Method for producing ferroboron alloy-coated lithium iron phosphate

The ferroboron alloy-coated lithium iron phosphate addresses interfacial resistance and conductivity issues in solid-state batteries by forming a stable conductive buffer layer, enhancing battery performance and safety through a specialized manufacturing process.

JP7567144B2Active Publication Date: 2024-10-16HUBEI WANRUN NEW ENERGY TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023544204
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-03-24
Filing Date
2022-12-09
Publication Date
2024-10-16
Estimated Expiration
2042-12-09

AI Technical Summary

Technical Problem

Solid-state batteries face issues with interfacial resistance and compatibility between electrodes due to the use of traditional conductive materials, which are prone to corrosion and have low conductivity, leading to poor performance and safety concerns.

Method used

A ferroboron alloy is coated onto lithium iron phosphate to form a stable conductive buffer layer, reducing interfacial resistance and enhancing conductivity, corrosion resistance, and compactness through a specific manufacturing process involving the steps of producing ferrous phosphate and lithium phosphate, mixing, adding hydrazine water, and reacting with sodium borohydride and sodium hydroxide solutions.

Benefits of technology

The ferroboron alloy-coated lithium iron phosphate achieves significantly lower interfacial resistance, improved conductivity, and higher consolidation density, resulting in enhanced battery performance and safety.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007567144000009
    Figure 0007567144000009
  • Figure 0007567144000010
    Figure 0007567144000010
  • Figure 0007567144000011
    Figure 0007567144000011
Patent Text Reader

Abstract

The present invention relates to a method for preparing ferroboron alloy-coated lithium iron phosphate, which comprises preparing ferrous phosphate and lithium phosphate, mixing the ferrous phosphate and lithium phosphate, adding hydrazine hydrate solution, pulverizing, drying, and calcining the mixture, adding pure water to the calcined mixture, and pulverizing the mixture. The resulting slurry is then added with PEG, ferrous sulfate crystals, and disodium EDTA, stirring and dissolving the mixture. The mixture is then added with sodium borohydride solution and sodium hydroxide solution under stirring, maintaining the pH of the process at 8.5-10.5, and reacting for 15-30 minutes. The mixture is then filtered, washed, and vacuum-dried to obtain ferroboron alloy-coated lithium iron phosphate. This method reduces interfacial resistance while improving electrical conductivity, corrosion resistance, antioxidant capacity, and product density.
Need to check novelty before this filing date? Find Prior Art

Description

CROSS-REFERENCE TO RELATED APPLICATIONS

[0001] This application claims priority to a Chinese patent application for invention, bearing application number 202210294927.5, filed on March 24, 2022, and entitled "Method for producing lithium iron phosphate coated with ferroboron alloy," the disclosure of which is incorporated herein by reference. [Technical field]

[0002] The present invention belongs to the technical field of solid-state batteries, and relates to a method for producing ferroboron alloy-coated lithium iron phosphate. [Background technology]

[0003] In recent years, with the rapid development of portable electronic devices, electric vehicles and hybrid cars, energy storage materials with abundant research resources, high energy efficiency and environmental friendliness have become an international research hotspot. In order to meet the huge market demand, it is not enough to measure battery materials only by the electrical performance of the battery, but the safety, manufacturing cost, energy consumption and environmental pollution of the battery are also important indicators for evaluating battery materials.

[0004] Solid-state batteries are a type of battery technology. Unlike the currently commonly used lithium-ion batteries and lithium-ion polymer batteries, solid-state batteries are batteries that use solid electrodes and solid electrolytes. In recent years, solid-state batteries have been viewed as a battery that can take over the position of lithium-ion batteries, as the scientific community believes that lithium-ion batteries have reached their limits. Solid-state lithium battery technology employs a glass compound made of lithium and sodium as a conductive material to replace the electrolyte in traditional lithium batteries, which can greatly improve the energy density of lithium batteries.

[0005] The principle of solid-state batteries is the same, but their electrolyte is solid, and due to its density and structure, more charged ions can be collected at one end, so they can conduct a larger current, thereby improving the battery capacity. Therefore, for the same amount of power, the volume of solid-state batteries is smaller. In addition, since solid-state batteries do not have electrolyte, they are easier to store, and when used in large equipment such as automobiles, there is no need to add cooling tubes or electronic control devices, which not only saves costs but also effectively reduces weight.

[0006] Solid-state batteries have the problem that the solid electrolyte increases the interfacial resistance between the electrodes and reduces interfacial compatibility.

[0007] For the development of all-solid-state batteries, the key to solving the above problems is the development of solid electrolyte materials and the control and optimization of interface performance.

[0008] The positive electrode of the solid-state lithium secondary battery generally adopts a composite electrode, which in addition to the electrode active material, further contains a solid electrolyte and a conductive agent, and plays the role of simultaneously transporting ions and electrons in the electrode. The research of LiCoO2, LiFePO4, LiMn2O4 is relatively universal, where the traditional carbon is coated with lithium iron phosphate, but the amorphous carbon has a very low compaction density and a lot of loose porous structure, so there is a certain degree of repulsion after compaction, and the contact interface between the positive electrode material and the solid electrolyte of the solid battery is smaller and the interface resistance is larger, so the traditional conductive material cannot meet this requirement, and at the same time, the solid electrolyte does not have the problem of decomposing corrosive gases, so the research of the positive electrode material of metal element-coated lithium iron phosphate has gradually begun. For example:

[0009] Chinese Patent No. 201710370271.X discloses a method for producing a tungsten-coated lithium iron phosphate positive electrode material, the method comprising: Producing a lithium iron phosphate material; A coating solution is prepared by dissolving a tungsten-containing compound in deionized water and thoroughly stirring and mixing until the compound is completely dissolved; The prepared coating solution and the spherical positive electrode lithium iron phosphate material are placed in a ball mill tank, and mixed in a ball mill at a rotation speed of 300 to 500 r / min for 4 to 6 hours to obtain a mixed solution; The mixed liquid after the ball mill mixing is vacuum-dried, and then heated from room temperature to 480-620°C at a rate of 15°C / min, calcined at a constant temperature of 480-620°C for 3-6 hours, then heated to 850-900°C at a rate of 10°C / min, calcined at a constant temperature of 850-900°C for 8-10 hours, and finally cooled to room temperature at a uniform temperature reduction rate of 5°C / min, and thoroughly pulverized to obtain a tungsten-coated lithium iron phosphate positive electrode material; The scheme employs tungsten metal to coat lithium iron phosphate, the metal element is easy to be eroded by the electrolyte, and at the same time, the metal coating layer is easy to be deposited on the negative electrode due to the electric potential.

[0010] Chinese Patent No. 201510227614.8 discloses a method for preparing a nickel-coated lithium iron phosphate positive electrode material, the positive electrode material being composed of lithium iron phosphate coated with a nickel plating layer on its surface, the preparation method being such that lithium iron phosphate is sequentially sensitized, activated and reduced under the action of a dispersant, and then plated with a nickel plating layer, and the lithium iron phosphate plated with the nickel plating layer is then heat treated to obtain a nickel-coated lithium iron phosphate positive electrode material, the preparation method being simple in operation, mild in process conditions and low in cost, the prepared nickel-coated lithium iron phosphate positive electrode material is uniformly coated with a nickel plating layer and has a stable structure, so that it can be used to prepare lithium ion batteries with good electrical conductivity, high specific capacity and large power density, the scheme employs nickel metal to coat the lithium iron phosphate, the metal element is easily eroded by the electrolyte, and at the same time, the metal coating layer is easily deposited on the negative electrode due to the electric potential.

