resin

The adhesive composition, featuring a resin derived from carboxyl and alicyclic epoxy group-containing compounds, addresses the issue of adhesive residue in semiconductor manufacturing by ensuring strong adhesion during high-temperature processing and easy peelability post-UV irradiation.

JP7568024B2Active Publication Date: 2024-10-16RESONAC CORP
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2023166256
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-09-03
Filing Date
2023-09-27
Publication Date
2024-10-16
Estimated Expiration
2039-06-17

AI Technical Summary

Technical Problem

Conventional pressure-sensitive adhesive sheets fail to maintain sufficient adhesion during high-temperature processing steps and often leave adhesive residue after UV irradiation, necessitating improved adhesive compositions for semiconductor manufacturing.

Method used

A pressure-sensitive adhesive composition containing a resin derived from a carboxyl group-containing ethylenically unsaturated monomer and an alicyclic epoxy group-containing ethylenically unsaturated compound, which forms a three-dimensional crosslinked structure upon UV irradiation, ensuring strong adhesion before UV exposure and easy peelability afterward.

Benefits of technology

The adhesive composition provides sufficient adhesion to semiconductor wafers during high-temperature processing, reduces adhesive residue, and facilitates easy peeling without leaving behind adhesive after UV irradiation, enhancing the efficiency of semiconductor manufacturing processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007568024000001
    Figure 0007568024000001
  • Figure 0007568024000002
    Figure 0007568024000002
  • Figure 0007568024000003
    Figure 0007568024000003
Patent Text Reader

Abstract

To provide an adhesive composition from which an adhesive sheet can be obtained that is used as a material forming an adhesive layer of an adhesive sheet, thereby has sufficient adhesive force to adherend, can obtain excellent easy peelability even when the adherend stuck with the adhesive sheet is converted into a high temperature state and is returned to a room temperature, is irradiated with UV and then is peeled, and prevents adhesive residues.SOLUTION: An adhesive composition contains a resin represented by formula (1-1) and a photopolymerization initiator. R1 to R4 are -H or -CH3. R5 is an alkyl group having 1 to 16 carbon atoms. R6 is an alicyclic hydrocarbon group or an aromatic hydrocarbon group. R7 is -H or -(CH2)j-COOH (in the formula, j is 1 or 2). R8 is a specific group.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a pressure-sensitive adhesive composition and a pressure-sensitive adhesive sheet. This application claims priority based on Japanese Patent Application No. 2018-164843, filed in Japan on September 3, 2018, the contents of which are incorporated herein by reference. [Background technology]

[0002] Conventionally, various adhesive sheets have been used in the manufacturing process of semiconductors. Specifically, there are protective sheets for protecting semiconductor wafers in the back grinding process, and fixing sheets used in the dicing process for cutting and dividing semiconductor wafers into small element pieces. These adhesive sheets are removably attached to the semiconductor wafer, which is the adherend, and are peeled off from the adherend after the completion of a predetermined processing step. 2. Description of the Related Art Known pressure-sensitive adhesive compositions used in pressure-sensitive adhesive layers of removable pressure-sensitive adhesive sheets include those that contain an ethylenically unsaturated group in the molecule and that are UV (ultraviolet light) curable.

[0003] Patent Document 1 discloses a method for producing a pressure-sensitive adhesive sheet, which includes a step of reacting a (meth)acrylic polymer having two or more hydroxyl groups in its side chains with a compound having an isocyanato group in the presence of a first catalyst to form a (meth)acrylic polymer having a urethane bond, and a step of reacting the (meth)acrylic polymer having a urethane bond with a compound having two or more isocyanato groups in one molecule in the presence of a second catalyst to form a pressure-sensitive adhesive layer, wherein the first catalyst is a complex of at least one metal selected from zirconium, titanium and aluminum, and the second catalyst is an amine-based catalyst. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Patent No. 5996985 Summary of the Invention [Problem to be solved by the invention]

[0005] A removable adhesive sheet is required to have sufficient adhesive strength to the adherend when the specified processing step is performed, to be easily peeled from the adherend after the specified processing step is completed (easy peelability), and not have the adhesive layer of the adhesive sheet transferred to the adherend after peeling (no adhesive residue). However, conventional pressure-sensitive adhesive sheets do not satisfy all of the above requirements. In particular, when the pressure-sensitive adhesive sheet is applied to an adherend, the adherend is processed at a high temperature of about 200°C, and then the sheet is peeled off by UV irradiation, there is a problem in that adhesive residue is easily left behind.

[0006] The present invention has been made in consideration of the above circumstances, and an object of the present invention is to provide a pressure-sensitive adhesive composition which, when used as a material for forming a pressure-sensitive adhesive layer of a pressure-sensitive adhesive sheet, can provide a pressure-sensitive adhesive sheet which has sufficient adhesive strength to an adherend, and which has excellent easy peelability and is less likely to leave adhesive residue, even when the adherend to which the pressure-sensitive adhesive sheet is attached is heated to a high temperature, then returned to room temperature, and irradiated with UV light and then peeled off. Another object of the present invention is to provide a pressure-sensitive adhesive sheet having a pressure-sensitive adhesive layer containing the pressure-sensitive adhesive composition. [Means for solving the problem]

[0007] The present inventors have conducted extensive research to solve the above problems, and have found that it is sufficient to use a pressure-sensitive adhesive composition containing, as essential components, a resin (A) obtained by addition reaction between a carboxyl-containing resin (b) obtained by polymerizing a carboxyl-containing ethylenically unsaturated monomer (a) as an essential monomer component and an alicyclic epoxy-containing ethylenically unsaturated compound (c), and a photopolymerization initiator (B).

[0008] The adhesive composition containing the resin (A) and the photopolymerization initiator (B) has good heat resistance because the resin (A) has a structure derived from an alicyclic compound. In addition, the adhesive composition is cured by irradiating ultraviolet (UV) rays, whereby the unsaturated bonds in the resin (A) form a three-dimensional crosslinked structure, and the adhesive strength changes. Specifically, the adhesive composition has sufficient adhesive strength to the adherend before irradiating UV rays, and after irradiating UV rays, the adhesive strength decreases, resulting in excellent peelability, and sufficient prevention of adhesive residue on the adherend after peeling. Based on these findings, the present inventors have arrived at the present invention.

[0009] [1] A pressure-sensitive adhesive composition comprising a resin (A) represented by the following general formula (1-1) and a photopolymerization initiator (B):

[0010] [ka]

[0011] [ka] (In formula (1-1), k, l, m, and n represent the molar composition ratio when k+l+m+n=100. k is greater than 0 and less than 92. l is 0 to 50. m is greater than 0 and less than 90. The total of k, l, and m is 65 to 95. n is 5 to 35. R 1 ~R 4 is -H or -CH3. 5 R is an alkyl group having 1 to 16 carbon atoms. 6 R is an alicyclic hydrocarbon group having 3 to 30 carbon atoms or an aromatic hydrocarbon group having 6 to 20 carbon atoms. 7 is -H or -(CH2) j -COOH (where j is 1 or 2). 8 is the above general formula (1-2) or (1-3). In formulas (1-2) and (1-3), p and q are selected from 0, 1, and 2. s is 0 when p is 0, and is 1 when p is 1 or 2. R9 is -H or -CH3.)

[0012] [2] The pressure-sensitive adhesive composition according to [1], wherein the resin (A) has a weight-average molecular weight of 200,000 to 1,000,000. [3] The pressure-sensitive adhesive composition according to [1] or [2], wherein n in the formula (1-1) is 10 to 33. [4] The pressure-sensitive adhesive composition according to any one of [1] to [3], wherein in the formula (1-1), k is 45 to 90, l is 4 to 40, and m is 1 to 15.

[0013] [5] The pressure-sensitive adhesive composition according to any one of [1] to [4], further comprising a crosslinking agent (C). [6] The pressure-sensitive adhesive composition according to any one of [1] to [5], wherein the resin (A) has a glass transition temperature of -80 to 0°C.

[0014] [7] A pressure-sensitive adhesive sheet comprising a sheet-like substrate and a pressure-sensitive adhesive layer formed on the substrate, the pressure-sensitive adhesive layer comprising the pressure-sensitive adhesive composition according to any one of [1] to [6]. Effect of the Invention

[0015] By using the adhesive composition of the present invention as a material for forming the adhesive layer of an adhesive sheet, an adhesive sheet can be obtained which has sufficient adhesive strength to an adherend, and which has excellent easy peelability and is less likely to leave adhesive residue, even when the adherend to which the adhesive sheet is attached is heated to a high temperature, then cooled to room temperature, and then irradiated with UV light and then peeled off. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] The pressure-sensitive adhesive composition and pressure-sensitive adhesive sheet of the present invention will be described in detail below. Note that the present invention is not limited to the embodiments described below. "Adhesive composition" The pressure-sensitive adhesive composition of the present embodiment contains a resin (A) and a photopolymerization initiator (B). (Resin (A)) The resin (A) contained in the pressure-sensitive adhesive composition of the present embodiment is a compound represented by the following general formula (1-1).

