GaN substrate wafer and method for producing same
By growing a GaN layer doped with compensating impurities on a low impurity GaN wafer, the method addresses inefficiencies in existing GaN substrate production, improving productivity and enabling the use in nitride semiconductor devices.
Patent Information
- Application Number
- JP2021522864
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-06-19
- Filing Date
- 2020-05-28
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2040-05-28
Smart Images

Figure 0007567786000001 
Figure 0007567786000002 
Figure 0007567786000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a substrate wafer made of GaN (gallium nitride) and a manufacturing method thereof. TECHNICAL FIELD The present invention relates to a substrate wafer made of GaN (gallium nitride) and a manufacturing method thereof. [Background technology]
[0002] A GaN substrate wafer with a high resistance region partially formed only on the front surface side has been proposed (Patent Document 1), which is obtained by growing a GaN thick film, which has a region with a high transition metal atom concentration only on the upper part, on a sapphire wafer by HVPE (hydride vapor phase epitaxy), and then peeling the GaN thick film from the sapphire wafer. GaN crystals that have been made highly resistive by doping with impurities are prone to cracking, but Patent Document 1 describes that GaN substrate wafers manufactured by this method are less likely to crack. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2012-232884 A Summary of the Invention [Problem to be solved by the invention]
[0004] When a GaN substrate wafer having a region with partially increased resistivity only on the front surface side is manufactured by the method disclosed in Cited Document 1, a GaN thick film needs to be grown by HVPE on a sapphire wafer for each GaN substrate wafer produced. [Means for solving the problem]
[0005] The present inventors have realized that, instead of the method disclosed in Cited Document 1, if a GaN wafer with a low impurity concentration is manufactured in advance and then a GaN layer doped with compensating impurities is grown thereon, a GaN substrate wafer having a region with partially increased resistivity only on the front surface side can be produced more efficiently. The present invention has been made based on this idea, and embodiments thereof include the following.
[0006] [1] A (0001) oriented GaN substrate wafer, a first region provided on the N-polarity side across a regrowth interface, and a second region having a minimum thickness provided on the Ga-polarity side; The second region has a minimum thickness of 20 μm or more; The total concentration of compensating impurities in at least a portion of the second region is 1×10 17 atoms / cm 3 That is all for the GaN substrate wafer. [2] The GaN substrate wafer according to [1] above, wherein the first region satisfies one or more conditions selected from the following (a) to (c): (a) Si concentration is 5×10 16 atoms / cm 3 That's all. (b) O concentration is 3 × 10 16 atoms / cm 3 The following is the result. (c) H concentration is 1×10 17 atoms / cm 3 The following is the result. [3] The GaN substrate wafer according to [1] or [2] above, wherein in the first region, a total concentration of compensating impurities is lower than a total concentration of donor impurities. [4] In the first region, the total concentration of compensating impurities is 1×10 17 atoms / cm 3 The GaN substrate wafer according to any one of the above [1] to [3], wherein the GaN substrate wafer is less than 100%. [5] In the first region, the concentrations of impurity elements other than Si, O, and H are independently 5×10 15 atoms / cm 3The GaN substrate wafer according to any one of the above [1] to [4], which is as follows: [6] A GaN substrate wafer according to any one of the above [1] to [5], which satisfies any one of the conditions selected from the following (1) to (3): (1) Having a diameter of 50 mm or more and 55 mm or less and a thickness of 250 μm or more and 450 μm or less. (2) Having a diameter of 100 mm or more and 105 mm or less and a thickness of 350 μm or more and 750 μm or less. (3) Having a diameter of 150 mm or more and 155 mm or less and a thickness of 450 μm or more and 800 μm or less. [7] The second region has a main doped region including at least a Ga-polar main surface, and a total concentration of compensating impurities in the main doped region is 1×10 17 atoms / cm 3 The GaN substrate wafer according to any one of the above [1] to [6]. [8] The total concentration of compensating impurities in the primary doped region is 1×10 18 atoms / cm 3 The GaN substrate wafer according to [7] above. [9] The GaN substrate wafer according to [7] or [8] above, wherein in the primarily doped region, the total concentration of compensating impurities is at least twice the total concentration of donor impurities.
[10] The GaN substrate wafer according to any one of [7] to [9] above, wherein the primarily doped region contains one or more elements selected from carbon and transition metal elements.
[11] The GaN substrate wafer according to any one of [7] to
[10] above, wherein the impurity contained in the primarily doped region at the highest concentration is Fe, Mn or C.
[12] The GaN substrate wafer according to any one of [7] to
[11] above, wherein the primarily doped region is a region within a specific length from a main surface on the GaN polarity side, and the specific length is 20 μm or more.
[13] The GaN substrate wafer according to any one of [7] to
[12] above, wherein in the primarily doped region, the variation in the total concentration of compensating impurities along the c-axis direction is within a range of ±25% from the median value.
[14] The GaN substrate wafer according to
[12] or
[13] above, wherein the specific length is greater than 50 μm.
[15] The GaN substrate wafer according to any one of
[12] to
[14] above, wherein the specific length is 50% or more of the minimum thickness of the second region.
[16] The total concentration of compensating impurities in the second region is 5×10 19 atoms / cm 3 The GaN substrate wafer according to any one of the above [1] to
[15] , which is as follows:
[17] The GaN substrate wafer according to any one of [1] to
[16] above, wherein the second region has a minimum thickness of 300 μm or less.
[18] A GaN substrate wafer according to any one of [1] to
[17] above, wherein the main surface on the Ga-polar side is a flat surface.
[19] The GaN substrate wafer according to
[18] , wherein the regrowth interface is inclined with respect to the Ga-polar primary surface.
[20] The GaN substrate wafer according to
[19] , wherein a difference in thickness between one end and the other end in a direction in which the regrowth interface in the second region is inclined does not exceed 200 μm.
[21] An epitaxial wafer comprising the GaN substrate wafer according to any one of [1] to
[20] above, and a nitride semiconductor layer epitaxially grown on a Ga-polar main surface of the GaN substrate wafer.
[22] A method for producing an epitaxial wafer, comprising the steps of: preparing a GaN substrate wafer according to any one of the above [1] to
[20] ; and growing a nitride semiconductor layer on a Ga-polar primary surface of the GaN substrate wafer.
[23] A method for manufacturing a nitride semiconductor device, comprising: a step of preparing a GaN substrate wafer according to any one of the above [1] to
[20] ; a step of growing a nitride semiconductor layer on a Ga-polar main surface of the GaN substrate wafer to obtain an epitaxial wafer; and a step of removing the first region of the GaN substrate wafer in at least a part of the epitaxial wafer.
[24] a second step of growing a (0001) oriented second thick GaN film on the substrate by HVPE and then slicing the second thick GaN film to obtain a second c-plane GaN wafer; and a third step of growing a (0001) oriented GaN film greater than 50 μm thick on the second c-plane GaN wafer by HVPE; and The GaN film has a total concentration of compensation impurities of 1×10 17 atoms / cm 3 A method for producing a GaN substrate wafer, comprising the steps of: providing a portion as described above;
[25] A method for producing a GaN substrate wafer having an N-polarity region and a Ga-polarity region sandwiching a regrowth interface, comprising the steps of: (i) a first step of growing a first thick GaN film, which is made of intentionally undoped GaN and has a (0001) orientation, on a seed wafer by HVPE and processing the first thick GaN film to obtain at least one first c-plane GaN wafer; (ii) a second step of growing a second thick GaN film, consisting of intentionally undoped GaN and having a (0001) orientation, on the first c-plane GaN wafer obtained in the first step by HVPE and slicing a second c-plane GaN wafer from the second thick GaN film; and (iii) a third step of growing a GaN film having a thickness of more than 50 μm and a (0001) orientation on the second c-plane GaN wafer obtained in the second step by HVPE to obtain a stacked structure, and the GaN film grown in the third step has a total concentration of compensating impurities of 1×10 17 atoms / cm 3 A method for producing a GaN substrate wafer, comprising the steps of: providing a portion as described above;
[26] The method for producing a GaN substrate wafer according to
[25] above, wherein the GaN film has a thickness of 300 μm or less.
[27] The method for producing a GaN substrate wafer according to
[25] or
[26] above, wherein the GaN substrate wafer satisfies any one of the conditions selected from the following (1) to (3): (1) Having a diameter of 50 mm or more and 55 mm or less and a thickness of 250 μm or more and 450 μm or less. (2) Having a diameter of 100 mm or more and 105 mm or less and a thickness of 350 μm or more and 750 μm or less. (3) Having a diameter of 150 mm or more and 155 mm or less and a thickness of 450 μm or more and 800 μm or less.
[28] The GaN film has a region length in the c-axis direction of 20 μm or more, and a total concentration of compensation impurities in the region is 1×10 17 atoms / cm 3 The method for producing a GaN substrate wafer having a specifically doped region according to any one of the above
[25] to
[27] .
[29] The total concentration of compensating impurities in the specific doped region is 1×10 18 atoms / cm 3 The above is a method for producing a GaN substrate wafer according to
[28] .
[30] The method for producing a GaN substrate wafer according to
[28] or
[29] above, wherein in the specific doped region, a total concentration of compensating impurities is at least twice as high as a total concentration of donor impurities.
[31] The method for producing a GaN substrate wafer according to any one of
[28] to
[30] above, wherein the variation in the total concentration of compensation impurities in the specific doped region along the c-axis direction is within a range of ±25% from the median value.