[0011] China Patent No. 201110190384.4 discloses a transition metal element-doped lithium iron phosphate composite positive electrode material coated with transition metal oxide and a preparation method thereof, the preparation method includes the following steps: 1) ball milling a lithium source, an iron source, a phosphorus source and a transition metal element with an atomic ratio of Li:Fe:PO4:M=0.995-0.95:1:1:0.005-0.05, drying and calcining in an inert atmosphere to obtain a transition metal element-doped lithium iron phosphate composite material; 2) mixing the transition metal element-doped lithium iron phosphate composite material obtained in step 1) with a transition metal oxide and ball milling, and then calcining in an inert atmosphere to obtain a transition metal element-doped lithium iron phosphate composite positive electrode material coated with transition metal oxide. The beneficial effect of the present invention is that the specific capacity and cycle performance of lithium iron phosphate can be improved by doping it with a transition metal element and coating it with a transition metal oxide. However, the metal oxide-coated positive electrode material produced by this scheme has a problem of relatively poor electrical conductivity.

[0012] In view of the above, there is room for further study of the metal element-coated lithium iron phosphate positive electrode material. Summary of the Invention

[0013] In order to solve the above problems of the prior art, the present invention proposes a method for producing ferroboron alloy-coated lithium iron phosphate, which can reduce the interfacial resistance while improving the electrical conductivity, corrosion resistance, antioxidant ability and denseness of the product.

[0014] The present invention is realized by the following technical solutions.

[0015] The method for producing the above-mentioned ferroboron alloy-coated lithium iron phosphate is to firstly produce ferrous phosphate and lithium phosphate, then mix the produced ferrous phosphate and lithium phosphate, add hydrazine hydrate solution thereto, pulverize and dry, and calcinate the calcined material obtained, add pure water to the calcined material and pulverize it, add PEG, ferrous sulfate crystals, and disodium EDTA to the obtained slurry, stir and dissolve it, and then continue to add sodium borohydride solution and sodium hydroxide solution under stirring, maintain the pH of the process at 8.5-10.5, react for 15-30 minutes, filter, wash, and vacuum dry to obtain ferroboron alloy-coated lithium iron phosphate.

[0016] The method for preparing the ferroboron alloy-coated lithium iron phosphate includes the following steps.

[0017] Step 1: Produce ferrous phosphate. Ferrous sulfate, urea, phosphoric acid, ammonium dihydrogen phosphate, and hydrazine hydrate are put together in a sealed reaction vessel, and the pH of the solution is maintained at 1.5-2. Then, nitrogen gas is introduced to make the oxygen content in the sealed reaction vessel less than 1000ppm. Under stirring, the temperature is raised to 100-110°C, and the reaction is stirred at this temperature for 30-60min. Then, the pressure is released and the temperature is lowered. After the material temperature is lower than 50°C, it is taken out, filtered, and washed to obtain the precipitate of ferrous phosphate.

[0018] Second step: preparing lithium phosphate. Add P204 extractant to sulfonated kerosene and mix evenly to obtain extractant solution, then prepare lithium hydroxide solution, mix both to obtain P204-lithium soap, add phosphoric acid solution, stir and mix both to obtain lithium phosphate precipitate and P204 extractant solution, then centrifuge it to obtain lithium phosphate precipitate, wash and dry it to obtain lithium phosphate.

[0019] Third step: Mix the above prepared ferrous phosphate and lithium phosphate, then add hydrazine hydrate solution to it, then add it to the sand grinder to grind it, and grind it until the particle size of the slurry is 200-350 nm, then spray dry it to get the spray-dried material.

[0020] Fourth step: The spray-dried material is calcined in a roller furnace to obtain a calcined material.

[0021] Fifth step: add pure water to the calcined material, then add it to the sand grinder to grind it, grind it until the particle size is 150-250nm, obtain a slurry, then add PEG, ferrous sulfate crystals and disodium EDTA to the slurry, stir and dissolve, then add sodium borohydride solution and sodium hydroxide solution under stirring, maintain the pH of the process at 8.5-10.5, continue to react for 15-30min after addition, then filter it, wash the obtained filter residue, and then vacuum dry to obtain ferroboron alloy coated lithium iron phosphate.

[0022] In the method for producing ferroboron alloy-coated lithium iron phosphate, the molar ratio of ferrous sulfate, urea, phosphoric acid, ammonium dihydrogen phosphate, and hydrazine hydrate in the first step is 3:1.2-2.4:0.3-0.6:1.45-1.8:0.1-0.2.

[0023] In the method for producing the ferroboron alloy-coated lithium iron phosphate, in the first step, the stirring speed is 200-400 r / min, the heating rate is 40-60°C / h, and after the temperature is raised to 85°C, the heating rate is reduced to a heating rate of 10-15°C / h.

[0024] In the manufacturing method of the ferroboron alloy-coated lithium iron phosphate, in the second step, the volume ratio of P204 extractant and sulfonated kerosene is 2-3:7-8, the concentration of lithium hydroxide solution is 5-10mol / L, the molar ratio of added lithium and P204 extractant is 0.7-0.8:1, the concentration of phosphoric acid solution is 1.5-2.5mol / L, in the process of stirring and mixing both, the stirring speed is 300-600r / min, P204-lithium soap and phosphoric acid solution are put into a mixing kettle together and stirred while being added, the stirring blade adopts a disk turbine stirrer, a water-in-oil droplet structure is formed, the oil phase is a continuous phase, the total adding time is 60-120min, after the addition is completed, the stirring reaction is continued for 30-60min, and the P204 extractant solution obtained by centrifugation is returned for further use.

[0025] In the method for producing the ferroboron alloy-coated lithium iron phosphate, when the ferrous phosphate and the lithium phosphate are mixed in the third step, the molar ratio of the two is 1:1.01-1.05, the concentration of the added hydrazine hydrate solution is 0.02-0.05 mol / L, the mass ratio of the total mass of the ferrous phosphate and the lithium phosphate to the mass of the added hydrazine hydrate solution is 1:2.5-3.5, and the spray drying process maintains that the particle size of the final sprayed material is 3-8 μm and the moisture mass content is less than 0.5%.

[0026] In the manufacturing method of the ferroboron alloy-coated lithium iron phosphate, in the fourth step, the temperature is increased to 650-700°C at a rate of 50-100°C / h in the calcination process, the temperature is kept at 650-700°C for 3-4 hours, and then the temperature is decreased at a rate of 100-150°C / h until the material temperature reaches 80°C or lower, and then the material is discharged.

[0027] In the manufacturing method of the ferroboron alloy-coated lithium iron phosphate, in the fifth step, the calcined material is pulverized before entering the sand grinder, and pulverized to a particle size of ≦1 μm.

[0028] In the method for producing the ferroboron alloy-coated lithium iron phosphate, in the process of adding pure water to the calcined material, the mass ratio is 1:4-5, and the molar ratio of the added calcined material, PEG, ferrous sulfate crystals, disodium EDTA, and sodium borohydride is 1:0.05-0.1:0.012-0.018:0.01-0.02:0.02-0.04.

