Edge polishing method for piezoelectric oxide single crystal wafer and manufacturing method for piezoelectric oxide single crystal wafer

By using a polishing cloth conditioned with a dummy wafer to form contact marks, the method maintains the rounded shape of piezoelectric oxide single crystal wafers during edge polishing, preventing cracking and ensuring wafer integrity.

JP7567454B2Active Publication Date: 2024-10-16SUMITOMO METAL MINING CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2020215155
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-12-24
Publication Date
2024-10-16
Estimated Expiration
2040-12-24

AI Technical Summary

Technical Problem

Existing edge polishing methods for piezoelectric oxide single crystal wafers often result in the flattening of the beveled round shape, leading to increased susceptibility to cracking due to the use of new polishing cloths that preferentially flatten the tip, compromising the wafer's shape.

Method used

The method involves using a polishing cloth that has undergone a break-in process with a dummy wafer to form contact marks, followed by edge polishing with the same cloth to maintain the rounded shape, employing a cylindrical roll with a brush-like polishing surface and a dummy wafer with a controlled radius of curvature.

Benefits of technology

This approach prevents the flattening of the single crystal wafer's edge during polishing, maintaining its shape and reducing the risk of cracking, ensuring the wafer's integrity for subsequent processing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007567454000002
    Figure 0007567454000002
  • Figure 0007567454000003
    Figure 0007567454000003
  • Figure 0007567454000004
    Figure 0007567454000004
Patent Text Reader

Abstract

To provide an edge polishing method for a piezoelectric oxide single crystal wafer that suppresses a single crystal wafer end face in a round shape from being flat by polishing so as to maintain the shape of the end part of the single crystal wafer.SOLUTION: An edge polishing method for a piezoelectric oxide single crystal wafer includes: a polishing cloth running-in process of while rotating unused polishing cloth 212 wound around a side face of a roll 211 in a columnar shape and having a brush-like polishing surface 215 on the axis G of the roll, bringing the polishing surface 215 into contact with an end face Da of a dummy wafer rotating on a center axis parallel with the axis G of the roll to form a contact mark of the end face Da of the dummy wafer on the polishing surface 215; and an edge polishing process of using the polishing cloth 212 after the polishing running-in process to mirror-polish an end face of a wafer after a beveling process, wherein the edge polishing process includes bringing the end face of the wafer into contact the polishing surface 215 along the part where the contact mark is formed on the polishing surface 215 after the polishing running-in process.SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for edge polishing a piezoelectric oxide single crystal wafer and a method for manufacturing a piezoelectric oxide single crystal wafer. [Background technology]

[0002] Lithium tantalate (LiTaO3; hereinafter also referred to as "LT") single crystal and lithium niobate (LiNbO3; hereinafter also referred to as "LN") single crystal are ferroelectrics with melting points of approximately 1650°C and approximately 1250°C, respectively, and Curie points of approximately 600°C and approximately 1140°C, respectively, and have piezoelectric properties. LT single crystal or LN single crystal are used to manufacture LT single crystal wafers and LN single crystal wafers (hereinafter, LT single crystal wafers and LN single crystal wafers may be simply referred to as "single crystal wafers").

[0003] LT single crystal wafers and LN single crystal wafers are mainly used as device materials for surface acoustic wave (SAW) filters for removing signal noise in mobile phones, optical elements, etc., and either single crystal wafer is selected depending on the characteristics required by the device. A SAW filter is an element that uses the above-mentioned lithium tantalate single crystal, etc., and is a device that inputs high-frequency power to a comb-shaped electrode formed on a piezoelectric single crystal wafer to generate a surface acoustic wave on the surface of the piezoelectric single crystal wafer, and then converts this surface acoustic wave back into a high-frequency electrical signal by another comb-shaped electrode.

[0004] In the case of LT single crystals, an ingot of LT single crystal grown by a single crystal growing method such as the Czochralski method (CZ method) is ground into a cylinder, and then the cylinder is sliced ​​into disk-shaped single crystal wafers of a specified thickness along the desired crystal orientation using a cutting device such as a wire saw.

[0005] Next, the sliced ​​single crystal wafer is polished to a predetermined thickness into a parallel and flat shape by double-sided lapping or the like to obtain a single crystal wafer with roughened surfaces on both sides. A processing method is known in which a specific single crystal wafer holding method is applied to this single crystal wafer with roughened surfaces on both sides, and one side is mirror-polished. This has made it possible to efficiently mirror-polish one side of a single crystal wafer.

[0006] LT single crystal wafers are beveled using a diamond grinding wheel to chamfer the outer periphery of the single crystal wafer to prevent cracking in subsequent processes and to ensure that the diameter of the single crystal wafer is a specified size.

[0007] Furthermore, in order to prevent cracks during the manufacture of the SAW filter, the outer periphery of the beveled edge of the single crystal wafer needs to be polished to a mirror finish (edge ​​polishing) by mechanochemical polishing using a slurry such as colloidal silica. For example, this edge polishing is described in Patent Document 1. Patent Document 1 describes a method for edge polishing a single crystal wafer, in which an elastic sponge sheet and a polishing cloth are attached to the outer periphery of a cylinder, and the outer periphery of a single crystal wafer attached to a rotating device is brought into contact with the polishing cloth while a polishing liquid is supplied to this contact surface to perform mirror finishing. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] Patent Publication No. 2020-015138 Summary of the Invention [Problem to be solved by the invention]

[0009] Incidentally, in order to prevent cracking of the single crystal wafer, the edge surface of the piezoelectric oxide single crystal wafer that has been subjected to the beveling process is subjected to mirror polishing (edge ​​polishing). Specifically, edge polishing refers to a process in which the edge surface of the single crystal wafer that has been rounded by beveling is mirror polished.

[0010] However, when performing edge polishing after beveling the edge of a single crystal wafer, if a new (unused) polishing cloth is used, the round shape of the beveled edge of the single crystal wafer is preferentially polished, causing the tip to become flat and deformed into an angular shape. When the edge shape is deformed, there is a problem that the single crystal wafer becomes more likely to crack.

