Adhesive composition for foldable displays and adhesive film for foldable displays containing the cured product
The adhesive composition for foldable displays, utilizing specific monomers and polymers, addresses the challenge of maintaining folding reliability under extreme temperatures by enhancing adhesive properties, ensuring durability and stress relief.
Patent Information
- Application Number
- JP2023515857
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-09-11
- Filing Date
- 2021-08-20
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2041-08-20
AI Technical Summary
Adhesive films for foldable displays face challenges in maintaining folding reliability, especially under sub-zero temperature conditions, due to stress and deformation, necessitating improved physical properties for effective application.
An adhesive composition comprising specific acrylate and methacrylate monomers with varying alkyl group sizes and polar functional groups, along with a (meth)acrylate polymer, is used to create an adhesive layer with enhanced folding properties at room and sub-zero temperatures.
The adhesive layer exhibits excellent folding reliability and adhesiveness at both room and sub-zero temperatures, reducing storage modulus and maintaining adhesive strength, thus improving the durability of foldable displays.
Smart Images

Figure 0007567130000003 
Figure 0007567130000004 
Figure 0007567130000001
Abstract
Description
[Technical field]
[0001] This specification claims the benefit of the filing date of Korean Patent Application No. 10-2020-0116499, filed with the Korean Intellectual Property Office on September 11, 2020, the entire contents of which are incorporated herein by reference.
[0002] The present invention relates to an adhesive film for a foldable display, comprising an adhesive layer containing an adhesive composition for a foldable display and a cured product thereof. [Background technology]
[0003] In recent years, with the advancement of display-related technologies, research and development has been conducted on display devices that can be transformed during use, such as by folding, rolling up, stretching like rubber thread, etc. These displays can be transformed into various shapes, and therefore can meet both the demand for larger displays during use and the demand for smaller displays for portability.
[0004] A deformable display device can not only be deformed into a preset form, but also be deformed into various forms according to a user's request or the needs of the situation in which the display device is used. Therefore, it is necessary to recognize the deformed form of the display and control the display device in response to the recognized form.
[0005] Meanwhile, in a deformable display device, each component of the display device is damaged due to deformation, so each component of the display device needs to satisfy folding reliability and stability. In particular, an adhesive film that fixes each component of the display device needs to be sufficiently deformable so as to relieve stress that each component receives when the display is deformed, and in recent years, physical properties that can realize folding characteristics even when used under sub-zero temperature conditions are required.
[0006] Therefore, there is a need for an adhesive film that has physical properties that make it easy to apply to foldable displays. Summary of the Invention [Problem to be solved by the invention]
[0007] The present invention provides an adhesive film that has excellent folding properties even under sub-zero temperature conditions and can be easily applied to a foldable display, and an adhesive composition for implementing the same.
[0008] However, the problems to be solved by the present invention are not limited to those mentioned above, and other problems not mentioned will be clearly understood by those skilled in the art from the following description. [Means for solving the problem]
[0009] One embodiment of the present invention provides an adhesive composition for a foldable display, comprising a (meth)acrylate polymer which is a reaction product of a monomer mixture comprising a first monomer comprising at least one of a first acrylate monomer having an alkyl group of 12 to 14 carbon atoms and a first methacrylate monomer having an alkyl group of 14 to 16 carbon atoms, a second monomer comprising at least one of a second acrylate monomer having an alkyl group of 3 to 10 carbon atoms and a second methacrylate monomer having an alkyl group of 8 to 12 carbon atoms, and a (meth)acrylate monomer having a polar functional group.
[0010] In addition, an embodiment of the present invention provides an adhesive film for a foldable display, comprising an adhesive layer including a cured product of the adhesive composition for a foldable display. Effect of the Invention
[0011] The adhesive composition for a foldable display according to an embodiment of the present invention may provide an adhesive layer having excellent folding properties at room temperature and sub-zero temperature conditions.
[0012] In addition, the adhesive film for a foldable display according to an embodiment of the present invention has excellent folding reliability under room temperature and sub-zero temperature conditions.
[0013] The effects of the present invention are not limited to those described above, and effects not mentioned will be clearly understood by those skilled in the art from the present specification and the accompanying drawings. [Brief description of the drawings]
[0014] [Figure 1] FIG. 1 is a schematic diagram of a sample for folding evaluation. [Diagram 2] FIG. 1 is a schematic diagram of the folding study. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] Throughout this specification, when a part is said to "comprise" a certain component, this does not mean to exclude other components, but means that it may further include other components, unless specifically stated to the contrary.
[0016] Throughout this specification, when an element is said to be "on" another element, this includes not only when the element is in contact with the other element, but also when there is another element between the two elements.
[0017] Throughout this specification, the unit "parts by weight" refers to the weight ratio between each component.
[0018] Throughout this specification, "(meth)acrylate" is used to collectively refer to acrylate and methacrylate.
[0019] Throughout this specification, terms including ordinal numbers such as "first" and "second" are used for the purpose of distinguishing a certain component from other components, and are not limited by the ordinal numbers. For example, a first component can also be named a second component, and similarly, a second component can be named a first component, within the scope of the invention.
