Friction stir welding method, friction stir welding apparatus, and method for manufacturing welded members
The friction stir welding method addresses roll scratches in high-Si steel plates by controlled burr removal and heating, maintaining joint efficiency through precise thickness and temperature management.
Patent Information
- Application Number
- JP2024544856
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2023-07-25
- Filing Date
- 2024-05-27
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2044-05-27
AI Technical Summary
Friction stir welding of high-Si steel plates results in roll scratches due to burrs and hardened structures at the joint, leading to decreased joint efficiency.
A friction stir welding method that includes surface treatment to remove burrs, heating to control deformation strain, and specific temperature and thickness reduction limits to maintain joint efficiency, using a device comprising pre-surface processing, joining, surface processing, and heating devices.
Prevents roll scratches and achieves excellent joint efficiency by controlling burr removal and heating conditions, ensuring the hardness of the surface layer region matches the base material's hardness range.
Smart Images

Figure 0007568178000002 
Figure 0007568178000003 
Figure 0007568178000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a friction stir welding method, a friction stir welding apparatus, and a method for manufacturing a welded member. [Background technology]
[0002] In friction stir welding, for example, double-sided friction stir welding, the workpieces are joined as follows. That is, a pair of rotating tools are placed on the front and back sides of the workpieces having at least two or more metal plates. Then, the rotating tools are pressed against the front and back sides of the workpieces, respectively, and moved in the joining direction while rotating the rotating tools. As a result, the metal plates are softened by frictional heat between the rotating tool and the workpieces, and the softened parts are stirred by the rotating tool. Then, plastic flow is generated in the area of the workpieces that will become the joint, and the workpieces are joined. Hereinafter, the area where the workpieces are butted or overlapped and not yet joined is referred to as the "unjoined area", and the area that has been joined and integrated is referred to as the "joined area".
[0003] As a technique related to such friction stir welding, for example, Patent Document 1 describes: "A friction stir welding method, characterized in that, when two steel sheets are butted against each other or overlapped and friction stir welded, the friction stir welding is performed by setting the rotation speed R of a tool rotating in the friction stir welding to more than 5 rpm and less than 5,000 rpm, setting the leading edge temperature T of the steel sheet contacting the leading edge in the moving direction of the tool to 25°C or higher, setting the shoulder diameter D of the tool to 8 to 40 mm, and setting the welding speed V accompanying the moving direction of the tool to 0.1 to 5 m / min." has been disclosed. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2019-166569 A Summary of the Invention [Problem to be solved by the invention]
[0005] Incidentally, in steel sheet production lines, for example, production lines for pickling, cold rolling, annealing, plating, etc., it is common to perform so-called coil joining before threading a steel sheet (steel strip) in order to improve productivity and increase yield. Here, coil joining refers to joining an end (rear end) of a preceding steel sheet or steel strip (hereinafter also referred to as a preceding steel sheet) and an end (front end) of a following steel sheet (hereinafter also referred to as a following steel sheet) as joined materials in the production line.
[0006] Resistance seam welding and laser welding are generally used for coil joining. In recent years, the use of friction stir welding for coil joining has also been considered. However, when coil joining is performed by friction stir welding on steel sheets with a Si content of 2.0 to 12.0 mass % (hereinafter also referred to as high-Si steel sheets), such as electromagnetic steel sheets, equipment defects may occur. Specifically, scratches may occur on the rolls through which the steel sheets pass downstream of the joining process (hereinafter simply referred to as roll scratches or roll scratches). Therefore, improvements in this regard are currently desired.
[0007] The present invention has been developed in view of the above-mentioned current situation, and aims to provide a friction stir welding method that can prevent the occurrence of roll scratches and obtain excellent joint efficiency even when a high-Si steel plate is used as the welded material. The present invention also aims to provide a friction stir welding apparatus that can be suitably used for the above-mentioned friction stir welding method. Furthermore, the present invention also aims to provide a manufacturing method for welded members. In this specification, any numerical range expressed using "~" means a range that includes the numerical values written before and after "~" as the lower limit and upper limit, respectively. [Means for solving the problem]
[0008] The inventors have conducted extensive research to achieve the above object. First, the inventors investigated the cause of roll marks when high-Si steel sheets are used as the joined materials. As a result, the inventors found that roll marks are caused by burrs at the joint that are generated during friction stir welding. In particular, when high-Si steel sheets are used as the joined materials, the hardness of the burrs at the joint increases, and even if even a small amount of burrs remain, roll marks are generated.