[32] The method for producing a GaN substrate wafer according to any one of
[28] to
[31] above, wherein the region length is 50% or more of the thickness of the GaN film.
[33] The method for producing a GaN substrate wafer according to any one of
[28] to
[32] above, wherein the length from a lower end of the specifically doped region to an interface between the GaN film and the second c-plane GaN wafer is 1 μm or more.
[34] The method for producing a GaN substrate wafer according to any one of
[28] to
[33] above, wherein the specifically doped region contains one or more elements selected from carbon and transition metal elements.
[35] The method for producing a GaN substrate wafer according to any one of
[28] to
[34] above, wherein the impurity contained in the specific doped region at the highest concentration is Fe, Mn or C.
[36] The total concentration of compensating impurities in the GaN film is 5×10 19 atoms / cm 3 A method for producing a GaN substrate wafer according to any one of the above
[24] to
[35] , which is as follows:
[37] The method for producing a GaN substrate wafer according to any one of
[24] to
[36] above, further comprising, after the third step, a thinning step of thinning the laminated structure.
[38] The method for producing a GaN substrate wafer according to
[37] above, wherein a difference in thickness of the GaN film before and after the thinning step is 50 μm or more.
[39] The method for producing a GaN substrate wafer according to
[37] or
[38] above, wherein a difference in thickness of the GaN film before and after the thinning step is 200 μm or less.
[40] The method for producing a GaN substrate wafer according to any one of
[37] to
[39] above, wherein an offcut orientation of the GaN substrate wafer is different from an offcut orientation of the second c-plane GaN wafer.
[41] The method for producing a GaN substrate wafer according to any one of
[24] to
[40] above, comprising a planarization step of planarizing a Ga-polarity main surface of the second c-plane GaN wafer sliced from the second GaN film in the second step, and a roughening step of roughening the main surface by etching, prior to growing the GaN film in the third step. Effect of the Invention
[0007] A GaN substrate wafer with improved productivity and a method for manufacturing the same, which can be preferably used for manufacturing nitride semiconductor devices having a lateral device structure, are provided. [Brief description of the drawings]
[0008] [Figure 1] FIG. 1 is a perspective view showing a GaN substrate wafer according to an embodiment. [Diagram 2] FIG. 2 is a cross-sectional view showing a GaN substrate wafer according to the embodiment. [Diagram 3] FIG. 3 is a cross-sectional view showing a GaN substrate wafer according to an embodiment. [Figure 4] 4A to 4C are cross-sectional views illustrating steps of a manufacturing process for a nitride semiconductor device using a GaN substrate wafer according to the embodiment. [Diagram 5] 5A to 5C are cross-sectional views illustrating the steps of a GaN substrate wafer manufacturing method according to an embodiment. [Figure 6] 6A to 6C are cross-sectional views illustrating the steps of a GaN substrate wafer manufacturing method according to an embodiment. [Figure 7] 7A to 7C are cross-sectional views illustrating the steps of a GaN substrate wafer manufacturing method according to an embodiment. [Figure 8] FIG. 8 is a schematic diagram showing the basic configuration of an HVPE apparatus. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] The following is a detailed description of the embodiments of the present invention. The following description of the components is an example (representative example) of the embodiments of the present invention, and the present invention is not limited to these contents as long as it does not exceed the gist of the present invention. In this specification, when expressed as "X to Y" (X and Y are any numbers), unless otherwise specified, it includes the meaning of "X or more and Y or less", as well as "preferably greater than X" and "preferably smaller than Y". In addition, in this specification, the term "independently" used when describing two or more objects together means that the two or more objects may be the same or different.
[0010] 1. GaN substrate wafer One embodiment of the present invention relates to a GaN substrate wafer. The GaN substrate wafer according to the embodiment is a (0001) oriented GaN substrate wafer, and has a first region provided on the N-polarity side across a regrowth interface, and a second region having a minimum thickness provided on the Ga-polarity side. The minimum thickness of the second region is 20 μm or more. In addition, in at least a part of the second region, the total concentration of compensation impurities is 1×10 17 atoms / cm 3 That's all. Furthermore, in the above-mentioned GaN substrate wafer, it is preferable that, with regard to the impurity concentration in the first region, one or more conditions selected from the following (a) to (c) are satisfied. (a) Si (silicon) concentration is 5×10 16 atoms / cm 3 That's it; (b) O (oxygen) concentration is 3×10 16 atoms / cm 3 Below is; (c) H (hydrogen) concentration is 1×10 17 atoms / cm 3 The following is the result. In this specification, the term "impurities" refers to components other than Ga and N contained in the GaN substrate. A (0001) oriented GaN wafer is a GaN wafer having a main surface (large area surface) parallel or approximately parallel to the (0001) crystal plane, that is, the c-plane, and is also called a c-plane GaN wafer.
[0011] An example of a GaN substrate wafer according to an embodiment is shown in Figures 1 and 2. Figure 1 is a perspective view, and Figure 2 is a cross-sectional view. 1 and 2 is a free-standing substrate wafer made only of GaN crystals, one of its two main surfaces being an N-polar surface 101 and the other being a Ga-polar surface 102. The N-polar surface 101 and the Ga-polar surface 102 are parallel to each other. The GaN substrate wafer 100 has a (0001) orientation, and the inclination of the Ga polar surface 102 with respect to the (0001) crystal plane is 10 degrees or less, preferably 5 degrees or less, and more preferably 2.5 degrees or less. The inclination can be 0.2 degrees or more and less than 1 degree, 1 degree or more and 2.5 degrees or less, etc.
[0012] The diameter of the GaN substrate wafer 100 is usually 45 mm or more, and may be 95 mm or more, or 145 mm or more, and is typically 50 to 55 mm (about 2 inches), 100 to 105 mm (about 4 inches), 150 to 155 mm (about 6 inches), etc. The preferred range of thickness of the GaN substrate wafer 100 varies depending on the diameter. When the diameter is about 2 inches, the thickness is preferably 250 μm or more, more preferably 300 μm or more, and preferably 450 μm or less, more preferably 400 μm or less. When the diameter is about 4 inches, the thickness is preferably 350 μm or more, more preferably 400 μm or more, and preferably 750 μm or less, more preferably 650 μm or less. When the diameter is about 6 inches, the thickness is preferably 450 μm or more, more preferably 550 μm or more, and preferably 800 μm or less, more preferably 700 μm or less.
[0013] As described above, the GaN substrate wafer 100 is usually disk-shaped, but in modified examples, the shape of the main surface may be a square, rectangle, hexagon, octagon, ellipse, or an irregular shape. In such modified examples, the above-mentioned diameter can be read as "the shortest length of a straight line passing through the center of gravity on the main surface."
[0014] The N-polar surface 101 of the GaN substrate wafer 100 is the "backside" surface and may be mirror-finished or may be roughened or matte-finished. The Ga polar surface 102 of the GaN substrate wafer 100 is the “front surface”, and when the GaN substrate wafer 100 is used for manufacturing a nitride semiconductor device, a nitride semiconductor layer is typically epitaxially grown on the Ga polar surface 102 . The Ga polar surface 102 may be an as-grown surface, but is usually planarized by processing. The processing performed to planarize the Ga polar surface 102 and make it a flat surface may include one or more selected from polishing and CMP (Chemical Mechanical Polishing). In addition to these processing, etching may be performed for the purpose of removing a damaged layer. The roughness of the flat surface is not limited, but for example, the root mean square (RMS) roughness of the Ga polar surface 102 measured by an atomic force microscope (AFM) is preferably less than 5 nm, more preferably less than 2 nm, and even more preferably less than 1 nm in a measurement range of 2 μm×2 μm, and may be less than 0.5 nm. The Ga polar surface 102 may be a surface formed by cutting, but is preferably a surface that has been subjected to only planarization such as polishing, CMP, or etching without cutting.
[0015] GaN substrate wafer 100 has a regrowth interface 103 between its two main surfaces, with a first region 110 on the N-polarity side and a second region 120 on the Ga-polarity side across the regrowth interface 103. The "regrowth interface" refers to a boundary surface that occurs when GaN crystals grow on any substrate, and its existence can be confirmed, for example, by observing a cross section of the GaN substrate wafer with a scanning electron microscope, cathodoluminescence observation, or fluorescence microscope. The regrowth interface 103 is preferably parallel to the Ga polar surface 102. When the regrowth interface 103 is inclined from the Ga polar surface 102, the thickness of the second region 120 is usually minimum at one end in the inclination direction and maximum at the other end. It is preferable that the difference between the thickness of the second region 120 at the one end and the thickness of the second region 120 at the other end does not exceed 200 μm. In the process of manufacturing a nitride semiconductor device using the GaN substrate wafer 100, it is assumed that the first region 110 will be removed eventually. In other words, it is assumed that a nitride semiconductor device chip manufactured using the GaN substrate wafer 100 will not include a portion derived from the first region 110. In such a usage mode, there are no particular restrictions on the electrical properties of the GaN crystal that constitutes the first region 110.