[0020] Throughout this specification, the "weight average molecular weight" and "number average molecular weight" of a compound can be calculated using the molecular weight and molecular weight distribution of the compound. Specifically, tetrahydrofuran (THF) and the compound are placed in a 1 ml glass bottle to prepare a sample specimen with a compound concentration of 1 wt%, and a standard sample (polystyrene) and the sample specimen are filtered through a filter (pore size 0.45 μm) and then injected into a GPC injector, and the elution time of the sample specimen is compared with the calibration curve of the standard specimen to obtain the molecular weight and molecular weight distribution of the compound. In this case, an Infinity II 1260 (Agilient) may be used as a measuring device, and the flow rate may be set to 1.00 mL / min and the column temperature to 40.0° C.
[0021] Throughout this specification, the storage modulus of the adhesive layer may be measured using a rheometer, ARES (Advanced Rheometric Expansion System)-G2, manufactured by TA instruments.
[0022] The present specification will be explained in more detail below.
[0023] One embodiment of the present invention provides an adhesive composition for a foldable display, comprising a (meth)acrylate polymer which is a reaction product of a monomer mixture comprising a first monomer comprising at least one of a first acrylate monomer having an alkyl group of 12 to 14 carbon atoms and a first methacrylate monomer having an alkyl group of 14 to 16 carbon atoms, a second monomer comprising at least one of a second acrylate monomer having an alkyl group of 3 to 10 carbon atoms and a second methacrylate monomer having an alkyl group of 8 to 12 carbon atoms, and a (meth)acrylate monomer having a polar functional group.
[0024] The adhesive composition for a foldable display according to an embodiment of the present invention may provide an adhesive layer having excellent folding properties at room temperature and sub-zero temperature conditions.
[0025] According to an embodiment of the present invention, the adhesive composition for a foldable display includes the (meth)acrylate polymer produced by reacting a monomer mixture including the first monomer, the second monomer, and a (meth)acrylate monomer having a polar functional group, thereby realizing an adhesive layer having excellent folding reliability even at low temperatures.
[0026] According to an embodiment of the present invention, the first monomer may include at least one of a first acrylate monomer containing an alkyl group having 12 to 14 carbon atoms and a first methacrylate monomer containing an alkyl group having 14 to 16 carbon atoms.
[0027] Specifically, the first acrylate monomer may contain a linear or branched alkyl group having a carbon number of 12 to 14. For example, the first acrylate monomer may include at least one of n-dodecyl acrylate (lauryl acrylate), isododecyl acrylate, n-tridecyl acrylate, isotridecyl acrylate, n-tetradecyl acrylate, and isotetradecyl acrylate.
[0028] The first methacrylate monomer may contain a linear or branched alkyl group having a carbon number of 14 to 16. For example, the first methacrylate monomer may include at least one of n-tetradecyl methacrylate, isotetradecyl methacrylate, n-pentadecyl methacrylate, isopentadecyl methacrylate, n-hexadecyl methacrylate, and isohexadecyl methacrylate.
[0029] By using at least one of the first acrylate-based monomer and the first methacrylate-based monomer as the first monomer, the folding reliability of the cured product of the adhesive composition for a foldable display at a low temperature (e.g., −20° C.) can be effectively improved.
[0030] According to an embodiment of the present invention, the content of the first monomer may be 20 parts by weight or more and 60 parts by weight or less, based on 100 parts by weight of the monomer mixture. Specifically, the content of the first monomer may be, based on 100 parts by weight of the monomer mixture, 25 parts by weight to 55 parts by weight, 30 parts by weight to 50 parts by weight, 35 parts by weight to 45 parts by weight, 20 parts by weight to 50 parts by weight, 22.5 parts by weight to 47.5 parts by weight, 25 parts by weight to 45 parts by weight, 27.5 parts by weight to 42.5 parts by weight, 30 parts by weight to 40 parts by weight, 32.5 parts by weight to 47.5 parts by weight, 35 parts by weight to 45 parts by weight, 37.5 parts by weight to 42.5 parts by weight, 35 parts by weight to 60 parts by weight, 38 parts by weight to 57.5 parts by weight, 40 parts by weight to 55 parts by weight, 43 parts by weight to 52.5 parts by weight, or 45 parts by weight to 50 parts by weight.
[0031] By adjusting the content of the first monomer contained in the monomer mixture within the above range, the storage modulus at low temperature of the cured product of the adhesive composition for a foldable display can be effectively reduced. In addition, when the content of the first monomer is within the above range, the cured product is prevented from having crystallinity, and the folding properties of the adhesive layer including the cured product can be improved.
[0032] According to an embodiment of the present invention, the second monomer may include at least one of a second acrylate monomer containing an alkyl group having 3 to 10 carbon atoms and a second methacrylate monomer containing an alkyl group having 8 to 12 carbon atoms.
