Method for identifying types of defects in silicon single crystal wafers
By using a particle counter to analyze defect changes before and after nitride film formation, the method addresses the challenge of identifying defect composition and shape in silicon single crystal wafers, providing efficient and cost-effective defect type identification.
Patent Information
- Application Number
- JP2021170918
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-10-19
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2041-10-19
AI Technical Summary
Existing methods for detecting defects in silicon single crystal wafers, such as using a nitride film lens effect to enlarge particle size, fail to identify the composition and shape of undetectable defects, making it difficult to determine their cause, and time-consuming cross-sectional TEM is inefficient for large-scale defect analysis.
A method involving a particle counter to detect defects before and after forming a nitride film on the wafer, analyzing changes in defect number and size to identify defect types based on specific patterns, eliminating the need for cross-sectional TEM.
Enables efficient and cost-effective identification of defect types on silicon single crystal wafers by analyzing defect changes before and after nitride film formation, simplifying the process and reducing reliance on time-consuming methods.
Smart Images

Figure 0007567747000001 
Figure 0007567747000002 
Figure 0007567747000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for identifying a type of defect in a silicon single crystal wafer. [Background technology]
[0002] The integration of silicon devices has progressed, and 5-nm node ICs are being manufactured. However, the minimum detection sensitivity for particles that can cause defects in these ICs is 12 nm. If particles that are several times the size of the line width are present on the wafer, the IC will naturally be defective, so it is desirable to establish a method for measuring smaller particles.
[0003] As a method for measuring minute particles, Patent Document 1 reports a method for increasing sensitivity by utilizing the lens effect of a nitride film formed by plasma CVD. In this method, a nitride film is formed by plasma CVD on a wafer containing tiny particles of an undetectable size. The nitride film is formed in such a way that it envelops the particles, making the apparent particle size larger after film formation, making them detectable by a particle counter.
[0004] In addition, there are cases where particles that were not found by the particle counter at the time of wafer shipment are detected by the particle counter inspection due to oxidation in the device process or after the nitride film is formed by CVD. This is presumably because particles that were below the lower limit of detection of the particle counter at the time of wafer shipment have become larger due to oxidation or the formation of the nitride film and are then detected. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2016-212009 A Summary of the Invention [Problem to be solved by the invention]
[0006] In the detection of defects by enlarging particle size using the lens effect of the nitride film, the original particles are too large to be detected, so their composition and shape are unknown, making it difficult to identify the cause of their occurrence. If the defect is of a size that can be detected by a particle counter, it is possible to measure its composition and shape using a SEM (Scanning Electron Microscope). On the other hand, if the composition and shape of defects of a size that cannot be detected by a particle counter can be found using an SEM, it is possible, but in reality they cannot be found. After the nitride film is formed, the position and density of the defects can be measured, but since they are buried in the nitride film, their composition and shape cannot be known unless the defect shape under the nitride film is confirmed using a cross-sectional TEM (Transmission Electron Microscope). This cross-sectional TEM is a time-consuming measurement, so it is difficult to measure many defects.
[0007] In order to identify the cause of the microparticles that cause the protrusions detected after nitride film formation, a simple method is needed to determine what material the microparticles are made of (what type of defect they are).
[0008] The present invention has been made to solve the above problems, and an object of the present invention is to provide a method for easily identifying the type of defect on the surface of a silicon single crystal wafer. [Means for solving the problem]
[0009] In order to achieve the above object, the present invention provides a method for identifying a type of defect in a silicon single crystal wafer, comprising: Detecting defects present on the surface of the silicon single crystal wafer with a particle counter to measure the number and size of the defects; forming a nitride film on the surface of the silicon single crystal wafer after the measurement; detecting defects present on the surface of the silicon single crystal wafer after the nitride film is formed using the particle counter and measuring the number and size of the defects; evaluating a change in the number of defects and a change in the size of the defects before and after forming the nitride film; The present invention provides a method for identifying the type of defect in a silicon single crystal wafer, characterized in that the type of the defect is identified based on the results of the evaluation.
[0010] In this way, by determining the change in the number and size of defects detected by the particle counter before and after the nitride film formation, it is possible to determine the cause of the defects (particles, etc.) buried under the formed nitride film. Normally, to identify this cause (identify the type of defect), it is necessary to evaluate the particles, etc. under the nitride film using a time-consuming cross-sectional TEM or the like, but with the present invention, it can be easily identified from the measurement results of the particle counter.