[0017] [ka]

[0018] [ka] (In formula (1-1), k, l, m, and n represent the molar composition ratio when k+l+m+n=100. k is greater than 0 and less than 92. l is 0 to 50. m is greater than 0 and less than 90. The total of k, l, and m is 65 to 95. n is 5 to 35. R 1 ~R 4 is -H or -CH3. 5 R is an alkyl group having 1 to 16 carbon atoms. 6 R is an alicyclic hydrocarbon group having 3 to 30 carbon atoms or an aromatic hydrocarbon group having 6 to 20 carbon atoms. 7 is -H or -(CH2) j -COOH (where j is 1 or 2). 8 is the above general formula (1-2) or (1-3). In formulas (1-2) and (1-3), p and q are selected from 0, 1, and 2. s is 0 when p is 0, and is 1 when p is 1 or 2. R 9 is -H or -CH3.)

[0019] In formula (1-1), k, l, m, and n represent the molar composition ratio when k+l+m+n=100. k is more than 0 and not more than 92. l is 0 to 50. m is more than 0 and not more than 90. The total of k, l, and m is 65 to 95. When the total of k, l, and m is 65 or more, the adhesive composition has sufficient adhesiveness to the adherend before UV irradiation. The total of k, l, and m is preferably 70 to 94, and more preferably 80 to 90.

[0020] In formula (1-1), the repeating unit shown in parentheses enclosed by k (hereinafter referred to as "repeating unit k") is an essential repeating unit. The repeating unit k contributes to the adhesive strength of the pressure-sensitive adhesive composition before UV irradiation. The repeat number k of the repeating unit k is more than 0 and 92 or less, preferably 45 to 90, and more preferably 60 to 88.

[0021] In formula (1-1), the repeating unit shown in the parentheses enclosed by l (hereinafter referred to as "repeating unit l") may be omitted. In other words, the number of repetitions of repeating unit l may be 0. The repeating unit 1 contributes to the heat resistance of the pressure-sensitive adhesive composition. The repeating number 1 of the repeating unit 1 is 0-50, preferably 4-40, and more preferably 5-30.

[0022] In formula (1-1), the repeating unit shown in ( ) enclosed by m (hereinafter referred to as "repeating unit m") is an essential repeating unit. The repeating unit m contributes to the adhesive strength and heat resistance of the pressure-sensitive adhesive composition before UV irradiation. In addition, when the pressure-sensitive adhesive composition contains a crosslinking agent having a functional group that reacts with a carboxy group, the repeating unit m reacts with the crosslinking agent to improve the cohesive strength of the pressure-sensitive adhesive composition. The number of repetitions m of the repeating unit m is more than 0 and not more than 90, preferably 1 to 15, and more preferably 1 to 5.

[0023] In formula (1-1), the repeating unit shown in ( ) enclosed by n (hereinafter referred to as "repeating unit n") is an essential repeating unit. The repeating unit n contributes to the heat resistance of the pressure-sensitive adhesive composition. The repeat number n of the repeating unit n is 5 to 35, preferably 10 to 33, and more preferably 10 to 20. When the repeating unit n is 35 or less, the unsaturated bonds in the resin (A) form a three-dimensional crosslinked structure upon UV irradiation and harden, resulting in a pressure-sensitive adhesive composition whose adhesive strength decreases to an appropriate range. When n is 5 or more, an effect of improving heat resistance due to the structure derived from the alicyclic compound is obtained.

[0024] Due to the synergistic effect of the functions contributed by each of these repeating units, the adhesive composition containing resin (A) has a better balance between the adhesive strength before ultraviolet (UV) irradiation and the adhesive strength after UV irradiation. As a result, the adhesive composition has sufficient adhesive strength to the adherend before UV irradiation, and the adhesive strength decreases after UV irradiation, resulting in an adhesive composition with excellent peelability. Moreover, this adhesive composition does not have too high adhesive strength even when it is heated to a high temperature before UV irradiation and then returned to room temperature, and has excellent peelability after UV irradiation and is less likely to leave adhesive residue on the adherend after peeling.

[0025] In repeat unit k, R 1 is -H or -CH3, preferably -H. 5 is an alkyl group having 1 to 16 carbon atoms, preferably an alkyl group having 1 to 8 carbon atoms, and particularly preferably an alkyl group having 2, 4 or 8 carbon atoms.

[0026] The repeating unit k is R 1 , R 5 When the repeating unit k includes multiple types of repeating units, the molar composition ratio k of the repeating unit k indicates the sum of the molar composition ratios of the multiple types of repeating units. For example, when the repeating unit k includes R 1 and / or R 5 In the case where the repeating unit A has a molar composition ratio of 2 mol % and the repeating unit B has a molar composition ratio of 3 mol %, the molar composition ratio k of the repeat number k is the sum of the molar composition ratios of the repeating unit A and the repeating unit B, which is "5".

[0027] In repeating unit l, R 2 is -H or -CH3, preferably -H. 6 is an alicyclic hydrocarbon group having 3 to 30 carbon atoms or an aromatic hydrocarbon group having 6 to 20 carbon atoms, and is preferably an alicyclic hydrocarbon group having 6 to 20 carbon atoms or an aromatic hydrocarbon group having 6 to 10 carbon atoms. Repeating unit l is R 2 , R 6When the repeating unit l contains a plurality of types of repeating units, the molar composition ratio l of the repeating unit l represents the sum of the molar composition ratios of the plurality of types of repeating units.

[0028] In repeating unit m, R 3 is -H or -CH3, preferably -H. 7 is -H or -(CH2) j -COOH (wherein j is 1 or 2), and -H is preferred. Repeating unit m is R 3 , R 7 In this case, the molar composition ratio m of the repeating unit m represents the sum of the molar composition ratios of the multiple repeating units.

[0029] In repeat unit n, R 4 is -H or -CH3, preferably -H. 8 is represented by formula (1-2) or (1-3). The groups represented by formula (1-2) or (1-3) each contain a structure derived from an alicyclic compound and have the function of improving the heat resistance of the pressure-sensitive adhesive composition. In formula (1-2) or (1-3), p and q are any one selected from 0, 1, and 2. s is 0 when p is 0, and is 1 when p is 1 or 2. R 9 is -H or -CH3. Repeat unit n is R 4 , R 8 In this case, the molar composition ratio n of the repeating unit n represents the sum of the molar composition ratios of the multiple repeating units.

[0030] The resin (A) represented by formula (1-1) may be any of a random copolymer, a block copolymer, and an alternating copolymer consisting of repeating units k, l, m, and n. The resin (A) represented by formula (1-1) may not contain the repeating unit l, and may be any of a random copolymer, a block copolymer, and an alternating copolymer consisting of repeating units k, m, and n.

[0031] The weight average molecular weight of the resin (A) is preferably 200,000 to 1,000,000, more preferably 300,000 to 800,000. When the weight average molecular weight of the resin (A) is 200,000 or more, when a pressure-sensitive adhesive sheet having a pressure-sensitive adhesive layer containing a pressure-sensitive adhesive composition is attached to an adherend and then peeled off, the pressure-sensitive adhesive layer is less likely to remain on the adherend. When the weight average molecular weight of the resin (A) is 1,000,000 or less, the viscosity of the resin (A) does not become too high, and the effect of good workability can be obtained. The weight average molecular weight of the resin (A) is a value measured by the method described in the examples.

[0032] The glass transition temperature (Tg) of the resin (A) is preferably −80 to 0° C., more preferably −60 to −10° C., and further preferably −50 to −10° C. When the glass transition temperature of the resin (A) is in the range of −80 to 0° C., the adhesive strength of the pressure-sensitive adhesive composition before UV irradiation becomes good. The Tg of the resin (A) is a value measured by the method described in the examples. The acid value of the resin (A) is preferably more than 0 to 20 mgKOH / g, more preferably 3 to 10 mgKOH / g. When the acid value of the resin (A) is in the range of more than 0 to 20 mgKOH / g, there is no contamination of the adherend (glue residue) after heating, which is good. In addition, when the pressure-sensitive adhesive composition contains a crosslinking agent, when the acid value of the resin (A) is in the above range, the resin (A) reacts with the crosslinking agent, and the cohesive force of the pressure-sensitive adhesive composition is good. The acid value of the resin (A) is a value measured by the method described in the examples.

[0033] (Method for producing resin (A)) The resin (A) contained in the pressure-sensitive adhesive composition of the present embodiment can be produced, for example, by the method described below. First, raw material monomers including a carboxyl group-containing ethylenically unsaturated monomer (a) and an ethylenically unsaturated monomer (d) are polymerized to produce a carboxyl group-containing resin (b). Here, the ethylenically unsaturated monomer (d) includes a monomer that forms a repeating unit k after polymerization, and may also include a monomer that forms a skeleton of a repeating unit l. Next, the resin (A) is produced by addition reaction of the carboxyl group-containing resin (b) with a specific alicyclic epoxy group-containing ethylenically unsaturated compound (c).

