Adhesive composition, adhesive, and adhesive tape
An adhesive composition with specific monomer units and dual crosslinking agents addresses the challenge of maintaining strong adhesion and stability with EPDM under harsh conditions, offering improved durability and stability for difficult-to-bond materials.
Patent Information
- Application Number
- JP2020516482
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-03-19
- Filing Date
- 2020-03-17
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2040-03-17
AI Technical Summary
Conventional acrylic resin-based adhesives struggle to provide sufficient adhesion and stability under high temperature and high humidity conditions, particularly with difficult-to-bond materials like ethylene propylene diene rubber (EPDM), and existing solutions fail to maintain strong holding power in such environments.
An adhesive composition comprising an acrylic resin with specific terminal carboxy group-containing monomer units, (meth)acrylic acid monomer units, and hydroxyl group-containing monomer units, crosslinked with both epoxy and isocyanate crosslinking agents, enhancing adhesion and stability to EPDM and other difficult-to-bond materials.
The composition achieves strong adhesion and maintains high holding power even under high temperature and high humidity conditions, suitable for applications requiring durability and stability, such as outdoor use with EPDM materials.
Smart Images

Figure 0007567474000001 
Figure 0007567474000002 
Figure 0007567474000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a pressure-sensitive adhesive composition, and more specifically to a pressure-sensitive adhesive composition which has high adhesion to high-polarity adherends, low-polarity adherends and rubber-based difficult-to-adhere adherends, in particular ethylene propylene diene rubber (EPDM), and which has excellent holding power stability under high temperature and high humidity conditions, and to a pressure-sensitive adhesive and pressure-sensitive adhesive tape using the same. [Background technology]
[0002] Conventionally, pressure-sensitive adhesives and pressure-sensitive adhesive tapes using acrylic resins have been used in a wide range of applications, such as packaging tapes such as craft tapes, OPP (Oriented Poly Propylene) tapes, and cloth adhesive tapes, cellophane adhesive tapes for light packaging, temporary fixing tapes, foam tapes for automobiles, vibration-damping sheets, removable double-sided tapes, protective tapes for housing, soundproofing seals, double-sided tapes for fixing carpets, temporary fixing tapes, vinyl tapes for electrical insulation, outdoor anticorrosive tapes, tapes for indoor displays, anti-slip tapes, various masking tapes, various surface protection tapes, airtight waterproof adhesive tapes, adhesive substrates for medical first aid bandages and the like, surgical tapes, adhesive bandages, tapes for electrical and electronic devices, double-sided tapes for optics, surface protection films, dicing tapes for semiconductors, heat conductive tapes, heat resistant tapes, conductive tapes, and the like.
[0003] The acrylic resin used in the above-mentioned pressure-sensitive adhesives and pressure-sensitive adhesive tapes is generally an acrylic resin copolymerized with alkyl (meth)acrylate as the main component. Also, acrylic resins using a carboxyl group-containing monomer as a copolymerization component to improve adhesion to adherends are known.
[0004] Furthermore, in order to improve the adhesion to the adherend, it has been proposed to use an acrylic acid adduct having a specific structure as a carboxy group-containing monomer (see, for example, Patent Documents 1 to 3). [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Japanese Patent Application Publication No. 2-196879 [Patent Document 2] JP 2008-127431 A [Patent Document 3] JP 2014-40500 A Summary of the Invention [Problem to be solved by the invention]
[0006] In the technology disclosed in the above Patent Document 1, a specific acrylic acid adduct is contained in a relatively large amount as a copolymerization component, thereby improving the adhesive strength to adherends with high polarity and adherends with low polarity. However, the adherend with low polarity that has been specifically evaluated is polypropylene, and the technology has not been evaluated for adherends with poor adhesion such as ethylene propylene diene rubber (EPDM), for which it is more difficult to improve the adhesive strength.
[0007] The technology disclosed in the above Patent Document 2 describes that an adhesive composition containing an acrylic resin having an acid value of 1 to 50 mgKOH / g, a hydroxyl value of 10 to 60 mgKOH / g, and a number average molecular weight of 50,000 to 500,000, copolymerized with an acrylic acid adduct, and a polyisocyanate compound, can provide an adhesive composition having excellent adhesion and adhesion retention over time, moisture and heat resistance, heat resistance, and rework adhesion. However, specifically, the content of the acrylic acid adduct is a relatively small content of 1% by weight relative to the copolymerization components, which is insufficient to improve the adhesive strength. In addition, the adherend in Patent Document 2 is adhered to a glass substrate or the like, which is different from an adherend that is difficult to adhere to.
[0008] The technology disclosed in the above Patent Document 3 describes that in a pressure-sensitive adhesive composition containing an acrylic resin (A) obtained by using a (meth)acrylic acid alkyl ester, a (meth)acrylic monomer having a carboxy group, and a (meth)acrylic monomer having a hydroxyl group, a solvent (B), and a crosslinking agent (C), the (meth)acrylic monomer having a carboxy group contains (meth)acrylic acid and a (meth)acrylic monomer having 2 to 6 carbonyl groups, and that the pressure-sensitive adhesive composition has little loss of adhesive strength and holding power even in a high temperature environment. However, no consideration is given to adhesive strength and holding power to poorly adhesive adherends, and the results are still unsatisfactory.
[0009] Furthermore, none of the above disclosed techniques take into consideration the stability of holding power to poorly adhesive substrates under high temperature and high humidity conditions, and the stability of holding power under high temperature and high humidity conditions is still unsatisfactory.
[0010] In general, adhesive tapes using acrylic resins exhibit excellent adhesion to highly polar substrates, but do not exhibit sufficient adhesion to poorly adhesive rubber substrates, especially substrates with low polarity such as ethylene propylene diene rubber (EPDM). For this reason, when adhesive tapes are used for the purpose of airtightness and waterproofing of seams of polymer roof sheet materials, such as sheets made of poorly adhesive materials such as ethylene propylene diene rubber (EPDM), butyl rubber (IIR), chloroprene rubber (CR), thermoplastic polyolefin rubber, modified asphalt, and sheets made of polyvinyl chloride and chlorinated polyethylene, adhesive tapes made of butyl rubber and asphalt, which have high adhesiveness to these poorly adhesive adherends, are used. However, adhesive tapes made of butyl rubber and adhesive tapes made of asphalt have problems such as poor durability and heat resistance, weakness against shear force, and poor creep (holding force) under a certain stress, causing the sheet to slip. In addition, tapes made of conventional acrylic adhesive compositions have been rarely used because of their poor adhesion to poorly adhesive adherends such as polymer roof sheet materials. However, there is a demand in the market for a tape using an acrylic pressure-sensitive adhesive composition that has adhesiveness equivalent to that of pressure-sensitive adhesive tapes using butyl rubber or pressure-sensitive adhesive tapes using asphalt, and that has improved holding power, when used on difficult-to-adhere substrates such as polymer roof sheeting materials. The adhesive tape is required to adhere firmly to low-polarity, poorly adhesive adherends such as EPDM, and to have a high holding power so that sheets, etc., fixed with the tape do not slip. Furthermore, considering that the tape will be used outdoors, the adhesive tape is required to have a stable holding power even when exposed to high temperature and humidity conditions.
[0011] Under these circumstances, the present invention provides a pressure-sensitive adhesive composition that firmly adheres to poorly adhesive substrates such as ethylene propylene diene rubber (EPDM), has high holding power, and stably maintains the high holding power even when exposed to high temperature and high humidity. [Means for solving the problem]
[0012] However, the present inventors have conducted extensive research in light of these circumstances and have found that, in a pressure-sensitive adhesive composition using an acrylic resin, when the acrylic resin contains specific terminal carboxy group-containing monomer units, (meth)acrylic acid monomer units and hydroxyl group-containing monomer units, and contains both an epoxy-based crosslinking agent and an isocyanate-based crosslinking agent, the pressure-sensitive adhesive composition adheres firmly to poorly adhesive rubber-based adherends, particularly poorly adhesive adherends such as EPDM, has high holding power, and further stably maintains its high holding power even when exposed to high temperature and high humidity.
[0013] That is, a first gist of the present invention is a pressure-sensitive adhesive composition characterized by containing an acrylic resin (A) containing a terminal carboxyl group-containing monomer (a1) unit, a (meth)acrylic acid monomer (a2) unit, and a hydroxyl group-containing monomer (a3) unit, which are represented by the following general formula (1):
[0014] [ka]
[0015] Furthermore, a second aspect of the present invention is a pressure-sensitive adhesive obtained by crosslinking the pressure-sensitive adhesive composition according to the first aspect above, and a third aspect of the present invention is a pressure-sensitive adhesive tape obtained by forming the pressure-sensitive adhesive according to the second aspect above on a substrate.
