Manufacturing method of the article

The use of laser-sintered flaky metal particles with specific diameters addresses the adhesion-conductivity trade-off in printed electronics, forming a conductive sintered body layer with enhanced properties on complex surfaces.

JP7567160B2Active Publication Date: 2024-10-16RESONAC CORP
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2019157995
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2019-08-30
Publication Date
2024-10-16
Estimated Expiration
2039-08-30

AI Technical Summary

Technical Problem

Conventional printed electronics methods face a trade-off between the adhesion of the sintered body layer to the base material and its conductivity, with the use of binder resins compromising electrical conductivity.

Method used

A manufacturing method involving the use of flaky metal particles with a median diameter of 4.0 μm or more, sintered by laser irradiation, forms a sintered body layer with excellent adhesion and conductivity by suppressing cracks through the combination of flaky and spherical copper particles.

Benefits of technology

The method achieves a sintered body layer with high adhesion and conductivity without the need for binder resins, enabling the formation of conductive wiring on complex surfaces.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007567160000001
    Figure 0007567160000001
  • Figure 0007567160000002
    Figure 0007567160000002
  • Figure 0007567160000003
    Figure 0007567160000003
Patent Text Reader

Abstract

To provide a method for manufacturing an article including a base material and a metal sintered body layer formed on a surface of the base material in which both excellent adhesion of the sintered body layer with respect to the base material and excellent conductivity of the sintered body layer reach a sufficiently high level.SOLUTION: A method for manufacturing an article includes: forming a metal particle-containing layer on a surface of a base material by using a composition containing metal particles; and irradiating laser toward the metal particle-containing layer so that the metal particles are sintered to form a metal sintered body layer, in which the metal particles include flaky metal particles whose median size is 4.0 μm or more.SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing an article and a composition for forming a metal sintered body layer. [Background technology]

[0002] A method known as a printed electronics method is known as a method for forming a circuit pattern (see, for example, Patent Documents 1 and 2). This method includes a step of forming a pattern composed of ink, paste, etc. containing metal particles on a substrate by inkjet printing, screen printing, dispense printing, etc., and a step of forming a conductive circuit pattern by heating the pattern containing metal particles. The metal particles contained in the ink or paste are sintered by heat to form a sintered layer, thereby exhibiting conductivity.

[0003] In recent years, from the viewpoint of miniaturization and weight reduction of wiring, attention has been focused on molded interconnect devices (hereinafter sometimes referred to as "MIDs"). MIDs are components in which wiring is formed directly on a molded body having a three-dimensional surface such as an uneven surface or a curved surface, and are used in various fields, for example, by mounting electronic components on the wiring using solder. According to the formation technology of MIDs, it is possible to manufacture a structure in which wiring is formed in the dead space of a device, a structure in which a harness is removed, etc., so that it is possible to reduce the weight of in-vehicle components and to miniaturize smartphones, etc. As one aspect of the formation technology of MIDs, the Laser Direct Structuring method (hereinafter sometimes referred to as "LDS method") is known. The LDS method includes a step of producing a molded body containing metal particles, a step of making the metal particles conductive by irradiating a laser to an area on the surface of the molded body where a circuit is to be formed, and a step of forming a circuit by performing electroless plating on the conductive part on the surface of the molded body. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2012-072418 A [Patent Document 2] JP 2014-148732 A Summary of the Invention [Problem to be solved by the invention]

[0005] In the printed electronics method, there is a trade-off between the adhesion of the sintered body layer constituting the circuit pattern to the substrate and the electrical conductivity of the sintered body layer. In other words, when a binder resin for improving the adhesion of the sintered body layer is mixed with metal particles in the ink or paste, the electrical conductivity of the sintered body layer tends to decrease. In this respect, there is room for improvement in the conventional printed electronics method.