[0029] In the manufacturing method of the ferroboron alloy-coated lithium iron phosphate, in the vacuum drying process of the fifth step, the drying temperature is 80 to 120° C., the vacuum degree is −0.09 to −0.08 MPa, and the product is dried until the moisture mass content becomes less than 500 ppm, and then vacuum-packed in a constant temperature and humidity drying chamber.

[0030] Beneficial Effects: The present invention introduces a stable conductive buffer layer (ferroboron alloy) to eliminate or weaken the space charge effect, thereby suppressing the generation of an interface layer, thereby reducing the interface resistance, making it suitable for application to solid-state battery materials; the present invention uses raw materials that do not generate gas to manufacture lithium iron phosphate, so the resulting product is more dense, and the compacted density of the final product is higher, at 2.55 g / mL or more; The present invention can realize the coating by adopting a metal alloy with better electrical conductivity instead of the conventional amorphous carbon, that is, it can realize better electrical conductivity and lower interface resistance. Since the product produced by the present invention is in an alloy state, it has very high corrosion resistance and oxidation resistance. The compaction density of the final product is also very high, so that the problem that amorphous carbon has a certain degree of repulsion after compaction can be overcome. The lithium iron phosphate powder having an alloyed coating layer produced according to the present invention has a low internal resistance of about 0.2 Ω·cm, and therefore the electronic conductivity can be significantly improved. [Brief description of the drawings]

[0031] [Figure 1] 1 is a SEM pattern of the iron phosphate produced in Example 1 of the present invention. [Diagram 2] 1 is a SEM pattern of the lithium phosphate produced in Example 1 of the present invention. [Diagram 3] 1 is a SEM pattern of the ferroboron alloy-coated lithium iron phosphate produced in Example 1 of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0032] The method for producing ferroboron alloy-coated lithium iron phosphate of the present invention is to produce ferrous phosphate and lithium phosphate, mix the produced ferrous phosphate and lithium phosphate, add hydrazine hydrate solution to it, pulverize and dry, calcinate, add pure water to the calcined material obtained and pulverize, add PEG, ferrous sulfate crystal and disodium EDTA to the obtained slurry, stir and dissolve, add sodium borohydride solution and sodium hydroxide solution under stirring, keep the pH of the process at 8.5-10.5, react for 15-30min, filter, wash and vacuum dry to obtain ferroboron alloy-coated lithium iron phosphate. The specific steps are as follows:

[0033] Step 1: Produce ferrous phosphate. Ferrous sulfate, urea, phosphoric acid, ammonium dihydrogen phosphate, and hydrazine hydrate are put together in a sealed reaction vessel, and the pH of the solution is maintained at 1.5-2. Then, nitrogen gas is introduced to expel oxygen from the sealed reaction vessel, and the oxygen content in the sealed reaction vessel is made less than 1000ppm. Under stirring, the temperature is raised to 100-110°C, and the reaction is carried out at this temperature for 30-60min with stirring. Then, the pressure is released and the temperature is lowered. After the material temperature is lower than 50°C, it is taken out, filtered, and washed to obtain ferrous phosphate precipitate.

[0034] Second step: prepare lithium phosphate. Add P204 extractant to sulfonated kerosene and mix evenly to obtain extractant solution, then prepare lithium hydroxide solution, mix both to obtain P204-lithium soap, then add phosphoric acid solution to it, stir and mix both to obtain lithium phosphate precipitate and P204 extractant solution, then centrifuge it to obtain lithium phosphate precipitate, wash and dry it to obtain lithium phosphate.

[0035] Third step: Mix the above prepared ferrous phosphate and lithium phosphate, then add hydrazine hydrate solution to it, then add it to the sand grinder to grind it, and grind it until the particle size of the slurry is 200-350 nm, then spray dry it to get the spray-dried material.

[0036] Fourth step: The spray-dried material is calcined in a roller furnace to obtain a calcined material.

[0037] Fifth step: add pure water to the calcined material, then add it to the sand grinder to grind it, grind it until the particle size is 150-250nm, obtain a slurry, then add PEG, ferrous sulfate crystals and disodium EDTA to the slurry, stir and dissolve, then add sodium borohydride solution and sodium hydroxide solution under stirring, maintain the pH of the process at 8.5-10.5, continue the reaction for 15-30min after addition, then filter it, wash the obtained filter residue, and then vacuum dry it to obtain ferroboron alloy coated lithium iron phosphate.

[0038] In the first step, the molar ratio of ferrous sulfate, urea, phosphoric acid, ammonium dihydrogen phosphate, and hydrazine hydrate is 3:1.2-2.4:0.3-0.6:1.45-1.8:0.1-0.2, the stirring speed is 200-400 r / min, the temperature rise rate is 40-60°C / h, and after the temperature is raised to 85°C, the temperature rise rate is reduced to a temperature rise rate of 10-15°C / h.

[0039] In the above second step, the volume ratio of P204 extractant and sulfonated kerosene is 2~3:7~8, the concentration of lithium hydroxide solution is 5~10mol / L, the molar ratio of added lithium and P204 extractant is 0.7~0.8:1, the concentration of phosphoric acid solution is 1.5~2.5mol / L, in the process of stirring and mixing the two, the stirring speed is 300~600r / min, P204-lithium soap and phosphoric acid solution are put into a mixing kettle together, and stirring is carried out while being put in, the stirring blade adopts a disk turbine stirrer, and a droplet structure of water in oil is formed, and the oil phase is a continuous phase, the total adding time is 60~120min, and after the addition is completed, the stirring reaction is continued for 30~60min, and the P204 extractant solution obtained by centrifugation is returned for further use.

[0040] In the above third step, when ferrous phosphate and lithium phosphate are mixed, the molar ratio of the two is 1:1.01-1.05, the concentration of the added hydrazine hydrate solution is 0.02-0.05 mol / L, the mass ratio of the total mass of ferrous phosphate and lithium phosphate to the mass of the added hydrazine hydrate solution is 1:2.5-3.5, the sand grinder adopts zirconia ceramic balls as the grinding medium, and the spray drying process maintains that the particle size of the final sprayed material is 3-8 μm and the moisture mass content is less than 0.5%.

[0041] In the fourth step, in the calcination process, the temperature is increased to 650-700°C at a rate of 50-100°C / h, the temperature is maintained for 3-4 hours, and then the temperature is decreased at a rate of 100-150°C / h until the material temperature reaches 80°C or lower, after which the material is discharged.

[0042] In the fifth step, the calcined material is crushed before entering the sand grinder, and the particle size can be pulverized to ≦1 μm; In the process of adding pure water to the calcined material, the mass ratio is 1:4-5, and the molar ratio of the added calcined material, PEG, ferrous sulfate crystals, disodium EDTA, and sodium borohydride is 1:0.05-0.1:0.012-0.018:0.01-0.02:0.02-0.04; In the vacuum drying process, the drying temperature is 80 to 120°C, and the vacuum degree is -0.09 to -0.08 MPa. After drying until the moisture mass content is less than 500 ppm, the drying is stopped and the product is vacuum-packed in a constant temperature and humidity drying chamber.

[0043] The present invention can realize the coating by adopting a metal alloy having better electrical conductivity instead of the conventional amorphous carbon, that is, it can realize better electrical conductivity and lower interface resistance. Since the product produced by the present invention is in an alloy state, it has very high corrosion resistance and oxidation resistance, and the compaction density of the final product is also very high. However, amorphous carbon has a very low compaction density and many loose porous structures, and has a certain degree of repulsion after compaction, so by adopting a coating layer in an alloy state, these problems can be avoided.

