Method for manufacturing silicon carbide single crystal substrate
By employing controlled dopant concentrations and growth conditions in chemical vapor deposition, the method addresses warping issues in SiC single crystal substrates, ensuring stable bonding and enhanced manufacturing efficiency.
Patent Information
- Application Number
- JP2020093064
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-05-28
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2040-05-28
AI Technical Summary
The challenge of warping in SiC single crystal substrates during epitaxial growth, which hinders transportation and bonding with SiC polycrystalline substrates, leading to reduced manufacturing yield.
A method involving chemical vapor deposition to grow SiC single crystal films with controlled dopant concentrations and adjusted supply ratios, pressures, and rotation speeds to balance stress and reduce warpage by alternating dopant concentrations between first and second films.
The method effectively suppresses warpage in SiC single crystal substrates, enabling stable bonding with SiC polycrystalline substrates and improving manufacturing yield.
Smart Images

Figure 0007567210000002 
Figure 0007567210000003 
Figure 0007567210000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for manufacturing a silicon carbide single crystal substrate comprising a silicon carbide single crystal film-growing substrate and a silicon carbide single crystal film epitaxially grown on a surface of the silicon carbide single crystal film-growing substrate, and in particular to an improvement in the manufacturing method for suppressing warping of the silicon carbide single crystal substrate. [Background technology]
[0002] Silicon carbide (hereafter abbreviated as SiC) is a compound semiconductor material composed of silicon (hereafter abbreviated as Si) and carbon. Not only does it have a dielectric breakdown field strength 10 times that of Si and a band gap three times that of Si, but it also allows for a wide range of control over the p-type and n-type required for device fabrication, making it a promising material for power devices that surpasses the limitations of Si.
[0003] However, compared to the widely used Si semiconductors, it is difficult to obtain large-area SiC single crystal substrates, and the manufacturing process is complicated. For these reasons, mass production of SiC semiconductors is more difficult and expensive than that of Si semiconductors. The high cost of SiC semiconductors has been one of the factors preventing the widespread use of SiC semiconductors.
[0004] Therefore, various efforts have been made to reduce the cost of SiC semiconductors. For example, Patent Document 1 discloses a method for manufacturing a SiC substrate by bonding a SiC single crystal substrate and a SiC polycrystalline substrate. 2 The following describes a method for manufacturing a SiC substrate for use in a SiC semiconductor, by bonding a single crystal SiC substrate and a polycrystalline SiC substrate together and then thinning the single crystal SiC substrate. The single crystal SiC substrate functions as the active layer of the SiC semiconductor device, and the polycrystalline SiC substrate takes on the roles of the mechanical support and heat dissipation parts at the bottom, making it possible to treat the entire SiC substrate in the same way as a substrate made of single crystal SiC.
[0005] Furthermore, Patent Document 1 also describes a method for thinning the SiC single crystal substrate by forming a hydrogen ion implanted layer in the SiC single crystal substrate before bonding the SiC single crystal substrate and the SiC polycrystalline substrate together, and then bonding the SiC single crystal substrate with the hydrogen ion implanted layer formed thereon to the SiC polycrystalline substrate, thereby performing a heat treatment at a temperature of 350° C. or less, thereby using the hydrogen ion implanted layer as a peeling surface for the SiC single crystal substrate.
[0006] The method described in Patent Document 1 has made it possible to obtain many more SiC substrates for use in SiC semiconductors from one SiC single crystal ingot. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2009-117533 A (claims 1, 5, paragraph 0008) Summary of the Invention [Problem to be solved by the invention]
[0008] Incidentally, SiC single crystal and SiC polycrystal are used for the bonded substrate manufactured by the method of Patent Document 1. The SiC single crystal for the bonded substrate can be manufactured by epitaxial growth using a sublimation method or a chemical vapor deposition method (CVD method) on a sublimation method substrate (a substrate for film formation of SiC single crystal manufactured by sublimation method), but epitaxially grown SiC single crystal is considered to be superior in quality to SiC single crystal obtained by sublimation method because it has fewer basal plane dislocations (BPDs), which become killer defects in devices when SiC devices are manufactured.
[0009] However, in order to obtain epitaxially grown SiC single crystal, it is necessary to form a thick film of the SiC single crystal on a sublimation substrate, and forming a thick film of the SiC single crystal may result in warping of the obtained SiC single crystal substrate (composed of a sublimation substrate and a SiC single crystal epitaxially grown on the surface of the sublimation substrate). If the SiC single crystal substrate is warped, for example, when the SiC single crystal substrate is transported to be bonded to a SiC polycrystalline substrate, it becomes difficult to vacuum-suck the SiC single crystal substrate using a suction cup or the like, which causes problems such as the inability to transport the SiC single crystal substrate, and thus reduces the manufacturing yield of the SiC substrate (composed of a SiC polycrystalline substrate and a SiC single crystal substrate).
[0010] The present invention has been made in view of these problems, and an object of the present invention is to provide a method for manufacturing a SiC single crystal substrate, which can suppress the occurrence of warping in a SiC single crystal substrate obtained by epitaxially growing a SiC single crystal film on a SiC single crystal film-growing substrate (the above-mentioned sublimation method substrate, i.e., a film-growing substrate for a SiC single crystal manufactured by sublimation method). [Means for solving the problem]
[0011] In order to solve the above problems, the present inventors have conducted intensive research and conducted repeated trial and error, and as a result, have completed the present invention.
[0012] That is, the first invention according to the present invention is: A method for manufacturing a silicon carbide single crystal substrate that constitutes a silicon carbide substrate (bonded substrate) to be bonded to a silicon carbide polycrystalline substrate and used for a silicon carbide semiconductor, comprising: Dopant included And it has a parallel plate shape. A method for producing a silicon carbide single crystal substrate comprising a silicon carbide single crystal film-growing substrate and the silicon carbide single crystal film, the method comprising epitaxially growing a silicon carbide single crystal film by chemical vapor deposition on a surface of the silicon carbide single crystal film-growing substrate, the method comprising the steps of: a first film formation step of supplying a mixed gas containing a source gas and a dopant gas into a film formation chamber in which the silicon carbide single crystal film formation substrate is disposed, and adjusting a supply ratio of the mixed gas to epitaxially grow a first silicon carbide single crystal film having a dopant concentration lower than a dopant concentration of the silicon carbide single crystal film formation substrate on a surface of the silicon carbide single crystal film formation substrate; a second film formation step of supplying a mixed gas containing a source gas and a dopant gas into the film formation chamber and adjusting a supply ratio of the mixed gas to epitaxially grow a second silicon carbide single crystal film having a dopant concentration higher than a dopant concentration of the silicon carbide single crystal film formation substrate on a surface of the first silicon carbide single crystal film; The present invention is characterized in that The second aspect of the present invention is A method for manufacturing a silicon carbide single crystal substrate that constitutes a silicon carbide substrate (bonded substrate) to be bonded to a silicon carbide polycrystalline substrate and used for a silicon carbide semiconductor, comprising: Dopant included And it has a parallel plate shape. A method for producing a silicon carbide single crystal substrate comprising a silicon carbide single crystal film-growing substrate and the silicon carbide single crystal film, the method comprising epitaxially growing a silicon carbide single crystal film by chemical vapor deposition on a surface of the silicon carbide single crystal film-growing substrate, the method comprising the steps of: a first film formation step of supplying a mixed gas containing a source gas and a dopant gas into a film formation chamber in which the silicon carbide single crystal film formation substrate is disposed, and adjusting a supply ratio of the mixed gas to epitaxially grow a first silicon carbide single crystal film on a surface of the silicon carbide single crystal film formation substrate, the first silicon carbide single crystal film having a dopant concentration higher than a dopant concentration of the silicon carbide single crystal film formation substrate; a second film formation step of supplying a mixed gas containing a source gas and a dopant gas into the film formation chamber and adjusting a supply ratio of the mixed gas to epitaxially grow a second silicon carbide single crystal film having a dopant concentration lower than a dopant concentration of the silicon carbide single crystal film formation substrate on a surface of the first silicon carbide single crystal film; The present invention is characterized by having the following.