[0011] Therefore, the present invention provides an edge polishing method for a piezoelectric oxide single crystal wafer, which is capable of preventing the rounded end face of the single crystal wafer from being flattened by polishing when edge polishing is performed on the beveled wafer end face, and is also capable of maintaining the shape of the edge of the single crystal wafer. [Means for solving the problem]

[0012] The edge polishing method of the present invention for a piezoelectric oxide single crystal wafer includes an abrasive cloth conditioning step in which an unused abrasive cloth having a brush-like abrasive surface is wound around the side of a cylindrical roll equipped in an edge polishing apparatus, and the abrasive cloth is rotated around the axis of the roll while the abrasive cloth is brought into contact with an edge face of a dummy wafer rotating around a central axis parallel to the axis of the roll, thereby forming a contact mark on the edge face of the dummy wafer on the polishing surface; and an edge polishing step in which the abrasive cloth after the abrasive cloth conditioning step is used to mirror-polish the edge face of the piezoelectric oxide single crystal wafer after the beveling step, and the edge polishing step is a step in which the edge face of the piezoelectric oxide single crystal wafer is brought into contact with the polishing surface along the portion of the polishing surface after the abrasive cloth conditioning step where the contact mark has been formed.

[0013] In the edge polishing method of a piezoelectric oxide single crystal wafer of the present invention, the dummy wafer may be used repeatedly in the polishing cloth conditioning step.

[0014] In the edge polishing method for a piezoelectric oxide single crystal wafer of the present invention, the shape of the side edge of the dummy wafer may be an arc shape with a radius of curvature of 75 μm to 375 μm.

[0015] In the edge polishing method of the present invention for a piezoelectric oxide single crystal wafer, the conditions for bringing the polishing cloth into contact with the dummy wafer in the polishing cloth conditioning step may be the same as the conditions for bringing the polishing cloth into contact with the piezoelectric oxide single crystal wafer in the edge polishing step.

[0016] In the edge polishing method for a piezoelectric oxide single crystal wafer of the present invention, the dummy wafer may be made of the same oxide single crystal as the piezoelectric oxide single crystal wafer.

[0017] The method for producing a piezoelectric oxide single crystal wafer of the present invention includes the method for edge polishing a piezoelectric oxide single crystal wafer of the present invention. Effect of the Invention

[0018] The method for edge polishing a piezoelectric oxide single crystal wafer of the present invention makes it possible to prevent the rounded edge surface of the single crystal wafer from becoming flattened by polishing when edge polishing is performed on the beveled edge surface of the wafer, thereby maintaining the shape of the edge of the single crystal wafer.

[0019] The method for producing a piezoelectric oxide single crystal wafer of the present invention includes the edge polishing method of the present invention, and therefore when edge polishing is performed on a beveled wafer edge surface, it is possible to prevent the rounded edge surface of the single crystal wafer from becoming flattened by polishing, and to maintain the shape of the edge of the single crystal wafer. [Brief description of the drawings]

[0020] [Figure 1] FIG. 2 is a flow diagram showing each step of a method for producing a single crystal wafer, which is an example of the present embodiment. [Diagram 2] 1A is a schematic cross-sectional view illustrating an aspect in which a single crystal wafer W1 is polished using a chamfering grindstone 110 in a beveling step of the manufacturing method for a single crystal wafer of this embodiment, FIG. 1B is a cross-sectional view of the single crystal wafer showing the shapes of the edges of the single crystal wafers W1 and W2 before and after the beveling step, and FIG. 1C is a cross-sectional view showing a modified shape of the edge of the single crystal wafer W2 after the beveling step. [Diagram 3] 3(A) is a schematic perspective view showing an aspect in which a dummy wafer D is used to break in an abrasive cloth 212 in an edge polishing apparatus used in the edge polishing method and manufacturing method of a single crystal wafer according to this embodiment, and FIG. 3(B) is an enlarged cross-sectional view showing the side end portion of the dummy wafer D surrounded by H in FIG. 3(A). [Figure 4] FIG. 1 is a schematic side view showing an aspect in which a dummy wafer D is used to condition an abrasive cloth 212 in an edge polishing apparatus used in the edge polishing method and manufacturing method of a single crystal wafer according to the present embodiment. [Diagram 5] 5 is a side view for explaining the position where a dummy wafer D is brought into contact with the polishing cloth shown in FIG. 3 and FIG. 4. FIG. [Figure 6] 1A is an enlarged schematic cross-sectional view of the polishing cloth 212a, and FIG. 1B is an enlarged schematic cross-sectional view of the polishing cloth 212a after a contact mark 214a has been formed thereon. [Figure 7] 7(A) is a schematic perspective view showing how the side edge of the single crystal wafer W3 is polished by a polishing cloth 212 of an edge polishing apparatus used in the edge polishing method and manufacturing method of the single crystal wafer of this embodiment, and FIG. 7(B) is an enlarged cross-sectional view showing the side edge of the single crystal wafer W3 surrounded by K in FIG. 7(A). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] A method for producing a piezoelectric oxide single crystal wafer and a method for edge polishing a piezoelectric oxide single crystal according to one embodiment of the present invention will be described with reference to the drawings. Note that the present invention is not limited to the following embodiment.

[0022] The method for producing a piezoelectric oxide single crystal wafer of this embodiment includes a method for edge polishing a piezoelectric oxide single crystal wafer, which will be described later. Specifically, as shown in Fig. 1, the method includes the steps of slicing an ingot of a piezoelectric oxide single crystal, beveling, lapping, edge polishing, and polishing, in that order. In this embodiment, the steps are performed in this order, but the order of the steps may be changed as long as it does not cause any problems in the production of the single crystal wafer, and other steps may be performed if necessary.

[0023] Each step of the method for producing a piezoelectric oxide single crystal wafer will be described below with reference to the drawings.

[0024] [material] Examples of single crystals used in the piezoelectric oxide single crystal wafer of this embodiment (hereinafter, may be referred to as "single crystal wafer" or "wafer") include lithium niobate (LiNbO3) single crystal (LN), lithium tantalate (LiTaO3) single crystal (LT), and yttrium aluminum garnet (Y3A l5 O 12 ) single crystal (YAG). Below, the manufacturing method of the single crystal wafer and the edge polishing method will be explained using the LT single crystal as a representative example of the piezoelectric oxide single crystal.