[0006] The present invention aims to provide a method for producing an article comprising a substrate and a metal sintered body layer formed on the surface thereof, in which the sintered body layer has a sufficiently high level of both excellent adhesion to the substrate and excellent electrical conductivity of the sintered body layer. The present invention also aims to provide a composition for forming a metal sintered body layer for forming the sintered body layer in such an article. [Means for solving the problem]

[0007] One aspect of the present invention relates to a method for producing an article. The method for producing an article includes the steps of forming a metal particle-containing layer on a surface of a substrate using a composition containing metal particles, and irradiating the metal particle-containing layer with a laser so that the metal particles are sintered to form a sintered metal layer. The metal particles include flake-shaped metal particles having a median diameter of 4.0 μm or more.

[0008] According to the research of the present inventors, a technique for sintering metal particles by laser irradiation to form a sintered body layer with a thickness of about 1 μm has been known. However, this technique has a risk of cracking the sintered body layer in the laser irradiated area. The cracks reduce the adhesion of the sintered body layer to the substrate and the conductivity of the sintered body layer.

[0009] In contrast, according to the manufacturing method of the present invention, it is possible to form a sintered layer on a substrate by sintering metal particles by laser irradiation, and it is also possible to suppress cracks in the sintered layer. The inventors of the present invention presume that the so-called large-diameter flake-shaped metal particles suppress shrinkage due to sintering.

[0010] One aspect of the present invention relates to a composition for forming a metal sintered layer by laser sintering, which contains flake-shaped metal particles having a median diameter of 4.0 μm or more. This composition can be used in, for example, the above-mentioned production method, and can form a layer having excellent adhesion to a substrate and excellent electrical conductivity on the surface of the substrate. Effect of the Invention

[0011] According to the present invention, there is provided a method for producing an article comprising a substrate and a metal sintered body layer formed on the surface thereof, the method being such that both excellent adhesion of the sintered body layer to the substrate and excellent electrical conductivity of the sintered body layer are at a sufficiently high level. Also, according to the present invention, there is provided a composition for forming a metal sintered body layer for forming the sintered body layer in the article. [Brief description of the drawings]

[0012] [Figure 1] FIG. 1 is a perspective view showing an article obtained by a method for producing an article according to one embodiment. [Diagram 2] 2(a) to 2(c) are cross-sectional views that typically show the steps of forming a sintered body layer on a substrate. [Diagram 3] FIG. 3(a) and FIG. 3(b) are photographs showing the appearance of metal sintered layers formed using the compositions for forming a metal sintered layer of the examples and the comparative examples, respectively. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] Hereinafter, the embodiment for carrying out the present invention will be described in detail. However, the present invention is not limited to the following embodiment. In the following embodiment, the components (including element steps, etc.) are not essential unless specifically stated. The same applies to the numerical values ​​and their ranges, and they do not limit the present invention.

[0014] In this specification, the term "process" includes processes that are independent of other processes, as well as processes that cannot be clearly distinguished from other processes, as long as the purpose of the process is achieved. In this specification, a numerical range indicated using "~" includes the numerical values ​​before and after "~" as the minimum and maximum values, respectively. In a numerical range described in stages in this specification, the upper limit or lower limit described in one numerical range may be replaced with the upper limit or lower limit of another numerical range described in stages. In addition, in a numerical range described in this specification, the upper limit or lower limit of the numerical range may be replaced with a value shown in an example. In this specification, the content or amount of each component in a composition means the total content or amount of the multiple substances present in the composition, unless otherwise specified, when multiple substances corresponding to each component are present in the composition.

[0015] <Goods> Fig. 1 is a perspective view showing an article obtained by a method for producing an article according to one embodiment. As shown in Fig. 1, the article 1 includes a substrate 2 and a sintered body layer 3 provided on the substrate 2. A roughened portion 2a (see Fig. 2(c)) may be formed on the surface of the substrate 2 with which the sintered body layer 3 is in contact. The roughened portion 2a is formed due to the laser irradiation used to form the sintered body layer 3.

