Manufacturing method of alloy powder for RTB sintered magnets and jet mill grinding system

By controlling the retention weight and rotation speed of the classification rotor in jet mill pulverizers, the method enhances pulverization efficiency and maintains fine particle sizes for R-T-B sintered magnets, addressing the inefficiencies in existing technologies.

JP7567319B2Active Publication Date: 2024-10-16PROTERIAL MAGNETICS CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020159620
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-03-27
Filing Date
2020-09-24
Publication Date
2024-10-16
Estimated Expiration
2040-09-24

AI Technical Summary

Technical Problem

Existing jet mill pulverizers face challenges in maintaining consistent particle size distribution and efficiency when producing fine powders for R-T-B sintered magnets, particularly as the target particle size decreases to 4 μm or less, leading to decreased pulverization efficiency.

Method used

The method involves controlling both the weight of powder retained in the jet mill and the rotation speed of the classification rotor, adjusting the rotor speed based on measured or estimated powder weight to maintain a higher powder concentration, promoting collisions and reducing the rotation speed to enhance pulverization efficiency without increasing particle size.

Benefits of technology

This approach improves grinding efficiency while maintaining fine particle sizes, allowing for the production of R-T-B sintered magnet powders with desired particle distributions and enhanced pulverization rates.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007567319000003
    Figure 0007567319000003
  • Figure 0007567319000004
    Figure 0007567319000004
  • Figure 0007567319000005
    Figure 0007567319000005
Patent Text Reader

Abstract

To improve pulverization efficiency by jet mill pulverization.SOLUTION: A method for producing an alloy powder for R-T-B-based sintered magnet of the present disclosure comprises: a step of supplying coarsely pulverized powder of alloy for R-T-B-based sintered magnet (R is at least one of the rare earth elements and always includes at least one of Nd and Pr, T is at least one of the transition metal elements and always includes Fe. B is boron.) into a jet-mill pulverizing device comprising a classification rotor; and a pulverization step of forming finely pulverized powder by pulverizing coarsely pulverized powder inside the jet-mill pulverizing device and discharging the finely pulverized powder by the classification rotor, in the pulverization step, both of a weight of powder retained inside the jet-mill pulverizing device and a rotation speed of the classification rotor are controlled.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present application relates to a method for producing alloy powder for RTB sintered magnets and a jet mill grinding system. [Background technology]

[0002] RTB sintered magnets (R is at least one rare earth element and must contain at least one of Nd and Pr, T is at least one transition metal element and must contain Fe, and B is boron) are represented by the formula RFe 14 It is composed of a main phase of a compound with a B-type crystal structure, a grain boundary phase located at the grain boundaries of this main phase, and a compound phase formed by the influence of trace added elements and impurities, and is known as the most high-performance magnet among permanent magnets.For this reason, RTB sintered magnets are used in a wide variety of applications, such as motors for electric vehicles (EV, HV, PHV), voice coil motors (VCM) for hard disk drives, motors for industrial equipment, and various other motors and home appliances.

[0003] Such an RTB based sintered magnet is manufactured, for example, through the steps of preparing a raw alloy powder, press-molding the raw alloy powder to produce a powder compact, and sintering the powder compact. The raw alloy powder is prepared, for example, by the following method.

[0004] First, a raw alloy is produced from molten metals of various raw metals by an ingot method, strip casting method, or the like. The obtained raw alloy is subjected to a pulverization process to obtain an alloy powder having a predetermined particle size distribution. This pulverization process usually includes a coarse pulverization process and a fine pulverization process, the former of which is carried out, for example, by mechanical pulverization or by utilizing the hydrogen embrittlement phenomenon, and the latter of which is carried out, for example, by using an airflow pulverizer (jet mill pulverizer).

[0005] Patent Document 1 discloses a jet mill grinding device that sets the supply amount of material to be ground (coarsely ground powder) so that a constant amount of material remains in the grinding chamber in order to suppress fluctuations in particle size distribution after grinding. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2000-317339 A Summary of the Invention [Problem to be solved by the invention]

[0007] In the jet mill grinding device, the materials to be ground are fed into the grinding chamber from the raw material feeder, and are crushed by collision with each other due to the high-speed inert gas sprayed from the grinding nozzle. The powder particles in the grinding chamber are finely ground, then removed via a classifying rotor and collected in a recovery tank. In order to ensure that the particle size distribution of the finely ground powder recovered is the same, it is necessary to keep the grinding conditions in the grinding chamber constant.

[0008] Conventionally, it has been considered necessary to maintain a constant weight of the material to be ground in the jet mill grinding device in order to keep the grinding conditions constant. Based on such common technical knowledge, Patent Document 1 discloses a configuration for measuring and managing the weight of the material to be ground remaining in the jet mill grinding device in order to prevent fluctuations in the particle size distribution of the powder.