[0033] Specifically, the second acrylate monomer may contain a linear or branched alkyl group having a carbon number of 3 to 10. For example, the second acrylate monomer may include at least one of n-propyl acrylate, isopropyl acrylate, n-butyl acrylate, isobutyl acrylate, n-pentyl acrylate, isopentyl acrylate, n-hexyl acrylate, isohexyl acrylate, n-heptyl acrylate, isoheptyl acrylate, n-octyl acrylate, isooctyl acrylate, ethylhexyl acrylate, n-nonyl acrylate, isononyl acrylate, n-decyl acrylate, and isodecyl acrylate.
[0034] The second methacrylate monomer may contain a linear or branched alkyl group having a carbon number of 8 to 12. For example, the second methacrylate monomer may include at least one of n-octyl methacrylate, isooctyl methacrylate, ethylhexyl methacrylate, n-nonyl methacrylate, isononyl methacrylate, n-decyl methacrylate, isodecyl methacrylate, n-undecyl methacrylate, isoundecyl methacrylate, n-dodecyl methacrylate, and isododecyl methacrylate.
[0035] By using at least one of the second acrylate-based monomer and the second methacrylate-based monomer as the second monomer, the folding reliability of the cured product of the adhesive composition for a foldable display at a low temperature (e.g., −20° C.) can be effectively improved.
[0036] According to an embodiment of the present invention, the content of the second monomer may be 35 parts by weight or more and 80 parts by weight or less, based on 100 parts by weight of the monomer mixture. Specifically, the content of the second monomer may be, based on 100 parts by weight of the monomer mixture, more than 35 parts by weight and less than 80 parts by weight, 36 parts by weight or more and less than 79 parts by weight, 40 parts by weight or more and less than 79 parts by weight, 45 parts by weight or more and less than 79 parts by weight, 50 parts by weight or more and less than 75 parts by weight, 55 parts by weight or more and less than 70 parts by weight, 60 parts by weight or more and less than 65 parts by weight, 35 parts by weight or more and less than 65 parts by weight, 37.5 parts by weight or more and less than 62.5 parts by weight, 40 parts by weight or more and less than 60 parts by weight, 42.5 parts by weight or more and less than 57.5 parts by weight, 45 parts by weight or more and less than 55 parts by weight, 47.5 parts by weight or more and less than 52.5 parts by weight, 50 parts by weight or more and less than 80 parts by weight, 52.5 parts by weight or more and less than 75 parts by weight, 55 parts by weight or more and less than 70 parts by weight, 57.5 parts by weight or more and less than 67.5 parts by weight, or 60 parts by weight or more and less than 65 parts by weight.
[0037] By adjusting the content of the second monomer contained in the monomer mixture within the above range, the storage modulus at low temperature of the cured product of the adhesive composition for a foldable display can be effectively reduced.
[0038] According to one embodiment of the present invention, the (meth)acrylate monomer containing a polar functional group may contain a carboxylic acid group. That is, the (meth)acrylate monomer may contain a carboxylic acid group as a polar functional group. By using the (meth)acrylate monomer containing a carboxylic acid group, the (meth)acrylate polymer can effectively undergo a curing reaction with an epoxy crosslinking agent described below. In addition, by using the (meth)acrylate monomer containing a carboxylic acid group, the adhesive strength of the cured product of the adhesive composition for a foldable display is maintained, and the adhesive film for a foldable display can be prevented from being detached from the substrate film during folding.
[0039] The (meth)acrylate monomer containing a polar functional group may include, for example, at least one of (meth)acrylic acid, 2-(meth)acryloyloxyacetic acid, 3-(meth)acryloyloxypropionic acid, 4-(meth)acryloyloxybutyric acid, and a (meth)acrylic acid dimer.
[0040] According to an embodiment of the present invention, the content of the (meth)acrylate monomer containing a polar functional group may be 1 to 4 parts by weight based on 100 parts by weight of the monomer mixture. Specifically, the content of the (meth)acrylate monomer containing a polar functional group may be 1 to 3 parts by weight, 1 to 2 parts by weight, 2 to 4 parts by weight, or 2 to 3 parts by weight based on 100 parts by weight of the monomer mixture. By adjusting the content of the (meth)acrylate monomer containing a polar functional group to the above range, the adhesive performance of the cured product of the adhesive composition for a foldable display can be effectively improved.
[0041] According to an embodiment of the present invention, the weight ratio of the first monomer to the (meth)acrylate monomer containing a polar functional group may be 1:0.025 to 1:0.1. Specifically, the weight ratio of the first monomer to the (meth)acrylate monomer containing a polar functional group contained in the monomer mixture may be 1:0.03 to 1:0.08, 1:0.04 to 1:0.06, 1:0.025 to 1:0.07, 1:0.035 to 1:0.05, 1:0.05 to 1:0.1, or 1:0.08 to 1:0.1. When the weight ratio of the first monomer to the (meth)acrylate monomer containing a polar functional group contained in the monomer mixture is within the above range, the storage modulus at low temperature of the cured product of the adhesive composition for a foldable display can be effectively reduced. In addition, the cured product is prevented from having crystallinity, and the folding properties of the adhesive layer including the cured product can be improved.