[0016] It is generally known that adhesive strength is improved by having a terminal carboxyl group-containing monomer (a1) unit represented by the above general formula (1) in a pressure-sensitive adhesive composition. The present inventors have also found that when a poorly adhesive adherend such as a rubber-based one, particularly an ethylene propylene diene rubber (EPDM), is used as the adherend, the holding power can be improved by using an acrylic resin (A) having a specific terminal carboxyl group-containing monomer (a1) unit, and have further found that a pressure-sensitive adhesive composition having stable holding power against poorly adhesive adherends even when exposed to high temperature and high humidity can be obtained by combining an acrylic resin (A) having a (meth)acrylic acid monomer (a2) unit and a hydroxyl group-containing monomer (a3) unit with an epoxy crosslinking agent (b1) and an isocyanate crosslinking agent (b2). Effect of the Invention
[0017] The present invention is a pressure-sensitive adhesive composition containing an acrylic resin (A) containing a terminal carboxyl group-containing monomer (a1) unit, a (meth)acrylic acid monomer (a2) unit, and a hydroxyl group-containing monomer (a3) unit, represented by the following general formula (1), an epoxy-based crosslinking agent (b1), and an isocyanate-based crosslinking agent (b2), and therefore has good adhesion and holding power to poorly adhesive rubber-based adherends, particularly poorly adhesive adherends such as EPDM, and further has stable holding power even when exposed to high temperature and high humidity. Therefore, it is useful as various pressure-sensitive adhesives and pressure-sensitive adhesive tapes used for poorly adhesive adherends, and can be suitably used as pressure-sensitive adhesive tapes for fixing EPDM sheets and the like used in buildings, etc. [ka]
[0018] In particular, among the pressure-sensitive adhesive compositions of the present invention, those having a gel fraction of 30% by weight or more when crosslinked can have superior adhesion and holding power to an adherend.
[0019] In the present invention, particularly when the acrylic resin (A) is an acrylic resin having the following monomer units (a1) to (a4), the adhesiveness and holding power to the adherend can be more excellent. (a1) 1 to 20% by weight of a terminal carboxyl group-containing monomer unit represented by the above general formula (1) (a2) (meth)acrylic acid monomer unit 0.1 to 5% by weight (a3) Hydroxyl group-containing monomer unit: 0.01 to 5% by weight (a4) 55 to 97% by weight of (meth)acrylate monomer units having an alkyl group having 4 to 24 carbon atoms
[0020] In the present invention, particularly, when the content of the (meth)acrylic acid monomer (a2) units per 100 parts by weight of the terminal carboxyl group-containing monomer (a1) units represented by the general formula (1) is 10 to 400 parts by weight, the adhesiveness to the adherend can be improved.
[0021] Furthermore, in the present invention, when the content of the epoxy-based crosslinking agent (b1) is 2.5 to 25 parts by weight per 100 parts by weight of the isocyanate-based crosslinking agent (b2), the stability of the holding power to the adherend under high temperature and high humidity conditions can be improved.
[0022] In the present invention, when the composition contains a tackifier (C), the adhesiveness to the adherend can be made even more excellent.
[0023] The pressure-sensitive adhesive composition of the present invention can also be used as a material suitable for use on poorly adherends.
[0024] Furthermore, the pressure-sensitive adhesive obtained by crosslinking the pressure-sensitive adhesive composition can have superior adhesion to an adherend.
[0025] In the present invention, when the gel fraction is 30% by weight or more, the adhesiveness and holding power to the adherend can be more excellent. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0026] The present invention will be described in detail below. In the present invention, "(meth)acrylic" means acrylic or methacrylic, "(meth)acryloyl" means acryloyl or methacryloyl, and "(meth)acrylate" means acrylate or methacrylate. The acrylic resin is a resin obtained by polymerizing a copolymerization component containing at least one (meth)acrylate monomer.
[0027] The pressure-sensitive adhesive composition of the present invention contains an acrylic resin (A) having a specific monomer unit.
[0028] <Acrylic resin (A)> The acrylic resin (A) used in the present invention has terminal carboxyl group-containing monomer (a1) units, (meth)acrylic acid monomer (a2) units, and hydroxyl group-containing monomer (a3) units, as shown in the following general formula (1).
[0029] [Monomer (a1) unit] The monomer (a1) unit of the present invention is a terminal carboxyl group-containing monomer unit represented by the following general formula (1).
[0030] [ka]
[0031] Above R 1 is preferably hydrogen, R 2 The hydrocarbon is usually preferably an alkylene, such as a methylene group, having 1 to 10 carbon atoms, more preferably 1 to 5, and particularly preferably 1 to 2 carbon atoms, such as phenyl, phenylene, or further preferably ethylene, and the above n is preferably 1 to 10, more preferably 1 to 5, particularly preferably 1 to 3, and particularly preferably 1 to 2, and may have a combination of these.
[0032] The content of the monomer (a1) unit in the acrylic resin (A) is usually 1 to 20% by weight, particularly 1.5 to 15% by weight, and more preferably 2 to 8.5% by weight. If the content is too low or high, the adhesion to poorly adherends tends to decrease.
[0033] The acrylic resin (A) having the above monomer (a1) units can be obtained by polymerization using a monomer of the following chemical formula (2) as a copolymerizable monomer. [Formula] CH2=CR 1 -CO-O-(R 2 -COO-) n H (2) (where R 1 is hydrogen or a methyl group, R 2 represents a divalent saturated aliphatic group, an unsaturated aliphatic group, an aromatic group, a saturated alicyclic group, or an unsaturated alicyclic hydrocarbon group, and n represents a positive number of 1 or more.
[0034] [Monomer (a2) unit] The content of the (meth)acrylic acid monomer (a2) unit is usually 0.1 to 5% by weight, particularly 0.5 to 4.5% by weight, and more preferably 1 to 4% by weight, of the entire acrylic resin (A). If the content is too low, the adhesiveness to poorly adhered adherends tends to decrease, whereas if the content is too high, the adhesiveness to poorly adhered adherends tends to decrease.
[0035] The ratio of the monomer (a1) unit to the monomer (a2) unit is preferably, by weight, usually 10 to 400 parts by weight, particularly 20 to 200 parts by weight, further 25 to 100 parts by weight, and particularly 30 to 75 parts by weight, of the monomer (a2) unit per 100 parts by weight of the monomer (a1) unit. If the monomer (a2) unit is too small, the holding power tends to decrease, whereas if it is too large, the adhesion to poorly adhered adherends tends to decrease.
[0036] [Monomer (a3) unit] Examples of copolymerizable monomers for forming the hydroxyl group-containing monomer (a3) units include (meth)acrylic acid hydroxyalkyl esters such as 2-hydroxyethyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 5-hydroxypentyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, and 8-hydroxyoctyl (meth)acrylate; caprolactone-modified monomers such as caprolactone-modified 2-hydroxyethyl (meth)acrylate; oxyalkylene-modified monomers such as diethylene glycol (meth)acrylate and polyethylene glycol (meth)acrylate; primary hydroxyl group-containing monomers such as 2-acryloyloxyethyl-2-hydroxyethyl phthalate; secondary hydroxyl group-containing monomers such as 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, and 3-chloro-2-hydroxypropyl (meth)acrylate; and tertiary hydroxyl group-containing monomers such as 2,2-dimethyl-2-hydroxyethyl (meth)acrylate.
[0037] Among these, primary hydroxyl group-containing monomers are preferred because of their excellent reactivity with crosslinking agents, and in particular, hydroxyalkyl (meth)acrylates, 2-hydroxyethyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate are preferred.
[0038] The hydroxyl group-containing monomer (a3) unit is useful because it becomes a crosslinking point with the isocyanate-based crosslinking agent (b2). The hydroxyl group-containing monomer (a3) unit is usually 0.01 to 5% by weight, particularly 0.05 to 3% by weight, and more preferably 0.05 to 2% by weight, based on the total acrylic resin (A). If the monomer (a3) unit is too small, the holding power tends to decrease, and if it is too large, the adhesion to a poorly adhered adherend tends to decrease.
[0039] [Monomer (a4) unit] The acrylic resin (A) used in the present invention preferably further contains a (meth)acrylate monomer (a4) unit having an alkyl group having 4 to 24 carbon atoms. The copolymerizable monomer for forming the (meth)acrylate monomer (a4) unit having an alkyl group having 4 to 24 carbon atoms preferably contains a (meth)acrylate monomer (a4-1) having an alkyl group having 4 to 7 carbon atoms and a (meth)acrylate monomer (a4-2) having an alkyl group having 8 to 24 carbon atoms.
[0040] Examples of the (meth)acrylate monomer (a4-1) having an alkyl group having 4 to 7 carbon atoms include n-butyl (meth)acrylate, t-butyl (meth)acrylate, isobutyl (meth)acrylate, n-hexyl (meth)acrylate, etc. Among these, n-butyl (meth)acrylate is preferred because it is easily available and economically advantageous.
[0041] Examples of the (meth)acrylate monomer (a4-2) having an alkyl group having 8 to 24 carbon atoms include 2-ethylhexyl (meth)acrylate, n-octyl (meth)acrylate, isooctyl (meth)acrylate, isononyl (meth)acrylate, isodecyl (meth)acrylate, lauryl (meth)acrylate, tridecyl (meth)acrylate, isotridecyl (meth)acrylate, myristyl (meth)acrylate, isomyristyl (meth)acrylate, cetyl (meth)acrylate, stearyl (meth)acrylate, isostearyl (meth)acrylate, and behenyl (meth)acrylate. Among these, (meth)acrylates having an alkyl group having 8 to 12 carbon atoms are preferred because of their low polarity and low glass transition temperature, and 2-ethylhexyl (meth)acrylate is particularly preferred.