[0034] (Carboxy Group-Containing Ethylenically Unsaturated Monomer (a)) The carboxyl group-containing ethylenically unsaturated monomer (a) used in producing the carboxyl group-containing resin (b) is a monomer that forms a skeleton of repeating units m by polymerization. The carboxyl group-containing ethylenically unsaturated monomer (a) has one carboxyl group. Examples of the carboxy group-containing ethylenically unsaturated monomer (a) include (meth)acrylic acid, β-carboxyethyl (meth)acrylate, and carboxypentyl (meth)acrylate. Among these, it is preferable to use (meth)acrylic acid and / or β-carboxyethyl (meth)acrylate as the carboxy group-containing ethylenically unsaturated monomer (a) in terms of reactivity.

[0035] As used herein, (meth)acrylic means "acrylic" or "methacrylic." (Meth)acrylate means "acrylate" or "methacrylate."

[0036] (Carboxy group-containing resin (b)) The carboxyl group-containing resin (b) is obtained by copolymerizing raw material monomers including at least a carboxyl group-containing ethylenically unsaturated monomer (a) and an ethylenically unsaturated monomer (d) copolymerizable with the carboxyl group-containing ethylenically unsaturated monomer (a). The carboxyl group-containing resin (b) is a component that becomes the skeleton of the resin (A) represented by the formula (1-1). The repeating unit k, the repeating unit l, and the repeating unit m are all repeating units derived from the carboxyl group-containing resin (b).

[0037] As the ethylenically unsaturated monomer (d), one or more monomers that form the skeleton of the repeating unit k by polymerization are used. As the ethylenically unsaturated monomer (d), one or more monomers that form the skeleton of the repeating unit l by polymerization may be used together with the monomer that forms the skeleton of the repeating unit k by polymerization.

[0038] The ethylenically unsaturated monomer (d) which forms the skeleton of the repeating unit k by polymerization is an alkyl(meth)acrylate having 1 to 16 carbon atoms, and from the viewpoint of adjusting the peel strength of the pressure-sensitive adhesive composition, preferably contains an alkyl(meth)acrylate having 2 to 16 carbon atoms, more preferably contains an alkyl(meth)acrylate having 4 to 12 carbon atoms. Specific examples include methyl(meth)acrylate, ethyl(meth)acrylate, n-propyl(meth)acrylate, n-butyl(meth)acrylate, tert-butyl(meth)acrylate, isobutyl(meth)acrylate, 2-ethylhexyl(meth)acrylate, isodecyl(meth)acrylate, n-hexyl(meth)acrylate, isooctyl(meth)acrylate, lauryl(meth)acrylate, and the like. Of these, methyl (meth)acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and isooctyl (meth)acrylate are preferred.

[0039] Examples of the ethylenically unsaturated monomer (d) that forms the skeleton of the repeating unit l by polymerization include (meth)acrylates containing a cyclic alkyl group having 3 to 30 carbon atoms, and (meth)acrylates containing an aromatic group having 6 to 20 carbon atoms.

[0040] Examples of the cyclic alkyl group-containing (meth)acrylate having 3 to 30 carbon atoms used as the ethylenically unsaturated monomer (d) that forms the skeleton of the repeating unit l by polymerization include cyclohexyl (meth)acrylate, norbornyl (meth)acrylate, isobornyl (meth)acrylate, norbornanyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, dicyclopentanyl (meth)acrylate, dicyclopentanyloxyethyl (meth)acrylate, and tricyclodecane dimethylol di(meth)acrylate. Among these, it is particularly preferable to use isobornyl (meth)acrylate. When a cyclic alkyl (meth)acrylate is contained in the raw material monomer of the carboxyl group-containing resin (b), the heat resistance of the adhesive composition containing the resin (A) produced using the carboxyl group-containing resin (b) is improved.

[0041] Examples of the aromatic group-containing (meth)acrylate having 6 to 20 carbon atoms used as the ethylenically unsaturated monomer (d) that forms the skeleton of the repeating unit l by polymerization include benzyl (meth)acrylate, phenoxyethyl (meth)acrylate, phenoxypolyethylene glycol (meth)acrylate, phenoxypropyl (meth)acrylate, and phenoxypolypropylene glycol (meth)acrylate. Among these, it is particularly preferable to use benzyl (meth)acrylate. When the aromatic group-containing (meth)acrylate is contained in the raw material monomer of the carboxyl group-containing resin (b), the heat resistance of the adhesive composition containing the resin (A) produced using the carboxyl group-containing resin (b) is improved.

[0042] The raw material monomers of the carboxy group-containing resin (b) may contain not only the above-mentioned carboxy group-containing ethylenically unsaturated monomer (a) and the above-mentioned ethylenically unsaturated monomer (d), but also a monomer copolymerizable with the carboxy group-containing ethylenically unsaturated monomer (a) other than the above-mentioned ethylenically unsaturated monomer (d).

[0043] Examples of the ethylenically unsaturated monomer copolymerizable with the carboxy group-containing ethylenically unsaturated monomer (a) other than the above ethylenically unsaturated monomer (d) include alkoxyalkyl (meth)acrylates, alkoxy(poly)alkylene glycol (meth)acrylates, hydroxy group-containing (meth)acrylates, fluorinated alkyl (meth)acrylates, dialkylaminoalkyl (meth)acrylates, and (meth)acrylamides.

[0044] Examples of alkoxyalkyl (meth)acrylates include ethoxyethyl (meth)acrylate, methoxyethyl (meth)acrylate, butoxyethyl (meth)acrylate, 2-methoxyethoxyethyl (meth)acrylate, and 2-ethoxyethoxyethyl (meth)acrylate.

[0045] Examples of the alkoxy(poly)alkylene glycol (meth)acrylate include methoxydiethylene glycol (meth)acrylate, ethoxydiethylene glycol (meth)acrylate, and methoxydipropylene glycol (meth)acrylate.

[0046] Examples of hydroxy group-containing (meth)acrylates include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 1,3-butanediol (meth)acrylate, 1,4-butanediol (meth)acrylate, 1,6-hexanediol (meth)acrylate, and 3-methylpentanediol (meth)acrylate.

[0047] An example of the fluorinated alkyl (meth)acrylate is octafluoropentyl (meth)acrylate. Examples of dialkylaminoalkyl (meth)acrylates include N,N-dimethylaminoethyl (meth)acrylate, N,N-diethylaminoethyl (meth)acrylate, and the like.

[0048] Examples of (meth)acrylamides include (meth)acrylamide, N-methyl(meth)acrylamide, N-ethyl(meth)acrylamide, N-propyl(meth)acrylamide, N-isopropylacrylamide, N-hexyl(meth)acrylamide, N,N-dimethyl(meth)acrylamide, N,N-diethyl(meth)acrylamide, (meth)acryloylmorpholine, and diacetone acrylamide.

[0049] Specific examples of monomers other than the ethylenically unsaturated monomer (d) that are copolymerizable with the carboxy group-containing ethylenically unsaturated monomer (a) include acrylonitrile, methacrylonitrile, styrene, α-methylstyrene, vinyl acetate, vinyl propionate, vinyl stearate, vinyl chloride, vinylidene chloride, alkyl vinyl ethers, vinyl toluene, N-vinylpyridine, N-vinylpyrrolidone, dialkyl itaconate esters, dialkyl fumarate esters, allyl alcohol, hydroxybutyl vinyl ether, hydroxyethyl vinyl ether, 4-hydroxymethylcyclohexylmethyl vinyl ether, triethylene glycol monovinyl ether or diethylene glycol monovinyl ether, methyl vinyl ketone, allyl trimethylammonium chloride, and dimethylallyl vinyl ketone.

[0050] The method for producing the carboxyl group-containing resin (b) is not particularly limited. For example, the carboxyl group-containing resin (b) can be obtained by copolymerizing raw material monomers including a carboxyl group-containing ethylenically unsaturated monomer (a) and an ethylenically unsaturated monomer (d), which are components of the carboxyl group-containing resin (b), by a known polymerization method. Specifically, the polymerization method may be a solution polymerization method, an emulsion polymerization method, a bulk polymerization method, a suspension polymerization method, an alternating copolymerization method, etc. Among these polymerization methods, in consideration of the addition reaction between the carboxyl group-containing resin (b) obtained after polymerization and the alicyclic epoxy group-containing ethylenically unsaturated compound (c), it is preferable to use the solution polymerization method from the viewpoint of ease of reaction.

[0051] When the carboxyl group-containing resin (b) is produced by the solution polymerization method, a radical polymerization initiator and / or a solvent is used, if necessary. The radical polymerization initiator is not particularly limited, and can be appropriately selected from known initiators. Examples of the radical polymerization initiator include 2,2'-azobis(isobutyronitrile), 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile), 2,2'-azobis(2,4-dimethylvaleronitrile), 2,2'-azobis(2-methylbutyronitrile), 1,1'-azobis(cyclohexane-1-carbonitrile), 2,2'-azobis(2,4,4-trimethylpentane), and dimethyl-2,2'-azobis. Examples of the polymerization initiator include an azo-based polymerization initiator such as bis(2-methylpropionate); and an oil-soluble polymerization initiator such as a peroxide-based polymerization initiator such as benzoyl peroxide, t-butyl hydroperoxide, di-t-butyl peroxide, t-butyl peroxybenzoate, dicumyl peroxide, 1,1-bis(t-butylperoxy)3,3,5-trimethylcyclohexane, and 1,1-bis(t-butylperoxy)cyclododecane.

