Method for producing positive electrode active material for lithium ion secondary battery

A method for producing a positive electrode active material with a lithium metal composite oxide powder addresses the non-uniform conductivity and peeling issues by forming a lithium tungsten compound coating, resulting in improved conductivity and reduced resistance for better battery performance.

JP7567179B2Active Publication Date: 2024-10-16SUMITOMO METAL MINING CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2020044303
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-03-28
Filing Date
2020-03-13
Publication Date
2024-10-16
Estimated Expiration
2040-03-13

AI Technical Summary

Technical Problem

Conventional coated lithium-nickel composite oxide particles face issues with non-uniform conductivity and peeling of the tungsten-containing coating layer during the positive electrode composite paste manufacturing process, which affects battery performance.

Method used

A method for producing a positive electrode active material with a lithium metal composite oxide powder that involves mixing a base material powder with a tungsten-containing compound at controlled ratios and temperatures, followed by a heat treatment to form a lithium tungsten compound coating, ensuring uniform conductivity and adhesion.

Benefits of technology

The method results in a positive electrode active material with a coating layer that adheres well to the surface of the particles, enhancing conductivity and reducing resistance, thereby improving battery output and cycle characteristics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007567179000002
    Figure 0007567179000002
  • Figure 0007567179000003
    Figure 0007567179000003
  • Figure 0007567179000004
    Figure 0007567179000004
Patent Text Reader

Abstract

To provide a positive electrode active material for a lithium ion secondary battery, which is superior in adhesion of a coating layer and allows a uniform conductivity to be ensured, and which can be adapted to achieve a high output and a low resistance.SOLUTION: A positive electrode active material for a lithium ion secondary battery comprises particles of a coated lithium metal composite oxide represented by the following general formula (I): LidNi1-a-b-cCoaWbMcO2+α (where 0≤a≤0.35, 0<b≤0.30, 0≤c≤0.35, 0≤α≤0.15 and 0.95≤d≤1.15, and M is at least one element selected from a group consisting of Mn, Ca, V, Mg, Mo, Nb, Ti and Al). After putting 10 g of the coated lithium metal composite oxide particles in a transparent glass container 1 of 10 ml in capacity, setting a lid to close an upper opening of the container with a lid, shaking the container for 0.5 hour, removing the lid, and then, taking off the lid to discharge a content of the container by free fall with the upper opening set right downward, the absorbance of the transparent container 1 is 0.7 or below.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a positive electrode active material for a lithium ion secondary battery and a method for producing the same. [Background technology]

[0002] In recent years, with the widespread use of portable electronic devices such as smartphones, tablet terminals, digital cameras, and notebook computers, there has been an increasing demand for lithium-ion secondary batteries that have high energy density and can be made small and lightweight. In addition, from the viewpoint of protecting the global environment, attention has been focused on so-called eco-friendly vehicles, such as hybrid vehicles, plug-in hybrid vehicles, and electric vehicles, which emit less carbon dioxide, and there has been an increasing demand for high-output lithium-ion secondary batteries with excellent output characteristics and charge / discharge cycle characteristics as batteries for driving or auxiliary devices of these vehicles.

[0003] A lithium-ion secondary battery with the above characteristics is mainly composed of a positive electrode, a negative electrode, a separator, and an electrolyte, and among these, lithium is released and inserted into the active materials of the positive and negative electrodes during charging and discharging. Various types of materials have been proposed as active materials that allow for this release and insertion of lithium, and among them, layered or spinel-type lithium metal composite oxides can be used as positive electrode materials to obtain high voltages of 4V, and have already been put to practical use as positive electrode active materials for lithium-ion secondary batteries.

[0004] The main lithium metal composite oxides that have been proposed so far are lithium cobalt composite oxide (LiCoO2), which is relatively easy to synthesize, lithium nickel composite oxide (LiNiO2), which uses nickel, which is cheaper than cobalt, lithium manganese composite oxide (LiMn2O4), which uses manganese, and lithium nickel manganese cobalt composite oxide (LiNi 1 / 3 Mn 1 / 3 Co 1 / 3Among these, lithium-nickel composite oxides, such as lithium-nickel composite oxide containing nickel, lithium-nickel manganese-cobalt composite oxide, and lithium-nickel-cobalt-aluminum composite oxide in which part of the nickel is replaced with cobalt or aluminum, are attracting particular attention as materials that not only provide high capacity but also have excellent battery cycle characteristics, and research into these materials is currently ongoing with the aim of achieving even higher output and lower resistance.

[0005] Meanwhile, in the above-mentioned lithium metal composite oxide having a powdered form, the particle surface is coated in order to improve the battery characteristics. For example, Patent Document 1 discloses a technique in which a lithium nickel composite oxide powder is mixed with a lithium-free tungsten compound powder and the mixture is heat-treated to react the tungsten compound with the lithium hydroxide contained in the surface portion of each lithium nickel composite oxide particle, thereby forming a coating layer containing tungsten.

[0006] It is described that this promotes the movement of lithium ions, thereby reducing reaction resistance and improving output characteristics. It is also described that the lithium transition metal compound powder for use as a positive electrode material for lithium secondary batteries can be easily produced with high productivity, making it possible to produce it on an industrial scale. In addition, Patent Document 1 lists two types of tungsten compounds, Li2WO4 and Li4WO5, as compounds to be coated on the surface of lithium nickel composite oxide particles. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2017-134996 A Summary of the Invention [Problem to be solved by the invention]

[0008] As described above, in lithium-ion secondary batteries, as the applications expand to include on-board use in eco-friendly automobiles, etc., there is a demand for further improvement in the characteristics of the positive electrode material containing the positive electrode active material in order to improve battery performance such as further increasing output and decreasing resistance. However, in the conventional coated lithium-nickel composite oxide particles and the manufacturing method thereof disclosed in the above Patent Document 1, the tungsten-containing coating layer is formed with varying thickness on the surface of the base particle made of lithium-nickel composite oxide, and is easily peeled off during the positive electrode composite paste manufacturing process, etc., so that it is difficult to ensure uniform conductivity.

[0009] The present invention has been made in consideration of the problems associated with conventional coated lithium metal composite oxide particles as described above, and aims to provide a positive electrode active material for lithium ion secondary batteries, in which the coating layer has excellent adhesion to the surface of the lithium metal composite oxide particle as the base material, thereby ensuring uniform conductivity and enabling the need for higher output and lower resistance, and a method for producing the same. [Means for solving the problem]

[0010] In order to achieve the above-mentioned object, the inventors have conducted extensive research into the powder characteristics of lithium metal composite oxides used as positive electrode active materials for lithium ion secondary batteries, and the effects of these powder characteristics on battery characteristics such as positive electrode resistance. As a result, they have found that by placing a powdered positive electrode active material made of coated lithium metal composite oxide particles in a transparent container and shaking it for a predetermined period of time, and then discharging the contents and measuring the absorbance of the transparent container, it is possible to satisfactorily evaluate the adhesion (resistance to peeling) of the coating layer to the surface of the base particle, and therefore to provide a positive electrode active material with excellent battery performance such as positive electrode resistance at low cost and stably, thereby completing the present invention.