[0042] The content of the monomer (a4) unit is usually 55 to 97% by weight, particularly 70 to 95% by weight, and further preferably 80 to 93% by weight, of the entire acrylic resin (A). If the content is too low, the adhesiveness to poorly adherends tends to decrease, whereas if the content is too high, the adhesiveness and holding power tend to decrease.
[0043] The ratio of the monomer (a4-1) units to the monomer (a4-2) units is preferably, by weight, (a4-1) / (a4-2)=1 / 99 to 85 / 15, particularly 2 / 98 to 75 / 25, further 3 / 97 to 70 / 30, particularly 5 / 95 to 60 / 40, and particularly 5 / 95 to 45 / 55. If the ratio of the monomer (a4-1) units is too small, the holding power tends to decrease, whereas if it is too large, the adhesion to poorly adhered adherends tends to decrease.
[0044] [Monomer (a5) unit] The acrylic resin (A) used in the present invention preferably further contains (meth)acrylate monomer (a5-1) units having an alkyl group with 1 to 3 carbon atoms, cyclic structure-containing monomer (a5-2) units, or vinyl ester monomer (a5-3) units having 3 to 10 carbon atoms. The collective term for the above (a5-1) to (a5-3) is monomer (a5).
[0045] Examples of copolymerizable monomers for forming the (meth)acrylate monomer (a5-1) units having an alkyl group having 1 to 3 carbon atoms include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, etc. Among these, methyl (meth)acrylate and ethyl (meth)acrylate are preferred.
[0046] The copolymerizable monomer for forming the cyclic structure-containing monomer (a5-2) unit is usually an acrylic monomer having a substituent containing a cyclic structure, and examples thereof include heterocycle-containing (meth)acrylates having a heterocycle such as a morpholine ring, a piperidine ring, a pyrrolidine ring, or a piperazine ring, such as N-(meth)acryloylmorpholine, N-vinylpyrrolidone, N-vinylcaprolactam, vinylpyrrolidone, N-(meth)acryloylpiperidine, and N-(meth)acryloylpyrrolidine, phenyl(meth)acrylate, phenoxyethyl(meth)acrylate, and phenyldiethylene glycol (meth)acrylate. ) acrylate, 2-hydroxy-3-phenoxypropyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, benzyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, dicyclopentanyl (meth)acrylate, nonylphenol polyethylene glycol (meth)acrylate, nonylphenoxy polyethylene glycol (meth)acrylate, isobornyl (meth)acrylate, biphenyloxyethyl (meth)acrylate, and others, such as styrene and α-methylstyrene. Among them, heterocycle-containing (meth)acrylates having a morpholine ring are preferred because of their good balance of various physical properties, and N-(meth)acryloylmorpholine is particularly preferred because of its ease of availability and safety.
[0047] Examples of copolymerizable monomers for forming the vinyl ester monomer (a5-3) units having 3 to 10 carbon atoms include vinyl formate, vinyl acetate, vinyl propionate, vinyl valerate, vinyl butyrate, vinyl isobutyrate, vinyl pivalate, etc. Among these, vinyl acetate is preferred because of its easy availability.
[0048] The content of the monomer (a5) unit is usually 11% by weight or less, preferably 10% by weight or less, and particularly preferably 8% by weight or less, based on the total acrylic resin (A). If the content of the (a5) component is too high, the adhesion to the adherend tends to decrease. The lower limit of the content of the (a5) component in the copolymerization component (a) is usually 1% by weight.
[0049] [Monomer (a6) unit] In the present invention, the copolymerizable monomer may have other copolymerizable monomer (a6) units as necessary. Examples of the copolymerizable monomer for forming the other copolymerizable monomer (a6) units include functional group-containing monomers such as acetoacetyl group-containing monomers, isocyanate group-containing monomers, glycidyl group-containing monomers, amino group-containing monomers, and amide group-containing monomers, as well as other copolymerizable monomers.
[0050] Examples of the acetoacetyl group-containing monomer include 2-(acetoacetoxy)ethyl (meth)acrylate and allyl acetoacetate.
[0051] Examples of the isocyanate group-containing monomer include 2-acryloyloxyethyl isocyanate, 2-methacryloyloxyethyl isocyanate, and alkylene oxide adducts thereof.
[0052] Examples of the glycidyl group-containing monomer include glycidyl (meth)acrylate and allyl glycidyl (meth)acrylate.
[0053] Examples of the amino group-containing monomer include monomers having an ethylenically unsaturated double bond and an amino group (unsubstituted or substituted amino group), such as mono-substituted amino group-containing (meth)acrylic acid esters of aminoalkyl (meth)acrylates such as aminomethyl (meth)acrylate, aminoethyl (meth)acrylate, aminopropyl (meth)acrylate, and aminoisopropyl (meth)acrylate, and (meth)acrylic acid esters of N-alkylaminoalkyl such as N-(t-butyl)aminoethyl (meth)acrylate; (meth)acrylic acid esters of N,N-dialkylaminoalkyl such as N,N-dimethylaminoethyl (meth)acrylate, N,N-diethylaminoethyl (meth)acrylate, and N,N-dimethylaminopropyl (meth)acrylate. disubstituted amino group-containing (meth)acrylic acid esters such as N,N-dimethylaminopropyl(meth)acrylamide; dialkylaminoalkyl(meth)acrylamides such as N,N-dimethylaminopropyl(meth)acrylamide, and quaternary salts of these amino group-containing monomers; amino group-containing styrenes such as p-aminostyrene; styrenes having a dialkylamino group such as 3-(dimethylamino)styrene and dimethylaminomethylstyrene; dialkylaminoalkyl vinyl ethers such as N,N-dimethylaminoethyl vinyl ether and N,N-diethylaminoethyl vinyl ether; allylamine, 4-diisopropylamino-1-butene, trans-2-butene-1,4-diamine, 2-vinyl-4,6-diamino-1,3,5-triazine, and the like.
[0054] The amide group-containing monomer includes a monomer having an ethylenically unsaturated double bond and an amide group (a group having an amide bond), such as (meth)acrylamide; N-methyl(meth)acrylamide, N-ethyl(meth)acrylamide, N-propyl(meth)acrylamide, N-isopropyl(meth)acrylamide, Nn-butyl(meth)acrylamide, N-isobutyl(meth)acrylamide, Ns-butyl(meth)acrylamide, Nt-butyl(meth)acrylamide, N-hexyl(meth)acrylamide, da N-alkyl(meth)acrylamides such as acetone(meth)acrylamide, N,N'-methylenebis(meth)acrylamide, and N-(1,1-dimethyl-3-oxobutyl)(meth)acrylamide; N,N-dimethyl(meth)acrylamide, N,N-diethyl(meth)acrylamide, N,N-dipropyl(meth)acrylamide, N,N-diisopropyl(meth)acrylamide, N,N-di(n-butyl)(meth)acrylamide, N,N-diisobutyl(meth)acrylamide, and N,N-di(s-butyl)(meth)acrylamide; amide, N,N-dialkyl (meth)acrylamides such as N,N-di(t-butyl) (meth)acrylamide, N,N-dipentyl (meth)acrylamide, N,N-dihexyl (meth)acrylamide, N,N-diheptyl (meth)acrylamide, N,N-dioctyl (meth)acrylamide, N,N-diallyl (meth)acrylamide, and N,N-ethylmethylacrylamide; dialkylaminoalkyl (meth)acrylamides such as N,N-dimethylaminopropyl (meth)acrylamide; N-vinylacetamide, N-vinyl phosphatase, and the like. Examples of such amide group-containing monomers include substituted amide group-containing monomers such as N-methylol (meth)acrylamide, (meth)acrylamide ethyl ethylene urea, and (meth)acrylamide-t-butylsulfonic acid; hydroxy group-containing (meth)acrylamides such as N-methylol (meth)acrylamide, N-hydroxyethyl (meth)acrylamide, and N-methylolpropane (meth)acrylamide; alkoxy group-containing (meth)acrylamides such as N-methoxymethyl (meth)acrylamide and N-(n-butoxymethyl) (meth)acrylamide; and quaternized salts of these amide group-containing monomers.
[0055] Examples of the other copolymerizable monomers include monomers containing an alkoxy group or an oxyalkylene group, such as 2-methoxyethyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, methoxydiethylene glycol (meth)acrylate, ethoxydiethylene glycol (meth)acrylate, methoxypolyethylene glycol (meth)acrylate, and polypropylene glycol mono(meth)acrylate; acrylonitrile, methacrylonitrile, vinyl stearate, vinyl chloride, vinylidene chloride, alkyl vinyl ether, vinyl toluene, dialkyl itaconate, dialkyl fumarate, allyl alcohol, acrylic chloride, methyl vinyl ketone, allyl trimethylammonium chloride, and dimethylallyl vinyl ketone.
[0056] The other copolymerizable monomers (a6) may be contained to such an extent that the effects of the present invention are not adversely affected, for example, 10% by weight or less, in order to adjust the physical properties according to the application.
[0057] Thus, the acrylic resin (A) is obtained by polymerizing the above monomers (a1) to (a3), preferably the monomer (a4), and if necessary, the monomers (a5) to (a6). That is, the acrylic resin (A) is obtained which has the above monomers (a1) to (a3) units, preferably the monomer (a4), and if necessary, the monomers (a5) to (a6). The monomers (a1) to (a6) may each be present alone or in combination of two or more kinds.