[0016] The shape of the substrate 2 is appropriately selected depending on the application. The substrate 2 may be a three-dimensional object having a three-dimensional shape such as a concave-convex shape. The substrate 2 is produced, for example, by molding a resin using a mold. The resin constituting the substrate 2 may be a resin having low heat resistance (for example, a resin having a glass transition temperature and / or a 5% thermal weight loss temperature described later), for example, a thermoplastic resin. The thermoplastic resin may be a polyolefin such as polyethylene, polypropylene, polymethylpentene, polycarbonate, polyethylene terephthalate, liquid crystal plastic, etc., and is preferably polypropylene, polycarbonate, polyethylene terephthalate, or liquid crystal plastic.

[0017] The glass transition temperature of the resin may be 150° C. or lower, 120° C. or lower, or 80° C. or lower, or may be 30° C. or higher. The glass transition temperature of the resin is measured by dynamic viscoelasticity measurement, specifically, for example, using a dynamic viscoelasticity measuring device, and is measured as the temperature at which tan δ is maximum under conditions of a frequency of 10 Hz, a heating rate of 5° C. / min, and a temperature range of 20 to 260° C.

[0018] The 5% thermal weight loss temperature of the resin may be 400° C. or less, 300° C. or less, 250° C. or less, or 200° C. or less. The 5% thermal weight loss temperature of the resin is defined as the temperature at which the weight of the resin decreases by 5 wt% relative to the weight of the resin at 25° C. (before heating) when the resin is heated from 25° C. at a heating rate of 5° C. / min in a nitrogen atmosphere using a thermogravimetric analyzer (TGA).

[0019] The sintered body layer 3 is provided, for example, on one surface 2f side (upper surface side in FIG. 1) of the substrate 2. The one surface 2f of the substrate 2 may be a surface having a three-dimensional shape such as an uneven surface or a curved surface. The sintered body layer 3 is a layer having electrical conductivity, and may be, for example, wiring that forms an electric circuit (which may be linear when viewed from above).

[0020] The sintered body layer 3 may be a layer containing a copper sintered body. The sintered body layer 3 may be obtained by sintering a composition containing copper particles (details will be described later). The sintered body layer 3 may be, for example, a porous layer. The porosity of the sintered body layer 3 may be 10% or more, 13% or more, or 15% or more, and may be 70% or less, 55% or less, or 40% or less. The porosity of the sintered body layer 3 means the ratio of the area of ​​the non-conductive part where no sintered body is present to the total area of ​​the cross section of the sintered body layer 3, which is obtained by analyzing a cross-sectional image of the sintered body layer 3 observed by a scanning electron microscope, a scanning ion microscope, or the like, using image analysis software.

[0021] The sintered body layer 3 can be a thin-line wiring having a sufficient thickness. The thickness of the sintered body layer 3 may be 5.0 μm or more, 7.0 μm or more, or 10.0 μm or more, and may be 60 μm or less, 50 μm or less, or 32 μm or less. The line width of the sintered body layer 3 (the length of the short side direction (direction perpendicular to the direction in which the wiring extends) of the sintered body layer (wiring) 3 when viewed from above) may be 1 mm or less, 0.7 mm or less, 0.5 mm or less, 0.4 mm or less, 0.3 mm or less, or 0.2 mm or less.

[0022] <Production method> A method for producing the article 1 will be described with reference to Fig. 2(a) to Fig. 2(c). This method includes a step of forming a metal particle-containing layer 3P on the surface of the substrate 2 using a composition containing metal particles, and a step of irradiating a laser toward the metal particle-containing layer 3P so that the metal particles are sintered to form a metal sintered body layer 3. Here, the metal particles may contain a sinterable metal, and may contain, for example, silver (Ag), copper (Cu), palladium (Pd), aluminum (Al), nickel (Ni), etc. A sinterable metal is a metal that can form a sintered body when its metal particles are heated at a temperature lower than the melting point. Hereinafter, an example will be described in which the sinterable metal is copper, but in the following description, "copper" may be replaced with another "metal" having sinterability.