[0012] In addition, the method for producing a positive electrode active material for a lithium ion secondary battery according to the present invention comprises the steps of: d Ni 1-a-b-c Co a Wb M c O 2+α (provided that 0 ≦ a ≦ 0.35, 0 < b ≦ 0.30, 0 ≦ c ≦ 0.35, 0 ≦ α ≦ 0.15, 0.95 ≦ d ≦ 1.15, and M is at least one element selected from the group consisting of Mn, Ca, V, Mg, Mo, Nb, Ti, and Al), which consists of coated lithium metal composite oxide particles The carbonate content is less than 0.3% by mass. A method for producing a positive electrode active material, comprising a general formula (II): Li d Ni 1-a-c Co a M c O2 (where 0 ≦ a ≦ 0.35, 0 ≦ c ≦ 0.35, 0.95 ≦ d ≦ 1.15, and M is at least one element selected from the group consisting of Mn, Ca, V, Mg, W, Mo, Nb, Ti, and Al), a wet base material powder, and a tungsten-containing compound powder are blended so that the lithium / tungsten ratio, which is the ratio of the molar amount of lithium derived from excess lithium present in the base material powder to the molar amount of tungsten in the tungsten-containing compound powder, is 2 or more and 4 or less, and mixed at 50°C or lower in a mixing step, and the obtained mixture is Over 100℃ Heat-treated in a vacuum atmosphere at 250°C or lower to form a coating layer composed of a lithium tungsten compound on the surface of each particle of the base material powder Li 4 WO 5 Includes It is characterized by having a heat treatment step

Advantages of the Invention

[0013] According to the present invention, it is possible to provide a positive electrode active material for a lithium ion secondary battery in which a coating layer excellent in adhesion is formed on the surface of each particle of a base material powder composed of a lithium metal composite oxide

Brief Description of the Drawings

[0014] [Figure 1] It is a schematic perspective view of a transparent container used for evaluating the adhesion (difficulty of peeling) of the positive electrode active material according to an embodiment of the present invention, and shows vibration by a reciprocating motion A in the central axis direction and a rotational motion B having the central axis as a rotation axis [Diagram 2]1A and 1B are a perspective view and a longitudinal sectional view of a coin-type battery produced for evaluating a positive electrode active material according to an embodiment of the present invention. [Diagram 3] FIG. 1 is a schematic explanatory diagram of a measurement example relating to impedance evaluation of a battery and an equivalent circuit used in the analysis. [Figure 4] 1 is an SEM image of a cross section of the positive electrode active material produced in Example 1. [Diagram 5] 5 is a STEM HAADF image of the coating layer of the positive electrode active material in FIG. 4. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] Hereinafter, embodiments of the positive electrode active material for a lithium ion secondary battery and the manufacturing method thereof according to the present invention will be described in detail in the order of 1 to 4. Note that the present invention is not limited to the following embodiments, and various modifications and alternative examples can be included within the scope of the present invention. 1. Positive electrode active material for lithium-ion secondary batteries 2. Manufacturing method of positive electrode active material for lithium-ion secondary batteries 3. Lithium-ion secondary battery 4. Evaluation of 1 to 3

[0016] 1. Positive electrode active material for lithium-ion secondary batteries The positive electrode active material for a lithium ion secondary battery according to an embodiment of the present invention is represented by the general formula (I): Li d Ni 1-a-b-c Co a W b M c O 2+α(However, 0 ≦ a ≦ 0.35, 0 < b ≦ 0.30, 0 ≦ c ≦ 0.35, 0 ≦ α ≦ 0.15, 0.95 ≦ d ≦ 1.15, and M is at least one element selected from the group consisting of Mn, Ca, V, Mg, Mo, Nb, Ti, and Al), and is composed of coated lithium metal composite oxide particles. The coated lithium metal composite oxide particles are composed of primary particles, secondary particles formed by aggregation of the primary particles, or a mixture of these primary particles and secondary particles. Then, 10 g of the coated lithium metal composite oxide particles are placed in a glass cylindrical transparent container with a volume of 10 ml, covered with a lid at the upper opening, shaken for 0.5 hours, then the lid is removed, the upper opening is placed directly below, and after the contents are discharged by natural fall, the absorbance of the transparent container is 0.7 or less.

[0017] In the positive electrode active material for a lithium ion secondary battery according to an embodiment of the present invention, an evaluation target sample of coated lithium metal composite oxide particles sampled from a lot of the positive electrode active material is placed in a transparent container as described above, shaken under predetermined conditions, and then the contents in the transparent container are discharged and the absorbance of the transparent container is measured. Then, based on the absorbance threshold required to obtain a desired battery characteristic determined from the correlation between the absorbance obtained by performing shaking and absorbance measurement on each of a sample group of positive electrode active materials prepared under various conditions in advance under the same conditions as above, and the battery characteristics of lithium ion secondary batteries prepared using each of the sample group, the above evaluation target sample is evaluated.

[0018] Thereby, a positive electrode active material excellent in the adhesion of the coating layer to the surface of each particle of the base material powder composed of lithium metal composite oxide can be provided. That is, a positive electrode material using a positive electrode active material composed of coated lithium metal composite oxide particles evaluated to be below the threshold value obtained as described above can ensure uniform conductivity and can exhibit the effects of desired high output and low resistance.

[0019] As the lithium metal composite oxide which is the positive electrode active material for the lithium ion secondary battery described above, the general formula (II): Li d Ni 1-a-c Co a Mc A base powder is used which is made up of primary particles represented by the formula: O2 (where 0≦a≦0.35, 0≦c≦0.35, 0.95≦d≦1.15, and M is at least one element selected from the group consisting of Mn, Ca, V, Mg, W, Mo, Nb, Ti, and Al), secondary particles formed by agglomeration of the primary particles, or a mixture of these primary particles and secondary particles.The coating layer which coats the surface of each particle of the base powder is preferably made of a lithium tungsten compound.

[0020] The coating layer made of the lithium tungsten compound preferably contains Li4WO5, because Li4WO5 has higher lithium ion conductivity than other lithium tungsten compounds, and therefore, when Li4WO5 is contained in the coating layer that coats the surface of each particle of the base powder, the resistance reducing effect of the obtained positive electrode active material for lithium ion secondary batteries can be further enhanced.

[0021] 2. Manufacturing method of positive electrode active material for lithium-ion secondary batteries The positive electrode active material for lithium ion secondary batteries according to the present invention can be manufactured by carrying out two steps, a mixing step and a heat treatment step, in the order described below. By going through these two steps, the adhesion of the coating layer to the surface of each particle of the base powder is improved, so that the manufactured positive electrode active material has uniform conductivity with little variation, and the lithium ion secondary battery manufactured using this positive electrode active material can have high output and low resistance.