[0016] The first region 110 is usually made of a GaN crystal grown by HVPE, and therefore satisfies one or more of the following conditions (a) to (c) regarding the impurity concentration. In this specification, HVPE stands for Hydride Vapor Phase Epitaxy. (a) Si concentration is 5×10 16 atoms / cm 3 End (b) O concentration is 3 × 10 16 atoms / cm 3 below (c) H concentration is 1×10 17 atoms / cm3 below In GaN crystals grown by HVPE, the total concentration of compensating impurities is usually lower than the total concentration of donor impurities, unless the crystal is intentionally doped with compensating impurities, which means that the target element is added as a raw material during the GaN crystal growth process. In the first region, the total concentration of the compensating impurities is 1×10 17 atoms / cm 3 It is preferable that it is less than 1000 .mu.m. The GaN crystal forming the first region 110 is preferably a GaN crystal that is not intentionally doped.
[0017] Second region 120 is grown by HVPE on first region 110. Regrowth interface 103 exists between first region 110 and second region 120 because the steps of growing first region 110 and second region 120 are not continuous. The minimum thickness of the second region 120 is 20 μm or more. The reason is that, in the process of manufacturing a nitride semiconductor device chip using the GaN substrate wafer 100, after the first region 110 is removed from the substrate wafer 100, the remaining second region 120 can play a role as a substrate that supports the structure of the semiconductor device chip. The minimum thickness means the thickness at the point where the thickness is smallest. The minimum thickness of the second region 120 may be greater than or equal to 50 μm, such as greater than or equal to 75 μm, such as greater than or equal to 100 μm, such as greater than or equal to 150 μm. The minimum thickness of the second region 120 is preferably 350 μm or less, more preferably 300 μm or less, and may be 250 μm or less, such as 200 μm or less. When the Ga-polar surface 102 and the regrowth interface 103 are parallel and the thickness of the second region 120 is uniform, the thickness of the second region is considered to be at its minimum thickness everywhere.
[0018] Preferably, the region of the second region 120 that includes at least the Ga polarity side main surface, specifically, the region within a specific length L from the Ga polarity surface 102 of the GaN substrate wafer 100, is defined as the primarily doped region 120a. The second region 120 has a total concentration of compensation impurities of 1×10 17 atoms / cm 3 The doping is carried out so that the above value is satisfied. The total concentration of compensating impurities is the sum of the concentrations of all types of compensating impurities. In GaN crystals grown by HVPE, the total concentration of compensating impurities is 1×10 unless intentionally doped. 17 atoms / cm 3 Therefore, it is not possible to intentionally dope the total concentration of compensating impurities to 1×10 17 atoms / cm 3 It can be more than that. In this specification, the compensating impurity refers to an impurity that has the function of compensating for n-type carriers in GaN crystals. Well-known compensating impurities are C (carbon) and transition metal elements. Representative transition metal elements are Fe (iron) and Mn (manganese), and others include Co (cobalt), Cr (chromium), V (vanadium), Ni (nickel), and Cu (copper).
[0019] The total concentration of compensating impurities in the primary doped region 120a is 1×10 17 atoms / cm 3 More than 2×10 17 atoms / cm 3 Less than 2×10 17 atoms / cm 3 5×10 or more 17 atoms / cm 3 Less than 5×10 17 atoms / cm 3 More than 1×10 18 atoms / cm 3 Less than 1×10 18 atoms / cm 3 More than 2×10 18 atoms / cm 3 Less than 2×10 18atoms / cm 3 5×10 or more 18 atoms / cm 3 Less than 5×10 18 atoms / cm 3 More than 1×10 19 atoms / cm 3 Less than 1×10 19 atoms / cm 3 More than 2×10 19 atoms / cm 3 Less than 2×10 19 atoms / cm 3 5×10 or more 19 atoms / cm 3 It can be less than, etc. In the primarily doped region 120a, the total concentration of the compensating impurities is preferably at least two times, more preferably at least five times, and even more preferably at least 10 times, and may be at least 50 times, the total concentration of the donor impurities. In addition, the compensating impurity contained in the primarily doped region 120a at the highest concentration is preferably Fe, Mn, or C. In a preferred embodiment, the GaN crystal forming the primary doped region 120a is semi-insulating, i.e., its room temperature resistivity is 1×10 5 The concentration of the compensating impurity added to the primary doped region 120a is set to be Ω·cm or more.
[0020] Elements that can act as donor impurities in GaN crystals include group 14 elements such as Si, Ge (germanium), and Sn (tin), and group 16 elements such as O, S (sulfur), Se (selenium), and Te (tellurium). Of these, Si and O are present in GaN crystals grown by HVPE at concentrations of 10 16 atoms / cm 3 In contrast, group 14 elements other than Si and group 16 elements other than O can be present in HVPE grown GaN crystals at concentrations of 10 or more unless intentionally added. 15 atoms / cm 3 It is never found in concentrations above 100,000.
[0021] The specific length L is at least 1 μm or more, preferably 20 μm or more, more preferably 25 μm or more, and further preferably 50 μm or more, and can be arbitrarily determined within a range not exceeding the minimum thickness of the second region 120 . In the primarily doped region 120a, it is desirable that there is small variation in resistivity along the c-axis direction, which is the thickness direction of the GaN substrate wafer 100. Therefore, the variation in the total concentration of compensation impurities along the c-axis direction in the primarily doped region 120a is preferably within ±25% from the median, more preferably within ±20%, even more preferably within ±15%, and even more preferably within ±10%. In a preferred embodiment, in the process of manufacturing a nitride semiconductor device chip using the GaN substrate wafer 100, even when the second region 120 is partially removed in addition to the first region 110 from the GaN substrate wafer 100 to expose the primarily doped region 120a, the specific length L is set to a value greater than 50 μm so that the GaN substrate consisting only of the remaining primarily doped region 120a can support the structure of the semiconductor device chip. In this preferred embodiment, the specific length L may be 75 μm or more, 100 μm or more, even 150 μm or more, or even 200 μm or more. In this preferred embodiment, the specific length L is preferably 50% or more of the minimum thickness of the second region 120, more preferably 75% or more, and even more preferably 90% or more. In addition, the length from the lower end (the end on the N-polar surface 101 side) of the specific length L to the regrowth interface is preferably 1 μm or more, more preferably 5 μm or more, or 10 μm or more, and the length from the lower end to the interface is preferably 50 μm or less, more preferably 30 μm or less.
[0022] The total concentration of compensating impurities in the second region 120, including the main doped region 120a, is set to 5×10 19 atoms / cm 3 The following is further 2×10 19 atoms / cm 3 Below, and further 1×10 19 atoms / cm 3 It can be as follows. At the bottom of the second region 120, i.e., the portion adjacent to the first region 110, the concentration of the compensating impurity of the same type as the compensating impurity intentionally added to the main doped region 120a may increase continuously or stepwise with increasing distance from the first region 110.
[0023] Since the second region 120 is usually grown by HVPE, its impurity concentration satisfies one or more conditions selected from the following (a') to (c'). (a') Si concentration is 5×10 16 atoms / cm 3 End (b') O concentration is 3×10 16 atoms / cm 3 below (c') H concentration is 1×10 17 atoms / cm 3 below
[0024] 3, the regrowth interface 103 may be rough. For example, when the surface of the first region 110 is roughened by etching before the second region 120 is grown, the regrowth interface 103 may be rough. When the direction perpendicular to the regrowth interface 103 from the first region 110 toward the second region 120 is defined as the height direction and the height difference between the highest point and the lowest point at the regrowth interface is defined as the roughness r of the regrowth interface, the roughness r may be, for example, 0.3 μm or more and 12 μm or less. 1 to 3, the edges of the GaN substrate wafer 100 may be chamfered. In addition, the GaN substrate wafer 100 may be provided with various markings as necessary, such as an orientation flat or a notch that indicates the crystal orientation, and an index flat that makes it easy to distinguish between the front and back surfaces.
[0025] The GaN substrate wafer 100 can be preferably used for manufacturing a nitride semiconductor device with a lateral device structure such as a GaN-HEMT. A nitride semiconductor device is a semiconductor device in which the main part of the device structure is formed of a nitride semiconductor. Nitride semiconductors are also called nitride-based III-V group compound semiconductors, group III nitride-based compound semiconductors, GaN-based semiconductors, etc., and include GaN as well as compounds in which part or all of the gallium in GaN is replaced with other group 13 elements of the periodic table (B, Al, In, etc.). The lateral device structure can also be adopted in electronic devices other than high electron mobility transistors (HEMTs), such as bipolar transistors, and in light-emitting devices, such as light-emitting diodes (LEDs) and laser diodes (LDs).
[0026] When a GaN-HEMT is manufactured using a GaN substrate wafer 100, the GaN substrate wafer 100 is prepared as shown in FIG. 4(a), and then an epitaxial film 200 including at least an undoped GaN channel layer 210 and an undoped AlGaN carrier supply layer 220 is grown on the Ga polarity surface 102 by, for example, metal-organic vapor phase epitaxy (MOVPE) as shown in FIG. 4(b), thereby forming an epitaxial wafer. After semiconductor processes that may include etching, ion implantation, electrode formation, protective film formation, and the like are performed, the epitaxial wafer is divided into GaN-HEMT chips. However, in order to thin the epitaxial wafer before division, at least a portion of the first region 110 of the GaN substrate wafer 100 is usually removed by a method such as grinding or etching, as shown in FIG. 4(c).