[0058] In the above polymerization, production by solution polymerization is preferred, since it allows the acrylic resin (A) to be produced safely and stably with any monomer composition.
[0059] Such solution polymerization may be carried out according to a conventional method, for example, by mixing or dropping copolymerization components such as the monomers (a1) to (a6) and a polymerization initiator into an organic solvent, and polymerizing the mixture under reflux or at 50 to 98° C. for 0.1 to 20 hours.
[0060] Specific examples of such polymerization initiators include azo-based polymerization initiators such as azobisisobutyronitrile and azobisdimethylvaleronitrile, which are normal radical polymerization initiators, and peroxide-based polymerization initiators such as benzoyl peroxide, lauroyl peroxide, di-t-butyl peroxide, and cumene hydroperoxide. These may be used alone or in combination of two or more. The amount of the polymerization initiator used is usually 0.001 to 5 parts by weight based on 100 parts by weight of the copolymerization components.
[0061] The weight-average molecular weight of the acrylic resin (A) thus obtained is usually 100,000 to 5,000,000, preferably 300,000 to 1,500,000, and particularly preferably 400,000 to 900,000. If the weight-average molecular weight is too small, the durability tends to decrease, and if it is too large, the adhesive strength tends to decrease.
[0062] The dispersity (weight average molecular weight / number average molecular weight) of the acrylic resin (A) is preferably 20 or less, particularly preferably 15 or less, further preferably 10 or less, and especially preferably 7 or less. If the dispersity is too high, the durability of the pressure-sensitive adhesive layer tends to decrease and foaming and the like tends to occur easily. The lower limit of the dispersity is usually 1.1 from the viewpoint of production limitations.
[0063] The weight average molecular weight of the acrylic resin (A) is a weight average molecular weight calculated based on the molecular weight of standard polystyrene. The weight average molecular weight was measured by a high performance liquid chromatograph (Waters Japan, "Waters 2695 (main body)" and "Waters 2414 (detector)") using a Shodex GPC KF-806L column (molecular weight exclusion limit: 2×10 7 , Separation range: 100~2×10 7 The number average molecular weight is measured by using three columns in series (10000 / column, theoretical plate number: 10,000 plates / column, filler material: styrene-divinylbenzene copolymer, filler particle size: 10 μm), and the same method can be used for measuring the number average molecular weight.
[0064] The glass transition temperature (Tg) of the acrylic resin (A) is preferably from -80 to 10°C, particularly from -70 to -10°C, and further preferably from -65 to -20°C. If the glass transition temperature is too high, the tack tends to be insufficient, whereas if the glass transition temperature is too low, the heat resistance tends to decrease.
[0065] The above glass transition temperature (Tg) is a value calculated by applying the glass transition temperature and weight fraction of each of the monomers constituting the acrylic resin (A) as a homopolymer to the following Fox's formula.
[0066]
number
[0067] Here, the glass transition temperature when the monomer constituting the acrylic resin (A) is made into a homopolymer is usually a value measured by a differential scanning calorimeter (DSC) using a method in accordance with JIS K7121-1987 or JIS K 6240, or a value listed in a catalog.
[0068] The acrylic resin (A) is usually adjusted in viscosity with a solvent or the like, and is used for coating as an acrylic resin (A) solution. The viscosity of the acrylic resin (A) solution is preferably 500 to 20,000 mPa·s from the viewpoint of ease of handling, particularly preferably 1,000 to 18,000 mPa·s, and more preferably 2,000 to 15,000 mPa·s. If the viscosity is too high, the fluidity tends to decrease, making handling difficult, and if the viscosity is too low, coating of the adhesive tends to be difficult. The solution concentration in this case is usually 10 to 70% by weight.
[0069] The solvent is not particularly limited as long as it dissolves the acrylic resin (A), and examples thereof include ester solvents such as methyl acetate, ethyl acetate, methyl acetoacetate, and ethyl acetoacetate, ketone solvents such as acetone, methyl ethyl ketone, and methyl isobutyl ketone, aromatic solvents such as toluene and xylene, and alcohol solvents such as methanol, ethanol, and propyl alcohol. Among these, ethyl acetate and methyl ethyl ketone, particularly ethyl acetate, are preferably used in terms of solubility, drying property, and price. These solvents may be used alone or in combination of two or more.
[0070] The viscosity of the acrylic resin (A) solution can be measured in accordance with JIS K5400 (1990), 4.5.3, rotational viscometer method.
[0071] <Crosslinking agent (B)> The pressure-sensitive adhesive composition of the present invention contains a crosslinking agent (B) in addition to the acrylic resin (A).
[0072] The crosslinking agent (B) reacts with the functional groups in the acrylic resin (A) to form a crosslinked structure. By using the epoxy crosslinking agent (b1) and the isocyanate crosslinking agent (b2) in combination, the stability of the holding power when exposed to high temperature and high humidity is excellent. The reason is not clear, but since the epoxy-based crosslinking agent (b1) has high reactivity with carboxyl groups, it reacts with the acrylic resin (A) having a terminal carboxyl group-containing monomer (a1) unit represented by the general formula (1) with a relatively long side chain from the main chain and high polarity of the side chain to form a crosslinked structure. Then, the adhesive layer after crosslinking is flexible but tough, and shows high peel strength and high holding power even against difficult-to-adhere adherends. However, when exposed to high temperature and high humidity, the holding power is likely to decrease, probably because the ester bond is the main crosslinked structure and is hydrolyzed. On the other hand, the isocyanate-based crosslinking agent (b2) has high reactivity with hydroxyl groups, so it reacts with the hydroxyl group-containing monomer (a3) unit of the acrylic resin (A) to form a crosslinked structure. Then, the crosslinked structure becomes a urethane bond with relatively high water resistance, and the holding power is stable when exposed to high temperature and high humidity. However, on the other hand, the adhesive layer is likely to become rigid, and the peel strength against difficult-to-adhere adherends is likely to decrease. In addition, the isocyanate crosslinking agent (b2) also reacts with carboxyl groups, accompanied by decarboxylation, to form amide bonds. Similar to urethane bonds, these bonds are also highly stable when exposed to high temperatures and high humidity. It is presumed that the use of an epoxy-based crosslinking agent (b1) and an isocyanate-based crosslinking agent (b2) in combination with an acrylic resin (A) containing a terminal carboxyl group-containing monomer (a1) unit, a (meth)acrylic acid monomer (a2) unit, and a hydroxyl group-containing monomer (a3) unit results in a pressure-sensitive adhesive composition that forms a pressure-sensitive adhesive layer that has high peel strength against difficult-to-adhere substrates and excellent holding power stability when exposed to high temperature and high humidity conditions, while compensating for each other's shortcomings.
[0073] Examples of the epoxy crosslinking agent (b1) include aliphatic epoxy crosslinking agents such as ethylene glycol diglycidyl ether, trimethylolpropane diglycidyl ether, and diglycidylamine; alicyclic epoxy crosslinking agents such as 1,3-bis(N,N'-diglycidylaminomethyl)cyclohexane, 1,6-hexanediol diglycidyl ether, and N,N,N',N'-tetraglycidyl-m-xylylenediamine; aromatic epoxy crosslinking agents such as diglycidylaniline; heterocyclic epoxy crosslinking agents such as 1,3,5-tris-(2,3-epoxybutyl)-isocyanurate, 1,3,5-tris-(3,4-epoxybutyl)-isocyanurate, and 1,3,5-tris-(4,5-epoxypentyl)-isocyanurate, among which alicyclic epoxy crosslinking agents are preferred. These can be used alone or in combination of two or more.
[0074] The isocyanate-based crosslinking agent (b2) contains at least two isocyanate groups, and examples thereof include aromatic polyisocyanates such as tolylene diisocyanate, diphenylmethane diisocyanate, and xylylene diisocyanate, aliphatic polyisocyanates such as hexamethylene diisocyanate, isophorone diisocyanate, and alicyclic polyisocyanates such as hydrogenated diphenylmethane diisocyanate, as well as their biuret and isocyanurate forms, and further adducts which are reaction products with low-molecular active hydrogen-containing compounds such as ethylene glycol, propylene glycol, neopentyl glycol, trimethylolpropane, and castor oil. In particular, the adduct of tolylene diisocyanate and trimethylolpropane is preferred. These can be used alone or in combination of two or more.
[0075] The content of the epoxy crosslinking agent (b1) is 0.005 to 0.028 parts by weight, particularly 0.008 to 0.025 parts by weight, and further preferably 0.012 to 0.022 parts by weight, based on 100 parts by weight of the acrylic resin (A). If the content is too low, the holding power tends to decrease, whereas if the content is too high, the adhesiveness to various adherends tends to decrease.
[0076] The content of the isocyanate crosslinking agent (b2) is 0.1 to 0.5 parts by weight, particularly 0.15 to 0.4 parts by weight, and further preferably 0.2 to 0.3 parts by weight, based on 100 parts by weight of the acrylic resin (A). If the content is too low, the holding power tends to decrease, whereas if the content is too high, the adhesion to low-polarity adherends tends to decrease.