[0022] (1)Mixing process First, in the mixing step, a compound represented by the general formula (II): Li d Ni 1-a-c Co a M cA hydrate of a base material powder consisting of primary particles represented by 0≦a≦0.35, 0≦c≦0.35, 0.95≦d≦1.15, M is at least one element selected from the group consisting of Mn, Ca, V, Mg, W, Mo, Nb, Ti, and Al, secondary particles formed by agglomeration of the primary particles, or a mixture of the primary particles and secondary particles is prepared. A tungsten-containing compound powder is also prepared as a material for the coating layer. Then, the base material powder and the tungsten-containing compound powder are mixed at 50° C. or less. During this mixing, the compounding ratio is adjusted so that the “lithium / tungsten ratio”, which is the molar ratio of lithium derived from excess lithium present in the base material powder to tungsten in the tungsten-containing compound powder, is 2 to 4.

[0023] The surplus lithium generally exists as lithium hydroxide or lithium carbonate on the surface of each particle of the base powder. Thus, the lithium metal composite oxide powder having surplus lithium on the particle surface can be obtained by manufacturing it by a known manufacturing method. For example, it can be produced by crystallizing a metal salt solution containing the metal elements constituting the base powder to produce a nickel composite hydroxide, and then oxidizing and roasting the nickel composite hydroxide to obtain a nickel composite oxide, which is mixed with a lithium compound such as lithium hydroxide or lithium carbonate as a lithium raw material, and then calcining the mixture. Alternatively, a commercially available base powder may be used as long as it is made of primary particles represented by the above general formula (II) and / or secondary particles formed by agglomeration of the primary particles, and surplus lithium in the form of lithium hydroxide or lithium carbonate exists on the particle surface.

[0024] On the other hand, the powdered tungsten-containing compound used as the raw material for the coating layer is preferably a water-soluble tungsten compound such as tungsten oxide, tungstic acid, ammonium tungstate, sodium tungstate, or lithium tungstate, and it is particularly preferable to use tungsten trioxide (WO3) or tungstic acid monohydrate (WO3·H2O), which are less likely to be contaminated by impurities.

[0025] When adding the tungsten-containing compound powder to the base material powder as described above, it is preferable to add water to the base material powder to make it in a wet state and then add and mix the tungsten-containing compound. By this method, the tungsten-containing compound dissolves in the water contained in the wet base material powder, and tungsten can be efficiently dispersed on the surface of each particle of the base material powder. Further, if this mixing step is carried out at a temperature exceeding 50°C, the amount of moisture necessary for promoting the reaction between lithium derived from excess lithium and the tungsten-containing compound in the subsequent heat treatment step may not be obtained. Therefore, it is more preferable to carry out the mixing step at a temperature of 50°C or lower.

[0026] As the blending ratio of the above base material powder and tungsten-containing compound powder, it is blended so that the "lithium / tungsten ratio (Li / W)", which is the ratio of the molar amount Li of lithium derived from excess lithium present in the base material powder to the molar amount W of tungsten in the tungsten-containing compound powder, is 2 or more and 4 or less. Thereby, it is possible to suppress the loss of excess lithium from the base material powder, and it is possible to easily form a coating layer made of a lithium tungsten compound such as lithium tungstate, which has a high effect of promoting intercalation and deintercalation, which are phenomena in which lithium ions move. Further, the positive electrode active material for a lithium ion secondary battery according to the embodiment of the present invention is composed of coated lithium metal composite oxide particles represented by the general formula (I) as described above. In this general formula (I), the composition ratio b indicating the amount of substance (number of moles) of W with respect to a total of 1 mole of Ni, Co, W, and M is preferably 0 < b ≦ 0.30, more preferably 0.0001 ≦ b ≦ 0.30, and most preferably 0.00075 ≦ b ≦ 0.30. Therefore, the addition amount of the tungsten-containing compound powder is adjusted so as to be within the range of the above composition ratio.

[0027] In the method for manufacturing a positive electrode active material for a lithium ion secondary battery according to an embodiment of the present invention, in order to improve the quality of the positive electrode active material obtained after manufacturing, it is preferable to perform a water washing treatment on the base material powder before the above mixing step to remove impurities such as sulfate ions and chloride ions in advance. There is no particular limitation on the specific method of this water washing treatment. For example, known washing techniques and washing conditions such as a method of adding water in a predetermined ratio to the base material powder, stirring, and then performing solid-liquid separation using a solid-liquid separation device such as a filter press can be adopted. However, it is preferable to pay attention to this point because excessive washing may cause excessive elution of lithium from the base material powder and deterioration of battery characteristics.

[0028] For the mixing of the wet base material powder obtained by performing solid-liquid separation after water washing treatment on the base material powder as described above or simply adding water to the base material powder, and the tungsten-containing compound powder, a general mixer can be used. For example, it is preferable to use a shaker mixer, a Lodige mixer, a Julia mixer, a V blender, etc. At that time, it is preferable to mix sufficiently under conditions such that the morphology of each particle constituting the base material powder is not destroyed.

[0029] (2) Heat treatment step Next, in the heat treatment step, the mixture composed of the base material powder and the tungsten-containing compound obtained in the above mixing step is heat-treated. Thereby, a positive electrode active material composed of coated lithium metal composite oxide particles represented by the general formula (I): Li d Ni 1-a-b-c Co a W b M c O 2+α (where 0 ≦ a ≦ 0.35, 0 < b ≦ 0.30, 0 ≦ c ≦ 0.35, 0 ≦ α ≦ 0.15, 0.95 ≦ d ≦ 1.15, and M is at least one element selected from the group consisting of Mn, Ca, V, Mg, Mo, Nb, Ti, and Al) can be produced.

[0030] During this heat treatment process, the water content of the mixture evaporates, and the lithium from the excess lithium present on the surface of each particle of the base powder and the tungsten provided by the tungsten-containing compound form a coating layer made of a lithium-tungsten compound that has good adhesion to the surface of each particle of the base powder, thereby obtaining a positive electrode active material for lithium-ion secondary batteries that can ensure uniform conductivity and can be adapted to high output and low resistance.

[0031] The heat treatment step is preferably performed at an atmospheric temperature of 100 to 250°C in order to form a highly adhesive coating layer on the surface of each particle of the base powder. If the atmospheric temperature is less than 100°C, the evaporation rate of moisture is slow, and the coating layer may not be formed sufficiently. Conversely, if the atmospheric temperature exceeds 250°C, the evaporation rate of moisture is too fast, and the thickness and adhesion (difficulty of peeling) of the coating layer may vary. If the moisture content of the wet base powder before mixing in the mixing step is 1 mass% or more, it is more preferable to perform the heat treatment at an atmospheric temperature not exceeding 150°C in order to suppress the loss of lithium from the base powder.