[0044] The internal resistance of typical carbon-coated lithium iron phosphate powder is 10 to 50 Ω.cm (at a pressure of 10 MPa), whereas the internal resistance of the lithium iron phosphate powder having an alloy-state coating layer produced according to the present invention is as low as about 0.2 Ω.cm, thereby enabling a significant improvement in electronic conductivity.

[0045] Regarding corrosion resistance, the material of the present invention and the carbon-coated lithium iron phosphate are simultaneously placed in 0.1 mol / L hydrochloric acid and left at 25°C for 60 minutes, and the iron element therein is measured. The final measured iron element concentration of the product of the present invention after this treatment corresponds to the iron element concentration of the carbon-coated lithium iron phosphate after this treatment.

[0046] The manufacturing method of the present invention will be further described below with reference to specific examples.

[0047] Example 1

[0048] Ferrous sulfate, urea, phosphoric acid, ammonium dihydrogen phosphate, and hydrazine hydrate are put together in a sealed reaction kettle in a molar ratio of 3:2:0.4:1.6:0.15, the pH of the solution is maintained at 1.8, nitrogen gas is introduced into the sealed reaction kettle to make the oxygen content 821ppm, the temperature is raised to 105°C under stirring, and the mixture is stirred and reacted for 50 minutes, after which the pressure is released and the temperature is lowered. After the material temperature reaches 49°C, it is taken out, filtered and washed to obtain ferrous phosphate precipitate, where the stirring speed is 300r / min and the heating rate is 50°C / h. After the temperature is raised to 85°C, the heating rate is reduced to 10°C / h.

[0049] P204 extractant is added to sulfonated kerosene with a volume ratio of P204 extractant and sulfonated kerosene of 3:7, and mixed uniformly to obtain extractant solution, and lithium hydroxide solution is prepared, the concentration of lithium hydroxide solution is 8mol / L, and the extractant solution and lithium hydroxide solution are mixed with a molar ratio of 1:0.75 to obtain P204-lithium soap, and then a phosphoric acid solution with a concentration of 2mol / L is added, and the stirring speed is 500r / min, P204-lithium soap and phosphoric acid solution are put into a mixing kettle together, and stirred while being put in, and the stirring blade adopts a disk turbine stirrer, and a droplet structure of water in oil is formed, and the oil phase is a continuous phase, and the total putting time is 80min, and after the putting is completed, the stirring reaction is continued for 50min, and it is mixed and stirred to obtain lithium phosphate precipitate and P204 extractant solution, and it is centrifuged to obtain lithium phosphate precipitate, which is washed and dried to obtain lithium phosphate, and the P204 extractant solution obtained by centrifugation is returned for further use.

[0050] The above-mentioned ferrous phosphate and lithium phosphate are mixed in a molar ratio of 1:1.03, and then a hydrazine hydrate solution with a concentration of 0.04 mol / L is added, and the mass ratio of the total mass of ferrous phosphate and lithium phosphate to the mass of the added hydrazine hydrate solution is 1:3. The mixture is added to a sand grinder for grinding, and zirconia ceramic balls are used as grinding media to grind the slurry until the particle size is 285 nm. The mixture is then spray-dried to obtain a spray-dried material, and the spray-drying process maintains that the final spray material has a particle size of 6.5 μm and a moisture mass content of 0.41%.

[0051] The spray-dried material is placed in a roller furnace and calcined to obtain a calcined material. In the calcination process, the temperature is increased at a rate of 80°C / h, and the material is heated to 680°C and kept at 680°C for 3.5 hours. The temperature is then decreased at a rate of 125°C / h until the material temperature reaches 80°C, after which the material is discharged.

[0052] The calcined material is pulverized to a particle size of ≦1μm, and then pulverized with pure water in a mass ratio of 1:4.5, and pulverized until the particle size is 190nm to obtain a slurry. The calcined material, PEG, ferrous sulfate crystals and disodium EDTA are added to the slurry in a molar ratio of 1:0.08:0.016:0.02:0.03, and after stirring and dissolving, sodium borohydride solution and sodium hydroxide solution are added under stirring, and the pH of the process is maintained at 9.2. After the addition, the reaction is continued for 30min, and then it is filtered. After washing the obtained filtration residue, it is vacuum-dried under the conditions of a temperature of 110℃ and a vacuum degree of -0.085MPa, and dried until the moisture mass content is 450ppm, and then vacuum-packed in a constant temperature and humidity drying chamber to obtain a ferroboron alloy-coated lithium iron phosphate.

[0053] The SEM of the final ferrous phosphate is shown in Figure 1. As can be seen from Figure 1, it has a loose porous granular structure, with a D50 of 6.2 μm, and the detection results of the final product are shown in Table 1.

[0054] [Table 1]

[0055] The SEM of the finally obtained lithium phosphate is shown in Figure 2, which shows a stripe structure. The present invention uses an interfacial reaction to prepare lithium phosphate, and the BET of the obtained lithium phosphate is as large as 12.7 m2 / g.

[0056] The final detection results for lithium iron phosphate are shown in Table 2.

[0057] [Table 2]

[0058] The measurement pressure of the internal resistance of the powder is 10 MPa, which is measured by the four-point probe method.

[0059] The compacted density is measured at a pressure of 3T.

[0060] The method for measuring iron dissolution is to take 10 g of material, add 100 mL of 0.01 mol / L hydrochloric acid solution, and soak it at 25°C for 60 minutes, then filter it and measure the iron in the filtrate.

[0061] The method for detecting free lithium is to add 100 mL of pure water to 10 g of material, stir for 30 min, then filter it and measure the amount of lithium in the filtrate.

[0062] From the data, the product powder produced in Example 1 has a very low internal resistance of 0.12 Ω.cm, which is more than two orders of magnitude lower than that of conventional carbon-coated lithium iron phosphate, a very high capacity retention at -20°C, and excellent multiplication performance, as shown in the SEM image in Figure 3.

[0063] Example 2

[0064] Ferrous sulfate, urea, phosphoric acid, ammonium dihydrogen phosphate and hydrazine hydrate are put together in a sealed reaction kettle with a molar ratio of 3:1.8:0.5:1.5:0.1, the pH of the solution is maintained at 1.9, nitrogen gas is introduced into the sealed reaction kettle to make the oxygen content 906ppm, the temperature is raised to 100°C under stirring, and the mixture is stirred and reacted for 45min, after which the pressure is released and the temperature is lowered. After the material temperature reaches 48°C, it is taken out, filtered and washed to obtain ferrous phosphate precipitate, where the stirring speed is 400r / min and the heating rate is 55°C / h. After the temperature is raised to 85°C, the heating rate is reduced to 15°C / h.