[0011] At this time, the thickness of the nitride film formed can be set to 30 to 120 nm.
[0012] By forming a nitride film with a thickness of 30 nm, it is possible to more reliably detect minute particles that cannot be detected before the nitride film formation by increasing their apparent size through the lens effect described above. Also, a thickness of 120 nm is sufficient, and it is efficient in that it does not require more time or cost than necessary.
[0013] Also, when evaluating the change in the defect size, The position coordinates of the defects are obtained before and after the formation of the nitride film, and defects at the same position coordinates can be evaluated.
[0014] In this way, when evaluating the change in defect size, it is preferable to evaluate defects at the same position coordinates based on the defect coordinates on the wafer surface.
[0015] Examples of patterns for identifying the type of defect from the evaluation results include the following: First, in the case where the result of the evaluation shows that the number of defects is reduced after the formation of the nitride film and the defect size of the remaining defects is reduced, The defect may be identified as a COP. In addition, if the result of the evaluation shows that the number of defects has not changed and the size of the defects has not changed after the nitride film is formed, The defect may be identified as a PID. In addition, in the result of the evaluation, if the defect detected before the formation of the nitride film remains after the formation of the nitride film and the defect size becomes large, and a new defect is detected after the formation of the nitride film, The defects may be identified as thermally stable particles. Furthermore, in the case where the result of the evaluation shows that some of the defects detected before the formation of the nitride film have disappeared after the formation of the nitride film, and the defect sizes of the defects remaining after the formation of the nitride film have increased, The defects may be identified as thermally unstable particles.
[0016] The inventors have found that there are trends in the change in the number of defects and the change in the size of the defects depending on the type of defect. For example, in the change pattern as described above, it is possible to identify the defects as COP, PID, thermally stable particles, and thermally unstable particles, respectively.
[0017] Currently, wafer manufacturing processes are highly controlled, and defects caused by the process are rarely detected. In other words, it is difficult to imagine that many types of particles that cause defects occur simultaneously, and it is unlikely that multiple combinations of the above-mentioned changes in the number of defects and changes in defect size will occur. Therefore, it is possible to sufficiently identify what types of defects exist on the surface of the silicon single crystal wafer being evaluated from the above-mentioned change patterns.
[0018] In this case, the thermally stable particles can be SiO2 or Al2O3. The thermally unstable particles may be organic.
[0019] Thus, SiO2, Al2O3, or organic substances are examples of thermally stable or unstable particles. Effect of the Invention
[0020] The method of the present invention for identifying the type of defect in a silicon single crystal wafer is useful because it makes it possible to easily identify the type of defect without relying on time-consuming methods such as cross-sectional TEM. [Brief description of the drawings]
[0021] [Figure 1] 1 is a flowchart showing an example of a method for identifying a type of defect in a silicon single crystal wafer according to the present invention. [Diagram 2] LPD map (COP). [Diagram 3] 1 is a defect size change graph (COP). [Figure 4] This is the defect histogram (COP). [Diagram 5] LPD map (PID). [Figure 6] 1 is a defect size change graph (PID). [Figure 7] This is a defect histogram (PID). [Figure 8] 1A and 1B are schematic diagrams showing the change in defect size before and after the formation of a nitride film in the cases of particles and PIDs. [Figure 9] This is an LPD map (thermally stable particles: SiO2). [Figure 10] This is a defect size change graph (thermally stable particle: SiO2). [Figure 11] This is a defect histogram (thermally stable particles: SiO2). [Figure 12]These are SEM measurement images (thermally stable particles: SiO2) of common defects and increased defects. [Figure 13] This is a cross-sectional TEM measurement image of an increased defect (thermally stable particle: SiO2). [Figure 14] This is an LPD map (Thermally Unstable Particles: Organics). [Figure 15] Graph showing change in defect size (thermally unstable particles: organic matter). [Figure 16] Defect histogram (thermally unstable particles: organic matter). [Figure 17] 1 is an LPD map (Example 1). [Figure 18] 1 is a defect size change graph (Example 1). [Figure 19] 1 is a defect histogram (Example 1). [Figure 20] 1 is an LPD map (Example 2). [Figure 21] 1 is a defect size change graph (Example 2). [Figure 22] 1 is a defect histogram (Example 2). [Diagram 23] 1 is an LPD map (Example 3). [Figure 24] 1 is a defect size change graph (Example 3). [Diagram 25] 11 is a defect histogram (Example 3). [Figure 26] 1 is an LPD map (Example 4). [Figure 27] 1 is a defect size change graph (Example 4). [Figure 28] 1 is a defect histogram (Example 4). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0022] Hereinafter, the present invention will be described in detail with reference to the drawings as an example of an embodiment, but the present invention is not limited thereto. FIG. 1 is a flow chart showing an example of a method for identifying the type of a defect in a silicon single crystal wafer according to the present invention. <Step 1: Measurement of the number and size of defects (measurement before nitride film formation)> First, a silicon single crystal wafer (hereinafter simply referred to as a wafer) to be evaluated for the purpose of identifying the type of defects (also referred to as the defect type) present on the surface is prepared, and surface defects are detected using a particle counter, and the number and size of the defects are measured. In this case, the particle counter used is not particularly limited as long as it can detect defects and measure the number and size of defects. For example, a conventional commercially available particle counter such as SP7 manufactured by KLA-Tencor can be used. Using such a particle counter, an LPD (Light Point Defect) map, i.e., the distribution of defects within the wafer surface, is obtained. As described later, the LPD detected by the particle counter includes, for example, particles (thermally stable particles and thermally unstable particles), COPs, PIDs, and the like.
[0023] By acquiring such an LPD map, it is possible to measure the number of defects (and their position coordinates (simply referred to as coordinates)) that exist on the wafer surface. At the same time, by adjusting the detection sensitivity and setting the level of the defect size to be detected, it is possible to measure the number of defects of a given size that exist on the surface, along with their respective position coordinates. The detection sensitivity can be adjusted on an ad-hoc basis according to the desired defect size. For example, it can be set to 12 nm, which is the maximum sensitivity of SP7. The defect size can be measured from the size of the LPD.
[0024] In addition, as described below, by performing measurements after forming the nitride film and comparing based on the coordinates of each defect on the wafer surface at each measurement, various data regarding the number of defects can be obtained, along with information on the size of each defect, such as the number of defects detected in the measurement before forming the nitride film, the number of defects detected in the measurement after forming the nitride film at the same position as in the measurement before forming the nitride film, the number of defects detected in the measurement before forming the nitride film but not at the same position in the measurement after forming the nitride film, and the number of defects newly detected in the measurement after forming the nitride film.
[0025] <Step 2: Nitride film formation> After the measurement in step 1, a nitride film is formed on the surface of the wafer. The method of forming the nitride film is not particularly limited, and it can be formed by a conventionally known method. For example, a film forming apparatus is used to form a nitride film with a thickness of 30 to 120 nm under nitriding conditions of a SiH2Cl2+NH3 atmosphere, a temperature of 700-850°C, and a time of 10 minutes or more. Although the thickness to be formed is not limited, if a nitride film with a thickness in the above range is formed, minute particles that are present on the wafer surface but could not be detected in the measurement in step 1 can be efficiently enlarged by the lens effect of the nitride film formation, and can be more reliably detected in the measurement in the next step 3.
[0026] <Step 3: Measurement of the number and size of defects (measurement after nitride film formation)> After the nitride film is formed in step 2, defects on the wafer surface are detected again using a particle counter (SP7), and the number and size of the defects are measured (obtaining an LPD map). The conditions for measuring defects on a nitride film can be, for example, a minimum size of 20 nm that can be detected when the nitride film is formed. If the haze of the nitride film is high and the minimum measurement size of 20 nm cannot be measured, the film formation conditions can be reviewed as appropriate.
[0027] <Step 4: Evaluation of changes in the number of defects and the size of defects before and after nitride film formation> The changes in the number of defects and the size of the defects before and after the nitride film formation are evaluated. For example, the LPD maps acquired in steps 1 and 3 before and after the nitride film formation are compared, and the change in the number of defects and the size change of defects at the same coordinates before and after the nitride film formation are obtained based on the change in the number of defects and their coordinates within the surface. The change in the number of defects and the change in the size of the defects do not necessarily have to show the same change trend for all of the defects, and it is sufficient to grasp the general change pattern, such as being able to confirm a specific change trend when viewed as a whole.
[0028] As for the change in defect size, it is preferable to obtain the position coordinates of the defect before and after the nitride film formation as described above, and evaluate how the defect at the same coordinates has changed, but this is not limiting. For example, it is also possible to use the average value of all the detected defects. This will be sufficient as long as a unique change pattern is created for a certain type of defect.