[0009] Jet mill pulverizers are suitable for efficiently performing fine pulverization, but the pulverization efficiency decreases as the target particle size becomes smaller. In recent years, in order to further improve the performance of RTB sintered magnets, there has been a growing demand for fine powders with an average particle size (median diameter) of 4 μm or less as raw alloy powders. For this reason, there has been a demand for a method of improving the pulverization efficiency of jet mill pulverizers that can accommodate the miniaturization of powder. The embodiments of the present disclosure provide a manufacturing method and a pulverization system for RTB sintered magnets that solves these problems. [Means for solving the problem]

[0010] In an embodiment, the manufacturing method of alloy powder for RTB-based sintered magnets disclosed herein includes a step of supplying coarsely pulverized powder of an alloy for RTB-based sintered magnets to a jet mill crushing device equipped with a classifying rotor, and a crushing step of crushing the coarsely pulverized powder inside the jet mill crushing device to form finely pulverized powder and discharging the finely pulverized powder by the classifying rotor, wherein both the weight of powder retained inside the jet mill crushing device and the rotational speed of the classifying rotor are controlled during the crushing step.

[0011] In one embodiment, the control is performed by changing the rotation speed of the classifying rotor in response to a measured or estimated weight of the retained powder during the pulverization step.

[0012] In one embodiment, the control involves decreasing the rotation speed of the classifying rotor while increasing the amount of retained powder.

[0013] In one embodiment, the grinding step includes a step of grinding in a state where a measured or estimated value of the weight of retained powder inside the jet mill grinding device becomes a first retained powder weight, and a step of grinding in a state where the measured or estimated value of the weight of retained powder becomes a second retained powder weight that is in a range of 1.05 to 3 times the first retained powder weight, and in the step of grinding in a state where the measured or estimated value of the weight of retained powder becomes the second retained powder weight, the rotation speed of the classifying rotor is set according to the measured or estimated value of the weight of retained powder.

[0014] In one embodiment, when the rotation speed of the classifying rotor in the process of performing pulverization in a state in which the measured or estimated value of the retained powder weight becomes the first retained powder weight is taken as 100%, the rotation speed of the classifying rotor in the process of performing pulverization in a state in which the measured or estimated value of the retained powder weight becomes the second retained powder weight is set in the range of 70% or more and 97% or less.

[0015] In one embodiment, the method further includes a step of pre-supplying the coarsely pulverized powder into the inside of the jet mill pulverizing apparatus before the start of the pulverizing step.

[0016] In an embodiment, the jet mill grinding system of the present disclosure includes a jet mill grinding device, a supply device connected to the jet mill grinding device and supplying coarsely ground powder of an alloy for an RTB-based sintered magnet to the jet mill grinding device, a classifying rotor connected to the jet mill grinding device, and a control device for controlling the classifying rotor, and the rotation speed of the classifying rotor is set in accordance with a measured or estimated weight of powder retained inside the jet mill grinding device. Effect of the Invention

[0017] According to the embodiments of the present disclosure, there is provided a method for producing alloy powder for RTB sintered magnets and a jet mill grinding system that can improve the grinding efficiency without increasing the particle size of the finely pulverized powder in a jet mill grinding device. [Brief description of the drawings]

[0018] [Figure 1] FIG. 1 is a block diagram showing an example of the configuration of a jet mill pulverization system 1000 according to this embodiment. [Diagram 2] FIG. 2 is a diagram showing an example of the configuration of a jet mill grinding device 100 that can be used in the jet mill grinding system 1000 of this embodiment. [Diagram 3] FIG. 3 is a schematic diagram showing how coarsely pulverized powder 60 is supplied to the jet mill pulverizing apparatus 100 and pulverized therein. [Figure 4] FIG. 4 is a diagram showing a schematic diagram of the classifying rotor 120 rotating at a rotational speed VR. [Diagram 5] FIG. 5 is a histogram showing a schematic diagram of the particle size distribution of the powder before, during, and after pulverization. [Figure 6] FIG. 6 is a diagram showing a schematic configuration example of a jet mill grinding system 1000 according to this embodiment. [Figure 7] FIG. 7 is a graph showing the particle size distribution of the finely pulverized powder in the examples of the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] First, an embodiment of a jet mill grinding system used in the manufacturing method of the RTB sintered magnet of the present disclosure will be described. Note that in this embodiment, a jet mill grinding system having a grinding mechanism with a collision plate is described, but other jet mill grinding systems include fluidized bed grinding systems that mainly grind powders by collision between powders, and these fluidized bed jet mill systems can also be used as long as they have a classification rotor for particle size classification.

[0020] FIG. 1 is a block diagram showing an example of the configuration of a jet mill pulverization system 1000 according to this embodiment.

[0021] The jet mill grinding system 1000 includes a jet mill grinding device 100, a supply device 110 connected to the jet mill grinding device 100, a classifying rotor 120 connected to the jet mill grinding device 100, and a control device 130 that sets the rotation speed of the classifying rotor 120.

[0022] The supply device 110 supplies the jet mill pulverizer 100 with coarsely pulverized powder (material to be pulverized) of an alloy for RTB sintered magnets. The supply device 110 may have any configuration, and various known devices may be used. As described below, the control device 130 is preferably configured to variably set the rotation speed of the classifying rotor 120 based on a measured or estimated weight of powder retained inside the jet mill pulverizer 100. The control device 130 may be configured to control the operation of the supply device 110 and the jet mill pulverizer 100 to adjust the supply rate of the material to be pulverized and the flow rate of the pulverization gas, etc. The operation of the control device 130 will be described in detail below.