[0009] Based on the above findings, the inventors attempted to prevent the occurrence of roll scratches by removing burrs at the joint by grinding, etc. However, in this case, the joint efficiency was significantly reduced.
[0010] Therefore, the inventors have conducted extensive research into the above-mentioned causes and further investigated the problem in order to achieve the intended object. As a result, the following findings have been obtained. (1) In the process of removing burrs, a deformed structure is formed in the joint. In particular, if a hardened phase, i.e., a structure with reduced ductility compared to the base material, exists in the region from the surface to 1 / 10 of the thickness position in the joint of the joined components (hereinafter also referred to as the surface layer region of the joint), defects will occur in the structure. Then, cracks will occur starting from the defects, reducing the joint efficiency. (2) In order to prevent roll damage and obtain excellent joint efficiency, it is important to simultaneously satisfy the following points: In the surface processing process, which is the process of removing burrs, the maximum thickness reduction of the joined parts is limited to 5.0% or less of the thickness of the joined materials. After the surface processing process, the joining parts are heated, and the heating conditions are appropriately controlled to reduce deformation strain in the surface area of the joint. The present invention was completed based on the above findings and through further investigation.
[0011] That is, the gist and configuration of the present invention are as follows. 1. A joining process in which a rotating tool is pressed against workpieces and the rotating tool is moved in a joining direction while being rotated to join the workpieces and obtain a joined member; Next, a surface processing step of performing a surface processing on the joining member; Next, a heating step of heating the joining member; having The joined material is a steel plate having a Si content of 2.0 to 12.0 mass%, The maximum thickness reduction of the joining member in the surface processing step is 5.0% or less of the thickness of the joined material, and The friction stir welding method, wherein the maximum temperature reached in the heating step is 400°C or higher and 1000°C or lower.
[0012] 2. The friction stir welding method according to 1 above, wherein the surface processing is carried out by grinding or pressing.
[0013] 3. The friction stir welding method according to 1 or 2 above, wherein the heating is performed by induction heating or resistance heating.
[0014] 4. After the heating step, the hardness of the surface layer region of the joint of the joint members is in the range of 95 to 115% of the hardness of the base material of the joint members; 4. The friction stir welding method according to any one of 1 to 3, wherein the surface layer region of the welded portion of the welded members is a region extending from the surface to a position corresponding to 1 / 10 of the thickness of the welded portion of the welded members.
[0015] 5. The friction stir welding method according to any one of 1 to 4 above, further comprising a preliminary surface treatment step of removing at least a region from the surface of the workpieces to a depth of 5 μm before the joining step.
[0016] 6. A friction stir welding apparatus used in the friction stir welding method according to any one of 1 to 4, A joining device that joins workpieces together to obtain a joined member; A surface processing device that processes the surface of the joining member; A heating device for heating the joining member; in the above order in a welding direction.
[0017] 7. A friction stir welding apparatus used in the friction stir welding method according to claim 5, A preliminary surface treatment device that performs preliminary surface treatment on the workpieces; a joining device for joining the workpieces to obtain a joined member; A surface processing device that processes the surface of the joining member; A heating device for heating the joining member; in the above order in a welding direction.
[0018] 8. A method for producing a welded member, comprising joining workpieces by the friction stir welding method according to any one of 1 to 5 above to obtain a welded member. Effect of the Invention
[0019] According to the present invention, even when high-Si steel sheets are used as materials to be joined, it is possible to prevent the occurrence of roll scratches and obtain excellent joint efficiency. [Brief description of the drawings]
[0020] [Figure 1] 1 is a schematic diagram showing an example of a friction stir welding method according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a schematic diagram showing an example of double-sided friction stir welding. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0021] The present invention will be described based on the following embodiments. [1]Friction stir welding method First, a friction stir welding method according to an embodiment of the present invention will be described. As shown in FIG. 1, a friction stir welding method according to an embodiment of the present invention includes the following steps: a joining process in which a rotating tool is pressed against workpieces and the rotating tool is moved in a joining direction while being rotated, thereby joining the workpieces to obtain a joined member; Next, a surface processing step of performing a surface processing on the joining member; Next, a heating step of heating the joining member; In Fig. 1, reference numeral 1 denotes a rotating tool (front surface side rotating tool), 3 denotes a material to be joined, 4 denotes a joining portion, 5 denotes a grinding device, and 6 denotes a heating device. Each of the above steps will be described below.
[0022] (Joining process) In the joining step, the rotating tool is pressed against the workpieces and moved in the joining direction while being rotated, thereby joining the workpieces to obtain a joined member.
