Starch-based hard carbon material and gradient oxidation annealing preparation method and application thereof

Through drying, sieving and step-by-step oxidation-annealing treatment, the insufficient capacity and morphological breakage of starch-based hard char material in sodium ion batteries is solved, forming a high-performance spherical particle structure, which significantly improves the first week of the battery Coulomb efficiency and capacity, simplifying process and reducing costs.

CN119038527AActive Publication Date: 2024-11-29CHINA UNIV OF MINING & TECH

Patent Information

Application Number
CN202411389426.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-30
Publication Date
2024-11-29
Estimated Expiration
2044-09-30

Smart Images

  • Figure CN119038527A_ABST
    Figure CN119038527A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of sodium ion battery negative electrode materials, and provides a starch-based hard carbon material and a gradient oxidation annealing preparation method and application thereof. The preparation method comprises the following steps: sequentially drying and sieving starch to obtain pretreated starch; carrying out stepped oxidation-annealing on the pretreated starch to obtain a precursor; carrying out carbonization treatment on the precursor to obtain a starch-based hard carbon material; the number of times of stepped oxidation-annealing is 2-10; and annealing to room temperature after each oxidation. According to the method, a multi-stage oxidation layer is constructed in a starch body phase through stepped oxidation treatment; and annealing treatment is carried out, so that stress of starch particles is removed, the starch structure is stabilized, volume shrinkage is relieved, starch fusion is prevented, the oxidation efficiency of next gradient oxidation treatment is enhanced, the oxidation effect in a starch bulk phase is enhanced, and the starch-based hard carbon material with spherical particles, an inert surface and an internal developed closed-pore structure is obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of negative electrode materials for sodium ion batteries, and in particular to a starch-based hard carbon material and a preparation method and application thereof through gradient oxidation annealing. Background Art

[0002] Sodium-ion batteries (SIBs) work similarly to lithium-ion batteries (LIBs) and show great promise in applications with higher energy density materials and lower costs, such as grid power storage systems and low-speed electric vehicles. Meanwhile, the successful experience of LIBs has made the development of cathode materials and electrolytes for SIBs possible. However, graphite, as a mature anode material for commercial LIBs, is not conducive to sodium storage due to the large ionic radius of sodium and the thermodynamic instability of sodium intercalation compounds. Therefore, there is still a need to vigorously develop high-performance anode materials to achieve the commercial application of SIBs.

[0003] Among the recently reported anode materials, hard carbons (HCs) are considered to be the most promising choice for SIBs due to their advantages such as increased interlayer spacing, low working potential, and stable skeleton. In addition, the amorphous microstructure of hard carbon (e.g., short-range crystallites, defects, and internal voids) is + storage provides sufficient active sites. In general, the large specific surface area of ​​the carbon anode formed by hydrocarbons leads to poor first-cycle coulombic efficiency (ICE) because the abundant defects and micropores on the carbon anode surface induce the electrolyte to decompose to form a thick solid electrolyte interphase (SEI) layer. In a full battery, the poor first-cycle coulombic efficiency of the anode will lead to additional consumption of sodium in the cathode material, resulting in lower energy density and higher production cost. Therefore, the practical application of hard carbon urgently needs to achieve high first-cycle coulombic efficiency and high specific capacity.

[0004] Starch-based hard carbon material is a natural spherical biomass material and an excellent sodium ion negative electrode material. However, the cumbersome synthesis process of starch-based hard carbon materials and the low specific capacity at low voltage limit their application in sodium ion batteries. In order to overcome these challenges, the research team has been exploring improvement methods. For example, Li et al. successfully inhibited the foaming and melting of starch by extending the oxidation time, thereby increasing the specific capacity of the material. Chen et al. used maleic anhydride to inhibit the foaming of starch and prepared hard carbon materials with better performance. Wang et al. used CO2 etching technology to regulate the morphology of starch particles and prepared hard carbon materials with higher capacity. Although these methods have achieved certain success in maintaining the spherical morphology of starch and improving capacity, they usually involve the use of oxidizing agents, which are complex and costly. Therefore, further optimizing the preparation method to maintain the spherical morphology and increase capacity remains an important direction for future research. Summary of the invention

[0005] The purpose of the present invention is to overcome the problem that the existing gas-phase oxidation technology has poor effect on starch pretreatment resulting in insufficient hard carbon performance, and to provide a starch-based hard carbon material and its gradient oxidation annealing preparation method and application to solve the problems of low capacity and broken spherical morphology of starch-based hard carbon materials in the prior art.

