Friction stir welded joint
By controlling the dislocation density ratio and post-heating conditions, the joint efficiency of friction stir welded ferrite-based steel plates is enhanced, addressing the ductility issues in conventional methods.
Patent Information
- Application Number
- JP2024544855
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2023-07-25
- Filing Date
- 2024-05-27
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2044-05-27
AI Technical Summary
Conventional friction stir welding methods fail to achieve sufficient joint efficiency when using ferrite-based steel plates due to microscopic dislocations that reduce ductility and lead to fractures.
Control the average dislocation density ratio (Dw/Dm) between the joint and base material to ensure it satisfies Dw/Dm ≦ 10.0, with both materials having a ferrite area ratio of 80% or more, and specific compositional limits for C, Si, Al, and Mn, followed by post-heating under controlled temperature and cooling rates.
Achieves excellent joint efficiency and manufacturability for friction stir welded joints using ferrite-based steel plates by minimizing dislocation-induced ductility loss.
Smart Images

Figure 0007568177000002 
Figure 0007568177000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a friction stir welded joint. [Background technology]
[0002] In friction stir welding, for example, double-sided friction stir welding, the workpieces are joined as follows. That is, a pair of rotating tools are placed on the front and back sides of the workpieces having at least two or more metal plates. Then, the rotating tools are pressed against the front and back sides of the workpieces, respectively, and moved in the joining direction while rotating the rotating tools. As a result, the metal plates are softened by frictional heat between the rotating tool and the workpieces, and the softened parts are stirred by the rotating tool. Then, plastic flow is generated in the area of the workpieces that will become the joint, and the workpieces are joined. Hereinafter, the area where the workpieces are butted or overlapped and not yet joined is referred to as the "unjoined area", and the area that has been joined and integrated is referred to as the "joined area".
[0003] As a technique related to such friction stir welding, for example, Patent Document 1 describes: "A friction stir welding method, characterized in that, when two steel sheets are butted against each other or overlapped and friction stir welded, the friction stir welding is performed by setting the rotation speed R of a tool rotating in the friction stir welding to more than 5 rpm and less than 5,000 rpm, setting the leading edge temperature T of the steel sheet contacting the leading edge in the moving direction of the tool to 25°C or higher, setting the shoulder diameter D of the tool to 8 to 40 mm, and setting the welding speed V accompanying the moving direction of the tool to 0.1 to 5 m / min." has been disclosed. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2019-166569 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, in the conventional friction stir welding method such as that described in Patent Document 1, when a steel plate having a metal structure mainly composed of ferrite (hereinafter also referred to as a steel plate mainly composed of ferrite) is used as a welded material, sufficient joint efficiency cannot be obtained. Therefore, improvement in this respect is currently desired.
[0006] The present invention was developed in consideration of the above-mentioned current situation, and aims to provide a friction stir welded joint in which a steel plate mainly composed of ferrite is used as a welded material (in other words, the base material has a metal structure mainly composed of ferrite) and which has excellent joint efficiency. Note that in this specification, any numerical range expressed using "to" means a range that includes the numerical values written before and after "to" as the lower limit and upper limit, respectively. [Means for solving the problem]
[0007] The inventors have conducted extensive research to achieve the above object. First, the inventors investigated the reason why a friction stir welded joint using a ferrite-based steel plate as the welded material cannot have excellent joint efficiency in a conventional friction stir welding method. Specifically, the inventors performed friction stir welding under various conditions using various materials as the welded material, and analyzed the obtained friction stir welded joints by tensile tests and electron backscatter diffraction measurements (hereinafter also referred to as EBSD measurements).
[0008] As a result, the inventors have found the following: That is, the ductility of the welded joint of a friction stir welded joint is microscopically reduced due to microscopic dislocations introduced into the metal structure of the welded joint during friction stir welding. This microscopic reduction in ductility makes the welded joint more susceptible to fracture, in other words, leads to a reduction in joint efficiency.
[0009] The inventors consider the above reasons as follows. That is, in a metal structure mainly composed of ferrite, the hardness distribution does not usually change significantly. However, when a region with low ductility exists microscopically in a metal structure mainly composed of ferrite, fracture occurs due to the lack of ductility in that region. This microscopic decrease in ductility is largely due to an increase in microscopic dislocations at the joint introduced by heat treatment, processing, etc. Also, macroscopically, the mismatch between the joint and the base material also has an effect.