[0052] These radical polymerization initiators may be used alone or in combination of two or more kinds. The amount of the radical polymerization initiator used is preferably 0.01 to 5 parts by mass, more preferably 0.02 to 4 parts by mass, and even more preferably 0.03 to 3 parts by mass, relative to 100 parts by mass of the total of the raw material monomers of the carboxy group-containing resin (b).

[0053] As the polymerization solvent used in producing the carboxyl group-containing resin (b), various general solvents can be used. Examples of the solvent include esters such as ethyl acetate, n-propyl acetate, and n-butyl acetate, aromatic hydrocarbons such as toluene, xylene, and benzene, aliphatic hydrocarbons such as n-hexane and n-heptane, alicyclic hydrocarbons such as cyclohexane and methylcyclohexane, ketones such as methyl ethyl ketone and methyl isobutyl ketone, glycols such as ethylene glycol, propylene glycol, and dipropylene glycol, glycol ethers such as methyl cellosolve, propylene glycol monomethyl ether, and dipropylene glycol monomethyl ether, and glycol esters such as ethylene glycol diacetate and propylene glycol monomethyl ether acetate. These solvents may be used alone or in combination of two or more kinds.

[0054] When producing the carboxyl group-containing resin (b), the content of the carboxyl group-containing ethylenically unsaturated monomer (a) in the raw material monomers including the carboxyl group-containing ethylenically unsaturated monomer (a), the ethylenically unsaturated monomer (d), and other monomers contained as necessary is preferably 5 to 40 mass%, more preferably 7 to 30 mass%, and even more preferably 10 to 25 mass%. By setting the content of the carboxyl group-containing ethylenically unsaturated monomer (a) in the raw material monomers within the above range, the adhesive strength of the adhesive layer obtained from the adhesive composition containing the resin (A) produced by the addition reaction of the carboxyl group-containing resin (b) and the alicyclic epoxy group-containing ethylenically unsaturated compound (c) before UV irradiation becomes good.

[0055] (Alicyclic epoxy group-containing ethylenically unsaturated compound (c)) The alicyclic epoxy group-containing ethylenically unsaturated compound (c) is an ethylenically unsaturated group-containing compound having an alicyclic epoxy group, and is a compound that gives a structure of general formula (1-2) or general formula (1-3). The alicyclic epoxy group in this embodiment refers to an epoxy group formed by bonding one oxygen atom to two adjacent carbon atoms on the ring of an alicyclic hydrocarbon compound. The alicyclic epoxy group-containing ethylenically unsaturated compound (c) is used to add the following partial structural formula (1-2') or (1-3') in the repeating unit n of the photosensitive resin (A) represented by formula (1-1). The partial structural formula (1-2') or (1-3') in the repeating unit n in formula (1-1) is a group derived from the alicyclic epoxy group-containing ethylenically unsaturated compound (c).

[0056] [ka] (In formulas (1-2') and (1-3'), q is any one selected from 0, 1, and 2. R 9 is -H or -CH3.)

[0057] Examples of the alicyclic epoxy group-containing ethylenically unsaturated compound (c) include compounds represented by the following formula (1) or (2).

[0058] [ka] (In formula (1), R 9 is -H or -CH3. q is selected from 0, 1, and 2. (In formula (2), R 9 is -H or -CH3. q is selected from 0, 1, and 2.

[0059] In formula (1), R 9 is -H or -CH3. q is any one selected from 0, 1 and 2, and q is preferably 1. In formula (2), R 9is -H or -CH3. q is any one selected from 0, 1 and 2, and q is preferably 1.

[0060] The alicyclic epoxy group-containing ethylenically unsaturated compound (c) is preferably a compound represented by formula (1), and it is particularly preferable to use 3,4-epoxycyclohexylmethyl(meth)acrylate. The alicyclic epoxy group-containing ethylenically unsaturated compound (c) may be used alone or in combination of two or more.

[0061] The resin (A) of this embodiment can be produced by subjecting the alicyclic epoxy group of the alicyclic epoxy group-containing ethylenically unsaturated monomer (c) to an addition reaction with the carboxy group of the carboxy group-containing resin (b). Resin (A) is preferably produced by addition reaction of 0.2 to 0.99 mol, more preferably 0.3 to 0.95 mol, and even more preferably 0.6 to 0.95 mol of alicyclic epoxy group-containing ethylenically unsaturated compound (c) per 1 mol of carboxy group in carboxy group-containing resin (b). The adhesive composition containing resin (A) obtained by using carboxy group-containing resin (b) and alicyclic epoxy group-containing ethylenically unsaturated compound (c) in the above ratio has sufficient adhesion to the adherend before UV irradiation, and the adhesive strength decreases after UV irradiation, resulting in better peelability. Moreover, this adhesive composition does not easily increase its adhesive strength even if it is kept in a high temperature state before UV irradiation and then returned to room temperature, and it has excellent peelability after UV irradiation and can more effectively prevent adhesive residue on the adherend after peeling.

[0062] The temperature of the addition reaction in producing the resin (A) is preferably 80 to 130° C., and particularly preferably 90 to 120° C. When the temperature of the addition reaction is 80° C. or higher, a sufficient reaction rate can be obtained. When the temperature of the addition reaction is 130° C. or lower, double bonds are crosslinked by radical polymerization due to heat, and the generation of gelled products can be prevented.

[0063] In the addition reaction in producing the resin (A), a known catalyst can be used, if necessary. Examples of the catalyst include tertiary amines such as triethylamine, tributylamine, dimethylbenzylamine, 1,8-diazabicyclo[5,4,0]undec-7-ene, 1,5-diazabicyclo[4,3,0]non-5-ene, and 1,4-diazabicyclo[2,2,2]octane; quaternary ammonium salts such as tetramethylammonium chloride, tetramethylammonium bromide, and tetrabutylammonium bromide; alkyl ureas such as tetramethylurea; alkyl guanidines such as tetramethylguanidine; and phosphine compounds such as triphenylphosphine, dimethylphenylphosphine, tricyclohexylphosphine, tributylphosphine, tris(4-methylphenyl)phosphine, tris(4-methoxyphenyl)phosphine, tris(2,6-dimethylphenyl)phosphine, tris(2,6-dimethoxyphenyl)phosphine, tris(2,4,6-trimethylphenyl)phosphine, and tris(2,4,6-trimethoxyphenyl)phosphine. Among the above, it is preferable to use a phosphine compound as a catalyst for the addition reaction in terms of reactivity.

[0064] The amount of the catalyst used in the addition reaction is preferably 0.01 to 30 parts by mass, more preferably 0.05 to 5 parts by mass, and most preferably 0.1 to 2 parts by mass, per 100 parts by mass of the total of the carboxyl group-containing resin (b) and the alicyclic epoxy group-containing ethylenically unsaturated monomer (c).

[0065] Furthermore, during the addition reaction, a gas having a polymerization-inhibiting effect may be introduced into the reaction system, or a polymerization inhibitor may be added. By introducing a gas having a polymerization-inhibiting effect into the reaction system, or by adding a polymerization inhibitor, gelation during the addition reaction can be prevented. Examples of gases that have a polymerization-inhibiting effect include gases that contain oxygen to an extent that does not fall within the explosive range of the substances in the system, such as air.

[0066] As the polymerization inhibitor, a known one can be used, and is not particularly limited, but examples thereof include 4-methoxyphenol, hydroquinone, methoquinone, 2,6-di-t-butylphenol, 2,2'-methylenebis(4-methyl-6-t-butylphenol), phenothiazine, etc. These polymerization inhibitors may be used alone or in combination of two or more kinds.

[0067] The amount of the polymerization inhibitor used is preferably 0.005 to 5 parts by mass, more preferably 0.03 to 3 parts by mass, and most preferably 0.05 to 1.5 parts by mass, based on 100 parts by mass of the total of the carboxyl group-containing resin (b) and the alicyclic epoxy group-containing ethylenically unsaturated monomer (c). If the amount of the polymerization inhibitor is too small, the polymerization inhibition effect may be insufficient. On the other hand, if the amount of the polymerization inhibitor is too large, the exposure sensitivity of the resin (A) may decrease. Furthermore, it is more preferable to use a gas having a polymerization inhibitor in combination with a polymerization inhibitor, since this makes it possible to reduce the amount of polymerization inhibitor used and to enhance the polymerization inhibitory effect.