[0077] The content ratio of the epoxy-based crosslinking agent (b1) and the isocyanate-based crosslinking agent (b2) is preferably 2.5 to 25 parts by weight, more preferably 3.5 to 15 parts by weight, and even more preferably 5 to 10 parts by weight, of the epoxy-based crosslinking agent (b1) per 100 parts by weight of the isocyanate-based crosslinking agent (b2).
[0078] The above crosslinking agent can be used after being diluted with a solvent or the like, but the above content and content ratio indicate the actual content and content ratio of the crosslinking agent excluding the solvent and the like.
[0079] The present invention is characterized by using the crosslinking agents (b1) and (b2) in combination, but in some cases, other crosslinking agents may also be used in combination. Examples of other crosslinking agents that may be used in combination include aziridine crosslinking agents, melamine crosslinking agents, aldehyde crosslinking agents, amine crosslinking agents, and metal chelate crosslinking agents. These may be used alone or in combination of two or more types, but the effects of the present invention will not be achieved with a combination of crosslinking agents that do not include the (b1) or (b2) components.
[0080] Examples of the aziridine-based crosslinking agent include diphenylmethane-4,4'-bis(1-aziridinecarboxamide), trimethylolpropane tri-β-aziridinylpropionate, tetramethylolmethane tri-β-aziridinylpropionate, toluene-2,4-bis(1-aziridinecarboxamide), triethylenemelamine, bisisophthaloyl-1-(2-methylaziridine), tris-1-(2-methylaziridine)phosphine, and trimethylolpropane tri-β-(2-methylaziridine)propionate.
[0081] Examples of the melamine-based crosslinking agent include melamine; methylolmelamine derivatives such as amino group-containing methylolmelamine, imino group-containing methylolmelamine, and hexamethylolmelamine obtained by condensing melamine with formaldehyde; and alkylated methylolmelamines such as partially or completely alkylated methylolmelamine and imino group-containing partially or completely alkylated methylolmelamine obtained by reacting a methylolmelamine derivative with a lower alcohol such as methyl alcohol or butyl alcohol to partially or completely etherify the methylolmelamine derivative.
[0082] Examples of the aldehyde crosslinking agent include aldehyde compounds that liberate aldehyde in an aqueous solution, such as formaldehyde, acetaldehyde, propionaldehyde, butylaldehyde, glyoxal, glutaraldehyde, dialdehyde starch, hexamethylenetetramine, 1,4-dioxane-2,3-diol, 1,3-bis(hydroxymethyl)-2-imidazolidine, dimethylol urea, N-methylol acrylamide, urea formalin resin, and melamine formalin resin, and aromatic aldehyde compounds, such as benzaldehyde, 2-methylbenzaldehyde, 4-methylbenzaldehyde, p-hydroxybenzaldehyde, and m-hydroxybenzaldehyde.
[0083] Examples of the amine-based crosslinking agent include 4,4'-methylene-bis(2-chloroaniline) (hereinafter abbreviated as "MOCA"), modified MOCA, and diethyltoluenediamine.
[0084] The above-mentioned metal chelate crosslinking agent can be, for example, chelate compounds whose metal atom is aluminum, zirconium, titanium, zinc, iron, tin, etc., and aluminum chelate compounds are preferred from the viewpoint of performance.As the aluminum chelate compounds, for example, diisopropoxyaluminum monooleyl acetoacetate, monoisopropoxyaluminum bisoleyl acetoacetate, monoisopropoxyaluminum monooleate monoethyl acetoacetate, diisopropoxyaluminum monolauryl acetoacetate, diisopropoxyaluminum monostearyl acetoacetate, diisopropoxyaluminum monoisostearyl acetoacetate, etc. can be mentioned.
[0085] <Tackifier (C)> The tackifier (C) is not an essential component, but is used to further exert the good physical properties of the acrylic resin (A), and is preferably contained in the adhesive composition of the present invention. Examples of the tackifier (C) include resins that are compatible with the acrylic resin (A), such as rosin-based resins, terpene-based resins, xylene-based resins, phenol-based resins, coumarone-based resins, and petroleum-based resins. These tackifiers (C) can be used alone or in combination of two or more. Among them, rosin-based resins, terpene-based resins, and petroleum-based resins are preferred.
[0086] Examples of the rosin resin include a rosin ester resin obtained by hydrogenating, disproportionating, dimerizing, and adding an acid to a raw rosin, and then esterifying the resultant with glycerin or pentaerythritol, and a rosin phenol resin obtained by adding phenol. Any of the rosin resins can be used to further exhibit the good physical properties of the acrylic resin (A). Among them, preferred are a disproportionated rosin ester obtained by disproportionating the raw rosin and esterifying it with glycerin or pentaerythritol, which has a softening point in the range of 70 to 130°C, a polymerized rosin ester obtained by dimerizing the raw rosin and esterifying it with pentaerythritol, which has a softening point in the range of 110 to 170°C, and a rosin phenol obtained by adding phenol to the raw rosin, which has a softening point in the range of 120 to 160°C.
[0087] The above terpene resin has the molecular formula (C5H8) n The tackifier (C) used in the present invention is a resin obtained by homopolymerization or copolymerization of monoterpene (e.g., α-pinene, β-pinene, limonene, etc.) with a Friedel-Crafts catalyst. Specifically, examples of the resin obtained by homopolymerization or copolymerization of monoterpene include α-pinene resin, β-pinene resin, dipentene resin, terpene phenol resin, aromatic modified terpene resin, and hydrogenated terpene resin obtained by hydrogenating these resins. Among these, terpene phenol resins are preferred due to their good compatibility with the acrylic resin (A). Any of the terpene phenol resins will further enhance the good physical properties of the acrylic resin (A). In particular, those having a softening point of 90 to 170°C and a hydroxyl value in the range of 20 to 250 (mgKOH / g) are preferred, and those having a softening point of 100 to 150°C and a hydroxyl value in the range of 50 to 150 (mgKOH / g) are more preferred.
[0088] The petroleum resin is obtained, for example, by polymerization and further hydrogenation of C4-C5 and C9-C11 fraction monomers produced by thermal decomposition of naphtha, etc., and depending on the type of raw material fraction, examples include pure monomer resins, aliphatic (C5) petroleum resins, aromatic (C9) petroleum resins, hydrogenated petroleum resins, etc. Any of the petroleum resins can be used to further exhibit the good physical properties of the acrylic resin (A), but among them, those with a softening point in the range of 90 to 130°C are preferred, and it is further preferred to use a copolymerization system of a styrene monomer and an aliphatic monomer.
[0089] The content of the tackifier (C) is usually 1 to 50 parts by weight, particularly 5 to 30 parts by weight, and further preferably 5 to 20 parts by weight, per 100 parts by weight of the acrylic resin (A), and is appropriately blended depending on the required physical properties.
[0090] Furthermore, the pressure-sensitive adhesive composition of the present invention may contain, as other components, various additives such as resin components other than the acrylic resin (A), acrylic monomers, polymerization inhibitors, antioxidants, corrosion inhibitors, crosslinking accelerators, radical generators, peroxides, ultraviolet absorbers, plasticizers, pigments, stabilizers, fillers, and radical scavengers, metals, and resin particles, within the scope of the present invention. These may be used alone or in combination of two or more. In addition to the above, the pressure-sensitive adhesive composition may contain a small amount of impurities contained in the manufacturing raw materials of the components of the pressure-sensitive adhesive composition.
[0091] The content of the other components is preferably 5 parts by weight or less, more preferably 1 part by weight or less, and even more preferably 0.5 parts by weight or less, based on 100 parts by weight of the acrylic resin (A). If the content is too high, the compatibility with the acrylic resin (A) decreases, and the durability tends to decrease. However, for additives (pigments, fillers, metals, resin particles, etc.) that do not exert their effects at the above content, an appropriate amount may be added within a range that exerts the effect of the additive while not inhibiting the effect of the present invention.
[0092] The pressure-sensitive adhesive composition of the present invention contains, as described above, the acrylic resin (A) and the crosslinking agent (B), as well as a tackifier (C) as required, and further other components. The adhesive composition of the present invention can be obtained by mixing the above-mentioned components. The adhesive composition is crosslinked to obtain the adhesive of the present invention. The adhesive can be applied to various substrates to be used as an adhesive for adhesive tapes, and is particularly suitable for use as an adhesive layer for adhesive tapes for poorly adherent substrates.
[0093] The pressure-sensitive adhesive composition of the present invention preferably has a gel fraction of 30% by weight or more when crosslinked, in terms of increasing the holding power to poorly adherends, and particularly preferably 35% by weight or more. In order to achieve a gel fraction of 30% by weight or more, the type and content of the epoxy-based crosslinking agent (b1) and the isocyanate-based crosslinking agent (b2) may be adjusted, and the upper limit of the gel fraction is preferably 50% by weight or less, and particularly preferably 45% by weight or less. If the gel fraction is less than 30% by weight, the holding power to poorly adherends tends to decrease, and if it exceeds 50% by weight, the peel strength to poorly adherends tends to decrease.
[0094] <Adhesive tape> The pressure-sensitive adhesive tape of the present invention contains the pressure-sensitive adhesive obtained by crosslinking the pressure-sensitive adhesive composition as a pressure-sensitive adhesive layer. Specifically, the pressure-sensitive adhesive composition is dissolved in a solvent such as ethyl acetate to prepare a pressure-sensitive adhesive composition solution for coating so that the solid content concentration is 10 to 70% by weight, and the solution is applied to a substrate and dried to produce a pressure-sensitive adhesive tape.
