Positive electrode active material for lithium ion secondary batteries, lithium ion secondary batteries

By replacing nickel with higher valence metals and sulfur in the positive electrode active material for lithium ion secondary batteries, the material addresses the nickel supply constraints and maintains battery capacity, offering a viable alternative to traditional nickel-based compositions.

JP7568214B2Active Publication Date: 2024-10-16SUMITOMO METAL MINING CO LTD +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2020167590
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-10-02
Publication Date
2024-10-16
Estimated Expiration
2040-10-02

AI Technical Summary

Technical Problem

The demand for nickel, a critical raw material in positive electrode active materials for lithium ion secondary batteries, is insufficient to meet growing demands, leading to potential price increases and the need for alternative materials that maintain battery performance while reducing nickel content.

Method used

A positive electrode active material with the general formula Li1+2yNi a M b O 2+y-x S x is developed, where M is a metal with a valence of 4 or more, replacing part of the nickel with elements like Mn, Nb, Ti, Zr, V, or W, and substituting a portion of oxygen with sulfur to suppress nickel content and enhance battery capacity.

Benefits of technology

The proposed active material achieves excellent battery capacity while minimizing nickel usage, maintaining performance levels comparable to traditional materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007568214000002
    Figure 0007568214000002
  • Figure 0007568214000001
    Figure 0007568214000001
Patent Text Reader

Abstract

To provide a lithium ion secondary battery positive electrode active material which has excellent battery capacity when applied to a lithium ion secondary battery, while reducing the nickel content.SOLUTION: The lithium ion secondary battery positive electrode active material is represented by general formula: Li1+2yNiaMbO2+y-xSx, where element M is an at least tetravalent metal, where x satisfies 0<x≤0.5 and y satisfies 0≤y≤0.3, and where a+b=1.0 and a≥b>0.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a positive electrode active material for a lithium ion secondary battery, and a lithium ion secondary battery. [Background technology]

[0002] In recent years, with the widespread use of small information terminals such as smartphones and tablet PCs, there is a strong demand for the development of small, lightweight secondary batteries with high energy density, as well as high-output secondary batteries for use in electric vehicles, including hybrid vehicles.

[0003] Lithium ion secondary batteries are a type of secondary battery that meets these requirements. Lithium ion secondary batteries are composed of a negative electrode, a positive electrode, an electrolyte, etc., and use materials capable of desorbing and inserting lithium as the active materials for the negative electrode and the positive electrode.

[0004] Research and development into lithium-ion secondary batteries is currently underway in earnest. In particular, lithium-ion secondary batteries that use layered or spinel-type lithium metal composite oxides as the positive electrode active material are capable of achieving a high voltage of around 4 V, and are therefore being put into practical use as batteries with high energy density.

[0005] Currently, lithium metal composite oxides such as lithium cobalt composite oxide (LiCoO2), which is relatively easy to synthesize, and lithium nickel composite oxide (LiNiO2), which uses nickel, which is less expensive than cobalt, have been proposed as positive electrode active materials for lithium ion secondary batteries (see Patent Document 1, etc.). [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Japanese Patent Application Publication No. 5-62668 Summary of the Invention [Problem to be solved by the invention]

[0007] As described above, lithium ion secondary batteries are being used in various applications. For this reason, it is expected that the demand for positive electrode active materials will also increase, but the production volume of nickel, which is the raw material, is insufficient to meet the predicted demand, and there is a risk that the price of nickel and the like will rise due to the tight supply and demand. Therefore, there has been a demand for a positive electrode active material for lithium ion secondary batteries that can exhibit sufficient battery performance, for example, sufficient battery capacity, when used in lithium ion secondary batteries while suppressing the amount of nickel used.