[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0007] The present invention provides a method for preparing a starch-based hard carbon material, comprising the following steps:

[0008] 1) drying and sieving the starch in sequence to obtain pretreated starch;

[0009] 2) performing stepwise oxidation-annealing on the pretreated starch to obtain a precursor;

[0010] 3) carbonizing the precursor to obtain a starch-based hard carbon material;

[0011] The number of step oxidation-annealing is 2 to 10 times; annealing to room temperature after each oxidation, and the cooling rate of the annealing process is 0.5 to 20°C / min.

[0012] Preferably, the starch comprises corn starch, potato starch, rice starch, pea starch or sorghum starch.

[0013] Preferably, the drying temperature in step 1) is 50-120° C., and the drying time is 6-48 hours.

[0014] Preferably, in step 2), the temperature of the stepwise oxidation is 120-300° C., the time of each oxidation is 1-12 h, and the oxidation temperature increases with the number of oxidation times.

[0015] Preferably, during the step oxidation process, the heating rate is 0.5-5°C / min.

[0016] Preferably, the temperature of the carbonization treatment in step 3) is 1100-2600° C., and the time of the carbonization treatment is 1-8 hours.

[0017] Preferably, during the carbonization treatment, the heating rate is 0.5-10°C / min.

[0018] The invention also provides a starch-based hard carbon material prepared by the preparation method.

[0019] The present invention also provides application of the starch-based hard carbon material in a sodium ion battery.

[0020] The beneficial effects of the present invention include the following:

[0021] 1) The present invention performs low-temperature pretreatment on starch to regulate moisture, which can remove excess moisture on the surface of starch balls and avoid the sticking of starch balls during heating, which causes the spherical morphology to be destroyed; the starch is sifted to control the particle size, which can increase the contact area between the starch balls and the air, further construct an oxygen diffusion channel, and reduce the blockage of the oxygen channel, thereby building a good foundation for the establishment of the oxidation layer.

[0022] 2) The present invention constructs a multi-level oxidation layer in the starch phase through a step-by-step oxidation treatment, and the step-by-step oxidation is conducive to the depth of the oxidation layer and enhances the oxidation effect; the annealing treatment removes stress from starch particles, stabilizes the starch structure, alleviates volume shrinkage, and prevents starch melting, which is conducive to the oxidation efficiency of the next gradient oxidation treatment, thereby obtaining a starch-based hard carbon material with spherical particles, an inert surface, and a developed internal closed-pore structure. The obtained carbon material is used as a negative electrode material for sodium ion batteries. Compared with the carbon material obtained by direct oxidation, it can achieve a significant improvement in the first-week coulomb efficiency and capacity, and significantly improve the low-voltage platform capacity, and has obvious performance advantages.

[0023] 3) The preparation method of the present invention is simple and easy, and solves the problems of complicated synthesis and serious pollution of starch-based hard carbon materials; the prepared starch-based hard carbon negative electrode material has an excellent sodium storage capacity of 450mAh / g for sodium ion batteries, especially the low-potential sodium storage capacity can reach 300mAh / g at a current density of 20mA / g. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 and Figure 2 This is a SEM image of the starch-based hard carbon material of Example 1;

[0025] Figure 3 This is the SEM image of the starch-based hard carbon material of Comparative Example 3;

[0026] Figure 4 This is a charge and discharge curve of a sodium ion button battery prepared from starch-based hard carbon material in Example 1 at a current density of 20 mA / g;

[0027] Figure 5 This is a charge and discharge curve of a sodium ion button battery prepared from starch-based hard carbon material of Comparative Example 1 at a current density of 20 mA / g;

[0028] Figure 6 This is a charge and discharge curve diagram of the sodium ion button battery prepared with starch-based hard carbon material of Comparative Example 3 at a current density of 20 mA / g. DETAILED DESCRIPTION

[0029] The present invention provides a method for preparing a starch-based hard carbon material, comprising the following steps:

[0030] 1) drying and sieving the starch in sequence to obtain pretreated starch;

[0031] 2) performing stepwise oxidation-annealing on the pretreated starch to obtain a precursor;

[0032] 3) carbonizing the precursor to obtain a starch-based hard carbon material;

[0033] The number of step oxidation-annealing is 2 to 10 times; annealing to room temperature after each oxidation, and the cooling rate of the annealing process is 0.5 to 20°C / min.

[0034] In the present invention, the starch comprises corn starch, potato starch, rice starch, pea starch or sorghum starch.

[0035] In the present invention, the drying temperature in step 1) is preferably 50-120°C, more preferably 60-100°C, and more preferably 80-90°C; the drying time is preferably 6-48h, more preferably 10-40h, and more preferably 20-30h.

