Composite metal foil, metal-clad laminated plate and circuit board
Through the design of composite metal foil, the existing temperature control components and thermistors have large volumes and ease of failure, and the temperature monitoring of small-volume circuit boards is realized, ensuring the stability of resistance value and the reliability of temperature monitoring.
Patent Information
- Application Number
- CN202411176521.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-11-29
AI Technical Summary
The existing temperature control components and surface-mounted thermistors of existing electronic components are large in size, and the temperature control of small-volume circuit boards cannot be achieved. The embedded resistors are prone to failure during the circuit board production, resulting in the inability to effectively monitor electronic components. temperature.
A composite metal foil is used, including a base layer and a resistive layer. The resistive layer is located on one side of the base layer. It is pressed onto the substrate by a side facing away from the base layer to form a circuit board, and covers part of the resistor after the solder resist ink is installed. The layer ensures that the change rate of resistance is less than or equal to 10%, so as to avoid the damage to the thermal effect of solder resist ink and realize the temperature monitoring of small electronic components.
The production and temperature monitoring of small and fine lines are realized, the reliability and stability of the temperature monitoring circuit is improved, the stability of the resistance value is ensured, the damage to the resistance layer by solder resist ink is avoided, and the service life is extended.
Smart Images

Figure CN119049818A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of electronic technology, and in particular to a composite metal foil, a metal-clad laminate and a circuit board. Background Art
[0002] With the continuous advancement of the electronics industry and information technology, electronic components are developing towards high performance and miniaturization. Electronic components will generate heat during operation, and the increase in temperature will affect the normal operation of electronic components. Therefore, it is necessary to control the temperature of electronic components to keep them running normally.
[0003] At present, temperature control elements or surface-mounted thermistors are usually set on the surface of electronic components. However, the temperature control elements and surface-mounted thermistors are large in size and cannot realize the production of temperature control circuits for small-volume circuit boards. In addition, conventional embedded resistors are prone to failure during the circuit board production process, resulting in the inability of the resistors in the circuit to monitor the temperature of electronic components. Summary of the invention
[0004] The present invention provides a composite metal foil, a metal-clad laminate and a circuit board, which can avoid the damage of solder resist ink to the thermal sensitive effect thereof, ensure the stability of resistance value, and can also be used in fine circuit boards to realize temperature monitoring of small electronic components.
[0005] According to one aspect of the present invention, there is provided a composite metal foil, the composite metal foil comprising:
[0006] Base layer and resistor layer;
[0007] The resistor layer is located on one side of the base layer, and the composite metal foil is used to be pressed onto the substrate through the side of the resistor layer facing away from the base layer to form a circuit board; wherein, after the circuit board is provided with solder resist ink, part of the resistor layer is covered, and the rate of change of the resistance of the resistor layer is less than or equal to 10% compared with before the solder resist ink is provided.
[0008] Optionally, the composite metal foil is arranged in a circuit board, and after the solder resist ink is arranged on the circuit board, after the temperature rises from 25° C. to 125° C. and then drops to 25° C., the resistance change rate of the resistance layer is less than or equal to 10%.
[0009] Optionally, the composite metal foil is arranged in the circuit board, and after the circuit board is provided with solder resist ink, the temperature rises from 25°C to 125°C and then drops to 25°C as one cycle, and after N cycles, the temperature rises from 25°C to 125°C and then drops to 25°C, and the resistance change rate of the resistance layer is less than or equal to 20%;
[0010] Wherein, N is an integer greater than or equal to 500.
[0011] Optionally, a composite metal foil is set in a circuit board. After the circuit board is set with solder resist ink, the temperature rises from 25°C to 125°C and then drops to 25°C as one cycle. After N cycles, in the process of the temperature rising from 25°C to 125°C and then dropping to 25°C, the resistance change rate of the resistance layer is greater than or equal to 3% for every 25°C temperature change.
[0012] Optionally, the resistance layer includes at least one element of Ni, Cr, Zn, Al, P, Si, Fe, N, O and Cu.
[0013] Optionally, the content of Cr in the resistance layer is less than or equal to 20%, the content of Fe is less than or equal to 30%, the content of Ni is greater than or equal to 30%, and the content of O is less than or equal to 60%.