[0008] In view of the problems associated with the above-described conventional techniques, one aspect of the present invention aims to provide a positive electrode active material for lithium ion secondary batteries that has excellent battery capacity when applied to lithium ion secondary batteries while suppressing the nickel content. [Means for solving the problem]

[0009] In order to solve the above problem, according to one aspect of the present invention, General formula: Li 1+2y Ni a M b O 2+y-x S x It is expressed as The element M is a metal with a valence of 4 or more, x is 0 <x≦0.5 y is 0≦y≦0.3 a+b=1.0 and a≧b>0 the law of nature, Has a rock-salt structure A positive electrode active material for a lithium ion secondary battery is provided. Effect of the Invention

[0010] According to one aspect of the present invention, it is possible to provide a positive electrode active material for a lithium ion secondary battery that has an excellent battery capacity when applied to a lithium ion secondary battery while suppressing the nickel content. [Brief description of the drawings]

[0011] [Figure 1] Explanatory drawing of the coin-type batteries fabricated in Examples 1 and 2 and Comparative Example 1.

Mode for Carrying Out the Invention

[0012] Hereinafter, embodiments for carrying out the present invention will be described with reference to the drawings. However, the present invention is not limited to the following embodiments, and various modifications and substitutions can be made to the following embodiments without departing from the scope of the present invention. [Positive Electrode Active Material for Lithium-Ion Secondary Battery] One configuration example of the positive electrode active material for a lithium-ion secondary battery according to the present embodiment will be described.

[0013] The positive electrode active material for a lithium-ion secondary battery according to the present embodiment (hereinafter, also simply referred to as "positive electrode active material") has the general formula: Li 1+2y Ni a M b O 2+y-x S x and can be represented by.

[0014] In the general formula above, the element M is a metal with a valence of 4 or more, and it is preferable that x satisfies 0 < x ≤ 0.5 and y satisfies 0 ≤ y ≤ 0.3. Further, for a and b, it is preferable that a + b = 1.0 and a ≥ b > 0.

[0015] The positive electrode active material of the present embodiment will be described below. (1) Regarding the composition

[0016] The elements contained in the positive electrode active material of the present embodiment and their content ratios will be described below. (1-1) Regarding Ni (nickel) and element M The inventor of the present invention studied a positive electrode active material in which a part of Ni was substituted with another element M based on conventionally used LiNiO2. Thus, by substituting a part of Ni with another element M, a positive electrode active material with a suppressed Ni content ratio can be obtained.

[0017] The element M that partially substitutes for Ni is preferably a metal element that can have a valence of 4 or more.

[0018] When LiNiO2 is used in a lithium-ion secondary battery, Ni is trivalent before the Li ions are released, i.e., during discharge. After the Li ions are released, i.e., during charge, Ni is tetravalent.

[0019] On the other hand, when a positive electrode active material in which a part of Ni is replaced with a metal element capable of taking a valence of 4 or more is used in a lithium ion secondary battery, Ni becomes less than 3, for example 2, before Li ions are released, in order to balance the valence in the positive electrode active material. After Li ions are released, Ni becomes 4, as in the case of LiNiO2. Therefore, when a positive electrode active material in which Ni is replaced with the above element M is used in a lithium ion secondary battery, the valence change of Ni during charging and discharging becomes large. Therefore, by using a positive electrode active material in which a part of Ni is replaced with an element M capable of taking a valence of 4 or more, it is possible to suppress the Ni content ratio and improve the amount of electricity that can be compensated by Ni, compared to when LiNiO2 is used as the positive electrode active material.

[0020] The amount of electricity that can be compensated for by Ni means the amount of electricity that can be supplied by the change in valence of Ni when Li ions are released from the positive electrode active material. The valence of Ni before Li ions are released from the positive electrode active material is n, and the valence of Ni after Li ions are released from the positive electrode active material is 4. The Ni content of the positive electrode active material, i.e., the ratio of the amount of Ni in the positive electrode active material, is a according to the general formula described above. In this case, the amount of electricity that can be compensated for by Ni, i.e., the amount of electricity that can be supplied by the change in valence of Ni when Li ions are released from the positive electrode active material, is, for example, a(4-n)e - As is clear from this formula, by decreasing the valence n of Ni before Li ions are released from the positive electrode active material, the amount of electricity that can be compensated for by Ni increases.

[0021] The above-mentioned metal element capable of having a valence of tetravalent or higher means that in the state during discharge when Li ions have not desorbed from the compound in which Ni of the above positive electrode active material is replaced with the metal element, the metal element is a metal element capable of having a valence of tetravalent or higher. As the metal element capable of having a valence of tetravalent or higher, it is more preferable that it is a transition metal element.