[0023] The bonding conditions are not particularly limited and may be in accordance with conventional methods.
[0024] In addition, the joining method may be single-sided friction stir welding in which a rotary tool is placed on one side of the workpieces to be joined, or double-sided friction stir welding in which a rotary tool is placed on both the front and back sides of the workpieces to be joined.
[0025] To explain the double-sided friction stir welding as an example, as shown in FIG. 2, a pair of rotating tools are placed on the front side and the back side of the workpiece having at least two metal plates. Hereinafter, the rotating tool placed on the front side of the workpiece is referred to as the front side rotating tool. Also, the rotating tool placed on the back side of the workpiece is referred to as the back side rotating tool. In FIG. 2, reference numeral 1 denotes the rotating tool (front side rotating tool), 2 denotes the rotating tool (back side rotating tool), 3 denotes the workpiece, and 4 denotes the joint. Then, the pair of opposing rotating tools are pressed against the front and back sides of the workpiece, respectively, and the rotating tools are moved in the joining direction while rotating. That is, the front side rotating tool is pressed against the front side of the workpiece, and the back side rotating tool is pressed against the back side of the workpiece, respectively, and these rotating tools are moved in the joining direction while rotating. As a result, the metal plates are softened by the frictional heat between the rotating tool and the workpiece, and the softened part is stirred by the rotating tool. Then, plastic flow is generated in the region that will be the joint of the workpiece, and the workpiece is joined.
[0026] Examples of joining methods include butt joining and lap joining. In butt joining, the end faces of the materials to be joined are placed opposite each other, and a rotating tool is pressed against the butt portion including the end faces (butt surfaces) of the materials to be joined while rotating. Then, in this state, the rotating tool is moved in the joining direction to join the materials to be joined. In lap joining, at least a portion of the ends of the materials to be joined are overlapped, and the rotating tool is pressed against the overlapping portion while rotating. Then, in this state, the rotating tool is moved in the joining direction to join the materials to be joined.
[0027] (Surface processing process) In the surface processing step, burrs on the surfaces of the joined members that were generated in the joining step are removed. Note that the equipment on the back side is not shown in Fig. 1. In this process, it is important to suppress the amount of joined members that are removed together with the burrs, in particular to keep the maximum thickness reduction of the joined members to 5.0% or less of the thickness of the joined materials.
[0028] Maximum thickness reduction of joined materials: 5.0% or less of the thickness of the joined materials When a high-Si steel plate is used as a workpiece and friction stir welding is performed, and then burrs formed at the welded portion are removed, a structure with reduced ductility compared to the base material is formed in the surface layer region of the welded portion, and defects occur in the structure. Then, cracks occur starting from the defects, and the joint efficiency decreases. As described above, in order to suppress deformation strain in the region, it is effective to heat the welded members in the heating process described below and appropriately control the heating conditions. However, when the maximum thickness reduction amount of the welded members exceeds 5.0% of the thickness of the welded materials, that is, when the ratio of the maximum thickness reduction amount of the welded members to the thickness of the welded materials (=[maximum thickness reduction amount of the welded members (mm)] / [thickness of the welded materials (mm)]×100, hereinafter also referred to as the thickness reduction ratio of the welded members) exceeds 5.0%, the joint efficiency decreases due to thinning. In addition, even if the welded members are heated after the surface processing process, the deformation strain in the above region cannot be sufficiently reduced, and excellent joint efficiency cannot be obtained. Therefore, the thickness reduction ratio of the welded members is set to 5.0% or less. The thickness reduction ratio of the welded members is preferably 3.0% or less. In addition, as long as the burrs generated in the joining process can be removed, the thickness reduction ratio of the joined members is not particularly limited and may be 0%. From the viewpoint of sufficiently removing the burrs generated in the joining process and more reliably preventing the occurrence of roll scratches, the thickness reduction ratio of the joined members is preferably 1.0% or more.
[0029] Here, the maximum thickness reduction of the joined members is the maximum value of the thickness reduction in each area of the joined members that have been surface-treated. In the case of butt joining, the thickness of the joined materials is the thickness of each steel plate that will become the joined material. However, if the thicknesses of the steel plates that will become the joined materials are different, the thickness of the joined material is the average thickness of the steel plates that will become the joined materials. In the case of lap joining, the thickness is the thickness of the overlapping part of the joined materials (i.e., the total thickness of the steel plates that overlap at the overlapping part).