[0027] This thinning process can be performed so that a ring-shaped thick portion remains on the outer periphery of the epitaxial wafer, that is, the first region 110 of the GaN substrate wafer 100 can be removed only in the portion excluding the outer periphery of the epitaxial wafer. 4(c), the second region 120 is also partially removed from the GaN substrate wafer 100 so that the primary doped region 120a is exposed on the N-polar surface side of the thinned epitaxial wafer. Note that the semiconductor device using the GaN substrate wafer 100 is not limited to only nitride semiconductor devices.
[0028] 2. GaN substrate wafer manufacturing method Next, a method for producing a GaN substrate wafer according to another embodiment of the present invention will be described. The method for producing the GaN substrate wafer described below is a preferred embodiment for producing the GaN substrate wafer described above. A preferred embodiment of the GaN substrate wafer obtained by the method for producing the GaN substrate wafer described below is the GaN substrate wafer described above. The above-described GaN substrate wafer 100 according to the embodiment can be preferably manufactured by the method described below. This method is applied to the manufacture of a GaN substrate wafer having an N-polarity region and a Ga-polarity region sandwiching a regrowth interface, and preferably has an increased resistivity in at least a part of the Ga-polarity region, and includes the following steps. (ii') a second step of growing a (0001) oriented second GaN thick film on the substrate by HVPE and then slicing the second GaN thick film to obtain a second c-plane GaN wafer; (iii') a third step of growing on the second c-plane GaN wafer by HVPE a (0001) oriented GaN film greater than 50 μm in thickness, the GaN film having a region having a higher total concentration of donor impurities than the second c-plane GaN wafer.
[0029] Furthermore, it is preferable to add the first step as the steps for manufacturing the substrate in the second step, as follows. Therefore, the first step described below is optional. (i) A first GaN layer is made of intentionally undoped GaN with a (0001) orientation. A first step of growing a thick film by HVPE on a seed wafer and processing the first GaN thick film to obtain at least one first c-plane GaN wafer. (ii) a second step of growing a second thick GaN film, consisting of intentionally undoped GaN and having a (0001) orientation, on the first c-plane GaN wafer obtained in the first step by HVPE, and slicing a second c-plane GaN wafer from the second thick GaN film. (iii) a third step of growing a (0001) oriented GaN film having a thickness greater than 50 μm on the second c-plane GaN wafer obtained in the second step by HVPE to obtain a stacked structure, provided that the GaN film has a total concentration of compensating impurities of 1×10 17 atoms / cm 3 A portion that satisfies the above requirements is provided. In this specification, "on the wafer" is synonymous with "on the surface of the wafer."
[0030] The above-mentioned first to third steps will be described in more detail below. The structures and characteristics of the first region and the second region described above can be applied to the structures and characteristics of the first c-plane GaN wafer obtained in the first step and the second GaN thick film obtained in the second step, respectively. In the first step, a seed wafer 1 shown in Fig. 5(a) is prepared, and a first GaN thick film 2 made of intentionally undoped GaN with a (0001) orientation is grown thereon by HVPE as shown in Fig. 5(b). Then, as shown in Fig. 5(c), at least one first c-plane GaN wafer 3 is obtained by processing the first GaN thick film 2.
[0031] An example of the seed wafer 1 is a c-plane sapphire wafer, preferably one having a peeling layer on the main surface. For example, a GaN layer having a thickness of several hundreds of nm is grown on a c-plane sapphire wafer by MOVPE via a low-temperature buffer layer, and then a Ti (titanium) layer having a thickness of several tens of nm is formed on the GaN layer by vacuum deposition. After that, the wafer is annealed in a mixed gas of 80% H2 (hydrogen gas) and 20% NH3 (ammonia) at, for example, 1060°C for 30 minutes to form a c-plane sapphire wafer with a peeling layer. The seed wafer 1 may be a c-plane GaN wafer manufactured in a separate process.
[0032] The first GaN thick film 2 is grown to a thickness that allows at least one free-standing c-plane GaN wafer to be fabricated by processing the first GaN thick film 2. In a preferred example, the first GaN thick film 2 is grown to a thickness of several mm or more, and at least two first c-plane GaN wafers 3 are sliced therefrom. 6(a) is a cross-sectional view showing one of the first c-plane GaN wafers 3 produced in the first step. However, the first c-plane GaN wafer 3 is not limited to the one obtained in the first step. In the second step, as shown in FIG. 6(b), a second GaN thick film 4 made of intentionally undoped GaN and oriented in (0001) is grown by HVPE on the Ga polarity plane of the first c-plane GaN wafer 3, and then, as shown in FIG. 6(c), a second c-plane GaN wafer 5 is sliced from the second GaN thick film 4. The second GaN thick film 4 is grown to a thickness that allows at least one second c-plane GaN wafer 5 to be fabricated by processing the second GaN thick film 4. In a preferred example, the second GaN thick film 4 is grown to a thickness of several mm or more, and at least two second c-plane GaN wafers 5 are sliced therefrom. Since the second GaN thick film 4 has a weak n-type conductivity, it is possible to slice it using a wire electric discharge machine. The wire electric discharge machine has a higher cutting speed and is easier to handle than a free abrasive wire saw. In addition, the kerf loss when slicing a GaN crystal using a wire electric discharge machine is smaller than when using a fixed abrasive wire saw.
[0033] As shown in the cross-sectional view of FIG. 7(a), the second c-plane GaN wafer 5 has, as its major surfaces, an N-polar plane and a Ga-polar plane which are parallel to each other. When manufacturing the above-described GaN substrate wafer 100 according to the embodiment, when slicing the second c-plane GaN wafer 5 from the second GaN thick film 4 in the second step, it is preferable, but not essential, that the inclination angle (offcut angle) and inclination direction (offcut direction) of the Ga polarity plane in the second c-plane GaN wafer 5 with respect to the (0001) crystal plane be the same as the offcut angle and offcut direction that the GaN substrate wafer 100 should have. The offcut orientation that the GaN substrate wafer 100 should have varies depending on the requirements of the manufacturer of the semiconductor device that uses the GaN substrate wafer 100, but preparing second c-plane GaN wafers 5 having various offcut orientations may lead to a decrease in the production efficiency of the GaN substrate wafer 100. It should also be noted that the optimal conditions for growing the GaN film 6 on the second c-plane GaN wafer 5 by HVPE in the next third step may change depending on the offcut orientation of the second c-plane GaN wafer 5.
[0034] The initial thickness t of the second c-plane GaN wafer 5 5i may be thinner than the usual thickness of a GaN substrate wafer used in the manufacture of nitride semiconductor devices, because, unlike a GaN substrate wafer that must withstand a semiconductor process consisting of many steps, the second c-plane GaN wafer 5 only needs to be undamaged during the next third step. For example, when the diameter of the second c-plane GaN wafer 5 is about 2 inches, its initial thickness t 5i is preferably 300 μm or less, and may be 250 μm or less, or even 200 μm or less. The initial thickness t of the second c-plane GaN wafer 5 5i By reducing the distance, the number of second c-plane GaN wafers 5 that can be sliced from the second GaN thick film 4 can be increased.
[0035] In the third step, as shown in FIG. 7(b), a GaN layer having a growth thickness of t 6g A (0001) oriented GaN film 6 having a diameter of more than 50 μm is grown by HVPE to obtain a layered structure, in which a regrowth interface is formed between the second c-plane GaN wafer 5 and the GaN film 6.
[0036] Typically, the Ga polar surface of the second c-plane GaN wafer 5 is flattened by appropriate techniques such as grinding, polishing, CMP, etc. before the GaN film 6 is grown (flattening step). In one example, the flattened Ga polar surface may be roughened by etching (roughening step) before the GaN film 6 is grown. When HCl (hydrogen chloride) is used as an etching gas, the Ga polar surface of GaN can be roughened without using an etching mask. If an HCl supply line for etching is provided in the HVPE apparatus used for growing the GaN film 6, the Ga polar surface of the second c-plane GaN wafer 5 can be roughened in the reactor of the HVPE apparatus immediately before the growth of the GaN film 6.
[0037] When HCl is used as the etching gas, the preferred etching conditions are as follows: The HCl partial pressure is, for example, 0.002 to 0.05 atm. The H2 partial pressure is, for example, 0.2 to 0.8 atm. The NH3 partial pressure is, for example, 0.01 to 0.05 atm. By flowing NH3, the Ga polarity surface of GaN is roughened more uniformly. The etching temperature is, for example, 900 to 1050°C. The etching time is, for example, 1 to 60 minutes. When the roughness of the Ga polar surface of the second c-plane GaN wafer 5 after etching is defined as the height difference between the highest point and the lowest point, the roughness can be, for example, 0.3 to 12 μm. In etching using HCl, when conditions other than the etching time are fixed, the roughness of the Ga polarity surface of the second c-plane GaN wafer tends to increase with increasing etching time.
[0038] When HCl is used as the etching gas, the etching time may be determined so that the roughness of the Ga polar surface does not exceed 0.5 μm. For example, when the Ga polar surface of the second c-plane GaN wafer 5 is etched under conditions of an HCl partial pressure of 0.01-0.02 atm, an H2 partial pressure of 0.05-0.08 atm, an NH3 partial pressure of 0.01-0.03 atm, and a temperature of 970-1000°C, the roughness of the Ga polar surface can be reduced to 0.5 μm or less by setting the etching time to 5 minutes or less. In one example, the Ga polar surface of the second c-plane GaN wafer 5 may be roughened by forming an etching mask patterned by photolithography and then dry etching. A dot pattern and a net pattern are typical examples of suitable patterns for the etching mask. The dry etching may be RIE (reactive ion etching) using Cl2 (chlorine gas) or a chlorine-containing compound as an etching gas.
