Method for manufacturing epitaxial wafer
By employing a predictive model to optimize heater output ratios in a film-forming chamber, the method addresses the conflict between uniform resistivity and slip defect suppression, resulting in high-quality epitaxial wafers with improved uniformity and defect reduction.
Patent Information
- Application Number
- JP2021212153
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-12-27
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2041-12-27
AI Technical Summary
Existing epitaxial wafer manufacturing methods face challenges in achieving both uniform resistivity and suppressing slip defects, as the optimal conditions for each often conflict with each other, leading to difficulties in manufacturing high-quality wafers.
The method employs a combination of upper and lower heaters in a film-forming chamber to control the temperature distribution across the wafer surface, using a predictive model to determine optimal heater output ratios that minimize slip defects and ensure uniform resistivity by independently adjusting the heating from multiple angles.
This approach allows for the production of epitaxial wafers with suppressed slip defects and highly uniform resistivity, improving the overall quality and consistency of the manufacturing process.
Smart Images

Figure 0007567773000001 
Figure 0007567773000002 
Figure 0007567773000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing an epitaxial wafer. [Background technology]
[0002] A known method for manufacturing epitaxial wafers of silicon or the like is to perform a temperature increase step and a pre-bake step with a uniform temperature distribution within the wafer, and an epitaxial film formation step with a temperature distribution in which the temperature at the outer periphery of the wafer is low (see Patent Document 1).
[0003] In this manufacturing method, if the wafer in-plane temperature distribution (%) is defined as {temperature at the wafer center (°C) - temperature at a point 5 mm inside from the wafer outer periphery (°C)} / temperature at the wafer center (°C) x 100 (%), the heating process and pre-bake process are performed with a uniform wafer in-plane temperature distribution (-0.5 to +0.5%), and the epitaxial film formation process is performed with a temperature distribution where the temperature at the wafer outer periphery is low (0.5% to 3%). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent No. 5780491 Summary of the Invention [Problem to be solved by the invention]
[0005] Slip defects in silicon wafers are mainly caused by thermal stress at the contact points between the wafer and the member supporting the wafer during heat treatment, and are thought to occur especially during heating. In addition, when a silicon wafer with impurities is heated to grow an epitaxial film, the impurities added to the wafer jump out of the wafer and are incorporated into the growing epitaxial film, which is called the autodoping phenomenon, and the resistivity distribution within the wafer becomes non-uniform. In order to suppress this, the wafer is heated so that the temperature of the outer periphery is lower than the temperature of the center of the wafer.
[0006] That is, to improve the uniformity of resistivity within the wafer surface, it is desirable to have a temperature distribution within the wafer surface in which the temperature at the outer periphery of the wafer is lower than the temperature at the center of the wafer, but to suppress the occurrence of slip defects, it is desirable for the temperature distribution at the outer periphery of the wafer to be the same as that at the center of the wafer.As such, the optimal conditions for the two qualities of uniformity of resistivity within the wafer surface and prevention of the occurrence of slip defects are in conflict with each other, making it difficult to achieve both.
[0007] In the above-mentioned conventional technology, the temperature rise process and pre-bake process are performed with a uniform temperature distribution (-0.5 to +0.5%) within the wafer surface that suppresses the occurrence of slip defects, and the epitaxial film formation process is performed with a low temperature distribution (0.5% to 3%) at the outer periphery of the wafer, which results in a good resistivity distribution, thereby solving this problem.
[0008] However, even if the temperature distribution in the heating process and the pre-bake process are adjusted to suppress the occurrence of slip defects and the temperature distribution in the epitaxial film formation process is adjusted to provide a good resistivity distribution according to the above technical overview, there is a problem that slip defects will occur if the temperature distribution in the epitaxial film formation process deviates from the temperature distribution in which the occurrence of slip defects is suppressed.
[0009] An object of the present invention is to provide a method for producing an epitaxial wafer in which the occurrence of slip defects is suppressed and which has high uniformity of resistivity within the wafer surface. [Means for solving the problem]
[0010] The present invention provides a method for manufacturing an epitaxial wafer, comprising the steps of: using an upper heater disposed in an upper portion of a film formation chamber and a lower heater disposed in a lower portion of the film formation chamber, heating a wafer in the film formation chamber from an upper side at an upper heater output ratio and heating a wafer in the film formation chamber from a lower side at a lower heater output ratio, thereby forming an epitaxial film on the wafer, setting a plurality of first combinations of the upper heater output ratio on the upper side and the lower heater output ratio on the lower side, forming the epitaxial film using the plurality of first combinations set, measuring in-plane resistivities at a plurality of points of the obtained plurality of epitaxial wafers, and predicting an in-plane distribution of resistivity from a correlation between the in-plane measured values of resistivity of the plurality of epitaxial wafers and the upper heater output ratio and the lower heater output ratio; extracting a second combination of the upper heater output ratio on the upper side and the lower heater output ratio on the lower side, which brings the predicted in-plane distribution of resistivity into a predetermined range; forming the epitaxial film with the second combination; inspecting the occurrence of slip defects in the obtained epitaxial wafer; and extracting a third combination of the upper heater output ratio on the upper side and the lower heater output ratio on the lower side, which brings the occurrence of slip defects into a predetermined range; The above-mentioned problem is solved by a method for manufacturing an epitaxial wafer, in which the third combination is set as the upper heater output ratio and the lower heater output ratio during manufacturing.