[0025] LT single crystals are grown by single crystal growth methods such as the Czochralski method (CZ method). The Czochralski method is a method for growing single crystals by immersing a seed crystal in the molten liquid obtained by melting raw material powder and then pulling it up. For example, by using a high-frequency induction heating device, large crystals can be stably produced.

[0026] The top and bottom ends of the grown LT single crystal ingot are cut off due to the lack of diameter of the LT single crystal, and the middle LT single crystal is subjected to a single polarization process (poling). This poling process is <001> The crystal is polarized in the axial direction by heating to a temperature equal to or higher than the Curie point, for example, 600 to 700° C., and applying a voltage of, for example, 200 to 500 V for about 0.5 to 2 hours.

[0027] [Slicing process] The slicing process is a process in which a cylindrical LT single crystal ingot is sliced ​​into a disk shape using a wire saw.

[0028] First, in the slicing process, the LT single crystal is sliced ​​into a disk-shaped single crystal wafer W1 (FIG. 2(B)) of a predetermined thickness along a desired crystal orientation using a wire saw (cutting device) with a diamond grinding wheel attached to the wire. The thickness of the single crystal wafer W1 can be, for example, about 0.15 mm to 0.6 mm. This single crystal wafer is then subjected to a beveling process.

[0029] [Beveling process] The beveling step is a step for shaping the edge portion 10 (FIG. 2(B)) of the single crystal wafer W1 obtained in the slicing step.

[0030] Fig. 2(B) is a cross-sectional view of the single crystal wafer showing the shape of the edge of the single crystal wafer before and after the beveling process. As shown in Fig. 2(B), the sliced ​​disk-shaped single crystal wafer W1 has corners 11 above and below the edge 10, and cracks or chips may occur from these corners 11. Therefore, by performing a beveling process on the edge 10 of the single crystal wafer W1, the corners 11 are polished and the edge 10 of the single crystal wafer W1 is chamfered.

[0031] FIG. 2(A) is a schematic cross-sectional view illustrating a mode in which a single crystal wafer W1 is polished using a chamfering grindstone 110 in the beveling step of the manufacturing method for a single crystal wafer of this embodiment. In the beveling step, a ring-shaped chamfering grindstone 110 is fixed to a groove on the peripheral surface of a core disk. A groove 111 having a shape corresponding to the desired chamfering shape is formed in the chamfering grindstone 110. In FIG. 2(A), line A indicates the central axis of the chamfering grindstone 110, and line B indicates the central axis of the single crystal wafer W1. The edge 10 of the single crystal wafer W1 held on the wafer holder 120 is pressed against the groove 111 of the chamfering grindstone 110 rotating in the direction of arrow a about the axis of line A in FIG. 2(A), and polished while rotating in the direction of arrow b about the axis of line B in FIG. 2(A), whereby the corner portion 11 is polished to obtain a single crystal wafer W2 (FIG. 2(B)) having a rounded edge 20. At this time, water is supplied to the polished surface of the single crystal wafer W1 that is in contact with the chamfering grindstone 110 to reduce frictional heat and remove polishing debris and the like.

[0032] The shape of the edge 20 of the single crystal wafer W2 obtained by the beveling process may be an arc-shaped semicircular shape like the edge 20 without any taper at the top or bottom as in the single crystal wafer W2 in FIG. 2(B), or may have tapered portions 21 at the top and bottom in the cross section of the wafer edge and an arc-shaped tip 22 as in the single crystal wafer W2a shown in FIG. 2(C). These shapes can be processed into a desired shape by the shape of the groove 111 of the chamfering grindstone 110. The shape of the edge 20 can be measured with a measuring device called an edge profiler, and the radius of curvature (R) of the chamfered round shape can be calculated and managed by the value of this radius of curvature.

[0033] In the following, a case will be described in which the shape of the edge 20 on the side surface of the single crystal wafer W2 is semicircular, that is, the shape of the single crystal wafer W2.

[0034] [Wrapping process] The single crystal wafer W2 obtained by the beveling step is then subjected to a lapping step.

[0035] In the lapping process, both sides of the single crystal wafer W2 are lapped. A slurry consisting of abrasive grains such as silica and water is usually used for the double-sided lapping. A double-sided lapping device (not shown) is used, which includes upper and lower polishing plates with polishing cloths attached to the opposing sides and a carrier plate placed between them. This removes damage to both sides of the single crystal wafer that occurred during the slicing process, and the single crystal wafer W2 is aligned to a predetermined thickness while obtaining a predetermined flatness and parallelism. This results in a single crystal wafer W3 that has been lapped.

[0036] [Edge polishing process] Next, the edge polishing method of the present embodiment will be described with reference to FIGS.

[0037] In the edge polishing method of the present embodiment, an unused polishing cloth 212 having a brush-like polishing surface 215 is wound around a side surface of a cylindrical roll (sponge roller 211) provided in an edge polishing device. The polishing cloth 212 is rotated around the central axis of the roll (line G in FIGS. 3 and 4), while the polishing surface 215 is brought into contact with an edge surface Da of a dummy wafer D rotating around a central axis (line F in FIGS. 3 and 4) parallel to the central axis of the roll (line G), thereby contacting the edge surface Da of the dummy wafer D. The method includes a polishing cloth conditioning step of forming a contact mark 214a (FIG. 6) on the polishing surface 215, and an edge polishing step of mirror-polishing the edge surface 30 of the piezoelectric oxide single crystal wafer (single crystal wafer W3) after the beveling step using the polishing cloth 212 after the polishing cloth conditioning step. The edge polishing step is a step of bringing the edge surface 30 of the piezoelectric oxide single crystal wafer (single crystal wafer W3) into contact with the polishing surface 215 along the portion of the polishing surface 215 after the polishing cloth conditioning step where the contact mark 214a is formed.