[0039] The GaN film 6 has a total concentration of compensation impurities of 1×10 17 atoms / cm 3 The doping is carried out so that the above-mentioned compensation impurities are particularly preferably used. In a preferred embodiment, a specially doped region 6a may be provided in the GaN film 6. The specially doped region 6a preferably has a region length in the c-axis direction of 20 μm or more, and a total concentration of compensating impurities in the region of 1×10 17 atoms / cm 3 In other words, the length of this region is the region where the total concentration of the compensation impurities is 1×10 17 atoms / cm 3 This means the thickness (height in the thickness direction) of the region that is equal to or greater than this. The length of the specifically doped region 6a in the c-axis direction can be 25 μm or more, 50 μm or more, 75 μm or more, 100 μm or more, 150 μm or more, 200 μm or more, and the like. The upper end (the end on the <0001> side) of the specifically doped region 6 a is preferably within 10 μm, more preferably within 5 μm, from the upper surface of the GaN film 6 . The length from the lower end (the end on the [000-1] side) of the specifically doped region 6a to the interface between the second c-plane GaN wafer 5 and the GaN film 6 is preferably 1 μm or more, more preferably 5 μm or more, or 10 μm or more, and the length from the lower end to the interface is preferably 50 μm or less, more preferably 30 μm or less. Furthermore, the length of the specifically doped region 6a in the c-axis direction is preferably 50% or more of the thickness of the GaN film 6, more preferably 75% or more, and even more preferably 90% or more. In the specific doped region 6a, the total concentration of compensating impurities is at least 1×10 17 atoms / cm 3 , which is 2 × 10 17 atoms / cm 3 That's it, 5 x 10 17 atoms / cm 3 That's it, 1×10 18 atoms / cm 3 That's it, 2 x 10 18 atoms / cm 3 That's it, 5 x 10 18 atoms / cm 3 The above may be possible.
[0040] In the specifically doped region 6a, the total concentration of the compensating impurities is preferably at least two times, more preferably at least five times, and even more preferably at least ten times, and may be at least 50 times, the total concentration of the donor impurities. In the specific doped region 6a, the GaN crystal is semi-insulating, i.e., its room temperature resistivity is 1×10 5 It may be Ω·cm or more. In the specially doped region 6a, it is desirable that the variation in resistivity along the c-axis direction is small. Therefore, the variation in the total concentration of the compensating impurities along the c-axis direction in the specially doped region 6a is preferably within ±25% from the median, more preferably within ±20%, even more preferably within ±15%, and even more preferably within ±10%. The total concentration of compensating impurities in the GaN film 6, including the specific doped region 6a, is set to 5×10 19 atoms / cm 3 The following is further 2×10 19 atoms / cm 3 Below, and further 1×10 19 atoms / cm 3 It can be as follows. The lowermost portion of the GaN film 6, i.e., the portion adjacent to the second c-plane GaN wafer 5, may be doped with the same type of compensating impurity as the specific doped region 6a, so that the concentration of the compensating impurity increases continuously or stepwise with increasing distance from the second c-plane GaN wafer 5.
[0041] The growth thickness t of the GaN film 6 6g is set according to the design thickness of the Ga-polarity side region of the GaN substrate wafer to be manufactured. Specifically, it may be 20 μm or more, 50 μm or more, or more than 50 μm, or even 75 μm or more, 100 μm or more, 150 μm or more, or 500 μm or less, 350 μm or less, 300 μm or less, 250 μm or less, 200 μm or less, etc. When manufacturing the above-mentioned GaN substrate wafer 100, the growth thickness t 6g may be the same as the design thickness of the second region 120 in the GaN substrate wafer, but is preferably larger than the design thickness, which allows the surface of the GaN film 6 to be flattened in the subsequent thinning process. 6g In order to ensure a processing margin for planarization, the thickness of the second region 120 is preferably 50 μm or more larger than the maximum design thickness of the second region 120, and more preferably 100 μm or more larger. A processing margin exceeding 200 μm is usually not required. In other words, it is preferable that the difference in thickness of the GaN film 6 before and after the thinning step is 200 μm or less. For example, the growth thickness t of the GaN film 6 6g is 50 μm or more larger than the designed maximum thickness of second region 120, the thickness of GaN film 6 is reduced by 50 μm or more in the subsequent thinning step. In other words, the difference in thickness of GaN film 6 before and after the thinning step is 50 μm or more.
[0042] When manufacturing the above-mentioned GaN substrate wafer 100, even if a wafer with a large diameter, for example a wafer with a diameter of 6 inches, the growth thickness t 6g It is possible to keep the thickness below 500 μm. Growth thickness t 6gSince the size of the GaN film 6 is small, the GaN film 6 can be formed in a relatively short time, and therefore it is possible to grow the GaN film 6 on many second c-plane GaN wafers 5 at once without worrying about the by-product NH4Cl (ammonium chloride) clogging the exhaust system of the HVPE apparatus. This allows the throughput in the third step to be extremely high. Furthermore, the shorter time required to form the GaN film 6 may also contribute to reducing costs associated with cleaning and maintaining the HVPE reactor. In general, the shorter the time required for a single growth step, the slower the degradation of the HVPE reactor will be, and the longer the service life will be.
[0043] After the third step, if necessary, a thinning step is performed to thin the laminated structure obtained in the third step, as shown in FIG. 7(c). In FIG. 7(c), the thickness of the second c-plane GaN wafer 5 is the initial thickness t 5i to final thickness t 5f and the thickness of the GaN film 6 is reduced to the initial thickness t 6i to final thickness t 6f However, only either the second c-plane GaN wafer 5 or the GaN film 6 may be processed in the thinning step. When manufacturing the above-described GaN substrate wafer 100 according to the embodiment, in the thinning step, the thicknesses of the second c-plane GaN wafer 5 and the GaN film 6 are reduced until they match the designed thicknesses of the first region 110 and the second region 120 in the GaN substrate wafer, respectively.
[0044] When the offcut orientation of the GaN substrate wafer 100 to be manufactured is the same as the offcut of the second c-plane GaN wafer 5, the back surface (the N-polarity surface of the stacked structure) of the second c-plane GaN wafer 5 can be used as the reference for the plane orientation during thinning processing. When the offcut orientation of the GaN substrate wafer 100 to be manufactured differs from the offcut of the second c-plane GaN wafer 5, i.e., when at least either the offcut angle or the offcut direction differs, the crystal orientation of the laminated structure is confirmed by an X-ray diffraction device before thinning processing. The processing technique used in the thinning step can be appropriately selected from grinding, lapping, CMP, dry etching, wet etching, and the like.
[0045] By using the manufacturing method described above, the GaN substrate wafers 100 according to the embodiment can be produced with a high yield. The reason is that there is no process for growing an intentionally doped thick GaN film to a thickness of 1 mm or more by HVPE, nor a process for slicing the GaN thick film thus grown. In the first and second steps, the GaN thick film may be grown by HVPE to a thickness on the order of millimeters. However, the first GaN thick film 2 and the second GaN thick film 4 grown in these steps are not intentionally doped, so that morphological abnormalities and cracks are unlikely to occur during growth, and the frequency of cracking during slicing is also low. On the other hand, the GaN film 6 grown in the third step has a thickness of 1×10 17 atoms / cm 3 Although a portion containing the compensating impurity at the above concentration is provided, the growth thickness of the GaN film 6 is 500 μm or less, so that morphology abnormalities and cracks are unlikely to occur during growth. Moreover, the GaN film 6 does not need to be sliced. That is, there is no need to perform a slice process in the thinning step described above. In particular, it is preferable that the GaN film 6 formed in the third step undergoes the thinning step without being sliced.
[0046] Furthermore, in the GaN substrate wafer obtained by the manufacturing method described above, the variation in offcut orientation within the primary surface can be extremely small. The reason is that the warp of the second GaN thick film 4, which is grown homoepitaxially without intentional doping on the first c-plane GaN wafer 3, which is not intentionally doped, can be extremely small, and therefore, in the second c-plane GaN wafer 5 sliced from the second GaN thick film 4, the variation in offcut orientation can be extremely small.
[0047] An example of an HVPE apparatus that can be used in the first to third steps included in the above-mentioned manufacturing method will be described below with reference to FIG. 8 includes a hot-wall type reactor 11, a gallium reservoir 12 and a susceptor 13 disposed within the reactor, and a first heater 14 and a second heater 15 disposed outside the reactor. The first heater 14 and the second heater 15 each surround the reactor 11 in an annular shape.
[0048] The reactor 11 is a quartz tube chamber. Inside the reactor 11, there are a first zone Z1 that is mainly heated by a first heater 14, and a second zone Z2 that is mainly heated by a second heater 15. An exhaust pipe P E is connected to the reactor end on the second zone Z2 side. The gallium reservoir 12 located in the first zone Z1 is a quartz vessel having a gas inlet and a gas outlet. The susceptor 13 disposed in the second zone Z2 is made of, for example, graphite. A mechanism for rotating the susceptor 13 can be provided as desired.