[0029] The same can be said about evaluating the change in the number of defects. For example, it is possible to focus on the change in the total number of defects detected, or on the number of defects (a change from zero to a certain number) newly detected after the formation of the nitride film in positions that were not detected before the formation of the nitride film.
[0030] <Step 5: Identifying the type of defect> From the evaluation results in step 4, the type of defect present on the surface of the wafer being evaluated is identified. If the change pattern understood in step 4 matches a change pattern specific to a certain type of defect, the defect in the wafer to be evaluated is identified as that type of defect. Note that it is preferable to understand the change pattern according to the defect type in advance by a preliminary experiment or the like, since this allows the defect type to be identified smoothly and reliably in step 5.
[0031] As described above, the method for identifying the type of defect according to the present invention makes it possible to identify the type of defect even after the formation of the nitride film without using a conventional time-consuming method such as a cross-sectional TEM. Moreover, it is very simple because it can be identified from the change pattern by comparing before and after the formation of the nitride film using a particle counter.
[0032] Below, examples of the relationship between representative defect types (COP, PID, thermally stable particles, thermally unstable particles) and change patterns for those defect types are shown together with various measurement diagrams, but the present invention is not limited to these. If a change pattern specific to a certain defect type can be confirmed, the relationship between them can be applied to the present invention. As for the various measurement diagrams mentioned above, Figures 2, 5, 9, and 14 show (1) LPD maps (defect maps) before and after the formation of the nitride film, Figures 3, 6, 10, and 15 show (2) graphs of defect size changes for defects at the same coordinates before and after the formation of the nitride film, and Figures 4, 7, 11, and 16 show (3) total LPD size histograms before the formation of the nitride film and size histograms (defect histograms) before the formation of the nitride film for LPDs that were commonly present before and after the formation of the nitride film.
[0033] In the LPD map display in (1), before SP7 is the defect map before the nitride film was formed, after SP7 is the defect map after the nitride film was formed, and match is a defect whose coordinate shift was within 10 μm before and after the nitride film was formed. In other words, before SP7 without the match mark is a defect that disappeared due to the nitride film formation, after SP7 is a defect that was newly detected after the nitride film was formed, and match is a defect that was present before the nitride film was formed and was also found after it. This is a map for a 300 mm diameter wafer, and the numerical units on the vertical and horizontal axes are μm. The defect size change graph (2) relates to LPD size (μm), with the horizontal axis representing the size before nitridation and the vertical axis representing the size after nitridation. The histogram in (3) shows a histogram of all defects detected before the nitride film was formed, and a size histogram of the defects remaining after the nitride film was formed (when defects exist in the same position before and after the nitride film was formed), which essentially shows the number of matches. The horizontal axis shows the LPD size (μm), and the vertical axis shows the number of LPD counts.
[0034] <Conditions for steps 1-3> The particle counter used was SP7. Detection sensitivity before nitride film formation: 12 nm Detection sensitivity after nitride film formation: 25 nm The nitride film was formed in a film forming apparatus in an SiH2Cl2+NH3 atmosphere at a temperature of 700°C for 10 minutes to a thickness of 50 nm.
[0035] [COP] For a silicon single crystal wafer sample containing COPs, Fig. 2 shows an LPD map, Fig. 3 shows a defect size change graph, and Fig. 4 shows a defect histogram. Looking at the map in Figure 2, we can see that the defects in the central region before the nitride film formation disappear in large numbers with the formation of the nitride film. This reduction in the number of defects due to their large-scale disappearance can also be seen in Figure 4. This sample has a COP in its center, and it is generally known that dents are filled by CVD, and COPs, which are a typical crystal defect, disappear with the formation of the nitride film. Or, even if they remain, they become smaller. As shown in Figure 3, for the remaining defects, there are some where the defect size remains almost unchanged before and after the nitride film formation, but in the case of COPs, there is also a tendency for the defect size to decrease.