[0014] Optionally, the thickness of the base layer is greater than or equal to 3 microns and less than or equal to 70 microns;
[0015] Optionally, the roughness of a side of the substrate layer close to the resistor layer is greater than or equal to 0.5 micrometers and less than or equal to 10 micrometers;
[0016] Optionally, the thickness of the resistance layer is greater than or equal to 5 nanometers and less than or equal to 1 micrometer.
[0017] Optionally, the composite metal foil further comprises:
[0018] The peeling layer and the carrier layer, the peeling layer is arranged on a side of the base layer facing away from the resistor layer, the carrier layer is arranged on a side of the peeling layer facing away from the base layer, and the carrier layer can be peeled off from the base layer.
[0019] Optionally, the composite metal foil further comprises:
[0020] At least one of the absorption layer, the first resistance layer and the adjustment layer is stacked with the base layer and the resistance layer.
[0021] According to another aspect of the present invention, a metal-clad laminate is provided. The metal-clad laminate comprises the composite metal foil according to any embodiment of the present invention.
[0022] According to another aspect of the present invention, a circuit board is provided. The circuit board comprises the composite metal foil according to any embodiment of the present invention. The composite metal foil is arranged on the surface of a single-layer or multi-layer circuit board or inside a multi-layer board.
[0023] In the embodiment of the present invention, the composite metal foil is pressed onto the substrate through the side of the resistor layer facing away from the base layer to form a circuit board. After the circuit board is provided with solder resist ink, part of the resistor layer is covered. Compared with before the solder resist ink is provided, the resistance change rate of the resistor layer is less than or equal to 10%. After covering with solder resist ink, the resistance value of the resistor changes stably, avoiding the damage of the solder resist ink to its thermal sensitive effect. In addition, since the composite metal foil is small in size, it can meet the production requirements of tiny fine circuits. In addition, the composite metal foil of the embodiment of the present invention has a stable resistance value after covering with solder resist ink. Such a composite metal foil is used in a fine circuit board, and the operating temperature of the components to be tested on the circuit board can be monitored, thereby improving the reliability of the temperature monitoring circuit.
[0024] It should be understood that the contents described in this section are not intended to identify the key or important features of the embodiments of the present invention, nor are they intended to limit the scope of the present invention. Other features of the present invention will become easily understood through the following description. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0026] Figure 1 is a schematic structural diagram of a composite metal foil provided by an embodiment of the present invention;
[0027] Figure 2 This is a schematic diagram of a structure of a composite metal foil embedded in a circuit board provided by an embodiment of the present invention;
[0028] Figure 3 This is a physical picture of a composite metal foil embedded in a circuit board provided by an embodiment of the present invention;
[0029] Figure 4 It is a schematic diagram of the structure of a composite metal foil after etching provided by an embodiment of the present invention;
[0030] Figure 5 is a schematic structural diagram of another composite metal foil provided by an embodiment of the present invention;
[0031] Figure 6 is a schematic structural diagram of another composite metal foil provided by an embodiment of the present invention;
[0032] Figure 7 is a schematic structural diagram of a composite metal foil provided by an embodiment of the present invention;
[0033] Figure 8is a schematic structural diagram of another composite metal foil provided by an embodiment of the present invention;
[0034] Fig. 9 This is a schematic diagram after etching the base layer and the resistor layer;
[0035] Fig.10 is a schematic diagram after etching the base layer;
[0036] Fig.11 This is a schematic diagram after removing the second dry film. DETAILED DESCRIPTION
[0037] In order to enable those skilled in the art to better understand the scheme of the present invention, the technical scheme in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
[0038] It should be noted that the terms "first", "second", etc. in the specification and claims of the present invention and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchanged where appropriate, so that the embodiments of the present invention described herein can be implemented in an order other than those illustrated or described herein. In addition, any variation of the terms "including" and "having" is intended to cover non-exclusive inclusions, for example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.
[0039] Figure 1 It is a schematic structural diagram of a composite metal foil provided in an embodiment of the present invention. Figure 2 It is a schematic diagram of the structure of a composite metal foil embedded in a circuit board provided by an embodiment of the present invention. Figure 3 This is a physical picture of a composite metal foil embedded in a circuit board provided by an embodiment of the present invention. Figure 1-Figure 3 The composite metal foil comprises: a base layer 20 and a resistor layer 10; the resistor layer 10 is located on one side of the base layer 20, and the composite metal foil 1 is used to be pressed onto a substrate 60 through a side of the resistor layer 10 facing away from the base layer 20 to form a circuit board; wherein, after the circuit board is provided with solder resist ink 70, a portion of the resistor layer 10 is covered, and the rate of change of the resistance of the resistor layer 10 is less than or equal to 10% relative to before the solder resist ink 70 is provided.