[0030] The surface processing method is not particularly limited. From the viewpoint of processing efficiency, the surface processing method is preferably grinding or rolling. In order to control the maximum thickness reduction of the joining members, it is preferable to check the surface condition (degree of burr, etc.) of the joining members before the surface processing, and then adjust the position and height of the surface processing.
[0031] In the joining step, when double-sided friction stir welding is performed, the above surface treatment is performed on both sides of the joining members. In the joining step, when single-sided friction stir welding is performed, the above surface treatment may be performed only on one side of the joining members (the side on which the rotary tool is placed (the side on which the bead is formed)), or the above surface treatment may be performed on both sides of the joining members. From the viewpoint of efficiency, the former is advantageous. In the case where the above surface treatment is performed on both sides of the joining members, the thickness reduction ratio of the joining members is controlled within the above range on both sides. In the heating step described later, similarly to the above, heating may be performed on one or both sides of the joining members depending on the joining method.
[0032] The other conditions than those mentioned above are not particularly limited, and may be those according to conventional methods.
[0033] (Heating process) In the heating step, the joining members are heated. As described above, when the high-Si steel plate is used as the joining material and friction stir welding is performed, and then the burrs formed at the joining portion are removed, a structure having reduced ductility compared to the base material is formed in the surface layer region of the joining portion, and defects are generated in the structure. Then, cracks are generated from the defects, and the joint efficiency is reduced. In order to reduce the deformation strain in the surface layer region of the joining portion, it is important to heat the joining members after removing the burrs, and to control the heating conditions as follows.
[0034] Maximum temperature reached: 400℃ or more and 1000℃ or less By setting the maximum temperature to 400°C or higher, the deformation strain in the surface layer region of the joint as described above is reduced, and excellent joint efficiency is obtained. However, if the maximum temperature exceeds 1000°C, the crystal grains become coarse. Therefore, the maximum temperature is set to 400°C or higher and 1000°C or lower. The maximum temperature is preferably 700°C or higher. Also, the maximum temperature is preferably 900°C or lower.
[0035] In addition, it is preferable that the heating step satisfies the following conditions, which more advantageously reduces the deformation strain in the surface layer region of the joint as described above and provides excellent joint efficiency. Average heating rate in the temperature range of 100 to 400°C (hereinafter referred to as heating rate): 10 to 300°C / sec Holding time at maximum temperature (hereinafter referred to as holding time): 0.1 to 10 seconds Average cooling rate in the temperature range of 400 to 100°C (hereinafter referred to as cooling rate): 10 to 300°C / sec
[0036] The temperatures here are all based on the surface temperature of the joint of the joining members. When one-sided friction stir welding is performed and the above surface processing is performed only on one side of the joining members (the side on which the rotary tool is placed (the side on which the bead is formed)), the maximum temperature is controlled to the above range at least on that side of the joining members. In this case, it is preferable to control the heating rate, holding time, and cooling rate to the above range on that side of the joining members. When double-sided friction stir welding is performed and the above surface processing is performed on both sides of the joining members, the maximum temperature is controlled to the above range on both sides of the joining members. In this case, it is preferable to control the heating rate, holding time, and cooling rate to the above range on both sides of the joining members.
[0037] The heating method is not particularly limited, but is preferably high-frequency induction heating or resistance heating (where electricity is passed between electrodes) from the viewpoint of heating efficiency.
[0038] The other conditions than those mentioned above are not particularly limited, and may be those according to conventional methods.
[0039] (Pre-surface processing process) In friction stir welding, if an oxide film or contaminants remain on the surface of the workpieces, the strength of the joint may be reduced. In order to avoid this, the friction stir welding method according to one embodiment of the present invention may optionally further include a pre-surface processing step of removing at least a region from the surface of the workpieces to a depth of 5 μm before the joining step. It is preferable that the removed region of the workpieces in the pre-surface processing step is a region from the surface of the workpieces to a depth of 50 μm at most. The pre-surface processing may be performed on only one side of the workpieces or on both sides of the workpieces, depending on the surface condition of the workpieces.
[0040] The surface processing method is not particularly limited, but is preferably grinding or polishing from the viewpoint of processing efficiency.
[0041] In addition, when the preliminary surface treatment is performed, the thickness of the joined materials, which is the denominator of the thickness reduction ratio of the joined members, is the thickness of the joined materials after the preliminary surface treatment. In other words, the thickness of the joined materials, which is the denominator of the thickness reduction ratio of the joined members, is the thickness of the joined materials provided in the joining process.
[0042] The other conditions than those mentioned above are not particularly limited, and may be those according to conventional methods.