[0068] (Photopolymerization initiator (B)) Examples of the photopolymerization initiator (B) contained in the pressure-sensitive adhesive composition include benzophenone, benzil, benzoin, ω-bromoacetophenone, chloroacetone, acetophenone, 2,2-diethoxyacetophenone, 2,2-dimethoxy-2-phenylacetophenone, p-dimethylaminoacetophenone, p-dimethylaminopropiophenone, 2-chlorobenzophenone, 4,4'-dichlorobenzophenone, 4,4'-bisdiethylaminobenzophenone, Michler's ketone, benzoin methyl ether, and benzoin isobutyl ether. carbonyl-based photopolymerization initiators such as benzoin-n-butyl ether, benzyl methyl ketal, 1-hydroxycyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenyl-propan-1-one, 1-(4-isopropylphenyl)-2-hydroxy-2-methylpropan-1-one, methylbenzoyl formate, 2,2-diethoxyacetophenone, 4-N,N'-dimethylacetophenone, and 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one.

[0069] Examples of the photopolymerization initiator (B) that can be used include sulfide-based photopolymerization initiators such as diphenyl disulfide, dibenzyl disulfide, tetraethyl thiuram disulfide, and tetramethyl ammonium monosulfide; acyl phosphine oxides such as 2,4,6-trimethylbenzoyl diphenyl phosphine oxide and 2,4,6-trimethylbenzoyl phenyl ethoxy phosphine oxide; quinone-based photopolymerization initiators such as benzoquinone and anthraquinone; sulfochloride-based photopolymerization initiators; and thioxanthone-based photopolymerization initiators such as thioxanthone, 2-chlorothioxanthone, and 2-methylthioxanthone.

[0070] Among these photopolymerization initiators (B), it is preferable to use 1-hydroxycyclohexyl phenyl ketone and / or 2,4,6-trimethylbenzoyldiphenylphosphine oxide from the viewpoint of solubility in the pressure-sensitive adhesive composition. The above photopolymerization initiators (B) may be used alone or in combination of two or more kinds.

[0071] The photopolymerization initiator (B) contained in the adhesive composition is preferably 0.1 to 5.0 parts by mass, more preferably 0.5 to 2.0 parts by mass, relative to 100 parts by mass of the resin (A). When the content of the photopolymerization initiator (B) relative to 100 parts by mass of the resin (A) is 0.1 parts by mass or more, the adhesive composition is cured at a sufficiently high curing speed by UV irradiation, and the adhesive strength of the adhesive composition after UV irradiation becomes sufficiently small, which is preferable. When the content of the photopolymerization initiator (B) is 5.0 parts by mass or less, when a pressure-sensitive adhesive sheet having a pressure-sensitive adhesive layer containing the pressure-sensitive adhesive composition is attached to an adherend and then peeled off, the pressure-sensitive adhesive layer is unlikely to remain on the adherend. In addition, even if the content of the photopolymerization initiator (B) exceeds 5.0 parts by mass, no effect commensurate with the content of the photopolymerization initiator (B) is observed.

[0072] (Crosslinking agent (C)) The pressure-sensitive adhesive composition of the present embodiment may contain not only the resin (A) and the photopolymerization initiator (B) but also a crosslinking agent (C). By containing the crosslinking agent (C), the pressure-sensitive adhesive composition has a better balance between the adhesive strength before UV irradiation and the adhesive strength after UV irradiation. The crosslinking agent (C) is not particularly limited, but is preferably a compound having two or more functional groups reactive with the hydroxyl group of the repeating unit n, or with the hydroxyl group of the repeating unit n and the carboxyl group of the repeating unit m.

[0073] Examples of the crosslinking agent (C) include isocyanate compounds such as 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, hydrogenated tolylene diisocyanate, 1,3-xylylene diisocyanate, 1,4-xylylene diisocyanate, diphenylmethane-4,4-diisocyanate, isophorone diisocyanate, 1,3-bis(N,N'-diglycidylaminomethyl)cyclohexane, 1,3-bis(isocyanatomethyl)cyclohexane, isocyanurate of hexamethylene diisocyanate, tetramethylxylylene diisocyanate, 1,5-naphthalene diisocyanate, tolylene diisocyanate adduct of trimethylolpropane, xylylene diisocyanate adduct of trimethylolpropane, triphenylmethane triisocyanate, and methylenebis(4-phenylmethane)triisocyanate; Bisphenol A·epichlorohydrin type epoxy resins, N,N'-[1,3-phenylenebis(methylene)]bis[bis(oxiran-2-ylmethyl)amine], ethylene glycol diglycidyl ether, polyethylene glycol diglycidyl ether, glycerin diglycidyl ether, glycerin triglycidyl ether, 1,6-hexanediol diglycidyl ether, trimethylolpropane triglycidyl ether, sorbitol polyglycidyl ether, polyglycerol polyglycidyl ether, pentaerythritol polyglycidyl erythritol, diglycerol polyglycidyl ether and other epoxy compounds, Aziridine compounds such as tetramethylolmethane-tri-β-aziridinylpropionate, trimethylolpropane-tri-β-aziridinylpropionate, N,N'-diphenylmethane-4,4'-bis(1-aziridinecarboxamide), and N,N'-hexamethylene-1,6-bis(1-aziridinecarboxamide); Examples of the melamine-based compounds include hexamethoxymethylmelamine, hexaethoxymethylmelamine, hexapropoxymethylmelamine, hexaptoxymethylmelamine, hexapentyloxymethylmelamine, and hexahexyloxymethylmelamine.

[0074] Among these, it is preferable to use an epoxy compound and / or an isocyanate compound as the crosslinking agent (C) because they have good reactivity with the resin (A). The above crosslinking agents (C) may be used alone or in combination of two or more kinds.

[0075] The crosslinking agent (C) contained in the pressure-sensitive adhesive composition is preferably 0.05 to 10 parts by mass, more preferably 0.1 to 5 parts by mass, and even more preferably 0.1 to 1.0 parts by mass, relative to 100 parts by mass of the resin (A). When the content of the crosslinking agent (C) relative to 100 parts by mass of the resin (A) is 0.05 parts by mass or more, a three-dimensional crosslinked structure is sufficiently formed in the pressure-sensitive adhesive composition. As a result, the adhesive strength of the pressure-sensitive adhesive composition after UV irradiation becomes sufficiently small, which is preferable. When the content of the crosslinking agent (C) relative to 100 parts by mass of the resin (A) is 10 parts by mass or less, the adhesive strength of the pressure-sensitive adhesive composition before UV irradiation becomes good.

[0076] (Other ingredients) The pressure-sensitive adhesive composition of the present embodiment may contain other components in addition to the above-mentioned resin (A), photopolymerization initiator (B) and crosslinking agent (C), as necessary. Examples of other components include tackifiers, solvents, and various additives.

[0077] (tackifier) The tackifier may be any known tackifier without any particular limitation. Examples of the tackifier include terpene-based tackifier resins, phenol-based tackifier resins, rosin-based tackifier resins, aliphatic petroleum resins, aromatic petroleum resins, copolymerized petroleum resins, alicyclic petroleum resins, xylene resins, epoxy-based tackifier resins, polyamide-based tackifier resins, ketone-based tackifier resins, and elastomer-based tackifier resins. These tackifiers may be used alone or in combination of two or more.

[0078] When the pressure-sensitive adhesive composition of the present embodiment contains a tackifier, the content thereof is preferably 30 parts by mass or less, and more preferably 5 to 20 parts by mass, per 100 parts by mass of the resin (A).

[0079] (solvent) The solvent can be used to dilute the PSA composition for the purpose of adjusting the viscosity of the PSA composition when the PSA composition is applied. Examples of the solvent that can be used include organic solvents such as methyl ethyl ketone, methyl isobutyl ketone, acetone, ethyl acetate, n-propyl acetate, tetrahydrofuran, dioxane, cyclohexanone, n-hexane, toluene, xylene, n-propanol, isopropanol, etc. These solvents may be used alone or in combination of two or more.

[0080] (Additives) Examples of the additives include plasticizers, surface lubricants, leveling agents, softeners, antioxidants, antiaging agents, light stabilizers, ultraviolet absorbers, polymerization inhibitors, benzotriazole-based light stabilizers, phosphate ester-based and other flame retardants, and antistatic agents such as surfactants.

[0081] [Method of manufacturing adhesive composition] The pressure-sensitive adhesive composition of the present embodiment can be produced by a conventionally known method. For example, the composition can be produced by mixing and stirring the above-mentioned resin (A) and photopolymerization initiator (B) with the crosslinking agent (C), tackifier, solvent, and various additives, which are contained as necessary, using a conventionally known method.

[0082] The pressure-sensitive adhesive composition of the present embodiment is suitable as a material for forming a pressure-sensitive adhesive layer of a pressure-sensitive adhesive sheet, and in particular, the pressure-sensitive adhesive composition of the present embodiment is suitable as a material for forming a pressure-sensitive adhesive layer of a removable pressure-sensitive adhesive sheet. The adhesive composition of the present embodiment contains the resin (A) represented by formula (1-1) and the photopolymerization initiator (B), and when used as a material for forming the adhesive layer of an adhesive sheet, an adhesive sheet having sufficient adhesive strength to an adherend can be obtained. Moreover, even if the adherend to which the adhesive sheet is attached is heated to a high temperature and then returned to room temperature for peeling, this adhesive sheet has excellent easy peelability after UV irradiation and is unlikely to leave adhesive residue.