[0036] [PID] For a silicon single crystal wafer sample in which PIDs exist, an LPD map is shown in FIG. 5, a defect size change graph is shown in FIG. 6, and a defect histogram is shown in FIG. 7. As can be seen from the maps in Figure 5 and Figure 7, most of the defects that existed before the nitride film formation still exist after nitridation, meaning that the number of defects has hardly changed. The defects that occurred after nitriding were clustered at the 12 o'clock and 3 o'clock points on the map, and it was found from the map that they were pseudo defects caused by the deterioration of haze. Furthermore, as shown in Figure 6, there was almost no change in size before and after the nitride film was formed, and the defect was not one for which the so-called lens effect could be expected. As shown in the schematic diagram in Figure 8, it is unlikely that PIDs, like particles, would become larger in defect size due to the formation of a nitride film. Therefore, it is a reasonable result that the defect was detected at the same size before and after the nitride film was formed.
[0037] [Thermal stable particles] For a silicon single crystal wafer sample containing thermally stable particles, Fig. 9 shows an LPD map, Fig. 10 shows a defect size change graph, and Fig. 11 shows a defect histogram. Looking at the map in Figure 9, we can see that almost all of the defects that were present before the nitride film was formed are still in the same place after the nitride film was formed, and have not been reduced. As shown in Figure 10, almost all of the sizes had increased. Furthermore, a large number of defects were found to be newly detected after the nitride film was formed, as shown in Figure 9. When these newly detected defects (increased defects) were observed with an SEM, they had the same protrusion shape as defects that have become larger due to the lens effect (common defects), as shown in Figure 12. Furthermore, as shown in Figure 13, a cross-sectional TEM confirmed particles with a size of 135 nm under the protrusions after the nitride film was formed. As shown in Figure 11, these thermally stable particles are defects that were originally detected but did not disappear but instead grew larger, and based on the SEM / TEM results, it is believed that the defects newly detected after the nitride film was formed were small particles that had not been confirmed in the initial SP7 measurements but became apparent and were detected by the nitride film formation.
[0038] This sample was one in which the abrasive had not been sufficiently removed, leaving tiny particles of abrasive (SiO2) remaining on the wafer surface. It was found that thermally stable particles such as SiO2 particles increase in size due to the formation of the nitride film, and that the number of defects on the entire wafer increases due to the detection of previously undetected small particles.
[0039] As mentioned above, the defect histogram in Figure 11 shows the number of residual defects (black column graph) after nitride film formation by defect size (match number) against the initial number of defects (white column graph) before nitride film formation, and from this, it can be seen that the number of residual defects is generally not larger than the initial number of defects. The reason why the number of residual defects in Figure 11 is larger than the initial number of defects is because [1] it is judged based on whether the coordinates are the same before and after nitride film formation, [2] the defect density of this sample is high, and [3] if there are two defects after nitride film formation near the coordinates of a defect before nitride film formation, the defect before nitride film formation is counted as one and the defect at the same coordinate after nitride film formation is counted as two defects. This does not mean that the initial defects before nitride film formation increase after nitride film formation.
[0040] In addition to SiO2, this type of defect also includes Al2O3.
[0041] [Thermal unstable particles] For a silicon single crystal wafer sample containing thermally unstable particles, FIG. 14 shows an LPD map, FIG. 15 shows a defect size change graph, and FIG. 16 shows a defect histogram. In the map in Figure 14, the defects detected after the nitride film formation are false defects caused by the worsening of haze, and no new defects have actually occurred. On the other hand, it can be seen that some of the defects that were present in the before SP7 in Figure 14 have disappeared due to the nitride film formation. The disappearance of some of them can also be seen in Figure 16. Furthermore, as shown in FIG. 15, when comparing the defects before and after the nitride film formation, the defects that did not disappear (remained) after the nitride film formation became larger in size. In other words, some of the defects that did not disappear have become larger, but not all of the defects have become larger, and some have become smaller and disappeared. This sample is thought to be organic particles remaining on the wafer, with small or unstable organic matter disappearing during the high temperature process of CVD, and a nitride film forming on the remaining organic particles, causing them to become larger in size.
[0042] In addition, for example, if almost all of the organic matter on the wafer surface has a certain size, it is possible that almost all of it remains even after the nitride film is formed, resulting in larger defect sizes. In other words, although the above describes an example in which some of the defects disappear before and after the nitride film is formed, it is also possible that the number of defects remains almost the same before and after the nitride film is formed.