[0032] In addition, in order to suppress carbonation of the coating layer by carbon dioxide, it is preferable to perform the heat treatment in an atmosphere containing almost no carbon dioxide gas, such as a decarbonated gas atmosphere or a vacuum atmosphere, and it is more preferable to perform the heat treatment in a vacuum atmosphere. This is because in an air atmosphere, the coating layer reacts with carbon dioxide in the air and is carbonated to produce carbonates such as lithium carbonate and sodium carbonate, which may cause a decrease in the strength and adhesion (difficulty in peeling) of the coating layer. The heat treatment time of this heat treatment step is preferably such that the maximum temperature in the temperature profile of the atmosphere in the heat treatment step is maintained for at least 0.5 hours so that the moisture in the base material powder on which the coating layer is formed is sufficiently evaporated.

[0033] 3. Lithium-ion secondary battery The lithium ion secondary battery in which the positive electrode active material according to the embodiment of the present invention is used is not particularly limited, and the positive electrode active material according to the embodiment of the present invention can be suitably used in known lithium ion secondary batteries. For example, the positive electrode active material may be used as a positive electrode material for a non-aqueous electrolyte secondary battery having a positive electrode, a negative electrode, a separator, and a non-aqueous electrolyte solution, or may be used as a positive electrode material for an all-solid-state battery having a positive electrode, a negative electrode, and a solid electrolyte.

[0034] 4. Evaluation of 1 to 3 (1) Composition The composition of the positive electrode active material made of the coated lithium metal composite oxide particles or the composition of the base material powder before coating can be quantitatively analyzed by thermally decomposing 1 g of the sample with an inorganic acid such as hydrochloric acid, nitric acid, or aqua regia, diluting the obtained analysis sample liquid with pure water as necessary, and then measuring it using, for example, a multi-type ICP optical emission spectrometer ICPE-9000 (manufactured by Shimadzu Corporation). The composition of the coating layer of the coated lithium metal composite oxide particles can be quantitatively analyzed by utilizing this property, since the lithium tungsten compound that forms the coating layer is easily soluble in water while the base material particles are almost insoluble in water. Specifically, 5 g of the sample is added to 100 ml of pure water and stirred, thereby dissolving only the coating layer contained in the sample in pure water. The slurry obtained after this dissolution is filtered to remove the solid content, and the analysis sample liquid obtained is diluted with pure water as necessary, and then quantitatively analyzed by measuring it with an ICP optical emission spectrometer in the same manner as above.

[0035] (2) Excess lithium (lithium hydroxide and lithium carbonate) The excess lithium is present on the surface of the base powder made of lithium metal composite oxide, and can be quantitatively analyzed by neutralization titration (sequential titration by RB Warder method). That is, the lithium hydroxide and lithium carbonate present on the surface of the sampled sample dissolve in water and ionize from the lithium ion in the form of hydroxide ion and carbonate ion, respectively. Therefore, the lithium hydroxide and lithium carbonate can be separately quantified by titrating these ionized anions with an inorganic acid or the like.

[0036] In the above titration, the first end point (pH: about 8.3) is the pH change when all of the lithium hydroxide reacts with half of the lithium carbonate, and the second end point (pH: about 3.8) is the pH change when the remaining half of the lithium carbonate reacts. The pH inflection point (end point) where the pH change occurs can be confirmed by visually determining the color change of an indicator such as phenolphthalein or methyl orange, or by automatically reading the change in potential difference by a pH composite electrode using an automatic titrator.

[0037] For example, 2 to 20 g of sample is mixed with 120 mL of pure water, and the solution is stirred while being potentiometrically titrated with 1 mol / L hydrochloric acid using an automatic titration device COMTITE-1750 (manufactured by Hiranuma Sangyo Co., Ltd.), and the two pH inflection points (end points) that appear are automatically read by a pH composite electrode. This allows the contents of lithium hydroxide and lithium carbonate in the sample to be determined, and from these contents, the total lithium content derived from the excess lithium present in the base powder, which is the basis for calculating the "lithium / tungsten ratio", which is the value obtained by dividing the molar amount of lithium in the mixing process described above by the molar amount of tungsten, can be determined.

[0038] (3) Adhesion (difficulty in peeling off) The positive electrode active material made of the coated lithium metal composite oxide particles according to the embodiment of the present invention has excellent adhesion (i.e., difficulty in peeling) of the coating layer to the surface of each particle of the base powder, so that the absorbance of the transparent container after discharging the contents after placing a sample of the coated lithium metal composite oxide particles in a transparent container and shaking it under predetermined conditions can be suppressed to a predetermined threshold value or less. That is, if the adhesion is low, the fine particles constituting the coating layer are easily peeled off by the above-mentioned shaking, and some of these peeled fine particles adhere to the inner wall of the transparent container, significantly reducing the transparency of the wall of the transparent container, so that the absorbance is high. Conversely, if the transparency of the wall of the transparent container is high and the absorbance is low, it can be evaluated that the adhesion (difficulty in peeling) of the coating layer to the surface of each particle of the base powder is better. In this way, the adhesion of the coating layer can be evaluated using the absorbance as an index.

[0039] Specifically, 10 g of the sample was placed in a cylindrical transparent container made of quartz glass (inner diameter 1 cm, length 12 cm, capacity 12 mL), and the top opening was covered with a lid, after which it was attached to a shaker mixer, TURBULA-Type-T2C (Willi & Bachofen). As shown in Fig. 1, the transparent container 1 was subjected to a reciprocating motion A (distance 220 cm, speed 154 cm / sec) in the direction of the central axis O and a unidirectional rotational motion B (speed 250° / sec) around the central axis as the rotation axis, which were continued simultaneously for 0.5 hours, thereby shaking the transparent container together with the sample contained therein.

[0040] After the 0.5 hour shaking is completed, the lid of the transparent container is removed and the upper opening is turned directly downward to allow the contents to drain by gravity. The absorption spectrum of the empty transparent container is scanned in the wavelength range of 380 to 780 nm using a spectrophotometer SE6000 (manufactured by Nippon Denshoku Industries Co., Ltd.). The absorbance ABS (ABS = -logT, T: transmittance (I / I0)) of the optimum wavelength (maximum absorption peak wavelength) obtained in this way is measured, and if the threshold value is 0.7 or less, it can be evaluated as having excellent adhesion (difficulty in peeling off). Note that I0 above is the intensity of incident light, and I above is the intensity of transmitted light.

[0041] (4) Compound identification The compound constituting the coating layer of the coated lithium metal composite oxide particles can be identified using an X-ray diffractometer (XRD) X'PertPRO (manufactured by Spectris Inc.). Specifically, a sample collected in a sample holder is measured using CuKα radiation as a radiation source under conditions of a measurement speed of 2° / min, a tube voltage of 45 kV, a tube current of 40 mA, and a measurement range of 2θ=10 to 80°. Then, the compound can be identified by comparing the standard diffraction pattern of the compound with the diffraction pattern of the sample using the PDF (Powder Diffraction File) database in the ICDD (International Centre for Diffraction Data).