[0042] According to an embodiment of the present invention, the weight ratio of the first monomer to the second monomer may be 1:0.5 to 1:4. Specifically, the weight ratio of the first monomer to the second monomer included in the monomer mixture may be 1:0.6 to 1:3.7, 1:0.7 to 1:3.5, 1:0.9 to 1:3, 1:1 to 1:2.7, 1:1.5 to 1:2.5, 1:0.5 to 1:3, 1:0.8 to 1:2.5, 1:1 to 1:2, 1:1.5 to 1:4, 1:2 to 1:4, or 1:3 to 1:4. By controlling the weight ratio of the first monomer to the second monomer included in the monomer mixture within the above range, the storage modulus at low temperature of the cured product of the adhesive composition for a foldable display can be effectively reduced. In addition, the cured product of the adhesive composition for a foldable display can be prevented from having crystallinity, and the folding properties of the adhesive layer including the cured product of the adhesive composition for a foldable display can be effectively improved.
[0043] According to an embodiment of the present invention, the weight ratio of the (meth)acrylate monomer containing a polar functional group to the second monomer may be 1:10 to 1:85. Specifically, the weight ratio of the (meth)acrylate monomer containing a polar functional group to the second monomer contained in the monomer mixture may be 1:15 to 1:80, 1:20 to 1:75, 1:25 to 1:70, 1:30 to 1:65, 1:30 to 1:50, 1:10 to 1:65, 1:15 to 1:60, 1:20 to 1:55, 1:25 to 1:50, 1:30 to 1:45, 1:30 to 1:85, 1:35 to 1:80, 1:40 to 1:75, 1:45 to 1:70, or 1:50 to 1:65. When the weight ratio of the polar functional group-containing (meth)acrylate monomer and the weight ratio of the second monomer contained in the monomer mixture are within the above-mentioned ranges, the storage modulus at low temperature of the cured product of the adhesive composition for a foldable display can be effectively reduced, and the adhesive performance of the cured product of the adhesive composition for a foldable display can be effectively improved.
[0044] According to an embodiment of the present invention, the (meth)acrylate-based polymer may be prepared by thermal polymerization. Specifically, the (meth)acrylate-based polymer may be formed by adding a thermal initiator to the monomer mixture and performing thermal polymerization.
[0045] According to an embodiment of the present invention, the (meth)acrylate polymer may have a weight average molecular weight of 1,500,000 or more and 2,500,000 or less. Specifically, the weight average molecular weight of the (meth)acrylate polymer may be 1,500,000 g / mol or more and 2,500,000 g / mol or less, 1,650,000 g / mol or more and 2,300,000 g / mol or less, 1,800,000 g / mol or more and 2,200,000 g / mol or less, 1,500,000 g / mol or more and 2,000,000 g / mol or less, 1,700,000 g / mol or more and 2,000,000 g / mol or less, 1,850,000 g / mol or more and 2,000,000 g / mol or less, 2,000,000 g / mol or more and 2,500,000 g / mol or less, or 2,100,000 g / mol or more and 2,400,000 g / mol or less. When the weight average molecular weight of the (meth)acrylate polymer is within the above range, the cured product of the adhesive composition for a foldable display has excellent folding reliability and adhesiveness, etc. In addition, by adjusting the weight average molecular weight of the (meth)acrylate polymer within the above range, the storage modulus of the cured product of the adhesive composition for a foldable display at low temperature can be effectively reduced and the storage modulus at room temperature can be maintained.
[0046] According to an embodiment of the present invention, the adhesive composition for a foldable display may further include an epoxy-based crosslinking agent. The epoxy-based crosslinking agent may be any epoxy-based crosslinking agent used in the art without limitation. Specifically, the epoxy-based crosslinking agent may be a multifunctional epoxy compound, and the multifunctional epoxy compound may include at least one of a diphenylmethane skeleton, a dinaphthalene skeleton, a triazine skeleton, and a biphenyl skeleton.
[0047] The epoxy crosslinking agent may include at least one of ethylene glycol diglycidyl ether, triglycidyl ether, trimethylolpropane triglycidyl ether, N,N,N',N'-tetraglycidylethylenediamine, and glycerin diglycidyl ether, but the type of the epoxy crosslinking agent is not limited thereto. For example, BXX-5240 may be used as the epoxy crosslinking agent.
[0048] According to an embodiment of the present invention, the content of the epoxy-based crosslinking agent may be 0.01 to 0.1 parts by weight based on 100 parts by weight of the (meth)acrylate-based polymer. Specifically, the content of the epoxy-based crosslinking agent may be 0.01 to 0.07 parts by weight, 0.01 to 0.05 parts by weight, or 0.01 to 0.03 parts by weight based on 100 parts by weight of the (meth)acrylate-based polymer. By adjusting the content of the epoxy-based crosslinking agent within the above range, the curing reaction of the (meth)acrylate-based polymer contained in the adhesive composition for a foldable display can be effectively performed.
