Fluororesin substrate laminate

The fluororesin substrate laminate with a specific adhesive layer composition addresses the adhesion and flexibility issues of fluororesins with low-roughness metal foils, providing low transmission loss and dielectric properties suitable for high-frequency applications.

JP7567304B2Active Publication Date: 2024-10-16RESONAC CORP
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2020154542
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-09-15
Publication Date
2024-10-16
Estimated Expiration
2040-09-15

AI Technical Summary

Technical Problem

Fluororesins like polytetrafluoroethylene (PTFE) have low adhesive strength with metal foils of low surface roughness, leading to increased transmission loss and flexibility issues in high-frequency applications, particularly in flexible printed wiring boards (FPCs).

Method used

A fluororesin substrate laminate with an adhesive layer containing a resin composition of maleimide compounds and inorganic fillers, which includes a maleimide compound with a saturated or unsaturated divalent hydrocarbon group and an aromatic maleimide compound, along with an inorganic filler content of 10 to 50 vol%, enhancing adhesion to both fluororesin and low-roughness metal foils.

Benefits of technology

The laminate achieves low hygroscopicity, excellent low dielectric constant, and low dielectric loss tangent, reducing transmission loss and maintaining flexibility in high-frequency regions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007567304000020
    Figure 0007567304000020
  • Figure 0007567304000021
    Figure 0007567304000021
  • Figure 0007567304000001
    Figure 0007567304000001
Patent Text Reader

Abstract

To provide a laminate of fluororesin substrates that has low hygroscopicity, and sufficiently low dielectric constants and low dielectric loss tangents, and can reduce transmission loss in a high-frequency region.SOLUTION: This invention relates to a laminate of fluororesin substrates for high-frequency circuits containing a fluororesin substrate and an adhesive layer provided on the fluororesin substrate. The adhesive layer contains a resin composition containing (A) a maleimide compound having a saturated or unsaturated, divalent hydrocarbon group, (B) an aromatic maleimide compound, and an inorganic filler. The content of the inorganic filler is 10-50 vol% or less relative to the total solid content of the resin composition.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a fluororesin substrate laminate for use in high frequency circuits. [Background technology]

[0002] The speed and capacity of signals used in electronic devices such as mobile phones, their base station equipment, network infrastructure devices such as servers and routers, and large computers are increasing year by year, and in particular, rapid growth in 5G (5th generation mobile communication system) is expected. As a result, the printed wiring boards mounted on these electronic devices must be compatible with higher frequencies, and there is a demand for board materials with low relative dielectric constant and low dielectric loss tangent properties that enable reduced transmission loss. In recent years, in addition to the electronic devices mentioned above, new systems that handle high-frequency wireless signals in the ITS field (related to automobiles and traffic systems) and in the field of indoor short-range communication have been put into practical use and are planned to be put into practical use as applications that handle such high-frequency signals. It is expected that in the future, board materials with even lower transmission loss will also be required for the printed wiring boards mounted on these devices.

[0003] In recent years, flexible printed circuit boards (hereinafter referred to as FPCs) have also been installed in these devices. FPCs are becoming essential wiring boards for high-density mounting in mobile devices such as smartphones, which are becoming thinner and faster to transmit signals, and they require reduced transmission loss and flexibility.

[0004] Conventionally, resins such as polyphenylene ether (PPE), polyimide (PI), liquid crystal polymer (LCP), and fluororesin have been used for printed wiring boards that require low transmission loss (see, for example, Patent Documents 1 to 4). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Japanese Patent Application Publication No. 58-69046 [Patent Document 2] JP 2012-255059 A [Patent Document 3] JP 2014-60449 A [Patent Document 4] JP 2003-171480 A Summary of the Invention [Problem to be solved by the invention]

[0006] Fluororesins are known to be materials with low moisture absorption, excellent low dielectric constant and low dielectric loss tangent. However, fluororesins such as polytetrafluoroethylene (PTFE) have low adhesive strength with metal foils, making it difficult to laminate them with metal foils with low surface roughness (e.g., low-roughness copper foil). Therefore, metal foils with high surface roughness (ten-point average roughness: Rz, the same applies below) must be bonded to fluororesin substrates, and transmission loss tends to increase in the high frequency range compared to substrates made of PPE, PI, LCP, etc.

[0007] Furthermore, as a result of the inventors' own investigations, it was found that when an adhesive layer is used to bond a fluororesin substrate and a metal foil, sufficient flexibility cannot be maintained, and there is room for improvement for use in FPCs. Therefore, an object of the present invention is to provide a fluororesin substrate laminate that has high flexibility, an excellent low dielectric constant and low dielectric tangent, and is capable of reducing transmission loss in the high frequency range. [Means for solving the problem]

[0008] One aspect of the present disclosure includes a fluororesin substrate and an adhesive layer provided on the fluororesin substrate, The present invention relates to a fluororesin substrate laminate for high-frequency circuits, wherein the adhesive layer comprises a resin composition containing (A) a maleimide compound having a saturated or unsaturated divalent hydrocarbon group, (B) an aromatic maleimide compound, and an inorganic filler, and the content of the inorganic filler is in the range of 10 to 50 vol% with respect to the total solid content in the resin composition. Effect of the Invention

[0009] According to the present invention, it is possible to provide a fluororesin substrate laminate that has low moisture absorption, excellent low dielectric constant and low dielectric tangent, and is capable of reducing transmission loss in the high frequency range. [Brief description of the drawings]

[0010] [Figure 1] 1 is a schematic cross-sectional view showing one embodiment of a fluororesin substrate laminate. [Diagram 2] 1 is a schematic cross-sectional view showing one embodiment of a fluororesin substrate laminate. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Preferred embodiments of the present invention will be described in detail below. However, the present invention is not limited to the following embodiments. In this specification, the high frequency region refers to the region of 0.3 to 300 GHz, and in particular, refers to the region of 3 to 300 GHz.

[0012] <Fluororesin Substrate Laminate> 1 is a schematic cross-sectional view showing one embodiment of a fluororesin substrate laminate for use in a high-frequency circuit according to this embodiment. The fluororesin substrate laminate includes a fluororesin substrate 1 and an adhesive layer 2 provided on the fluororesin substrate 1.

[0013] [Adhesive layer] The adhesive layer 2 according to this embodiment contains a resin composition containing (A) a maleimide compound having a saturated or unsaturated divalent hydrocarbon group and (B) an aromatic maleimide compound. The adhesive layer 2 not only has excellent adhesion to the fluororesin substrate 1, but also has excellent adhesion to a metal foil, which will be described later. This allows the use of a metal foil with a small surface roughness (Rz: ten-point average roughness), thereby reducing transmission loss in the high frequency range of the fluororesin substrate laminate.