[0022] According to the study of the inventors of the present invention, as the element M that replaces Ni, it is preferable that it is one or more selected from Mn (manganese), Nb (niobium), Ti (titanium), Zr (zirconium), V (vanadium), Y (yttrium), W (tungsten), Mo (molybdenum). When a part of Ni is replaced, these elements can have a valence of tetravalent or higher, and it is also possible to improve the amount of electricity that can be charge-compensated by Ni compared to the case where LiNiO2 is used as the positive electrode active material as described above.

[0023] Particularly from the viewpoint of easy availability, it is more preferable that the element M is one or more selected from Mn, Nb, Ti, Zr, V.

[0024] Since the element M replaces a part of the Ni element in LiNiO2, when the subscript indicating the content ratio of Ni in the above general formula is a and the subscript indicating the content ratio of the element M is b, it is preferable that a + b satisfies 1.0.

[0025] The degree of replacing the Ni element with the element M is not particularly limited, but it is preferably half or less of Ni. For this reason, it is preferable that a ≥ b. By replacing a part of Ni with the element M, the amount of Ni used can be suppressed compared to the case of LiNiO2, so b may be 0 < b, but from the viewpoint of particularly suppressing the content ratio of Ni, it is more preferable that 0.2 ≤ b. (1 - 2) Regarding O (oxygen), S (sulfur) As described above, by replacing a part of Ni with the element M, while suppressing the content ratio of Ni, the battery capacity when the positive electrode active material is used in a lithium ion secondary battery can be maintained at approximately the same level as when LiNiO2 is used as the positive electrode active material.

[0026] However, according to the study by the inventor of the present invention, when Ni is replaced with element M, the voltage required to desorb Li ions increases, and the amount of Li ions that can be extracted within the practical voltage range during normal use of the lithium-ion secondary battery may decrease, resulting in a reduction in capacity. Therefore, through further study, it was found that by replacing a part of O with an element having a lower electronegativity than O, the voltage required to desorb Li ions can be suppressed, and the capacity can be increased even at the practical voltage.

[0027] And the inventor of the present invention found that S (sulfur) is a suitable element for replacing O. Therefore, as shown in the above general formula, a part of O in the positive electrode active material of the present embodiment can be replaced by S.

[0028] x indicating the substitution ratio by S is not particularly limited, but for example, it is preferably 0 < x ≤ 0.5, and more preferably 0.01 ≤ x ≤ 0.2.

[0029] In addition, in order to balance the charges in the positive electrode active material, the content ratio of O can vary according to the content ratio of Li. As will be described later, the positive electrode active material of the present embodiment can also contain Li in excess of the stoichiometric ratio 1 of Li in LiNiO2. Therefore, O can also have a corresponding content ratio. (1 - 3) Regarding Li (Lithium) In the positive electrode active material of the present embodiment, by replacing a part of Ni with element M, cation mixing is likely to occur. Therefore, Li can be made more than the stoichiometric ratio 1.0 of Li in the case of LiNiO2 to suppress the occurrence of cation mixing.

[0030] As shown in the above general formula, Li can be represented by 1 + 2y, and y of 2y indicating the excess amount is preferably 0 ≤ y ≤ 0.3, and more preferably 0 ≤ y ≤ 0.2.

[0031] As described above, from the viewpoint of suppressing the occurrence of cation mixing, it is preferable that the Li content is high, but if the Li content is excessively high, there is a risk that unintended lithium compounds may be mixed in. For this reason, it is preferable that y in 1+2y, which indicates the Li content, satisfies the above range. (2) Crystal structure The crystal structure of the positive electrode active material of this embodiment is not particularly limited, but it is preferable that the crystal structure be a rock salt type structure, and more preferably that the crystal structure be a layered rock salt type structure. [Method of manufacturing positive electrode active material] An example of the method for producing a positive electrode active material according to this embodiment will be described.

[0032] According to the method for producing a positive electrode active material of this embodiment, the positive electrode active material already described can be produced, so some of the matters already described will not be described again.