[0023] (Step of forming metal particle-containing layer) This step is a step of forming a metal particle-containing layer 3P made of (containing) a composition containing copper particles by applying the composition onto one surface 2f of the substrate 2 (see FIG. 2(a)). In this embodiment, the metal particle-containing layer 3P is formed so as to cover an area on the surface of the substrate 2 where a pattern is to be formed. That is, in this embodiment, the metal particle-containing layer 3P is formed in a predetermined area on the surface of the substrate 2 by so-called solid coating.

[0024] The metal particle-containing layer 3P can be formed, for example, by a method using an aerosol jet. As the device, a spraying device equipped with an atomizer and a discharge nozzle connected to the atomizer can be used. As such a spraying device, a device to which a known spraying method is applied can be used as it is. As the known spraying method, for example, an aerosol deposition method, a cold spray method, a thermal spray method, etc. can be mentioned.

[0025] The composition used in this step (composition for forming a metal sintered body layer) contains at least copper particles, and further contains, for example, a dispersion medium. The copper particles contain copper as a main component from the viewpoint of thermal conductivity and sinterability. The proportion of copper element in the copper particles may be 80 atomic % or more, 90 atomic % or more, or 95 atomic % or more based on all elements excluding hydrogen, carbon, and oxygen. When the element proportion is 80 atomic % or more, the thermal conductivity and sinterability derived from copper tend to be easily expressed.

[0026] The shape of the copper particles is not particularly limited, and examples thereof include spherical, approximately spherical, polyhedral, needle-like, flake-like, and rod-like. The copper particles may contain at least flake-like copper particles, and may further contain other copper particles of different shapes. By containing copper particles of different shapes, cracks in the wiring to be formed tend to be suppressed, and wiring having a sufficient thickness tends to be easily formed. The reason for this is not necessarily clear, but it is thought that this is because copper particles of different shapes complement each other's gaps, and the occurrence of volume reduction in all directions due to fusion between copper particles is suppressed. As a result, it is presumed that cracks are suppressed even in wiring having a sufficient thickness. The combination of different shapes is not particularly limited, and for example, a combination of flake-like copper particles (A1) and spherical copper particles (A2) is preferable.

[0027] The median diameter of the flaky copper particles (A1) is 4.0 μm or more. This can suppress cracking of the sintered body layer due to laser sintering. From this viewpoint, the median diameter may be 5.0 μm or more or 8.0 μm or more. The upper limit of the median diameter may be 20.0 μm from the viewpoint of easily maintaining good low-temperature sinterability and coatability. The median diameter of the spherical copper particles (A2) may be 0.1 to 2.0 μm, 0.1 to 1.2 μm, 0.1 to 0.9 μm, or 0.1 to 0.6 μm. By combining the flaky copper particles (A1) and the spherical copper particles (A2) having such a median diameter, the fusibility at low temperatures tends to be more excellent. The median particle size refers to the D50 value (cumulative median of volume distribution) measured using a laser diffraction particle size distribution analyzer (e.g., Submicron Particle Analyzer N5 PLUS (Beckman Coulter)).

[0028] The ratio of the content of the spherical copper particles (A2) to the content of the flaky copper particles (A1) in the composition (content of spherical copper particles (A2) / content of flaky copper particles (A1)) may be 0.25 to 4.0, 0.3 to 3.0, or 0.4 to 2.5. When the content of the spherical copper particles (A2) to the content of the flaky copper particles (A1) is within such a range, cracking tends to be further suppressed.

[0029] The content of the copper particles may be 20 to 80 parts by mass relative to 100 parts by mass of the total composition. The content of the copper particles may be 30 parts by mass or more, 40 parts by mass or more, or 50 parts by mass or more. When the content of the copper particles is 20 parts by mass or more relative to 100 parts by mass of the total composition, wiring having a sufficient thickness tends to be formed. The content of the copper particles may be 75 parts by mass or less, 70 parts by mass or less, or 65 parts by mass or less. When the content of the copper particles is 80 parts by mass or less relative to 100 parts by mass of the total composition, the dischargeability from the device tends to be better.