[0049] According to an embodiment of the present invention, the adhesive composition for a foldable display may further include a solvent. The solvent may be any solvent used in the art without limitation. For example, the solvent may include at least one of methyl ethyl ketone, ethyl acetate, toluene, xylene, benzene, cyclohexane, and cycloheptane, but the type of the solvent is not limited thereto.
[0050] According to an embodiment of the present invention, the adhesive composition for a foldable display may further include an additive. For example, the additive may include at least one of a release force regulator, an additional crosslinking agent, an antistatic agent, a tackifier resin, a curing agent, an ultraviolet stabilizer, an antioxidant, a color toning agent, a reinforcing agent, a filler, an antifoaming agent, and a surfactant, but the type of the additive is not limited thereto.
[0051] According to an embodiment of the present invention, the adhesive composition for a foldable display may have a solid content of 10% by weight or more and 30% by weight or less. The solid content refers to components other than the solvent contained in the adhesive composition for a foldable display. For example, the solid content may include the (meth)acrylate-based polymer and the epoxy-based crosslinking agent contained in the adhesive composition for a foldable display. The adhesive composition for a foldable display having a solid content satisfying the above range has an appropriate viscosity and excellent coating property.
[0052] According to one embodiment of the present invention, the adhesive composition for a foldable display may have a viscosity of 500 cp to 2,500 cp. Specifically, the adhesive composition for a foldable display may have a viscosity of 500 cp to 2,500 cp, 700 cp to 2,300 cp, or 850 cp to 2,200 cp at 25° C. The adhesive composition for a foldable display having a viscosity in the above range has excellent coating properties.
[0053] An embodiment of the present invention provides an adhesive film for a foldable display, comprising an adhesive layer including a cured product of the adhesive composition for a foldable display.
[0054] The adhesive film for a foldable display according to one embodiment of the present invention has excellent folding reliability under room temperature and sub-zero temperature conditions.
[0055] According to an embodiment of the present invention, the adhesive film for a foldable display may include a release film and an adhesive layer including a cured product of the adhesive composition for a foldable display provided on the release film. The release film may be any release film used in the art without limitation. For example, the release film may be a polyester film that is release-treated with silicone.
[0056] According to an embodiment of the present invention, the adhesive layer may include a heat-cured product of the adhesive composition for a foldable display. For example, the adhesive composition for a foldable display may be coated on a release film and heat-cured at a temperature of 100° C. to 150° C. for 1 minute to 5 minutes to form the adhesive layer.
[0057] According to an embodiment of the present invention, the adhesive layer may have a thickness of 10 μm to 100 μm. Specifically, the adhesive layer may have a thickness of 15 μm to 80 μm, 20 μm to 65 μm, or 25 μm to 50 μm. When the adhesive layer has a thickness within the above range, the adhesive layer may achieve excellent adhesive strength and folding properties when applied to a foldable display.
[0058] According to an embodiment of the present invention, the adhesive layer may have a storage modulus of 100,000 Pa or less when measured at -20°C. Specifically, the adhesive layer may have a storage modulus of 30,000 Pa to 100,000 Pa when measured at a temperature of -20°C and a frequency of 1 Hz. More specifically, the adhesive layer may have a storage modulus of 35,000 Pa to 98,000 Pa, 40,000 Pa to 98,000 Pa, 43,000 Pa to 98,000 Pa, 45,000 Pa to 95,000 Pa, 50,000 Pa to 90,000 Pa, 55,000 Pa to 85,000 Pa, 60,000 Pa to 80,000 Pa, 65,000 Pa to 75,000 Pa, and more preferably, 75,000 Pa to 85,000 Pa. Pa or less, 30,000 Pa to 65,000 Pa, 35,000 Pa to 63,000 Pa, 40,000 Pa to 61,000 Pa, 45,000 Pa to 59,000 Pa, 60,000 Pa to 100,000 Pa, 61,000 Pa to 98,000 Pa, 63,000 Pa to 95,000 Pa, 65,000 Pa to 90,000 Pa, or 70,000 Pa to 85,000 Pa. When the storage modulus of the adhesive layer at -20°C is within the above range, the adhesive layer can achieve excellent folding properties even at low temperatures.
[0059] According to one embodiment of the present invention, the adhesive layer may have a storage modulus of 10,000 Pa or more measured at 25° C. Specifically, the storage modulus of the adhesive layer measured at a temperature of 25° C. and a frequency of 1 Hz may be 10,000 Pa or more and 40,000 Pa or less. More specifically, the storage modulus of the adhesive layer measured at a temperature of 25° C. and a frequency of 1 Hz may be 10,000 Pa or more and 37,000 Pa or less, 10,000 Pa or more and 36,000 Pa or less, 15,000 Pa or more and 35,000 Pa or less, 20,000 Pa or more and 30,000 Pa or less, 10,000 Pa or more and 30,000 Pa or less, 12,000 Pa or more and 28,000 Pa or less, 15 ... The storage modulus may be 0 Pa or more and 26,000 Pa or less, 17,000 Pa or more and 25,000 Pa or less, 20,000 Pa or more and 24,000 Pa or less, 20,000 Pa or more and 40,000 Pa or less, 20,000 Pa or more and 36,000 Pa or less, 22,000 Pa or more and 34,000 Pa or less, 24,000 Pa or more and 31,000 Pa or less, or 25,000 Pa or more and 28,000 Pa or less. The adhesive layer having a storage modulus at 25°C that satisfies the above-mentioned range has excellent folding properties and can effectively relieve the stress applied to the foldable display configuration.