[0043] (material to be joined) The material to be joined is a steel plate having a Si content of 2.0 to 12.0% by mass. The content of elements other than Si is not particularly limited. An example of the composition of such a steel plate is, in mass%, C: 0.1% or less, Si: 2.0 to 12.0%, Al: 2.0% or less, and Mn: 1.0% or less, with the balance being Fe and unavoidable impurities. The unavoidable impurities are, for example, P: 0.2% or less, S: 0.01% or less, and N: 0.01% or less. The above composition can optionally contain, in mass%, at least one selected from the group consisting of Cr: 1% or less, Ni: 1% or less, Cu: 1% or less, Sn: 0.2% or less, Sb: 0.2% or less, Ca: 0.01% or less, REM: 0.05% or less, and Mg: 0.01% or less. Note that all of the elements other than Si and Fe may be 0% by mass. The Si content is preferably 3.0 mass% or more. The Si content is preferably 8.0 mass% or less, more preferably 5.0 mass% or less. The C content is more preferably 0.001 mass% or more. The Mn content and the Al content are each more preferably 0.01 mass% or more. The steel plates used for the materials to be joined may be of the same steel type or different steel types. Furthermore, the thickness of each steel plate used for the materials to be joined is preferably 0.2 to 3.2 mm.
[0044] (Jointing material) A welded member obtained by the friction stir welding method according to one embodiment of the present invention has two or more base materials (workpieces to be welded) and a welded portion between the base materials (a welded portion that welds the base materials together). Here, each base material is constituted by a steel plate to be welded. The welded portion is a region that has been subjected to hot working due to frictional heat between a rotary tool and workpieces and plastic flow, and has a recrystallized structure. In addition, the hardness of the surface layer region of the welded portion of the welded member is preferably in the range of 95 to 115% of the hardness of the base material, and more preferably in the range of 100 to 110% of the hardness of the base material. In other words, the conditions of each of the above steps, particularly the conditions of the heating step, are controlled so that the hardness of the surface layer region of the welded portion of the finally obtained welded member is preferably in the range of 95 to 115% of the hardness of the base material, and more preferably in the range of 100 to 110% of the hardness of the base material.
[0045] Here, the surface layer region is a region from the surface to a position 1 / 10 the thickness of the joint of the joining members (depth (in the thickness direction) from the surface: a region up to 1 / 10 the thickness of the part). When one-sided friction stir welding is performed and the above-mentioned surface processing and heating are performed only on one side of the joining members (the side on which the rotary tool is placed (the side on which the bead is formed)), the hardness of the surface layer region of the joining part is preferably in the range of 95 to 115% of the hardness of the base material at least on that side of the joining part of the joining members, and more preferably in the range of 100 to 110% of the hardness of the base material. When two-sided friction stir welding is performed and the above-mentioned surface processing and heating are performed on both sides of the joining members, the hardness of the surface layer region of the joining part is preferably in the range of 95 to 115% of the hardness of the base material at both sides of the joining part of the joining members, and more preferably in the range of 100 to 110% of the hardness of the base material.
[0046] The hardness of the surface layer of the joint and the hardness of the base material are measured by a Vickers hardness test in accordance with JIS Z 2244 (2009). The test force is 100 gf.
[0047] Specifically, the joining members are cut in the thickness (vertical) direction so that the joint cross section (a surface including the joining vertical direction and the thickness direction of the joining members, where the joining vertical direction is a direction perpendicular to both the joining direction and the thickness direction) is the cut surface. Next, in the surface layer region of the joining part of the cut surface, starting from a position 50 μm deep from the surface of the joining part and 50 μm away from one of the boundaries between the base material and the joining part in the joining vertical direction (joint side), the Vickers hardness is measured under the above conditions at intervals of 50 μm in the thickness direction and 50 μm in the joining vertical direction in a lattice pattern. In addition, the Vickers hardness is measured under the above conditions at the center position of the thickness of the base material of the cut surface. Then, if the Vickers hardness measured in the surface layer region of the joining part of the cut surface is in the range of 95 to 115% of the Vickers hardness measured in the center position of the thickness of the base material of the cut surface, it is determined that the hardness of the surface layer region of the joining part is in the range of 95 to 115% of the hardness of the base material. In addition, when the Vickers hardness differs depending on the base material joined through the joint, the above judgment is made based on the Vickers hardness of each base material joined through the joint. For example, in a joint member in which a first base material and a second base material are joined through a joint, if the Vickers hardness measured in the surface layer region of the joint at the cut surface is in the range of 95 to 115% of the Vickers hardness measured at the thickness center of the first base material at the cut surface and is also in the range of 95 to 115% of the Vickers hardness measured at the thickness center of the second base material at the cut surface, the hardness of the surface layer region of the joint is judged to be in the range of 95 to 115% of the hardness of the base material.