[0065] P204 extractant is added to sulfonated kerosene with a volume ratio of P204 extractant to sulfonated kerosene of 2:7.5, and mixed uniformly to obtain extractant solution, and lithium hydroxide solution is prepared, the concentration of lithium hydroxide solution is 7mol / L, and the extractant solution and lithium hydroxide solution are mixed with a molar ratio of 1:0.7 to obtain P204-lithium soap, and then a phosphoric acid solution with a concentration of 2.3mol / L is added, and the stirring speed is 480r / min. P204-lithium soap and phosphoric acid solution are put into a mixing kettle together, and are stirred while being put in, and the stirring blade adopts a disk turbine stirrer, and a droplet structure of water in oil is formed, and the oil phase is a continuous phase, and the total pouring time is 100min, and after the pouring is completed, the stirring reaction is continued for 60min, and the mixture is stirred and mixed to obtain lithium phosphate precipitate and P204 extractant solution, and the mixture is centrifuged to obtain lithium phosphate precipitate, which is washed and dried to obtain lithium phosphate, and the P204 extractant solution obtained by centrifugation is returned for further use.

[0066] The above-mentioned ferrous phosphate and lithium phosphate are mixed in a molar ratio of 1:1.02, and then a hydrazine hydrate solution with a concentration of 0.03 mol / L is added, and the mass ratio of the total mass of ferrous phosphate and lithium phosphate to the mass of the added hydrazine hydrate solution is 1:2.5. The mixture is added to a sand grinder for grinding, and zirconia ceramic balls are used as grinding media to grind the slurry until the particle size is 230 nm. The mixture is then spray-dried to obtain a spray-dried material, and the spray-drying process maintains that the final spray material has a particle size of 9 μm and a moisture mass content of 0.5%.

[0067] The spray-dried material is placed in a roller furnace and calcined to obtain a calcined material. In the calcination process, the temperature is increased at a rate of 50°C / h, the material is heated to 650°C, and kept at that temperature for 3 hours. The temperature is then decreased at a rate of 150°C / h, and the material is cooled to 79°C before being discharged.

[0068] The calcined material is added with pure water in a mass ratio of 1:5, and then pulverized until the particle size is 150nm to obtain a slurry. The calcined material, PEG, ferrous sulfate crystals and disodium EDTA are added to the slurry in a molar ratio of 1:0.1:0.015:0.01:0.02, and after stirring and dissolving, sodium borohydride solution and sodium hydroxide solution are added under stirring, and the pH of the process is maintained at 10. After the addition, the reaction is continued for 25min, and then the filtered residue obtained is washed and then vacuum-dried under the conditions of a temperature of 100℃ and a vacuum degree of -0.09MPa, until the moisture mass content is 420ppm, and then vacuum-packed in a constant temperature and humidity drying chamber to obtain a ferroboron alloy-coated lithium iron phosphate.

[0069] The properties of the finally obtained lithium iron phosphate are shown in Table 3.

[0070] [Table 3]

[0071] The product powder obtained in Example 2 has an extremely low internal resistance of 0.11 Ω.cm, which is more than two orders of magnitude lower than that of conventional carbon-coated lithium iron phosphate, a very high capacity retention at -20°C, and excellent multiplication performance.

[0072] Example 3

[0073] Ferrous sulfate, urea, phosphoric acid, ammonium dihydrogen phosphate and hydrazine hydrate are put together in a sealed reaction kettle with a molar ratio of 3:1.9:0.6:1.7:0.2, the pH of the solution is maintained at 2, nitrogen gas is introduced into the sealed reaction kettle to make the oxygen content 830ppm, the temperature is raised to 103℃ under stirring, the reaction is stirred for 30min, the pressure is released and the temperature is lowered, after the material temperature reaches 49℃, it is taken out, filtered and washed to obtain ferrous phosphate precipitate, where the stirring speed is 350r / min, the heating rate is 40℃ / h, the temperature is raised to 85℃, and then the heating rate is reduced to 11℃ / h.

[0074] P204 extractant is added to sulfonated kerosene with a volume ratio of P204 extractant to sulfonated kerosene of 2.5:7.8, and mixed uniformly to obtain extractant solution, and lithium hydroxide solution is prepared, the concentration of lithium hydroxide solution is 9mol / L, and the extractant solution and lithium hydroxide solution are mixed with a molar ratio of 1:0.8 to obtain P204-lithium soap, and then a phosphoric acid solution with a concentration of 1.9mol / L is added, and the stirring speed is 530r / min, P204-lithium soap and phosphoric acid solution are put into a mixing kettle together, and are stirred while being put in, and the stirring blade adopts a disk turbine stirrer, and a droplet structure of water in oil is formed, and the oil phase is a continuous phase, and the total adding time is 60min, and after the addition is completed, the stirring reaction is continued for 30min, and the mixture is stirred and mixed to obtain lithium phosphate precipitate and P204 extractant solution, and the mixture is centrifuged to obtain lithium phosphate precipitate, which is washed and dried to obtain lithium phosphate, and the P204 extractant solution obtained by centrifugation is returned for further use.

[0075] The above-mentioned ferrous phosphate and lithium phosphate are mixed in a molar ratio of 1:1.02, and then a hydrazine hydrate solution with a concentration of 0.02 mol / L is added, and the mass ratio of the total mass of ferrous phosphate and lithium phosphate to the mass of the added hydrazine hydrate solution is 1:2.8. The mixture is added to a sand grinder for grinding, and zirconia ceramic balls are used as grinding media to grind the slurry until the particle size is 300 nm. The mixture is then spray-dried to obtain a spray-dried material, and the spray-drying process maintains that the final spray material has a particle size of 6 μm and a moisture mass content of 0.45%.

[0076] The spray-dried material is placed in a roller furnace and calcined to obtain a calcined material. In the calcination process, the temperature is increased at a rate of 75°C / h, and the material is heated to 670°C and kept at 670°C for 3.6 hours. The temperature is then decreased at a rate of 130°C / h until the material temperature reaches 80°C, after which the material is discharged.

[0077] The calcined material is pulverized to a particle size of 1 μm, and then pulverized with pure water in a mass ratio of 1:4 until the particle size is 250 nm, to obtain a slurry, and PEG, ferrous sulfate crystals and disodium EDTA are added to the slurry in a molar ratio of 1:0.09:0.017:0.01:0.04 between the calcined material, PEG, ferrous sulfate crystals and disodium EDTA, and stirred to dissolve. Then, under stirring, sodium borohydride solution and sodium hydroxide solution are added, and the pH of the process is maintained at 9. After the addition, the reaction is continued for 15 min, and then the filtered residue obtained is washed, and then vacuum-dried under the conditions of a temperature of 90°C and a vacuum degree of -0.08MPa, until the moisture mass content is 499 ppm, and then vacuum-packed in a constant temperature and humidity drying chamber to obtain a ferroboron alloy-coated lithium iron phosphate.

[0078] The properties of the finally obtained lithium iron phosphate are shown in Table 4.

[0079] [Table 4]

[0080] The product powder obtained in Example 3 has an extremely low internal resistance of 0.08 Ω.cm, which is more than two orders of magnitude lower than that of conventional carbon-coated lithium iron phosphate, a very high capacity retention at -20°C, and excellent multiplication performance.

[0081] Example 4

[0082] Ferrous sulfate, urea, phosphoric acid, ammonium dihydrogen phosphate and hydrazine hydrate are put together in a sealed reaction kettle with a molar ratio of 3:2.1:0.3:1.45:0.18, the pH of the solution is maintained at 1.7, nitrogen gas is introduced into the sealed reaction kettle to make the oxygen content 980ppm, the temperature is raised to 110°C under stirring, and the mixture is stirred and reacted for 35 minutes, after which the pressure is released and the temperature is lowered. After the material temperature reaches 49°C, it is taken out, filtered and washed to obtain ferrous phosphate precipitate, where the stirring speed is 250r / min and the heating rate is 60°C / h. After the temperature is raised to 85°C, the heating rate is reduced to 13°C / h.