[0049] To grow GaN in the HVPE apparatus 10, a seed is placed on the susceptor 13, and the inside of the reactor 11 is heated by the first heater 14 and the second heater 15. At the same time, NH3 (ammonia) diluted with a carrier gas is supplied to the second zone Z2 through the ammonia inlet pipe P1, and HCl (hydrogen chloride) diluted with a carrier gas is supplied to the gallium reservoir 12 through the hydrogen chloride inlet pipe P2. This HCl reacts with the metallic gallium in the gallium reservoir 12, and the resulting GaCl (gallium chloride) is transported to the second zone Z2 through the gallium chloride inlet pipe P3.
[0050] In the second zone Z2, NH3 and GaCl react, and the resulting GaN crystallizes on a seed placed on a susceptor 13. When the growing GaN is to be intentionally doped, a doping gas diluted with a carrier gas is introduced into the second zone Z2 in the reactor 11 through a dopant introduction pipe P4. The portions of the ammonia introduction pipe P1, the hydrogen chloride introduction pipe P2, the gallium chloride introduction pipe P3 and the dopant introduction pipe P4 that are disposed within the reactor 11 are made of quartz. As a carrier gas for diluting NH3, HCl and the doping gas, H2 (hydrogen gas), N2 (nitrogen gas) or a mixed gas of H2 and N2 is preferably used.
[0051] The preferred conditions for growing GaN using the HVPE apparatus 10 are as follows. The temperature of the gallium reservoir is, for example, 500 to 1000°C, preferably 700°C or higher, and preferably 900°C or lower. The susceptor temperature is, for example, 900 to 1100° C., preferably 930° C. or higher, more preferably 950° C. or higher, and preferably 1050° C. or lower, more preferably 1020° C. or lower.
[0052] The V / III ratio, which is the ratio of the NH3 partial pressure to the GaCl partial pressure in the reactor, is, for example, 1 to 20, preferably 2 or more, more preferably 3 or more, and is preferably 10 or less. If the V / III ratio is too large or too small, the morphology of the growth surface of GaN deteriorates, which can cause a decrease in crystal quality. The incorporation efficiency of certain impurities into GaN crystals strongly depends on the crystal orientation of the growth surface. The uniformity of the concentration of such impurities decreases inside GaN crystals grown under conditions with poor growth surface morphology. This is because the growth surface with poor morphology has facets with various orientations. A typical example of an impurity whose incorporation efficiency into GaN crystals differs significantly depending on the crystal orientation of the growth surface is O (oxygen). Since O is a donor impurity, a decrease in the uniformity of its concentration leads to a decrease in the uniformity of the resistivity.
[0053] In addition, using too low a V / III ratio increases the concentration of nitrogen vacancies in the growing GaN crystal. Although the effect of nitrogen vacancies on GaN crystals, GaN substrates using such crystals, or nitride semiconductor devices formed on such GaN substrates is not yet clear, the concentration of nitrogen vacancies should be as low as possible because they are point defects. The growth rate of GaN is preferably 40 to 200 μm / h, and can be controlled by using the product of the NH3 partial pressure and the GaCl partial pressure in the reactor as a parameter. An excessively high growth rate deteriorates the surface morphology of the grown GaN. When doping the GaN film 6 in the third step described above, in order to prevent deterioration of the morphology of the growth surface, it is preferable to gradually increase the supply rate of the doping gas to a predetermined value over a period of several minutes to several tens of minutes from the start of supply. For the same reason, it is preferable to start supplying the doping gas when the GaN film 6 has grown to at least several μm.
[0054] Although there is no particular limitation on the method for doping the GaN film 6 with compensating impurities, a method of introducing a doping gas into the HVPE apparatus is usually adopted. The doping gas for C doping can be a hydrocarbon gas such as CH4 (methane). For example, vaporized iron chloride can be used as the doping gas for Fe doping. Iron chloride vapor can be generated by contacting HCl with metallic iron heated under a carrier gas flow, or by reacting ferrocene (bis(cyclopentadienyl)iron) vaporized by heating under a carrier gas flow with HCl in a dopant introduction tube. Here, ferrocene may be replaced with other organic compounds containing iron. The doping gas for Mn doping can be, for example, metallic Mn placed in an inlet tube, which is heated and used with a flow of a carrier gas or the like. When other transition metal elements are added to GaN, the vapor of the transition metal element or the vapor of the chloride of the transition metal element can be used as the doping gas.
[0055] GaN grown using the HVPE apparatus 10 may contain O and Si at concentrations detectable by SIMS (secondary ion mass spectrometry) even when not intentionally doped. The Si source is the quartz (SiO2) used in the reactor and the piping within the reactor, and the O source is either or both of the quartz and moisture remaining or penetrating into the reactor. The components arranged in the reactor 11, including those not shown in FIG. 8, are made of quartz and carbon, as well as silicon carbide (SiC), silicon nitride (SiN x (silicon nitride), BN (boron nitride), alumina, W (tungsten), Mo (molybdenum), etc. can be used. In this way, the concentration of impurity elements other than Si, O, and H in GaN grown using the HVPE apparatus 10 is independently 5×10 15 atoms / cm 3 It can be the following: EXAMPLES
[0056] The present invention will be described in more detail below with reference to examples. However, the present invention is not limited to these examples, and various applications are possible within the scope of the technical concept of the present invention.
[0057] [Example] <Creating the first c-plane GaN wafer (first step)> First, a GaN seed was placed on the susceptor of the HVPE apparatus. The GaN seed was a GaN template substrate on sapphire fabricated by MOCVD (metal organic chemical vapor deposition), with the c-plane side serving as the growth surface.
[0058] <Creating a second c-plane GaN wafer (second process)> Next, N2, H2 and NH3 were supplied into the reactor so that their partial pressures were 0.67 atm, 0.31 atm and 0.02 atm, respectively, while the inside of the reactor was heated by a heater installed outside the reactor. After the susceptor temperature reached 1000 °C, the susceptor temperature was kept constant and GaN was grown. The temperature of the gallium reservoir was set at 900 °C. The carrier gas supplied into the reactor during growth was 69 mol% H2 and the rest was N2. GaCl and NH3 were supplied into the reactor so that their partial pressures became 7.9×10 -3 atm and 0.024 atm, respectively, and a second GaN thick film containing no donor impurities was grown to a thickness of about 2.5 mm. The growth rate of the second GaN thick film calculated from the thickness and the growth time was about 40 μm / h. Next, after slicing this GaN thick film parallel to the c-plane to obtain a wafer, the Ga-polar surface of the wafer was subjected to planarization by grinding followed by CMP finishing. The slice damage on the N-polar surface side of the wafer was removed by etching. Further, by cutting the wafer, a second c-plane GaN wafer with a thickness of 400 μm and containing no donor impurities was fabricated. The dislocation density of the obtained wafer was about 2×10 6 ~4×10 6 cm -2 It was. Note that by increasing the growth time to increase the thickness of the second GaN thick film, two or more second c-plane GaN wafers can be obtained.
[0059] <Fabrication of GaN Substrate (Third Step)> Using the second c-plane GaN wafer as a seed, the c-plane side was set as the growth surface on the susceptor of the HVPE apparatus. Next, while introducing N2 and NH3 into the reactor so that their partial pressures became 0.84 atm and 0.16 atm, respectively, the inside of the reactor was heated by a heater installed outside the reactor. After the temperature of the gallium reservoir reached 900 °C and the susceptor temperature reached 1030 °C, the susceptor temperature was kept constant, and the growth of GaN crystals was started by supplying GaCl and NH3 so that their partial pressures became 0.013 atm and 0.16 atm, respectively. The carrier gas supplied during growth was only N2. Fe doping was carried out by introducing HCl at 9.4×10 one minute after the start of growth.-4 The experiment started by flowing metallic Fe at 1 atm into the dopant introduction tube. A GaN film doped with Fe as a donor impurity was grown to a thickness of about 0.4 mm. The growth rate of the Fe-doped GaN crystal layer was 1.6 μm / min. The entire surface of the GaN film was observed with a differential interference microscope, and it was confirmed that no surface defects such as pits or cracks were present.
[0060] If the GaN film is grown to about 0.8 mm under the same growth conditions as above, pits may occur on the crystal surface due to the influence of irregular falling objects caused by deterioration of the equipment components. The crystal surface that forms the pits incorporates donor impurities such as oxygen and silicon, which exhibit electrical conductivity, at high concentrations, which may cause problems with the occurrence of locations with different resistivities on the crystal surface. In addition, doping with a high concentration of compensating impurities tends to generate stress in the GaN film, which becomes more pronounced as the growth thickness increases. The stress accumulated in the GaN film may cause defects such as dislocations and cracks. In this example, it is believed that the growth thickness of the GaN film (Fe-doped GaN crystal layer) was limited to about 0.4 mm, which was successful. When the growth thickness is increased, the above-mentioned defects such as dislocations and cracks can be suppressed by reducing the doping concentration of the compensating impurities, improving the equipment, improving the manufacturing conditions, etc.
[0061] The surface of the GaN film grown to a thickness of approximately 0.4 mm was not sliced, but was finished by grinding and polishing the front surface (the GaN film side) and the back surface (the second c-plane GaN wafer side), respectively, to produce an Fe-doped GaN substrate wafer with a total thickness of 400 μm and a diameter of approximately 50 mm. The obtained GaN substrate wafer has a regrowth interface and is a two-layer substrate having a first region (corresponding to a second c-plane GaN wafer) having a thickness of 100 μm on the N-polarity side and a second region (corresponding to a GaN film) having a thickness of 300 μm on the Ga-polarity side.