[0011] The present invention also provides a method for setting heater output ratios in a vapor phase growth apparatus for forming an epitaxial film on a wafer by using an upper heater disposed in an upper portion of a deposition chamber and a lower heater disposed in a lower portion of the deposition chamber, and heating a wafer in the deposition chamber from an upper side at an upper heater output ratio and from a lower side at a lower heater output ratio, comprising the steps of: setting a plurality of first combinations of the upper heater output ratio on the upper side and the lower heater output ratio on the lower side, forming the epitaxial film using the plurality of first combinations set, measuring in-plane resistivities at a plurality of points of the obtained plurality of epitaxial wafers, and predicting an in-plane distribution of resistivity from a correlation between the in-plane measured values of resistivity of the plurality of epitaxial wafers and the upper heater output ratio and the lower heater output ratio; extracting a second combination of the upper heater output ratio on the upper side and the lower heater output ratio on the lower side, which brings the predicted in-plane distribution of resistivity into a predetermined range; forming the epitaxial film with the second combination; inspecting the occurrence of slip defects in the obtained epitaxial wafer; and extracting a third combination of the upper heater output ratio on the upper side and the lower heater output ratio on the lower side, which brings the occurrence of slip defects into a predetermined range; The above-mentioned problem is solved by a method for setting heater output ratios of a vapor phase growth apparatus, in which the third combination is set as the upper heater output ratio and the lower heater output ratio during manufacturing.
[0012] In the above invention, an upper outer heater for heating the outer periphery of the wafer and an upper inner heater for heating the center are disposed in the upper part of the deposition chamber, and a lower outer heater for heating the outer periphery of the back surface of a susceptor on which the wafer is placed and a lower inner heater for heating the center are disposed in the lower part of the deposition chamber, The upper heater output ratio includes the ratio of the output of the upper inner heater to the sum of the output of the upper inner heater and the output of the upper outer heater, and the lower heater output ratio includes the ratio of the output of the lower inner heater to the sum of the output of the lower inner heater and the output of the lower outer heater.
[0013] In the above invention, the resistivities of the multiple epitaxial wafers obtained by the first combination are measured at multiple reference measurement points, the deviation of the resistivity at each reference measurement point is determined, and a correlation between the deviation and the upper heater output ratio on the upper side and the lower heater output ratio on the lower side is determined, and the in-plane distribution of resistivity is predicted from the correlation.
[0014] In the above invention, the resistivities of a plurality of epitaxial wafers obtained by the first combination are measured at a plurality of reference measurement points, the difference and sum of the resistivities at each reference measurement point are calculated, a correlation is calculated between the difference and sum and the upper heater output ratio on the upper side and the lower heater output ratio on the lower side, and an in-plane distribution of resistivity is predicted from the correlation. Effect of the Invention
[0015] According to the present invention, it is possible to provide a method for producing an epitaxial wafer in which the occurrence of slip defects is suppressed and which has high uniformity of resistivity within the wafer surface. [Brief description of the drawings]
[0016] [Figure 1] 1 is a cross-sectional view showing a vapor phase growth apparatus according to an embodiment of the present invention. [Diagram 2] FIG. 4 is a process diagram showing a method for setting a heater output ratio of each heater in the vapor phase growth apparatus according to the embodiment of the present invention. [Diagram 3] FIG. 3 is a diagram showing a result of step S1 in FIG. 2 in the first embodiment of the present invention. [Figure 4] FIG. 2 is a plan view of a wafer showing resistivity measurement points. [Diagram 5] FIG. 3 is a diagram showing the results of steps S2 to S3 in FIG. 2 in the first embodiment of the present invention. [Figure 6] FIG. 3 is a diagram showing a result of step S5 in FIG. 2 in the first embodiment of the present invention. [Figure 7] FIG. 1 is a diagram showing the results of Comparative Example 1 compared to Example 1 of the present invention. [Figure 8] FIG. 3 is a diagram showing a result of step S1 in FIG. 2 in the second embodiment of the present invention. [Figure 9] FIG. 3 is a diagram showing the results of steps S2 to S3 in FIG. 2 in Example 2 of the present invention. [Figure 10] FIG. 3 is a diagram showing a result of step S5 in FIG. 2 in the second embodiment of the present invention. [Figure 11]FIG. 1 is a diagram showing the results of Comparative Example 2 compared to Example 2 of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] FIG. 1 is a cross-sectional view showing a vapor phase growth apparatus 1 according to an embodiment of the present invention. The vapor phase growth apparatus 1 of this embodiment has a film formation chamber 14 formed by mounting an upper dome 12 and a lower dome 13 to a dome mounting body 11. The upper dome 11 and the lower dome 12 constituting the film formation chamber 14 are made of a transparent material such as quartz. A susceptor 15 on which a wafer W is placed is provided inside the film formation chamber 14. The susceptor 15 is formed of a material such as a carbon base material coated with a SiC film on its surface, and supports, for example, the outer periphery of the back surface of the wafer W. During epitaxial growth processing, the susceptor 15 rotates at a constant rotation speed by a susceptor support 16 with the wafer W placed thereon.