[0013] Next, the third invention according to the present invention is In the method for producing a silicon carbide single crystal substrate according to the first or second invention, In the first film formation step and the second film formation step, at least one of a supply amount of the mixed gas, a pressure in the film formation chamber, and a film formation temperature is adjusted to adjust dopant concentrations of the first silicon carbide single crystal film and the second silicon carbide single crystal film; The fourth invention is In the method for producing a silicon carbide single crystal substrate according to the first or second invention, In the first film formation step and the second film formation step, the first silicon carbide single crystal film and the second silicon carbide single crystal film are epitaxially grown while rotating the silicon carbide single crystal film formation substrate, and a dopant concentration of the first silicon carbide single crystal film and the second silicon carbide single crystal film is adjusted by adjusting a rotation speed of the silicon carbide single crystal film formation substrate, The fifth invention is In the method for producing a silicon carbide single crystal substrate according to any one of the first to fourth aspects of the present invention, The dopant gas is one or more selected from the group consisting of boron, aluminum, gallium, nitrogen, phosphorus, and vanadium; The sixth invention is, In the method for producing a silicon carbide single crystal substrate according to any one of the first to fifth aspects of the present invention, The film formation temperature in the first film formation step and the second film formation step is 1200°C to 1700°C, The seventh invention is , In the method for producing a silicon carbide single crystal substrate according to any one of the first to sixth aspects of the present invention, , The silicon carbide single crystal substrate thus obtained is characterized in that, when the difference between the maximum and minimum values of the deviation of the center plane of the substrate from a reference plane is measured as the amount of warpage using a flatness measuring device, the amount of warpage is within ±100 μm. . Effect of the Invention
[0014] According to the method for producing a silicon carbide single crystal substrate according to the first aspect of the present invention, In a first film formation step, a first silicon carbide single crystal film having a lower dopant concentration than the single crystal film formation substrate is epitaxially grown on a surface of the silicon carbide single crystal film formation substrate; In the second film formation step, a second silicon carbide single crystal film having a higher dopant concentration than the silicon carbide single crystal film formation substrate is epitaxially grown on the surface of the first silicon carbide single crystal film. The stress acting between the silicon carbide single crystal film growth substrate and the silicon carbide single crystal film (composed of the first silicon carbide single crystal film and the second silicon carbide single crystal film) is reduced, making it possible to suppress the occurrence of warping of the silicon carbide single crystal substrate.
[0015] Moreover, according to a method for producing a silicon carbide single crystal substrate according to the second aspect of the present invention, In a first film formation step, a first silicon carbide single crystal film having a dopant concentration higher than that of the silicon carbide single crystal film formation substrate is epitaxially grown on a surface of the silicon carbide single crystal film formation substrate; In the second film formation step, a second silicon carbide single crystal film having a lower dopant concentration than the silicon carbide single crystal film formation substrate is epitaxially grown on the surface of the first silicon carbide single crystal film. The stress acting between the silicon carbide single crystal film growth substrate and the silicon carbide single crystal film (composed of the first silicon carbide single crystal film and the second silicon carbide single crystal film) is reduced, making it possible to suppress the occurrence of warping of the silicon carbide single crystal substrate. [Brief description of the drawings]
[0016] [Figure 1] FIG. 1 is a configuration explanatory diagram showing an example of a film formation apparatus for forming a SiC single crystal film by chemical vapor deposition (CVD). [Diagram 2] Figure 2(A) is a cross-sectional view of a SiC single crystal film-growing substrate, Figure 2(B) is a cross-sectional view of a SiC single crystal substrate composed of a first SiC single crystal film epitaxially grown on the surface of the SiC single crystal film-growing substrate and a second SiC single crystal film epitaxially grown on the surface of the first SiC single crystal film, and Figure 2(C) is a cross-sectional view of a SiC single crystal substrate whose diameter dimension has been adjusted by grinding or otherwise processing the outer periphery. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] Hereinafter, an embodiment of the present invention will be described in detail with reference to the drawings, but the present invention is not limited to the following embodiment.
[0018] (1) Film deposition equipment FIG. 1 is a configuration explanatory diagram showing an example of a film formation apparatus for forming a SiC single crystal film by chemical vapor deposition (CVD). The following explanation is an example of a film formation procedure, and the configuration of the film formation apparatus, various conditions such as temperature, pressure, and gas atmosphere, and procedures may be changed within a range that does not cause problems.
[0019] This film formation apparatus 100 includes a housing 101 which is the exterior of the apparatus, a film formation chamber 102 in which a SiC single crystal film (comprised of a first SiC single crystal film 21 and a second SiC single crystal film 22) 20 is formed on a SiC single crystal film formation substrate 10, an exhaust gas introduction chamber 105 which introduces the source gas, dopant gas, and carrier gas exhausted from the film formation chamber 102 into a gas exhaust port 104 which will be described later, and a box 106 which covers the exhaust gas introduction chamber 105. The film formation chamber 102 has a carbon heater 107 for heating the inside of the film formation chamber 102 from outside the box 106, a gas inlet 103 provided at the top of the film formation chamber 102 for introducing raw material gas, dopant gas, and carrier gas into the film formation chamber 102, a gas outlet 104 for discharging the raw material gas and the like to the outside of the film formation apparatus, a support 108 for rotatably supporting a susceptor 90 described below, and the susceptor 90 on which a SiC single crystal film formation substrate 10 is placed.
[0020] The support 108 has a holding mechanism (not shown) that holds the susceptor 90, and a rotation mechanism (not shown) that rotates the susceptor 90 during film formation. The susceptor 90 also has a flat mounting portion 91 on which the SiC single crystal film growth substrate 10 is placed, and a wall portion 92 standing upright from the outer periphery of the mounting portion 91. Since the susceptor 90 has the wall portion 92, it is possible to suppress the SiC single crystal film growth substrate 10 from flying outward due to centrifugal force when the susceptor 90 rotates.