[0038] The single crystal wafer W3 (FIG. 7(B)) obtained by the lapping process is further subjected to an edge polishing process. Fine irregularities remain on the surface of the edge 30 of the beveled single crystal wafer W3, which may lead to cracking in subsequent processes. Therefore, in order to prevent cracking of the single crystal wafer in subsequent processes, edge mirror processing (edge ​​polishing) is performed to mirror-polish the edge 30 of the single crystal wafer W3 after the beveling process.

[0039] It should be noted that a single crystal wafer that has been subjected to a beveling process may be obtained by purchase or the like and used in the edge polishing method of this embodiment.

[0040] The edge polishing process can be performed using a single-wafer type of equipment, which processes the single crystal wafers W3 one by one, or a type in which a plurality of single crystal wafers W3 are stacked and processed via spacers. The type of equipment applied to the single crystal wafer manufacturing method and edge polishing method of this embodiment is not particularly limited. The following description will be given taking a single-wafer type edge polishing equipment as an example.

[0041] (Abrasive cloth break-in process) As described above, when edge polishing is performed on the edge surface 30 of the beveled single crystal wafer W3, the round shape of the beveled edge surface 30 of the single crystal wafer W3 may be preferentially polished by polishing, resulting in a flat tip. If the edge surface 30 of the single crystal wafer W3 is polished to a flat tip, there is a problem that the edge surface 30 of the single crystal wafer W3 may be deformed into an angular shape, making the single crystal wafer more likely to crack due to impact, etc. The inventors conducted a detailed investigation and found that the edge shape of the single crystal wafer that was subjected to edge polishing immediately after replacing with a new polishing cloth does not maintain its round shape and is more likely to collapse.

[0042] . Therefore, in the edge polishing method of this embodiment, when a new polishing cloth is used, the edge of the single crystal wafer W3 is polished using a polishing cloth that has been subjected to a polishing cloth conditioning process.

[0043] Specifically, as shown in Figures 3, 4 and 6, the polishing cloth conditioning step is a step in which an unused polishing cloth 212 having a brush-like polishing surface 215 is wound around the side surface of a cylindrical roll (sponge roller 211) equipped in an edge polishing device, and the polishing cloth 212 is rotated around the central axis (line G) of the roll (sponge roller 211), while the polishing surface 215 is brought into contact with an edge surface Da of a dummy wafer D rotating around a central axis (line F) parallel to the central axis (line G) of the roll, to form a contact mark 214a of the edge surface Da of the dummy wafer D on the polishing surface 215. The edge polishing step described below is performed using the polishing cloth that has been subjected to this conditioning process.

[0044] (Device) 3 and 4 are schematic perspective views showing how a polishing cloth 212 of a single-wafer edge polishing apparatus is seasoned using a dummy wafer D. The edge polishing apparatus has a cylindrical polishing body 210 that comes into contact with the edge (outer periphery) of the dummy wafer D, a table 220 that suction-fixes the dummy wafer D, a processing liquid supply unit (not shown) that supplies processing liquid to a contact portion T between the dummy wafer D and the polishing body 210, and a stage unit (not shown) on which these are placed.

[0045] In Fig. 3 and Fig. 4, line G is the central axis of the polishing body 210. Also, line F in Fig. 3 and Fig. 4 is the central axis of the dummy wafer D and the table 220. In addition to rotating around line G in Fig. 3 and Fig. 4, the polishing body 210 can move horizontally in the direction connecting the central axis (line F) of the table 220 and the central axis (line G) of the polishing body (arrow C direction in Fig. 3), so that after placing the single crystal wafer W3, it can be abutted against the end surface Da of the dummy wafer D so that line F and line G are parallel. In addition to rotating around line F in Fig. 4, the table 220 can move in the height direction (axial direction of line F, arrow E direction in Fig. 3), so that the dummy wafer D can be held at a predetermined position of the polishing body 210.

[0046] 3 and 4, the polishing body 210 has a cylindrical sponge roller 211 and a polishing cloth 212 wound around and fixed to the sponge roller 211. The polishing cloth 212 has a polishing cloth 212a for rough processing fixed to the lower part of the sponge roller 211, and a polishing cloth 212b for finish processing.

[0047] Here, the structure of the polishing cloth 212 will be described by taking the polishing cloth 212a as an example. The polishing cloths 212a and 212b have the same basic structure, except that they are used for rough processing and finish processing. Fig. 6(A) is a schematic enlarged cross-sectional view of the polishing cloth 212a, and Fig. 6(B) is a schematic enlarged cross-sectional view of the polishing cloth 212a with a contact mark 214a formed thereon.

[0048] 6, the polishing cloth 212a may be made of, for example, a base material 213 formed of a resin cured product and a brush portion 214 formed of a fiber material. The brush portion 214 is attached to the surface of the base material 213, and abrasive grains are attached to the brush portion 214. The surface on the brush portion 214 side forms the polishing surface 215 of the polishing cloth 212a. The thickness of the base material 213 may be, for example, about 0.1 mm to 0.5 mm, and the thickness of the brush portion 214 may be, for example, about 0.3 mm to 0.7 mm.

[0049] The polishing cloth 212a for rough processing may be a polishing cloth with a grit size of about #1500, and the polishing cloth 212b for finish processing may be a polishing cloth with a grit size of about #3000. The polishing cloth may be a polishing cloth with multiple grit sizes as in this embodiment, or a polishing cloth with one type of grit size. The polishing abrasive grains attached to the polishing cloth are not particularly limited, and may be, for example, diamond abrasive grains. In this embodiment, the polishing abrasive grains are attached to the polishing cloth 212, but the polishing abrasive grains may be mixed into the processing liquid and supplied during processing without being attached to the polishing cloth.

[0050] The sponge roller 211 is a cylindrical member, and may be made of polyurethane, for example, with a hardness of about Asker C11.

[0051] The polishing cloth 212 is formed in a ring shape so as to fit the roll diameter of the sponge roller 211 and to be able to cover the sponge roller 211. The ring shape of the polishing cloth 212 can be formed, for example, by partially overlapping both ends of a strip-shaped polishing cloth and adhering them with an adhesive or the like. The sponge roller 211 and the polishing cloth 212 have the same diameter, and the polishing cloth 212 is held in place so as not to fall off due to the pressure caused by the sponge roller 211 expanding due to the processing fluid supplied during polishing.