[0018] A plurality of heaters 17A to 17D are provided above and below the film formation chamber 14, and these heaters heat the wafer W placed in the film formation chamber 14 to a predetermined temperature. The heaters 17A to 17D in this embodiment are, for example, halogen lamps or the like, and include an upper outer heater 17A arranged on the upper outside of the film formation chamber 14, an upper inner heater 17B arranged on the upper inside, a lower outer heater 17C arranged on the lower outside of the film formation chamber 14, and a lower inner heater 17D arranged on the lower inside.
[0019] The upper outer heater 17A, the upper inner heater 17B, the lower outer heater 17C and the lower inner heater 17D are arranged at equal intervals radially around the center point of the wafer W placed on the susceptor 15 in plan and bottom views. The upper outer heater 17A mainly supplies heating energy to the outer periphery of the upper part of the wafer W, the upper inner heater 17B mainly supplies heating energy to the center part of the upper part of the wafer W, the lower outer heater 17C mainly supplies heating energy to the outer periphery of the lower part of the wafer W via the susceptor 15, and the lower inner heater 17D mainly supplies heating energy to the center part of the lower part of the wafer W via the susceptor 15.
[0020] The power supplied to each of the heaters 17A-17D is supplied by a heating control device 18, and each of the heaters 17A-17D is controlled independently of each other. The heating energy of each of the heaters 17A-17D is adjusted by the heating control device 18 in response to a command set by a heater output ratio setting method described later. The method of setting the heater output ratio for setting the power supplied to each of the heaters 17A-17D will be described later.
[0021] A gas inlet 19 is provided on a side of the film formation chamber 14, and a gas outlet 20 is provided on the opposite side of the film formation chamber 14. A reactive gas is introduced into the film formation chamber 14 from the gas inlet 19, and the introduced reactive gas passes through the surface of the wafer W to grow an epitaxial film, and is then exhausted from the gas outlet 20 to the outside of the vapor phase growth apparatus 1. For example, the reactive gas for forming a silicon epitaxial film is a reactive gas obtained by diluting a Si source such as dichlorosilane SiH2Cl2 or trichlorosilane SiHCl3 with hydrogen gas and mixing a trace amount of a dopant therein.
[0022] Next, a method for setting the heater output ratio for setting the power supplied to each of the heaters 17A to 17D will be described. As described above, when forming a silicon epitaxial film on a silicon wafer, it is required that the uniformity of the resistivity of the epitaxial film in the wafer plane is good and that slip defects do not occur. In order to improve the uniformity of the resistivity of the epitaxial film in the wafer plane, it is desirable to have a wafer-plane temperature distribution in which the temperature of the outer periphery of the wafer is lower than the temperature of the center of the wafer. On the other hand, in order to suppress the occurrence of slip defects, it is desirable that the temperature of the outer periphery of the wafer and the temperature of the center of the wafer have the same temperature distribution. As described above, the optimal conditions for two qualities, the uniformity of resistivity in the wafer plane and the prevention of the occurrence of slip defects, are contradictory, so it is difficult to achieve both.
[0023] Here, the resistivity of the epitaxial film is affected by the temperature distribution of the surface of the wafer (the upper surface in FIG. 1) on which the epitaxial film is formed, and is therefore significantly affected by the output ratio (= heating energy supply ratio) between the upper outer heater 17A and the upper inner heater 17B, which directly heat the wafer surface. On the other hand, the origin of the occurrence of slip defects is scratches and stress occurring at the contact position between the wafer W and the susceptor 15, and therefore the temperature environment at this contact position affects the occurrence of slip defects. Since the temperature of the susceptor 15 is strongly affected by the output ratio between the lower outer heater 17C and the lower inner heater 17D, the occurrence of slip defects is significantly affected by the output ratio between the lower outer heater 17C and the lower inner heater 17D.