[0060] According to one embodiment of the present invention, the storage modulus of the adhesive layer at −25° C. and at 20° C. can be measured using the ARES-G2 equipment as described above.
[0061] Therefore, the adhesive layer according to an embodiment of the present invention has excellent folding properties and can be easily applied to a foldable display.
[0062] [Example] The present invention will now be described in detail with reference to examples.
[0063] Example 1 Production of (meth)acrylate polymers Lauryl acrylate was prepared as a first monomer, 2-ethylhexyl acrylate was prepared as a second monomer, and acrylic acid was prepared as a (meth)acrylate monomer containing a polar functional group, and these were mixed to prepare a monomer mixture.
[0064] In this case, based on 100 parts by weight of the monomer mixture, the content of the first monomer was 20 parts by weight, the content of the second monomer was 79 parts by weight, and the content of the (meth)acrylate monomer containing a polar functional group was 1 part by weight.
[0065] The monomer mixture was introduced into a 1L reactor equipped with a cooling device to allow nitrogen gas to be refluxed and to facilitate temperature control, and then ethyl acetate (EAc) was introduced as a solvent. Nitrogen gas was then purged for about 1 hour to remove oxygen, and the reactor temperature was maintained at 85°C. After homogenizing the monomer mixture, 5,000 ppm of benzoyl peroxide (BPO) was introduced as a reaction initiator, and the monomer mixture was reacted for 6 hours to produce a (meth)acrylate-based polymer with a weight average molecular weight of 1,850,000 g / mol, which was then diluted with ethyl acetate to produce a (meth)acrylate-based polymer solution.
[0066] Manufacturing of adhesive composition for foldable displays To the (meth)acrylate polymer solution prepared above, 0.03 parts by weight of BXX-5240, an epoxy crosslinking agent, was added per 100 parts by weight of the (meth)acrylate polymer, diluted with methyl ethyl ketone and methyl isobutyl ketone, and mixed for 15 minutes or more using a mechanical stirrer. Then, the mixture was left at room temperature (25°C) to remove air bubbles generated during mixing, and an adhesive composition for foldable displays with a solid content of 22% by weight and a viscosity of about 1,500 cp at 25°C was prepared.
[0067] Manufacturing of adhesive films for foldable displays The adhesive composition for foldable displays prepared above was coated on a polyester film that had been treated with silicone for release using a blade, and then dried for 3 minutes at 140°C using a Mathis oven. As a result, an adhesive film for foldable displays including an adhesive layer with a thickness of 25μm was prepared.
[0068] Examples 2 to 17 Except for preparing the monomer mixture as shown in Table 1 below, a (meth)acrylate-based polymer, an adhesive composition for a foldable display, and an adhesive film for a foldable display were prepared in the same manner as in Example 1.
[0069] The weight average molecular weight (Mw) of the produced (meth)acrylate polymer is shown in Table 1 below.
[0070] Comparative Examples 1 to 7
[0071] Except for preparing the monomer mixture as shown in Table 1 below, a (meth)acrylate-based polymer, an adhesive composition for a foldable display, and an adhesive film for a foldable display were prepared in the same manner as in Example 1.
[0072] The weight average molecular weight (Mw) of the produced (meth)acrylate polymer is shown in Table 1 below.
[0073] Comparative Example 8 Production of (meth)acrylate polymers Lauryl acrylate was prepared as a first monomer, 2-ethylhexyl acrylate was prepared as a second monomer, and acrylic acid was prepared as a (meth)acrylate monomer containing a polar functional group, and these were mixed to prepare a monomer mixture.
[0074] In this case, based on 100 parts by weight of the monomer mixture, the content of the first monomer was 20 parts by weight, the content of the second monomer was 79 parts by weight, and the content of the (meth)acrylate monomer containing a polar functional group was 1 part by weight.
[0075] The monomer mixture was introduced into a 1L reactor equipped with a cooling device to allow nitrogen gas to be refluxed and to facilitate temperature control, and then ethyl acetate (EAc) was introduced as a solvent. Nitrogen gas was then purged for about 1 hour to remove oxygen, and the reactor temperature was maintained at 85°C. After homogenizing the monomer mixture, 5,000 ppm of benzoyl peroxide (BPO) was introduced as a reaction initiator, and the monomer mixture was reacted for 3 hours to produce a (meth)acrylate-based polymer with a weight average molecular weight of 500,000 g / mol, which was then diluted with ethyl acetate to produce a (meth)acrylate-based polymer solution.