[0014] The thickness of the adhesive layer 2 is not particularly limited, and may be, for example, 1 to 200 μm, 3 to 180 μm, 5 to 150 μm, 10 to 100 μm, or 15 to 80 μm. By setting the thickness of the adhesive layer 2 within the above range, it becomes easier to further improve the high-frequency characteristics of the laminate according to this embodiment. (The above "to" indicates a range including the numerical values ​​before and after it as the minimum and maximum values, respectively. The same applies hereinafter.)

[0015] The adhesive layer 2 may be formed by applying the above-mentioned resin composition to the fluororesin substrate 1, or may be formed by preparing a resin film of the above-mentioned resin composition and laminating the resin film on the fluororesin substrate 1. The resin film refers to an uncured or semi-cured film-like resin composition. Each component contained in the resin composition will be described in detail below.

[0016] ((A) Maleimide Compound Having a Saturated or Unsaturated Divalent Hydrocarbon Group) The maleimide compound having a saturated or unsaturated divalent hydrocarbon group according to this embodiment may be referred to as component (A). Component (A) is a compound having (a) a maleimide group and (c) a saturated or unsaturated divalent hydrocarbon group. The (a) maleimide group may be referred to as structure (a), and the (c) saturated or unsaturated divalent hydrocarbon group may be referred to as structure (c). By using component (A), a resin composition having excellent high-frequency characteristics and adhesiveness may be obtained.

[0017] In addition to the structures (a) and (c), the component (A) may further have (b) a divalent group having at least two imide bonds. (b) The divalent group having at least two imide bonds is sometimes referred to as structure (b).

[0018] The (a) maleimide group is not particularly limited and is a general maleimide group. The (a) maleimide group may be bonded to an aromatic ring or an aliphatic chain, but from the viewpoint of dielectric properties, it is preferable that the (a) maleimide group is bonded to a long-chain aliphatic chain (for example, a saturated hydrocarbon group having 8 to 100 carbon atoms). When the (A) component has a structure in which the (a) maleimide group is bonded to a long-chain aliphatic chain, the high-frequency properties of the resin composition can be further improved.

[0019] Although there is no particular limitation on the structure (b), examples thereof include a group represented by the following formula (I): The structure (b) is a group that does not have a maleimide group.

[0020] [ka]

[0021] In formula (I), R1 represents a tetravalent organic group. R1 is not particularly limited as long as it is a tetravalent organic group, but from the viewpoint of ease of handling, for example, it may be a hydrocarbon group having 1 to 100 carbon atoms, a hydrocarbon group having 2 to 50 carbon atoms, or a hydrocarbon group having 4 to 30 carbon atoms.

[0022] R1 may contain a substituted or unsubstituted siloxane moiety. Examples of the siloxane moiety include structures derived from dimethylsiloxane, methylphenylsiloxane, diphenylsiloxane, and the like.

[0023] When R1 is substituted, examples of the substituent include an alkyl group, an alkenyl group, an alkynyl group, a hydroxyl group, an alkoxy group, a mercapto group, a cycloalkyl group, a substituted cycloalkyl group, a heterocyclic group, a substituted heterocyclic group, an aryl group, a substituted aryl group, a heteroaryl group, a substituted heteroaryl group, an aryloxy group, a substituted aryloxy group, a halogen atom, a haloalkyl group, a cyano group, a nitro group, a nitroso group, an amino group, an amido group, -CHO, -NR x C(O)-N(R x )2, -OC(O)-N(R x) 2, acyl group, oxyacyl group, carboxyl group, carbamate group, sulfonamide group, etc. x teeth The substituent represents a hydrogen atom or an alkyl group. One or more of these substituents can be selected according to the purpose, application, etc.

[0024] R1 is preferably, for example, a tetravalent residue of an acid anhydride having two or more anhydride rings in one molecule, that is, a tetravalent group obtained by removing two acid anhydride groups (-C(=O)OC(=O)-) from an acid anhydride. Examples of the acid anhydride include compounds described below.

[0025] From the viewpoint of mechanical strength, R1 is preferably aromatic, and more preferably a group in which two acid anhydride groups have been removed from pyromellitic dianhydride. That is, structure (b) is more preferably a group represented by the following formula (III).

[0026] [ka]

[0027] From the viewpoint of fluidity and circuit embedding property, it is preferable that a plurality of structures (b) are present in the component (A). In this case, the structures (b) may be the same or different. The number of structures (b) in the component (A) is preferably 2 to 40, more preferably 2 to 20, and even more preferably 2 to 10.

[0028] From the viewpoint of dielectric properties, the structure (b) may be a group represented by the following formula (IV) or the following formula (V).

[0029] [ka]

[0030] [ka]

[0031] Structure (c) is not particularly limited, and may be linear, branched, or cyclic. From the viewpoint of high frequency characteristics, structure (c) is preferably an aliphatic hydrocarbon group. In addition, the carbon number of the saturated or unsaturated divalent hydrocarbon group may be 8 to 100. Structure (c) is preferably an alkylene group having 8 to 100 carbon atoms which may be branched, more preferably an alkylene group having 10 to 70 carbon atoms which may be branched, and even more preferably an alkylene group having 15 to 50 carbon atoms which may be branched. When structure (c) is an alkylene group having 8 or more carbon atoms which may be branched, the molecular structure is easily three-dimensional, and the free volume of the polymer is easily increased to reduce the density. In other words, the dielectric constant can be reduced, and the high frequency characteristics of the resin composition are easily improved. In addition, when component (A) has structure (c), the flexibility of the resin composition is improved, and it is possible to increase the handleability (tackiness, cracking, powder fall, etc.) and strength of the adhesive layer (resin film) produced from the resin composition.

[0032] Examples of the structure (c) include alkylene groups such as a nonylene group, a decylene group, an undecylene group, a dodecylene group, a tetradecylene group, a hexadecylene group, an octadecylene group, and a nonadecylene group; arylene groups such as a benzylene group, a phenylene group, and a naphthylene group; arylene alkylene groups such as a phenylenemethylene group, a phenyleneethylene group, a benzylpropylene group, a naphthylenemethylene group, and a naphthyleneethylene group; and arylene dialkylene groups such as a phenylenedimethylene group and a phenylenediethylene group.

[0033] From the viewpoints of high frequency characteristics, low thermal expansion characteristics, adhesion to a conductor, heat resistance, and low moisture absorption, a group represented by the following formula (II) is particularly preferred as the structure (c).

[0034] [ka]

[0035] In formula (II), R2 and R3 each independently represent an alkylene group having 4 to 50 carbon atoms. From the viewpoint of further improving flexibility and ease of synthesis, R2 and R3 each independently represent an alkylene group having 5 to 25 carbon atoms, more preferably an alkylene group having 6 to 10 carbon atoms, and further preferably an alkylene group having 7 to 10 carbon atoms.