[0062] The impurity concentration of the fabricated Fe-doped GaN substrate wafer was measured by SIMS, and it was found that Fe was 6.4×10 18 atoms / cm3 , Si is 1.9 × 10 16 atoms / cm 3 , O is 2.0 x 10 16 atoms / cm 3 , C is 7.1 × 10 15 atoms / cm 3 It was. Five locations were selected from the surface of the Fe-doped GaN substrate, and the dislocation density at each location was calculated from the number of dark spots observed in a 100 μm × 100 μm square area by cathodoluminescence. The dislocation density was found to be approximately 2 × 10 6 ~3×10 6 cm -2 This was equivalent to the dislocation density of the single-crystal GaN (0001) substrate used as the seed.
[0063] Resistivity evaluation by the double ring method The resistivity of the fabricated Fe-doped GaN substrate was measured by the double ring method. The room temperature resistivity was found to be 7×10 11 It was Ωcm.
[0064] Although the present invention has been described above with reference to specific embodiments, each embodiment is presented as an example and does not limit the scope of the present invention. Each embodiment described in this specification can be modified in various ways without departing from the spirit of the invention, and can be combined with features described in other embodiments within the scope of feasibility. [Explanation of symbols]
[0065] 1 Seed wafer 2 First GaN thick film 3. First c-plane GaN wafer 4 Second GaN thick film 5 Second c-plane GaN wafer 6 GaN film 6a Specific doped region 10 HVPE Equipment 11. Reactor 12 Gallium reservoir 13 Susceptor 14 First Heater 15 Second Heater 100 GaN substrate wafer 101 N polar plane 102 Ga polar surface 103 Regrowth interface 110 First area 120 Second area 120a Main doped region 200 Epitaxial film 210 Undoped GaN channel layer 220 Undoped AlGaN carrier supply layer
Claims
1. A (0001) oriented GaN substrate wafer, a first region on the N-polarity side of a regrowth interface and a second region having a minimum thickness on the Ga-polarity side; The second region has a minimum thickness of 20 μm or more; The total concentration of the compensating impurities in at least a portion of the second region is 1×10 17 atoms / cm 3 That's all. The first region satisfies one or more conditions selected from the following (a) to (c): (a) The Si concentration is 5×10 16 atoms / cm 3 or more. (b) The O concentration is 3×10 16 atoms / cm 3 or less. (c) The H concentration is 1×10 17 atoms / cm 3 or less.
2. A (0001) oriented GaN substrate wafer, a first region on the N-polarity side of a regrowth interface and a second region having a minimum thickness on the Ga-polarity side; The second region has a minimum thickness of 20 μm or more; a total concentration of compensation impurities in at least a portion of the second region is 1×10 17 atoms / cm 3 or more; A GaN substrate wafer, wherein in the first region, a total concentration of compensating impurities is lower than a total concentration of donor impurities.
3. A (0001) oriented GaN substrate wafer, comprising: a first region on the N-polarity side of a regrowth interface and a second region having a minimum thickness on the Ga-polarity side; The second region has a minimum thickness of 20 μm or more; a total concentration of compensation impurities in at least a portion of the second region is 1×10 17 atoms / cm 3 or more; In the first region, the concentrations of impurity elements other than Si, O, and H are independently 5×10 A GaN substrate wafer having a density of 15 atoms / cm 3 or less.
4. A (0001) oriented GaN substrate wafer, comprising: a first region on the N-polarity side of a regrowth interface and a second region having a minimum thickness on the Ga-polarity side; The second region has a minimum thickness of 20 μm or more; a total concentration of compensation impurities in at least a portion of the second region is 1×10 17 atoms / cm 3 or more; The second region has a main doped region including at least a Ga-polar main surface, A GaN substrate wafer, wherein in said primarily doped region, the total concentration of compensating impurities is at least twice the total concentration of donor impurities.
5. A (0001) oriented GaN substrate wafer, comprising: a first region on the N-polarity side of a regrowth interface and a second region having a minimum thickness on the Ga-polarity side; The second region has a minimum thickness of 20 μm or more; a total concentration of compensation impurities in at least a portion of the second region is 1×10 17 atoms / cm 3 or more; The second region has a main doped region including at least a Ga-polar main surface, The GaN substrate wafer, wherein the primarily doped region is a region within a specific length from a main surface on the GaN polarity side, and the specific length is 20 μm or more.
6. A (0001) oriented GaN substrate wafer, comprising: a first region on the N-polarity side of a regrowth interface and a second region having a minimum thickness on the Ga-polarity side; The second region has a minimum thickness of 20 μm or more; a total concentration of compensation impurities in at least a portion of the second region is 1×10 17 atoms / cm 3 or more; The second region has a main doped region including at least a Ga-polar main surface, A GaN substrate wafer, wherein the variation of the total concentration of compensating impurities along the c-axis direction in the primarily doped region is within a range of ±25% from a median value.
7. A (0001) oriented GaN substrate wafer, comprising: a first region on the N-polarity side of a regrowth interface and a second region having a minimum thickness on the Ga-polarity side; The second region has a minimum thickness of 20 μm or more; a total concentration of compensation impurities in at least a portion of the second region is 1×10 17 atoms / cm 3 or more; The second region has a main doped region including at least a Ga-polar main surface, A GaN substrate wafer, wherein the primarily doped region is a region within a specific length from a main surface on a GaN polarity side, and the specific length is greater than 50 μm.
8. A (0001) oriented GaN substrate wafer, comprising: a first region on the N-polarity side of a regrowth interface and a second region having a minimum thickness on the Ga-polarity side; The second region has a minimum thickness of 20 μm or more; a total concentration of compensation impurities in at least a portion of the second region is 1×10 17 atoms / cm 3 or more; The second region has a main doped region including at least a Ga-polar main surface, The main doped region is a region within a specific length from a main surface on the GaN polarity side, and the specific length is the GaN substrate wafer being at least 50% of the minimum thickness of the second region.
9. A (0001) oriented GaN substrate wafer, comprising: a first region on the N-polarity side of a regrowth interface and a second region having a minimum thickness on the Ga-polarity side; The second region has a minimum thickness of 20 μm or more; a total concentration of compensation impurities in at least a portion of the second region is 1×10 17 atoms / cm 3 or more; A GaN substrate wafer, wherein the second region has a minimum thickness of 300 μm or less.
10. A (0001) oriented GaN substrate wafer, comprising: a first region on the N-polarity side of a regrowth interface and a second region having a minimum thickness on the Ga-polarity side; The second region has a minimum thickness of 20 μm or more; a total concentration of compensation impurities in at least a portion of the second region is 1×10 17 atoms / cm 3 or more; A GaN substrate wafer, the Ga-polar main surface of which is flat, and the regrowth interface is inclined with respect to the Ga-polar main surface.
11. 11. The GaN substrate wafer according to claim 2, wherein the first region satisfies one or more conditions selected from the following (a) to (c): (a) Si concentration is 5×10 16 atoms / cm 3 That's all. (b) O concentration is 3×10 16 atoms / cm 3 The following is the result. (c) H concentration is 1×10 17 atoms / cm 3 The following is the result.
12. 11. The GaN substrate wafer according to claim 1, wherein in the first region, a total concentration of compensating impurities is lower than a total concentration of donor impurities.
13. In the first region, the total concentration of the compensating impurities is 1×10 17 atoms / cm 3 The GaN substrate wafer according to any one of claims 1 to 12, wherein the thickness of the GaN substrate wafer is less than 100 nm.
14. In the first region, the concentrations of impurity elements other than Si, O, and H are independently 5×10 15 atoms / cm 3 11. The GaN substrate wafer according to claim 1, 2, or 4 to 10, wherein:
15. 15. The GaN substrate wafer according to claim 1, which satisfies any one of the following conditions (1) to (3): (1) Having a diameter of 50 mm or more and 55 mm or less and a thickness of 250 μm or more and 450 μm or less. (2) Having a diameter of 100 mm or more and 105 mm or less and a thickness of 350 μm or more and 750 μm or less. (3) Having a diameter of 150 mm or more and 155 mm or less and a thickness of 450 μm or more and 800 μm or less.
16. A GaN substrate wafer as described in any one of claims 1 to 3, 9 and 10, wherein the second region has a primary doped region including at least a Ga-polar primary surface.
17. The total concentration of compensating impurities in the primary doped region is 1×10 17 atoms / cm 3 The GaN substrate wafer according to any one of claims 4 to 8 and 16, as described above.
18. The total concentration of compensating impurities in the main doped region is 1×10 18 atoms / cm 3 The GaN substrate wafer according to any one of claims 4 to 8, 16 and 17, as described above.
19. 19. The GaN substrate wafer according to claims 5 to 8 and 16 to 18, wherein in said main doped region, the total concentration of compensating impurities is at least twice the total concentration of donor impurities.
20. 20. The GaN substrate wafer according to claim 4, wherein the primary doped region contains one or more elements selected from the group consisting of carbon and transition metal elements.
21. 21. The GaN substrate wafer according to claim 4, wherein the impurity contained in the primary doped region at the highest concentration is Fe, Mn or C.
22. 22. The GaN substrate wafer according to claim 4, wherein the primary doped region is a region within a specific length from a main surface on the GaN polarity side, and the specific length is 20 μm or more.