[0040] The composite metal foil 1 is embedded in the circuit board, and the material of the base layer 20 is a conductive material or a dielectric material. The base layer 20 may be a single-layer structure or a multi-layer structure. The conductive material includes but is not limited to at least one of copper, aluminum, titanium, zinc, iron, nickel, chromium, cobalt, silver and gold. Specifically, the base layer 20 may be copper foil, aluminum foil, titanium foil, zinc foil, iron foil, nickel foil, chromium foil, cobalt foil, silver foil or gold foil, or may be an alloy foil containing at least two of copper, aluminum, titanium, zinc, iron, nickel, chromium, cobalt, silver and gold, or may be a composite foil composed of at least two of copper foil, aluminum foil, titanium foil, zinc foil, iron foil, nickel foil, chromium foil, cobalt foil, silver foil and gold foil. The dielectric material includes but is not limited to PET (Polyethylene Terephthalate), PP (Polypropylene), PS (Polystyrene), ABF (Acrylonitrile-Butadiene-Styrene Terpolymer, polyacrylamide / styrene / styrene sulfate terpolymer) film, BT resin, polyacrylic acid, polyurethane, polyimide, etc., which are not listed in detail here. Among them, BT resin is a thermosetting resin formed by adding bismaleimide (BMI) and triazine as the main resin components, and epoxy resin, polyphenylene ether resin (PPE) or allyl compounds as modified components. In the base layer 20 with a multi-layer structure, the materials between different layers can be the same or different.
[0041] The base layer 20 plays a bearing and conductive role for the resistor layer 10, so that the resistor layer 10 can be formed on its surface and can be used normally to make circuits. The resistor layer 10 can be formed by spraying, electroplating, chemical plating, evaporation plating, vacuum sputtering or other deposition methods. For example, it can be processed on the base layer 20 by vacuum sputtering. The thickness of the resistor layer sputtering can be accurately controlled by the vacuum sputtering process to make the resistance of the resistor layer 10 more stable and uniform. Electroplating, chemical plating, physical vapor deposition, chemical vapor deposition or other formation methods can also be used. The resistance change rate of the resistor layer 10 is the change rate of the resistance of the resistor layer 10 after it is covered with solder resist ink 70 relative to the resistance of the resistor layer 10 when it is not covered with solder resist ink 70; that is, the resistance change rate of the resistor layer 10 is equal to the absolute value of the difference between the resistance of the resistor layer 10 before covering the solder resist ink 70 and the resistance of the resistor layer 10 after covering the solder resist ink 70, divided by the resistance of the resistor layer 10 before covering the solder resist ink 70.
[0042] It should be noted that solder resist ink needs to be applied during circuit board processing. Solder resist ink 70 has multiple properties such as good insulation performance, high temperature resistance, chemical corrosion resistance, adhesion, optical performance and environmental protection. Solder resist ink 70 covers the circuit board to form a uniform insulating layer, which can protect the circuit, effectively isolate different circuit tracks, and prevent current from forming paths where it should not flow, thereby ensuring the normal operation of electronic equipment.
[0043] Figure 4 Schematic diagram of the structure of a composite metal foil after etching provided by an embodiment of the present invention. Figure 2-Figure 4 After the composite metal foil is pressed onto the substrate, the surface of the base layer 20 away from the resistor layer 10 is etched, and after etching, the base layer 20 and the resistor layer 10 together form an embedded thin film resistor in the circuit. Then, the side of the base layer 20 away from the substrate and the side of the substrate away from the resistor layer 10 are covered with solder resist ink.
[0044] Specifically, the processing technology of solder resist ink is as follows: firstly, the composite metal foil and the substrate are washed with water, then the solder resist ink is covered on the side of the base layer 20 away from the substrate and the side of the substrate away from the resistor layer 10, the solder resist ink on the side of the base layer 20 away from the substrate is baked at 75°C for 43 minutes, then exposed and developed, and finally baked at 155°C for 60 minutes. The solder resist ink on the side of the substrate away from the resistor layer 10 is baked at 75°C for 25 minutes.