[0024] From this viewpoint, in the vapor phase growth apparatus 1 of this embodiment, the output ratio between the upper outer heater 17A and the upper inner heater 17B (hereinafter also referred to as the output ratio PU of the upper heater) and the output ratio between the lower outer heater 17C and the lower inner heater 17D (hereinafter also referred to as the output ratio PL of the lower heater) are set according to the procedure shown in Fig. 2, on the premise that the four heaters 17A to 17D are controlled independently of one another. Fig. 2 is a process diagram showing a method of setting the heater output ratio of each of the heaters 17A to 17D in the vapor phase growth apparatus 1 of this embodiment. Note that the output of a heater means the amount of power supplied to the heater, and the heating temperature of the wafer W is set according to this. In addition, the output ratio PU of the upper heaters is defined as (output of upper inner heater 17B) / (output of upper outer heater 17A + output of upper inner heater 17B), and the output ratio PL of the lower heaters is defined as (output of lower inner heater 17D) / (output of lower outer heater 17C + output of lower inner heater 17D).
[0025] In the heater output ratio setting method of the present embodiment shown in Fig. 2, in step S1, as the initial value (first combination) of the combination of the output ratio PU of the upper heater and the output ratio PL of the lower heater, for example, a combination of the maximum and minimum values of the settable range of each is selected, an epitaxial wafer is actually manufactured under this condition, and the resistivity of the epitaxial film in the wafer surface is actually measured. The combination of the maximum and minimum values (output ratio PU of the upper heater, output ratio PL of the lower heater) selected as the initial value (first combination) of the combination of the output ratio PU of the upper heater and the output ratio PL of the lower heater is four levels, (0,0), (0,100), (100,0), and (100,100), as shown in Fig. 3. The values (0 to 100) of the upper heater output ratio PU and the lower heater output ratio PL shown in the four levels are values obtained by normalizing the maximum and minimum values of the settable range of each of the upper heater and the lower heater to 0 to 100. However, the initial value (first combination) of the combination of the output ratio PU of the upper heater and the output ratio PL of the lower heater selected in step S1 is not limited to only the combination of the maximum and minimum values shown in Fig. 3, but may be any combination that allows for accurate prediction of the in-plane distribution of resistivity at any measurement point in the next step S2. Also, the actual measurement value of the resistivity of the epitaxial film in the wafer plane is measured, for example, at the center P1 of the wafer and five points P2 to P5 on the periphery of the wafer as shown in Fig. 4. These P1 to P5 are referred to as measurement points.
[0026] In the next step S2, the resistivity of the epitaxial film in the wafer plane obtained in step S1 is used to calculate a predicted value of the in-plane distribution of resistivity in a combination of an arbitrary upper heater output ratio and an arbitrary lower heater output ratio by using a multiple regression method or the like. That is, the difference (deviation) between the average value and the average value at each of the measurement points P1 to P5 of each epitaxial wafer for four levels obtained by the initial value (first combination) of the combination of the upper heater output ratio PU and the lower heater output ratio PL is calculated from the actual measurement values of the resistivity at each of the measurement points P1 to P5 of each epitaxial wafer, and from this result, a correlation equation between the deviation at each of the measurement points P1 to P5 and the upper heater output ratio PU and the lower heater output ratio PL is calculated by using a multiple regression method. Then, the in-plane distribution (standard deviation) of resistivity at an arbitrary upper heater output ratio and an arbitrary lower heater output ratio is calculated and predicted from the sum of squares of the deviation of resistivity at each of the measurement points P1 to P5 and the number of measurement points, as shown in FIG. 5. The solid line in FIG. 5 is a contour plot of the standard deviation calculated from the correlation equation between the deviation calculated by the multiple regression method and the output ratio PU of the upper heater and the output ratio PL of the lower heater, and 0.08, 0.16, 0.24, 0.32, and 0.40 indicate the predicted values of the standard deviation for each multiple regression line.
[0027] In the next step S3, among the predicted values of the in-plane distribution (standard deviation) of resistivity at any upper heater output ratio and any lower heater output ratio calculated in step S2, a favorable range that results in the target resistivity distribution is specified, and several combinations (second combinations) of the upper heater output ratio PU and the lower heater output ratio PL are extracted from the range. The values of the second combinations to be extracted here are not particularly limited. If a large number of second combinations are extracted, the number of times the next step S4 is performed increases, which increases the work man-hours, but if the number of extracted second combinations is too small, there is a possibility that a range with favorable slip defects cannot be found in the next step S4. Therefore, it is desirable to extract as few second combinations as possible that cover all ranges. For example, in FIG. 5, the range indicated by the dotted line is the range with the smallest standard deviation (0.08) or less, and therefore is the range with the most favorable variation in the in-plane distribution of resistivity. Therefore, in order to cover the range indicated by the dotted line with the minimum number of extractions, the four combinations indicated by "■" (PU,PL) = (90,10), (60,30), (30,50), and (0,70) are extracted.