[0036] In formula (II), R4 represents an alkyl group having 4 to 50 carbon atoms. From the viewpoint of further improving flexibility and ease of synthesis, R4 is preferably an alkyl group having 5 to 25 carbon atoms, more preferably an alkyl group having 6 to 10 carbon atoms, and further preferably an alkyl group having 7 to 10 carbon atoms.

[0037] In formula (II), R5 represents an alkyl group having 2 to 50 carbon atoms. From the viewpoint of further improving flexibility and ease of synthesis, R5 is preferably an alkyl group having 3 to 25 carbon atoms, more preferably an alkyl group having 4 to 10 carbon atoms, and further preferably an alkyl group having 5 to 8 carbon atoms.

[0038] From the viewpoint of fluidity and circuit embedding property, it is preferable that a plurality of structures (c) are present in the (A) component. In this case, the structures (c) may be the same or different. For example, it is preferable that 2 to 40 structures (c) are present in the (A) component, more preferably 2 to 20 structures (c), and even more preferably 2 to 10 structures (c).

[0039] The content of the (A) component in the resin composition is not particularly limited. From the viewpoint of heat resistance, the content of the (A) component is preferably 2 to 98 mass % based on the total mass of the resin composition, more preferably 10 to 50 mass %, and further preferably 10 to 30 mass %.

[0040] The molecular weight of the (A) component is not particularly limited. From the viewpoints of handling, flowability, and circuit embedding properties, the weight average molecular weight (Mw) of the (A) component is preferably 500 to 10,000, more preferably 1,000 to 9,000, even more preferably 1,500 to 9,000, even more preferably 1,500 to 7,000, and particularly preferably 1,700 to 5,000.

[0041] The Mw of the component (A) can be measured by gel permeation chromatography (GPC).

[0042] The GPC measurement conditions are as follows. Pump: L-6200 type [manufactured by Hitachi High-Technologies Corporation] Detector: L-3300 type RI [Hitachi High-Technologies Corporation] Column oven: L-655A-52 [Hitachi High-Technologies Corporation] Guard column and column: TSK Guardcolumn HHR-L + TSKgel G4000HHR + TSKgel G2000HHR [all manufactured by Tosoh Corporation, product names] Column size: 6.0 x 40 mm (guard column), 7.8 x 300 mm (column) Eluent: Tetrahydrofuran Sample concentration: 30mg / 5mL Injection volume: 20μL Flow rate: 1.00mL / min Measurement temperature: 40℃

[0043] There are no limitations on the method for producing component (A). Component (A) may be produced, for example, by reacting an acid anhydride with a diamine to synthesize an amine-terminated compound, and then reacting the amine-terminated compound with an excess of maleic anhydride.

[0044] Examples of the acid anhydride include pyromellitic anhydride, maleic anhydride, succinic anhydride, 3,3',4,4'-benzophenonetetracarboxylic dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, and 3,3',4,4'-diphenylsulfonetetracarboxylic dianhydride. The acid anhydride may be used alone or in combination of two or more types according to the purpose, application, etc. As described above, a tetravalent organic group derived from the acid anhydride listed above can be used as R1 in the above formula (I). From the standpoint of better dielectric properties, the acid anhydride is preferably pyromellitic anhydride.

[0045] Examples of diamines include dimer diamine, 2,2-bis(4-(4-aminophenoxy)phenyl)propane, 1,3-bis(4-aminophenoxy)benzene, 4,4'-bis(4-aminophenoxy)biphenyl, 4,4'-diamino-3,3'-dihydroxybiphenyl, 1,3-bis[2-(4-aminophenyl)-2-propyl]benzene, 1,4-bis[2-(4-aminophenyl)-2-propyl]benzene, polyoxyalkylene diamine, and [3,4-bis(1-aminoheptyl)-6-hexyl-5-(1-octenyl)]cyclohexene. Depending on the purpose, application, etc., one type of diamine may be used alone, or two or more types may be used in combination.

[0046] The component (A) may be, for example, a compound represented by the following formula (XIII).

[0047] [ka]

[0048] In the formula, R and Q each independently represent a divalent organic group. R can be the same as in the above-mentioned structure (c), and Q can be the same as the above-mentioned R1. In addition, n represents an integer of 1 to 10.

[0049] A commercially available compound can also be used as component (A). Examples of commercially available compounds include products manufactured by Designer Molecules Inc., specifically, BMI-1500, BMI-1700, BMI-3000, BMI-5000, and BMI-9000 (all trade names). From the viewpoint of obtaining better high-frequency characteristics, it is more preferable to use BMI-3000 as component (A).

[0050] ((B) Aromatic Maleimide Compound) The aromatic maleimide compound (B) according to the present embodiment may be referred to as component (B). Component (B) is a maleimide compound different from component (A). A compound that can be classified as both component (A) and component (B) is considered to belong to component (A), but when two or more compounds that can be classified as both component (A) and component (B) are included, one of them is considered to belong to component (A) and the other compounds are considered to belong to component (B). For example, a compound having an aromatic ring contained in a group represented by formula (I) may be considered as component (A), and a compound having an aromatic ring other than the aromatic ring contained in the group represented by formula (I) may be considered as component (B). By using component (B), the hygroscopicity of the resin composition can be reduced. A cured product of a resin composition containing components (A) and (B) contains a polymer having a structural unit composed of component (A) having low dielectric properties and a structural unit composed of component (B) having low hygroscopicity, and thus can improve low hygroscopicity while maintaining good dielectric properties.

[0051] The (B) component preferably has a lower thermal expansion coefficient than the (A) component. Examples of the (B) component having a lower thermal expansion coefficient than the (A) component include a maleimide group-containing compound having a lower molecular weight than the (A) component, a maleimide group-containing compound having more aromatic rings than the (A) component, and a maleimide group-containing compound having a shorter main chain than the (A) component.

[0052] The content of the (B) component in the resin composition is not particularly limited. From the viewpoint of low moisture absorption and dielectric properties, the content of the (B) component is preferably 1 to 95 mass %, more preferably 3 to 90 mass %, and further preferably 5 to 85 mass %, based on the total mass of the resin composition.

[0053] The blending ratio of the (A) component to the (B) component in the resin composition is not particularly limited. From the viewpoint of low moisture absorption and dielectric properties, the mass ratio of the (A) component to the (B) component (B) / (A) is preferably 0.01 to 3, more preferably 0.03 to 2, and even more preferably 0.05 to 1.

[0054] The (B) component is not particularly limited as long as it has an aromatic ring. Since an aromatic ring is rigid and has low thermal expansion, the thermal expansion coefficient of the resin composition can be reduced by using a (B) component having an aromatic ring. The maleimide group may be bonded to an aromatic ring or an aliphatic chain, but from the viewpoint of low thermal expansion, it is preferable that the maleimide group is bonded to an aromatic ring. In addition, the (B) component may be a polymaleimide compound containing two or more maleimide groups. The (B) component may be used alone or in combination of two or more types.