[0076] Manufacturing of adhesive composition for foldable displays To the (meth)acrylate polymer solution prepared above, 0.03 parts by weight of BXX-5240, an epoxy crosslinking agent, was added per 100 parts by weight of the (meth)acrylate polymer, diluted with methyl ethyl ketone and methyl isobutyl ketone, and mixed for 15 minutes or more using a mechanical stirrer. Then, the mixture was left at room temperature (25°C) to remove air bubbles generated during mixing, and an adhesive composition for foldable displays with a solid content of 22% by weight and a viscosity of about 200 cp at 25°C was prepared.
[0077] However, the weight average molecular weight of the (meth)acrylate polymer prepared in Comparative Example 8 was 500,000 g / mol, and the viscosity of the adhesive composition for a foldable display was about 200 cp at 25°C. When the adhesive composition for a foldable display was applied to a polyester film that had been subjected to a silicone release treatment using a blade to form a coating, a dewetting phenomenon occurred due to the low viscosity, making coating impossible.
[0078] Comparative Example 9 Production of (meth)acrylate polymers Lauryl acrylate was prepared as a first monomer, 2-ethylhexyl acrylate was prepared as a second monomer, and acrylic acid was prepared as a (meth)acrylate monomer containing a polar functional group, and these were mixed to prepare a monomer mixture.
[0079] In this case, based on 100 parts by weight of the monomer mixture, the content of the first monomer was 20 parts by weight, the content of the second monomer was 79 parts by weight, and the content of the (meth)acrylate monomer containing a polar functional group was 1 part by weight.
[0080] The monomer mixture was put into a 1L reactor where nitrogen gas was refluxed, and then purged with nitrogen gas for about 1 hour to remove oxygen.The monomer mixture was then homogenized, and about 500 ppm of a reaction initiator (Irgacure 184) was added. A (meth)acrylate-based polymer with a weight average molecular weight of 3,000,000 g / mol was produced by bulk polymerization with ultraviolet light irradiation, and a (meth)acrylate-based polymer solution was produced by diluting with ethyl acetate.
[0081] Manufacturing of adhesive composition for foldable displays To the (meth)acrylate polymer solution prepared above, 0.03 parts by weight of BXX-5240, an epoxy crosslinking agent, was added per 100 parts by weight of the (meth)acrylate polymer, diluted with methyl ethyl ketone and methyl isobutyl ketone, and mixed for 15 minutes or more using a mechanical stirrer. Then, the mixture was left at room temperature (25°C) to remove air bubbles generated during mixing, and an adhesive composition for foldable displays with a solid content of 22% by weight and a viscosity of about 20,000 cp at 25°C was prepared.
[0082] However, the weight average molecular weight of the (meth)acrylate polymer prepared in Comparative Example 9 was 3,000,000 g / mol, and the viscosity of the adhesive composition for a foldable display was about 20,000 cp at 25°C. When the adhesive composition for a foldable display was applied to a polyester film that had been subjected to a silicone release treatment using a blade to form a coating, the high viscosity caused significant thickness unevenness, making coating impossible.
[0083] [Table 1]
[0084] In Table 1, "LA" means lauryl acrylate, "TDMA" means tetradecyl methacrylate, "2-EHA" means 2-ethylhexyl acrylate, "BA" means butyl acrylate, "AA" means acrylic acid, and "HBA" means hydroxybutyl acrylate.
[0085] In Table 1, the contents of the first monomer, the second monomer, and the polar functional group-containing monomer (the (meth)acrylate monomer containing a polar functional group) are based on 100 parts by weight of the monomer mixture, and the content of the crosslinking agent is based on 100 parts by weight of the (meth)acrylate polymer.
[0086] Experimental Example Measurement of storage modulus The storage modulus at -20°C and the storage modulus at 25°C of the adhesive layers produced in Examples 1 to 17 and Comparative Examples 1 to 4 were measured using an Advanced Rheometric Expansion System G2 (TA) as follows.
[0087] Specifically, a sample was manufactured by laminating the adhesive layer manufactured in Example 1 to a thickness of 1 mm. Then, the storage modulus at the temperature was measured using a parallel plate fixture with a diameter of 8 mm. <Measurement conditions> Strain: 5% Frequency: 1Hz Initial temperature: -40℃, final temperature: 90℃ Heating rate: 10℃ / min
[0088] In addition, using the same method as described above, the storage modulus at -20°C and the storage modulus at 25°C of the adhesive layers produced in Examples 2 to 17 and Comparative Examples 1 to 4 were measured, and the results are shown in Table 2 below.
[0089] Folding evaluation The adhesive layers produced in Examples 1 to 17 and Comparative Examples 1 to 7 were evaluated for folding as follows.
[0090] FIG. 1 is a schematic diagram of the sample for folding evaluation.
[0091] As shown in FIG. 1, a laminate was manufactured by bonding a cover window (LGC) having a 13 μm thick hard coat (HC) formed on one side of a 50 μm thick PET film and a 40 μm thick CPI (Colorless Polyimide) film using the adhesive layer (PSA) manufactured in Examples 1 to 17 and Comparative Examples 1 to 7.
