; The electrode assembly, wherein the halide represents CaCl 2 , CaF 2 , or a combination thereof.
2. The second oxide further includes a component 2, which is FeO, MgO, BaO, K 2 O, Na 2 O, TiO 2 , CuO, Cr 2 O 3 , P 2 O 5 , S.O. 3 or a combination of two or more thereof, and the mass ratio of component 1 to component 2 is (95-100):(0-5).
3. The hydraulic inorganic material comprises one or more of the compounds shown in Formula 1-1 to Formula 1-8, CaO.a1 SiO 2 b Sulfate c Halide Formula 1-1 CaO.a2Al 2 O 3 b Sulfate c Halide Formula 1-2 CaO.a3Fe 2 O 3 b Sulfate c Halide Formula 1-3 CaO.a4Al 2 O 3 a5 SiO 2 b Sulfate c Halide Formula 1-4 CaO・a6 Al 2 O 3 ・a7 Fe 2 O 3 b. Sulfates c. Halides Formula 1-5 BaO.a8SiO 2 b Sulfate c Halide Formula 1-6 BaO.a9Al 2 O 3 b Sulfate c Halide Formula 1-7 BaO・a10 Al 2 O 3 a11 SiO 2 b. Sulfates c. Halides Formula 1-8 Where: 0<a1≦6, 0<a2≦6, 0<a3≦6, 0<a4<6, 0<a5<6, and 0<a4+a5≦6; 0<a6<6, 0<a7<6, and 0<a6+a7≦6, 0<a8≦6, 0<a9≦6, 0<a10<6, 0<a11<6, and 0<a10+a11≦6; 0≦b≦4, 0≦c≦4, Sulfate is CaSO 4 , MgSO 4 , BaSO 4 , SrSO 4 , ZnSO 4 , Al 2 (SO 4 ) 3 , FeSO 4 , Fe 2 (SO 4 ) 3 or a combination of two or more of them, The halide is CaCl 2 , CaF 2 3. The electrode assembly according to claim 1 or 2, wherein said electrode assembly comprises:
4. b=0, and / or 4. The electrode assembly according to claim 2 or 3, wherein c=0.
5. The hydraulic inorganic material is 2CaO·SiO 2 , 3CaO·SiO 2 , CaO·Al 2 O 3 , CaO·2Al 2 O 3 , 3CaO·Al 2 O 3 , 6CaO·2Al 2 O 3 , 12CaO·7Al 2 O 3 , CaO·Fe 2 O 3 , 2CaO·Fe 2 O 3 , 2CaO·Al 2 O 3 ·SiO 2 , CaO·Al 2 O 3 ·2SiO 2 , 4CaO·Al 2 O 3 ·Fe 2 O 3 , 6CaO·Al 2 O 3 ·2Fe 2 O 3 , 3CaO·3Al 2 O 3 ·CaSO 4 , 3CaO·3Al 2 O 3 ·MgSO 4 , 3CaO·3Al 2 O 3 ·BaSO 4 , 3CaO·3Al 2 O 3 ·SrSO 4 , 3CaO·3Al 2 O 3 ·ZnSO 4 , 3CaO·3Al 2 O 3 ·Al 2 (SO 4 ) 3 , 3CaO·3Al 2 O 3 ·FeSO 4 , 3CaO·3Al 2 O 3 ·Fe 2 (SO 4 ) 3 , 2CaO.SiO 2 CaSO 4 , 11CaO・7Al 2 O 3 CaF 2 , 3CaO.3Al 2 O 3 CaF 2 , CaO.3Al 2 O 3 ・3CaF 2 , CaO.3Al 2 O 3 ・4CaF 2 , 2BaO.SiO 2 , 3BaO.SiO 2 , BaO.Al 2 O 3 , 3BaO.Al 2 O 3 , BaO.6Al 2 O 3 , BaO.Al 2 O 3 SiO 2 , BaO.Al 2 O 3 2SiO 2 5. The electrode assembly according to claim 1, further comprising one or more of:
6. The electrode assembly according to any one of claims 1 to 5, wherein the hydraulic inorganic material is a particle having a volume particle size Dv10 of 1 µm to 10 µm.
7. 7. The electrode assembly according to claim 1, wherein the mass percentage of the hydraulic inorganic material, relative to the total mass of the coating, is between 95% and 100%.
8. 8. The electrode assembly of claim 1, wherein the coating further comprises an additive, the additive comprising one or more of a water reducer, gypsum, pozzolan, fly ash, slag, silica sand, limestone, and clay.
9. 9. The electrode assembly of claim 8, wherein the mass percentage of the additive is ≦5%, relative to the total mass of the coating.
10. the total thickness of the coating is between 0.5 μm and 5 μm; and / or The electrode assembly according to any one of claims 1 to 9, wherein the base film has a thickness of 5 µm to 12 µm.
11. The electrode assembly according to any one of claims 1 to 10, wherein the base film is one or more selected from a polyolefin porous membrane, a nonwoven fabric, and a glass fiber.
12. The heat of hydration of the coating with water within 2 days is between 300 J / g and 500 J / g; and / or 12. The electrode assembly according to any one of claims 1 to 11, wherein the compressive strength of the coating after reacting with water and curing is between 2500 Pa and 20000 Pa.
13. A battery comprising an electrode assembly and an electrolyte, the electrode assembly being the electrode assembly according to any one of claims 1 to 12, and the electrolyte comprising an electrolyte salt and water.
14. 14. The battery of claim 13, wherein the battery is a lithium ion battery, a sodium ion battery, a potassium ion battery, a zinc ion battery, a calcium ion battery, a magnesium ion battery, an aluminum ion battery, or a hybrid ion battery, and an electrolyte of the hybrid ion battery contains two or more types of active ions, and the active ions are selected from lithium ions, sodium ions, potassium ions, zinc ions, calcium ions, magnesium ions, and aluminum ions.
15. A battery module comprising the battery according to claim 13 or 14.
16. A battery pack comprising one of the battery according to claim 13 or 14 and the battery module according to claim 15.
17. A power consuming device comprising at least one of the battery according to claim 13 or 14, the battery module according to claim 15, and the battery pack according to claim 16.
Citation Information
Patent Citations
Lithium ion secondary battery as well as composition for porus diaphragm layer of the same
CN101276895A
Composition for battery diaphragm, battery diaphragm and lithium-ion secondary battery
CN102206420A
Isolation membrane and lithium ion secondary battery
CN106328865A
Composite isolation film, preparation method of composite isolation film and electrochemical device using composite isolation film
CN109994690A
Inorganic coating slurry coated on diaphragm, manufacturing method and inorganic coating diaphragm
CN112310558A