[0028] In the next step S4, an epitaxial wafer is actually manufactured under the conditions of the second combination extracted in step S3, and the occurrence of slip defects is inspected. Then, in step S5, a combination of the upper heater output ratio PU and the lower heater output ratio PL that is in a good range for the occurrence of slip defects is identified from among the second combinations implemented in step S4, and this is extracted as a third combination. If there are multiple third combinations, any one of them may be extracted. In step S5, the combination of the upper heater output ratio PU and the lower heater output ratio PL related to the third combination extracted in step S4 is set to the heater setting value during actual manufacturing, and the vapor phase growth apparatus 1 is operated to manufacture an epitaxial wafer.
[0029] As described above, the vapor phase growth apparatus 1 of the present embodiment can manufacture epitaxial wafers that suppress the occurrence of slip defects and have high uniformity of resistivity in the wafer surface. In selecting a combination of the upper heater output ratio PU and the lower heater output ratio PL that affect the uniformity of resistivity in the wafer surface and the suppression of the occurrence of slip defects, the in-plane distribution of resistivity is predicted from the in-plane actual measured values of resistivity of multiple epitaxial wafers and the upper heater output ratio and the lower heater output ratio, and the occurrence status of slip defects is confirmed within a range where the predicted in-plane distribution of resistivity is favorable, so that the final combination can be determined in a short time with a minimum number of steps. EXAMPLES
[0030] Below, we will give specific examples of combinations of the upper heater output ratio PU and the lower heater output ratio PL of the vapor phase growth apparatus 1 of the present embodiment described above, and more specifically explain the epitaxial wafer manufacturing method of the present invention and the method of setting the heater output ratio of the vapor phase growth apparatus.
[0031] Example 1 1, a silicon epitaxial film was formed on the surface of a silicon wafer having a diameter of 300 mm with a target film thickness of 4 μm and a target resistivity of 10 Ωcm. In Example 1, the standard deviation of the actual measured resistivity values was used as an index of the in-plane distribution of resistivity, and the favorable range (standard deviation) of the in-plane distribution of resistivity of the silicon epitaxial film was set to 0.08 or less, and the favorable range of slip defects was set to a total slip length of 3 mm or less.
[0032] First, as the first combination of the output ratio PU of the upper heater and the output ratio PL of the lower heater, four levels shown in Fig. 3, (output ratio PU of the upper heater, output ratio PL of the lower heater) = (0,0), (0,100), (100,0), (100,100), were selected, and a silicon epitaxial film was formed on the surface of a silicon wafer with a diameter of 300 mm at these four levels with a target film thickness of 4 μm and a target resistivity of 10 Ω cm. The resistivity of the obtained silicon epitaxial wafer was measured at five points shown in Fig. 4, P1 = (0,0), P2 = (0,145), P3 = (145,0), P4 = (0,-145), P5 = (-145,0) (the wafer center is the origin and the plane is shown in xy plane coordinates (unit: mm)), and the resistivity was measured by the HgCV method. Then, for each of the four levels, the deviation of resistivity at all measurement points (the difference between the average value of all measurement points and the resistivity at each measurement point) was calculated. The results of the deviation of resistivity at each level and each measurement point are shown in Figure 3.
[0033] When the correlation between the output ratio PU of the upper heater and the output ratio PL of the lower heater is determined by multiple regression from the resistivity deviation at each level and each measurement point shown in Figure 3, the correlation formula is given as follows: -Deviation of measuring point P1 = +0.005467×PU+0.00752288×PL-0.550285 -Deviation of measuring point P2 = -0.0014748 x PU -0.001754 x PL +0.0703375 -Deviation of measuring point P3 = -0.0014545×PU-0.0017027×PL+0.1358425 -Deviation of measuring point P4 = -0.0013878×PU-0.0021094×PL+0.2201525 -Deviation of measuring point P5 = -0.0011501 x PU - 0.0019569 x PL + 0.1239525
[0034] The above correlation equation was used to calculate the predicted value of the resistivity deviation at any heater output ratio PU, PL. Furthermore, the predicted value of the resistivity in-plane distribution (standard deviation) was calculated from the sum of squares of the deviation and the number of measurement points. The results are shown in Figure 5. Figure 5 is a contour diagram of the deviation calculated by the multiple regression method and the standard deviation calculated by the correlation equation between the upper heater output ratio PU and the lower heater output ratio PL, and the numbers 0.08, 0.16, 0.24, 0.32, and 0.40 indicate the predicted value of the standard deviation for each multiple regression line. Therefore, the range in which the resistivity in-plane distribution at any measurement point on the wafer is smallest is the range with the smallest standard deviation, that is, the range of standard deviation = 0.08 or less shown by the dotted line in Figure 5.