[0036] In step 2) of the present invention, the temperature of the step oxidation is preferably 120-300°C, more preferably 150-280°C, and more preferably 200-260°C; the time of each oxidation is preferably 1-12h, more preferably 3-10°C, and more preferably 5-8°C; the oxidation temperature increases with the number of oxidation times.

[0037] In the step oxidation process of the present invention, the heating rate is preferably 0.5 to 5° C. / min, more preferably 1 to 4° C. / min, and even more preferably 2 to 3° C. / min.

[0038] In the present invention, the number of step oxidation-annealing is preferably 4 to 8 times, more preferably 5 to 7 times; each oxidation is followed by annealing to room temperature, and the cooling rate during the annealing process is preferably 1 to 15°C / min, more preferably 3 to 12°C / min, and more preferably 5 to 10°C / min.

[0039] In the present invention, the temperature of the carbonization treatment in step 3) is preferably 1100-2600°C, more preferably 1400-2300°C, more preferably 1600-2000°C, and the time of the carbonization treatment is preferably 1-8h, more preferably 3-7h, more preferably 4-5h.

[0040] In the present invention, during the carbonization treatment, the heating rate is preferably 0.5 to 10° C. / min, more preferably 1 to 8° C. / min, and even more preferably 3 to 5° C. / min.

[0041] The invention also provides a starch-based hard carbon material prepared by the preparation method.

[0042] The present invention also provides application of the starch-based hard carbon material in a sodium ion battery.

[0043] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0044] Example 1

[0045] The corn starch was dried at 80°C for 24h and then passed through a 300-mesh sieve. The sieved starch was subjected to four oxidation-annealing treatments in a muffle furnace. The specific process was as follows: the starch was heated to 200°C at a rate of 2°C / min for oxidation for 3h, and then annealed to room temperature at a rate of 2°C / min. After the first oxidation-annealing, the starch was heated to 220°C at a rate of 2°C / min for oxidation for 3h, and then annealed to room temperature at a rate of 2°C / min. After the second oxidation-annealing, the starch was heated to 240°C at a rate of 2°C / min for oxidation for 3h, and then annealed to room temperature at a rate of 1°C / min. After the third oxidation-annealing, the starch was heated to 260°C at a rate of 2°C / min for oxidation for 6h, and then annealed to room temperature at a rate of 1°C / min. After four oxidation-annealings, a precursor was obtained. The precursor was heated to 1400°C at a rate of 2°C / min for carbonization for 3h to obtain a starch-based hard carbon material.

[0046] Example 2

[0047] The corn starch was dried at 80°C for 12h and then passed through a 300-mesh sieve. The sieved starch was subjected to four oxidation-annealing treatments in a muffle furnace. The specific process was as follows: the starch was heated to 120°C at a rate of 2°C / min for oxidation for 12h, and then annealed to room temperature at a rate of 1°C / min. After the first oxidation-annealing, the starch was heated to 200°C at a rate of 2°C / min for oxidation for 3h, and then annealed to room temperature at a rate of 1°C / min. After the second oxidation-annealing, the starch was heated to 240°C at a rate of 2°C / min for oxidation for 3h, and then annealed to room temperature at a rate of 1°C / min. After the third oxidation-annealing, the starch was heated to 300°C at a rate of 2°C / min for oxidation for 6h, and then annealed to room temperature at a rate of 1°C / min. After four oxidation-annealings, a precursor was obtained. The precursor was heated to 1400°C at a rate of 2°C / min and carbonized for 3h to obtain a starch-based hard carbon material.

[0048] Example 3

[0049] The corn starch was dried at 80°C for 24h and then passed through a 300-mesh sieve. The sieved starch was subjected to four oxidation-annealing treatments in a muffle furnace. The specific process was as follows: the starch was heated to 200°C at a rate of 2°C / min for oxidation for 4h, and then annealed to room temperature at a rate of 1°C / min. After the first oxidation-annealing, the starch was heated to 230°C at a rate of 2°C / min for oxidation for 3h, and then annealed to room temperature at a rate of 1°C / min. After the second oxidation-annealing, the starch was heated to 245°C at a rate of 2°C / min for oxidation for 3h, and then annealed to room temperature at a rate of 1°C / min. After the third oxidation-annealing, the starch was heated to 265°C at a rate of 2°C / min for oxidation for 5h, and then annealed to room temperature at a rate of 1°C / min. After four oxidation-annealings, a precursor was obtained. The precursor was heated to 1300°C at a rate of 2°C / min and carbonized for 3h to obtain a starch-based hard carbon material.