23. 23. The GaN substrate wafer according to claim 4, wherein the variation in the total concentration of compensation impurities along the c-axis direction in the primary doped region is within a range of ±25% from the median value.
24. 23. The GaN substrate wafer according to claims 5, 8 and 22, wherein said specific length is greater than 50 μm.
25. 23. The GaN substrate wafer according to claims 5, 7 and 22, wherein said particular length is 50% or more of a minimum thickness of said second region.
26. The total concentration of the compensating impurities in the second region is 5×10 19 atoms / cm 3 26. The GaN substrate wafer according to claim 1, wherein:
27. The GaN substrate wafer according to any one of claims 1 to 8 and 10, wherein the second region has a minimum thickness of 300 µm or less.
28. The GaN substrate wafer according to any one of claims 1 to 27, wherein a main surface on the Ga polar side is a flat surface.
29. 10. The GaN substrate wafer according to claim 1, wherein the regrowth interface is inclined with respect to the Ga-polar main surface.
30. 30. The GaN substrate wafer according to claim 29, wherein a thickness difference between one end and the other end in a direction in which the regrowth interface in the second region is inclined does not exceed 200 μm.
31. 31. An epitaxial wafer comprising: the GaN substrate wafer according to claim 1; and a nitride semiconductor layer epitaxially grown on a Ga-polar main surface of the GaN substrate wafer.
32. A method for producing an epitaxial wafer, comprising the steps of: preparing the GaN substrate wafer according to any one of claims 1 to 30; and growing a nitride semiconductor layer on a Ga-polar main surface of the GaN substrate wafer.
33. A method for manufacturing a GaN substrate wafer according to any one of claims 1 to 30, 1. A method for manufacturing a nitride semiconductor device, comprising: growing a nitride semiconductor layer on a Ga-polar major surface of a substrate wafer to obtain an epitaxial wafer; and removing the first region of the GaN substrate wafer in at least a portion of the epitaxial wafer.
34. a second step of growing a (0001) oriented second thick GaN film on the substrate by HVPE and then slicing the second thick GaN film to obtain a second c-plane GaN wafer; and a third step of growing a (0001) oriented GaN film greater than 50 μm thick on the second c-plane GaN wafer by HVPE; and The GaN film has a total concentration of compensation impurities of 1×10 17 atoms / cm 3 A part that is equal to or more than the above is provided, A method for producing a GaN substrate wafer, characterized in that the GaN film has a thickness of 300 μm or less.
35. 1. A method for producing a GaN substrate wafer having an N-polar region and a Ga-polar region separated by a regrowth interface, comprising: (i) a first GaN layer made of intentionally undoped GaN with a (0001) orientation; A first step of growing a thick film on a seed wafer by HVPE and processing the first GaN thick film to obtain at least one first c-plane GaN wafer; (ii) a second step of growing a second thick GaN film, which is made of intentionally undoped GaN and has a (0001) orientation, on the first c-plane GaN wafer obtained in the first step by HVPE and slicing a second c-plane GaN wafer from the second thick GaN film; and (iii) The GaN film having a thickness of more than 50 μm and a (0001) orientation is formed on the first GaN film obtained in the second step. a third step of growing a GaN film on a c-plane GaN wafer by HVPE to obtain a laminated structure, and the GaN film grown in the third step has a total concentration of compensation impurities of 1×10 17 atoms / cm 3 and the GaN film has a thickness of 300 μm or less.
36. A method for producing a GaN substrate wafer having an N-polarity region and a Ga-polarity region separated by a regrowth interface, comprising: (i) a first GaN layer made of intentionally undoped GaN with a (0001) orientation; A first step of growing a thick film on a seed wafer by HVPE and processing the first GaN thick film to obtain at least one first c-plane GaN wafer; (ii) a second step of growing a second thick GaN film, which is made of intentionally undoped GaN and has a (0001) orientation, on the first c-plane GaN wafer obtained in the first step by HVPE and slicing a second c-plane GaN wafer from the second thick GaN film; and (iii) The GaN film having a thickness of more than 50 μm and a (0001) orientation is formed on the first GaN film obtained in the second step. A method for manufacturing a GaN substrate wafer, comprising: a third step of growing a layered structure on a double c-plane GaN wafer by HVPE; the GaN film grown in the third step has a portion having a total concentration of compensation impurities of 1 x 1017 atoms / cm3 or more; and the GaN film has a region length in the c-axis direction of 20 μm or more and a total concentration of compensation impurities in the region of 1 x 1017 atoms / cm3 or more.
37. A method for producing a GaN substrate wafer having an N-polarity region and a Ga-polarity region separated by a regrowth interface, comprising: (i) a first GaN layer made of intentionally undoped GaN with a (0001) orientation; A first step of growing a thick film on a seed wafer by HVPE and processing the first GaN thick film to obtain at least one first c-plane GaN wafer; (ii) a second step of growing a second thick GaN film, consisting of intentionally undoped GaN and having a (0001) orientation, on the first c-plane GaN wafer obtained in the first step by HVPE and slicing a second c-plane GaN wafer from the second thick GaN film; (iii) The GaN film having a thickness of more than 50 μm and a (0001) orientation is formed on the first GaN film obtained in the second step. a third step of growing the GaN film on a c-plane GaN wafer by HVPE to obtain a laminated structure, and the GaN film grown in the third step has a portion having a total concentration of compensating impurities of 1×10 17 atoms / cm 3 or more; A method for producing a GaN substrate wafer, comprising the steps of: thinning the laminated structure after the third step;
38. 38. The method for producing a GaN substrate wafer according to claim 36 or 37, wherein the GaN film has a thickness of 300 μm or less.
39. The method for producing a GaN substrate wafer according to any one of claims 35 to 38, wherein the GaN substrate wafer satisfies any one of the conditions selected from the following (1) to (3): (1) Having a diameter of 50 mm or more and 55 mm or less and a thickness of 250 μm or more and 450 μm or less. (2) Having a diameter of 100 mm or more and 105 mm or less and a thickness of 350 μm or more and 750 μm or less. (3) Having a diameter of 150 mm or more and 155 mm or less and a thickness of 450 μm or more and 800 μm or less.
40. The GaN film has a region length in the c-axis direction of 20 μm or more, and a total concentration of compensation impurities in the region is 1×10 17 atoms / cm 3 The method for producing a GaN substrate wafer according to claim 35 or 37, having a specifically doped region.
41. The total concentration of the compensation impurities in the specific doped region is 1×10 18 atoms / cm 3 The method for producing a GaN substrate wafer according to claim 36 or 40.
42. 42. The method for producing a GaN substrate wafer according to claim 36, 40, or 41, wherein in the specific doped region, a total concentration of compensating impurities is at least twice as high as a total concentration of donor impurities.
43. The method for producing a GaN substrate wafer according to any one of claims 36 and 40 to 42, wherein the variation in the total concentration of compensation impurities in the specific doped region along the c-axis direction is within a range of ±25% from the median value.
44. The method for producing a GaN substrate wafer according to any one of claims 36 and 40 to 43, wherein the region length is 50% or more of the thickness of the GaN film.
45. 45. The method for manufacturing a GaN substrate wafer according to claim 36, wherein a length from a lower end of the specific doped region to an interface between the GaN film and the second c-plane GaN wafer is 1 μm or more.
46. The method for producing a GaN substrate wafer according to any one of claims 36 and 40 to 45, wherein the specific doped region contains one or more elements selected from carbon and transition metal elements.
47. The method for producing a GaN substrate wafer according to any one of claims 36 and 40 to 46, wherein the impurity contained in the specific doped region at the highest concentration is Fe, Mn or C.
48. The total concentration of compensating impurities in the GaN film is 5×10 19 atoms / cm 3 The method for producing a GaN substrate wafer according to any one of claims 35 to 47, wherein:
49. The method for producing a GaN substrate wafer according to any one of claims 35, 36 and 38 to 48, further comprising a thinning step of thinning the laminated structure after the third step.
50. 50. The method for producing a GaN substrate wafer according to claim 37 or 49, wherein a difference in thickness of the GaN film before and after the thinning step is 50 μm or more.
51. 51. The method for producing a GaN substrate wafer according to any one of claims 37, 49 and 50, wherein a difference in thickness of the GaN film before and after the thinning step is 200 μm or less.
52. The method for producing a GaN substrate wafer according to any one of claims 37 and 49-51, wherein an offcut orientation of the GaN substrate wafer is different from an offcut orientation of the second c-plane GaN wafer.
53. The method for producing a GaN substrate wafer according to any one of claims 34 to 52, further comprising a planarization step of planarizing a Ga-polarity side main surface of the second c-plane GaN wafer sliced from the second GaN thick film in the second step, and a roughening step of roughening the main surface by etching, before growing the GaN film in the third step.
Citation Information
Patent Citations
Nitride semiconductor substrate, manufacturing method therefor and device employing the same
JP2012232884A
Semi-insulating crystal, n-type semiconductor crystal, and p-type semiconductor crystal
JP2018070405A
METHOD FOR PRODUCTION OF GaxIn1-xN (0≤x≤1) CRYSTAL, GaxIn1-xN (0≤x≤1) CRYSTAL SUBSTRATE, METHOD FOR PRODUCTION OF GaN CRYSTAL, GaN CRYSTAL SUBSTRATE AND PRODUCT
WO2007023722A1
Semiconductor substrate manufacturing method
WO2015114732A1