[0095] Such an adhesive tape may be produced by a known method for producing an adhesive tape, for example, by coating one side of a substrate with an adhesive and drying it, and then overlaying a release liner on the surface of the formed adhesive layer, or by coating one side of a release liner with an adhesive and drying it, and then overlaying a substrate on the surface of the formed adhesive layer. Among these, the method of coating one side of a release liner with an adhesive and drying it, and then overlaying a substrate on the surface of the formed adhesive layer is preferred from the viewpoint of handling, etc.
[0096] The substrate is preferably hand-tearable, and the surface of the substrate having hand-tearability may be appropriately subjected to a known and commonly used surface treatment, for example, a physical treatment such as a corona discharge treatment or a plasma treatment, or a chemical treatment such as a primer treatment.
[0097] The substrate is not particularly limited as long as it is a conventionally known substrate, and examples thereof include rayon cloth, cotton cloth, polyester cloth, cloth made of blended yarn of rayon and polyester, nonwoven fabric, flat yarn cloth, laminated film in which a plastic film is laminated on a flat yarn cloth, etc. Among these, those containing flat yarn cloth are preferred because of their high tensile strength in the longitudinal direction.
[0098] Flat yarn cloth is a woven fabric made by cutting polyethylene or polypropylene film called flat yarn into strips and stretching it to give it strength, then weaving the flat yarns into a fabric. The intersections of the flat yarns that cross vertically and horizontally of this woven fabric are fixed by heat fusion to prevent misalignment.
[0099] Examples of the release liner include plastic films made of plastics such as polyolefin resins such as polyethylene, polyester resins such as polyethylene terephthalate, vinyl acetate resins, polyimide resins, fluorine resins, and cellophane; paper such as kraft paper and Japanese paper; rubber sheets made of natural rubber, butyl rubber, and the like; foam sheets obtained by foaming polyurethane, polychloroprene rubber, and the like; metal foils such as aluminum foil and copper foil; composites of these, etc. Furthermore, these may be subjected to a surface treatment such as a corona treatment on one or both sides.
[0100] Further, examples of the release liner include paper obtained by laminating a film such as polyethylene onto glassine paper, craft paper, or clay-coated paper; paper coated with a resin such as polyvinyl alcohol or an acrylic acid ester copolymer; and synthetic resin films such as polyester or polypropylene coated with a release agent such as a fluorine-based resin or a silicone-based resin.
[0101] Among these, paper release liners are preferred because they are easily torn by hand, and the basis weight of the base paper is 40 to 120 g / m 2 , preferably 50 to 80 g / m 2Particularly preferred is a paper release liner having a thickness of 40 to 180 μm, particularly 60 to 140 μm, and further preferably 80 to 120 μm. If the thickness is too thin, wrinkles may occur during winding, making production difficult, while if the thickness is too thick, hand tearability may decrease.
[0102] The coating device used when coating one side of the above-mentioned substrate or release liner with the adhesive may be any commonly used coating device, such as a roll knife coater, die coater, roll coater, bar coater, gravure roll coater, reverse roll coater, dipping, blade coater, etc.
[0103] The thickness of the pressure-sensitive adhesive layer after drying is preferably from 5 to 200 μm, particularly preferably from 10 to 150 μm, and further preferably from 15 to 130 μm. If the thickness is too thick, it tends to be difficult to apply the adhesive, whereas if the thickness is too thin, sufficient adhesive strength tends to be difficult to obtain.
[0104] The pressure-sensitive adhesive tape of the present invention may be a single-sided pressure-sensitive adhesive tape or a double-sided pressure-sensitive adhesive tape. The pressure-sensitive adhesive layers of the double-sided pressure-sensitive adhesive tape may be the same pressure-sensitive adhesive layer or may be pressure-sensitive adhesive layers having different compositions.
[0105] In addition, when a release liner is laminated on the adhesive layer of the double-sided adhesive tape, it is preferable to select the release liners laminated on both sides so that they have different peel strengths in order to improve workability. For example, the workability is improved by selecting a release liner with a lighter peel strength on the side of the double-sided adhesive tape that is first applied than the release liner on the side of the double-sided adhesive tape that is next applied.
[0106] The drying conditions may be any conditions under which the solvent and residual monomers in the adhesive are dried and removed during drying, and when a crosslinking agent (B) is used, the functional group of the acrylic resin (A) reacts with the crosslinking agent (B) to form a crosslinked structure. For example, drying conditions are preferably 60 to 120°C and about 1 to 5 minutes. After drying, the adhesive layer is sandwiched between sheet-like substrates and aged to further promote the crosslinking reaction.
[0107] The pressure-sensitive adhesive tape of the present invention may be in the form of a roll or in the form of sheets, or may be further processed into various shapes. When the adhesive tape is a double-sided adhesive tape in a sheet state, it is preferable that a release liner be provided on the surface of both of the two adhesive layers, and when it is in a roll state, it is preferable that a release liner be provided on the surface of only one of the two adhesive layers.
[0108] The adhesive tape of the present invention is thus obtained, and the adhesive tape of the present invention has good holding power without deterioration of adhesive properties even when applied to adherends or substrates that deteriorate the adhesive properties. Furthermore, when a substrate having hand-tearability is used as the substrate film, the tape can be easily cut by hand at any position in the width direction of the tape without using a tape cutter or the like, making the tape particularly useful as an adhesive tape.
[0109] The adhesive composition of the present invention, when processed into a tape, preferably has a peel strength against ethylene propylene diene rubber (EPDM) of 15 N / 25 mm or more, more preferably 16 N / 25 mm or more, and even more preferably 18 N / 25 mm or more. In addition, the holding power after being applied to ethylene propylene diene rubber and subjected to a moist heat treatment at 40°C and 90% RH for 14 days is preferably 50 minutes or more, more preferably 80 minutes or more, and even more preferably 120 minutes or more. In order to obtain a peel strength of 15 N / 25 mm or more and a holding power after moist heat treatment of 50 minutes or more, the composition of the acrylic resin (A) in the adhesive composition may be adjusted, or the type and content of the epoxy crosslinking agent (b1) and the isocyanate crosslinking agent (b2) may be adjusted.
[0110] The adhesive strength of the adhesive layer in the above-mentioned adhesive tape is preferably such that the 180° peel strength in accordance with JIS Z0237 against the adherend to be used is 1 to 100 N / 25 mm.
[0111] In particular, when test plates made of ethylene propylene diene rubber, chloroprene rubber (CR), natural rubber (NR), styrene butadiene rubber (SBR), or butyl rubber (IIR), which are difficult to adhere to, are used as the adherend, the 180° peel strength is preferably 15 N / 25 mm or more, particularly preferably 16 N / 25 mm or more, and further preferably 18 N / 25 mm or more. The upper limit is usually about 100 N / 25 mm. When a test plate made of SUS304 stainless steel, which has a relatively high polarity, is used as the adherend, the 180° peel strength is preferably 25 N / 25 mm or more, more preferably 30 N / 25 mm or more, and even more preferably 35 N / 25 mm or more. The upper limit is usually about 100 N / 25 mm.
[0112] The adhesive strength varies depending on the composition (material) and surface condition (surface roughness) of the adherend, treatment (cleaning) conditions, etc., and is not limited to the above peel strength range.
[0113] The adhesive strength is a value measured in accordance with JIS Z 0237. Specifically, it can be measured by the method described in the Examples below.
[0114] If the test piece is a double-sided adhesive tape, the adhesive side not being tested can be measured by covering it with a polyethylene terephthalate film (Lumirror S10, manufactured by Toray Industries, Inc.) having a nominal thickness of 25 μm as specified in JIS C2318.
[0115] Furthermore, when the holding power of the pressure-sensitive adhesive layer in the pressure-sensitive adhesive tape of the present invention is measured by the method described in the Examples below, it is particularly preferable that the test piece does not fall off the test plate after 24 hours have passed, and even if the test piece falls off within 24 hours, the holding time is preferably 100 minutes or more.
[0116] Furthermore, the holding power of the pressure-sensitive adhesive tape of the present invention against ethylene propylene diene rubber (EPDM) after wet heat treatment at 40° C. and 90% RH for 14 days is preferably 50 minutes or more, particularly preferably 80 minutes or more, and further preferably 120 minutes or more.
[0117] Furthermore, the gel fraction of the adhesive layer in the above adhesive tape is preferably 30 to 50% by weight, particularly preferably 35 to 42% by weight, from the viewpoints of adhesion and holding power. If the gel fraction is too low, the holding power to the adherend tends to decrease, and if it is too high, the adhesiveness to the adherend tends to decrease. The gel fraction is in the preferred range, and an adhesive composition using an epoxy-based crosslinking agent (b1) and an isocyanate-based crosslinking agent (b2) in combination is preferred in that it has a good balance between adhesive strength and holding power at a high level, and is easy to stably maintain a high holding power even when exposed to high temperature and high humidity.