[0045] Specifically, the composite metal foil 1 is a thin film resistor. The material used for the resistor layer 10 of the composite metal foil 1 includes one element, two or more elements selected from Ni, Cr, Zn, P, Si, Al, Fe, N, O and Cu. The ratio of different elements is adjusted so that the resistor layer 10 has the properties of solder resist ink and thermistor properties. The composite metal foil is pressed on the substrate 60 through the side of the resistor layer 10 facing away from the base layer 20 to form a circuit board circuit. After the circuit board is provided with solder resist ink 70, part of the resistor layer 10 is covered. The performance of the resistor layer 10 having solder resist ink is reflected in that the resistance change rate of the resistor layer 10 after the resistor layer is provided with solder resist ink 70 is less than 10% relative to before the solder resist ink 70 is provided. After covering the solder resist ink 70, the resistance value of the resistor layer 10 changes relatively stably without jumps, thereby avoiding the damage of the solder resist ink 70 to its thermal effect. Therefore, the working temperature of the components to be tested can be monitored in real time through the thermistor properties of the resistor layer 10.
[0046] In the embodiment of the present invention, the composite metal foil 1 is pressed onto the substrate 60 through the side of the resistance layer 10 facing away from the base layer 20 to form a circuit board. After the circuit board is provided with solder resist ink 70, part of the resistance layer 10 is covered, and the resistance change rate of the resistance layer 10 is limited to be less than or equal to 10% before the solder resist ink 70 is provided. After covering with solder resist ink 70, the resistance value change of the composite metal foil 1 before and after pressing is guaranteed to be stable, and the damage of the thermal sensitive effect of the solder resist ink 70 to the composite metal foil 1 is avoided. In addition, since the composite metal foil 1 is small in size, it can meet the production requirements of tiny fine circuits. In addition, the composite metal foil 1 of the embodiment of the present invention has a stable resistance value after being covered with solder resist ink 70. Such a composite metal foil 1 is used in a fine circuit board, and the operating temperature of the components to be tested on the circuit board can be monitored, thereby improving the reliability of the temperature monitoring circuit.
[0047] See also Figure 2 Optionally, based on the above embodiment, the composite metal foil 1 is arranged in the circuit board, and after the solder resist ink 70 is arranged on the circuit board, after the temperature rises from 25°C to 125°C and then drops to 25°C, the resistance change rate of the resistor layer 10 is less than or equal to 10%.
[0048] When the temperature rises from 25° C. to 125° C. and then drops to 25° C., the change rate of the resistance value of the resistor layer 10 relative to the initial resistance value of the resistor layer 10 after being covered with the solder resist ink 70 is less than or equal to 10%.
[0049] It should be noted that the resistance change rate of the resistor layer here = |initial resistance value of the resistor layer 10 after covering with solder resist ink - resistance value after temperature change after covering with solder resist ink| / initial resistance value of the resistor layer 10 after covering with solder resist ink, and the initial resistance value of the resistor layer 10 after covering with solder resist ink 70 is the resistance value of the resistor layer 10 at an initial temperature of 25°C when the temperature cycle is not performed after covering with solder resist ink 70.
[0050] After the composite metal foil 1 is processed in the circuit board and the solder resist ink 70 is set, the temperature rises from 25°C to 125°C, and the resistance value of the resistor layer 10 decreases regularly. For example, the change trend is a straight line or a curve, and the temperature drops from 125°C to 25°C, and the resistance value of the resistor layer 10 increases linearly, and the resistance value of the resistor layer 10 can return to the vicinity of the initial resistance value, and the change rate of the initial resistance value of the resistor layer 10 is within 10%. Within this change rate, it can be ensured that the embedded thermistor made of the composite metal foil 1 can recover the resistance recovery accuracy under the temperature cycle under the use state, realize the temperature monitoring function of the circuit board, and the embedded thermistor made of the composite metal foil 1 has a longer service life, ensures the working accuracy, and improves the working reliability.
[0051] See also Figure 2Further, on the basis of the above embodiment, the composite metal foil 1 is arranged in the circuit board to make an embedded thermistor. After the circuit board is provided with the solder resist ink 70, the temperature rises from 25°C to 125°C and then drops to 25°C as one cycle. After N cycles, the temperature rises from 25°C to 125°C and then drops to 25°C, and the resistance change rate of the resistor layer 10 is less than or equal to 20%; wherein N is an integer greater than or equal to 500.