[0021] First, the SiC single crystal film-forming substrate 10 is placed on the mounting portion 91 of the susceptor 90 as shown in Fig. 1, and the SiC single crystal film-forming substrate 10 is heated by the heater 107 to a film-forming reaction temperature under an inert gas atmosphere such as Ar under reduced pressure. After the preset film-forming reaction temperature (about 1200°C to 1700°C) is reached, the supply of the inert gas is stopped, the pressure inside the film-forming chamber 102 is set to about several kPa to several hundred kPa, and a mixed gas of a source gas containing the components of the SiC single crystal film 20, a dopant gas, a carrier gas, and the like is supplied into the film-forming chamber 102. At this time, a first SiC single crystal film 21 is formed on the surface of the SiC single crystal film-forming substrate 10 while rotating the susceptor 90 in the direction of the arrow A in Fig. 1, and then a second SiC single crystal film 22 is formed on the surface of the first SiC single crystal film 21. The rotation speed of the SiC single crystal film growth substrate 10 can be set to about 0 rpm to 1000 rpm when a 4 inch or 6 inch diameter SiC single crystal film growth substrate 10 is used.
[0022] In each of the deposition steps of the first SiC single crystal film 21 and the second SiC single crystal film 22, the supply ratio of the mixed gas is adjusted to adjust the dopant concentration (dopant content) of the first SiC single crystal film 21 and the second SiC single crystal film 22. Regarding the supply ratio of the mixed gas, the dopant concentration of the deposited first SiC single crystal film 21 and second SiC single crystal film 22 tends to be higher as the ratio of the dopant gas increases.
[0023] In addition, the amount of mixed gas supplied, the pressure in the film formation chamber 102, the film formation temperature, and the rotation speed of the SiC single crystal film formation substrate 10 affect the film formation speed of the SiC single crystal film 20. Therefore, by adjusting at least one of the amount of mixed gas supplied, the pressure in the film formation chamber 102 (e.g., several kPa to several hundred kPa), the film formation temperature (e.g., 1200°C to 1700°C), and the rotation speed of the SiC single crystal film formation substrate 10, it is also possible to adjust the dopant concentration (dopant content) of the first SiC single crystal film 21 and the second SiC single crystal film 22.
[0024] (2) Substrates for growing SiC single crystal films 2(A) may be, for example, a 4H-SiC single crystal wafer obtained by processing a bulk single crystal of SiC produced by a sublimation method or the like. The shape of the SiC single crystal film-growing substrate 10 may be, for example, a circular parallel plate shape. When a SiC single crystal film 20 (composed of the first SiC single crystal film 21 and the second SiC single crystal film 22) having a thickness of about 5 μm to 100 μm is grown, the thickness of the SiC single crystal film-growing substrate 10 may be about 250 μm to 750 μm.
[0025] In addition, the dopant concentration (dopant content) of the SiC single crystal film growth substrate 10 is not particularly limited and can be appropriately set based on the desired electrical resistance value, etc. When the dopant gas is nitrogen, the dopant concentration (dopant content) is 6×10 18 cm -3 ~10×10 18 cm -3 A SiC single crystal film growth substrate 10 of about 100 mm in diameter can be used.
[0026] (3) Source gas, carrier gas, purge gas, and dopant gas The raw material gas is not particularly limited as long as it can form a SiC single crystal film (consisting of a first SiC single crystal film 21 and a second SiC single crystal film 22) 20, and a Si-based raw material gas or a C-based raw material gas that is generally used for forming SiC single crystal films can be used.
[0027] For example, as the silicon (Si)-based raw material gas, silane (SiH4) can be used, as well as chlorine-based Si raw material-containing gas (chloride-based raw material) containing Cl having an etching effect, such as monochlorosilane (SiH3Cl), dichlorosilane (SiH2Cl2), trichlorosilane (SiHCl3), tetrachlorosilane (SiCl4), etc. When the above silane gas is used, HCl may be supplied together.
[0028] Examples of carbon (C)-based source gases that can be used include hydrocarbons such as methane (CH4), propane (C3H8), and acetylene (C2H2). In addition to the above, gases that contain both Si and C, such as trichloromethylsilane (CH3Cl3Si), trichlorophenylsilane (C6H5Cl3Si), dichloromethylsilane (CH4Cl2Si), dichlorodimethylsilane [(CH3)2SiCl2], and chlorotrimethylsilane [(CH3)3SiCl], can also be used as source gases.
[0029] As the carrier gas, any commonly used carrier gas can be used as long as it can spread the source gas to the substrate without interfering with the deposition. For example, hydrogen (H2), which has excellent thermal conductivity and has an etching effect on SiC, can be used.
[0030] In addition, a purge gas may be supplied as the third gas. The purge gas is a gas that does not contain Si or C, and in addition to a gas that contains H2 and has an etching effect, an inert gas (rare gas) such as Ar or He can also be used.
[0031] Moreover, an impurity doping gas is simultaneously supplied to control the conductivity type of the SiC single crystal film (composed of the first SiC single crystal film 21 and the second SiC single crystal film 22) 20. For example, N2 can be used to make the conductivity type n-type, and TMA (trimethylaluminum) can be used to make the conductivity type p-type.
[0032] The dopant gas is not limited to nitrogen and aluminum, but may be, for example, a gas containing one or more elements selected from boron, aluminum, gallium, nitrogen, phosphorus, and vanadium.
[0033] In addition, when the dopant gas is boron (B), boron trichloride (BCl3) or diborane (B2H6) can be used, when the dopant gas is gallium (Ga), trimethylgallium (TMAL) or triethylgallium (TEGa) can be used, when the dopant gas is phosphorus, phosphine (PH3) can be used, and when the dopant gas is vanadium, vanadium tetrachloride (VCl4) can be used. When the dopant gas is nitrogen, ammonia (NH3) can be used as the dopant gas in addition to nitrogen gas.
[0034] In order to adjust the dopant concentration (dopant content) of the dopant gas, for example, when a mixed gas containing silane (SiH4) gas as a Si-based gas, propane (C3H8) gas and hydrogen (H2) gas as a carbon-based gas, hydrogen chloride (HCl) gas as a chlorine-based gas, and nitrogen (N2) gas as a dopant gas is supplied, the supply ratio of the above mixed gas can be SiH4:C3H8:H2:HCl:N2=0.23:0.11:97.36:2.10:0.001 to 0.23:0.11:97.36:2.10:1.02.
[0035] The supply amount of the mixed gas can be about 1 slm to 500 slm in total to be supplied into the film formation chamber 102. The unit of gas flow rate "slm" indicates standard liter / min, that is, the flow rate (L) per minute converted into the standard condition (0°C, 1 atm).