[0030] In one embodiment, the copper particles may be copper-containing particles having a core particle containing copper and an organic material that covers at least a part of the surface of the core particle. The copper-containing particles may have, for example, a core particle containing copper and an organic material containing a substance derived from an alkylamine present on at least a part of the surface of the core particle. The alkylamine may be an alkylamine having a hydrocarbon group with 7 or less carbon atoms. Since the chain length of the hydrocarbon group of the alkylamine constituting the organic material is relatively short, the copper-containing particles are thermally decomposed even at a relatively low temperature (for example, 150°C or less), and the core particles are easily fused together. As such copper-containing particles, for example, the copper-containing particles described in JP 2016-037627 A can be suitably used. Note that, from the viewpoint of achieving excellent conductivity, it is preferable that no organic material remains in the sintered body layer 3, and the content of the organic material in the sintered body layer 3 is preferably 3% by mass or less, more preferably 2% by mass or less, and even more preferably 1% by mass or less. According to the manufacturing method of this embodiment, even if the sintered body layer 3 does not contain a binder resin (organic substance), excellent adhesion of the sintered body layer 3 to the substrate 2 can be achieved.

[0031] The organic matter may contain an alkylamine having a hydrocarbon group with 7 or less carbon atoms. The alkylamine having a hydrocarbon group with 7 or less carbon atoms may be, for example, a primary amine, a secondary amine, an alkylenediamine, etc. Examples of the primary amine include ethylamine, 2-ethoxyethylamine, propylamine, 3-ethoxypropylamine, butylamine, 4-methoxybutylamine, isobutylamine, pentylamine, isopentylamine, hexylamine, cyclohexylamine, heptylamine, etc. Examples of the secondary amine include diethylamine, dipropylamine, dibutylamine, ethylpropylamine, ethylpentylamine, etc. Examples of the alkylenediamine include ethylenediamine, N,N-dimethylethylenediamine, N,N'-dimethylethylenediamine, N,N-diethylethylenediamine, N,N'-diethylethylenediamine, 1,3-propanediamine, 2,2-dimethyl-1,3-propanediamine, N,N-dimethyl-1,3-diaminopropane, N,N'-dimethyl-1,3-diaminopropane, N,N-diethyl-1,3-diaminopropane, 1,4-diaminobutane, 1,5-diamino-2-methylpentane, 1,6-diaminohexane, N,N'-dimethyl-1,6-diaminohexane, and 1,7-diaminoheptane.

[0032] The organic matter coating at least a portion of the surface of the core particle may contain an organic matter other than the alkylamine having a hydrocarbon group with a carbon number of 7 or less. The ratio of the alkylamine having a hydrocarbon group with a carbon number of 7 or less to the total organic matter is preferably 50% by mass or more, more preferably 60% by mass or more, and even more preferably 70% by mass or more.

[0033] The proportion of the organic material covering at least a part of the surface of the core particle is preferably 0.1 to 20% by mass based on the total of the core particle and the organic material. When the proportion of the organic material is 0.1% by mass or more, sufficient oxidation resistance tends to be obtained. When the proportion of the organic material is 20% by mass or less, it tends to be easier to achieve conductorization at low temperatures. The proportion of the organic material based on the total of the core particle and the organic material is more preferably 0.3 to 10% by mass, and even more preferably 0.5 to 5% by mass.

[0034] The copper-containing particles contain at least copper, and may contain other substances as necessary. Examples of other substances include metals such as gold, silver, platinum, tin, and nickel, or compounds containing these metal elements, reducing compounds or organic substances, oxides, chlorides, and the like. From the viewpoint of forming a conductor with excellent electrical conductivity, the copper content in the copper-containing particles is preferably 50% by mass or more, more preferably 60% by mass or more, and even more preferably 70% by mass or more. The method for producing the copper-containing particles is not particularly limited. Examples of the production method include the method for producing copper-containing particles disclosed in JP 2016-037626 A.