[0052] The temperature rises from 25°C to 125°C and then drops to 25°C. After more than 500 cycles, the change rate of the initial resistance value of the resistor layer 10 is within 20%. After multiple cycles, the resistance value of the resistor layer 10 can still be restored to near the initial resistance value, and the resistance value still changes steadily, thereby ensuring that the service life of the composite metal foil 1 is longer.
[0053] See also Figure 2 Optionally, based on the above embodiment, the composite metal foil 1 is arranged in the circuit board, and after the circuit board is provided with the solder resist ink 70, the temperature rises from 25°C to 125°C and then drops to 25°C as one cycle, and after N cycles, in the process of the temperature rising from 25°C to 125°C and then dropping to 25°C, the resistance change rate of the resistor layer 10 is greater than or equal to 3% for every 25°C change in temperature.
[0054] For example, when the temperature rises from 25°C to 50°C, the resistance of the resistor layer changes by 3% or more relative to the resistance at 25°C. When the temperature drops from 125°C to 100°C, the resistance of the resistor layer 10 changes by 3% or more relative to the resistance at 125°C, that is, for every 25°C change in temperature, the resistance of the resistor layer 10 changes by 3% or more relative to the resistance before the temperature changes by 25°C.
[0055] In the embodiment of the present invention, as the temperature increases, the resistance of the resistor layer 10 will change, and as the temperature decreases, the resistance of the resistor layer 10 will also change. In the process of the temperature rising from 25°C to 125°C and then falling to 25°C, the resistance change rate of the resistor layer 10 is greater than or equal to 3% for every 25°C change in temperature, so that the resistance value of the resistor layer 10 changes greatly, the detection accuracy is higher, the operating temperature of the components to be tested can be better monitored, and the accuracy of temperature monitoring is improved.
[0056] See also Figure 1 and Figure 2 Optionally, based on the above embodiment, the resistance layer 10 includes at least one element of Ni, Cr, Zn, Al, P, Si, Fe, N, O and Cu.
[0057] Specifically, the resistor layer 10 includes at least one element of Ni, Cr, Zn, Al, P, Si, Fe, N, O and Cu, which can achieve the performance of the resistor layer 10 being resistant to solder resist ink and the performance of resistance changing with temperature.
[0058] Exemplarily, the material of the resistor layer 10 is a nickel-chromium-iron alloy, and oxygen is added to form a metal oxide, that is, the resistor layer 10 includes oxides of nickel, chromium and iron. When the resistor layer 10 includes at least one element of Ni, Cr, Zn, P, Al, Si, Fe and Cu, it may also include oxides of at least one element of Ni, Cr, Zn, Al, P, Si, Fe and Cu.
[0059] See also Figure 1 and Figure 2 Optionally, based on the above embodiment, the content of Cr element in the resistance layer 10 is less than or equal to 20%, the content of Fe element is less than or equal to 30%, the content of Ni is greater than or equal to 30%, and the content of O element is less than or equal to 60%.
[0060] Specifically, the content of Cr in the resistor layer 10 is less than or equal to 20%, the content of Fe is less than or equal to 30%, the content of Ni is greater than or equal to 30%, and the content of O is less than or equal to 60%. By adjusting the ratio of the elements, the performance of the resistor layer 10 in resisting soldering ink and the performance of the resistance of the resistor layer 10 changing with temperature can be achieved, and the variable resistance performance of the thermistor can be ensured, so as to monitor the operating temperature of the components to be tested on the circuit board and improve the reliability of the temperature monitoring circuit.
[0061] See also Figure 1 Optionally, based on the above embodiment, the composite metal foil 1 further includes: the thickness of the base layer 20 is greater than or equal to 3 microns and less than or equal to 70 microns.
[0062] Specifically, if the thickness of the base layer 20 is too large or too small, it will increase the difficulty of etching and affect the etching efficiency and quality of the circuit board. By setting the thickness of the base layer 20 to be greater than or equal to 3 microns and less than or equal to 70 microns, the base layer of such thickness ensures the support effect. When the base layer 20 is a copper layer, it can be used to directly etch the temperature measurement circuit to meet the circuit etching requirements.
[0063] See also Figure 1 Optionally, based on the above embodiment, the roughness of the side of the base layer 20 close to the resistance layer 10 is greater than or equal to 0.5 microns and less than or equal to 10 microns.