[0010] In addition, the inventors considered that the amount of microscopic dislocations introduced in the joint may be correlated with the average characteristics of the matrix, based on the above findings and the fact that the ferrite grains in the joint of the friction stir welded joint are fine. Based on this idea, the inventors conducted further studies to quantify the amount of microscopic dislocations introduced in the joint. As a result, the inventors found that when the average dislocation density of the joint is greater than the average dislocation density of the base material by a certain amount, the ductility of the joint of the friction stir welded joint decreases, leading to a decrease in joint efficiency.
[0011] Based on the above findings, the inventors conducted further studies and obtained the following findings: By appropriately controlling the ratio of the average dislocation density of the weld to the average dislocation density of the base material, a friction stir welded joint having excellent joint efficiency can be obtained even when the welded material is a steel plate mainly composed of ferrite. The present invention was completed based on the above findings and through further investigation.
[0012] That is, the gist and configuration of the present invention are as follows. A friction stir welded joint having a base material having a thickness of 1.2 or more and a joint between the base materials, The area ratio of ferrite in the base material and the area ratio of ferrite in the joint are both 80% or more, A friction stir welded joint that satisfies the following formula (1). Dw / Dm≦10.0 (1) Where: Dw: Average dislocation density at the joint ( / m 2 ) Dm: Average dislocation density of the base material ( / m 2 ) It is.
[0013] 2. The friction stir welded joint according to 1 above, wherein the base metal has a composition, in mass%, of C: 0.1% or less, Si: 2.0 to 8.0%, Al: 2.0% or less, and Mn: 1.0% or less.
[0014] 3. The average dislocation density of the joint is 1.0 x 10 16 / m 2 3. The friction stir welded joint according to claim 1 or 2, which is as follows:
[0015] 4. The friction stir welded joint according to any one of 1 to 3 above, which is a double-sided friction stir welded joint. Effect of the Invention
[0016] According to the present invention, a friction stir welded joint having excellent joint efficiency can be obtained when a steel plate mainly composed of ferrite is used as a weld material. The friction stir welded joint of the present invention is also advantageous in terms of manufacturability. [Brief description of the drawings]
[0017] [Figure 1] This is an example of the KAM diagram of the base material and the joint obtained by EBSD measurement. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] The present invention will be described based on the following embodiments. First, a friction stir welded joint according to one embodiment of the present invention will be described.
[0019] As described above, a friction stir welded joint according to one embodiment of the present invention has two or more base materials and a joint between the base materials (a joint that joins the base materials together).
[0020] [Base material] The base materials have a metal structure mainly composed of ferrite, specifically, a metal structure in which the area ratio of ferrite is 80% or more. Each base material is composed of each steel plate to be joined.
[0021] The area ratio of ferrite in the base material is 80% or more, preferably 90% or more. The area ratio of ferrite in the base material may be 100%. The area ratio of the remaining structure other than ferrite in the base material is 20% or less, preferably 10% or less, and more preferably 5% or less. Examples of the remaining structure other than ferrite include bainite, martensite, sulfides, nitrides, and carbides. The area ratio of the remaining structure in the base material may be 0%.
[0022] The area ratio of ferrite in the base material is measured as follows. That is, a test piece is taken from the base material. Next, the observation surface of the test piece is polished and then etched with 3 vol.% nital (a solution of nitric acid and ethanol) to reveal the structure. Next, an image is taken with an optical microscope at a magnification of 40 to 500 times. The total area of the observation area is preferably 50 μm square (50 μm × 50 μm) or more. Next, the area of ferrite is calculated from the obtained structure image using Adobe Photoshop of Adobe Systems. Next, the area of ferrite calculated for each field of view is divided by the total area of the observation area, and the value multiplied by 100 is taken as the area ratio of ferrite. The area ratio of ferrite can also be obtained by EBSD measurement.
[0023] The composition of the base material may be, in mass%, C: 0.1% or less, Si: 2.0 to 8.0%, Al: 2.0% or less, and Mn: 1.0% or less, with the remainder being Fe and unavoidable impurities. The unavoidable impurities are, for example, P: 0.2% or less, S: 0.01% or less, and N: 0.01% or less. The above composition may optionally contain, in mass%, at least one selected from the group consisting of Cr: 1% or less, Ni: 1% or less, Cu: 1% or less, Sn: 0.2% or less, Sb: 0.2% or less, Ca: 0.01% or less, REM: 0.05% or less, and Mg: 0.01% or less. Note that all elements other than Si and Fe may be 0 mass%. The Si content is more preferably 5.0 mass% or less. The C content is more preferably 0.001 mass% or more. The Mn content and the Al content are each more preferably 0.01 mass % or more. Furthermore, the thickness of the base material 1 is preferably 0.2 to 3.2 mm.