[0036] (4) SiC single crystal substrate In the first film-forming step, a first SiC single crystal film 21 shown in FIG. 2(B) having a dopant concentration lower than that of the SiC single crystal film-forming substrate 10 is epitaxially grown on the surface of the SiC single crystal film-forming substrate 10 having a dopant shown in FIG. 2(A), and in the second film-forming step, a second SiC single crystal film 22 having a dopant concentration higher than that of the SiC single crystal film-forming substrate 10 is epitaxially grown on the surface of the first SiC single crystal film 21, and then the diameter dimension of the outer periphery is adjusted by grinding or the like, thereby manufacturing a SiC single crystal substrate 200 shown in FIG. 2(C) having a dopant concentration of the second SiC single crystal film 22 higher than that of the SiC single crystal film-forming substrate 10. In a first film-forming step, a first SiC single crystal film 21 shown in FIG. 2(B) having a dopant concentration higher than that of the SiC single crystal film-forming substrate 10 is epitaxially grown on the surface of a SiC single crystal film-forming substrate 10 having a dopant as shown in FIG. 2(A), and in a second film-forming step, a second SiC single crystal film 22 having a dopant concentration lower than that of the SiC single crystal film-forming substrate 10 is epitaxially grown on the surface of the first SiC single crystal film 21. Then, the diameter dimension of the outer periphery is adjusted by grinding or the like, thereby manufacturing a SiC single crystal substrate 200 shown in FIG. 2(C) having a lower doping concentration of the second SiC single crystal film 22 than that of the SiC single crystal film-forming substrate 10.
[0037] (5) Other processes The method for manufacturing a SiC single crystal substrate according to this embodiment can include the following steps: For example, a step of heating the SiC single crystal film-growing substrate 10 arranged on the susceptor 90 of the film-growing chamber 102, and a step of circulating an inert gas such as argon in the film-growing chamber 102 in which the SiC single crystal film-growing substrate 10 is arranged so as not to cause any reaction that would inhibit film growth before chemical vapor deposition, to create an inert atmosphere.
[0038] In addition, as shown in FIG. 2(B), the SiC single crystal film (first SiC single crystal film 21 and second SiC single crystal film 22) 20 may be formed not only on the film-forming surface 10a (see FIG. 1) of the SiC single crystal film-forming substrate 10 but also along the side surface of the SiC single crystal film-forming substrate 10. For this reason, after the second film-forming step, it is preferable to adjust the diameter of the outer periphery by grinding or the like as described above. Furthermore, in order to obtain a desired thickness for the SiC single crystal substrate 200 shown in FIG. 2(C), grinding or polishing may be performed as necessary.
[0039] (6) Comparison of the manufacturing method of the SiC single crystal substrate according to the present invention with the conventional method (6-1) Conventional manufacturing method for SiC single crystal substrates (conventional method) (6-1-1) In the conventional method of producing a SiC single crystal substrate by epitaxially growing a SiC single crystal on a sublimation substrate (a substrate for film formation of a SiC single crystal produced by sublimation) using chemical vapor deposition (CVD), the obtained SiC single crystal substrate may warp. When bonding the SiC single crystal substrate with a SiC polycrystalline substrate to produce a SiC substrate (composed of a SiC polycrystalline substrate and a SiC single crystal substrate), the substrate cannot be vacuum-adsorbed, and the Si single crystal substrate cannot be transported. These problems reduce the production yield of the SiC substrate.
[0040] (6-1-2) The above-mentioned warpage of the SiC single crystal substrate occurs when there is a stress difference between the SiC single crystal film-growing substrate (substrate for sublimation method) and the formed SiC single crystal film, and this stress difference is considered to be caused in large part by the difference in dopant content (dopant concentration, doping amount) between the SiC single crystal film-growing substrate and the SiC single crystal film.
[0041] (6-1-3) Here, in the crystal structure of SiC, the dopant substitutes for the C (carbon) site and dissolves. When the dopant is nitrogen, the lattice constant becomes smaller as the doping amount (dopant content) increases, because nitrogen has a smaller covalent bond radius than carbon.
[0042] Furthermore, when the doping amount of the SiC single crystal film is greater than that of the SiC single crystal film growth substrate, the lattice constant of the SiC single crystal film becomes smaller than that of the SiC single crystal film growth substrate, causing the SiC single crystal substrate to warp in a concave shape with the SiC single crystal film facing inward.
[0043] On the other hand, when the doping amount of the SiC single crystal film is smaller than that of the SiC single crystal film growth substrate, the lattice constant of the SiC single crystal film becomes larger than that of the SiC single crystal film growth substrate, and the SiC single crystal substrate develops a convex warp with the SiC single crystal film on the outside.
[0044] When the covalent bond radius of the dopant substituting the C site is larger than that of carbon [e.g., boron (B), aluminum (Al), gallium (Ga), etc.], the lattice constant increases as the doping amount (dopant content) increases, and the warping of the SiC single crystal substrate becomes opposite to that described above.
[0045] (6-2) Method for manufacturing a SiC single crystal substrate according to the present invention (6-2-1) The method of the present invention adjusts the dopant concentration of the first SiC single crystal film formed in the first film formation step and the second SiC single crystal film formed in the second film formation step relative to the dopant concentration of the SiC single crystal film formation substrate, thereby reducing the stress acting between the SiC single crystal film formation substrate and the SiC single crystal film (composed of the first SiC single crystal film and the second SiC single crystal film) and suppressing the occurrence of warping of the SiC single crystal substrate. Note that the dopant concentration of the SiC single crystal film formation substrate is appropriately set based on the desired electrical resistance value, etc., as described above.
[0046] (6-2-2) When the doping concentration of the second SiC single crystal film is made higher than that of the SiC single crystal film growth substrate The method for producing a SiC single crystal substrate according to claim 1 is characterized by comprising a first film formation step of epitaxially growing a first SiC single crystal film having a lower dopant concentration than the SiC single crystal film formation substrate on a surface of the SiC single crystal film formation substrate, and a second film formation step of epitaxially growing a second SiC single crystal film having a higher dopant concentration than the SiC single crystal film formation substrate on the surface of the first SiC single crystal film.
[0047] And when the dopant is nitrogen, which has a smaller covalent bond radius than carbon, The dopant concentration of the first SiC single crystal film formed on the surface of the SiC single crystal film-forming substrate in the first film-forming step is lower than the dopant concentration of the SiC single crystal film-forming substrate, and the lattice constant of the first SiC single crystal film is larger than the lattice constant of the SiC single crystal film-forming substrate. Therefore, a stress that warps the SiC single crystal film-forming substrate in a convex shape with the first SiC single crystal film, which has the larger lattice constant, on the outside acts between the SiC single crystal film-forming substrate and the first SiC single crystal film.
[0048] On the other hand, the dopant concentration of the second SiC single crystal film formed on the surface of the first SiC single crystal film in the second film formation process is higher than the respective dopant concentrations of the SiC single crystal film formation substrate and the second SiC single crystal film, and the lattice constant of the second SiC single crystal film is smaller than the respective lattice constants of the SiC single crystal film formation substrate and the first SiC single crystal film, so that a stress that warps the SiC single crystal film formation substrate concavely with the second SiC single crystal film, which has the smaller lattice constant, on the inside acts between the SiC single crystal film formation substrate and the second SiC single crystal film via the first SiC single crystal film.