[0055] Examples of the component (B) include 1,2-dimaleimidoethane, 1,3-dimaleimidopropane, bis(4-maleimidophenyl)methane, bis(3-ethyl-4-maleimidophenyl)methane, bis(3-ethyl-5-methyl-4-maleimidophenyl)methane, 2,7-dimaleimidofluorene, N,N'-(1,3-phenylene)bismaleimide, N,N'-(1,3-(4-methylphenylene))bismaleimide, bis(4-maleimidophenyl)sulfone, bis(4-maleimidophenyl)sulfide, bis(4-maleimidophenyl)ether, 1,3-bis(3-maleimidophenoxy)benzene, 1,3-bis(3-(3-maleimidophenoxy)phenoxy)benzene, bis( 4-maleimidophenyl)ketone, 2,2-bis(4-(4-maleimidophenoxy)phenyl)propane, bis(4-(4-maleimidophenoxy)phenyl)sulfone, bis[4-(4-maleimidophenoxy)phenyl]sulfoxide, 4,4'-bis(3-maleimidophenoxy)biphenyl, 1,3-bis(2-(3-maleimidophenyl)propyl)benzene, 1,3-bis(1-(4-(3-maleimidophenoxy)phenyl)-1-propyl)benzene, bis(maleimidocyclohexyl)methane, 2,2-bis[4-(3-maleimidophenoxy)phenyl]-1,1,1,3,3,3-hexafluoropropane, and bis(maleimidophenyl)thiophene. From the viewpoint of further reducing the moisture absorption and the thermal expansion coefficient, bis(3-ethyl-5-methyl-4-maleimidophenyl)methane may be used as the component (B). From the viewpoint of further increasing the breaking strength and metal foil peel strength of the resin film formed from the resin composition, 2,2-bis(4-(4-maleimidophenoxy)phenyl)propane may be used as the component (B).

[0056] From the standpoint of moldability, a compound represented by the following formula (VI) may be used as the component (B).

[0057] [ka]

[0058] In formula (VI), A4 represents a residue represented by the following formula (VII), (VIII), (IX) or (X), and A5 represents a residue represented by the following formula (XI). From the viewpoint of low thermal expansion, A4 may be a residue represented by the following formula (VII), (VIII) or (IX).

[0059] [ka]

[0060] In formula (VII), R 10 each independently represents a hydrogen atom, an aliphatic hydrocarbon group having 1 to 5 carbon atoms, or a halogen atom.

[0061] [ka]

[0062] In formula (VIII), R 11 and R 12 each independently represents a hydrogen atom, an aliphatic hydrocarbon group having 1 to 5 carbon atoms, or a halogen atom, and A6 represents an alkylene group or alkylidene group having 1 to 5 carbon atoms, an ether group, a sulfide group, a sulfonyl group, a ketone group, a single bond, or a residue represented by the following formula (VIII-1):

[0063] [ka]

[0064] In formula (VIII-1), R 13 and R 14 each independently represents a hydrogen atom, an aliphatic hydrocarbon group having 1 to 5 carbon atoms or a halogen atom, and A7 represents an alkylene group having 1 to 5 carbon atoms, an isopropylidene group, an ether group, a sulfide group, a sulfonyl group, a ketone group or a single bond.

[0065] [ka]

[0066] In formula (IX), i is an integer of 1 to 10.

[0067] [ka]

[0068] In formula (X), R 15 and R 16 each independently represents a hydrogen atom or an aliphatic hydrocarbon group having 1 to 5 carbon atoms; and j is an integer of 1 to 8.

[0069] [ka]

[0070] In formula (XI), R 17 and R 18 each independently represents a hydrogen atom, an aliphatic hydrocarbon group having 1 to 5 carbon atoms, an alkoxy group having 1 to 5 carbon atoms, a hydroxyl group, or a halogen atom, and A8 represents an alkylene group or alkylidene group having 1 to 5 carbon atoms, an ether group, a sulfide group, a sulfonyl group, a ketone group, a fluorenylene group, a single bond, a residue represented by the following formula (XI-1) or a residue represented by the following formula (XI-2).

[0071] [ka]

[0072] In formula (XI-1), R 19 and R 20 each independently represents a hydrogen atom, an aliphatic hydrocarbon group having 1 to 5 carbon atoms, or a halogen atom, and A9 represents an alkylene group having 1 to 5 carbon atoms, an isopropylidene group, an m-phenylenediisopropylidene group, a p-phenylenediisopropylidene group, an ether group, a sulfide group, a sulfonyl group, a ketone group, or a single bond.

[0073] [ka]

[0074] In formula (XI-2), R 21 each independently represents a hydrogen atom, an aliphatic hydrocarbon group having 1 to 5 carbon atoms, or a halogen atom; A 10 and A 11 each independently represents an alkylene group having 1 to 5 carbon atoms, an isopropylidene group, an ether group, a sulfide group, a sulfonyl group, a ketone group, or a single bond.

[0075] The component (B) may be a compound having an amino group and a maleimide group from the viewpoints of solubility in an organic solvent, high frequency characteristics, high adhesion to a conductor, etc. The compound having an amino group and a maleimide group can be obtained, for example, by subjecting a bismaleimide compound to a Michael addition reaction with an aromatic diamine compound having two primary amino groups in an organic solvent.

[0076] Examples of aromatic diamine compounds include 4,4'-diaminodiphenylmethane, 4,4'-diamino-3,3'-dimethyl-diphenylmethane, 2,2'-dimethyl-4,4'-diaminobiphenyl, 2,2-bis(4-(4-aminophenoxy)phenyl)propane, 4,4'-[1,3-phenylenebis(1-methylethylidene)]bisaniline, and 4,4'-[1,4-phenylenebis(1-methylethylidene)]bisaniline. These may be used alone or in combination of two or more.

[0077] From the viewpoints of high solubility in organic solvents, high reaction rate during synthesis, and high heat resistance, the aromatic diamine compound may be 4,4'-diaminodiphenylmethane or 4,4'-diamino-3,3'-dimethyl-diphenylmethane.

[0078] Examples of organic solvents include alcohol compounds such as methanol, ethanol, butanol, butyl cellosolve, ethylene glycol monomethyl ether, and propylene glycol monomethyl ether; ketone compounds such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; aromatic hydrocarbons such as toluene, xylene, and mesitylene; ester compounds such as methoxyethyl acetate, ethoxyethyl acetate, butoxyethyl acetate, and ethyl acetate; and nitrogen-containing compounds such as N,N-dimethylformamide, N,N-dimethylacetamide, and N-methyl-2-pyrrolidone. One type of organic solvent may be used alone, or two or more types may be mixed and used. Among these, methyl ethyl ketone, cyclohexanone, propylene glycol monomethyl ether, N,N-dimethylformamide, and N,N-dimethylacetamide are preferred from the viewpoint of solubility.