[0024] The number of base materials joined at one joint may be 2 or more. The number of base materials joined at one joint may be, for example, 2, or may be 3 to 5. Furthermore, the base materials joined at one joint may be the same or different in steel type and thickness as long as they are steel plates mainly composed of ferrite.
[0025] [Joint] The weld is an area that has been recrystallized by hot working due to the frictional heat between the rotating tool and the welded materials and the plastic flow. The weld also has a metal structure mainly composed of ferrite, specifically, a metal structure with an area ratio of ferrite of 80% or more.
[0026] The area ratio of ferrite in the joint is 80% or more, preferably 90% or more. The area ratio of ferrite in the joint may be 100%. The area ratio of the remaining structure other than ferrite in the joint is 20% or less, preferably 10% or less, and more preferably 5% or less. Examples of the remaining structure other than ferrite include martensite, sulfides, nitrides, and carbides. The area ratio of the remaining structure in the joint may be 0%.
[0027] The area ratio of ferrite in the joint is measured, for example, as follows. That is, the friction stir welded joint is cut in the thickness (vertical) direction so that the joint cross section (a surface including the weld vertical direction and the thickness direction of the friction stir welded joint, where the weld vertical direction is a direction perpendicular to both the weld direction and the thickness direction) is the cut surface. Then, a test piece is cut out so that the joint cross section of the joint is the observation surface. Then, the observation surface of the test piece is polished and etched with 3 vol.% nital to reveal the structure. Then, an image is taken with an optical microscope at a magnification of 40 to 500 times. The total area of the observation area is preferably 50 μm square (50 μm × 50 μm) or more. Then, the area of ferrite is calculated from the obtained structure image using Adobe Photoshop of Adobe Systems. Then, the area of ferrite calculated for each field of view is divided by the total area of the observation area, and the value multiplied by 100 is determined as the area ratio of ferrite. The area ratio of ferrite can also be determined by EBSD measurement or the like.
[0028] The base material and the joint can be defined, for example, as follows. That is, the friction stir welded joint is cut in the thickness (vertical) direction so that the cross section of the joint becomes the cut surface. The cut surface is then polished and etched with 3 vol.% nital. The cut surface is then observed under an optical microscope, and the base material and the joint are defined based on the degree of etching, etc.
[0029] In a friction stir welded joint according to one embodiment of the present invention, it is important to appropriately control the relative relationship between the average dislocation density of the weld and the average dislocation density of the base material, specifically, to satisfy the relationship of the following equation (1) regarding the ratio of the average dislocation density of the weld to the average dislocation density of the base material. Dw / Dm≦10.0 (1) Where: Dw: Average dislocation density at the joint ( / m 2 ) Dm: Average dislocation density of the base material ( / m 2 ) It is. In addition, when the average dislocation density differs depending on the base material, Dm is the minimum average dislocation density among the base materials joined by the joint.
[0030] As described above, microscopic dislocations introduced into the metal structure of the weld during friction stir welding can be quantified by the average dislocation density, and excellent joint efficiency can be obtained by controlling the relative relationship between the average dislocation density of the weld and the average dislocation density of the base material so as to satisfy the relationship of the above formula (1). Therefore, Dw / Dm≦10.0. Preferably, Dw / Dm≦5.0, and more preferably, Dw / Dm≦3.0. The lower limit of Dw / Dm is not particularly limited, and may be, for example, 1.0≦Dw / Dm.
[0031] Also, Dw is, for example, 1.0×10 16 / m 2 The preferred range is 1.0×10 13 / m 2 The above is preferred.