[0052] In the polishing cloth conditioning step, in order to cool the frictional heat generated when the dummy wafer D and the polishing body 210 come into contact with each other and to prevent the scattering of polishing debris, it is preferable to use a processing liquid at the contact portion T (FIG. 4) between the single crystal wafer W3 and the polishing body 210. For example, pure water can be suitably used as the processing liquid. As described above, a polishing cloth to which no abrasive grains are attached may be used, and abrasive grains may be mixed into the processing liquid.

[0053] (dummy wafer) The dummy wafer D used in the break-in process of the polishing cloth 212 may be a beveled or edge-polished single crystal wafer. The single crystal constituting the dummy wafer D is not particularly limited, but from the viewpoint of preventing contamination, it is preferable that the single crystal is the same oxide single crystal as the crystal of the single crystal wafer to be manufactured. The shape of the end face Da of the dummy wafer D may be set to the same shape as the single crystal wafer obtained by the method for manufacturing a piezoelectric oxide single crystal wafer of this embodiment. The polishing cloth break-in process using the dummy wafer D is performed every time the polishing cloth 212 is replaced.

[0054] Furthermore, a new dummy wafer D may be used each time the polishing cloth 212 is replaced, or the dummy wafer D may be used repeatedly for polishing cloth break-in processing. However, by repeatedly using the dummy wafer D, the end face Da is polished by the polishing cloth 212, and the rounded tip of the end face Da of the dummy wafer D gradually becomes flat and loses its shape. The flatter the end face Da of the dummy wafer D becomes, the larger the radius of curvature of the end face Da of the dummy wafer D becomes. Therefore, the shape of the dummy wafer D can be managed using the radius of curvature of the end face Da as an index. Furthermore, the radius of curvature of the end face of the dummy wafer is preferably equal to the radius of curvature of the side end face of the single crystal wafer W3 after the edge polishing process so as not to affect the processing of the single crystal wafer W3.

[0055] When the side end portion of the single crystal wafer is formed into a semicircular shape, the radius of curvature of the dummy wafer D is preferably 0.5 to 0.63 times the thickness of the dummy wafer D. That is, when the thickness of the dummy wafer D is 150 μm, the radius of curvature of the side end portion of the dummy wafer D is preferably about 75 μm to 95 μm, when the thickness of the dummy wafer D is 200 μm, the radius of curvature of the side end portion of the dummy wafer D is preferably about 100 μm to 126 μm, and when the thickness of the dummy wafer D is 600 μm, the radius of curvature of the side end portion of the dummy wafer D is preferably about 300 μm to 378 μm.

[0056] Since the thickness of the single crystal wafer to be manufactured is generally about 150 μm to 600 μm, when the shape of the side end of the dummy wafer is semicircular, it is preferable to use a semicircular dummy wafer with a radius of curvature of 75 μm to 378 μm. When the shape of the side end of the dummy wafer D is an arc shape and not a semicircular shape, the value of the radius of curvature is not limited to the above.

[0057] It is not necessary to use a single crystal wafer to be commercialized as the dummy wafer D. For example, a wafer that does not meet the manufacturing process standards due to large reduction unevenness caused by the reduction treatment, but has no problems with the end face shape, etc., can be used.

[0058] (Device Operation) The operation of the apparatus in the polishing cloth conditioning step will be described with reference to Figures 3 and 4. First, the polishing body 210 is horizontally moved outward in a direction (arrow C direction) connecting the central axis (line F) of the table 220 and the central axis (line G) of the polishing body so that the polishing body 210 does not contact the dummy wafer D, and the dummy wafer D is placed on the table 220 and fixed by suction. Next, the height of the table is adjusted in the E direction so that the dummy wafer D contacts a predetermined position (Figure 4(A)) of the polishing cloth 212a, and the polishing body 210 is horizontally moved inward in the arrow C direction so as to contact the dummy wafer D, and is brought into contact with the end surface Da of the dummy wafer D in the arrow C direction in Figures 3 and 4.

[0059] Next, while the processing liquid is being supplied, the table 220 and the polishing body 210 are rotated to form a contact mark 214a of the edge surface Da of the dummy wafer D on the polishing surface 215 of the polishing cloth 212, as shown in FIG. 6(B).

[0060] In the single-wafer edge polishing apparatus of this embodiment, which processes the single-crystal wafers W3 one by one, the position where the single-crystal wafer W3 is brought into contact with the polishing cloth 212 is moved each time a single wafer is polished.

[0061] Therefore, in the break-in process, the dummy wafer D is replaced every time the position on the polishing cloth 212 where the dummy wafer D is placed is moved, and the break-in process is performed on the polishing cloth 212.

[0062] That is, for example, a first dummy wafer D is abutted at the topmost position in the height direction of the portion of the polishing cloth 212a used for polishing processing, and when a second dummy wafer D is abutted against the polishing cloth 212a, it is abutted at a position shifted a predetermined distance below the position at which the first dummy wafer D was abutted.

[0063] For example, when a dummy wafer D having a thickness of 400 μm is used, a margin of 200 μm is provided and the second dummy wafer D is brought into contact with the first dummy wafer D at a position shifted 600 μm below the position at which the first dummy wafer D was brought into contact. A more detailed description will be given with reference to FIG.

[0064] Fig. 5 is a side view for explaining the contact position of the dummy wafer D on the polishing cloth 212a. In Fig. 5, the contact positions of the first, second, and third dummy wafers D1, D2, and D3 correspond to P1, P2, and P3, respectively. The height dimension Lp of P1, P2, and P3 is 600 µm, and the thickness dimension Ld of the dummy wafer D is 400 µm. Similarly, the contact positions of the fourth and subsequent dummy wafers D can be set to positions shifted downward by 600 µm each.

[0065] In this manner, the polishing cloth conditioning step is performed while shifting the position where the dummy wafer D is brought into contact, and a plurality of contact marks 214a corresponding to a plurality of dummy wafers D1, D2 are formed, for example, as shown in FIG. 6(B).