[0118] The gel fraction is a measure of the degree of crosslinking (degree of hardening) and is calculated, for example, by the following method. That is, a 200-mesh SUS wire mesh large enough to encase the obtained adhesive tape is prepared and its weight is measured (1). The paper release liner is peeled off from the adhesive tape, wrapped in the aforementioned SUS wire mesh, and the weight of the tape together with the wire mesh is measured (2). After immersion in toluene kept at 23°C for 48 hours, it is thoroughly dried and the weight of the tape together with the wire mesh is measured (3). After immersion, the tape is removed from the wire mesh, the remaining adhesive layer is removed, and the weight of the base material is measured (4). Subtraction is performed as shown in the following formula, and the weight percentage of the adhesive component after immersion compared to before immersion is determined as the gel fraction. [Formula] Gel fraction (%) = (weight of tape after immersion including the weight of SUS wire mesh (3) - weight of substrate (4) - weight of SUS wire mesh (1)) / (weight of tape before immersion including the weight of SUS wire mesh (2) - weight of substrate (4) - weight of SUS wire mesh (1)) x 100
[0119] The gel fraction of the pressure-sensitive adhesive can be adjusted to fall within the above range by adjusting the type and amount of the crosslinking agent (B), for example.
[0120] In addition, the adhesive tape of the present invention is preferably one having a large tensile strength, and is required to have the strength necessary for pulling it without distortion when attaching it to a poorly adhesive adherend or peeling it off for position correction. The tensile strength of the adhesive tape is preferably 20N / 25mm or more, more preferably 30N / 25mm or more, and even more preferably 50N / 25mm or more. The upper limit of the tensile strength is usually 250N / 25mm. In order to obtain a double-sided adhesive tape with a large tensile strength, the tensile strength of the base film can be achieved by using a film having a tensile strength equal to or greater than that of the desired adhesive tape.
[0121] The adhesive tape of the present invention can be used in a wide range of applications, for example, as packaging tapes such as craft tape, OPP tape, and cloth adhesive tape, cellophane adhesive tape for light packaging, foam tape for automobiles, vibration-damping sheets, protective tapes for homes, soundproofing seals, double-sided tapes for fixing carpets, vinyl tapes for electrical insulation, outdoor anticorrosion tapes, tapes for indoor displays, slip-prevention tapes, airtight and waterproof adhesive tapes, adhesive substrates for medical first aid bandages and the like, surgical tapes, adhesive bandages, tapes for electrical and electronic devices, double-sided tapes for optics, dicing tapes for semiconductors, heat conductive tapes, heat resistant tapes, and conductive tapes.
[0122] The pressure-sensitive adhesive tape can be used, for example, in housing structures and their components, gaps between components, etc. The adherend is not particularly limited, but when used as a pressure-sensitive adhesive tape, it can be suitably used for sheet materials made of poorly adhesive adherends such as ethylene propylene diene rubber (EPDM), butyl rubber (IIR), chloroprene rubber (CR), natural rubber (NR), styrene butadiene rubber (SBR), polyvinyl chloride, chlorinated polyethylene, thermoplastic polyolefin rubber, and modified asphalt. EXAMPLES
[0123] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples as long as it does not depart from the gist of the invention. In the examples, "parts" and "%" are by weight.
[0124] First, various acrylic resins (A) were prepared as follows. The weight average molecular weight, dispersity and glass transition temperature of the acrylic resin (A) were measured according to the methods described above.
[0125] <Acrylic resin (A)> Prior to the production of the acrylic resin (A), the following were prepared as copolymerization components (a) to be used in the production. Component (a1) A monomer having a terminal carboxyl group represented by the following general formula (2): CH2=CR 1 -CO-O-(R 2 -COO-) n H (2) In the above general formula (2), R 1 is hydrogen, R 2 is an ethylene chain, n is 1 to 5 (a2) Component Acrylic Acid (a3) Component 2-Hydroxyethyl methacrylate (a4-1) Component n-Butyl acrylate (a4-2) Component 2-Ethylhexyl acrylate (a5) Component Methyl acrylate
[0126] For the above component (a1), "Sipomer H" manufactured by Solvay Nicca was used. Sipomer H is a compound represented by the general formula (1): 1 is hydrogen, R 2 is an ethylene chain, n = 1 compound (a1-1) is 56%, R 1 is hydrogen, R 2 The mixture contains 16.1% of the compound (a1-2) having an ethylene chain and n=2 to 5, and 27.9% of acrylic acid (a2) (hereinafter, R 1 is hydrogen, R 2 is an ethylene chain, and compounds with n = 1 to 5 are sometimes referred to as "CAO").
[0127] [Production of acrylic resin (A)] In a reactor equipped with a thermometer, a stirrer and a reflux condenser, 5 parts of Sipomer H [3.6 parts of CAO (a1), 1.4 parts of acrylic acid (a2)], 0.1 parts of 2-hydroxyethyl methacrylate (a3), 25.8 parts of n-butyl acrylate (a4-1), 63.1 parts of 2-ethylhexyl acrylate (a4-2), 6 parts of methyl acrylate (a5), 55 parts of ethyl acetate as a solvent, and 0.15 parts of azobisisobutyronitrile as a polymerization initiator were charged as copolymerization components, and the temperature was raised with stirring. After polymerization for 7 hours at the reflux temperature of the ethyl acetate (mixture), the reaction mixture was diluted with ethyl acetate to obtain an acrylic resin (A) solution with a solid content of 50%. The weight average molecular weight of the resulting acrylic resin (A) was 620,000, the dispersity was 5.8, and the glass transition temperature was -59°C.
[0128] <Crosslinking agent (B)> The following was prepared as the crosslinking agent (B). Epoxy crosslinking agent (b1): Tetrad C (1,3-bis(N,N'-diglycidylaminomethyl)cyclohexane), manufactured by Mitsubishi Gas Chemical Company, Inc. Isocyanate-based crosslinking agent (b2): Tosoh Corporation, Coronate L-55E (solid content 55%)
[0129] <Tackifier (C)> The following tackifiers (C) were prepared: Disproportionated rosin ester: Arakawa Chemical Industries, Super Ester A-100 (glycerin ester of disproportionated rosin, softening point 95-105°C)
[0130] <Example 1> For 100 parts of the solid content (resin content) of the acrylic resin (A) solution prepared as described above, 0.015 parts of epoxy-based crosslinking agent (b1) (Tetrad C) converted to solid content (resin content), 0.25 parts of isocyanate-based crosslinking agent (b2) (Coronate L-55E) converted to solid content (resin content), and 15 parts of tackifier (C) were mixed, and the solution was adjusted to a solid content concentration of 40% with ethyl acetate and stirred until uniform, thereby obtaining a solution of an adhesive composition.
[0131] <Examples 2 and 3 and Comparative Examples 1 to 4> The same procedure as in Example 1 above was carried out except that the components of the adhesive composition were changed as shown in Table 1 below, to obtain solutions of the adhesive compositions of Examples 2 and 3 and Comparative Examples 1 to 4.
[0132] For the obtained pressure-sensitive adhesive compositions of Examples 1 to 3 and Comparative Examples 1 to 4, pressure-sensitive adhesive tapes were produced as described below and the following evaluations were carried out. The evaluation results are shown in Table 1 below.
[0133] [Preparation of adhesive tape] The adhesive composition solution prepared as described above was applied to the release surface of a paper release liner [SS-70-SBX (Shinomura Chemical Industry)] using an applicator so that the thickness after drying would be 110 μm, and then it was dried at 80° C. for 5 minutes, and flat yarn (Diatex, thickness 130 μm) was attached. Then, it was subjected to heat aging treatment in a dryer at 40° C. for 7 days to prepare an adhesive tape.
[0134] <Gel fraction> A 200-mesh SUS wire mesh large enough to encase the resulting adhesive tape is prepared and its weight is measured (1). The paper release liner is peeled off from the adhesive tape and wrapped in the aforementioned SUS wire mesh, and the weight of the tape together with the wire mesh is measured (2). After immersion in toluene maintained at 23°C for 48 hours, it is thoroughly dried and the weight of the tape together with the wire mesh is measured (3). After immersion, the tape is removed from the wire mesh, the remaining adhesive layer is removed, and the weight of the base material is measured (4). Subtraction is performed as shown in the following formula, and the weight percentage of the adhesive component after immersion compared to before immersion is determined as the gel fraction. [Formula] Gel fraction (%) = (weight of tape after immersion including the weight of SUS wire mesh (3) - weight of substrate (4) - weight of SUS wire mesh (1)) / (weight of tape before immersion including the weight of SUS wire mesh (2) - weight of substrate (4) - weight of SUS wire mesh (1)) x 100
[0135] <180° peel strength> The above adhesive tape was cut to a width of 25 mm and a length of 150 mm to prepare a test specimen. In addition, a test plate of ethylene propylene diene rubber (EPDM) (manufactured by Engineering Test Services, standard test version EPDM-70) was used as an adherend after cleaning the surface with methanol and leaving it to stand overnight in an atmosphere of 23 ° C. and 50% RH. The paper release liner was peeled off from the above test specimen, and the adhesive layer of the test specimen was pressed onto the above test plate by moving a roller weighing 2 kg back and forth once at a pressing speed of 5 mm / s. After pressing, it was left to stand for 30 minutes in an atmosphere of 23 ° C. and 50% RH, the play part of the test specimen was folded back by 180 ° and peeled off by 30 mm, and then the test plate was fixed to the lower chuck of the peel strength tester and the end of the test specimen was fixed to the upper chuck in the same atmosphere, and the adhesive tape was peeled off from the adherend at a peel angle of 180 ° and a speed of 300 mm / min, and the adhesive force was measured.