[0064] Specifically, the roughness of the side of the base layer 20 close to the resistor layer 10 is greater than or equal to 0.5 microns and less than or equal to 10 microns. The roughness within the above range can improve the bonding force between the base layer 20 and the resistor layer 10, avoid the skin effect, and meet the application of high-frequency circuits.
[0065] See also Figure 1 Optionally, based on the above embodiment, the thickness of the resistance layer 10 is greater than or equal to 5 nanometers and less than or equal to 1 micrometer.
[0066] Specifically, the thickness of the resistor layer 10 is greater than or equal to 5 nanometers and less than or equal to 1 micron. If the thickness of the resistor layer 10 is too large or too small, it will affect the resistance of the resistor layer, thereby affecting the recovery accuracy of the resistance of the resistor layer 10 and the accuracy of the monitoring circuit. Therefore, by setting the thickness of the resistor layer 10 to be greater than or equal to 5 nanometers and less than or equal to 1 micron, the resistance of the resistor layer can be within a suitable range, so that the recovery accuracy of the resistance of the resistor layer 10 and the accuracy of the monitoring circuit are both high, which can meet the requirements of monitoring the temperature of the component to be measured on the circuit board.
[0067] Figure 5 is a schematic diagram of the structure of another composite metal foil provided by an embodiment of the present invention, see Figure 5 Optionally, the composite metal foil further includes: a peeling layer 80 and a carrier layer 90, wherein the peeling layer 80 is disposed on a side of the base layer 20 facing away from the resistor layer 10, and the carrier layer 90 is disposed on a side of the peeling layer 80 facing away from the base layer, and the carrier layer 90 can be peeled off from the base layer 20.
[0068] The material used for the carrier layer 90 is a conductive material. The conductive material includes but is not limited to at least one of copper, aluminum, titanium, zinc, iron, nickel, chromium, cobalt, silver and gold. A peeling layer 80 is formed on one side of the carrier layer 90, and a base layer 20 and a resistor layer 10 are sequentially formed on the side of the peeling layer 80 away from the carrier layer 90. The surface of the resistor layer 10 away from the base layer 20 is pressed with the substrate to form a circuit board. The thickness of the carrier layer 90 is relatively thick. The carrier layer 90 is peeled off by the peeling layer 80, so that the thickness of the resistor layer 10 and the base layer 20 becomes thinner. The ultra-thin resistor layer 10 and the base layer 20 are convenient for making thermistors, and the peeled carrier layer 90 can be used to make conductive circuits.
[0069] Figure 6 It is a schematic diagram of the structure of another composite metal foil provided by an embodiment of the present invention. Figure 7 It is a schematic diagram of a composite metal foil provided in an embodiment of the present invention. Figure 8 Schematic diagram of another composite metal foil provided by an embodiment of the present invention. Figure 6-Figure 8Optionally, the composite metal foil further includes: at least one layer of an absorption layer 40 , a first resistance layer 50 and an adjustment layer 30 stacked with the base layer 20 and the resistance layer 10 .
[0070] Specifically, the absorption layer 40 can be disposed between the resistor layer 10 and the base layer 20, or on the surface of the resistor layer 10 away from the base layer, or on the surface of the base layer 20 away from the resistor layer 10, and the embodiment of the present invention is not limited to this. The material used for the absorption layer includes a polymer material, which can be used to absorb electromagnetic waves.
[0071] The first resistor layer 50 is located on the side of the resistor layer 10 away from the base layer 20. The first resistor layer 50 can also be located between the resistor layer 10 and the base layer 20. As the temperature changes, the resistance value of the first resistor layer 50 remains unchanged. The first resistor layer 50 is used to adjust the overall resistance of the composite metal foil, so that the basic resistance is larger, thereby improving the temperature measurement accuracy.
[0072] The adjustment layer 30 can be arranged on the side of the resistor layer 10 away from the base layer 20, and the side of the resistor layer 10 away from the base layer 20 is pressed on the substrate to form a circuit board; the function of the adjustment layer 30 is to improve the bonding force between the composite metal foil and the substrate to prevent the composite metal foil and the substrate from falling off. The material of the adjustment layer 30 may include at least one of a silane coupling agent, an aluminate coupling agent, a metal composite coupling agent, a phosphate coupling agent, a borate coupling agent, polyethylene (PE), polypropylene (PP) and polyvinyl chloride (PVC).