[0023] Fig. 2 is a diagram showing an example of the configuration of a jet mill grinding apparatus 100 that can be used in the jet mill grinding system 1000 of this embodiment. For reference, an XYZ coordinate system including an X-axis, a Y-axis, and a Z-axis that are orthogonal to each other is shown in Fig. 2. In the example of Fig. 2, the Z-axis is oriented in the vertical direction.

[0024] The jet mill grinding device 100 in the example of FIG. 2 includes a grinding chamber (grinding chamber) 10 in which grinding is performed, a raw material inlet 20 for receiving a supply of coarsely ground powder, an inner cylinder 30 surrounding the center axis of the grinding chamber 10, an impact plate 40 disposed inside the inner cylinder 30, and a grinding nozzle 50 for spraying grinding gas onto the impact plate 40 from below. The arrows drawn inside the grinding chamber 10 in FIG. 2 show the flow of the grinding gas. The impact plate 40 is attached to a support 42 fixed to the grinding chamber 10, for example. The inner cylinder 30 and the impact plate 40 are formed from a material having high hardness and abrasion resistance to withstand collision by the material to be ground, and may be formed from, for example, zirconium.

[0025] The lower and upper ends of the inner cylinder 30 are open, and the classifying rotor 120 is provided above the inner cylinder 30. The classifying rotor 120 is supported rotatably around a horizontal axis (parallel to the X-axis) and can rotate at a desired rotation speed by obtaining a driving force from a motor (not shown). The classifying rotor 120 has a generally cylindrical structure, and a plurality of slits (openings) extending in a direction parallel to the axis of rotation are arranged along the circumferential direction on the peripheral surface. The pulverization gas ejected from the pulverization nozzle 50 into the pulverization chamber 10 can pass through the slits of the classifying rotor 120 and exit from the outlet 122 to the outside. The installation direction of the classifying rotor may be parallel to the Y-axis. In the example shown in the figure, the classifying rotor 120 is built into the jet mill pulverization device 100, but the position of the classifying rotor 120 in the embodiment of the present disclosure is not limited to this example. The classifying rotor 120 may be arranged outside the pulverization chamber 10, and the classifying rotor 120 and the pulverization chamber 10 may be connected by a pipe or the like.

[0026] 3 is a schematic diagram showing how coarsely pulverized powder 60 is supplied to and pulverized inside the jet mill pulverizer 100. In the present disclosure, the powder undergoing pulverization inside the jet mill pulverizer 100 during the pulverization process is referred to as "retained powder" and its weight is referred to as "retained powder weight."

[0027] Inside the jet mill crushing device 100, crushing progresses through collisions between powder particles and the inner wall surface of the device. In the example of Fig. 3, the inner cylinder 30 and the collision plate 40 are provided, so that the area of ​​the inner wall surface of the device against which the powder particles collide is enlarged. The powder particles can be crushed further finely by colliding with the inner cylinder 30 and the collision plate 40.

[0028] The classifying rotor 120 is a device that performs classification by selectively moving to the outside a portion of the powder particles that have been sufficiently finely ground and are floating or moving inside the grinding chamber 10. The slits in the rotating classifying rotor 120 allow relatively fine particles to pass through among the powder particles approaching the classifying rotor 120, while pushing back relatively large particles. As a result, the relatively large particles circulate inside the grinding chamber 10 and are repeatedly ground until they are ground to a size equal to or smaller than a predetermined particle size.

[0029] Figure 4 shows the rotation speed V R FIG. 1 is a schematic diagram of a classifying rotor 120 rotating at a rotation speed V R is expressed as the number of rotations per unit time, for example, the number of rotations per minute (rpm: Revolutions Per Minute). The classifying rotor 120 has a number of slits 120S arranged in the circumferential direction and a number of blades 120W that partition each slit 120S. As the classifying rotor 120 rotates, centrifugal force toward the outside in the radial direction is generated in each slit 120S sandwiched between adjacent blades 120W. For this reason, the moving speed C R The powder particles 60P entering the slits 120S of the classifying rotor 120 have a peripheral velocity C S The centrifugal force F is proportional to the product of the square of and the mass of the powder particles 60P. C Therefore, larger and heavier particles are subjected to a larger centrifugal force F C As a result, it becomes difficult for the air to pass through the slit 120S.

[0030] When the radius of the classifying rotor 120 is r, the particle size (diameter) of the powder particle 60P is d, and the density is ρ, the mass of the powder particle 60P is (π / 6) d 3Therefore, the centrifugal force F acting on the powder particle 60P is C is (π / 6) d 3 ρ(C S ) 2 / r.