[0035] The dispersion medium is not particularly limited and can be appropriately selected from organic solvents generally used in the production of conductive inks, conductive pastes, etc. according to the application. The dispersion medium may be used alone or in combination of two or more. From the viewpoint of viscosity adjustment, the dispersion medium may be terpineol, isobornylcyclohexanol, dihydroterpineol, dihydroterpineol acetate, etc. The content of the dispersion medium may be 1 part by mass or more, 3 parts by mass or more, or 5 parts by mass or more, and 300 parts by mass or less, 200 parts by mass or less, or 150 parts by mass or less, relative to 100 parts by mass of copper particles.

[0036] The composition may further contain other components other than the copper particles and the dispersion medium as necessary. Examples of the other components include a silane coupling agent, a polymer compound (resin), a radical initiator, a reducing agent, and the like. Examples of the other components include metal particles other than copper particles. Examples of the other metal particles include nickel, silver, gold, palladium, platinum, and the like particles. From the viewpoint of obtaining sufficient bonding properties, the content of the other metal particles may be less than 20% by mass, and may be 10% by mass or less, based on the total mass of the metal particles contained in the composition. When the other metal particles are contained, the content of the dispersion medium set based on the content of the copper particles can be set based on the content of the copper particles and the metal particles.

[0037] The viscosity of the composition at 25°C can be appropriately set depending on the method of use of the composition, and may be, for example, 10 to 5000 mPa·s, 50 to 3000 mPa·s, 100 to 1500 mPa·s, or 200 to 1000 mPa·s. The viscosity of the composition at 25°C means the viscosity at 25°C measured using an E-type viscometer (manufactured by Toki Sangyo Co., Ltd., product name: VISCOMETER-TV22, applicable cone-plate rotor: 3°×R17.65).

[0038] The method for producing the composition is not particularly limited, and a method commonly used in the technical field can be used. For example, the composition can be prepared by dispersing copper particles, a dispersion medium, and other components as necessary. For the dispersion treatment, a media dispersing machine such as an Ishikawa type mixer, a planetary centrifugal mixer, an ultra-thin high-speed rotary dispersing machine, a roll mill, an ultrasonic dispersing machine, or a bead mill, a cavitation mixing machine such as a homomixer or a Silverson mixer, or a counter collision method such as an Ultemizer can be used. These methods may also be used in appropriate combination.

[0039] Prior to the step of forming the metal particle-containing layer, the surface of the substrate 2 may be subjected to a roughening treatment. This allows for better adhesion of the sintered body layer to the substrate 2. Examples of the roughening treatment method include laser irradiation, polishing, sandblasting, wet blasting, flame treatment, corona treatment, plasma treatment, and the like. Alternatively, the substrate 2 that has been roughened may be a substrate 2 molded using a mold having projections and recesses. The roughening treatment may be performed so that the surface roughness Ra of the substrate 2 is about 0.3 to 6.0 μm.

[0040] (Laser irradiation process) This step is a step of irradiating the metal particle-containing layer 3P with a laser so that the copper particles are sintered to form a copper sintered layer 3 (see FIG. 2(b)). At this time, a roughened portion 2a may be formed on the surface of the base material 2 that is in contact with the sintered layer 3. It is presumed that the roughened portion 2a is formed by heat caused by the laser irradiation, that is, direct heat by the laser irradiation and heat of the copper particles heated by the laser irradiation.

[0041] As the device, for example, a laser marker used for processing resin or ceramics can be used. As the laser, for example, a near-infrared laser (wavelength: 1064 nm), a visible light laser (wavelength: 532 nm), an ultraviolet laser (wavelength: 355 nm), etc. can be used.

[0042] Examples of parameters for laser irradiation include average laser power (W), frequency (Hz) and scan speed (mm / s). These parameters may be appropriately set according to the thickness of the metal particle-containing layer 3P, the shape (line or surface) of the sintered body layer 3 to be formed, and the material of the base material 2. For example, when a laser is irradiated under a predetermined condition toward the metal particle-containing layer 3P, if scorching occurs on the surface of the base material 2 that is the base of the metal particle-containing layer 3P, measures such as lowering the laser output, increasing the Q-switch frequency, and increasing the scan speed may be taken. According to the study by the present inventors, when the sintered body layer 3 is formed in a planar shape, it is preferable to increase the scan speed compared to when the sintered body layer 3 is formed in a linear shape.