[0050] Example 4

[0051] The corn starch was dried at 80°C for 24 hours and then passed through a 300-mesh sieve. The sieved starch was subjected to three oxidation-annealing treatments in a muffle furnace. The specific process was as follows: heating to 210°C at a rate of 3°C / min for oxidation for 3 hours, and then annealing to room temperature at a rate of 3°C / min. After the first oxidation-annealing, the starch was heated to 230°C at a rate of 2°C / min for oxidation for 3 hours, and then annealed to room temperature at a rate of 3°C / min. After the second oxidation-annealing, the starch was heated to 245°C at a rate of 5°C / min for oxidation for 3 hours, and then annealed to room temperature at a rate of 3°C / min. After three oxidation-annealings, a precursor was obtained. The precursor was heated to 1400°C at a rate of 2°C / min and carbonized for 3 hours to obtain a starch-based hard carbon material.

[0052] Example 5

[0053] The potato starch was dried at 80°C for 24h and then passed through a 100-mesh sieve. The sieved starch was subjected to four oxidation-annealing treatments in a muffle furnace. The specific process was as follows: the starch was heated to 215°C at a rate of 5°C / min for oxidation for 3h, and then annealed to room temperature at a rate of 1°C / min. After the first oxidation-annealing, the starch was heated to 230°C at a rate of 2°C / min for oxidation for 3h, and then annealed to room temperature at a rate of 1°C / min. After the second oxidation-annealing, the starch was heated to 245°C at a rate of 5°C / min for oxidation for 3h, and then annealed to room temperature at a rate of 1°C / min. After the third oxidation-annealing, the starch was heated to 265°C at a rate of 5°C / min for oxidation for 6h, and then annealed to room temperature at a rate of 1°C / min. After four oxidation-annealings, the precursor was obtained. The precursor was heated to 2000°C at a rate of 2°C / min for carbonization for 3h to obtain a starch-based hard carbon material.

[0054] Comparative Example 1

[0055] The corn starch was dried at 85°C for 20 hours and then passed through a 300-mesh sieve. The sieved starch was oxidized in a muffle furnace. The specific process was as follows: the temperature was raised to 200°C at a rate of 1°C / min for oxidation for 15 hours to obtain a precursor. The precursor was heated to 1400°C at a rate of 1°C / min for carbonization for 3 hours to obtain a starch-based hard carbon material.

[0056] Comparative Example 2

[0057] The corn starch was dried at 85°C for 20 hours and then passed through a 300-mesh sieve. The sieved starch was oxidized in a muffle furnace. The specific process was as follows: the temperature was raised to 260°C at a rate of 1°C / min for oxidation for 15 hours to obtain a precursor. The precursor was heated to 1400°C at a rate of 1°C / min for carbonization for 3 hours to obtain a starch-based hard carbon material.

[0058] Comparative Example 3

[0059] The corn starch was dried at 80°C for 24 hours and then passed through a 300-mesh sieve. The sieved starch was subjected to four oxidation-no annealing treatments in a muffle furnace. The specific process was as follows: the temperature was raised to 200°C at a rate of 5°C / min for oxidation for 3 hours. After the first oxidation, the starch was heated to 230°C at a rate of 2°C / min for oxidation for 3 hours. After the second oxidation, the starch was heated to 240°C at a rate of 5°C / min for oxidation for 3 hours. After the third oxidation, the starch was heated to 260°C at a rate of 5°C / min for oxidation for 6 hours. After four oxidations without annealing, a precursor was obtained. The precursor was heated to 1400°C at a rate of 2°C / min for carbonization treatment for 3 hours to obtain a starch-based hard carbon material.

[0060] The starch-based hard carbon materials of the embodiment and the comparative example were used to prepare sodium ion button batteries, respectively. The specific steps were as follows: starch-based hard carbon materials, sodium carboxymethyl cellulose and carbon black in a mass ratio of 8:1:1 were mixed and coated on copper foil to prepare electrode sheets, the obtained battery sheet was used as the working electrode, the sodium sheet was used as the counter electrode, and the sodium ion button batteries were assembled in a glove box. The electrochemical performance of the sodium ion button batteries was tested.

[0061] The charge and discharge values ​​of the sodium ion button batteries prepared in the examples and comparative examples at a current density of 20 mA / g are shown in Table 1.