[0031] On the other hand, the force of the grinding gas flowing into the slit 120S (thrust force F R ) is 3π d μ C where μ is the viscosity of the grinding gas. R It is expressed as the moving speed C R is proportional to the flow rate Q of the grinding gas divided by the total opening area of ​​the classifying rotor 120. Therefore, by adjusting the flow rate Q of the grinding gas, the moving speed C R It is possible to control the

[0032] Centrifugal force F C and the thrust F R The particle size d of the powder particle 60P when the balance is reached is F C =F C The particle size at this time is the theoretically calculated classification diameter D t Then, D t =((C R ) 1 / 2 / C S )·(18μ·r / ρ) 1 / 2 In other words, the particle size is the theoretically calculated classification diameter D t For powder particles 60P, the centrifugal force F is equal to C and the driving force of the grinding gas F R On the other hand, the particle size is the theoretically calculated classification diameter D t For powder particles smaller than 60P, the centrifugal force F C is the driving force of the grinding gas F R As a result, the particle size becomes smaller than the theoretically calculated classification diameter D t Powder particles 60P smaller than the theoretically calculated classification diameter D t The powder particles 60P are driven by the driving force F of the grinding gas. R is the centrifugal force F CAs a result, the powder particles 60P of such a size cannot pass through the classifying rotor 120 and circulate or remain inside the grinding chamber 10, and further grinding will result in the theoretically calculated classification diameter D t before passing through the classifying rotor 120 and exiting the discharge port 122.

[0033] FIG. 5 is a histogram showing the particle size distribution of the powder before, during, and after pulverization. The horizontal axis of the histogram is the particle size (diameter of the powder particles), and the vertical axis is the frequency. For reference, FIG. 5 also shows the theoretically calculated classification diameter D t The particle size corresponding to is indicated by a dashed line. In Fig. 5, (a) shows the particle size distribution of the raw alloy (coarsely pulverized powder) before pulverization, (b) shows the particle size distribution of the powder remaining in the pulverization chamber during pulverization, and (c) shows the particle size distribution of the powder (fine powder) that has passed through the classifying rotor 120 and exited from the discharge port 122. These particle size distributions can be obtained by a particle size distribution measurement method that uses the diffraction and scattering phenomenon of He-Ne laser light, for example.

[0034] When the material to be pulverized (coarsely pulverized powder) having a particle size distribution as shown in FIG. 5(a) is supplied to the pulverization chamber 10 from the raw material inlet 20 of the jet mill pulverization apparatus 100 shown in FIG. 3, the particle size distribution of the powder (retained powder) present inside the pulverization chamber 10 immediately after the start of the pulverization process is the distribution shown in FIG. 5(a). After the start of the pulverization process, as the pulverization process progresses, the powder particles are pulverized and become smaller, so that particles with relatively large particle sizes decrease and particles with relatively small particle sizes increase. When the pulverization process is steadily progressing, retained powder having a particle size distribution as shown in FIG. 5(b) exists inside the pulverization chamber 10, and the theoretically calculated classification diameter D t The powder particles that are ground smaller than 100 mm can be collected through the classifying rotor 120 .

[0035] During the pulverization process, when the pulverization state is substantially steady, the weight of the powder (finely pulverized powder) discharged from the classifying rotor 120 is balanced with the weight of the material to be pulverized (coarsely pulverized powder) supplied from the raw material inlet 20 to the inside of the pulverization chamber 10. More specifically, while the steady pulverization process is being performed, the weight of the coarsely pulverized powder supplied from the raw material inlet 20 per unit time (supply amount or supply rate) is controlled to match the weight of the finely pulverized powder discharged from the outlet 122 per unit time (pulverized amount or pulverization rate). When the steady state is maintained, the weight of the powder present inside the jet mill pulverization device 100 (amount of retained powder) shows an almost constant value.

[0036] Conventionally, in order to reduce the particle size of the fine powder to be collected, the rotation speed of the classification rotor is set to a higher value to make it difficult for coarse powder particles to pass through the classification rotor. t =((C R ) 1 / 2 / C S )·(18μ·r / ρ) 1 / 2 As is clear from the equation, the peripheral speed of the classifying rotor C S The larger the theoretical classification diameter D t This means that in order to reduce the particle size of the finely pulverized powder to be recovered, the rotation speed V of the classifying rotor must be R This means that it is essential to increase the recovery rate, and it has been thought that a decrease in the recovery rate, i.e., the crushing efficiency, is unavoidable as a result.

[0037] In addition, conventionally, when the classifying rotor is rotated at high speed, the recovery rate decreases, so the amount of coarsely pulverized powder supplied to the jet mill pulverizer is set to be small. This is because when the amount of powder (finely pulverized powder) recovered per unit time is small, if the amount of powder to be pulverized per unit time is not reduced, the amount of powder remaining in the pulverizing chamber will increase rapidly, and the pulverizer will have to be stopped immediately.