[0083] P204 extractant is added to sulfonated kerosene in a volume ratio of 2.8:7.2, and mixed uniformly to obtain an extractant solution. The concentration of the lithium hydroxide solution is 5 mol / L. The extractant solution and the lithium hydroxide solution are mixed in a molar ratio of 1:0.77 to obtain P204-lithium soap. Then, a phosphoric acid solution with a concentration of 2.5 mol / L is added, and the stirring speed is 600 r / min. The P204-lithium soap and the phosphoric acid solution are mixed in a mixing kettle. The mixture is stirred while being added, and the stirring blade is a disk turbine agitator, which forms a water-in-oil droplet structure, and the oil phase is a continuous phase. The total addition time is 120 minutes. After the addition is completed, the mixture is stirred and reacted for 40 minutes, and then stirred and mixed to obtain lithium phosphate precipitate and P204 extractant solution, which is centrifuged to obtain lithium phosphate precipitate, which is washed and dried to obtain lithium phosphate, and the P204 extractant solution obtained by centrifugation is returned for further use.

[0084] The above-mentioned ferrous phosphate and lithium phosphate are mixed in a molar ratio of 1:1.04, and then a hydrazine hydrate solution with a concentration of 0.05 mol / L is added, and the mass ratio of the total mass of ferrous phosphate and lithium phosphate to the mass of the added hydrazine hydrate solution is 1:3. The mixture is added to a sand grinder for grinding, and zirconia ceramic balls are used as grinding media to grind the slurry until the particle size is 200 nm. The mixture is then spray-dried to obtain a spray-dried material, and the spray-drying process maintains that the final spray material has a particle size of 5 μm and a moisture mass content of 0.39%.

[0085] The spray-dried material is placed in a roller furnace and calcined to obtain a calcined material. In the calcination process, the temperature is increased at a rate of 100°C / h, the material is heated to 700°C, and kept at this temperature for 4 hours. The temperature is then decreased at a rate of 100°C / h until the material temperature reaches 78°C, after which the material is discharged.

[0086] The calcined material is pulverized to a particle size of 0.95 μm, and then pulverized with pure water in a mass ratio of 1:4.5 until the particle size is 150 nm to obtain a slurry. The calcined material, PEG, ferrous sulfate crystals and disodium EDTA are added to the slurry in a molar ratio of 1:0.07:0.013:0.02:0.03, and after stirring and dissolving, sodium borohydride solution and sodium hydroxide solution are added under stirring, and the pH of the process is maintained at 8.5. After the addition, the reaction is continued for 20 min, and then it is filtered. The obtained filtration residue is washed, and then vacuum-dried under the conditions of a temperature of 80°C and a vacuum degree of -0.088 MPa, until the moisture mass content is 490 ppm, and then vacuum-packed in a constant temperature and humidity drying chamber to obtain a ferroboron alloy-coated lithium iron phosphate.

[0087] The properties of the finally obtained lithium iron phosphate are shown in Table 5.

[0088] [Table 5]

[0089] The product powder obtained in Example 4 has an extremely low internal resistance of 0.09 Ω.cm, which is more than two orders of magnitude lower than that of conventional carbon-coated lithium iron phosphate, has a very high capacity retention at -20°C, and is excellent in terms of multiplication performance.

[0090] Example 5

[0091] Ferrous sulfate, urea, phosphoric acid, ammonium dihydrogen phosphate and hydrazine hydrate are put together in a sealed reaction kettle with a molar ratio of 3:2.4:0.4:1.8:0.12, the pH of the solution is maintained at 1.6, nitrogen gas is introduced into the sealed reaction kettle to make the oxygen content 850ppm, the temperature is raised to 107°C under stirring, and the mixture is stirred and reacted for 60min, after which the pressure is released and the temperature is lowered. After the material temperature is lower than 50°C, it is taken out, filtered and washed to obtain ferrous phosphate precipitate, where the stirring speed is 320r / min and the heating rate is 45°C / h. After the temperature is raised to 85°C, the heating rate is reduced to 12°C / h.

[0092] P204 extractant is added to sulfonated kerosene in a volume ratio of 2.2:7.9, and mixed uniformly to obtain an extractant solution. A lithium hydroxide solution is prepared, the concentration of which is 10 mol / L. The extractant solution and the lithium hydroxide solution are mixed in a molar ratio of 1:0.73 to obtain P204-lithium soap. Then, a phosphoric acid solution with a concentration of 1.5 mol / L is added, and the stirring speed is 450 r / min. The P204-lithium soap and the phosphoric acid solution are mixed. The mixture is put into a kettle together and stirred while being added. The stirring blade is a disc turbine stirrer, which forms a water-in-oil droplet structure, and the oil phase is a continuous phase. The total addition time is 110 minutes. After the addition is completed, the mixture is stirred and reacted for 35 minutes, which is then mixed and stirred to obtain lithium phosphate precipitate and P204 extractant solution, which is centrifuged to obtain lithium phosphate precipitate, which is washed and dried to obtain lithium phosphate, and the P204 extractant solution obtained by centrifugation is returned for further use.

[0093] The above-mentioned ferrous phosphate and lithium phosphate are mixed in a molar ratio of 1:1.03, and then a hydrazine hydrate solution with a concentration of 0.03 mol / L is added, and the mass ratio of the total mass of ferrous phosphate and lithium phosphate to the mass of the added hydrazine hydrate solution is 1:3.2. The mixture is added to a sand grinder for grinding, and zirconia ceramic balls are used as grinding media to grind the slurry until the particle size is 300 nm. The mixture is then spray-dried to obtain a spray-dried material, and the spray-drying process maintains that the final spray material has a particle size of 4 μm and a moisture mass content of 0.48%.

[0094] The spray-dried material is placed in a roller furnace and calcined to obtain a calcined material. In the calcination process, the temperature is increased at a rate of 60°C / h, and the material is heated to 690°C and kept at that temperature for 3.2 hours. The temperature is then decreased at a rate of 120°C / h until the material temperature reaches 79°C, after which the material is discharged.

[0095] The calcined material is added with pure water in a mass ratio of 1:4.8, and pulverized until the particle size is 200nm to obtain a slurry; the calcined material, PEG, ferrous sulfate crystals, disodium EDTA, and sodium borohydride are added to the slurry in a molar ratio of 1:0.06:0.014:0.01:0.04; after stirring and dissolving, sodium borohydride solution and sodium hydroxide solution are added under stirring; the pH of the process is maintained at 10.5; after addition, the reaction is continued for 28min; then, it is filtered; the obtained filtration residue is washed, and then vacuum-dried under the conditions of a temperature of 120℃ and a vacuum degree of -0.082MPa, until the moisture mass content is 480ppm; and then vacuum-packed in a constant temperature and humidity drying chamber to obtain a ferroboron alloy-coated lithium iron phosphate.

[0096] The properties of the finally obtained lithium iron phosphate are shown in Table 6.

[0097] [Table 6]

[0098] The product powder obtained in Example 5 has an extremely low internal resistance of 0.10 Ω.cm, which is more than two orders of magnitude lower than that of conventional carbon-coated lithium iron phosphate, a very high capacity retention at -20°C, and excellent multiplication performance.