[0079] (catalyst) The resin composition according to the present embodiment may further contain a catalyst for promoting the curing of the (A) component. The content of the catalyst is not particularly limited, but may be 0.1 to 5 mass% based on the total mass of the resin composition. As the catalyst, for example, peroxides, azo compounds, etc. can be used.

[0080] Examples of peroxides include dicumyl peroxide, dibenzoyl peroxide, 2-butanone peroxide, tert-butyl perbenzoate, di-tert-butyl peroxide, 2,5-dimethyl-2,5-di(t-butylperoxy)hexane, bis(tert-butylperoxyisopropyl)benzene, and tert-butyl hydroperoxide. Examples of azo compounds include 2,2'-azobis(2-methylpropanenitrile), 2,2'-azobis(2-methylbutanenitrile), and 1,1'-azobis(cyclohexanecarbonitrile).

[0081] (Inorganic filler) The resin composition according to the present embodiment may further contain an inorganic filler. By adding an appropriate inorganic filler, the adhesive layer can be improved in low thermal expansion properties, high elastic modulus, heat resistance, flame retardancy, etc. Examples of inorganic fillers include silica, alumina, titanium oxide, mica, beryllia, barium titanate, potassium titanate, strontium titanate, calcium titanate, aluminum carbonate, magnesium hydroxide, aluminum hydroxide, aluminum silicate, calcium carbonate, calcium silicate, magnesium silicate, silicon nitride, boron nitride, calcined clay, talc, aluminum borate, and silicon carbide. These may be used alone or in combination of two or more.

[0082] There is no particular restriction on the shape and particle size of the inorganic filler. The particle size of the inorganic filler may be, for example, 0.01 to 20 μm or 0.1 to 10 μm. The particle size refers to the average particle size, and is the particle size at the point corresponding to 50% volume when the cumulative frequency distribution curve of the particle size is calculated with the total volume of the particles being 100%. The average particle size can be measured by a particle size distribution measuring device using a laser diffraction scattering method.

[0083] When an inorganic filler is used, its amount is not particularly limited, but for example, the content ratio of the inorganic filler based on the total solid content in the resin composition is preferably in the range of 10 to 50 vol%, more preferably 10 to 40 vol%. When the content ratio of the inorganic filler in the resin composition is in the above range, good curability, moldability and chemical resistance are easily obtained. In this embodiment, it is important that the content of the inorganic filler is equal to or less than a certain amount, which allows the composition to maintain flexibility while taking advantage of the properties of the inorganic filler.

[0084] When an inorganic filler is used, a coupling agent can be used in combination as necessary for the purpose of improving the dispersibility of the inorganic filler and the adhesion to the organic component. As the coupling agent, a silane coupling agent, a titanate coupling agent, etc. can be used. These can be used alone or in combination of two or more. The amount of the coupling agent added can be, for example, 0.1 to 5 parts by mass or 0.5 to 3 parts by mass per 100 parts by mass of the inorganic filler used. Within this range, the deterioration of various properties is small, and the features of the inorganic filler can be easily and effectively exhibited.

[0085] When using a coupling agent, the so-called integral blending method may be used in which the inorganic filler is blended in the resin composition and then the coupling agent is added, but it is preferable to use an inorganic filler that has been surface-treated in advance by a dry or wet method with a coupling agent. By using this method, the characteristics of the inorganic filler can be more effectively expressed.

[0086] (thermosetting resin) The resin composition of this embodiment may further contain a thermosetting resin (C) (hereinafter, sometimes referred to as "component (C)") different from components (A) and (B). Compounds that may fall under component (A) or component (B) are not considered to belong to component (C). By including component (C), the low thermal expansion properties of the resin composition can be further improved. Examples of component (C) include epoxy resins and cyanate ester resins. One type of component (C) may be used alone, or two or more types may be used in combination.

[0087] Examples of epoxy resins include bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol S type epoxy resins, alicyclic epoxy resins, aliphatic chain epoxy resins, phenol novolac type epoxy resins, cresol novolac type epoxy resins, bisphenol A novolac type epoxy resins, phenol aralkyl type epoxy resins, naphthol novolac type epoxy resins, naphthol aralkyl type epoxy resins, and other naphthalene skeleton-containing epoxy resins, bifunctional biphenyl type epoxy resins, biphenyl aralkyl type epoxy resins, dicyclopentadiene type epoxy resins, and dihydroanthracene type epoxy resins. From the viewpoint of high frequency characteristics and thermal expansion characteristics, naphthalene skeleton-containing epoxy resins or biphenyl aralkyl type epoxy resins may be used.

[0088] Examples of cyanate ester resins include 2,2-bis(4-cyanatophenyl)propane, bis(4-cyanatophenyl)ethane, bis(3,5-dimethyl-4-cyanatophenyl)methane, 2,2-bis(4-cyanatophenyl)-1,1,1,3,3,3-hexafluoropropane, α,α'-bis(4-cyanatophenyl)-m-diisopropylbenzene, cyanate ester compounds of phenol-added dicyclopentadiene polymers, phenol novolac type cyanate ester compounds, and cresol novolac type cyanate ester compounds. Considering the overall balance of low cost, high frequency characteristics, and other characteristics, 2,2-bis(4-cyanatophenyl)propane may be used.

[0089] (hardening agent) When the resin composition according to the present embodiment contains the (C) component, it may further contain a curing agent for the (C) component. This allows the reaction to proceed smoothly when obtaining a cured product of the resin composition, and also allows the physical properties of the cured product of the obtained resin composition to be appropriately adjusted. The curing agent may be used alone or in combination of two or more types.

[0090] Examples of the curing agent for the epoxy resin include polyamine compounds such as diethylenetriamine, triethylenetetramine, diaminodiphenylmethane, m-phenylenediamine, and dicyandiamide; polyphenol compounds such as bisphenol A, phenol novolac resin, cresol novolac resin, bisphenol A novolac resin, and phenol aralkyl resin; acid anhydrides such as phthalic anhydride and pyromellitic anhydride; carboxylic acid compounds; and active ester compounds.

[0091] Examples of the curing agent for the cyanate ester resin include monophenol compounds, polyphenol compounds, amine compounds, alcohol compounds, acid anhydrides, and carboxylic acid compounds.

[0092] (Cure accelerator) The resin composition according to the present embodiment may further contain a curing accelerator depending on the type of component (C). Examples of the curing accelerator for the epoxy resin include imidazole-based curing accelerators, BF3 amine complexes, and phosphorus-based curing accelerators. From the viewpoints of storage stability of the resin composition, handling of the semi-cured resin composition, and solder heat resistance, imidazole-based curing accelerators and phosphorus-based curing accelerators are preferred.