[0038] However, according to the research of the inventor, it was found that by maintaining a larger amount of powder remaining in the grinding chamber than before, the powder particles are pushed to collide with each other, which has the effect of reducing the particle size of the finely ground powder. At the same time, even if the flow rate Q is the same, the amount of finely ground powder to be moved also increases, so the powder movement speed C R Therefore, even if the rotation speed of the classifying rotor is reduced, the theoretically calculated classification diameter D t It was also found that the effect of increasing the amount of powder discharged through the classifying rotor can be achieved without changing the rotation speed of the classifying rotor. According to this method, it is possible to achieve fine powder even if the rotation speed of the classifying rotor is set low. In addition, since this effect is related only to the flow rate, which depends on the specific gravity of the grinding gas, it can be achieved regardless of the type of grinding gas, even if high purity nitrogen, argon, helium, etc. are used, and high grinding efficiency can be achieved.

[0039] FIG. 6 is a diagram showing a schematic configuration example of the jet mill grinding system 1000 in this embodiment. In this example, the jet mill grinding system 1000 includes the jet mill grinding device 100 described above, a cyclone collector 200 connected to the discharge port 122, and a bag filter device 300 connected to the outlet pipe 240 of the cyclone collector 200. A leg 420 is fixed to the jet mill grinding device 100, and the leg 400 is placed on a base 440 via a weight sensor 430 such as a load cell. The weight sensor 430 detects the weight or weight fluctuation of the jet mill grinding device 100, thereby measuring the weight of the retained powder. The jet mill grinding device 100 is connected to devices, wiring, or pipes such as the supply device 110, the control device 130, and the cyclone collector 200, but because the connections are made via flexible members such as flexible pipes, the weight sensor 430 can measure the weight fluctuation of the jet mill grinding device 100 without being affected by other devices. The weight of the jet mill pulverizer 100 includes the weight of the retained powder present inside the pulverization chamber 10. Since the weight of the main body of the jet mill pulverizer 100 excluding the retained powder is known, the measured weight of the retained powder can be obtained from the weight value measured by the weight sensor 430.

[0040] The discharge port 122 of the jet mill pulverizer 100 is connected to the inlet pipe 210 of the cyclone collector 200 via a flexible pipe 222. The rotating shaft of the classifying rotor 120 is connected to a motor 124, and the drive circuit of the motor 124 is connected to a control device 130.

[0041] The jet mill pulverizer 100 receives the material to be pulverized (coarsely pulverized powder) from the supply device 110 including a raw material tank through the raw material inlet 20. The raw material inlet 20 is provided with a valve (not shown), and the internal pressure of the jet mill pulverizer 100 is appropriately maintained by opening and closing the valve. The material to be pulverized introduced into the jet mill pulverizer 100 is finely pulverized by collision with each other and with the collision plate 40 due to high-speed injection of inert gas from the pulverizer nozzle 50. Some of the powder particles thus pulverized ride on the air current and reach the upper classifying rotor 120, and are led from the classifying rotor 120 through the discharge port 122 to the cyclone collector 200. Coarse particles that are not sufficiently pulverized are separated by the classifying rotor 120, remain inside the jet mill pulverizer 100, and are further subjected to a pulverization process by collision. The material to be pulverized that has been fed into the jet mill pulverizer 100 is transferred to the cyclone collector 200 as finely pulverized powder having a particle size distribution with a median diameter of, for example, about 2 to 5 μm.

[0042] The cyclone collector 200 separates the powder and gas from the mixture of powder and gas supplied therein. The powder separated from the gas is collected in the powder collector 230 via the exhaust port 220. The gas is supplied to the back filter device 300 via the outlet pipe 240. The back filter device 300 collects a small amount of fine particles that may be unavoidably contained, and the clean gas is discharged to the outside from the exhaust port 310. The powder collected in the powder collector 230 is used for the production of sintered magnets through known production processes such as press molding in a magnetic field and a sintering process.

[0043] In the jet mill grinding system 1000 in this embodiment, the control device 130 is configured to control the rotation speed of the classifying rotor 120. The control device 130 typically has a processor that executes digital calculations and a memory that records a computer program. The computer program includes a plurality of instructions necessary for the operation of the processor. The control device 130 in this embodiment acquires the measured value of the retained powder weight from the weight sensor 430 that measures the weight of the jet mill grinding device 100, but the measured value of the retained powder weight may be acquired by other methods. The control device 130 may estimate the retained powder weight based on the supply rate of the material to be ground from the supply device 110 and the discharge rate from the discharge port 122. Such a supply rate and discharge rate may be measured values ​​or may be estimated values ​​(e.g., the estimated value includes not only a value obtained by calculation but also a value (set value) set by the user. The control device 130 may also be a motor control device such as an inverter that drives the motor 124 to rotate the classifying rotor 120 according to a specified value input by the user for the rotation speed of the classifying rotor 120.

[0044] The estimated value of the retained powder weight can also be obtained based on a table or an approximation that relates a set of parameters that determine the grinding conditions to the experimentally measured retained powder weight for each set. Such a set of parameters can include the supply amount of the material to be ground (coarsely ground powder), the ground amount of the finely ground powder, the rotation speed of the classifying rotor, and the flow rate of the grinding gas.