[0033] The method for producing the positive electrode active material of this embodiment may include the following milling step.

[0034] A milling step milling a feed mixture containing lithium, nickel, element M, and sulfur.

[0035] The inventors of the present invention have conducted research into the above-mentioned method for producing a positive electrode active material and have found that the material can be produced by milling a raw material mixture mixed to obtain a target composition. (Regarding raw material mixture) The raw material mixture is preferably prepared by weighing out the lithium, nickel, element M, and sulfur according to the composition ratio of the desired positive electrode active material, that is, so as to have the same composition ratio as the above-mentioned general formula.

[0036] The raw material mixture is preferably prepared so that the ratio of the amounts of substances is Li:Ni:M:S=1+2y:a:b:x. Since the valence of each element hardly changes before and after the milling process, it is preferable to use a compound corresponding to the valence of each element in the positive electrode active material as a raw material. That is, it is preferable to use a compound containing Ni in a divalent state and a compound containing element M in a valence of 4 or more.

[0037] It is not necessary to prepare a compound for each element individually as a raw material, and a compound containing two or more elements simultaneously can be used as a raw material.

[0038] Examples of raw materials used in preparing the raw material mixture include one or more selected from NiO, NiS, Li2MO3, Li2S, NiO, MO2, and the like. (Milling conditions) The milling conditions are not particularly limited, but for example, the milling can be carried out in a dry manner with an inert atmosphere in a milling container.

[0039] During the milling step, the milling conditions can be selected so that sufficient energy is imparted to the raw material mixture to obtain the desired positive electrode active material. [Lithium-ion secondary battery] The lithium ion secondary battery (hereinafter also referred to as "secondary battery") of this embodiment can have a positive electrode containing the above-mentioned positive electrode active material.

[0040] Hereinafter, one configuration example of the secondary battery of this embodiment will be described for each component. The secondary battery of this embodiment includes, for example, a positive electrode, a negative electrode, and a non-aqueous electrolyte, and is composed of the same components as a general lithium-ion secondary battery. Note that the embodiment described below is merely an example, and the lithium-ion secondary battery of this embodiment can be embodied in various forms that have been modified and improved based on the knowledge of those skilled in the art, including the following embodiment. In addition, the secondary battery is not particularly limited in its use. (positive electrode) The positive electrode of the secondary battery of this embodiment can contain the positive electrode active material described above.

[0041] An example of a method for manufacturing a positive electrode is described below. First, the positive electrode active material (powder), conductive material, and binder are mixed to prepare a positive electrode mixture, and activated carbon and a solvent for viscosity adjustment, etc. are added as necessary, and the mixture is kneaded to prepare a positive electrode mixture paste.

[0042] The mixing ratio of each material in the positive electrode mixture is a factor that determines the performance of the lithium ion secondary battery, and can be adjusted depending on the application. The mixing ratio of the materials can be the same as that of the positive electrode of a known lithium ion secondary battery, and for example, when the total mass of the solid content of the positive electrode mixture excluding the solvent is taken as 100 mass%, the positive electrode active material can be contained in a ratio of 60 mass% to 95 mass%, the conductive material can be contained in a ratio of 1 mass% to 20 mass%, and the binder can be contained in a ratio of 1 mass% to 20 mass%.

[0043] The obtained positive electrode mixture paste is applied to the surface of a current collector made of, for example, aluminum foil, and dried to remove the solvent, thereby producing a sheet-like positive electrode. If necessary, pressure can be applied by a roll press or the like to increase the electrode density. The sheet-like positive electrode thus obtained can be cut to an appropriate size according to the desired battery and used for the production of the battery.

[0044] As the conductive material, for example, graphite (natural graphite, artificial graphite, expanded graphite, etc.) and carbon black-based materials such as acetylene black and Ketjen Black (registered trademark) can be used.

[0045] The binder serves to bind the active material particles together, and may be, for example, one or more selected from polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), fluororubber, ethylene propylene diene rubber, styrene butadiene, cellulose-based resin, polyacrylic acid, etc.