[0083] "Adhesive sheet" The pressure-sensitive adhesive sheet of the present invention has a sheet-like substrate and a pressure-sensitive adhesive layer formed on the substrate. It is preferable that a release sheet (separator) is provided on the surface of the adhesive layer opposite to the substrate. When a release sheet is provided on the adhesive layer, the release sheet can protect the adhesive layer until it is used. In addition, when a release sheet is provided on the adhesive layer, the release sheet can be peeled off to expose the adhesive layer, and the adhesive layer (attachment surface) can be efficiently pressed against the adherend. The pressure-sensitive adhesive sheet of the present embodiment may be used as a pressure-sensitive adhesive tape formed into a shape corresponding to the shape of an adherend by a punching method, etc. The pressure-sensitive adhesive sheet of the present embodiment may also be used as a pressure-sensitive adhesive tape by being wound up and cut.

[0084] The substrate can be appropriately selected from known sheet-like materials, and it is preferable to use a resin sheet made of a transparent resin material as the substrate. Examples of resin materials include polyolefins such as polyethylene (PE) and polypropylene (PP); polyester sheets such as polyethylene terephthalate (PET), polybutylene terephthalate (PBT), and polyethylene naphthalate; polyvinyl chloride (PVC); polyimide (PI); polyphenylene sulfide (PPS); ethylene vinyl acetate (EVA); and polytetrafluoroethylene (PTFE). Among these resin materials, it is preferable to use PE, PP, and PET because they provide sheets with appropriate flexibility. The resin materials may be used alone or in combination of two or more.

[0085] When a resin sheet is used as the substrate, the resin sheet may be a single layer or a multi-layer structure of two or more layers (e.g., a three-layer structure). In a resin sheet having a multi-layer structure, the resin material constituting each layer may be a resin material containing only one type alone or a resin material containing two or more types.

[0086] The thickness of the substrate can be appropriately selected depending on the application of the adhesive sheet, the material of the substrate, and the like. When the adhesive sheet is for protecting the wafer during the wafer dicing process and a resin sheet is used as the substrate, the thickness of the substrate is preferably, for example, 10 to 1000 μm, more preferably 50 to 300 μm. When the thickness of the substrate is 10 μm or more, the rigidity (stiffness) of the adhesive sheet is high. Therefore, when the adhesive sheet is attached to an adherend such as a wafer or peeled off from the adherend, the adhesive sheet tends to be less prone to wrinkles or lifting. In addition, when the thickness of the substrate is 10 μm or more, the adhesive sheet attached to the adherend can be easily peeled off from the adherend, and the workability (handling ability, handling) is improved. When the thickness of the substrate is 1000 μm or less, the rigidity (stiffness) of the adhesive sheet can be prevented from becoming too high, which can prevent the workability from decreasing.

[0087] When a resin sheet is used as the substrate, the substrate can be produced by appropriately employing a conventionally known general sheet molding method (for example, extrusion molding, T-die molding, inflation molding, or uniaxial or biaxial stretch molding).

[0088] The surface of the substrate that comes into contact with the pressure-sensitive adhesive layer may be subjected to a surface treatment in order to improve the adhesion between the substrate and the pressure-sensitive adhesive layer. Examples of the surface treatment include corona discharge treatment, acid treatment, ultraviolet irradiation treatment, plasma treatment, and application of a primer.

[0089] The pressure-sensitive adhesive layer of the pressure-sensitive adhesive sheet of the present embodiment contains the above-mentioned pressure-sensitive adhesive composition. The thickness of the adhesive layer is preferably 1 to 100 μm, more preferably 2 to 80 μm, and even more preferably 5 to 50 μm. When the thickness of the adhesive layer is 1 μm or more, the thickness uniformity of the adhesive layer is good. On the other hand, when the thickness of the adhesive layer is 100 μm or less, even if the adhesive layer is formed using a solvent, the solvent can be easily removed, which is preferable.

[0090] When a release sheet is provided on the surface of the pressure-sensitive adhesive layer opposite to the substrate, a known sheet-like material can be appropriately selected and used as the release sheet. The release sheet can be the same as the above-mentioned resin sheet used as the substrate. The thickness of the release sheet can be appropriately selected depending on the application of the pressure-sensitive adhesive sheet, the material of the release sheet, etc. When a resin sheet is used as the release sheet, the thickness of the release sheet is, for example, preferably 5 to 300 μm, more preferably 10 to 200 μm, and even more preferably 25 to 100 μm.

[0091] The release surface of the release sheet (the surface that is placed in contact with the adhesive layer) may be subjected to a release treatment using a conventionally known release agent such as a silicone-based, long-chain alkyl-based, or fluorine-based release agent, if necessary.

[0092] [Method of manufacturing adhesive sheet] The pressure-sensitive adhesive sheet of the present embodiment can be produced, for example, by the method described below. First, the above-mentioned adhesive composition is dissolved or dispersed in a solvent to prepare an adhesive solution. The above-mentioned adhesive composition may be used as the adhesive solution as it is. Next, the adhesive solution is applied onto the substrate and dried by heating to form an adhesive layer, and then, if necessary, a release sheet is attached onto the adhesive layer to obtain the adhesive layer. Another method for producing the pressure-sensitive adhesive sheet of the present embodiment includes a method in which the above-mentioned pressure-sensitive adhesive solution is applied onto a release sheet, and the solution is dried by heating to form a pressure-sensitive adhesive layer, and then the release sheet having the pressure-sensitive adhesive layer is placed on a substrate with the surface of the pressure-sensitive adhesive layer facing the substrate, and the pressure-sensitive adhesive layer is transferred onto the substrate.

[0093] The above-mentioned adhesive solution can be applied to the substrate (or release sheet) by a known method.Specific examples of the method include coating using a conventional coater such as a gravure roll coater, a reverse roll coater, a kiss roll coater, a dip roll coater, a bar coater, a knife coater, a spray coater, a comma coater, or a direct coater.

[0094] [Uses of adhesive sheets] The adhesive sheet of this embodiment can be used as a removable adhesive sheet. The adhesive sheet of this embodiment can be used, for example, when manufacturing electronic components. Specifically, the adhesive sheet of this embodiment is used in each step of manufacturing electronic components, in which an adherend is fixed, subjected to various processing steps, and then irradiated with ultraviolet (UV) light to peel off the adherend and collect it. Therefore, the adhesive sheet of this embodiment can be used as a backgrind tape, dicing tape, etc. when processing a semiconductor wafer. In addition, the adhesive sheet of this embodiment can be suitably used as a support tape for fragile members such as ultrathin glass substrates, plastic films, flexible printed circuit boards (FPC boards), and other members that are prone to warping. In particular, the adhesive sheet of this embodiment is suitable as a dicing tape that protects a wafer when a wafer dicing process is performed.

[0095] When the adhesive sheet of this embodiment is used as a dicing tape for a wafer, the adhesive sheet is attached to a wafer on which a plurality of components are formed before a dicing process is performed. Next, the wafer is cut and cut (diced) into individual components to form element pieces (chips). Then, the adhesive sheet attached to each element piece is irradiated with UV light. As a result, the adhesive layer is irradiated with UV light through the base material of the adhesive sheet, and the unsaturated bonds in the adhesive form a three-dimensional crosslinked structure and harden. As a result, the adhesive strength of the adhesive layer is reduced. Then, the adhesive sheet is peeled off from each element piece.

[0096] Examples of light sources used when irradiating an adhesive sheet attached to an adherend with UV light before peeling include high-pressure mercury lamps, ultra-high-pressure mercury lamps, carbon arc lamps, xenon lamps, metal halide lamps, chemical lamps, and black lights. The UV irradiation dose applied to the adhesive sheet is 50 to 3000 mJ / cm 2 is preferably 100 to 600 mJ / cm 2 It is more preferable that the UV irradiation dose applied to the adhesive sheet is 50 mJ / cm. 2 When the amount of UV irradiation is 3000 mJ / cm or more, the adhesive layer is cured at a sufficiently high curing speed by UV irradiation, and the adhesive strength of the adhesive layer after UV irradiation is sufficiently small, which is preferable. 2 Even if you do this, you won't get the results you deserve. EXAMPLES

[0097] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to the following examples.

[0098] "Production of Resin (A)" (Production Example 1) [Preparation of first mixed solution] As shown in Table 1, a first mixed solution was prepared containing raw material monomers including 23.9 parts by mass of acrylic acid as a carboxy group-containing ethylenically unsaturated monomer (a), 71.8 parts by mass of n-butyl acrylate and 143.6 parts by mass of 2-ethylhexyl acrylate as ethylenically unsaturated monomers (d) copolymerizable with the above (a), and 0.1 part by mass of 2,2'-azobisisobutyronitrile as a polymerization initiator per 100 parts by mass of the raw material monomers of the carboxy group-containing resin (b).