[0043] Laser irradiation may be performed while moving the relative position of the laser irradiation with respect to the metal particle-containing layer 3P so that the sintered body layer 3 forms a pattern. Laser irradiation may be performed while spraying a reducing gas onto the region to be irradiated with the laser, or may be performed in an air atmosphere without spraying such a gas. In the examples described later, a sintered body layer 3 that shines copper-colored was formed simply by irradiating a laser onto the metal particle-containing layer 3P in an air atmosphere (in the atmosphere) (see FIG. 2(c) and FIG. 3(a)).

[0044] According to the manufacturing method of this embodiment, since a laser is used in the step of forming the sintered body layer 3, the sintered body layer 3 can be formed in a predetermined pattern even when one surface 2f of the substrate 2 has a three-dimensional shape. By forming the roughened portion 2a on the sintered body layer 3 and the surface of the substrate 2 in contact therewith by laser irradiation, excellent adhesion of the sintered body layer to the substrate 2 can be achieved without using a binder resin that reduces electrical conductivity.

[0045] The article 1 can be suitably used as an MID (also called a molded circuit component, a three-dimensional molded circuit component, a three-dimensional molded circuit component, etc.). Specifically, the article 1 can be suitably used as a smartphone antenna, an in-vehicle wiring, a laminate, a solar panel, a display, a transistor, a semiconductor package, a multilayer ceramic capacitor, etc. The article 1 can also be used as a member for electrical wiring, a heat dissipation film, a surface coating film, etc.

[0046] Although the embodiment of the present invention has been described, the present invention is not limited to the above embodiment. For example, in the above embodiment, the case where copper particles, which have the advantage of low material cost but are easily oxidized, are used as the metal particles is exemplified, but silver particles, silver-palladium particles, aluminum particles, or nickel particles may be used instead of the copper particles.

[0047] In the above embodiment, the case where the metal particle-containing layer 3P is formed as a so-called solid coating is exemplified, but the metal particle-containing layer 3P may be formed to have a pattern corresponding to the pattern of the sintered body layer 3. In this case, a non-contact printing method can be adopted for forming the metal particle-containing layer 3P. Specifically, a method using a jet dispenser, a method using an aerosol jet, a method using a piezo jet dispenser, etc. may be used, and from the viewpoint of being able to suitably print on a surface of the substrate 2 having a three-dimensional shape, the method using an aerosol jet is preferable.

[0048] <Composition for forming metal sintered layer> The composition used in the method for producing the above-mentioned article contains flake-shaped metal particles having a median diameter of 4.0 μm or more. Such a composition is useful for forming a sintered body layer on a substrate with suppressed cracks by sintering the metal particles by laser irradiation. Therefore, the above-mentioned composition can be said to be a composition for forming a metal sintered body layer by laser sintering. EXAMPLES

[0049] The present invention will be described in detail below based on examples, but the present invention is not limited to the following examples.

[0050] <Preparation of Composition> 46 parts by mass of copper particles (A) or copper particles (a) shown below and 54 parts by mass of organic solvent (B) shown below were mixed to prepare compositions for forming metal sintered layers in the examples and comparative examples. The median diameter (D50) of the copper particles was measured using a submicron particle analyzer N5 PLUS (Beckman Coulter).

[0051] (Copper particles (A)) As the copper particles (A), a mixture of flaky copper particles (A1) and spherical copper particles (A2) in a mass ratio of 30:70 (ratio of the content of spherical copper particles (A2) to the content of flaky copper particles (A1): 2.3) was used. Flake-shaped copper particles (A1): Product name: 3L3N, Fukuda Metal Foil and Powder Co., Ltd., Median diameter (D50): 5.0 μm Spherical copper particles (A2): Product name: CH0200, Mitsui Mining & Smelting Co., Ltd., Median diameter (D50): 0.15 μm