[0049] Furthermore, a stress acting between the SiC single crystal film-growing substrate and the first SiC single crystal film and causing the SiC single crystal film-growing substrate to warp in a convex shape with the first SiC single crystal film on the outside, and a stress acting between the SiC single crystal film-growing substrate and the second SiC single crystal film via the first SiC single crystal film and causing the SiC single crystal film-growing substrate to warp in a concave shape with the second SiC single crystal film on the inside, cancel each other out, making it possible to suppress warping of the SiC single crystal substrate composed of the SiC single crystal film-growing substrate and the SiC single crystal films (the first SiC single crystal film and the second SiC single crystal film).
[0050] (6-2-3) When the doping concentration of the second SiC single crystal film is made lower than that of the SiC single crystal film growth substrate The method for producing a SiC single crystal substrate according to claim 2 is characterized by comprising a first film formation step of epitaxially growing a first SiC single crystal film having a higher dopant concentration than the SiC single crystal film formation substrate on a surface of the SiC single crystal film formation substrate, and a second film formation step of epitaxially growing a second SiC single crystal film having a lower dopant concentration than the SiC single crystal film formation substrate on the surface of the first SiC single crystal film.
[0051] And when the dopant is nitrogen, which has a smaller covalent bond radius than carbon, The dopant concentration of the first SiC single crystal film formed on the surface of the SiC single crystal film-forming substrate in the first film-forming step is higher than the dopant concentration of the SiC single crystal film-forming substrate, and the lattice constant of the first SiC single crystal film is smaller than the lattice constant of the SiC single crystal film-forming substrate. Therefore, a stress that warps the SiC single crystal film-forming substrate into a concave shape with the first SiC single crystal film, which has the smaller lattice constant, on the inside acts between the SiC single crystal film-forming substrate and the first SiC single crystal film.
[0052] On the other hand, the dopant concentration of the second SiC single crystal film formed on the surface of the first SiC single crystal film in the second film formation process is lower than the respective dopant concentrations of the SiC single crystal film formation substrate and the first SiC single crystal film, and the lattice constant of the second SiC single crystal film is larger than the respective lattice constants of the SiC single crystal film formation substrate and the first SiC single crystal film, so that a stress that warps the SiC single crystal film formation substrate in a convex shape with the second SiC single crystal film, which has a larger lattice constant, on the outside, acts between the SiC single crystal film formation substrate and the second SiC single crystal film via the first SiC single crystal film.
[0053] Furthermore, a stress acting between the SiC single crystal film-growing substrate and the first SiC single crystal film and causing the SiC single crystal film-growing substrate to warp concavely with the first SiC single crystal film on the inside, and a stress acting between the SiC single crystal film-growing substrate and the second SiC single crystal film via the first SiC single crystal film and causing the SiC single crystal film-growing substrate to warp convexly with the second SiC single crystal film on the outside, cancel each other out, making it possible to suppress warping of the SiC single crystal substrate composed of the SiC single crystal film-growing substrate and the SiC single crystal films (the first SiC single crystal film and the second SiC single crystal film). EXAMPLES
[0054] Hereinafter, the present invention will be described in detail with reference to examples and comparative examples, but the present invention is not limited to these examples. In the present examples, a SiC single crystal substrate was manufactured using the above-mentioned film formation apparatus 100.
[0055] [Example 1] Nitrogen was used as the dopant gas. The SiC single crystal deposition substrate for epitaxial growth of the SiC single crystal was a 6-inch diameter, 350 μm thick substrate fabricated by sublimation, with a dopant (nitrogen) concentration of 6 × 10 per unit volume. 18 cm -3 The n-type 4H—SiC single crystal wafer was used.
[0056] First, the film formation chamber 102 in the film formation apparatus 100 was evacuated by an exhaust pump, and then the temperature in the film formation chamber 102 was increased to 1650° C. while supplying Ar gas to heat the SiC single crystal film formation substrate.
[0057] After the temperature was raised to 1650°C, the supply of Ar gas was stopped, and raw material gases for the first film formation process and the like were supplied into the film formation chamber 102. Silane gas (SiH4), which is a Si-based gas, and propane gas (C3H8), which is a carbon-based gas, hydrogen gas (H2) and hydrogen chloride gas (HCl) were used as purge gases, and nitrogen gas (N2) was used as a dopant gas.
[0058] The mixed gas supply ratio was SiH4:C3H8:H2:HCl:N2=0.23:0.11:97.36:2.10:0.001, and the mixed gas supply amount was 180 slm in total for 12 minutes. While rotating the substrate at 600 rpm, a first SiC single crystal film was epitaxially grown on the surface (film formation target surface) of the SiC single crystal film formation substrate.
[0059] Next, after the first SiC single crystal film was formed, raw material gases for the second film formation process were supplied into the film formation chamber 102. Silane gas (SiH4) which is a Si-based gas, propane gas (C3H8) which is a carbon-based gas, hydrogen gas (H2) and hydrogen chloride gas (HCl) which are purge gases, and nitrogen gas (N2) which is a dopant gas were used.
[0060] The mixed gas supply ratio was SiH4:C3H8:H2:HCl:N2=0.23:0.11:97.36:2.10:1.02, the mixed gas supply amount was 180 slm in total, and was supplied for 60 minutes. A second SiC single crystal film was epitaxially grown on the surface of the first SiC single crystal film while the substrate was rotated at 600 rpm.
[0061] The pressure inside the film formation chamber 102 in the first and second film formation steps was 25 kPa.
[0062] Then, a SiC single crystal substrate composed of a SiC single crystal film-growing substrate and a SiC single crystal film (a first SiC single crystal film and a second SiC single crystal film) was obtained.
[0063] [Evaluation of SiC single crystal substrates] The produced SiC single crystal substrates were evaluated for the dopant concentrations (dopant contents) of the first SiC single crystal film and the second SiC single crystal film, the film thicknesses of the first SiC single crystal film and the second SiC single crystal film, and the amount of warping of the SiC single crystal substrate.
[0064] First, the dopant concentration (dopant content) of each of the epitaxially grown first and second SiC single crystal films was measured using a secondary ion mass spectrometer (hereinafter sometimes referred to as D-SIMS). As a result, the dopant concentration (dopant content) of the first SiC single crystal film was 6×10 15 cm -3 The dopant concentration (dopant content) of the second SiC single crystal film is 9×10 18 cm -3 That is, the dopant concentration of the first SiC single crystal film (6 × 10 15 cm -3 ) is the dopant concentration (6×10 18 cm -3 ) and the dopant concentration of the second SiC single crystal film (9×10 18 cm -3 ) is the dopant concentration (6×10 18 cm -3 ) was set higher.
[0065] In addition, when the thicknesses of the first SiC single crystal film and the second SiC single crystal film were measured, the average thickness of the first SiC single crystal film epitaxially grown on the surface of the SiC single crystal film-growing substrate was 10 μm, and the average thickness of the second SiC single crystal film epitaxially grown on the surface of the first SiC single crystal film was 50 μm.
[0066] Furthermore, the amount of warpage of the obtained SiC single crystal substrate was measured using a flatness measuring device, and the difference between the maximum and minimum deviations of the central surface of the substrate from a reference plane was taken as the amount of warpage. The amount of warpage of the SiC single crystal substrate was found to be 50 μm, which was a level that would not cause any problems when bonding it to a SiC polycrystalline substrate (if the amount of warpage of the SiC single crystal substrate is within ±100 μm, no problems will arise; the same applies below).