[0045] In this embodiment, the weight of the retained powder is managed, and the retained powder weight is not simply maintained at a constant value, but is increased from the conventional value, thereby increasing the number of collisions between powder particles and promoting the generation of finer powder particles. In addition to increasing the weight of the retained powder, the rotation speed of the classification rotor 120 is reduced, and the theoretical calculation classification diameter D t appears to increase, but the powder movement speed C R Since the diameter of the particle is relatively small, the theoretically calculated classification diameter D tThe theoretical calculation classification diameter D t It is believed that an increase in the weight of powder increases the particle size, but in the embodiment of the present disclosure, an increase in the particle size can be suppressed by increasing the weight of the retained powder.

[0046] Hereinafter, an embodiment of a method for producing an RTB based sintered magnet according to the present embodiment will be described.

[0047] The method for producing the RTB based sintered magnet of the present embodiment is as follows: supplying a coarsely pulverized powder of an alloy for RTB-based sintered magnets to a jet mill pulverizer equipped with a classifying rotor; A crushing step of crushing the coarse powder to form fine powder in the jet mill crushing device and discharging the fine powder by the classification rotor; Includes.

[0048] The coarsely pulverized powder of an alloy for an RTB sintered magnet (R is at least one rare earth element and necessarily includes at least one of Nd and Pr, T is at least one transition metal element and necessarily includes Fe, and B is boron) can be produced by subjecting a known alloy for an RTB sintered magnet to hydrogen pulverization or mechanical pulverization, and the composition of the alloy for an RTB sintered magnet is not limited. The coarsely pulverized powder has a particle size distribution with a median diameter of, for example, about 50 to 1000 μm. The particle size can be measured using a test sieve specified in JIS Z 8801 (ISO 3310).

[0049] In the method for producing an RTB-based sintered magnet according to the present disclosure, in the pulverization step, both the weight of the retained powder inside the jet mill pulverizer and the rotation speed of the classifying rotor are controlled. The control preferably changes the rotation speed of the classifying rotor according to a measured or estimated value of the retained powder weight during the pulverization step. More specifically, the control preferably decreases the rotation speed of the classifying rotor while increasing the amount of retained powder. Such a pulverization step includes, for example, a step of performing pulverization in a state where the measured or estimated value of the retained powder weight inside the jet mill pulverizer is a first retained powder weight, and a step of performing pulverization in a state where the measured or estimated value of the retained powder weight is a second retained powder weight in a range of 1.05 to 3 times the first retained powder weight. Then, in the step of performing pulverization in a state where the measured or estimated value of the retained powder weight is the second retained powder weight, the rotation speed of the classifying rotor is set according to the measured or estimated value of the retained powder weight.

[0050] Here, the first retained powder weight is the retained powder weight when the retained powder weight inside the jet mill grinding device becomes relatively stable (steady state) after the grinding process is started. In jet mill grinding, even after the supply of coarsely ground powder is started, it takes time for the powder to reach the desired particle size, so the same amount of powder as the amount supplied is not immediately recovered from the classification rotor. For this reason, in the early stage of the grinding process, the retained powder weight inside the jet mill grinding device gradually increases. In addition, the amount recovered from the classification rotor also increases accordingly, and the retained powder weight stabilizes at a set amount. The weight of the powder inside the jet mill grinding device when the retained powder weight stabilizes in this way is the first retained powder weight.

[0051] The measurement or estimation of the retained powder weight may be carried out not only during the grinding process in the jet mill grinding apparatus (online measurement or estimation), but also before the grinding process (offline measurement or estimation).

[0052] In an embodiment of the present disclosure, when the measured or estimated value of the retained powder weight inside the jet mill grinding device is increased in the grinding process, the rotation speed of the classifying rotor 120 is reduced. However, if the rotation speed of the classifying rotor 120 is reduced, the retained powder weight will decrease if left as is, so it is necessary to increase the supply rate of the coarsely ground powder and maintain the retained powder weight at a constant level. In addition, in a preferred embodiment of the present disclosure, the retained powder weight is maintained at a higher level than in the past. Specifically, the measured or estimated value of the retained powder weight is further increased from the first retained powder weight at which grinding is performed stably to a second retained powder weight that is in the range of 1.05 to 3 times the first retained powder weight. In that case, it is preferable to set the rotation speed of the classifying rotor 120 to be reduced in the range of 3% to 30% compared to the value when grinding is performed in a state where the first retained powder weight is obtained. In other words, if the rotation speed of the classifying rotor in the step of performing pulverization in a state where the measured or estimated value of the retained powder weight is the first retained powder weight is taken as 100%, the rotation speed of the classifying rotor in the step of performing pulverization in a state where the measured or estimated value of the retained powder weight is the second retained powder weight (=first retained powder weight x 1.05 to 3) can be set in the range of 70% to 99%. Preferably, it is set in the range of 70% to 98%, more preferably 70% to 97%. More preferably, the second retained powder weight is 1.2 to 3 times the first retained powder weight.

[0053] When the supply amount of coarsely pulverized powder to the jet mill pulverizer 100 is increased, the operation of the supply device 110 may be controlled by the control device 130, by another control device, or manually.