[0043] We have explained the typical defect types above, but for example, some defects will become larger and some will disappear, which is a possible phenomenon if the above-mentioned [COP] defect and [thermally stable particle] defects such as SiO2 are mixed on one wafer. However, in reality, in the current silicon wafer manufacturing process, thermally stable particles remain on the wafer and wafers with COPs are not manufactured, so there is no need to consider the simultaneous occurrence of two defects. In addition, as mentioned above, current wafer manufacturing is highly controlled, making it unlikely that different defect factors will occur simultaneously. Therefore, it is more realistic to exclude such complicated cases, and basically, one defect type can be identified by the present invention. However, even in the case of multiple types, as long as the change pattern can be grasped and each type can be identified, there is no particular limitation, and the present invention can be applied as a matter of course. EXAMPLES
[0044] The present invention will be described in more detail below by showing examples of the present invention, but the present invention is not limited to these. The particles present on the surface of silicon single crystal wafers before and after the formation of a nitride film were actually measured and evaluated using a particle counter to estimate the cause of the particles (defect type).The estimated defect type was then compared with the results of the cause investigation to confirm whether the estimated defect type was valid. Example 1 The silicon single crystal wafer thus prepared was subjected to the steps 1-3 of the present invention shown in Fig. 1 under the same conditions as those described above under <Various conditions in steps 1-3>. LPD maps before and after the nitride film formation, a defect size change graph, and a size histogram (defect histogram) of enlarged defects before the nitride film formation are shown in Figs. 17-19. From the map, it can be seen that the LPD (defect) in the center part has disappeared by the formation of the nitride film. It was confirmed from the haze map of SP7 that the newly detected LPDs on the periphery were false defects caused by the deterioration of haze. Since many of the defects were eliminated and the size of the remaining defects tended to become smaller, it can be inferred that the defects present on this wafer were COPs.
[0045] Furthermore, based on the manufacturing history of this wafer and SEM measurements of wafers from the same lot (wafers cut from the same crystal), it was found that the defect present in this wafer was a COP, proving that the inference made by the present invention was correct.
[0046] Example 2 A silicon single crystal wafer different from that in Example 1 was prepared, and steps 1-3 were carried out in the same manner as in Example 1. LPD maps before and after the nitride film formation, a defect size change graph, and a size histogram (defect histogram) of enlarged defects before the nitride film formation are shown in Figures 20-22. In Example 2, unlike Example 1, many defects remained and did not disappear. In addition, since there was no change in LPD size, it was expected that most of the defects were PIDs.
[0047] When the same lot of wafers was examined, it was found that the crystal manufacturing method did not result in COPs, and PIDs were confirmed by SEM. In other words, the LPDs present in these wafers are presumed to be PIDs, as predicted above.
[0048] Both Example 1 and Example 2 are wafers that have defects in the center of the wafer. It is not possible to distinguish between COP and PID from only the LPD map before the nitride film formation. However, it is possible to identify the type of defect by comparing the number of defects and the defect size using the LPD maps before and after the nitride film formation.
[0049] Example 3 A silicon single crystal wafer different from that in Example 1 was prepared, and steps 1-3 were carried out in the same manner as in Example 1. LPD maps before and after the nitride film formation, a defect size change graph, and a size histogram (defect histogram) of enlarged defects before the nitride film formation are shown in Figures 23-25. Defects that remain after the nitride film is formed often occur when thermally stable particles, i.e., SiO2 powder or Al2O3 powder, cannot be completely removed by cleaning, in which case the LPDs often have a flow pattern caused by cleaning. This wafer does not have this flow pattern. However, it does show a characteristic of thermally stable particles, namely, the initial LPDs (defects detected before the nitride film is formed) do not disappear even after the nitride film is formed. Furthermore, new defects were detected after the nitride film was formed. Furthermore, there is a characteristic that the size of the LPDs at the same point increases before and after the nitride film is formed, and it is inferred that this wafer has thermally stable particles on it.
[0050] To confirm this, a cross-sectional TEM was used to check the particles buried under the nitride film, and O was found. It is believed that the cause was probably small grains of SiO2. Normally, the LPD distribution on the wafer is a useful indicator of whether or not cleaning is the cause, and in most cases this will be a flow pattern. On the other hand, in this case, it was not possible to determine whether LPD was caused by cleaning based on the initial LPD map alone, but it was confirmed that this is possible by looking at the change in the number and size of defects before and after the formation of the nitride film.