[0099] [Preparation of second mixed solution] As shown in Table 1, a second mixed solution was prepared containing 59.8 parts by mass of 3,4-epoxycyclohexylmethyl methacrylate as the alicyclic epoxy group-containing ethylenically unsaturated compound (c), 0.6 parts by mass of tris(4-methylphenyl)phosphine (TPTP) as a catalyst, 100.0 parts by mass of n-butyl acetate and 91.1 parts by mass of toluene as a solvent, relative to a total of 100 parts by mass of the carboxy group-containing resin (b) and the alicyclic epoxy group-containing ethylenically unsaturated monomer (c).

[0100] In a four-neck flask equipped with a stirrer, a dropping funnel, a cooling tube, and a nitrogen inlet tube, 175.6 parts by mass of n-butyl acetate was charged as a solvent, and the temperature was raised to 80°C under a nitrogen gas atmosphere. Then, while maintaining the reaction temperature at 80°C±2°C, the first mixed solution was uniformly dropped into the four-neck flask over 4 hours, and after the dropping was completed, stirring was continued for another 6 hours at a temperature of 80°C±2°C to polymerize the carboxyl group-containing resin (b). Then, 0.15 parts by mass of 4-methoxyphenol was added as a polymerization inhibitor to the reaction system relative to a total of 100 parts by mass of the carboxyl group-containing resin (b) and the alicyclic epoxy group-containing ethylenically unsaturated monomer (c).

[0101] The reaction system to which 4-methoxyphenol had been added was heated to 100°C, and the second mixed solution was added dropwise over 0.5 hours. The mixture was then stirred at 100°C for 8 hours to synthesize resin (A-1), and then cooled to room temperature (23°C). Resin (A-1) was identified by nuclear magnetic resonance (NMR) analysis and found to be a compound represented by general formula (2-1). The repeating unit k in formula (1-1) in the compound represented by general formula (2-1) is R 5 There are two different repeating units (k-1, k-2).

[0102] [ka] (In formula (2-1), k-1 is 34, k-2 is 47, m is 1, and the sum of k-1, k-2, and m is 82. n is 18.)

[0103] The weight average molecular weight and glass transition temperature of the resin (A-1) were examined by the following methods. The acid value of the resin (A-1) was also measured according to JIS K0070. The results are shown in Table 3.

[0104] <Weight average molecular weight (Mw)> Measurements were performed at room temperature under the following conditions using gel permeation chromatography (Shodex (registered trademark) GPC-101, manufactured by Showa Denko KK), and calculations were made in terms of polystyrene. Column: Showa Denko K.K., Showdex (registered trademark) LF-804 Column temperature: 40℃ Sample: 0.2% by mass solution of resin (A) in tetrahydrofuran Flow rate: 1ml / min Eluent: Tetrahydrofuran Detector: RI detector

[0105] <Glass transition temperature (Tg)> A 10 mg sample was taken from the resin (A). Differential scanning calorimetry was performed using a differential scanning calorimeter (DSC) by changing the temperature of the sample from -100°C to 200°C at a heating rate of 10°C / min, and the endothermic start temperature due to the observed glass transition was taken as Tg. When two Tgs were observed, the simple average of the two Tgs was taken.

[0106] (Examples 2-8, 10-12) A first mixed solution was prepared in the same manner as in Production Example 1, except that the carboxyl group-containing ethylenically unsaturated monomer (a), the ethylenically unsaturated monomer (d), and the polymerization initiator were used in the amounts (parts by mass) shown in Tables 1 and 2. In addition, a second mixed solution was prepared in the same manner as in Production Example 1, except that an alicyclic epoxy group-containing ethylenically unsaturated compound (c) (glycidyl methacrylate (GMA) in Production Example 8) and a catalyst were used in the amounts (parts by mass) shown in Tables 1 and 2.

[0107] Resins (A-2) to (A-8) and (A-10) to (A-12) were obtained in the same manner as in Production Example 1, except that the first mixed solution and the second mixed solution were used. Resins (A-2) to (A-8), (A-10) to (A-12) were identified in the same manner as in Production Example 1, and were found to be compounds represented by general formulas (2-2) to (2-8), (2-10) to (2-12). The repeating unit k in formula (1-1) in the compounds represented by general formulas (2-2) to (2-8) and (2-10) is R 5 Or, R 1 and R 5 are two different repeating units (k-1, k-2).

[0108] The resin (A-2) is a compound represented by the following general formula (2-2). The resin (A-3) is a compound represented by the following general formula (2-3). The resin (A-4) is a compound represented by the following general formula (2-4). The resin (A-5) is a compound represented by the above general formula (2-5). The resin (A-6) is a compound represented by the following general formula (2-6). The resin (A-7) is a compound represented by the following general formula (2-7). The resin (A-8) is a compound represented by the following general formula (2-8). The resin (A-10) is a compound represented by the following general formula (2-10). The resin (A-11) is a compound represented by the following general formula (2-11). The resin (A-12) is a compound represented by the following general formula (2-12).

[0109] [ka] (In formula (2-2), k-1 is 32, k-2 is 48, m is 1, and the sum of k-1, k-2, and m is 81. n is 19.) (In formula (2-3), k-1 is 70, k-2 is 16, m is 1, and the sum of k-1, k-2, and m is 87. n is 13.)

[0110] [ka] (In formula (2-4), k-1 is 52, k-2 is 34, m is 3, and the sum of k-1, k-2, and m is 89. n is 11.) (In formula (2-5), k-1 is 11, k-2 is 52, m is 4, the sum of k-1, k-2, and m is 67, and n is 33.)

[0111] [ka] (In formula (2-6), k-1 is 56, k-2 is 24, m is 0.2, and the sum of k-1, k-2, and m is 80.2. n is 19.8.) (In formula (2-7), k-1 is 15, k-2 is 72, m is 1, and the sum of k-1, k-2, and m is 88. n is 12.)

[0112] [ka] (In formula (2-8), k-1 is 37, k-2 is 44, m is 2, and the sum of k-1, k-2, and m is 83. n' is 17.) (In formula (2-10), k-1 is 34, k-2 is 47, m is 4, and the sum of k-1, k-2, and m is 85. n is 15.)

[0113] [ka] (In formula (2-11), k is 66, l is 12, m is 2, and the sum of k, l, and m is 80. n is 20.) (In formula (2-12), k is 55, l is 23, m is 2, and the sum of k, l, and m is 80. n is 20.)

[0114] The weight average molecular weight, glass transition temperature, and acid value of each of the resins (A-2) to (A-8), (A-10), and (A-12) were examined in the same manner as for the photosensitive resin (A-1). The results are shown in Table 3.

[0115] (Production Example 9) A first mixed solution was prepared in the same manner as in Production Example 1, except that the carboxyl group-containing ethylenically unsaturated monomer (a), the ethylenically unsaturated monomer (d), and the polymerization initiator were used in the amounts (parts by mass) shown in Table 2.

[0116] A four-neck flask equipped with a stirrer, a dropping funnel, a cooling tube and a nitrogen inlet tube was charged with 261.7 parts by mass of ethyl acetate as a solvent, and heated under reflux. After heating under reflux, the first mixed solution shown in Table 2 was dripped uniformly over 4 hours, and after dripping, stirring was continued for 6 hours under heating under reflux. Thereafter, the reaction system was cooled to 60°C, and 286.4 parts by mass of ethyl acetate was added as a solvent, 0.15 parts by mass of 4-methoxyphenol was added as a polymerization inhibitor to a total of 100 parts by mass of the carboxyl group-containing resin (b) and 2-isocyanatoethyl methacrylate (MOI) described below, and 0.3 parts by mass of dioctyltin dilaurate was added as a catalyst to a total of 100 parts by mass of the carboxyl group-containing resin (b) and 2-isocyanatoethyl methacrylate (MOI) described below.

[0117] After 4-methoxyphenol was dissolved, 47.8 parts by mass of 2-isocyanatoethyl methacrylate (MOI) was added to the reaction system, and stirring was continued at 60° C. for 8 hours to synthesize resin (A-9), which was then cooled to room temperature (23° C.). Resin (A-9) was identified in the same manner as in Production Example 1, and was found to be a compound represented by general formula (2-9). The repeating unit k in formula (1-1) in the compound represented by general formula (2-9) is R5 There are two different repeating units (k-1, k-2).

[0118] [ka] (In formula (2-9), k-1 is 48, k-2 is 32, m is 1, and the sum of k-1, k-2, and m is 81. j is 2, and n'' is 17.)

[0119] The weight average molecular weight, glass transition temperature, and acid value of Resin (A-9) were examined in the same manner as Resin (A-1), and the results are shown in Table 3. In addition, for resins (A-1) to (A-12), the values ​​of k-1, k-2, k (the sum of k-1 and k-2), l, m, n, n', and n'' in chemical formulas (2-1) to (2-12) are shown in Table 3.

[0120] [Table 1]

[0121] [Table 2]

[0122] [Table 3]

[0123] Tables 1 and 2 show the types and amounts (parts by mass) of the carboxyl group-containing ethylenically unsaturated monomer (a), the ethylenically unsaturated monomer (d) copolymerizable with (a), the polymerization initiator, the alicyclic epoxy group-containing ethylenically unsaturated compound (c), the catalyst, the polymerization inhibitor and the solvent used in the production of the resins (A-1) to (A-12), and the amounts (parts by mass) of glycidyl methacrylate (GMA) and 2-isocyanatoethyl methacrylate (MOI), respectively.