[0046] If necessary, a solvent for dispersing the positive electrode active material, conductive material, etc. and dissolving the binder can be added to the positive electrode mixture. Specifically, an organic solvent such as N-methyl-2-pyrrolidone can be used as the solvent. Activated carbon can also be added to the positive electrode mixture to increase the electric double layer capacity.

[0047] The method for producing the positive electrode is not limited to the above-mentioned example, and other methods may be used. For example, the positive electrode may be produced by pressing the positive electrode mixture and then drying it in a vacuum atmosphere. (Negative electrode) The negative electrode may be made of metallic lithium, a lithium alloy, etc. Alternatively, the negative electrode may be made by mixing a binder with a negative electrode active material capable of absorbing and desorbing lithium ions, adding an appropriate solvent to make a paste-like negative electrode mixture, applying the mixture to the surface of a metal foil current collector such as copper, drying it, and compressing it to increase the electrode density as necessary.

[0048] As the negative electrode active material, for example, natural graphite, artificial graphite, sintered organic compounds such as phenol resin, and powder of carbon material such as coke can be used. In this case, as with the positive electrode, fluorine-containing resin such as PVDF can be used as the negative electrode binder, and an organic solvent such as N-methyl-2-pyrrolidone can be used as the solvent for dispersing these active materials and binders. (Separator) A separator may be sandwiched between the positive electrode and the negative electrode as necessary. The separator separates the positive electrode and the negative electrode and holds the electrolyte, and any known separator may be used, such as a thin membrane made of polyethylene or polypropylene having many minute pores. (Non-aqueous electrolyte) As the non-aqueous electrolyte, for example, a non-aqueous electrolytic solution can be used.

[0049] As the non-aqueous electrolyte, for example, a solution in which a lithium salt as a supporting salt is dissolved in an organic solvent can be used. Alternatively, as the non-aqueous electrolyte, a solution in which a lithium salt is dissolved in an ionic liquid can be used. Note that the ionic liquid refers to a salt that is composed of cations and anions other than lithium ions and is liquid even at room temperature.

[0050] The organic solvent may be one selected from cyclic carbonates such as ethylene carbonate, propylene carbonate, butylene carbonate, and trifluoropropylene carbonate; chain carbonates such as diethyl carbonate, dimethyl carbonate, ethyl methyl carbonate, and dipropyl carbonate; ether compounds such as tetrahydrofuran, 2-methyltetrahydrofuran, and dimethoxyethane; sulfur compounds such as ethyl methyl sulfone and butane sultone; and phosphorus compounds such as triethyl phosphate and trioctyl phosphate. Two or more of these organic solvents may be used in combination.

[0051] The supporting salt may be LiPF6, LiBF4, LiClO4, LiAsF6, LiN(CF3SO2)2, or a composite salt thereof. Furthermore, the non-aqueous electrolyte may contain a radical scavenger, a surfactant, a flame retardant, and the like.

[0052] The non-aqueous electrolyte may be a solid electrolyte. The solid electrolyte has a property of being able to withstand high voltage. Examples of the solid electrolyte include inorganic solid electrolytes and organic solid electrolytes.

[0053] Examples of the inorganic solid electrolyte include oxide-based solid electrolytes and sulfide-based solid electrolytes.

[0054] The oxide-based solid electrolyte is not particularly limited, and for example, an oxide-based solid electrolyte containing oxygen (O) and having lithium ion conductivity and electronic insulation can be suitably used. Examples of the oxide-based solid electrolyte include lithium phosphate (Li3PO4), Li3PO4N X , LiBON X, LiNbO3, LiTaO3, Li2SiO3, Li4SiO4-Li3PO4, Li4SiO4-Li3VO4, Li2O-B2O3-P2O5, Li2O-SiO2, Li2O-B2O3-ZnO, Li 1+X Al X Ti 2-X (PO4)3(0≦X≦1), Li 1+X Al X Ge 2-X (PO4)3(0≦X≦1), LiTi2(PO4)3, Li 3X La 2 / 3-X TiO3(0≦X≦2 / 3), Li5La3Ta2O 12 , Li7La3Zr2O 12 , Li6BaLa2Ta2O 12 , Li 3.6 S 0.6 P 0.4 One or more types selected from O4, etc. can be used.