[0073] An embodiment of the present invention further provides a metal-clad laminate, which includes the composite metal foil described in any embodiment of the present invention.
[0074] The metal-clad laminate of the present invention has the same beneficial effects as the composite metal foil of any embodiment of the present invention.
[0075] See also Figure 2 An embodiment of the present invention further provides a circuit board 2, the circuit board 2 includes the composite metal foil 1 described in any embodiment of the present invention, the composite metal foil 1 is arranged on the surface of a single-layer or multi-layer circuit board 2 or inside a multi-layer board, and the composite metal foil 1 can monitor the temperature of the circuit board 2 to prevent the circuit board 2 from being damaged by excessive temperature.
[0076] The present invention also provides a process for forming the circuit board in the above embodiment. Figure 9-11 shows the formation process of the circuit board, Fig. 9 This is a schematic diagram after etching the base layer and the resistor layer. Fig.10 This is a schematic diagram after etching the base layer. Fig.11 This is a schematic diagram after removing the second dry film, refer to Fig. 9After the composite metal foil is attached to the surface of the substrate 60, the first dry film 101 can be provided, and then the base layer 20 and the resistor layer 10 can be etched with an acid solution to form an I-shaped base layer 20 and a resistor layer 10. Fig.10 Then, after the second dry film 102 is disposed on the surface of the base layer 20, the base layer 20 is etched with an alkaline solution to break the middle of the I-shaped base layer 20 to form Figure 8 The structure is then removed, and the second dry film 102 is removed. Fig.11 As shown, in Fig.11 The base layer 20, the resistor layer 10 and the substrate 60 are covered with solder resist ink to form Figure 2 The embedded composite metal foil circuit board is shown.
[0077] Example 1
[0078] A composite copper foil is a double-layer laminated structure of a copper layer and a resistor layer. The components of the resistor layer include Ni, Cr, Fe, and O. The thickness of the resistor layer is 200nm, and the thickness of the copper layer is 20μm. After being pressed on a PTFE substrate, solder resist ink is applied. The resistance change rate before and after applying solder resist ink is 4.8%. After the temperature monitoring circuit is made, the resistance value returns to stability and the circuit works normally.
[0079] Example 2
[0080] A composite copper foil, which is different from Example 1 in that the components of the resistance layer include Ni and Fe, wherein the mass percentage of Fe is 21.4%, the thickness of the resistance layer is 330nm, and the thickness of the copper layer is 15μm. After being pressed on a PTFE substrate, solder resist ink is applied. The resistance change rate before and after applying solder resist ink is 7.1%. The temperature is increased from 25°C to 125°C and then decreased to 25°C for 300 cycles, and the resistance change rate of the composite copper foil is 6.7%. After the temperature monitoring circuit is made, the resistance recovery accuracy meets the use requirements, and the circuit works normally.
[0081] Example 3
[0082] A composite copper foil, which is different from Example 2 in that the components of the resistance layer include Ni, Cr, Fe, O, and N, the thickness of the resistance layer is 310nm, and the thickness of the copper layer is 18μm. The mass percentage of Fe is 11.4%, and after being pressed on a PTFE substrate, solder resist ink is brushed. The resistance change rate before and after brushing the solder resist ink is 1.4%. The temperature rises from 25°C to 125°C and then drops to 25°C for 50 cycles, and the resistance change rate of the composite copper foil is 2.7%. After the temperature monitoring circuit is made, the resistance recovery accuracy meets the use requirements, and the circuit works normally.
[0083] Example 4
[0084] A composite copper foil includes a three-layer structure of an adjustment layer, a resistance layer, and a copper layer. The adjustment layer is a silane coupling agent. The components of the resistance layer include Ni, Cr, Fe, O, and N. The thickness of the resistance layer is 800nm, and the thickness of the copper layer is 18μm. The mass percentage of Fe is 25.6%. After being pressed on a PTFE substrate, solder resist ink is applied. The resistance change rate before and after applying solder resist ink is 3.9%. The temperature rises from 25°C to 125°C and then drops to 25°C for 1000 cycles, and the resistance change rate of the composite copper foil is 9.7%. After the temperature monitoring circuit is made, the resistance recovery accuracy meets the use requirements, and the circuit works normally.
[0085] Comparative Example 1
[0086] Different from Example 1, the material of the resistance layer of the buried copper foil includes Ni and P, and the resistance change rate before and after applying solder resist ink is 24.1%. After the temperature monitoring circuit is made, the error is too large and the circuit cannot work.