[0067] Table 1 shows the dopant concentrations (dopant contents) of the first SiC single crystal film and the second SiC single crystal film, the film thicknesses of the first SiC single crystal film and the second SiC single crystal film, and the amount of warping and evaluation of the SiC single crystal substrate.
[0068] [Example 2] A Si-based gas, silane gas (SiH4), a carbon-based gas, propane gas (C3H8), a purge gas, hydrogen gas (H2), hydrogen chloride gas (HCl), and nitrogen gas (N2) were used as raw material gases for the first film-forming process, the supply ratio of the mixed gas was SiH4:C3H8:H2:HCl:N2=0.23:0.11:97.36:2.10:0.001, and the mixed gas was supplied at a total amount of 180 slm for 36 minutes. In the same manner as in Example 1, except for this, a SiC single crystal substrate composed of a SiC single crystal film-forming substrate and a SiC single crystal film (first SiC single crystal film and second SiC single crystal film) was manufactured.
[0069] [Evaluation of SiC single crystal substrates] As in Example 1, the dopant concentration (dopant content) of each of the first SiC single crystal film and the second SiC single crystal film was measured using a secondary ion mass spectrometer (D-SIMS). As a result, the dopant concentration (dopant content) of the first SiC single crystal film was 6×10 15 cm -3 The dopant concentration (dopant content) of the second SiC single crystal film is 9×10 18 cm -3 It was.
[0070] That is, the dopant concentration of the first SiC single crystal film (6 × 10 15 cm -3 ) is the dopant concentration (6×10 18 cm -3 ) and the dopant concentration of the second SiC single crystal film (9×10 18 cm -3 ) is the dopant concentration (6×10 18 cm -3 ) was set higher.
[0071] In addition, when the thicknesses of the first SiC single crystal film and the second SiC single crystal film were measured, the average thickness of the first SiC single crystal film epitaxially grown on the surface of the SiC single crystal film-growing substrate was 30 μm, and the average thickness of the second SiC single crystal film epitaxially grown on the surface of the first SiC single crystal film was 50 μm.
[0072] Furthermore, the amount of warping of the obtained SiC single crystal substrate was measured using a flatness measuring device, and the difference between the maximum and minimum deviations of the center plane of the substrate from a reference plane was taken as the amount of warping. The amount of warping of the SiC single crystal substrate was found to be 30 μm, which was at a level that would not cause any problems when bonding it to a SiC polycrystalline substrate.
[0073] As in Example 1, the dopant concentrations (dopant contents) of the first SiC single crystal film and the second SiC single crystal film, the film thicknesses of the first SiC single crystal film and the second SiC single crystal film, and the amount of warping and evaluation of the SiC single crystal substrate are shown in Table 1.
[0074] [Example 3] A Si-based gas, silane gas (SiH4), a carbon-based gas, propane gas (C3H8), a purge gas, hydrogen gas (H2), hydrogen chloride gas (HCl), and a dopant gas, nitrogen gas (N2), were used as the raw material gas for the second film-forming process, the supply ratio of the mixed gas was SiH4:C3H8:H2:HCl:N2=0.23:0.11:97.36:2.10:1.02, and the mixed gas was supplied at a total amount of 180 slm for 120 minutes. In the same manner as in Example 1, except for this, a SiC single crystal substrate composed of a SiC single crystal film-forming substrate and a SiC single crystal film (first SiC single crystal film and second SiC single crystal film) was manufactured.
[0075] [Evaluation of SiC single crystal substrates] As in Example 1, the dopant concentration (dopant content) of each of the first SiC single crystal film and the second SiC single crystal film was measured using a secondary ion mass spectrometer (D-SIMS). As a result, the dopant concentration (dopant content) of the first SiC single crystal film was 6×10 15 cm -3 The dopant concentration (dopant content) of the second SiC single crystal film is 9×10 18 cm -3 It was.
[0076] That is, the dopant concentration of the first SiC single crystal film (6 × 10 15 cm -3 ) is the dopant concentration (6×1018 cm -3 ) and the dopant concentration of the second SiC single crystal film (9×10 18 cm -3 ) is the dopant concentration (6×10 18 cm -3 ) was set higher.
[0077] In addition, when the thicknesses of the first SiC single crystal film and the second SiC single crystal film were measured, the average thickness of the first SiC single crystal film epitaxially grown on the surface of the SiC single crystal film-growing substrate was 10 μm, and the average thickness of the second SiC single crystal film epitaxially grown on the surface of the first SiC single crystal film was 100 μm.
[0078] Furthermore, the amount of warping of the obtained SiC single crystal substrate was measured using a flatness measuring device, and the difference between the maximum and minimum deviations of the center plane of the substrate from a reference plane was taken as the amount of warping. The amount of warping of the SiC single crystal substrate was found to be 80 μm, which was at a level that would not cause any problems when bonding it to a SiC polycrystalline substrate.
[0079] As in Example 1, the dopant concentrations (dopant contents) of the first SiC single crystal film and the second SiC single crystal film, the film thicknesses of the first SiC single crystal film and the second SiC single crystal film, and the amount of warping and evaluation of the SiC single crystal substrate are shown in Table 1.
[0080] [Example 4] The raw material gases for the first film formation process were silane gas (SiH4), a Si-based gas, propane gas (C3H8), a carbon-based gas, hydrogen gas (H2), hydrogen chloride gas (HCl), and nitrogen gas (N2) as a dopant gas. The mixed gas supply ratio was SiH4:C3H8:H2:HCl:N2=0.23:0.11:97.36:2.10:1.02. The mixed gas was supplied at a total amount of 180 slm for 12 minutes, and a first SiC single crystal film was epitaxially grown on the surface (film formation target surface) of the SiC single crystal film formation substrate while rotating the substrate at 600 rpm.
[0081] Next, silane gas (SiH4) which is a Si-based gas, propane gas (C3H8) which is a carbon-based gas, hydrogen gas (H2) and hydrogen chloride gas (HCl) which are purge gases, and nitrogen gas (N2) which is a dopant gas were used as the raw material gas for the second film formation process, the supply ratio of the mixed gas was SiH4:C3H8:H2:HCl:N2=0.23:0.11:97.36:2.10:0.001, the mixed gas was supplied at a total amount of 180 slm for 60 minutes, and a second SiC single crystal film was epitaxially grown on the surface of the first SiC single crystal film while rotating the substrate at 600 rpm.
[0082] The pressure inside the film formation chamber 102 in the first and second film formation steps was 25 kPa.
[0083] Then, a SiC single crystal substrate composed of a SiC single crystal film-growing substrate and a SiC single crystal film (a first SiC single crystal film and a second SiC single crystal film) was obtained.
[0084] [Evaluation of SiC single crystal substrates] As in Example 1, the dopant concentration (dopant content) of each of the first SiC single crystal film and the second SiC single crystal film was measured using a secondary ion mass spectrometer (D-SIMS). As a result, the dopant concentration (dopant content) of the first SiC single crystal film was 9×10 18 cm -3 The dopant concentration (dopant content) of the second SiC single crystal film is 6×10 15 cm -3 It was.