[0048] The base material and the joint can be defined, for example, as follows. That is, the joint members are cut in the thickness (vertical) direction so that the joint cross section becomes the cut surface. The cut surface is then polished and etched with 3 vol.% nital (a solution of nitric acid and ethanol), a saturated aqueous solution of picric acid, or aqua regia (a solution of hydrochloric acid and nitric acid mixed in a volume ratio of 3:1). The cut surface is then observed under an optical microscope, and the base material and the joint are defined based on the degree of etching, etc.
[0049] The joining member may be a single-sided friction stir welded joint or a double-sided friction stir welded joint. Here, the single-sided friction stir welded joint is a joining member in which the workpieces are joined by single-sided friction stir welding in which a rotary tool is placed on one side of the workpieces. That is, the single-sided friction stir welded joint has a bead only on one surface of the joint. In the single-sided friction stir welded joint, it is preferable to control the conditions of each of the above steps, particularly the conditions of the heating step, so that the above-mentioned surface layer region is obtained on at least one surface side of the joint. In addition, the double-sided friction stir welded joint is a joining member in which the workpieces are joined by double-sided friction stir welding in which a rotary tool is placed on both the front and back surfaces of the workpieces. That is, the double-sided friction stir welded joint has beads on both surfaces of the joint. When the joining member is a double-sided friction stir welded joint, it is preferable to control the conditions of each of the above steps, particularly the conditions of the heating step, so that the above-mentioned surface layer region is obtained in the vicinity of both surfaces of the joint.
[0050] [2]Friction stir welding equipment Next, a friction stir welding apparatus according to an embodiment of the present invention will be described. A friction stir welding apparatus according to one embodiment of the present invention is a friction stir welding apparatus that can be suitably used in the friction stir welding method described above in [1], An optional pre-surface processing device for performing pre-surface processing on the workpieces; a joining device for joining the workpieces to obtain a joined member; A surface processing device that processes the surface of the joining member; A heating device for heating the joining member; In addition, if necessary, a surface shape measuring device may be provided between the bonding device and the surface processing device.
[0051] Here, the aspect of the preliminary surface processing device is not particularly limited as long as it can process the surfaces of the workpieces and partially remove the workpieces. Examples of the preliminary surface processing device include a grinding device such as a grinder, or a polishing device.
[0052] The embodiment of the welding apparatus is not particularly limited as long as it is an apparatus capable of performing friction stir welding. The welding apparatus includes, for example, a rotating tool and a driving device for the rotating tool.
[0053] The type of the surface profile measuring device is not particularly limited as long as it can confirm the degree of burrs on the surface of the joint of the joining members. Examples of the surface profile measuring device include a contact type (tracing the surface of the sample with a stylus) or a non-contact type (such as a laser) surface profile measuring device.
[0054] The embodiment of the surface processing device is not particularly limited as long as it can process the surface of the joined members and remove burrs on the surfaces of the joints of the joined members. Examples of the surface processing device include a grinding device such as a grinder, and a rolling device.
[0055] The embodiment of the heating device is not particularly limited. Examples of the heating device include an atmosphere furnace (a furnace that covers the entire joint and heats it with an atmosphere), and an induction heating device and a resistance heating device that heat locally without contact. In addition, it is preferable that the heating device has a device for measuring the surface temperature of the joint members, such as a thermograph.
[0056] In addition, the friction stir welding apparatus according to one embodiment of the present invention preferably has a drive device that moves the optional preliminary surface processing device, the welding device, the optional surface shape measuring device, the surface processing device, and the heating device together in the welding direction in accordance with the welding speed. This allows a series of steps to be performed continuously, which is extremely advantageous in terms of efficiency.
[0057] Other than the above, there are no particular limitations, and the device configuration may be the same as that of a conventionally known device.