[0035] Next, within the range where the standard deviation in FIG. 5 is 0.08 or less, four levels of (upper heater output ratio PU, lower heater output ratio PL) = (90, 10), (60, 30), (30, 50), and (0, 70) were extracted as the second combination of the upper heater output ratio PU and the lower heater output ratio PL, and using the same vapor phase growth apparatus 1, a silicon epitaxial film was formed on the surface of a silicon wafer with a diameter of 300 mm with a target film thickness of 4 μm and a target resistivity of 10 Ω cm. The occurrence of slip defects in the obtained silicon epitaxial wafer was inspected. The results are shown in FIG. 6. As a result, among the four levels of the second combination, the occurrence of slip defects was also good for the combinations of (upper heater output ratio PU, lower heater output ratio PL) = (90, 10) and (60, 30), so these two combinations were extracted as the final third combination.
[0036] Comparative Example 1 As a comparative example of the above-mentioned Example 1, a combination of the output ratio PU of the upper heater and the output ratio PL of the lower heater was determined in advance as shown in the following formula 1 (a and b are constants) in Comparative Example 1. Using the same vapor phase growth apparatus 1 as in Example 1, and under the same conditions as in Example 1, a silicon epitaxial film was formed on the surface of a silicon wafer having a diameter of 300 mm with a target film thickness of 4 μm and a target resistivity of 10 Ωcm. The resistivity at measurement points P1 to P5 of the obtained silicon epitaxial wafer was measured by the HgCV method, and the occurrence of slip defects was inspected. The results are shown in FIG. 7. None of the levels satisfied both the judgment of the in-plane distribution of resistivity and the judgment of slip defects. Number 1 Upper heater output ratio PU(%) = a × Lower heater output ratio PL(%) + b(%) ... Equation 1
[0037] Example 2 Using the vapor phase growth apparatus 1 shown in Fig. 1, a silicon epitaxial film was formed on the surface of a silicon wafer having a diameter of 300 mm with a target film thickness of 4 µm and a target resistivity of 10 Ωcm. In Example 2, the ratio of the difference to the sum of the maximum in-plane resistance value and the minimum in-plane resistance value ((maximum in-plane value [Ωcm] - minimum in-plane value [Ωcm]) / (maximum in-plane value [Ωcm] + minimum in-plane value [Ωcm]) x 100) was used as an index of the in-plane distribution of resistivity, and the favorable range of the in-plane distribution of resistivity of the silicon epitaxial film was set to 1.0% or less, and the favorable range of slip defects was set to a total slip length of 3 mm or less.
[0038] First, as the first combination of the output ratio PU of the upper heater and the output ratio PL of the lower heater, four levels shown in Fig. 8, (output ratio PU of the upper heater, output ratio PL of the lower heater) = (0,0), (0,100), (100,0), (100,100), were selected, and a silicon epitaxial film was formed on the surface of a silicon wafer with a diameter of 300 mm at these four levels with a target film thickness of 4 μm and a target resistivity of 10 Ω cm. The resistivity of the obtained silicon epitaxial wafer was measured at five points shown in Fig. 4, P1 = (0,0), P2 = (0,145), P3 = (145,0), P4 = (0,-145), P5 = (-145,0) (the wafer center is the origin and the plane is shown in xy plane coordinates (unit: mm)), and the resistivity was measured by the HgCV method. Then, for each of the four levels, the difference and sum of the resistivity between any two of all the measurement points were calculated. The results of the difference and sum of the resistivity at each level and each measurement point are shown in Figure 8. In Figure 8, "resistivity difference (P1-P2)" shows the difference in resistivity between measurement points P1 and P2, and "resistivity sum (P1+P2)" shows the sum of the resistivity between measurement points P1 and P2. The difference and sum between all the measurement points were calculated, but some are not shown in the figure.