[0085] That is, the dopant concentration of the first SiC single crystal film (9×10 18 cm -3 ) is the dopant concentration (6×10 18 cm -3 ) and the dopant concentration of the second SiC single crystal film (6×10 15 cm -3 ) is the dopant concentration (6×10 18 cm -3 ) was set lower.
[0086] In addition, when the thicknesses of the first SiC single crystal film and the second SiC single crystal film were measured, the average thickness of the first SiC single crystal film epitaxially grown on the surface of the SiC single crystal film-growing substrate was 10 μm, and the average thickness of the second SiC single crystal film epitaxially grown on the surface of the first SiC single crystal film was 50 μm.
[0087] Furthermore, the amount of warpage of the obtained SiC single crystal substrate was measured using a flatness measuring device, and the difference between the maximum and minimum deviations of the center plane of the substrate from a reference plane was taken as the amount of warpage. The amount of warpage of the SiC single crystal substrate was found to be 50 μm, which was at a level that would not cause any problems when bonding it to a SiC polycrystalline substrate.
[0088] As in Example 1, the dopant concentrations (dopant contents) of the first SiC single crystal film and the second SiC single crystal film, the film thicknesses of the first SiC single crystal film and the second SiC single crystal film, and the amount of warping and evaluation of the SiC single crystal substrate are shown in Table 1.
[0089] [Example 5] A Si-based gas, silane gas (SiH4), a carbon-based gas, propane gas (C3H8), a purge gas, hydrogen gas (H2), hydrogen chloride gas (HCl), and a dopant gas, nitrogen gas (N2), were used as the raw material gas for the first film-forming process, the supply ratio of the mixed gas was SiH4:C3H8:H2:HCl:N2=0.23:0.11:97.36:2.10:1.02, and the mixed gas was supplied at a total amount of 180 slm for 36 minutes. In the same manner as in Example 4, except for this, a SiC single crystal substrate composed of a SiC single crystal film-forming substrate and a SiC single crystal film (first SiC single crystal film and second SiC single crystal film) was manufactured.
[0090] [Evaluation of SiC single crystal substrates] As in Example 1, the dopant concentration (dopant content) of each of the first SiC single crystal film and the second SiC single crystal film was measured using a secondary ion mass spectrometer (D-SIMS). As a result, the dopant concentration (dopant content) of the first SiC single crystal film was 9×10 18 cm -3 The dopant concentration (dopant content) of the second SiC single crystal film is 6×1015 cm -3 It was.
[0091] That is, the dopant concentration of the first SiC single crystal film (9×10 18 cm -3 ) is the dopant concentration (6×10 18 cm -3 ) and the dopant concentration of the second SiC single crystal film (6×10 15 cm -3 ) is the dopant concentration (6×10 18 cm -3 ) was set lower.
[0092] In addition, when the thicknesses of the first SiC single crystal film and the second SiC single crystal film were measured, the average thickness of the first SiC single crystal film epitaxially grown on the surface of the SiC single crystal film-growing substrate was 30 μm, and the average thickness of the second SiC single crystal film epitaxially grown on the surface of the first SiC single crystal film was 50 μm.
[0093] Furthermore, the amount of warping of the obtained SiC single crystal substrate was measured using a flatness measuring device, and the difference between the maximum and minimum deviations of the center plane of the substrate from a reference plane was taken as the amount of warping. The amount of warping of the SiC single crystal substrate was found to be 30 μm, which was at a level that would not cause any problems when bonding it to a SiC polycrystalline substrate.
[0094] As in Example 1, the dopant concentrations (dopant contents) of the first SiC single crystal film and the second SiC single crystal film, the film thicknesses of the first SiC single crystal film and the second SiC single crystal film, and the amount of warping and evaluation of the SiC single crystal substrate are shown in Table 1.
[0095] [Example 6] A Si-based gas, silane gas (SiH4), a carbon-based gas, propane gas (C3H8), a purge gas, hydrogen gas (H2), hydrogen chloride gas (HCl), and a dopant gas, nitrogen gas (N2), were used as the raw material gas for the second film formation process, the supply ratio of the mixed gas was SiH4:C3H8:H2:HCl:N2=0.23:0.11:97.36:2.10:0.001, and the mixed gas was supplied at a total amount of 180 slm for 120 minutes. In the same manner as in Example 4, except for this, a SiC single crystal substrate composed of a SiC single crystal film formation substrate and a SiC single crystal film (first SiC single crystal film and second SiC single crystal film) was manufactured.
[0096] [Evaluation of SiC single crystal substrates] As in Example 1, the dopant concentration (dopant content) of each of the first SiC single crystal film and the second SiC single crystal film was measured using a secondary ion mass spectrometer (D-SIMS). As a result, the dopant concentration (dopant content) of the first SiC single crystal film was 9×10 18 cm -3 The dopant concentration (dopant content) of the second SiC single crystal film is 6×10 15 cm -3 It was.
[0097] That is, the dopant concentration of the first SiC single crystal film (9×10 18 cm -3 ) is the dopant concentration (6×10 18 cm -3 ) and the dopant concentration of the second SiC single crystal film (6×10 15 cm -3 ) is the dopant concentration (6×10 18 cm -3 ) was set lower.
[0098] In addition, when the thicknesses of the first SiC single crystal film and the second SiC single crystal film were measured, the average thickness of the first SiC single crystal film epitaxially grown on the surface of the SiC single crystal film-growing substrate was 10 μm, and the average thickness of the second SiC single crystal film epitaxially grown on the surface of the first SiC single crystal film was 100 μm.
[0099] Furthermore, the amount of warping of the obtained SiC single crystal substrate was measured using a flatness measuring device, and the difference between the maximum and minimum deviations of the center plane of the substrate from a reference plane was taken as the amount of warping. The amount of warping of the SiC single crystal substrate was found to be 80 μm, which was at a level that would not cause any problems when bonding it to a SiC polycrystalline substrate.
[0100] As in Example 1, the dopant concentrations (dopant contents) of the first SiC single crystal film and the second SiC single crystal film, the film thicknesses of the first SiC single crystal film and the second SiC single crystal film, and the amount of warping and evaluation of the SiC single crystal substrate are shown in Table 1.
[0101] [Comparative Example 1] Silane gas (SiH4) of Si-based gas, propane gas (C3H8) of carbon-based gas, hydrogen gas (H2) and hydrogen chloride gas (HCl) as purge gases, and nitrogen gas (N2) as dopant gas were used as the raw material gas for the film formation process, the supply ratio of the mixed gas was SiH4:C3H8:H2:HCl:N2=0.23:0.11:97.36:2.10:1.02, the supply amount of the mixed gas was 180 slm in total, and the substrate was rotated at 600 rpm, while a single layer of SiC single crystal film was epitaxially grown on the surface (film formation target surface) of the SiC single crystal film formation substrate, and a SiC single crystal substrate composed of a SiC single crystal film formation substrate and a SiC single crystal film was manufactured in the same manner as in Example 1, except that a second SiC single crystal film was not formed.