[0093] (thermoplastic resin) The resin composition according to the present embodiment may further contain a thermoplastic resin from the viewpoint of improving the handling property of the resin film. The type of the thermoplastic resin is not particularly limited, and the molecular weight is also not limited, but the number average molecular weight (Mn) of the thermoplastic resin is preferably 200 to 60,000 from the viewpoint of further improving the compatibility with the (A) component.

[0094] From the viewpoint of film forming property and moisture absorption resistance, the thermoplastic resin is preferably a thermoplastic elastomer. Examples of the thermoplastic elastomer include saturated thermoplastic elastomers, and examples of the saturated thermoplastic elastomer include chemically modified saturated thermoplastic elastomers and unmodified saturated thermoplastic elastomers. Examples of the chemically modified saturated thermoplastic elastomer include styrene-ethylene-butylene copolymers modified with maleic anhydride. Specific examples of the chemically modified saturated thermoplastic elastomer include Tuftec M1911, M1913, M1943 (trade names, manufactured by Asahi Kasei Corporation). On the other hand, examples of the unmodified saturated thermoplastic elastomer include unmodified styrene-ethylene-butylene copolymers. Specific examples of the unmodified saturated thermoplastic elastomer include Tuftec H1041, H1051, H1043, H1053 (trade names, manufactured by Asahi Kasei Corporation).

[0095] From the viewpoints of film formability, dielectric properties, and moisture absorption resistance, it is more preferable that the saturated thermoplastic elastomer has a styrene unit in the molecule. In this specification, the styrene unit refers to a unit derived from a styrene monomer in a polymer, and the saturated thermoplastic elastomer refers to a structure in which the aliphatic hydrocarbon portion other than the aromatic hydrocarbon portion of the styrene unit is all constituted by a saturated bond group.

[0096] The content ratio of the styrene unit in the saturated thermoplastic elastomer is not particularly limited, but is preferably 10 to 80 mass%, more preferably 20 to 70 mass%, in terms of the mass percentage of the styrene unit relative to the total mass of the saturated thermoplastic elastomer. When the content ratio of the styrene unit is within the above range, the film appearance, heat resistance and adhesiveness tend to be excellent.

[0097] A specific example of a saturated thermoplastic elastomer having a styrene unit in the molecule is a styrene-ethylene-butylene copolymer, which can be obtained, for example, by hydrogenating the unsaturated double bonds of the structural units derived from butadiene in a styrene-butadiene copolymer.

[0098] The content of the thermoplastic resin is not particularly limited, but from the viewpoint of further improving the dielectric properties, the content may be 0.1 to 15 mass%, 0.3 to 10 mass%, or 0.5 to 5 mass% of the total solid content in the resin composition.

[0099] (Flame retardant) The resin composition according to the present embodiment may further contain a flame retardant. The flame retardant is not particularly limited, but a bromine-based flame retardant, a phosphorus-based flame retardant, a metal hydroxide, or the like is preferably used. The flame retardant may be used alone or in combination of two or more kinds.

[0100] Examples of brominated flame retardants include brominated epoxy resins such as brominated bisphenol A type epoxy resins and brominated phenol novolac type epoxy resins; brominated additive type flame retardants such as hexabromobenzene, pentabromotoluene, ethylene bis(pentabromophenyl), ethylene bistetrabromophthalimide, 1,2-dibromo-4-(1,2-dibromoethyl)cyclohexane, tetrabromocyclooctane, hexabromocyclododecane, bis(tribromophenoxy)ethane, brominated polyphenylene ether, brominated polystyrene, and 2,4,6-tris(tribromophenoxy)-1,3,5-triazine; and brominated reaction type flame retardants containing unsaturated double bond groups such as tribromophenylmaleimide, tribromophenyl acrylate, tribromophenyl methacrylate, tetrabromobisphenol A type dimethacrylate, pentabromobenzyl acrylate, and brominated styrene.

[0101] Examples of phosphorus-based flame retardants include aromatic phosphoric acid esters such as triphenyl phosphate, tricresyl phosphate, trixylenyl phosphate, cresyl diphenyl phosphate, cresyl di-2,6-xylenyl phosphate, and resorcinol bis(diphenyl phosphate); phosphonic acid esters such as divinyl phenylphosphonate, diallyl phenylphosphonate, and bis(1-butenyl) phenylphosphonate; phosphinic acid esters such as phenyl diphenylphosphinate, methyl diphenylphosphinate, and 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide derivatives; phosphazene compounds such as bis(2-allylphenoxy)phosphazene and dicresylphosphazene; and phosphorus-based flame retardants such as melamine phosphate, melamine pyrophosphate, melamine polyphosphate, melam polyphosphate, ammonium polyphosphate, phosphorus-containing vinylbenzyl compounds, and red phosphorus. Examples of metal hydroxide flame retardants include magnesium hydroxide and aluminum hydroxide.

[0102] The resin composition according to the present embodiment can be obtained by uniformly dispersing and mixing the above-mentioned components. The preparation means and conditions of the resin composition are not particularly limited. The resin composition may be prepared, for example, by thoroughly and uniformly stirring and mixing the components in a predetermined amount with a mixer or the like, kneading the mixture with a mixing roll, an extruder, a kneader, a roll, an extruder, or the like, and then cooling and pulverizing the kneaded mixture.

[0103] The dielectric constant of the cured product (cured adhesive layer) of the resin composition according to this embodiment is not particularly limited, but from the viewpoint of suitable use in the high frequency band, the dielectric constant at 10 GHz is preferably 3.6 or less, more preferably 3.1 or less, and even more preferably 3.0 or less. There is no particular limit to the lower limit of the dielectric constant, but it may be, for example, about 1.0. In addition, from the viewpoint of suitable use in the high frequency band, the dielectric loss tangent of the cured product of the resin composition is preferably 0.004 or less, more preferably 0.003 or less. There is no particular limit to the lower limit of the dielectric constant, but it may be, for example, about 0.0001. The dielectric constant and dielectric loss tangent can be measured by the method shown in the examples described later.

[0104] From the viewpoint of suppressing warping of the laminate, the thermal expansion coefficient of the cured product of the resin composition is preferably 10 to 90 ppm / ° C., more preferably 10 to 45 ppm / ° C., and even more preferably 10 to 40 ppm / ° C. The thermal expansion coefficient can be measured in accordance with IPC-TM-650 2.4.24.