[0124] "Examples 1 to 12, Comparative Examples 1 to 2" Ethyl acetate, a solvent, was added to the reaction solution of resins (A-1) to (A-12) synthesized in Production Examples 1 to 12 so that the content of each of resins (A-1) to (A-12) was adjusted to 30 mass%. A pressure-sensitive adhesive composition was obtained by the method described below using the resin (A-1) to (A-12) solution in which the content of resins (A-1) to (A-12) was 30 mass%.

[0125] In a room shielded from actinic radiation, the resin (A), photopolymerization initiator (B) and crosslinking agent (C) shown in Tables 4 to 6 were added to a plastic container in the amounts (parts by mass) shown in Tables 4 to 6, respectively, and stirred to obtain pressure-sensitive adhesive compositions of Examples 1 to 12 and Comparative Examples 1 and 2. The numerical values ​​of resins (A-1) to (A-12) in Tables 4 to 6 are the amounts (parts by mass) of resin (A-1) to (A-12) solutions in which the content of resin (A-1) to (A-12) is 30% by mass. The numerical value of photopolymerization initiator (B) is the amount (parts by mass) of photopolymerization initiator (B) used relative to 100 parts by mass of resin (A). The numerical value of crosslinking agent (C) is the amount (parts by mass) of crosslinking agent (C) used relative to 100 parts by mass of resin (A).

[0126] [Table 4]

[0127] [Table 5]

[0128] [Table 6]

[0129] "TETRAD-C", "HX", and "TPO" in Tables 4 to 6, and "TETRAD-X" in Tables 4 and 5 are as follows: "TETRAD-C" 1,3-bis(N,N-diglycidylaminomethyl)cyclohexane (manufactured by Mitsubishi Gas Chemical Company, Inc., product name: TETRAD-C) "TETRAD-X" N,N'-[1,3-phenylenebis(methylene)]bis[bis(oxiran-2-ylmethyl)amine] (manufactured by Mitsubishi Gas Chemical Company, Inc., product name: TETRAD-X) "HX" isocyanurate of hexamethylene diisocyanate (manufactured by Tosoh Corporation, product name: Coronate (registered trademark) HX) "TPO" 2,4,6-trimethylbenzoyldiphenylphosphine oxide (manufactured by BASF, product name: L-TPO)

[0130] "Manufacturing of adhesive sheets" The adhesive compositions of Examples 1 to 12 and Comparative Examples 1 and 2 were directly coated onto a substrate so that the film thickness after drying was 20 μm, and the substrate was dried by heating at 100° C. for 2 minutes to form an adhesive layer. A release sheet was then attached onto the adhesive layer to obtain the adhesive sheets of Examples 1 to 12 and Comparative Examples 1 and 2. A polyethylene terephthalate (PET) film having a thickness of 50 μm was used as the substrate and the release sheet.

[0131] The adhesive sheets thus obtained of Examples 1 to 12 and Comparative Examples 1 and 2 were evaluated for the following items by the following methods. The results are shown in Tables 4 to 6.

[0132] "Peel strength before UV irradiation" The adhesive sheet was cut into a size of 25 mm length and 100 mm width, and the release sheet was peeled off to expose the adhesive layer. Next, the adhesive sheet was attached to a glass plate so that the exposed adhesive layer (measurement surface) was in contact with the glass plate, and a 2 kg rubber roller (width: about 50 mm) was rolled back and forth once to prepare a sample for measuring peel strength before UV irradiation. The obtained measurement sample was left for 24 hours in an environment of 23°C temperature and 50% humidity. After that, a tensile test was carried out in the 180° direction at a peel speed of 300 mm / min according to JIS Z0237, and the peel strength (N / 25 mm) of the pressure-sensitive adhesive sheet against the glass plate was measured.

[0133] "Peel strength after UV irradiation" Prepare a sample identical to the one used to measure peel strength before UV irradiation, and irradiate the adhesive sheet side with a dose of 500 mJ / cm 2 The specimens were irradiated with ultraviolet (UV) rays under the above conditions to prepare samples for measuring peel strength after UV irradiation. A conveyor-type UV irradiation device (manufactured by iGraphics, 2KW lamp, 80W / cm) was used for UV irradiation. For the obtained measurement sample, the peel strength (N / 25 mm) of the pressure-sensitive adhesive sheet to the glass plate was measured in the same manner as in "Peel strength before UV irradiation."

[0134] "Heat-resistant peel strength after UV irradiation" A sample identical to that used to measure the peel strength before UV irradiation was prepared, heat-treated by holding it at 200°C for 2 hours, then cooled to room temperature (23°C), and irradiated with UV under the same conditions as for "peel strength after UV irradiation" to obtain a sample for measuring the heat-resistant peel strength after UV irradiation. The peel strength (N / 25 mm) of the pressure-sensitive adhesive sheet against the glass plate of the obtained measurement sample was measured in the same manner as in "Peel strength after UV irradiation".

[0135] "Glue residue" After the peel strength was measured after UV irradiation, the glass plate was visually observed and evaluated according to the following criteria. The results are shown in Tables 4 to 6. (Evaluation Criteria) ○: No adhesive remains on the glass plate. △: Adhesive remained on part of the glass plate. ×: Adhesive remained on the entire surface of the glass plate.

[0136] As shown in Tables 4 and 5, the adhesive sheets of Examples 1 to 12 all had a "pre-UV peel strength" of 1.0 N / 25 mm or more, a "heat-resistant post-UV peel strength" of less than 2.5 N / 25 mm, and the adhesive residue was rated as good or fair. In contrast, as shown in Table 6, the adhesive sheets of Comparative Example 1 and Comparative Example 2, in which the resin (A) does not contain a structure derived from an alicyclic compound, both had sufficiently low "peeling strength after UV irradiation" but high "heat-resistant peeling strength after UV irradiation," and were rated as × for adhesive residue.

Claims

1. A resin represented by the following general formula (1-1), having a weight average molecular weight of 200,000 to 1,000,000 and a glass transition temperature of -80 to 0°C. 【Chemistry 1】 【Chemistry 2】 (In formula (1-1), k, l, m, and n represent the molar composition ratio when k+l+m+n=100. k is greater than 0 and less than 92. l is 0 to 50. m is greater than 0 and less than 90. The sum of k, l, and m is 65 to 95. n is 5 to 35. R 1 ~R 4 is -H or -CH 3 It is. 5 is an alkyl group having 1 to 16 carbon atoms. 6 R is a group having 6 to 20 carbon atoms containing an alicyclic hydrocarbon group having 3 to 30 carbon atoms or an aromatic hydrocarbon group. 7 is -H or -(CH 2 ) j -COOH (where j is 1 or 2). R8 is the above general formula (1-2) or (1-3). In formulas (1-2) and (1-3), p and q are any one selected from 0, 1, and 2. s is 0 when p is 0, and is 1 when p is 1 or 2. R 9 is -H or -CH 3 It is.)

2. The resin according to claim 1, wherein n in the formula (1-1) is 10 to 33.

3. The resin according to claim 1, characterized in that, in the formula (1-1), k is 45 to 90, l is 4 to 40, and m is 1 to 15.

4. an addition reaction product of a carboxyl group-containing resin (b) and an alicyclic epoxy group-containing ethylenically unsaturated compound (c), The carboxyl group-containing resin (b) 2. The resin according to claim 1, which is a polymer of an ethylenically unsaturated monomer including a carboxyl group-containing ethylenically unsaturated monomer (a).

5. 5. The resin according to claim 4, wherein the carboxyl group-containing ethylenically unsaturated monomer (a) is at least one selected from the group consisting of (meth)acrylic acid and β-carboxyethyl (meth)acrylate.

6. The carboxyl group-containing resin (b) The resin according to claim 4 or claim 5, which is obtained by copolymerizing raw material monomers including at least the carboxyl group-containing ethylenically unsaturated monomer (a) and the carboxyl group-containing ethylenically unsaturated monomer (d) copolymerizable with the carboxyl group-containing ethylenically unsaturated monomer (a).

7. 7. The resin according to claim 6, wherein the ethylenically unsaturated monomer (d) is at least one selected from the group consisting of isobornyl (meth)acrylate and benzyl (meth)acrylate.

8. The resin according to claim 4 or 5, wherein the alicyclic epoxy group-containing ethylenically unsaturated compound (c) is 3,4-epoxycyclohexylmethyl methacrylate.

Citation Information

Patent Citations

  • printer

    JP1984096985A

  • Polymer having unsaturated group in side chain and its production

    JP1998087725A

  • Production of curable resin and composition containing curable resin

    JP2000072814A

  • Photo-sensitive paste and production of display material using the same

    JP2000204130A

  • Polyfunctional (METH)acrylic acid ester, method for producing the same, active energy ray-curable type (METH)acrylic acid ester resin composition, and its cured product

    JP2005002064A