[0054] In the embodiment of the present disclosure, by maintaining the weight of the retained powder at a sufficiently high level, the reduction in the pulverization efficiency can be suppressed or the pulverization efficiency can be improved without increasing the particle size even if the rotation speed of the classifying rotor is reduced. This is because an increase in the weight of the retained powder can increase the frequency of collision of the retained powder particles. Note that reducing the rotation speed of the classifying rotor when the weight of the retained powder (amount retained in the tank) is low will result in an increase in particle size. In this way, changing only the rotation speed of the classifying rotor changes the particle size distribution, so in the past, the rotation speed of the classifying rotor was not controlled to improve the pulverization efficiency.

[0055] In a preferred embodiment, the ratio of the retained powder weight to the volume of the grinding chamber (powder concentration) is adjusted to a range of 1.05 to 2 times the normal retained powder amount. In order to quickly achieve a powder concentration in this range, coarsely ground powder may be supplied in advance to the inside of the jet mill grinding device 100 before the start of grinding.

[0056] In order to achieve high performance in RTB sintered magnets, it is preferable that the finely pulverized powder discharged by the classifying rotor has a particle size distribution with a median diameter of about 100 to 800 μm.

[0057] Example 1 A coarsely pulverized powder of a rare earth magnet alloy, consisting of 30.5 mass% Nd+Pr, 0.95 mass% B, and the remainder Fe, was prepared by a hydrogen absorption pulverization method. Specifically, the alloy was produced by a strip casting method. Then, coarse pulverization was performed using the hydrogen absorption method to prepare a coarse powder before jet mill pulverization. Trace additive elements such as Co, Al, Cu, Ga, Ti, Zr, and Mn were added in a total amount of about 3 mass%. To improve the coercive force, a portion of (Nd+Pr) may be replaced with an appropriate amount of heavy rare earth elements such as Dy and Tb. The density of this alloy was measured and found to be 7.55 Mg / m 3 It was.

[0058] The basic configuration of the jet mill pulverizing device used in this embodiment is as described with reference to Figures 1 to 3. In the jet mill pulverizing device used in this embodiment, the diameter of the pulverizing chamber 10 was 95.6 mm, the diameter of the inner cylinder 30 was 43 mm, the length of the inner cylinder 30 was 230 mm, and the distance from the tip of the pulverizing nozzle 50 to the collision plate 40 was 26 mm.

[0059] In this example, nitrogen gas with a purity of 99.9% or more was used, and jet mill pulverization was carried out under conditions where the oxygen content in the gas was 0.4 mass% or less, so that the average particle size was 3 to 4 μm. Jet mill pulverization gas (nitrogen) was used to supply to the cyclone collection device. However, the pulverization gas may be any inert gas such as argon or helium. The pressure of the jet mill pulverization gas was 0.5 MPa, and the flow rate was 1 m. 3 / min.

[0060] First, the raw material was fed at a feed rate of about 26 g / min in the grinding chamber without any coarse raw material powder. When the classifying rotor rotation speed was set to 8000 rpm, the amount of raw material powder retained in the grinding tank stabilized at about 85 g, and a grinding efficiency of about 26 g / min, the same as the feed rate, was obtained. The average particle size (median diameter) of the obtained powder was 4.0 μm (condition 1). The process of grinding under condition 1 corresponds to the process of grinding with the first retained powder weight.

[0061] As shown in Table 1 below, the retained powder weight and powder concentration were increased based on condition 1, and the rotation speed of the classifying rotor was decreased (conditions 2, 3, and 4). As a result, finely pulverized powder with the average particle size shown in Table 1 was obtained with the pulverization efficiency shown in Table 1. This average particle size was measured with a He-Ne laser type particle size distribution measuring device. The process of pulverization under conditions 2, 3, and 4 corresponds to the process of pulverization with the second retained powder weight.

[0062] [Table 1]

[0063] FIG. 7 is a graph showing the particle size distribution of the finely pulverized powder obtained when pulverization was performed under conditions 1 to 4. The horizontal axis of the graph is the particle size of the powder particles, and the vertical axis is the frequency. This particle size distribution is based on the results measured using a He-Ne laser type particle size distribution measuring device. In the graph of FIG. 7, the particle size distributions of the finely pulverized powder obtained by pulverization under conditions 1, 2, 3, and 4 are shown by the dashed line, dashed line, solid line, and dotted line, respectively.

[0064] In this embodiment, the grinding efficiency after the start of grinding was set to 26 g / min (condition 1). Thereafter, in order to increase the concentration of the retained powder in the grinding chamber, the weight of the retained powder was increased by increasing the supply rate of the coarsely ground powder to the grinding chamber. More specifically, the measured weight of the retained powder was increased from the first retained powder weight to the second retained powder weight. This increase in the retained powder weight increased the probability of collision between the powders and with the collision plate. In addition, by setting the classifying rotor rotation speed low, the grinding efficiency could be significantly improved without increasing the average particle size of the finely ground powder to be recovered. As shown in FIG. 7, the particle size distribution hardly changed.