[0102] [Evaluation of SiC single crystal substrates] As in Example 1, the dopant concentration (dopant content) of the SiC single crystal film composed of a single layer was measured using a secondary ion mass spectrometer (D-SIMS). As a result, the dopant concentration (dopant content) of the SiC single crystal film was 9×10 18 cm -3 It was.
[0103] That is, the dopant concentration of the SiC single crystal film (9×10 18 cm -3 ) is the dopant concentration (6×10 18 cm-3 ) was set higher.
[0104] Furthermore, when the thickness of the SiC single crystal film was measured, the average thickness of the SiC single crystal film epitaxially grown on the surface of the SiC single crystal film-growing substrate was 50 μm.
[0105] Furthermore, the amount of warpage of the obtained SiC single crystal substrate was measured using a flatness measuring device, and the difference between the maximum and minimum deviations of the central surface of the substrate from a reference plane was taken as the amount of warpage. The amount of warpage of the SiC single crystal substrate was found to be 120 μm, a level that could potentially cause a transportation error when transporting the substrate for bonding to a SiC polycrystalline substrate.
[0106] As in Example 1, the dopant concentration (dopant content) of the SiC single crystal film, the thickness of the SiC single crystal film, and the amount of warping and evaluation of the SiC single crystal substrate are shown in Table 1.
[0107] [Table 1]
[0108] In the above Examples 1 to 6 and Comparative Example 1, nitrogen is used as the dopant gas. However, when phosphorus and vanadium, which have a smaller covalent bond radius than carbon, are used as the dopant gas, the lattice constant decreases as the doping amount (dopant content) increases, and it has been confirmed that the warping of the SiC single crystal substrate becomes similar to that in Examples 1 to 6. [Industrial Applicability]
[0109] According to the method for producing a silicon carbide single crystal substrate of the present invention, the occurrence of warping in the obtained silicon carbide single crystal substrate is suppressed, and therefore the method has industrial applicability in that it is used as a silicon carbide single crystal substrate to which a silicon carbide polycrystalline substrate is bonded for use in a silicon carbide semiconductor. [Explanation of symbols]
[0110] 10. SiC single crystal deposition substrate 10a Film formation surface 20 SiC single crystal film 21 First SiC single crystal film 22 Second SiC single crystal film 90 Susceptor 91 Placement section 92 Wall section 100 Film deposition equipment 101 Case 102 Deposition chamber 103 Gas inlet 104 Gas exhaust port 105 Exhaust gas introduction chamber Box 106 107 Heater 108 Pillars 200 SiC single crystal substrate
Claims
1. A method for manufacturing a silicon carbide single crystal substrate that constitutes a silicon carbide substrate (bonded substrate) to be bonded to a silicon carbide polycrystalline substrate for use in a silicon carbide semiconductor, comprising: A method for producing a silicon carbide single crystal substrate comprising a silicon carbide single crystal film-growing substrate having a dopant and a parallel plate shape, and epitaxially growing a silicon carbide single crystal film by chemical vapor deposition, the method comprising the steps of: a first film formation step of supplying a mixed gas containing a source gas and a dopant gas into a film formation chamber in which the silicon carbide single crystal film formation substrate is disposed, and adjusting a supply ratio of the mixed gas to epitaxially grow a first silicon carbide single crystal film having a dopant concentration lower than a dopant concentration of the silicon carbide single crystal film formation substrate on a surface of the silicon carbide single crystal film formation substrate; a second film formation step of supplying a mixed gas containing a source gas and a dopant gas into the film formation chamber and adjusting a supply ratio of the mixed gas to epitaxially grow a second silicon carbide single crystal film having a dopant concentration higher than a dopant concentration of the silicon carbide single crystal film formation substrate on a surface of the first silicon carbide single crystal film; 2. A method for producing a silicon carbide single crystal substrate comprising the steps of:
2. A method for manufacturing a silicon carbide single crystal substrate that constitutes a silicon carbide substrate (bonded substrate) to be bonded to a silicon carbide polycrystalline substrate for use in a silicon carbide semiconductor, comprising: A method for producing a silicon carbide single crystal substrate comprising a silicon carbide single crystal film-growing substrate having a dopant and a parallel plate shape, and epitaxially growing a silicon carbide single crystal film by chemical vapor deposition, the method comprising the steps of: a first film formation step of supplying a mixed gas containing a source gas and a dopant gas into a film formation chamber in which the silicon carbide single crystal film formation substrate is disposed, and adjusting a supply ratio of the mixed gas to epitaxially grow a first silicon carbide single crystal film on a surface of the silicon carbide single crystal film formation substrate, the first silicon carbide single crystal film having a dopant concentration higher than a dopant concentration of the silicon carbide single crystal film formation substrate; a second film formation step of supplying a mixed gas containing a source gas and a dopant gas into the film formation chamber and adjusting a supply ratio of the mixed gas to epitaxially grow a second silicon carbide single crystal film having a dopant concentration lower than a dopant concentration of the silicon carbide single crystal film formation substrate on a surface of the first silicon carbide single crystal film; 2. A method for producing a silicon carbide single crystal substrate comprising the steps of:
3. 3. The method for manufacturing a silicon carbide single crystal substrate according to claim 1, wherein in the first film formation process and the second film formation process, at least one of the supply amount of the mixed gas, the pressure in the film formation chamber, and the film formation temperature is adjusted to adjust dopant concentrations in the first silicon carbide single crystal film and the second silicon carbide single crystal film.
4. 3. The method for manufacturing a silicon carbide single crystal substrate according to claim 1 or 2, characterized in that, in the first film formation step and the second film formation step, the first silicon carbide single crystal film and the second silicon carbide single crystal film are epitaxially grown while rotating the silicon carbide single crystal film formation substrate, and dopant concentrations of the first silicon carbide single crystal film and the second silicon carbide single crystal film are adjusted by adjusting the rotation speed of the silicon carbide single crystal film formation substrate.
5. 5. The method for producing a silicon carbide single crystal substrate according to claim 1, wherein the dopant gas is one or more kinds selected from the group consisting of boron, aluminum, gallium, nitrogen, phosphorus and vanadium.
6. 6. The method for producing a silicon carbide single crystal substrate according to claim 1, wherein the film formation temperature in the first film formation step and the second film formation step is 1200°C to 1700°C.
7. A method for manufacturing a silicon carbide single crystal substrate as described in any one of claims 1 to 6, characterized in that when the obtained silicon carbide single crystal substrate is measured using a flatness measuring device to measure the difference between the maximum and minimum deviations of the central surface of the substrate from a reference plane as the amount of warping, the amount of warping is within ±100 μm.
Citation Information
Patent Citations
Semiconductor device and manufacturing method therefor
JP2003318388A
Method for manufacturing silicon carbide semiconductor device and silicon carbide semiconductor device
JP2008091656A
Manufacturing method of silicon carbide substrate
JP2009117533A
Semiconductor substrate and semiconductor device, and method of manufacturing the same
JP2009130266A
Multilayer semiconductor substrate and method for manufacturing the same
JP2014526138A