[0099] Example 6

[0100] Ferrous sulfate, urea, phosphoric acid, ammonium dihydrogen phosphate and hydrazine hydrate are put together in a sealed reaction kettle with a molar ratio of 3:1.5:0.5:1.65:0.15, the pH of the solution is maintained at 1.5, nitrogen gas is introduced into the sealed reaction kettle to make the oxygen content 890ppm, the temperature is raised to 109°C under stirring, and the reaction is stirred for 55 minutes, after which the pressure is released and the temperature is lowered. After the material temperature is lower than 50°C, it is taken out, filtered and washed to obtain ferrous phosphate precipitate, where the stirring speed is 200r / min and the heating rate is 53°C / h. After the temperature is raised to 85°C, the heating rate is reduced to 14°C / h.

[0101] P204 extractant is added to sulfonated kerosene with a volume ratio of P204 extractant and sulfonated kerosene of 2:7, and mixed uniformly to obtain extractant solution. Lithium hydroxide solution is prepared, and the concentration of lithium hydroxide solution is 6mol / L. Extractant solution and lithium hydroxide solution are mixed with a molar ratio of 1:0.78 to obtain P204-lithium soap. Then, phosphoric acid solution with a concentration of 1.8mol / L is added. The stirring speed is 300r / min. P204-lithium soap and phosphoric acid solution are put into a mixing kettle together, and are stirred while being put in. The stirring blade adopts a disk turbine stirrer, and a droplet structure of water in oil is formed, and the oil phase is a continuous phase. The total pouring time is 70min. After the pouring is completed, the stirring reaction is continued for 55min, and the mixture is stirred to obtain lithium phosphate precipitate and P204 extractant solution. The mixture is centrifuged to obtain lithium phosphate precipitate, which is washed and dried to obtain lithium phosphate. The P204 extractant solution obtained by centrifugation is returned for further use.

[0102] The above-mentioned ferrous phosphate and lithium phosphate are mixed in a molar ratio of 1:1.05, and then a hydrazine hydrate solution with a concentration of 0.05 mol / L is added, and the mass ratio of the total mass of ferrous phosphate and lithium phosphate to the mass of the added hydrazine hydrate solution is 1:3.5. The mixture is added to a sand grinder for grinding, and zirconia ceramic balls are used as grinding media to grind the slurry until the particle size is 250 nm. The mixture is then spray-dried to obtain a spray-dried material, and the spray-drying process maintains that the final spray material has a particle size of 3 μm and a moisture mass content of 0.43%.

[0103] The spray-dried material is placed in a roller furnace and calcined to obtain a calcined material. In the calcination process, the temperature is increased at a rate of 70°C / h, and the material is heated to 660°C and kept at 660°C for 3.8 hours. The temperature is then decreased at a rate of 140°C / h until the material temperature reaches 77°C, after which the material is discharged.

[0104] The calcined material is added with pure water in a mass ratio of 1:4.2 and pulverized until the particle size is 180 nm to obtain a slurry; the calcined material, PEG, ferrous sulfate crystals and disodium EDTA are added to the slurry in a molar ratio of 1:0.05:0.018:0.02:0.02 of PEG, ferrous sulfate crystals and disodium EDTA; after stirring and dissolving, add sodium borohydride solution and sodium hydroxide solution under stirring; maintain the pH of the process at 9.2; continue to react for 30 min after addition; then filter it; wash the obtained filtration residue, and vacuum dry it under the conditions of a temperature of 105°C and a vacuum degree of -0.08MPa, until the moisture mass content is 470 ppm, and vacuum package it in a constant temperature and humidity drying room to obtain ferroboron alloy-coated lithium iron phosphate. The properties of the final product are as shown in Table 7.

[0105] [Table 7] The product powder obtained in Example 6 has an extremely low internal resistance of 0.21 Ω.cm, which is more than two orders of magnitude lower than that of conventional carbon-coated lithium iron phosphate, a very high capacity retention at -20°C, and excellent multiplication performance.

[0106] Example 7

[0107] Ferrous sulfate, urea, phosphoric acid, ammonium dihydrogen phosphate and hydrazine hydrate are put together in a sealed reaction kettle with a molar ratio of 3:1.2:0.6:1.55:0.17, the pH of the solution is maintained at 1.8, nitrogen gas is introduced into the sealed reaction kettle to make the oxygen content 932ppm, the temperature is raised to 106°C under stirring, and the mixture is stirred and reacted for 40min, after which the pressure is released and the temperature is lowered. After the material temperature is lower than 50°C, it is taken out, filtered and washed to obtain ferrous phosphate precipitate, where the stirring speed is 250r / min and the heating rate is 50°C / h. After the temperature is raised to 85°C, the heating rate is reduced to 10°C / h.

[0108] P204 extractant is added to sulfonated kerosene with a volume ratio of P204 extractant and sulfonated kerosene of 3:8, and mixed uniformly to obtain extractant solution, and lithium hydroxide solution is prepared, the concentration of lithium hydroxide solution is 8mol / L, and the extractant solution and lithium hydroxide solution are mixed with a molar ratio of 1:0.74 to obtain P204-lithium soap, and then a phosphoric acid solution with a concentration of 1.5mol / L is added, and the stirring speed is 360r / min, P204-lithium soap and phosphoric acid solution are put into a mixing kettle together, and are stirred while being put in, and the stirring blade adopts a disk turbine stirrer, and a droplet structure of water in oil is formed, and the oil phase is a continuous phase, and the total adding time is 90min, and after the addition is completed, the stirring reaction is continued for 45min, and the stirring and mixing are performed to obtain lithium phosphate precipitate and P204 extractant solution, which is centrifuged to obtain lithium phosphate precipitate, which is washed and dried to obtain lithium phosphate, and the P204 extractant solution obtained by centrifugation is returned for further use.

[0109] The above-mentioned ferrous phosphate and lithium phosphate are mixed in a molar ratio of 1:1.01, and then a hydrazine hydrate solution with a concentration of 0.03 mol / L is added, and the mass ratio of the total mass of ferrous phosphate and lithium phosphate to the mass of the added hydrazine hydrate solution is 1:3.3. The mixture is added to a sand grinder for grinding, and zirconia ceramic balls are used as grinding media to grind the slurry until the particle size is 325 nm. The mixture is then spray-dried to obtain a spray-dried material, and the spray-drying process maintains that the final spray material has a particle size of 8 μm and a moisture mass content of 0.40%.

[0110] The spray-dried material is placed in a roller furnace and calcined to obtain a calcined material. In the calcination process, the temperature is increased at a rate of 90°C / h, the material is heated to 680°C, and kept at 680°C for 3.5 hours. The temperature is then decreased at a rate of 110°C / h, and the material is cooled to a temperature below 80°C before being discharged.

[0111] The calcined material is pulverized to a particle size of 0.96 μm, and then pulverized with pure water in a mass ratio of 1:4.5 until the particle size is 190 nm to obtain a slurry. The calcined material, PEG, ferrous sulfate crystals and disodium EDTA are added to the slurry in a molar ratio of 1:0.07:0.012:0.02:0.03, and after stirring and dissolving, sodium borohydride solution and sodium hydroxide solution are added under stirring, and the pH of the process is maintained at 8.9. After the addition, the reaction is continued for 30 min, and then it is filtered. The obtained filtration residue is washed, and then vacuum-dried under the conditions of a temperature of 115°C and a vacuum degree of -0.09MPa, until the moisture mass content is 460 ppm, and then vacuum-packed in a constant temperature and humidity drying chamber to obtain a ferroboron alloy-coated lithium iron phosphate.