[0039] When the correlation between the output ratio PU of the upper heater and the output ratio PL of the lower heater is calculated by multiple regression from the difference and sum of the resistivity at each level and each measurement point shown in Figure 8, the correlation formula is as follows. Note that only a part of the correlation formula is shown. Resistivity of measurement point P1 - Resistivity of P2 = -0.0067149 x PU - 0.009058 x PL + 0.574995 Resistivity of measurement point P1 - Resistivity of P3 = -0.0064342×PU-0.0094731×PL+0.631915 Resistivity of measurement point P4 - Resistivity of P5 = +0.0000284×PU+0.0001442×PL-0.08632 Resistivity of measurement point P1 + resistivity of P2 = +0.0030495×PU+0.0030836×PL+19.599615 Resistivity of measurement point P1 + resistivity of P3 = +0.0027688×PU+0.0034987×PL+19.542695 Resistivity of measurement point P4 + resistivity of P5 = +0.009825×PU+0.0141122×PL+18.70439
[0040] From the above correlation equation, the predicted values of the resistivity difference and sum at any heater output ratio PU, PL were obtained. Furthermore, the predicted value of the resistivity in-plane distribution (maximum of difference) / (minimum of sum) was obtained from the maximum of multiple differences and the minimum of multiple sums at any heater output ratio PU, PL. The result is shown in FIG. 9. FIG. 9 is a contour diagram of the in-plane distribution obtained from the correlation equation of the difference and sum obtained by the multiple regression method and the output ratio PU of the upper heater and the output ratio PL of the lower heater, and each number of 1.0, 2.0, 3.0, 4.0, and 5.0 indicates the predicted value of the ratio of the maximum of the difference to the minimum of the sum in each multiple regression analysis. Therefore, the range in which the in-plane distribution of the resistivity of the wafer is smallest is the range in which the ratio of the maximum of the difference to the minimum of the sum is small, that is, the range in which the ratio of the maximum of the difference to the minimum of the sum shown by the dotted line in FIG. 9 is 1.0 or less.
[0041] Next, within the range where the ratio of the maximum difference to the minimum sum in FIG. 9 is 1.0 or less, four levels of (upper heater output ratio PU, lower heater output ratio PL)=(90,10), (60,30), (30,50), and (0,70) were extracted as the second combination of the upper heater output ratio PU and the lower heater output ratio PL. Using the same vapor phase growth apparatus 1, a silicon epitaxial film was formed on the surface of a silicon wafer with a diameter of 300 mm with a target film thickness of 4 μm and a target resistivity of 10 Ω cm. The occurrence of slip defects in the obtained silicon epitaxial wafer was inspected. The results are shown in FIG. 10. As a result, among the four levels of the second combination, the occurrence of slip defects was also good for the combination of (upper heater output ratio PU, lower heater output ratio PL)=(90,10), and therefore this combination was extracted as the final third combination.
[0042] Comparative Example 2 As a comparative example of the above-mentioned Example 2, a combination of the output ratio PU of the upper heater and the output ratio PL of the lower heater was determined in advance as shown in the following formula 2 (c and d are constants) in Comparative Example 2. Using the same vapor phase growth apparatus 1 as in Example 2, and under the same conditions as in Example 2, a silicon epitaxial film was formed on the surface of a silicon wafer having a diameter of 300 mm with a target film thickness of 4 μm and a target resistivity of 10 Ωcm. The resistivity at measurement points P1 to P5 of the obtained silicon epitaxial wafer was measured by the HgCV method, and the occurrence of slip defects was inspected. The results are shown in FIG. 11. None of the levels satisfied both the judgment of the in-plane distribution of resistivity and the judgment of slip defects. Number 2 Upper heater output ratio PU(%) = c × Lower heater output ratio PL(%) + d(%)…Equation 2 [Explanation of symbols]
[0043] 1...Vapor growth equipment 11...Dome mounting body 12...Upper dome 13…Lower dome 14...Deposition chamber 15…Susceptor 16...Susceptor support 17, 17A~17D...Heater 18... Heating control device 19…Gas inlet 20…Gas exhaust port PU: Upper heater output ratio PL: Lower heater output ratio P1~P5…Measurement points
Claims
1. A method for manufacturing an epitaxial wafer, comprising the steps of: using an upper heater disposed in an upper portion of a film formation chamber and a lower heater disposed in a lower portion of the film formation chamber, heating a wafer in the film formation chamber from an upper side at an upper heater output ratio and heating a wafer in the film formation chamber from a lower side at a lower heater output ratio, thereby forming an epitaxial film on the wafer, setting a plurality of first combinations of an upper heater output ratio on the upper side and a lower heater output ratio on the lower side, forming the epitaxial film using the plurality of first combinations set, measuring in-plane resistivities at a plurality of points of the obtained plurality of epitaxial wafers, and predicting an in-plane distribution of resistivity from a correlation between the in-plane measured values of resistivity of the plurality of epitaxial wafers and the upper heater output ratio and the lower heater output ratio; extracting a second combination of the upper heater output ratio on the upper side and the lower heater output ratio on the lower side, which brings the predicted in-plane distribution of resistivity into a predetermined range; forming the epitaxial film with the second combination; inspecting the occurrence of slip defects in the obtained epitaxial wafer; and extracting a third combination of the upper heater output ratio on the upper side and the lower heater output ratio on the lower side, which brings the occurrence of slip defects into a predetermined range; A method for manufacturing an epitaxial wafer, the method comprising: setting the third combination as the upper heater output ratio and the lower heater output ratio during manufacturing.