[0055] The sulfide-based solid electrolyte is not particularly limited, and for example, one containing sulfur (S) and having lithium ion conductivity and electronic insulation can be suitably used. For example, the sulfide-based solid electrolyte can be one or more selected from Li2S-P2S5, Li2S-SiS2, LiI-Li2S-SiS2, LiI-Li2S-P2S5, LiI-Li2S-B2S3, Li3PO4-Li2S-Si2S, Li3PO4-Li2S-SiS2, LiPO4-Li2S-SiS, LiI-Li2S-P2O5, LiI-Li3PO4-P2S5, etc.

[0056] As the inorganic solid electrolyte, materials other than those mentioned above may be used, for example, Li3N, LiI, Li3N-LiI-LiOH, etc. may be used.

[0057] The organic solid electrolyte is not particularly limited as long as it is a polymer compound exhibiting ion conductivity, and examples of the organic solid electrolyte that can be used include polyethylene oxide, polypropylene oxide, copolymers thereof, etc. The organic solid electrolyte may also contain a supporting salt (lithium salt). (Shape and structure of secondary battery)

[0058] The lithium ion secondary battery of the present embodiment described above can be made into various shapes such as a cylindrical shape, a laminated shape, etc. Regardless of the shape, if the secondary battery of the present embodiment uses a non-aqueous electrolyte solution as the non-aqueous electrolyte, the positive electrode and the negative electrode are laminated via a separator to form an electrode body, the obtained electrode body is impregnated with a non-aqueous electrolyte solution, and the positive electrode current collector and the positive electrode terminal connected to the outside, and the negative electrode current collector and the negative electrode terminal connected to the outside are connected using a current collecting lead or the like, and the battery case is sealed to form a structure.

[0059] As described above, the secondary battery of the present embodiment is not limited to a form using a non-aqueous electrolyte solution as a non-aqueous electrolyte, and may be, for example, a secondary battery using a solid non-aqueous electrolyte, i.e., an all-solid-state battery. When making an all-solid-state battery, the configuration other than the positive electrode active material may be changed as necessary. EXAMPLES

[0060] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to these examples in any way. (Method of evaluating positive electrode active material)

[0061] The composition of the positive electrode active material was evaluated by analysis using an ICP optical emission spectrometer (VARIAN, 725ES). (Evaluation method for lithium-ion secondary batteries) The performance of the manufactured lithium ion secondary battery was evaluated as follows.

[0062] The coin-type batteries produced in each of the Examples and Comparative Examples were left to stand for about 12 hours after production, and after the open circuit voltage OCV had stabilized, the current density to the positive electrode was increased to 0.1 mA / cm 2The discharge capacity was determined as the capacity at the time when the battery was discharged to a cut-off voltage of 2.0 V after one hour of rest. The discharge capacity is shown as an index, with the discharge capacity in Comparative Example 1 being set to 1.00. [Example 1] A positive electrode active material was prepared by the following procedure.

[0063] NiS, NiO, and Li2MnO3 were weighed and mixed so that the mass ratio of the substances was Li:Ni:Mn:S=1:0.5:0.5:0.1 to prepare a raw material mixture.

[0064] The resulting raw material mixture was placed in a zirconia milling container together with zirconia balls, and the atmosphere in the container was replaced with Ar gas. Then, milling was performed using a planetary ball mill to prepare a positive electrode active material.

[0065] The composition of the obtained positive electrode active material was analyzed and found to be LiNi 0.5 Mn 0.5 O 1.9 S 0.1 It was also confirmed that the powder X-ray diffraction pattern showed that the compound had a rock salt structure. (Coin cell battery) A lithium ion secondary battery was produced using the obtained positive electrode active material, and the charge / discharge capacity was measured.

[0066] As shown in FIG. 1, a coin battery 10 is composed of a case 11 and an electrode 12 housed within this case 11.