[0051] Example 4 A silicon single crystal wafer different from that in Example 1 was prepared, and steps 1-3 were carried out in the same manner as in Example 1. LPD maps before and after the nitride film formation, defect size change graphs, and size histograms of enlarged defects before the nitride film formation (defect histograms) are shown in Figures 26-28. Few new LPDs were detected due to the nitride film formation, but many LPDs disappeared due to the nitride film formation. The size of the LPDs increased before and after the nitride film formation, and among the initial LPDs, the probability of small-sized LPDs disappearing was high. In other words, it can be assumed that thermally unstable particles are attached.
[0052] To confirm, we checked the manufacturing history of this sample and found that although there was no LPD generation at the time of shipping after cleaning, the LPD increased during transportation. In other words, it is believed that impurities generated from inside the box during transportation adhered to the wafers, and it is expected that the volatile components or plastic pieces generated from the plastic (polycarbonate) that is the material of the box adhered to the wafers. In either case, it is a thermally unstable substance, and as expected, it was found that thermally unstable particles had adhered to the wafers.
[0053] As can be seen from the results of Examples 1 to 4, the identification method of the present invention makes it possible to estimate / identify the original defect type of defects on a silicon single crystal wafer simply by comparing the number of defects (defect map) and defect size before and after the nitride film formation. This is simpler than the conventional method, which required time-consuming and labor-intensive methods such as cross-sectional TEM to identify the defect type.
[0054] The present invention is not limited to the above-described embodiment. The above-described embodiment is merely an example, and any configuration that is substantially the same as the technical idea described in the claims of the present invention and that provides similar effects is included in the technical scope of the present invention.
Claims
1. A method for identifying a type of defect in a silicon single crystal wafer, comprising the steps of: Detecting defects present on the surface of the silicon single crystal wafer with a particle counter to measure the number and size of the defects; forming a nitride film on the surface of the silicon single crystal wafer after the measurement; detecting defects present on the surface of the silicon single crystal wafer after the nitride film is formed using the particle counter and measuring the number and size of the defects; evaluating a change in the number of defects and a change in the size of the defects before and after forming the nitride film; A method for identifying a type of defect in a silicon single crystal wafer, comprising identifying the type of the defect from the results of the evaluation.
2. 2. The method for identifying a type of defect in a silicon single crystal wafer according to claim 1, wherein the thickness of the nitride film formed is set to 30 to 120 nm.
3. When evaluating the change in defect size, 3. The method for identifying a type of defect in a silicon single crystal wafer according to claim 1, further comprising obtaining position coordinates of the defect before and after the nitride film is formed, and evaluating defects at the same position coordinates.
4. If the result of the evaluation shows that the number of defects is reduced after the formation of the nitride film and the size of the remaining defects is reduced, 4. The method for identifying a type of defect in a silicon single crystal wafer according to claim 1, further comprising identifying the defect as a COP.
5. If the result of the evaluation shows that the number of defects has not changed and the size of the defects has not changed after the nitride film is formed, 4. The method for identifying a type of defect in a silicon single crystal wafer according to claim 1, further comprising identifying the defect as a PID.
6. In the result of the evaluation, if the defects detected before the formation of the nitride film remain after the formation of the nitride film and the defect size becomes large, and new defects are detected after the formation of the nitride film, 4. The method for identifying a type of defect in a silicon single crystal wafer according to claim 1, wherein the defect is identified as a thermally stable particle.
7. The thermally stable particles are made of SiO 2 Or Al 2 O 3 7. The method for identifying a type of defect in a silicon single crystal wafer according to claim 6, further comprising:
8. If the result of the evaluation shows that some of the defects detected before the formation of the nitride film have disappeared after the formation of the nitride film, and the defect sizes of the defects remaining after the formation of the nitride film have increased, 4. The method for identifying a type of defect in a silicon single crystal wafer according to claim 1, further comprising identifying the defect as a thermally unstable particle.
9. 9. The method for identifying a type of defect in a silicon single crystal wafer according to claim 8, wherein the thermally unstable particles are organic matter.
Citation Information
Patent Citations
Defect inspection method
JP2016212009A
Method for pinpointing silicon single crystal defect region
JP2018186195A
Defect Classification Device, Inspection Device, and Inspection System
US20200256807A1
Apparatus for Aiding Manufacturing of Optoelectronic Device
US20220236194A1
Defect classification device, inspection device, and inspection system
WO2019049387A1
Cited By
Organic defect source identification using artificial intelligence
US20260220769A1
Organic defect source identification using artificial intelligence
WO2026161118A1