[0105] The method for producing the resin film is not limited. For example, the resin film may be obtained by applying the resin composition onto a supporting substrate and drying the formed resin layer. Specifically, the resin composition may be applied onto a supporting substrate using a kiss coater, roll coater, comma coater, or the like, and then dried in a heating and drying oven or the like at a temperature of, for example, 70 to 250°C, preferably 70 to 200°C, for 1 to 30 minutes, preferably 3 to 15 minutes. This makes it possible to obtain a resin film in which the resin composition is in a semi-cured state.

[0106] The semi-cured resin film can be further heated in a heating furnace at a temperature of, for example, 170 to 250° C., preferably 185 to 230° C., for 60 to 150 minutes to thermally cure the resin film.

[0107] The thickness of the resin film is not particularly limited, and may be 0.01 to 2.0 times, 0.05 to 1.0 times, or 0.1 to 0.9 times the thickness of the fluororesin substrate. When the thickness of the resin film is 2.0 times or less, the dielectric constant of the laminate is easily reduced. When the thickness of the resin film is 0.01 times or more, the rigidity and dimensional stability of the laminate are easily improved. The thickness of the resin film may be, for example, 1 to 200 μm, 3 to 180 μm, 5 to 150 μm, 10 to 100 μm, or 15 to 80 μm.

[0108] The supporting substrate is not particularly limited, but is preferably at least one selected from the group consisting of glass, metal foil, and PET film. By providing the resin film with a supporting substrate, storage properties and handling properties when used in the production of a laminate tend to be improved.

[0109] [Fluororesin substrate] Examples of fluororesin constituting the fluororesin substrate 1 include polytetrafluoroethylene (PTFE), tetrafluoroethylene-perfluoroalkylvinylether copolymer (PFA), tetrafluoroethylene-perfluoroalkoxyethylene polymer (PFE), tetrafluoroethylene-hexafluoropropylene polymer (FEP), and tetrafluoroethylene-ethylene copolymer (ETFE).The fluororesin substrate is preferably a substrate containing polytetrafluoroethylene, since it has superior high-frequency characteristics.

[0110] The relative dielectric constant (Dk) of the fluororesin substrate may be 2.2 to 3.5 or 2.8 to 3.1. The dielectric loss tangent (Df) of the fluororesin substrate may be 0.0010 to 0.0020 or 0.0010 to 0.0013. The thermal expansion coefficient of the fluororesin substrate in the substrate direction may be 30 ppm / °C or less or 20 ppm / °C or less. Since the insulation reliability and antenna characteristics of the laminate are improved, the thickness of the fluororesin substrate may be 100 μm or more, 110 μm or more, or 120 μm or more, and may be 12700 μm or less, 6350 μm or less, or 2540 μm or less.

[0111] [Metal foil] A metal foil can be further laminated on the fluororesin substrate laminate comprising a fluororesin substrate and an adhesive layer. Fig. 2 is a schematic cross-sectional view showing one embodiment of a fluororesin substrate laminate comprising a metal foil. The laminate comprises a fluororesin substrate 1, an adhesive layer 2 provided on the fluororesin substrate 1, and a metal foil 4 laminated on the adhesive layer 2. The fluororesin substrate 1 and the metal foil 4 are bonded via the adhesive layer 2.

[0112] As the metal foil according to the present embodiment, a metal foil having a small surface roughness (low-roughening metal foil) can be used. The surface roughness (Rz) of the metal foil may be 0.05 to 2 μm, 0.1 to 1.5 μm, or 0.15 to 1 μm. The thickness of the metal foil may be 5 to 105 μm, 8 to 70 μm, 10 to 40 μm, or 10 to 20 μm. As the metal foil, an electrolytic copper foil may be used from the viewpoint of peel strength.

[0113] The fluororesin substrate laminate including the metal foil may be produced by forming an adhesive layer 2 on a fluororesin substrate 1 and then laminating the metal foil 4 on the adhesive layer 2, or may be produced by laminating the fluororesin substrate 1, a resin film, and the metal foil 4 in this order. The fluororesin substrate laminate according to this embodiment may be a laminate in which adhesive layers 2 are formed on both sides of a fluororesin substrate 1 and a metal foil 4 is laminated on the adhesive layer 2. The fluororesin substrate laminate may have a relative dielectric constant (Dk) of 2.2 to 3.5 or 2.8 to 3.1. The dielectric loss tangent (Df) may be 0.0013 to 0.0023 or 0.0013 to 0.0016. The transmission loss at 24 GHz may be -0.30 to -0.10 dB / cm or -0.20 to -0.10 dB / cm.

[0114] <Laminated plate> According to this embodiment, a metal-clad laminate can be produced by providing a laminate having a resin layer containing a cured product of a resin composition and a conductor layer.

[0115] The method for producing the metal-clad laminate is not limited. For example, one or more of the above-mentioned resin films are laminated on both sides of a fluororesin substrate, a metal foil that will be a conductor layer is arranged on at least one side, and the metal-clad laminate having a metal foil on at least one side of a resin layer that will be an insulating layer is obtained by, for example, heating and pressing at a temperature of 170 to 250°C, preferably 185 to 230°C, and a pressure of 0.5 to 5.0 MPa for 60 to 150 minutes. Heating and pressing can be performed, for example, under conditions of a vacuum degree of 10 kPa or less, preferably 5 kPa or less, and is preferably performed in a vacuum from the viewpoint of increasing efficiency. Heating and pressing are preferably performed from the start to the end of molding for 30 minutes. The metal-clad laminate may be produced by placing a metal foil 4 on the adhesive layer 2 of a fluororesin substrate having a fluororesin substrate 1 and an adhesive layer 2, and heating and pressing the fluororesin substrate.

[0116] Although the preferred embodiments of the present invention have been described above, these are merely examples for the purpose of explaining the present invention, and the scope of the present invention is not limited to these embodiments. The present invention can be embodied in various forms different from the above-described embodiments without departing from the gist of the present invention. EXAMPLES

[0117] The present invention will be described in more detail below with reference to examples and comparative examples, although the present invention is not limited to the following examples.

[0118] [Resin composition] Example 1 Into a vessel equipped with a stirrer, 14 g of silica slurry (manufactured by Admatechs Co., Ltd., product name "SC-2050KNK"), 106.6 g of toluene, 67.4 g of component (A), 9.0 g of component (B), and 1.9 g of catalyst (di(2-t-butylperoxyisopropyl)benzene, manufactured by NOF Corporation, product name "Perbutyl P") were charged and mixed by stirring for 1 hour at 25° C. The mixture was filtered using a #200 nylon mesh to obtain a resin composition. Example 2 In the same manner as in Example 1, a resin composition was obtained by adding silica slurry so that the amount was 30 vol % based on the total solid content in the resin composition. Example 3 In the same manner as in Example 1, a resin composition was obtained by adding silica slurry so that the amount was 40 vol % based on the total solid content in the resin composition. Example 4 In the same manner as in Example 1, a resin composition was obtained by adding silica slurry so that the amount was 50 vol % based on the total solid content in the resin composition.