[0032] Here, the average dislocation density is calculated, for example, by performing EBSD measurement and using the following formula: D = 2KAMave÷(u×|b|) During the ceremony, D: Average transition density ( / m 2 ) KAMave: Average value of KAM value u: Measurement interval (m) b: Burgers vector (m) It is. For example, the friction stir welded joint is cut in the thickness (vertical) direction so that the joint cross section becomes the cutting surface, and a test piece is cut out so that the joint cross section of the base material and the joint part become the observation surface. Then, EBSD measurement is performed to obtain local crystal orientation data of the base material and the joint part. The measurement interval (step size) is preferably 0.1 to 20 μm. Also, each measurement area is preferably 50 μm square (50 μm × 50 μm) or more. Next, from the analysis result of the local crystal orientation data, the KAM value (average value of the orientation difference between the measurement point and all the adjacent measurement points) is obtained for each measurement point, and the KAMave, which is the average value of these, is calculated for the base material and the joint part, respectively. Then, the average dislocation density of the base material and the joint part is obtained. For reference, Figure 1 shows an example of the KAM diagram of the base material and the joint part obtained by EBSD measurement for a friction stir welded joint obtained by friction stir welding according to a conventional method using a steel plate mainly composed of ferrite as the welded material.
[0033] The friction stir welded joint may be a single-sided friction stir welded joint, but a double-sided friction stir welded joint is preferable. Here, the single-sided friction stir welded joint is a joint in which the workpieces are welded by single-sided friction stir welding in which a rotary tool is placed on one side of the workpieces. That is, the single-sided friction stir welded joint has a bead only on one of the welded surfaces in the thickness direction. Moreover, the double-sided friction stir welded joint is a joint in which the workpieces are welded by double-sided friction stir welding in which a rotary tool is placed on both the front and back sides of the workpieces. That is, the double-sided friction stir welded joint has beads on both of the welded surfaces in the thickness direction.
[0034] Moreover, the friction stir welded joint according to one embodiment of the present invention may be a butt joint or a lap joint.
[0035] Furthermore, in the friction stir welded joint according to one embodiment of the present invention, another base material may be joined to the above-mentioned base material via another joint. The type of the other joint is not particularly limited.
[0036] Moreover, a friction stir welded joint according to one embodiment of the present invention can be manufactured, for example, as follows.
[0037] First, two or more ferrite-based steel sheets, specifically steel sheets having a metal structure with a ferrite area ratio of 80% or more, are prepared as the materials to be joined. Here, the materials to be joined constitute the base material after joining, and the metal structure, component composition, thickness, etc. are the same as those of the base material described above. Therefore, the explanation will be omitted here.
[0038] Next, the workpieces are joined by friction stir welding. The joining conditions are not particularly limited, and may be the same as those used in the past.
[0039] Examples of joining methods include butt joining and lap joining. In butt joining, the end faces of the materials to be joined are placed opposite each other, and a rotating tool is pressed against the butt portion including the end faces (butt surfaces) of the materials to be joined while rotating. Then, in this state, the rotating tool is moved in the joining direction to join the materials to be joined. In lap joining, at least a portion of the ends of the materials to be joined are overlapped, and the rotating tool is pressed against the overlap portion while rotating. Then, in this state, the rotating tool is moved in the joining direction to join the materials to be joined.
[0040] Next, in order to satisfy the relationship of the above formula (1), the friction stir welded joint obtained as described above is post-heated under the following conditions. Average heating rate in the temperature range of 100 to 700°C (hereinafter referred to as heating rate): 30 to 300°C / sec Maximum temperature reached: 710~1200℃ Holding time at maximum temperature (hereinafter referred to as holding time): 0.1 to 10 seconds Average cooling rate in the temperature range of 700 to 100°C (hereinafter referred to as cooling rate): 30 to 300°C / sec In addition, all of the temperatures mentioned here are based on the surface temperature of the welded portion of the friction stir welded joint. It is preferable to control the heating rate, holding time, and cooling rate within the above ranges on both sides of the welded portion of the friction stir welded joint.
[0041] The method of post-heating is not particularly limited, and examples thereof include high-frequency induction heating, laser irradiation, and gas heating. Furnace heating may also be used.