[0136] <Holding force> The above adhesive tape was cut to a width of 25 mm and a length of 75 mm to prepare a test piece. In addition, an EPDM test plate was used as an adherend after the surface was washed with methanol and left to stand overnight in an atmosphere of 23°C, 50% RH. The above test piece was pressed against the test plate by a roller weighing 2 kg and moving it back and forth at a pressing speed of 5 mm / s so that the contact area between the adhesive layer of the test piece, from which the paper release liner had been peeled off, and the test plate was 25 mm wide x 25 mm long. In addition, the part of the test piece where the adhesive was exposed was folded back. After pressing, the test piece was left to stand for 30 minutes in an environment of 23°C, 50% RH, and then moved to an environment of 40°C and left to stand for 20 minutes. A 1000g weight was attached to the test plate so that the test piece was hanging vertically, and the time it took for the test piece to fall was measured in an environment of 40°C.
[0137] <Retention after wet heat treatment> The test pieces prepared in the same manner as above were left to stand in a thermohygrostat adjusted to 40° C. and 90% RH for 7 and 14 days to carry out a moist heat treatment, and then the holding power was measured in the same manner as above.
[0138] [Table 1]
[0139] From the results in Table 1 above, all of the examples of the present invention using the epoxy-based crosslinking agent (b1) and the isocyanate-based crosslinking agent (b2) in combination had high peel strength and adhered firmly to the adherend, even to a difficult-to-adhere adherend such as EPDM. In addition, the adhesive had high holding power against EPDM and excellent creep resistance under a certain stress. In addition, the adhesive maintained high holding power after a wet heat treatment at 40°C and 90% RH.
[0140] In contrast, Comparative Example 1, which used only the isocyanate-based crosslinking agent (b2), had low retention to EPDM and was not suitable for use. In Comparative Example 2, which used only the isocyanate-based crosslinking agent (b2) and added a slightly larger amount than Comparative Example 1, the peel strength to EPDM was low and the adhesiveness was poor. When only the isocyanate-based crosslinking agent (b2) was used, both the adhesiveness and retention to EPDM could not be stably satisfied. Moreover, Comparative Example 3, in which only the epoxy-based crosslinking agent (b1) was used, had excellent adhesion and holding power to EPDM, but the holding power after moist heat treatment was significantly reduced, and the moist heat resistance was poor. In Comparative Example 4, in which the content of the epoxy-based crosslinking agent (b1) was slightly increased from that in Comparative Example 3 in order to improve the holding power after the moist heat treatment of Comparative Example 3, an improvement in the holding power after the moist heat treatment was observed, but the peel strength was low and the adhesion was poor.
[0141] In other words, it is found that for poorly adhesive substrates such as EPDM, and in particular CR, NR, SBR and IIR, a pressure-sensitive adhesive tape using a pressure-sensitive adhesive composition containing an acrylic resin (A) obtained by copolymerizing a copolymerization component (a) containing a specific terminal carboxyl group-containing monomer (a1), a (meth)acrylic acid monomer (a2) and a hydroxyl group-containing monomer (a3), an epoxy-based crosslinking agent (b1) and an isocyanate-based crosslinking agent (b2) combines superior adhesion and high holding power, and stably maintains high holding power even when exposed to high temperatures and high humidity.
[0142] In the above embodiment, specific embodiments of the present invention are shown, but the above embodiment is merely illustrative and should not be interpreted as being limiting. Various modifications that are obvious to those skilled in the art are intended to be within the scope of the present invention. [Industrial Applicability]
[0143] The adhesive composition of the present invention has excellent adhesion to poorly adhesive rubber-based adherends, particularly poorly adhesive adherends such as ethylene propylene diene rubber (EPDM). Therefore, it can be used in a wide range of applications, such as packaging tapes such as craft tapes, OPP tapes, and cloth adhesive tapes, cellophane adhesive tapes for light packaging, foam tapes for automobiles, vibration-damping sheets, protective tapes for housing, soundproofing seals, double-sided tapes for fixing carpets, vinyl tapes for electrical insulation, outdoor anticorrosive tapes, tapes for indoor displays, slip prevention tapes, adhesive tapes for airtight waterproofing, adhesive substrates for medical first aid bandages, surgical tapes, adhesive bandages, tapes for electrical and electronic devices, double-sided tapes for optics, dicing tapes for semiconductors, thermally conductive tapes, heat-resistant tapes, conductive tapes, etc. It is particularly suitable for tapes used outdoors that require resistance to moisture and heat.
Claims
1. The present invention relates to an acrylic resin (A) that includes a terminal carboxyl group-containing monomer (a1) unit represented by the following general formula (1), a (meth)acrylic acid monomer (a2) unit, a hydroxyl group-containing monomer (a3) unit, and a (meth)acrylate monomer (a4) unit having an alkyl group having 4 to 24 carbon atoms; an epoxy-based crosslinking agent (b1); and an isocyanate-based crosslinking agent (b2); the content of the terminal carboxyl group-containing monomer (a1) unit is 1 to 20% by weight and the content of the (meth)acrylic acid monomer (a2) unit is 0.1 to 5% by weight relative to the entire acrylic resin (A); a content ratio of the (meth)acrylate monomer (a4) unit having an alkyl group having 4 to 24 carbon atoms of 0.01 to 5 wt %, a content ratio of the (meth)acrylate monomer (a4) unit having an alkyl group having 4 to 24 carbon atoms of 55 to 97 wt %, a content of the epoxy-based crosslinking agent (b1) of 0.005 to 0.028 parts by weight relative to 100 parts by weight of the acrylic resin (A), a content of the isocyanate-based crosslinking agent (b2) of 0.1 to 0.5 parts by weight relative to 100 parts by weight of the acrylic resin (A), and a content of the epoxy-based crosslinking agent (b1) of 2.5 to 25 parts by weight relative to 100 parts by weight of the isocyanate-based crosslinking agent (b2). 【Chemistry 1】
2. The pressure-sensitive adhesive composition according to claim 1, wherein the pressure-sensitive adhesive composition has a gel fraction of 30% by weight or more when crosslinked.
3. 3. The pressure-sensitive adhesive composition according to claim 1 or 2, in an adhesive tape having an adhesive formed on a substrate by crosslinking the pressure-sensitive adhesive composition, the 180° peel strength against ethylene propylene diene rubber in accordance with JIS Z0237 is 15 N / 25 mm or more, and the holding power measured by the following measurement method is 50 minutes or more. <Method of measuring holding power> The adhesive tape was cut to a width of 25 mm and a length of 150 mm, and the adhesive layer of the above-mentioned adhesive tape was pressed against the ethylene propylene diene rubber so that the contact area between the adhesive layer and the ethylene propylene diene rubber was 25 mm wide x 25 mm long. After a moist heat treatment at 40°C and 90% RH for 14 days, a 1000 g weight was attached to the ethylene propylene diene rubber so that the adhesive tape hung vertically, and the time it took for the adhesive tape to fall in a 40°C environment was then measured.
4. The pressure-sensitive adhesive composition according to any one of claims 1 to 3, characterized in that the content of the (meth)acrylic acid monomer (a2) unit is 10 to 400 parts by weight based on 100 parts by weight of the terminal carboxyl group-containing monomer (a1) unit represented by the general formula (1).
5. The pressure-sensitive adhesive composition according to any one of claims 1 to 4, further comprising a tackifier (C).
6. The pressure-sensitive adhesive composition according to any one of claims 1 to 5, which is for use on poorly adhesive adherends.
7. A pressure-sensitive adhesive obtained by crosslinking the pressure-sensitive adhesive composition according to any one of claims 1 to 6.
8. The pressure-sensitive adhesive according to claim 7, which has a gel fraction of 30% by weight or more.
9. The pressure-sensitive adhesive according to claim 7, which has a gel fraction of 50% by weight or less.
10. An adhesive tape comprising a substrate and an adhesive formed on the substrate, the adhesive being the adhesive according to any one of claims 7 to 9.
11. The pressure-sensitive adhesive tape according to claim 10, which has a 180° peel strength against ethylene propylene diene rubber in accordance with JIS Z0237 of at least 15 N / 25 mm and a holding power measured by the following method for at least 50 minutes. <Method of measuring holding power> The adhesive tape was cut to a width of 25 mm and a length of 150 mm, and the adhesive layer of the above-mentioned adhesive tape was pressed against the ethylene propylene diene rubber so that the contact area between the adhesive layer and the ethylene propylene diene rubber was 25 mm wide x 25 mm long. After a moist heat treatment at 40°C and 90% RH for 14 days, a 1000 g weight was attached to the ethylene propylene diene rubber so that the adhesive tape hung vertically, and the time it took for the adhesive tape to fall in a 40°C environment was then measured.
Citation Information
Patent Citations
Pressure-sensitive adhesive composition
JP1990196879A
Pressure-sensitive adhesive composition for polarizing film
JP2006282687A
Pressure-sensitive adhesive composition
JP2008127431A
Adhesive agent composition and adhesive sheet
JP2011116916A
Easy adhesive for solar cell surface protective sheet, solar cell surface protective sheet, and solar cell module