[0058] [3] Manufacturing method for joining components Next, a method for manufacturing a joint member according to one embodiment of the present invention will be described. A method for manufacturing a welded member according to one embodiment of the present invention is to weld workpieces by the friction stir welding method described above in [1] to obtain a welded member. The welded member obtained is as described above in [1]. A specific example of the welded member obtained is a coil having a welded portion that joins a preceding steel sheet and a following steel sheet. Other conditions than those described above are not particularly limited and may be performed according to conventional methods. EXAMPLES
[0059] Two steel plates having the Si content and thickness shown in Table 1 as the materials to be joined were butted together, and friction stir welding was performed on both sides to obtain a joined member (joining process). In both cases, the conditions were a rotation speed of 1000 rpm and a joining speed of 2 m / min on both sides. For the rotary tools (front side rotary tool and back side rotary tool), a ceramic tool with a shoulder diameter (diameter of the shoulder part): 16 mm, a probe diameter (diameter of the probe): 8 mm, and a probe length: 1 mm was used. Next, surface processing was performed by grinding on both sides of the obtained joined member using a grinder with a width of 20 mm under the conditions shown in Table 1, and burrs were removed from the joint part of the joined member (surface processing process). Here, the maximum thickness reduction of the joined member was measured using a laser displacement meter. Next, the joined member was heated under the conditions shown in Table 1 (heating process). Here, heating was performed using an atmosphere furnace. In addition, the maximum temperature reached was measured by measuring the surfaces (both sides) of the joined member using thermography. Conditions not specified were as described above or in accordance with standard practice. No. 15 did not undergo a surface treatment process. No. 16 did not undergo a heating process. In both cases, the conditions for the surface treatment process and heating process, as well as the hardness of the surface layer region of the joint / hardness of the base material x 100, described below, were almost the same on both sides, so only one side is listed in Table 1. In addition, the prevention of roll scratches, described below, was confirmed on both sides of the joint of the joined parts.
[0060] For the thus obtained bonded members, the hardness of the surface layer region of the bonded portion and the hardness of the base material were measured in the above-mentioned manner, and it was judged whether the hardness of the surface layer region of the bonded portion was within the range of 95 to 115% of the hardness of the base material. The hardness of the surface layer region of the bonded portion / hardness of the base material x 100 is also shown in Table 1.
[0061] The joint efficiency of the obtained joint members was evaluated. In the evaluation of joint efficiency, joint efficiency (= breaking strength of joint part / breaking strength of base material x 100) of more than 95% was evaluated as "excellent", 95% or less and more than 90% was evaluated as "good", and 90% or less was evaluated as "poor". The results are shown in Table 1.
[0062] Here, the fracture strength of the joint was measured as follows. That is, a test piece of the same shape as the No. 1 test piece specified in JIS Z 3121 (2013) was taken from the obtained friction stir welded joint so that the welding direction and thickness direction were perpendicular to the longitudinal direction of the test piece and the joint was located at the center of the parallel part. Next, a tensile test in accordance with JIS Z 3121 (2013) was performed using the taken test piece to determine the maximum test force (N). The determined maximum test force (N) was then multiplied by the cross-sectional area (mm 2 ) was used as the breaking strength of the joint.
[0063] The breaking strength of the base material can also be called the tensile strength (TS) of the base material (the material to be joined). In other words, the breaking strength of the base material can be measured by conducting a tensile test in accordance with JIS Z 2241 (2022). For example, a JIS No. 5 test piece is taken from the base material or the same material as the base material. Then, a tensile test is conducted using the taken test piece at a crosshead speed of 10 mm / min to measure the tensile strength (TS). Note that if the breaking strength differs depending on the base material, the maximum breaking strength of each base material is used in the evaluation of joint efficiency.
[0064] In order to confirm the prevention of roll scratches, the joint of the joining member was pressed against a surface-polished high carbon chromium bearing steel (SUJ-2, hereinafter also referred to as bearing steel) (simulating a roll) and slid 100 times. At this time, the pressing pressure (pressure applied when the joint of the joining member was pressed against the bearing steel) was 400 MPa. Next, the presence or absence of scratches on the bearing steel was confirmed visually. If scratches were confirmed, the depth of the scratches was measured by cross-sectional observation using an optical microscope. Then, the prevention of roll scratches was evaluated according to the following criteria. The results are also shown in Table 1. Good: No scratches deeper than 50 μm were observed. Poor: Scratches with a depth of 50 μm or more were observed.
[0065] [Table 1]
[0066] As shown in Table 1, in all of the inventive examples, excellent joint efficiency was obtained while preventing the occurrence of roll marks. On the other hand, in the comparative examples, roll marks occurred or sufficient joint efficiency was not obtained.
[0067] In addition, even when the joining members were manufactured in the same manner as described above except for carrying out the preliminary surface treatment process, in all cases where the thickness reduction ratio of the joining members in the surface treatment process was 5.0% or less and the maximum temperature reached in the heating process was 400°C or higher and 1000°C or lower, excellent joint efficiency was obtained while preventing the occurrence of roll scratches.