[0042] (5) Average particle size MV, particle size distribution and average coating layer thickness The positive electrode active material made of the coated lithium metal composite oxide particles and the base powder before coating preferably have an index of particle size distribution [(d90-d10) / average particle size MV] of 1.0 or less, which improves the packing property of the positive electrode active material and the battery capacity per battery volume, uniforms the applied voltage between the secondary particles constituting the positive electrode active material, and uniforms the load between the secondary particles to improve the cycle characteristics.

[0043] In the index [(d90-d10) / average particle diameter MV] indicating the spread of the particle size distribution, d10 means a particle diameter at which the number of particles of each particle diameter of the powder or granular material to be measured is accumulated from the smallest particle diameter side, and the accumulated volume is 10% of the total volume of all particles. On the other hand, d90 means a particle diameter at which the number of particles of the powder or granular material to be measured is accumulated, and the accumulated volume is 90% of the total volume of all particles, similar to d10. Also, the average particle diameter MV is an average volume particle diameter. In the positive electrode active material for lithium ion secondary batteries according to the embodiment of the present invention, the base powder made of lithium metal composite oxide before coating preferably has an average particle diameter MV of about 3 to 20 μm.

[0044] The above d10, d90, and average particle diameter MV, as well as the particle size distribution index determined from these, [(d90-d10) / average particle diameter MV], can be determined, for example, from a volume-based distribution measured using a laser diffraction / scattering particle size distribution measuring device, Microtrac MT3300EXII (manufactured by Microtrac Bell Co., Ltd.) Note that, as with d10 and d90, the median diameter d50, at which the cumulative volume is 50% of the total particle volume, may be used instead of the average particle diameter MV as the index of the above particle size distribution.

[0045] In addition, the positive electrode active material made of the coated lithium metal composite oxide particles preferably has an average thickness of 0.001 to 0.2 μm for the coating layer made of the lithium tungsten compound. The average thickness of the coating layer is determined by measuring the thicknesses of the coating layer at four points where two straight lines intersect at right angles at the center of each of 10 arbitrarily selected particles in the image of the cross section of the coated lithium metal composite oxide particle group embedded in resin, which is produced by a cross-section polisher (IB-19530CP), a cross-section sample preparation device manufactured by JEOL Ltd., using a scanning transmission electron microscope STEM (HD-2300A manufactured by Hitachi High-Technologies Corporation), and calculating the arithmetic mean of the thicknesses of the coating layer at a total of 40 points.

[0046] (6) Tap density The tap density of the positive electrode active material made of the coated lithium metal composite oxide particles and the base material powder before coating is 1.0 to 3.0 g / cm 3 This makes it possible to reduce voids when an electrode for a lithium ion secondary battery is produced, and also to increase the contact area of ​​the positive electrode active material with the electrolytic solution or solid electrolyte, thereby improving the battery performance.

[0047] This tap density can be measured by the following method. That is, 12 g of the sample is put into a 20 ml measuring cylinder, and the measuring cylinder is attached to a shaking specific gravity measuring instrument KRS-409 (manufactured by Kuramochi Scientific Instruments Manufacturing Co., Ltd.), and then the measuring cylinder is allowed to freely fall from a height of 2 cm 500 times. This makes it possible to determine the tap density, which is the density of a powder in a densely packed state.

[0048] (7) Specific surface area The specific surface area of ​​the positive electrode active material made of the coated lithium metal composite oxide particles and the base material powder before coating is 0.15 to 7.0 m 2 The base powder before coating and after washing with water preferably has a specific surface area of ​​0.5 m 2 / g or more. This ensures a sufficient contact area of ​​the positive electrode active material with the electrolyte or solid electrolyte, just as in the case of having the desired tap density. 2 If the specific surface area is less than 7.0 m / g, the contact area becomes too small and sufficient charge / discharge capacity may not be obtained. 2 If it exceeds 1 / g, the contact area becomes too large, and the surface activity may become too high.

[0049] The specific surface area can be measured by the nitrogen gas adsorption-desorption method using the BET multipoint method or the BET single point method. For example, the specific surface area can be obtained by taking 1 g of the sample in a U-shaped BET glass cell, mounting the U-shaped BET glass cell on a specific surface area measuring device, the Maxsorb 1200 series (manufactured by Mountec Co., Ltd.), and measuring it using the nitrogen gas adsorption-desorption method using the BET single point method.

[0050] (8) Carbonate The carbonate radicals (CO3 2-) is preferably less than 0.3 mass% based on the total amount of the positive electrode active material. This can further improve the strength and adhesion (difficulty in peeling) of the coating layer. This positive electrode active material having less than 0.3 mass% of carbonate radicals can be produced by performing heat treatment in an atmosphere containing almost no carbon dioxide gas in the heat treatment step as described above, since carbonation of the coating layer by carbon dioxide can be suppressed.

[0051] The carbonate radicals can be measured by ion chromatography. The compounds containing the carbonate radicals are easily soluble in water, and this property can be utilized for quantitative analysis. Specifically, 5 g of the sample is added to 100 ml of pure water and stirred, thereby dissolving the carbonate radicals contained in the sample in the pure water. The slurry obtained after the dissolution is filtered to remove solids to obtain an analytical specimen liquid, which can be diluted with pure water as necessary and then quantitatively analyzed by, for example, measuring with an ion chromatography analyzer ICS-2100 (manufactured by Thermo Fisher Scientific Co., Ltd.).

[0052] (9) Battery evaluation The positive electrode active material made of the coated lithium metal composite oxide according to the embodiment of the present invention described above can be used as a positive electrode material for a 2032-type coin battery 1 (hereinafter also referred to as a coin battery) shown in Fig. 2, which is one form of a lithium-ion secondary battery, and its battery performance can be evaluated. That is, the coin battery 1 shown in Fig. 2 is composed of a case 2 and an electrode 3 housed in this case 2.

[0053] The case 2 is constructed by fitting together a cylindrical positive electrode can 2a with an open top end and another cylindrical positive electrode can 2b with an open bottom end and an outer diameter slightly smaller than the positive electrode can 2a, with their open sides facing each other. An electrode 3 is housed inside the space formed by the positive electrode can 2a and the negative electrode can 2b. The electrode 3 has a structure in which a positive electrode 3a, a separator 3c, and a negative electrode 3b are layered in this order from bottom to top, with the positive electrode 3a in contact with the inner surface of the positive electrode can 2a and the negative electrode 3b in contact with the inner surface of the negative electrode can 2b.

[0054] A gasket 2c is provided on the periphery of both the positive electrode can 2a and the negative electrode can 2b to keep them out of contact with each other. The gasket 2c fixes the positive electrode can 2a and the negative electrode can 2b so that they do not move relative to each other. The gasket 2c also seals the gap between the positive electrode can 2a and the negative electrode can 2b, isolating the inside of the case 2 from the outside in an airtight and liquid-tight manner.

[0055] The coin-type battery 1 can be fabricated as follows. First, 52.5 mg of the coated lithium metal composite oxide powder according to the embodiment of the present invention, 15 mg of acetylene black, and 7.5 mg of polytetrafluoroethylene resin (PTFE) are mixed and pressed under a pressure of 100 MPa to fabricate a disk-shaped positive electrode 3a having a diameter of 11 mm and a thickness of 100 μm. The resulting positive electrode 3a is placed in a vacuum dryer and dried at an atmospheric temperature of 120° C. for 12 hours.