[0042] The other conditions than those mentioned above are not particularly limited, and may be those according to conventional methods. EXAMPLES
[0043] Two steel plates having the above-mentioned preferred composition (in mass%, C: 0.1% or less, Si: 2.0 to 8.0%, Al: 2.0% or less, and Mn: 1.0% or less, and further containing at least one selected from the group consisting of Cr: 1% or less, Ni: 0.5% or less, Cu: 0.5% or less, Sn: 0.2% or less, Sb: 0.2% or less, Ca: 0.01% or less, REM: 0.05% or less, and Mg: 0.01% or less, with the remainder being Fe and unavoidable impurities) as the material to be welded, and having a thickness of 2.0 mm were butted together, and friction stir welding was performed on both sides under the conditions shown in Table 1 to obtain a friction stir welded joint. Next, post-heating was performed on the friction stir welded joint under the conditions shown in Table 1. Conditions not specified were as described above or in accordance with the usual method. In either case, the bonding conditions and post-heating conditions were almost the same for both sides, so Table 1 lists only one side as a representative example.
[0044] For the friction stir welded joints thus obtained, the ferrite area ratios of the base metals and the welded joints, and Dw / Dm were determined in the manner described above. The results are shown in Table 1. In Table 1, when the ferrite area ratios of the base metals welded at one welded joint differ, the value with the smaller ferrite area ratio is shown as a representative.
[0045] The obtained friction stir welded joints were also evaluated for joint efficiency. In the evaluation of joint efficiency, joint efficiency (= fracture strength of joint / fracture strength of base material x 100) of over 90% was evaluated as "excellent," and joint efficiency of 90% or less was evaluated as "poor." The results are shown in Table 1.
[0046] Here, the fracture strength of the joint was measured as follows. That is, a test piece of the same shape as the No. 1 test piece specified in JIS Z 3121 (2013) was taken from the obtained friction stir welded joint so that the welding direction and thickness direction were perpendicular to the longitudinal direction of the test piece and the joint was located at the center of the parallel part. Next, a tensile test in accordance with JIS Z 3121 (2013) was performed using the taken test piece to determine the maximum test force (N). The determined maximum test force (N) was then multiplied by the cross-sectional area (mm 2 ) was used as the breaking strength of the joint.
[0047] The breaking strength of the base material can also be referred to as the tensile strength (TS) of the base material (the material to be joined). In other words, the breaking strength of the base material can be measured by conducting a tensile test in accordance with JIS Z 2241 (2022). For example, a JIS No. 5 test piece is taken from the base material or the same material as the base material. Then, a tensile test is conducted using the taken test piece at a crosshead speed of 10 mm / min to measure the tensile strength (TS). When the breaking strength differs depending on the base material, the maximum breaking strength of each base material is used in the evaluation of joint efficiency.
[0048] [Table 1]
[0049] As shown in Table 1, in the inventive examples, a friction stir welded joint having excellent joint efficiency was obtained when the welded materials were steel plates mainly composed of ferrite. On the other hand, in the comparative examples, sufficient joint efficiency was not obtained.
[0050] In addition, in friction stir welded butt joints and lap joints (i.e., the area ratio of ferrite in the base material and the area ratio of ferrite in the welded joint are both 80% or more) using various ferrite-based steel plates (various steel plates having the above-mentioned preferred composition and thickness: 0.2 to 3.2 mm) that were separately prepared, excellent joint efficiency was obtained similarly to the above, when Dw / Dm satisfied the above formula (1).
Claims
1. A friction stir welded joint having two or more base materials and a joint between the base materials, The area ratio of ferrite in the base material and the area ratio of ferrite in the joint are both 80% or more, A friction stir welded joint that satisfies the following formula (1). Dw / Dm≦10.0 (1) Where: Dw: Average dislocation density of the joint ( / m 2 ) Dm: average dislocation density of the base material ( / m 2 ) It is.
2. 2. The friction stir welded joint according to claim 1, wherein the composition of the base material is, in mass%, C: 0.1% or less, Si: 2.0 to 8.0%, Al: 2.0% or less, and Mn: 1.0% or less.
3. The average dislocation density of the joint is 1.0×10 16 / m 2 3. The friction stir welded joint according to claim 1 or 2, wherein:
4. 3. The friction stir welded joint according to claim 1 or 2, which is a double-sided friction stir welded joint.
5. The friction stir welded joint according to claim 3, which is a double-sided friction stir welded joint.
Citation Information
Patent Citations
Friction agitation joint method of metal
JP2015057292A
Article of manufacture having a sub-surface friction stir welded channel
US20110240372A1
Friction stir welding method for electromagnetic steel strip and method for manufacturing electromagnetic steel strip
WO2023100420A1
Friction agitation welding method
JP2019166569A
Cited By
Friction stir welding method and friction stir welding apparatus
US20260084233A1