[0068] Furthermore, even when various steel plates having the above-mentioned preferred component composition with a Si content of 2.0 to 12.0 mass% and a thickness of 0.2 to 3.2 mm were used as the joined materials and joined members were produced by butt joining or lap joining under various joining conditions, in all cases where the thickness reduction ratio of the joined members was 5.0% or less and the maximum temperature reached in the heating process was 400°C or higher and 1000°C or lower, excellent joint efficiency was obtained while preventing the occurrence of roll scratches. [Explanation of symbols]
[0069] 1 Rotation tool (front side rotation tool) 2 Rotation tool (reverse side rotation tool) 3 Material to be joined 4 Joint 5 Grinding equipment 6 Heating device
Claims
1. a joining process in which a rotating tool is pressed against workpieces and the rotating tool is moved in a joining direction while being rotated, thereby joining the workpieces to obtain a joined member; Next, a surface processing step of performing a surface processing on the joining member; Next, a heating step of heating the joining member; having The joined material is a steel plate having a Si content of 2.0 to 12.0 mass %, The maximum thickness reduction of the joining member in the surface processing step is 5.0% or less of the thickness of the joined material, and The friction stir welding method, wherein the maximum temperature reached in the heating step is 400°C or higher and 1000°C or lower.
2. The friction stir welding method according to claim 1 , wherein the surface processing is performed by grinding or pressing.
3. The friction stir welding method according to claim 1 , wherein the heating is performed by induction heating or resistance heating.
4. The friction stir welding method according to claim 2 , wherein the heating is performed by induction heating or resistance heating.
5. After the heating step, the hardness of the surface layer region of the joint portion of the joint members is in the range of 95 to 115% of the hardness of the base material of the joint members, 2. The friction stir welding method according to claim 1, wherein the surface layer region of the welded portion of the welded members is a region from the surface of the welded portion of the welded members to a position corresponding to 1 / 10 of the thickness of the welded portion.
6. After the heating step, the hardness of the surface layer region of the joint portion of the joint members is in the range of 95 to 115% of the hardness of the base material of the joint members, 3. The friction stir welding method according to claim 2, wherein the surface layer region of the welded portion of the welded members is a region from the surface of the welded portion of the welded members to a position corresponding to 1 / 10 of the thickness of the welded portion.
7. After the heating step, the hardness of the surface layer region of the joint portion of the joint members is in the range of 95 to 115% of the hardness of the base material of the joint members, The friction stir welding method according to claim 3 , wherein the surface layer region of the welded portion of the welded members is a region from the surface of the welded portion of the welded members to a position corresponding to 1 / 10 of the thickness of the welded portion.
8. After the heating step, the hardness of the surface layer region of the joint portion of the joint members is in the range of 95 to 115% of the hardness of the base material of the joint members, 5. The friction stir welding method according to claim 4, wherein the surface layer region of the welded portion of the welded members is a region from the surface to a position corresponding to 1 / 10 of the thickness of the welded portion of the welded members.
9. The friction stir welding method according to any one of claims 1 to 8, further comprising a pre-surface processing step of removing at least a region from the surface of the workpiece to a depth of 5 µm before the joining step.
10. A friction stir welding apparatus used in the friction stir welding method according to any one of claims 1 to 8, A joining device that joins workpieces together to obtain a joined member; A surface processing device that processes the surface of the joining member; A heating device for heating the joining member; in the above order in a welding direction.
11. A friction stir welding apparatus used in the friction stir welding method according to claim 9, A preliminary surface treatment device that performs preliminary surface treatment on the workpieces; a joining device for joining the workpieces to obtain a joined member; A surface processing device that processes the surface of the joining member; A heating device for heating the joining member; in the above order in a welding direction.
12. A method for producing a welded member, comprising joining workpieces by the friction stir welding method according to any one of claims 1 to 8 to obtain a welded member.
13. A method for producing a welded member, comprising: welding workpieces by the friction stir welding method according to claim 9 to obtain a welded member.
Citation Information
Patent Citations
Manufacturing method of heat exchanger
JP2010069503A
Method for manufacturing heat exchanger plate
JP2014050890A
Apparatus and method for increasing weld pin speed and stability in friction stir welding
JP2022530588A
Friction stir welding method for electromagnetic steel strips and manufacturing method for electromagnetic steel strips
JP7279866B1
Friction agitation welding method
JP2019166569A