[0112] The properties of the finally obtained lithium iron phosphate are shown in Table 8.

[0113] [Table 8]

[0114] The product powder obtained in Example 7 has an extremely low internal resistance of 0.28 Ω.cm, which is more than two orders of magnitude lower than that of conventional carbon-coated lithium iron phosphate, has a very high capacity retention at -20°C, and is excellent in terms of multiplication performance.

[0115] As can be seen from the above examples, the present invention can eliminate or weaken the space charge effect by introducing a stable conductive buffer layer (ferroboron alloy), thereby suppressing the generation of the interface layer, thereby reducing the interface resistance, which is suitable for application to solid battery materials; and the lithium iron phosphate is produced using raw materials that do not generate gas, so the resulting product is more dense and the compaction density of the final product is higher.

Claims

1. First, ferrous phosphate and lithium phosphate are produced, The produced ferrous phosphate and lithium phosphate are then mixed, a hydrazine hydrate solution is added, the mixture is pulverized and dried, and then calcined. Pure water is added to the calcined material obtained, and the mixture is pulverized. PEG, ferrous sulfate crystals, and disodium EDTA are added to the resulting slurry, which is stirred and dissolved. Then, a sodium borohydride solution and a sodium hydroxide solution are added under stirring, the pH of the process is maintained at 8.5 to 10.5, and the reaction is carried out for 15 to 30 minutes. The resulting mixture is filtered, washed, and vacuum dried to obtain a ferroboron alloy-coated lithium iron phosphate.

2. The specific steps are: The first step for producing ferrous phosphate is to add ferrous sulfate, urea, phosphoric acid, ammonium dihydrogen phosphate and hydrazine hydrate together into a sealed reaction kettle, maintain the pH of the solution at 1.5-2, then introduce nitrogen gas to make the oxygen content in the sealed reaction kettle less than 1000 ppm, and heat the temperature to 100-110°C under stirring, react at this temperature for 30-60 minutes with stirring, then release the pressure and cool the material, and after the material temperature is less than 50°C, take it out, filter and wash it to obtain ferrous phosphate precipitate; The second step of preparing lithium phosphate is to add P204 extractant to sulfonated kerosene and mix uniformly to obtain extractant solution, then prepare lithium hydroxide solution and mix them to obtain P204-lithium soap, then add phosphoric acid solution and stir mix them to obtain lithium phosphate precipitate and P204 extractant solution, then centrifuge it to obtain lithium phosphate precipitate, wash and dry it to obtain lithium phosphate; The third step is to mix the above prepared ferrous phosphate and lithium phosphate, then add hydrazine hydrate solution, then add it to a sand grinder to grind, and grind until the particle size of the slurry is 200-350 nm, then spray dry it to obtain a spray-dried material; a fourth step of calcining the spray-dried material in a roller furnace to obtain a calcined material; and a fifth step of adding pure water to the calcined material, then adding it to a sand grinder to grind it, and grinding it until the particle size is 150-250 nm to obtain a slurry, then adding PEG, ferrous sulfate crystals and disodium EDTA to the slurry, stirring and dissolving, and then adding sodium borohydride solution and sodium hydroxide solution under stirring, maintaining the pH of the process at 8.5-10.5, and continuing to react for 15-30 min after adding, and then filtering it, and washing the obtained filtration residue, and then drying it in vacuum to obtain a ferroboron alloy-coated lithium iron phosphate.

3. 3. The method for producing ferroboron alloy-coated lithium iron phosphate according to claim 2, wherein in the first step, a molar ratio of ferrous sulfate, urea, phosphoric acid, ammonium dihydrogen phosphate, and hydrazine hydrate is 3:1.2-2.4:0.3-0.6:1.45-1.8:0.1-0.

2.

4. 3. The method for producing ferroboron alloy-coated lithium iron phosphate according to claim 2, wherein in the first step, the stirring speed is 200-400 r / min, the heating rate is 40-60° C. / h, and after the temperature is raised to 85° C., the heating rate is reduced to a heating rate of 10-15° C. / h.

5. The method for producing ferroboron alloy-coated lithium iron phosphate according to claim 2, characterized in that in the second step, the volume ratio of P204 extractant to sulfonated kerosene is 2-3:7-8, the concentration of lithium hydroxide solution is 5-10 mol / L, the molar ratio of added lithium to P204 extractant is 0.7-0.8:1, and the concentration of phosphoric acid solution is 1.5-2.5 mol / L. In the process of stirring and mixing the two, the stirring speed is 300-600 r / min, the P204-lithium soap and the phosphoric acid solution are put into a mixing kettle together and stirred while being added, the stirring blade adopts a disk turbine stirrer, a water-in-oil droplet structure is formed, and the oil phase is a continuous phase, the total adding time is 60-120 min, and after the addition is completed, the stirring reaction is continued for 30-60 min, and the P204 extractant solution obtained by centrifugation is returned for further use.

6. In the third step, when ferrous phosphate and lithium phosphate are mixed, the molar ratio of the two is 1:1.01 to 1.05, the concentration of the added hydrazine hydrate solution is 0.02 to 0.05 mol / L, and the mass ratio of the total mass of ferrous phosphate and lithium phosphate to the mass of the added hydrazine hydrate solution is 1:2.5 to 3.5; The method for producing ferroboron alloy-coated lithium iron phosphate according to claim 2, characterized in that the spray-drying process maintains the particle size of the final sprayed material to be 3-8 μm and the moisture mass content to be less than 0.5%.

7. The method for producing ferroboron alloy-coated lithium iron phosphate according to claim 2, characterized in that in the fourth step, the temperature is increased at a rate of 50-100°C / h in the calcination process, the temperature is increased to 650-700°C, the temperature is maintained for 3-4 hours, and then the temperature is decreased at a rate of 100-150°C / h, and the material is cooled to a temperature of 80°C or less, and then the material is discharged.

8. 3. The method for producing ferroboron alloy-coated lithium iron phosphate according to claim 2, wherein in the fifth step, the calcined material is pulverized before entering the sand grinder to a particle size of ≦1 μm.

9. The method for producing ferroboron alloy-coated lithium iron phosphate according to claim 2 or 8, characterized in that in the process of adding pure water to the calcined material, the mass ratio is 1:4-5, and the molar ratio of the added calcined material, PEG, ferrous sulfate crystals, disodium EDTA, and sodium borohydride is 1:0.05-0.1:0.012-0.018:0.01-0.02:0.02-0.

04.

10. The method for producing ferroboron alloy-coated lithium iron phosphate according to claim 2 or 8, characterized in that in the vacuum drying process of the fifth step, the drying temperature is 80 to 120°C, the vacuum degree is -0.09 to -0.08 MPa, and the product is dried until the moisture mass content is less than 500 ppm, and then vacuum-packed in a constant temperature and humidity drying chamber.

Citation Information

Patent Citations

  • Lithium ion battery with high energy density

    CN105470559A

  • Preparation method of coated lithium iron borate

    CN108511736A