[0066] At this time, when the polishing cloth 212a has a height dimension of 30 mm, 25 dummy wafers D (30 / 0.6=25) can be abutted. The first dummy wafer D may be abutted at the lowest position of the polishing cloth 212, and the second and subsequent dummy wafers D may be abutted by shifting them upward by a predetermined distance at a time, and the order in which the positions are shifted is not particularly limited. In addition, it is preferable that the predetermined dimension when shifting the positions is set to include the thickness dimension of the dummy wafer D and a margin (200 μm in this embodiment). The size of the margin is not particularly limited and can be set appropriately, for example, to about half the thickness dimension of the dummy wafer D.

[0067] Note that one dummy wafer may be used for break-in processing at multiple locations on the polishing cloth 212, or a different dummy wafer may be used for break-in processing at each location. When a new polishing cloth is used for polishing processing, the side edge of the dummy wafer D is likely to be polished, and therefore, if the dummy wafer D is used multiple times repeatedly, variations may occur in the shape (contact mark 214a) formed on the polishing cloth 212. For this reason, it is more preferable to prepare in advance the number of dummy wafers D that can be processed with one polishing cloth 212, and use a different dummy wafer D for each contact position for break-in processing.

[0068] As described above, while shifting the position at which the dummy wafer D is in contact with the polishing cloth 212, contact marks 214a are formed at all positions on the polishing cloth 212 where the single crystal wafer W3 will be in contact in the edge polishing process, and the polishing cloth conditioning process is completed.

[0069] (Edge polishing process)

[0070] The edge polishing process is a process of mirror-finishing the edge surface 30 of the single crystal wafer W3 using an abrasive cloth 212. Abrasive grains attached to the abrasive cloth 212 remove processing marks (so-called "bevel residues") remaining on the edge surface 30 of the single crystal wafer W3 during the beveling process.

[0071] The edge polishing step of this embodiment is a step of mirror-polishing the end face 30 of the piezoelectric oxide single crystal wafer (single crystal wafer W3) after the beveling step using the polishing cloth 212 after the polishing cloth conditioning step. Moreover, in the edge polishing step, the end face 30 of the piezoelectric oxide single crystal wafer (single crystal wafer W3) is brought into contact with the polishing surface 215 along the portion where the contact mark 214a of the polishing surface 215 after the polishing cloth conditioning step is formed.

[0072] In addition, the edge polishing step may use an edge polishing device having the same configuration as the polishing cloth conditioning step. As shown in Fig. 7, the dummy wafer D shown in Fig. 3 may be replaced with a single crystal wafer W3, and the edge surface 30 of the single crystal wafer W3 may be mirror-polished. In Fig. 7, the line J indicates the central axis of the single crystal wafer W3 and the table 220.

[0073] The conditions for bringing the polishing cloth 212 into contact with the dummy wafer D in the polishing cloth conditioning step and the conditions for bringing the polishing cloth 212 into contact with the single crystal wafer W3 in the edge polishing step may be the same, or the conditions may be different. In this embodiment, the conditions for bringing the polishing cloth 212 into contact with the dummy wafer D and the conditions for bringing the polishing cloth 212 into contact with the single crystal wafer W3 are the same, and detailed description thereof will be omitted.

[0074] (Device Operation) The operation of the device in the edge polishing step will be described with reference to FIG. 7. First, the polishing body 210 is horizontally moved outward in the direction (arrow C direction) connecting the central axis (line J) of the table 220 and the central axis (line G) of the polishing body, and the single crystal wafer W3 is placed on the table 220 and fixed by suction. Next, the height of the table 220 is adjusted so that the single crystal wafer W3 abuts on a position (predetermined position) of the polishing cloth 212a corresponding to the contact mark 214a formed by the edge shape of the dummy wafer D, and the polishing body 210 is horizontally moved inward in the direction of arrow C to abut on the edge of the single crystal wafer W3 in the direction of arrow C. This completes the installation of the single crystal wafer W3.

[0075] Next, while supplying the processing liquid, the table 220 and the polishing body 210 are rotated to polish the edge of the single crystal wafer W3 for rough processing. After the rough processing is completed, the polishing body 210 is temporarily moved outward, and the height of the table 220 is adjusted so that the single crystal wafer W3 abuts against a predetermined position of the polishing cloth 212b, and the polishing body 210 is again brought into contact with the edge of the single crystal wafer W3 for polishing and finishing. This completes the edge polishing process.

[0076] As described above, for example, when a single crystal wafer W3 having a thickness of 400 μm is polished at a position shifted downward by 600 μm with a margin of 200 μm, if the polishing cloth 212a has a height dimension of 25 mm, the effective length used for polishing is, for example, 15 mm, and 25 (15 / 0.6=25) single crystal wafers W3 can be polished. When polishing the 26th single crystal wafer W3, the polishing may be performed again using the portion of the polishing cloth 212a used for polishing the first single crystal wafer W3, or the polishing cloth 212 may be replaced with a new polishing cloth 212 and a polishing cloth break-in process may be performed before polishing.

[0077] Furthermore, the radius of curvature of the edge of the single crystal wafer after the edge polishing step depends on the plate thickness of the single crystal wafer, but since the thickness of the single crystal wafer is about 0.15 mm to 0.6 mm as described above, the radius of curvature of the edge can be set to about 0.075 mm to 0.378 mm, which is 0.5 to 0.63 times the thickness of the single crystal wafer.

[0078] [Polishing process] Finally, the single crystal wafer that has been subjected to the edge polishing step is subjected to a polishing step, which is not a step for polishing the edge face but a step for mirror-polishing either the front or back surface of the single crystal wafer whose edge face has been polished.

[0079] [Other processes] In the method for producing a single crystal wafer according to the present embodiment, the steps other than the beveling step and the edge polishing step are optional. In addition to the steps described above, a reduction treatment step, a step for removing processing distortion, a surface grinding step for smoothing the surface condition of the single crystal wafer, etc. may be added.