[0056] A negative electrode sheet was prepared as the negative electrode 3b, in which graphite powder with an average particle size of about 20 μm and polyvinylidene fluoride were applied to one side of a copper foil punched into a disk shape with a diameter of 14 mm, and a polyethylene porous film with a thickness of 25 μm was prepared as the separator 3c. Furthermore, a mixture of equal amounts of ethylene carbonate (EC) and diethyl carbonate (DEC) with 1M LiClO4 as the supporting electrolyte (manufactured by Toyama Pharmaceutical Co., Ltd.) was prepared as the electrolyte.

[0057] The coin-type battery 1 is assembled using the positive electrode 3a, negative electrode 3b, separator 3c, and electrolyte in a glove box in an argon gas atmosphere controlled at a dew point of -80°C. The battery performance of the coin-type battery 1 thus fabricated can be evaluated by measuring the positive electrode resistance by the following method. That is, the coin-type battery 1 is charged at a charging potential of 4.1 V, and the resistance is measured by an AC impedance method using a frequency response analyzer and a potentiogalvanostat 1255B (manufactured by Solartron, UK).

[0058] This results in the Nyquist plot shown in Figure 3. This Nyquist plot is expressed as the sum of characteristic curves showing the solution resistance, the negative electrode resistance and its capacity, and the positive electrode resistance and its capacity, so that the value of the positive electrode resistance can be obtained by performing fitting calculations using an equivalent circuit based on this Nyquist plot. Next, the present invention will be described with reference to examples, but the present invention is not limited to the following examples. EXAMPLES

[0059] [Example 1] The composition is Li 1.02 Ni 0.82 Co 0.15 Al 0.03 O2, mean particle size MV is 11.8 μm, the particle size distribution is broad [(d90-d10) / mean particle size] is 0.91, and the tap density is 2.6 g / cm 3 , specific surface area is 0.35m 2 Powdered base material particles represented by the mass ratio of 1.0 to 1.0 were prepared. 1250 g of these base material particles were mixed with 1 L of water to prepare a slurry, which was then washed with water by stirring. The slurry was then filtered to obtain a hydrated base material powder. 10 g of this hydrated base material powder in a wet state was collected, dried, and the moisture content was measured, which was 6.8% by mass. The amount of lithium derived from the surplus lithium was measured using the dried product obtained, which was 0.54% by mass.

[0060] Based on the above measurement results, 55.5g (44.0g in terms of tungsten equivalent) of tungsten trioxide (WO3) was added as a tungsten raw material to 1000g of the hydrated base powder (including 5.4g of lithium derived from surplus lithium), and the "lithium / tungsten ratio", which is the ratio of the molar amount of lithium derived from surplus lithium to the molar amount of tungsten, was adjusted to 3. The mixture was then charged into a mixer and mixed for 3 hours while keeping the internal atmosphere temperature at 30°C. The resulting mixture (also called tungsten mixture) was charged into a vacuum dryer and heat-treated for 10 hours while keeping the internal atmosphere temperature at 100°C. After that, some of the aggregates contained in the powder after the heat treatment were deflocculated by a deflocculator. As a result, a positive electrode active material consisting of a coated lithium metal composite oxide powder for lithium ion secondary batteries was obtained.

[0061] The coated lithium metal composite oxide powder was used as a positive electrode active material to evaluate the adhesion (difficulty of peeling) of the coating layer according to the above-mentioned (3) Adhesion, and the compound species forming the coating layer were identified according to the above-mentioned (4) Compound Identification, and the carbonate content was measured according to the above-mentioned (8). Furthermore, a coin-type battery was produced using the coated lithium metal composite oxide powder as a positive electrode active material according to the above-mentioned (9) Battery Evaluation, and the positive electrode resistance and discharge capacity retention rate were evaluated. As a result, the absorbance, which is an index of the adhesion (difficulty of peeling) of the coating layer, was "0.166", the carbonate content was "0.16 mass%, "Li2WO4" and "Li4WO5" were identified as the compounds forming the coating layer, the positive electrode resistance was "0.58" (value when the positive electrode resistance value of Comparative Example 9 described later is 1.00), and the discharge capacity retention rate was "81%".

[0062] [Example 2] A positive electrode active material was prepared from a coated lithium metal composite oxide powder under the same conditions as in Example 1, except that the atmospheric temperature during mixing of the wet base material powder and the tungsten-containing compound was 35°C and the heat treatment temperature of the mixture was 150°C, and this was evaluated in the same manner as in Example 1. As a result, the absorbance, which is an index of the adhesion (difficulty of peeling off) of the coating layer, was "0.042", the carbonate content was "0.14 mass%, "Li2WO4" and "Li4WO5" were identified as the compounds forming the coating layer, the positive electrode resistance was "0.45" (value when the positive electrode resistance value of Comparative Example 9 described later is 1.00), and the discharge capacity retention rate was "87%".

[0063] [Example 3] A positive electrode active material was prepared from a coated lithium metal composite oxide powder under the same conditions as in Example 1, except that the atmospheric temperature during mixing of the wet base material powder and the tungsten-containing compound was 40°C, and the heat treatment temperature of the mixture was 180°C, and this was evaluated in the same manner as in Example 1. As a result, the absorbance, which is an index of the adhesion (difficulty of peeling off) of the coating layer, was "0.098", the carbonate content was "0.11 mass%, "Li2WO4" and "Li4WO5" were identified as the compounds forming the coating layer, the positive electrode resistance was "0.52" (value when the positive electrode resistance value of Comparative Example 9 described later is 1.00), and the discharge capacity retention rate was "83%".

[0064] [Example 4] A positive electrode active material was prepared from a coated lithium metal composite oxide powder under the same conditions as in Example 1, except that the atmospheric temperature during mixing of the wet base material powder and the tungsten-containing compound was 45°C and the heat treatment temperature of the mixture was 200°C, and this was evaluated in the same manner as in Example 1. As a result, the absorbance, which is an index of the adhesion (difficulty of peeling off) of the coating layer, was "0.311", the carbonate content was "0.18 mass%, "Li2WO4" and "Li4WO5" were identified as the compounds forming the coating layer, the positive electrode resistance was "0.64" (value when the positive electrode resistance value of Comparative Example 9 described later is 1.00), and the discharge capacity retention rate was "76%".

[0065] [Example 5] A positive electrode active material was prepared from a coated lithium metal composite oxide powder under the same conditions as in Example 1, except that the atmospheric temperature during mixing of the wet base material powder and the tungsten-containing compound was 50°C, and the heat treatment temperature of the mixture was 250°C, and this was evaluated in the same manner as in Example 1. As a result, the absorbance, which is an index of the adhesion (difficulty of peeling off) of the coating layer, was "0.685", the carbonate content was "0.17 mass%, "Li2WO4" and "Li4WO5" were identified as the compounds forming the coating layer, the positive electrode resistance was "0.69" (value when the positive electrode resistance value of Comparative Example 9 described later is 1.00), and the discharge capacity retention rate was "72%".