2. An upper outer heater for heating the outer periphery of the wafer and an upper inner heater for heating the center of the wafer are disposed in the upper portion of the deposition chamber; A lower outer heater for heating the outer periphery of the back surface of a susceptor on which the wafer is placed and a lower inner heater for mainly heating the center portion are disposed in the lower portion of the deposition chamber; 2. The method for manufacturing an epitaxial wafer according to claim 1, wherein the upper heater output ratio includes a ratio of the output of the upper inner heater to the sum of the output of the upper inner heater and the output of the upper outer heater, and the lower heater output ratio includes a ratio of the output of the lower inner heater to the sum of the output of the lower inner heater and the output of the lower outer heater.
3. 3. The method for manufacturing an epitaxial wafer according to claim 1 or 2, further comprising the steps of: measuring resistivities of a plurality of epitaxial wafers obtained by the first combination at a plurality of reference measurement points; determining a deviation of resistivity at each reference measurement point; determining a correlation between the deviation and an upper heater output ratio on the upper side and a lower heater output ratio on the lower side; and predicting an in-plane distribution of resistivity from the correlation.
4. 3. The method for manufacturing an epitaxial wafer according to claim 1 or 2, further comprising the steps of: measuring resistivities of a plurality of epitaxial wafers obtained by the first combination at a plurality of reference measurement points; determining a difference and a sum of the resistivities at each reference measurement point; determining a correlation between the difference and the sum and an upper heater output ratio on the upper side and a lower heater output ratio on the lower side; and predicting an in-plane distribution of resistivity from the correlation.
5. A method for setting heater output ratios of a vapor phase growth apparatus for forming an epitaxial film on a wafer by using an upper heater disposed in an upper portion of a deposition chamber and a lower heater disposed in a lower portion of the deposition chamber, and heating a wafer in the deposition chamber from an upper side at an upper heater output ratio and from a lower side at a lower heater output ratio, comprising the steps of: setting a plurality of first combinations of an upper heater output ratio on the upper side and a lower heater output ratio on the lower side, forming the epitaxial film using the plurality of first combinations set, measuring in-plane resistivities at a plurality of points of the obtained plurality of epitaxial wafers, and predicting an in-plane distribution of resistivity from a correlation between the in-plane measured values of resistivity of the plurality of epitaxial wafers and the upper heater output ratio and the lower heater output ratio; extracting a second combination of the upper heater output ratio on the upper side and the lower heater output ratio on the lower side, which brings the predicted in-plane distribution of resistivity into a predetermined range; forming the epitaxial film with the second combination; inspecting the occurrence of slip defects in the obtained epitaxial wafer; and extracting a third combination of the upper heater output ratio on the upper side and the lower heater output ratio on the lower side, which brings the occurrence of slip defects into a predetermined range; A method for setting heater output ratios of a vapor phase growth apparatus, the method comprising: setting the third combination as the upper heater output ratio and the lower heater output ratio at the time of manufacture.
6. An upper outer heater for heating the outer periphery of the wafer and an upper inner heater for heating the center of the wafer are disposed in the upper portion of the deposition chamber; A lower outer heater for heating the outer periphery of the back surface of a susceptor on which the wafer is placed and a lower inner heater for heating the center portion are disposed in the lower portion of the deposition chamber; 6. The method for setting heater output ratios in a vapor phase growth apparatus according to claim 5, wherein the upper heater output ratio includes a ratio of the output of the upper inner heater to the sum of the output of the upper inner heater and the output of the upper outer heater, and the lower heater output ratio includes a ratio of the output of the lower inner heater to the sum of the output of the lower inner heater and the output of the lower outer heater.
7. 7. The method for setting a heater output ratio of a vapor phase growth apparatus according to claim 5 or 6, further comprising the steps of: measuring resistivities of a plurality of epitaxial wafers obtained by the first combination at a plurality of reference measurement points; determining a deviation in resistivity at each reference measurement point; determining a correlation between the deviation and an upper heater output ratio on the upper side and a lower heater output ratio on the lower side; and predicting an in-plane distribution of resistivity from the correlation.
8. 7. The method for setting a heater output ratio of a vapor phase growth apparatus according to claim 5 or 6, further comprising the steps of: measuring resistivities of a plurality of epitaxial wafers obtained by the first combination at a plurality of reference measurement points; determining a difference and a sum of the resistivities at each reference measurement point; determining a correlation between the difference and the sum and an upper heater output ratio on the upper side and a lower heater output ratio on the lower side; and predicting an in-plane distribution of resistivity from the correlation.