[0080] In the edge polishing process, the end surface 30 of the single crystal wafer W3 is pressed against the polishing cloth 212 to perform the polishing process. When a new polishing cloth 212 is used that has never been used for the edge polishing process and is pressed strongly against the end surface 30 of the single crystal wafer W3, the beveled round shape is preferentially polished away from the tip of the end surface of the single crystal wafer, causing the tip to become flattened and collapse into an angular shape.

[0081] When the edge of the single crystal wafer W3 that is to be brought into contact with the same portion of the polishing cloth 212 for the second or subsequent times is polished, the shape of the wafer edge when the wafer that was brought into contact with the polishing cloth 212 for the first time remains as a contact mark 214a, and the single crystal wafer W3 is polished to match this conditioned shape. Therefore, in the edge polishing method of this embodiment, the contact mark 214a is formed on the polishing surface 215 of the polishing cloth 212 in advance using a dummy wafer D in the polishing cloth break-in process, and the edge 30 of the single crystal wafer W3 is brought into contact with the polishing surface 215 along the portion where the contact mark 214a is formed and mirror-finished, so that the rounded edge of the single crystal wafer W3 becomes flat by polishing, and the edge of the single crystal wafer W3 can be prevented from collapsing into an angular shape.

[0082] According to the method for edge polishing a single crystal wafer of the present embodiment, when edge polishing is performed on the edge face 30 of the beveled single crystal wafer W3, the rounded edge face 30 of the single crystal wafer W3 is prevented from being flattened by polishing, and the shape of the edge of the single crystal wafer can be maintained.

[0083] In the method for manufacturing a single crystal wafer of this embodiment, the edge polishing method of this embodiment is included in the edge polishing step, so that when edge polishing is performed on the edge face 30 of the beveled single crystal wafer W3, the rounded edge face 30 of the single crystal wafer W3 is prevented from being flattened by polishing, and the shape of the edge of the single crystal wafer can be maintained.

[0084] It should be noted that the present invention is not limited to the above-described embodiment, but includes other configurations that can achieve the object of the present invention, and modifications of the above-described embodiment are also included in the present invention.

[0085] In addition, the best configuration, method, etc. for implementing the present invention are disclosed in the above description, but the present invention is not limited thereto. That is, the present invention has been mainly described with respect to a specific embodiment, but a person skilled in the art can make various modifications to the above-described embodiment in terms of shape, material, quantity, and other detailed configurations without departing from the scope of the technical idea and purpose of the present invention. Therefore, the description of the shape, material, etc. disclosed above that limits the present invention is illustrative and is not intended to limit the present invention, and therefore the description of the names of components that are free from some or all of the limitations on the shape, material, etc. is included in the present invention. EXAMPLES

[0086] Examples of the present invention will now be described in detail below. In these examples, a single crystal wafer was manufactured using a LT single crystal.

[0087] [Example 1] First, an LT single crystal ingot was sliced ​​with a wire saw and reduced to prepare five LT single crystal wafers with a thickness of 200 μm and a diameter of 4 inches (100.16 mm). First, a beveling process was performed to process the side edge of the single crystal wafer W2 into a round shape (semicircular shape) with a curvature radius R = 100 μm. Next, both sides of the single crystal wafer were ground in a lapping process.

[0088] Next, the edge polishing process was performed using the device of the embodiment described above. A new polishing cloth 212 was attached to the sponge roller 211. The sponge roller 211 was made of polyurethane with a diameter of 35 mm and a height of 50 mm, and had a hardness of Asker C11. The polishing cloth 212 had a base material made of a resin cured material with a thickness of 0.3 mm and a brush part with a thickness of 0.5 mm, and was a polishing cloth to which diamond abrasive grains were fixed. The grit sizes were #1500 (polishing cloth 212a) and #3000 (polishing cloth 212b). The polishing cloths 212a and 212b were each 25 mm high. In the height direction of the polishing cloths 212a and 212b, the central 15 mm area with 5 mm above and below was used for polishing. A 200 μm thick single crystal wafer was polished by leaving a 200 μm margin and moving the position of contact with the polishing cloth at a pitch of 400 μm per wafer. In other words, it was set up so that 38 single crystal wafers could be processed along the height of one polishing cloth.

[0089] First, the polishing cloth was subjected to a break-in process. The dummy wafers used were of the same shape as the single crystal wafers that had been beveled. In other words, 38 LT single crystal wafers with a thickness of 200 μm, a semicircular side edge of the dummy wafer, and a curvature radius R of the semicircular part set to 100 μm were used as the dummy wafers.

[0090] The dummy wafers were subjected to polishing processing using new polishing cloths one by one. At this time, the rotation speed of the polishing body was set to 2200 rpm, and the polishing body was pressed against the dummy wafer to imitate the polishing body. The polishing cloths were used in two stages, #1500 (polishing cloth 212a) and #3000 (polishing cloth 212b). The dummy wafer was also rotated simultaneously with the rotation of the polishing body, and the rotation speed was 4 rpm when using the #1500 polishing cloth, and 2 rpm when using the #3000 polishing cloth. In addition, at this time, pure water was supplied as a processing liquid to the contact point between the dummy wafer and the polishing body. In this way, the dummy wafer was polished by 15 μm in the diameter direction of the dummy wafer (30 μm including both ends of the side of the dummy wafer). The above polishing conditions were the same as those for the polishing of the single crystal wafer.

[0091] Using the polishing cloth that had been run-in as described above, five single crystal wafers were subjected to edge polishing. As described above, the polishing conditions were the same as those of the polishing cloth run-in process using a dummy wafer. The radius of curvature of the side edge of the single crystal wafer before and after edge polishing (edge ​​curvature radius of the single crystal wafer) and the radius of curvature of the side edge of the dummy wafer after run-in (edge ​​curvature radius of the dummy wafer) were measured using an edge profiler (manufactured by Yuhi Electronics Co., Ltd.), and the average values ​​of five single crystal wafers and 38 dummy wafers were calculated. In addition, the maximum value of the edge curvature radius of the single crystal wafer after edge polishing was confirmed. In addition, the quality of the edge shape of the single crystal wafer after the edge polishing process was judged as follows. The results of the above are shown in Table 1. In terms of the quality of the end face shape, when single crystal wafers with an end curvature radius of 125 μm or more were included, the end curvature radius was deemed too large and unsuitable for subsequent processing, and was rated as “bad.” When all of the end curvature radii of the obtained single crystal wafers were less than 125 μm, the end face shape was rated as “good.”