[0066] [Example 6] A positive electrode active material was prepared from a coated lithium metal composite oxide powder under the same conditions as in Example 1, except that the atmospheric temperature during mixing of the wet base powder and the tungsten-containing compound was 40°C, the ratio of the molar amount of lithium derived from excess lithium to the molar amount of tungsten was adjusted to 2, and the heat treatment temperature of the mixture was 180°C. The positive electrode active material was evaluated in the same manner as in Example 1. As a result, the absorbance, which is an index of the adhesion (difficulty of peeling) of the coating layer, was "0.124", the carbonate content was "0.12 mass%, "Li2WO4" and "Li4WO5" were identified as the compounds forming the coating layer, the positive electrode resistance was "0.55" (the value when the positive electrode resistance value of Comparative Example 9 described later is 1.00), and the discharge capacity retention rate was "82%".

[0067] [Example 7] A positive electrode active material was prepared from a coated lithium metal composite oxide powder under the same conditions as in Example 1, except that the atmospheric temperature during mixing of the wet base powder and the tungsten-containing compound was 40°C, the ratio of the molar amount of lithium derived from excess lithium to the molar amount of tungsten was adjusted to 4, and the heat treatment temperature of the mixture was 180°C. The positive electrode active material was evaluated in the same manner as in Example 1. As a result, the absorbance, which is an index of the adhesion (difficulty of peeling) of the coating layer, was "0.117", the carbonate content was "0.20 mass%, "Li2WO4" and "Li4WO5" were identified as the compounds forming the coating layer, the positive electrode resistance was "0.55" (value when the positive electrode resistance value of Comparative Example 9 described later is 1.00), and the discharge capacity retention rate was "82%".

[0068] [Comparative Example 1] The atmosphere temperature during mixing of the wet base powder and the tungsten-containing compound was adjusted to 60°C, the ratio of the molar amount of lithium derived from excess lithium to the molar amount of tungsten was adjusted to 1, and the mixture was heat-treated at an atmosphere temperature of 280°C using a normal dryer (air atmosphere). Except for this, a positive electrode active material consisting of a coated lithium metal composite oxide powder was produced under the same conditions as in Example 1, and was evaluated in the same manner as in Example 1. As a result, the absorbance, which is an index of the adhesion (difficulty of peeling) of the coating layer, was "0.773", the carbonate content was "0.45 mass%, "Li2WO4", "WO3", and "Li2CO3" were identified as compounds forming the coating layer, the positive electrode resistance was "0.91" (value when the positive electrode resistance value of Comparative Example 9 described later is 1.00), and the discharge capacity retention rate was "65%".

[0069] [Comparative Example 2] A positive electrode active material was prepared from a coated lithium metal composite oxide powder under the same conditions as in Example 1, except that the atmospheric temperature during mixing of the wet base powder and the tungsten-containing compound was 60°C, and the mixture was heat-treated at an atmospheric temperature of 280°C using a normal dryer (air atmosphere), and this was evaluated in the same manner as in Example 1. As a result, the absorbance, which is an index of the adhesion (difficulty in peeling off) of the coating layer, was "0.750", the carbonate content was "0.65 mass%, "Li2WO4" and "Li2CO3" were identified as the compounds forming the coating layer, the positive electrode resistance was "0.87" (value when the positive electrode resistance value of Comparative Example 9 described later is 1.00), and the discharge capacity retention rate was "67%".

[0070] [Comparative Example 3] The atmosphere temperature during mixing of the wet base powder and the tungsten-containing compound was adjusted to 60°C, the ratio of the molar amount of lithium derived from excess lithium to the molar amount of tungsten was adjusted to 5, and the mixture was heat-treated at an atmosphere temperature of 280°C using a normal dryer (air atmosphere). Except for this, a positive electrode active material made of lithium metal composite oxide powder was produced under the same conditions as in Example 1, and was evaluated in the same manner as in Example 1. As a result, the absorbance, which is an index of the adhesion (difficulty of peeling off) of the coating layer, was "0.849", the carbonate content was "0.82 mass%, "Li2WO4", "LiOH", and "Li2CO3" were identified as compounds forming the coating layer, the positive electrode resistance was "0.96" (value when the positive electrode resistance value of Comparative Example 9 described later is 1.00), and the discharge capacity retention rate was "61%".

[0071] [Comparative Example 4] The atmosphere temperature during mixing of the wet base powder and the tungsten-containing compound was adjusted to 60°C, the ratio of the molar amount of lithium derived from excess lithium to the molar amount of tungsten was adjusted to 1, and the mixture was heat-treated at an atmosphere temperature of 80°C using a normal dryer (air atmosphere). Except for this, a positive electrode active material consisting of a coated lithium metal composite oxide powder was produced under the same conditions as in Example 1, and was evaluated in the same manner as in Example 1. As a result, the absorbance, which is an index of the adhesion (difficulty of peeling) of the coating layer, was "0.805", the carbonate content was "0.49 mass%, "Li2WO4", "WO3", and "Li2CO3" were identified as compounds forming the coating layer, the positive electrode resistance was "0.94" (value when the positive electrode resistance value of Comparative Example 9 described later is 1.00), and the discharge capacity retention rate was "63%".

[0072] [Comparative Example 5] A positive electrode active material consisting of a coated lithium metal composite oxide powder was prepared under the same conditions as in Example 1, except that the atmospheric temperature during mixing of the wet base powder and the tungsten-containing compound was 60°C, and the mixture was heat-treated at an atmospheric temperature of 80°C using a normal dryer (air atmosphere), and was evaluated in the same manner as in Example 1. As a result, the absorbance, which is an index of the adhesion (difficulty in peeling off) of the coating layer, was "0.786", the carbonate content was "0.50 mass%, "Li2WO4" and "Li2CO3" were identified as the compounds forming the coating layer, the positive electrode resistance was "0.92" (value when the positive electrode resistance value of Comparative Example 9 described later is 1.00), and the discharge capacity retention rate was "64%".

[0073] [Comparative Example 6] The atmosphere temperature during mixing of the wet base powder and the tungsten-containing compound was adjusted to 60°C, the ratio of the molar amount of lithium derived from excess lithium to the molar amount of tungsten was adjusted to 5, and the mixture was heat-treated at an atmosphere temperature of 80°C using a normal dryer (air atmosphere). Except for this, a positive electrode active material made of lithium metal composite oxide powder was produced under the same conditions as in Example 1, and was evaluated in the same manner as in Example 1. As a result, the absorbance, which is an index of the adhesion (difficulty of peeling off) of the coating layer, was "0.862", the carbonate content was "0.90 mass%, "Li2WO4", "LiOH", and "Li2CO3" were identified as compounds forming the coating layer, the positive electrode resistance was "0.98" (value when the positive electrode resistance value of Comparative Example 9 described later is 1.00), and the discharge capacity retention rate was "59%".