[0062] Table 1 Charging and discharging effects of sodium ion button batteries prepared in the examples and comparative examples at a current density of 20 mA / g

[0063] sample Charging capacity at 20mA / g current density (mAh / g) First week coulomb efficiency / % Example 1 410 88 Example 2 405 87 Example 3 389 86 Example 4 370 87 Example 5 380 89 Comparative Example 1 45 28 Comparative Example 2 325 80 Comparative Example 3 275 78

[0064] The SEM image of the starch-based hard carbon material of Example 1 is as follows: Figure 1 and Figure 2 As shown, the SEM image of the starch-based hard carbon material of Comparative Example 3 is as follows Figure 3 As shown. Figure 1 It can be seen that the starch carbon ball particles have good monodispersity and maintain the natural spherical morphology of starch. In contrast, in the starch-based hard carbon material of Comparative Example 3, the original spherical structure of starch collapsed and broke, indicating that the gradient oxidation annealing technology has significant advantages in maintaining the structure and morphology of starch-based hard carbon materials.

[0065] The charge and discharge curve of the sodium ion button battery prepared from starch-based hard carbon material in Example 1 at a current density of 20 mA / g is shown in FIG. Figure 4 As shown, its capacity below 0.1V is as high as 300mAh·g -1 , and the first week coulombic efficiency reached 88%. The charge and discharge curve of the sodium ion button battery prepared from starch-based hard carbon material in comparative example 1 at a current density of 20 mA / g is shown in the figure below: Figure 5 As shown, its low voltage capacity is only 20mAh·g -1 , the capacity and first-cycle coulombic efficiency are only 35%, indicating that the gradient annealing technology has significant advantages in improving the reversible capacity and first-cycle coulombic efficiency. The charge and discharge curves of the sodium ion button battery prepared from starch-based hard carbon material in comparative example 3 at a current density of 20 mA / g are shown in the figure below: Figure 6 As shown, its low voltage capacity is only 150mAh·g -1 , the capacity and the first-cycle coulombic efficiency were only 76%, indicating that the annealing process played a promoting role in increasing the reversible capacity and the first-cycle coulombic efficiency.

[0066] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing starch-based hard carbon material, It is characterized in that The following steps are included: 1) drying and sieving the starch in sequence to obtain pretreated starch; 2) performing stepwise oxidation-annealing on the pretreated starch to obtain a precursor; 3) carbonizing the precursor to obtain a starch-based hard carbon material; The number of step oxidation-annealing is 2 to 10 times; annealing to room temperature after each oxidation, and the cooling rate of the annealing process is 0.5 to 20°C / min.

2. The preparation method according to claim 1, It is characterized in that The starch comprises corn starch, potato starch, rice starch, pea starch or sorghum starch.

3. The preparation method according to claim 1 or 2, It is characterized in that Step 1) The drying temperature is 50-120° C. and the drying time is 6-48 hours.

4. The preparation method according to claim 3, It is characterized in that In step 2), the temperature of the step oxidation is 120-300° C., the time of each oxidation is 1-12 hours, and the oxidation temperature increases with the number of oxidation times.

5. The preparation method according to claim 4, It is characterized in that During the step oxidation process, the heating rate is 0.5 to 5°C / min.

6. The preparation method according to claim 1 or 5, It is characterized in that Step 3) The temperature of the carbonization treatment is 1100-2600° C., and the time of the carbonization treatment is 1-8 hours.

7. The preparation method according to claim 6, It is characterized in that During the carbonization process, the heating rate is 0.5-10°C / min.

8. The starch-based hard carbon material prepared by the preparation method according to any one of claims 1 to 7.

9. Use of the starch-based hard carbon material according to claim 8 in sodium ion batteries.

Citation Information

Patent Citations

  • Preparation methods for high capacity biomass hard carbon anode material of sodium ion battery

    CN109921018A

  • Preparation method and application of biomass carbon material

    CN111470487A

  • Annealed modified starch and preparation method and application thereof

    CN113603900A

  • Hard carbon negative electrode material, preparation method thereof and lithium ion battery

    CN115084513A

  • Sodium-ion battery hard carbon negative electrode material with ultralow specific surface area and preparation method of sodium-ion battery hard carbon negative electrode material

    CN115207350A

Cited By

  • Sulfur-doped starch-based hard carbon material, preparation method and application thereof, and sodium ion battery

    CN119637849A

  • Starch-based hard carbon material as well as preparation method and application thereof

    CN119774579A

  • Starch-based hard carbon material and preparation method and application thereof

    CN119774579B

  • Asphalt-modified starch-based hard carbon negative electrode material and preparation method thereof

    CN121044568A

  • Sodium-ion battery biomass derived hard carbon negative electrode material and preparation method and application thereof based on cross-linking pore-forming

    CN121317693A