[0119] Comparative Example 1 A resin composition was obtained in the same manner as in Example 1, except that the silica slurry was not used. Comparative Example 2 In the same manner as in Example 1, a resin composition was obtained by adding silica slurry so that the amount was 60 vol % based on the total solid content in the resin composition. Comparative Example 3 The fluororesin substrate does not use a resin film made of the above resin composition.

[0120] Component (A): A maleimide compound having a structure represented by the following formula (XII-3) (manufactured by Designer Molecules Inc., product name "BMI-1500") was used as component (A).

[0121] [ka]

[0122] Component (B): 2,2-bis(4-(4-maleimidophenoxy)phenylpropane (manufactured by Daiwa Chemical Industry Co., Ltd., product name "BMI-4000"), which is an aromatic maleimide compound, was used as component (B).

[0123] [Resin film] The resin composition was applied onto a PET film (manufactured by Teijin Limited, product name "G2-38", thickness: 38 μm) using a comma coater, and then dried at 130° C. to produce a resin film with a PET film having a semi-cured resin layer. The thickness of the resin film (adhesive layer) was 5 μm.

[0124] [Laminate] A resin film from which the PET film had been peeled off was placed on both sides of a high-frequency PTFE substrate (manufactured by Rogers, product name "RO3003", thickness: 127μm) with the copper foil on both sides etched completely. Copper foil (manufactured by Furukawa Electric Co., Ltd., product name "FZ-WS", thickness: 18μm, surface roughness (Rz: 0.2μm or less) was then laminated. Next, a plate was placed on top of the laminate, and it was heated and pressure molded under press conditions of 200℃ / 3.0MPa / 70min to produce a double-sided metal-clad laminate.

[0125] [evaluation] The double-sided metal-clad laminate and the high-frequency PTFE substrate were evaluated as follows. The results are shown in Table 1.

[0126] (Dielectric properties) The dielectric properties, namely, the relative permittivity (Dk) and the dielectric loss tangent (Df), were measured by the cavity resonator perturbation method using test pieces made by etching the outer copper foil of double-sided metal-clad laminates at a frequency of 10 GHz and a temperature of 25°C.

[0127] (Transmission loss) The copper foil on one side of the double-sided metal-clad laminate produced in Example 1 was etched to produce a microstrip line 10 cm long and 65 μm wide, and the transmission loss was measured under conditions of impedance 50 Ω, temperature 25° C., and humidity 60%. As Comparative Example 4, a high-frequency PTFE substrate (manufactured by Rogers, product name "RO3003", thickness: 127 μm) was used and the transmission loss was measured in the same manner.

[0128] (flexibility) A test specimen was prepared by etching the copper foils on both sides of the double-sided metal-clad laminate prepared in Example 1, and a mandrel test (based on JIS K 5600-5-1:1999) was performed using a bending tester (product name "Mandrel Bending Tester", manufactured by Yoshimitsu Seiki Co., Ltd.) That is, at room temperature (25°C), the test specimen was placed horizontally on a flat surface and stretched out, and then folded 180° at the center of the test specimen so that the bending radius was 2 mm or 1 mm, and then stretched again and returned to the original state. This operation was counted as one set, and the number of sets in which no cracks occurred in the test specimen was used as an index of flexibility.

[0129] [Table 1]

[0130] As is clear from the results in Table 1, it was confirmed that the resin films of Examples 1 to 4 could be produced without any problem in terms of film appearance and flexibility. In addition, it was confirmed that the dielectric properties shown in Dk, Df, and transmission loss were excellent.

[0131] As is clear from the results in Table 1, according to the resin films of Comparative Examples 1 to 3, it was confirmed that the film appearance was poor, although there was no problem with the flexibility, in Comparative Example 1. It was confirmed that the dielectric properties were not a problem, but the flexibility was poor in Comparative Example 2. From these results, it was confirmed that it is useful to specify an appropriate amount of inorganic filler for a resin film that shows flexibility and excellent dielectric properties. [Explanation of symbols]

[0132] 1: Fluorine resin substrate 2: Adhesive layer 4: Metal foil

Claims

1. A fluororesin substrate and an adhesive layer provided on the fluororesin substrate, a fluororesin substrate laminate for high frequency circuits, wherein the adhesive layer comprises a resin composition containing (A) a maleimide compound having a saturated or unsaturated divalent hydrocarbon group, (B) an aromatic maleimide compound, and an inorganic filler, and the content of the inorganic filler is in the range of 10 to 50 vol % with respect to the total amount of solids in the resin composition.

2. 2. The fluororesin substrate laminate for high frequency circuits according to claim 1, wherein the content of said inorganic filler is 10 to 40 vol %.

3. 3. The fluororesin substrate laminate according to claim 1, wherein the fluororesin substrate is a substrate containing polytetrafluoroethylene.

4. The fluororesin substrate laminate according to any one of claims 1 to 3, wherein the aromatic maleimide compound (B) has a structure in which a maleimide group is bonded to an aromatic ring.

5. 5. The fluororesin substrate laminate according to claim 1, wherein the saturated or unsaturated divalent hydrocarbon group has 8 to 100 carbon atoms.

6. The fluororesin substrate laminate according to any one of claims 1 to 5, wherein the saturated or unsaturated divalent hydrocarbon group is a group represented by the following formula (II): 【Chemistry 1】 [In formula (II), R 2 and R 3 each independently represents an alkylene group having 4 to 50 carbon atoms; R 4 represents an alkyl group having 4 to 50 carbon atoms; R 5 represents an alkyl group having 2 to 50 carbon atoms.

7. The fluororesin substrate laminate according to any one of claims 1 to 6, wherein the (A) maleimide compound having a saturated or unsaturated divalent hydrocarbon group further has a divalent group having at least two imide bonds.

8. 8. The fluororesin substrate laminate according to claim 7, wherein the divalent group having at least two imide bonds is a group represented by the following formula (I): 【Chemistry 2】 [In formula (I), R 1 represents a tetravalent organic group.

9. 9. The fluororesin substrate laminate according to claim 1, wherein the weight average molecular weight of the (A) maleimide compound having a saturated or unsaturated divalent hydrocarbon group is 500 to 10,000.

10. A fluororesin substrate laminate described in any one of claims 1 to 9, further comprising a metal foil laminated on the adhesive layer, the metal foil having a surface roughness (Rz) of 0.05 to 2 μm.

Citation Information

Patent Citations

  • JP1981114576U

  • Laminated board and its molding method

    JP1983069046A

  • Manufacture of dielectric sheet for circuit board

    JP1993183267A

  • Fluorine resin substrate

    JP2003171480A

  • Resin composition, prepreg, laminate, resin sheet, printed wiring board and semiconductor device

    JP2012255059A