[0092] Thereafter, a laminate having a laminated structure of cover window (HC / PET) / adhesive layer (PSA) / CPI was cut into a size of 140 mm×80 mm to prepare a sample.
[0093] FIG. 2 is a schematic diagram of the folding test.
[0094] As shown in FIG. 2, the sample was sandwiched between parallel plates of the folding test equipment at a temperature of -20°C, and the sample was folded with a curvature radius of 5 mm at one folding per second, for a total of 200,000 dynamic folding tests.
[0095] After the test, the sample was collected and visually observed for the occurrence of bubbles, lifting, and cracks in the hard coat layer. If there was no occurrence of bubbles, lifting, or cracks in the hard coat layer, it was evaluated as "OK", and if there was any occurrence of bubbles, lifting, or cracks in the hard coat layer, it was evaluated as "NG", and the results are shown in Table 2 below.
[0096] [Table 2]
[0097] Referring to Tables 1 and 2, it was confirmed that the adhesive layers prepared in Examples 1 to 17 of the present invention had a storage modulus of 100,000 Pa or less measured at -20° C., and thus had excellent folding evaluation results at -20° C. In addition, it was confirmed that the adhesive layers prepared in Examples 1 to 17 had a storage modulus of 10,000 Pa or more measured at 25° C.
[0098] On the other hand, the adhesive layers of Comparative Example 1, which did not use the first monomer LA, and Comparative Example 2, which did not use the second monomer 2-EHA, were found to have poor folding evaluation results at -20°C because the storage modulus measured at -20°C exceeded 100,000 Pa.
[0099] In addition, the adhesive layers prepared in Comparative Examples 3 and 4, in which the contents of the first and second monomers did not satisfy the content ranges according to an embodiment of the present invention, were found to have poor folding evaluation results at -20°C because the storage modulus measured at -20°C exceeded 100,000 Pa.
[0100] On the other hand, in the case of Comparative Example 5 in which a hydroxyl group-containing (meth)acrylate monomer was used as the polar functional group-containing (meth)acrylate monomer, the storage modulus at -20°C and 25°C was at an appropriate level, but the folding evaluation result at -20°C was poor.
[0101] In addition, in the case of Comparative Example 6 and Comparative Example 7, in which the content of the (meth)acrylate monomer containing a polar functional group was too low or too high, the folding evaluation results performed at -20°C were poor.
[0102] Therefore, it can be seen that the adhesive composition for a foldable display according to one embodiment of the present invention can provide an adhesive layer having excellent folding properties even at a low temperature condition such as -20°C.
Claims
1. a first monomer including at least one of a first acrylate monomer having an alkyl group having 12 to 14 carbon atoms and a first methacrylate monomer having an alkyl group having 14 to 16 carbon atoms; a second monomer including at least one of a second acrylate monomer including an alkyl group having 3 to 10 carbon atoms and a second methacrylate monomer including an alkyl group having 8 to 12 carbon atoms; The (meth)acrylate polymer is a reaction product of a monomer mixture containing only a (meth)acrylate monomer having a polar functional group, Based on 100 parts by weight of the monomer mixture, The content of the first monomer is 20 parts by weight or more and 60 parts by weight or less, The content of the second monomer is 35 parts by weight or more and 80 parts by weight or less, The content of the (meth)acrylate monomer containing a polar functional group is 1 part by weight or more and 4 parts by weight or less, a weight ratio of the first monomer to the (meth)acrylate monomer having a polar functional group is 1:0.025 to 1:0.1; The (meth)acrylate monomer containing a polar functional group contains a carboxylic acid group, The weight average molecular weight of the (meth)acrylate polymer is 1,500,000 or more and 2,500,000 or less. Adhesive composition for foldable displays.
2. The adhesive composition for a foldable display according to claim 1, wherein a weight ratio of the first monomer to the second monomer is 1:0.5 to 1:
4.
3. The adhesive composition for a foldable display according to claim 1 or 2, wherein the weight ratio of the (meth)acrylate monomer containing a polar functional group to the second monomer is 1:10 to 1:
85.
4. The adhesive composition for a foldable display according to claim 1 , further comprising an epoxy-based crosslinking agent.
5. The adhesive composition for a foldable display according to claim 4 , wherein the content of the epoxy-based crosslinking agent is 0.01 parts by weight or more and 0.1 parts by weight or less with respect to 100 parts by weight of the (meth)acrylate-based polymer.
6. An adhesive film for a foldable display, comprising an adhesive layer containing a cured product of an adhesive composition, the adhesive composition being the adhesive composition for a foldable display according to any one of claims 1 to 5.
7. The adhesive film for a foldable display according to claim 6, wherein the adhesive layer has a storage modulus of 100,000 Pa or less measured at -20°C.
8. The adhesive film for a foldable display according to claim 6 or 7, wherein the adhesive layer has a storage modulus measured at 25°C of 10,000 Pa or more.
Citation Information
Patent Citations
Adhesive agent layer for flexible image display device, laminate body for flexible image display device, and flexible image display device
JP2019218513A