[0065] According to the conventional understanding, if the rotation speed of the classification rotor is reduced, the particle size of the powder collected should become larger. However, the powder concentration in the grinding chamber increases, and the moving speed of the powder particles in the grinding chamber, C R It is considered that the powder particle moving speed C R As a result, if the rotation speed of the classification rotor remains constant, the classification diameter will decrease and only powder particles with small diameters will be collected. However, by reducing the rotor rotation speed, the classification diameter can be maintained.

[0066] Example 2 The pulverization was carried out using a jet mill pulverizer larger than that used in Example 1.

[0067] Specifically, a coarsely pulverized powder of a rare earth magnet alloy was prepared in the same manner as in Example 1. The density of this alloy was measured and found to be 7.55 Mg / m 3 It was.

[0068] The basic configuration of the jet mill pulverizing device used in this embodiment is as described with reference to Figures 1 to 3. In the jet mill pulverizing device used in this embodiment, the diameter of the pulverizing chamber 10 was about 400 mm, the diameter of the inner cylinder 30 was about 100 mm, the length of the inner cylinder 30 was about 600 mm, and the distance from the tip of the pulverizing nozzle 50 to the collision plate 40 was about 200 mm.

[0069] In this example, nitrogen gas with a purity of 99.9% or more was used, and jet mill pulverization was performed under conditions where the oxygen content in the gas was 0.4 mass% or less, so that the average particle size was 4 to 5 μm. Jet mill pulverization gas (nitrogen) was used to supply to the cyclone collection device. The pressure of the jet mill pulverization gas was 0.6 MPa, and the flow rate was 8 m. 3 / min.

[0070] As shown in Table 2 below, conditions 6 to 9 of the present disclosure, in which the retained powder weight and powder concentration are increased and the rotation speed of the classifying rotor is reduced based on condition 5, have improved pulverization efficiency compared to condition 5. In particular, conditions 8 and 9, in which the retained powder weight is increased by 1.05 times or more while the rotation speed of the classifying rotor is reduced to 97% or less, have an efficiency ratio of 1.30 or more compared to condition 5, and thus show a significant improvement in pulverization efficiency.

[0071] [Table 2] [Explanation of symbols]

[0072] 10···Crushing chamber, 20···Raw material supply port, 30···Inner cylinder, 100···Jet mill crushing device, 110···Supply device, 120···Classifying rotor, 130···Control device, 200···Cyclone collecting device, 1000···Jet mill crushing system

Claims

1. A step of supplying a coarsely pulverized powder of an R-T-B based sintered magnet alloy (R is at least one rare earth element and always contains at least one of Nd and Pr, T is at least one transition metal element and always contains Fe, and B is boron) to a jet mill pulverizer equipped with a classification rotor; A pulverization step of pulverizing the coarse pulverized powder inside the jet mill pulverization device to form a fine pulverized powder, and discharging the fine pulverized powder by the classification rotor, In the pulverization step, both the weight of powder retained in the jet mill pulverization device and the rotation speed of the classifying rotor are controlled, The method for producing alloy powder for RTB based sintered magnets comprises controlling the rotation speed of the classifying rotor according to a measured or estimated weight of the retained powder during the pulverization step.

2. 2. The method for producing alloy powder for an R-T-B system sintered magnet according to claim 1, wherein the control comprises increasing an amount of retained powder while decreasing the rotation speed of the classifying rotor.

3. The pulverization step includes a step of pulverizing the powder in a state where a measured or estimated value of a retained powder weight in the jet mill pulverization device is a first retained powder weight; performing pulverization in a state in which the measured or estimated value of the retained powder weight is a second retained powder weight in a range of 1.05 to 3 times the first retained powder weight; Including, 3. The method for producing an alloy powder for an R-T-B based sintered magnet according to claim 1 or 2, wherein in the step of performing pulverization in such a state that the measured or estimated value of the retained powder weight becomes a second retained powder weight, the rotation speed of the classifying rotor is set according to the measured or estimated value of the retained powder weight.

4. When the rotation speed of the classifying rotor in the step of performing pulverization in a state in which the measured or estimated value of the retained powder weight becomes the first retained powder weight, is set to 100%, 4. The method for producing alloy powder for R-T-B based sintered magnets according to claim 3, wherein a rotation speed of the classifying rotor in the step of pulverizing in a state in which the measured or estimated value of the retained powder weight becomes the second retained powder weight is set in a range of 70% or more and 97% or less.

5. 5. The method for producing an alloy powder for an R-T-B based sintered magnet according to claim 1, further comprising the step of supplying the coarsely pulverized powder in advance to the inside of the jet mill pulverizing device before the start of a pulverizing step.

Citation Information

Patent Citations

  • Preparation method for low-demagnetization-rate neodymium iron boron (NdFeB) alloy superfine permanent magnetic powder

    CN107464645A

  • Method for regenerating inorganic filler

    JP1998137619A

  • Pulverizing system of air flow type pulverizer

    JP1999290711A

  • Grinding apparatus and method

    JP2000317339A

  • Rare earth magnet and its manufacturing method

    JP2002175931A