[0052] (Copper particles (a)) As the copper particles (a), a mixture of flaky copper particles (a1) and spherical copper particles (A2) in a mass ratio of 30:70 (ratio of the content of spherical copper particles (A2) to the content of flaky copper particles (a1): 2.3) was used. Flake-shaped copper particles (a1): Product name: 1050YF, Mitsui Mining & Smelting Co., Ltd., Median diameter (D50): 1.4 μm Spherical copper particles (A2): Product name: CH0200, Mitsui Mining & Smelting Co., Ltd., Median diameter (D50): 0.15 μm

[0053] (Organic solvent (B)) As the organic solvent, a mixture of 70 parts by mass of terpineol and 30 parts by mass of Tersolve MTPH (trade name, manufactured by Nippon Terpene Chemical Co., Ltd., isobornylcyclohexanol) was used.

[0054] (Step of forming metal particle-containing layer) Both sides of a polypropylene substrate (size: 40 mm x 25 mm) were masked with tape. This polypropylene substrate was placed on a flat stage, and the above composition was applied to its surface. The paste-like composition was left on the polypropylene substrate to the thickness of the tape. Then, a drying process was carried out at a temperature condition of 110°C for 60 minutes. As a result, a metal particle-containing layer having a thickness of about 20 μm was formed on the polypropylene substrate.

[0055] (Laser irradiation process) A laser was irradiated toward the metal particle-containing layer on the polypropylene substrate. A fiber laser processing machine (Gunyucut GT1300R, manufactured by Gunkyo Seisakusho Co., Ltd.) was used as the device. The laser was irradiated under the following conditions. Laser: Near infrared laser (wavelength: 1.07μm) Laser average power: 18W Frequency: 500Hz Scan speed: 500~4000mm / s Laser irradiation atmosphere: Air

[0056] <Various evaluations> (Exterior photo) 3(a) and 3(b) are photographs of the appearance of the metal sintered body layer formed using the compositions for forming the metal sintered body layer of the Example and Comparative Example, respectively. As shown in the figure, the cracking of the metal sintered body layer of the Example was suppressed compared to the Comparative Example. Even when the metal sintered body layer of the Example was scratched with a fingernail, the sintered body layer did not peel off.

[0057] (Conductivity evaluation) Conductivity evaluation was performed on the metal sintered body layer (wiring) formed using the composition for forming the metal sintered body layer of the embodiment. Specifically, the resistance value of the wiring at a length of 15 mm was measured using a tester. The wiring resistance of the embodiment was 3.2Ω, and it had excellent conductivity. [Explanation of symbols]

[0058] 1...Article, 2...Base material, 2a...Roughened portion, 2f...One side of base material, 3...Sintered body layer, 3P...Metal particle-containing layer.

Claims

1. forming a copper particle-containing layer on a surface of a substrate using a composition containing copper particles; and irradiating the copper particle-containing layer with a laser so that the copper particles are sintered to form a copper sintered layer. The copper particles include flaky copper particles having a median diameter of 4.0 to 20.0 μm and spherical copper particles having a median diameter of 0.1 to 0.6 μm, and the ratio of the content of the spherical copper particles to the content of the flaky copper particles (content of spherical copper particles / content of flaky copper particles) is 0.25 to 4.

0.

2. The method according to claim 1, wherein the sintered layer has a thickness of 5.0 to 60 μm.

3. The method according to claim 1 or 2, wherein the copper particle-containing layer is irradiated with a laser in an air atmosphere.

4. The method according to any one of claims 1 to 3, wherein the substrate is made of a resin.

5. The method according to claim 4, wherein the resin is polypropylene, polycarbonate, polyethylene terephthalate or liquid crystal plastic.

Citation Information

Patent Citations

  • Method for manufacturing board having electric circuit

    JP2003198100A

  • Wiring formation method

    JP2011014716A

  • Fine coated copper particles and method for producing the same

    JP2012072418A

  • Novel coated copper fine particle and production method thereof

    JP2014148732A

  • Method of manufacturing wiring board, wiring board and dispersion liquid for manufacturing wiring board

    JP2016039239A