[0074] [Comparative Example 7] A positive electrode active material was prepared from a coated lithium metal composite oxide powder under the same conditions as in Example 1, except that the temperature of the atmosphere when mixing the wet base powder and the tungsten-containing compound was 40°C, and the heat treatment was performed at a temperature of 280°C in the vacuum dryer, and this was evaluated in the same manner as in Example 1. As a result, the absorbance, which is an index of the adhesion (difficulty of peeling off) of the coating layer, was "0.711", the carbonate content was "0.21 mass%, only "Li2WO4" was identified as the compound forming the coating layer, the positive electrode resistance was "0.75" (value when the positive electrode resistance value of Comparative Example 9 described later is 1.00), and the discharge capacity retention rate was "69%".

[0075] [Comparative Example 8] A positive electrode active material was prepared from a coated lithium metal composite oxide powder under the same conditions as in Example 1, except that the atmospheric temperature during mixing of the wet base powder and the tungsten-containing compound was 40°C, and the mixture was heat-treated at an atmospheric temperature of 280°C using a normal dryer (air atmosphere), and this was evaluated in the same manner as in Example 1. As a result, the absorbance, which is an index of the adhesion (difficulty in peeling off) of the coating layer, was "0.738", the carbonate content was "0.54 mass%, "Li2WO4" and "Li2CO3" were identified as the compounds forming the coating layer, the positive electrode resistance was "0.84" (value when the positive electrode resistance value of Comparative Example 9 described later is 1.00), and the discharge capacity retention rate was "67%".

[0076] [Comparative Example 9] The base material powder was used as it was without forming a coating layer on it to evaluate the absorbance as a blank test in other examples and comparative examples, and the positive electrode resistance and discharge capacity retention rate were evaluated using a coin-type battery fabricated using the base material powder as the positive electrode active material. As a result, it was found that the absorbance in the blank test was only "0.005", which is not a value that would affect other examples and comparative examples. In addition, the carbonate content was "0.40 mass %, the positive electrode resistance was "1.00", and the discharge capacity retention rate was "56%".

[0077] The results of the above-mentioned Examples 1 to 7 and Comparative Examples 1 to 9 are summarized in Table 1 below. FIG. 4 shows an SEM image of the cross section of the positive electrode active material prepared in Example 1. This SEM image was taken using an SEM (FE-SEM: JSM-6360LA, manufactured by JEOL Ltd.) after embedding a part of the positive electrode active material in a resin and processing it with a cross-section polisher (IB-19530CP, manufactured by JEOL Ltd.) to make the cross section observable. Furthermore, FIG. 5 shows a HAADF image of a STEM of the coating layer part of the cross section of the positive electrode active material used for the image of FIG. 4. This HAADF image was taken using a scanning transmission electron microscope STEM (HD-2300A, manufactured by Hitachi High-Technologies Corporation), and the direction of the black area is the front side.

[0078] [Table 1]

[0079] [comprehensive evaluation] As shown in Table 1 above, the lithium metal composite oxides obtained in each Example all had an absorbance of 0.7 or less, which is an index of the adhesion (difficulty of peeling) of the coating layer, and all had a carbonate content of less than 0.3 mass%, and "Li2WO4" and "Li4WO5" were identified as compounds forming the coating layer. From these results, it was found that in each Example, a lithium metal composite oxide was obtained in which the coating layer had excellent adhesion to the surface of the base powder, and the coating layer contained Li4WO5, which has a higher lithium ion conductivity than other lithium tungsten compounds. Therefore, the positive electrode resistance of the lithium ion secondary battery prepared using the lithium metal composite oxide of each Example as the positive electrode active material was all 0.70 or less, and the discharge capacity retention rate was all 70% or more, which confirmed the extremely excellent effect.

[0080] In contrast, the lithium metal composite oxides obtained in Comparative Examples 1 to 8 all had an absorbance, which is an index of the adhesion (difficulty in peeling off) of the coating layer, exceeding 0.7, and the carbonate content exceeded 0.3 mass% except for Comparative Example 7, in which a vacuum dryer was used, and the coating layer did not contain Li4WO5, so it was found that they had inferior battery characteristics, along with the lithium metal composite oxide of Comparative Example 9, which did not have a coating layer. This is thought to be because carbonate groups were generated in the coating layer by carbonation due to heat treatment in the air atmosphere, resulting in a high carbonate group content in the positive electrode active material. [Explanation of symbols]

[0081] 1 transparent container 1 coin cell battery 2 Cases 2a Positive electrode can 2b Negative electrode can 2c Gasket 3 electrodes 3a positive electrode 3b negative electrode 3c Separator

Claims

1. General formula (I): Li d Ni 1-a-b-c Co a W b M c O 2+α (wherein 0≦a≦0.35, 0<b≦0.30, 0≦c≦0.35, 0≦α≦0.15, 0.95≦d≦1.15, and M is at least one element selected from the group consisting of Mn, Ca, V, Mg, Mo, Nb, Ti, and Al), and the positive electrode active material has a carbonate group content of less than 0.3 mass%, General formula (II): Li d Ni 1-a-c Co a M c O 2 a mixing step of blending a wet base material powder represented by the formula (wherein 0≦a≦0.35, 0≦c≦0.35, 0.95≦d≦1.15, and M is at least one element selected from the group consisting of Mn, Ca, V, Mg, W, Mo, Nb, Ti, and Al) with a tungsten-containing compound powder at a temperature of 50° C. or less, such that a lithium / tungsten ratio, which is the ratio of the molar amount of lithium derived from excess lithium present in the base material powder to the molar amount of tungsten in the tungsten-containing compound powder, is 2 or more and 4 or less; The mixture thus obtained is heat-treated in a vacuum atmosphere at 100° C. or higher and 250° C. or lower to form a matrix powder having Li on the surface of each particle. 4 WO 5 and forming a coating layer made of a lithium tungsten compound containing the lithium tungsten compound.

2. 2. The method for producing a positive electrode active material for a lithium ion secondary battery according to claim 1, wherein the tungsten-containing compound is at least one selected from the group consisting of tungsten oxide, tungstic acid, ammonium tungstate, sodium tungstate, and lithium tungstate.

Citation Information

Patent Citations

  • Positive electrode active material for nonaqueous electrolyte secondary batteries, manufacturing method thereof, and nonaqueous electrolyte secondary battery arranged by use of positive electrode active material

    JP2015216105A

  • Positive electrode active material for nonaqueous electrolyte secondary battery, manufacturing method thereof, and nonaqueous electrolyte secondary battery arranged by use of positive electrode active material

    JP2016127004A

  • Positive electrode active material for nonaqueous electrolyte secondary battery and method of producing the same, and nonaqueous electrolyte secondary battery including the positive electrode active material

    JP2017134996A

  • Nonaqueous-electrolyte secondary battery

    WO2015129188A1