[0092] [Examples 2 to 5] Examples 2 to 5 were performed in the same manner as Example 1, except that the polishing cloth installed in the edge polishing device was replaced with a new polishing cloth, and the dummy wafer used in Example 1 was repeatedly used without replacement. That is, in Example 2, the dummy wafer used in Example 1 was repeatedly used, and in Example 5, the dummy wafer used in Examples 1, 2, 3, and 4 was repeatedly used. Table 1 shows the measurement results of the average value of the edge curvature radius of the single crystal wafer before and after edge polishing, the average value of the edge curvature radius of the dummy wafer after break-in processing, the maximum value of the edge curvature radius of the single crystal wafer after edge polishing, and the result of the pass / fail judgment of the single crystal wafer after the edge polishing process.

[0093] [Comparative Example 1] In Comparative Example 1, a new polishing cloth was not run-in processed using a dummy wafer, and the edge polishing process of the single crystal wafer was performed as is. The other conditions were the same as in Example 1. Table 1 shows the average value of the edge curvature radius of the single crystal wafer before and after edge polishing, the measurement results of the maximum value of the edge curvature radius of the single crystal wafer after edge polishing, and the result of the pass / fail judgment of the single crystal wafer after the edge polishing process.

[0094] [Table 1]

[0095] According to the results in Table 1, the average value of the radius of curvature of the end (the end of the single crystal wafer subjected to the beveling process) before the edge polishing was 103.0 μm to 105.2 μm, and both the examples and the comparative examples had similar shapes. Here, in the comparative example 1 in which the break-in process was not performed, the average value of the end curvature radius after the edge polishing was 122.4 μm, and the maximum value was 129 μm, and a single crystal wafer unsuitable for the post-processing was obtained. On the other hand, in the examples 2 to 5 in which the break-in process of the polishing cloth was performed using a dummy wafer, the average value of the end curvature radius was 120.0 to 121.6 μm, and the maximum value was 123 μm to 124 μm, and the shape of the end was maintained in the single crystal wafer after the edge polishing, and all the single crystal wafers were suitable for use in the post-processing. This shows that a single crystal wafer having a desired end curvature radius can be stably obtained by performing the break-in process using a dummy wafer on the polishing cloth.

[0096] In addition, in Examples 2 to 5, although the edge curvature radius of the dummy wafer gradually increases, the curvature radius of the obtained single crystal wafer does not increase and maintains a nearly constant curvature radius, which indicates that the dummy wafer can be used repeatedly.

[0097] (summary) The results of Examples 1 to 5, which are exemplary aspects of the present invention, show that when edge polishing is performed on the beveled end surface of a single crystal wafer, the rounded end surface of the single crystal wafer can be prevented from becoming flatter than the original shape due to polishing, the shape of the end of the single crystal wafer can be maintained, and a single crystal wafer of a desired shape can be obtained. It was also shown that the dummy wafer can be repeatedly used in multiple break-in processes. [Explanation of symbols]

[0098] 210 Polishing body 211 Sponge roller (roll) 212 Polishing cloth 213 Base material 214 Brush section 214a Contact trace 215 Polished surface 220 Table W3 Single crystal wafer (piezoelectric oxide single crystal wafer) 30 Edge surface of single crystal wafer W3 D Dummy wafer Da Edge of dummy wafer D

Claims

1. an abrasive cloth conditioning process in which an unused abrasive cloth having a brush-like abrasive surface is wound around a side surface of a cylindrical roll of the edge polishing device, the abrasive cloth being rotated around the axis of the roll while the abrasive surface is brought into contact with an edge surface of a dummy wafer rotating around a central axis parallel to the axis of the roll, thereby forming a contact mark of the edge surface of the dummy wafer on the abrasive surface; an edge polishing step of mirror-polishing an edge surface of the piezoelectric oxide single crystal wafer after the beveling step using the polishing cloth after the polishing cloth conditioning step; the edge polishing step is a step of bringing the end face of the piezoelectric oxide single crystal wafer into contact with the polishing surface along a portion of the polishing surface on which the contact mark is formed after the polishing cloth conditioning step, A method for edge polishing a piezoelectric oxide single crystal wafer, in which a dummy wafer does not hold abrasive grains.

2. 2. The method for polishing edges of a piezoelectric oxide single crystal wafer according to claim 1, wherein the dummy wafer is repeatedly used in the polishing cloth conditioning step.

3. 3. The method for edge polishing a piezoelectric oxide single crystal wafer according to claim 1, wherein the shape of the side edge of the dummy wafer is an arc shape with a radius of curvature of 0.5 to 0.63 times the thickness of the dummy wafer.

4. 4. The method for edge polishing a piezoelectric oxide single crystal wafer according to claim 1, wherein the conditions for bringing the polishing cloth into contact with the dummy wafer in the polishing cloth conditioning step are the same as the conditions for bringing the polishing cloth into contact with the piezoelectric oxide single crystal wafer in the edge polishing step.

5. 5. The method for edge polishing a piezoelectric oxide single crystal wafer according to claim 1, wherein the dummy wafer is made of the same oxide single crystal as the piezoelectric oxide single crystal wafer.

6. A method for producing a piezoelectric oxide single crystal wafer, comprising the method for edge polishing a piezoelectric oxide single crystal wafer according to any one of claims 1 to 5.

Citation Information

Patent Citations

  • Method and apparatus for formation of specular chamfered part at semiconductor wafer

    JP1998189510A

  • Dressing wheel and dressing method for grinding member

    JP2005081513A

  • Dressing tool for abrasive cloth

    JP2006075922A

  • Truing tool of grinding wheel and its manufacturing method, truing device using the same, method of manufacturing grinding wheel and wafer edge grinding device

    JP2009142979A

  • Dressing plate for abrasive cloth, method of dressing abrasive cloth, and method of grinding semiconductor substrate

    JP2009269150A