[0087] Comparative Example 2
[0088] Different from Example 1, the resistance layer of the buried copper foil includes Ni, Cr, and Fe, wherein the Cr content is 45%, the Fe content is 41%, and the Cr content is 14%. The change rate of the resistance reduction before and after applying the solder resist ink is 31.5%. If the change rate exceeds the range, the circuit board cannot monitor the high temperature of the chip.
[0089] It should be understood that the various forms of processes shown above can be used to reorder, add or delete steps. For example, the steps described in the present invention can be executed in parallel, sequentially or in different orders, as long as the desired results of the technical solution of the present invention can be achieved, and this document does not limit this.
[0090] The above specific implementations do not constitute a limitation on the protection scope of the present invention. It should be understood by those skilled in the art that various modifications, combinations, sub-combinations and substitutions can be made according to design requirements and other factors. Any modification, equivalent substitution and improvement made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A composite metal foil, characterized in that: The composite metal foil comprises: Base layer and resistor layer; The resistor layer is located on one side of the base layer, and the composite metal foil is used to be pressed onto the substrate through the side of the resistor layer facing away from the base layer to form a circuit board; wherein, after the circuit board is provided with solder resist ink, a portion of the resistor layer is covered, and the rate of change of the resistance of the resistor layer is less than or equal to 10% compared with before the solder resist ink is provided.
2. The composite metal foil according to claim 1, characterized in that: The composite metal foil is arranged in a circuit board. After the circuit board is provided with solder resist ink, after the temperature rises from 25° C. to 125° C. and then drops to 25° C., the resistance change rate of the resistance layer is less than or equal to 10%.
3. The composite metal foil according to claim 1, characterized in that: The composite metal foil is arranged in the circuit board, and after the circuit board is provided with solder resist ink, the temperature rises from 25°C to 125°C and then drops to 25°C as one cycle, and after N cycles, the temperature rises from 25°C to 125°C and then drops to 25°C, and the resistance change rate of the resistance layer is less than or equal to 20%; Wherein, N is an integer greater than or equal to 500.
4. The composite metal foil according to claim 1, characterized in that: The composite metal foil is arranged in a circuit board. After the circuit board is provided with solder resist ink, a cycle is defined as a temperature rise from 25°C to 125°C and then drop to 25°C. After N cycles, in a process in which the temperature rises from 25°C to 125°C and then drops to 25°C, the resistance change rate of the resistance layer is greater than or equal to 3% for every 25°C change in temperature.
5. The composite metal foil according to claim 1, characterized in that: The resistance layer includes at least one element of Ni, Cr, Zn, Al, P, Si, Fe, N, O and Cu; Preferably, the content of Cr in the resistor layer is less than or equal to 20%, the content of Fe is less than or equal to 30%, the content of Ni is greater than or equal to 30%, and the content of O is less than or equal to 60%.
6. The composite metal foil according to claim 1, characterized in that: The thickness of the base layer is greater than or equal to 3 microns and less than or equal to 70 microns; Preferably, the roughness of the side of the substrate layer close to the resistor layer is greater than or equal to 0.5 microns and less than or equal to 10 microns; Preferably, the thickness of the resistance layer is greater than or equal to 5 nanometers and less than or equal to 1 micrometer.
7. The composite metal foil according to claim 1, characterized in that: Also includes: A peeling layer and a carrier layer, wherein the peeling layer is arranged on a side of the base layer facing away from the resistor layer, and the carrier layer is arranged on a side of the peeling layer facing away from the base layer, and the carrier layer can be peeled off from the base layer.
8. The composite metal foil according to claim 1, characterized in that: Also includes: At least one of an absorption layer, a first resistance layer and an adjustment layer is stacked with the base layer and the resistance layer.
9. A metal-clad laminate, characterized in that: The metal-clad laminate comprises the composite metal foil according to any one of claims 1 to 8.
10. A circuit board, characterized in that: The circuit board comprises the composite metal foil according to any one of claims 1 to 8, and the composite metal foil is arranged on the surface of a single-layer or multi-layer circuit board or inside a multi-layer board.
Citation Information
Cited By
Composite metal foil and circuit board
CN119724777A
Composite metal foil and circuit board
CN119889845A
Composite metal foil and metal-clad laminate
CN120280246A