[0067] Case 11 has a hollow positive electrode can 111 with one end open, and a negative electrode can 112 placed in the opening of positive electrode can 111, and is configured so that when negative electrode can 112 is placed in the opening of positive electrode can 111, a space for accommodating electrode 12 is formed between negative electrode can 112 and positive electrode can 111.

[0068] Electrode 12 consists of a positive electrode 121, a separator 122, and a negative electrode 123, which are stacked in this order and are housed in case 11 so that positive electrode 121 contacts the inner surface of positive electrode can 111 and negative electrode 123 contacts the inner surface of negative electrode can 112.

[0069] Case 11 is provided with gasket 113, which restricts relative movement between positive electrode can 111 and negative electrode can 112 and fixes them in place so as to maintain a non-contact state between them, i.e., an electrically insulated state. Gasket 113 also has the function of sealing the gap between positive electrode can 111 and negative electrode can 112 to provide an airtight and liquidtight barrier between the inside of case 11 and the outside.

[0070] This coin-type battery 10 was fabricated as follows: First, 52.5 mg of the obtained positive electrode active material, 15 mg of acetylene black, and 7.5 mg of polytetrafluoroethylene (PTFE) resin were mixed and pelletized to a diameter of 11 mm and a weight of about 75 mg to fabricate the positive electrode 121, which was then dried in a vacuum dryer at 100° C. for 12 hours.

[0071] Using the positive electrode 121, the negative electrode 123, the separator 122 and the electrolyte, a coin-type battery 10 was fabricated in a glove box in an Ar atmosphere with a dew point controlled at -60°C.

[0072] For the negative electrode 123, lithium metal punched into a disk shape with a diameter of 13 mm was used.

[0073] A polyethylene porous film having a thickness of 25 μm was used for the separator 122. A mixed solution (manufactured by Toyama Pharmaceutical Co., Ltd.) of ethylene carbonate (EC) and dimethyl carbonate (DMC) with a volume ratio of 4:6, with 1M LiPF6 as the supporting electrolyte, was used for the electrolyte.

[0074] The discharge capacity of the prepared positive electrode active material was measured as described above. The results are shown in Table 1. [Example 2] A positive electrode active material and a coin-type battery were produced and evaluated in the same manner as in Example 1, except that NiS, NiO, and Li2MnO3 were weighed and mixed so that the mass ratio of the materials was Li:Ni:Mn:S=1.4:0.5:0.5:0.2 to prepare a raw material mixture.

[0075] A composition analysis of the obtained positive electrode active material revealed that Li 1.4 Ni 0.5 Mn 0.5 O2S 0.2 It was confirmed that the obtained powder X-ray diffraction pattern showed that the product had a rock salt structure. The evaluation results are shown in Table 1. [Comparative Example 1] A positive electrode active material and a coin-type battery were produced and evaluated in the same manner as in Example 1, except that LiO and NiO were weighed and mixed so that the substance amount ratio was Li:Ni=1:1 to prepare a raw material mixture.

[0076] A composition analysis was performed on the obtained positive electrode active material, and it was confirmed that LiNiO2 was obtained. The evaluation results are shown in Table 1.

[0077] [Table 1] As shown in Table 1, it was confirmed that the positive electrode active materials obtained in Examples 1 and 2 can improve the battery capacity when used in a lithium ion secondary battery while suppressing the Ni content more than that of LiNiO2 in Comparative Example 1.

Claims

1. General formula: Li 1+2y Ni a M b O 2+y-x S x It is expressed as The element M is a metal with a valence of 4 or more; x is 0<x≦0.5 y is 0≦y≦0.3 a+b=1.0 and a≧b>0; A positive electrode active material for lithium-ion secondary batteries with a rock-salt structure.

2. 2. The positive electrode active material for a lithium ion secondary battery according to claim 1, wherein the element M is at least one element selected from the group consisting of Mn, Nb, Ti, Zr, V, Y, W, and Mo.

3. A lithium ion secondary battery comprising a positive electrode containing the positive electrode active material for lithium ion secondary batteries according to claim 1 or 2.

Citation Information

Patent Citations

  • Manufacture of positive electrode for nonaqueous solvent secondary battery

    JP1993062668A

  • Lithium secondary battery

    JP1996250119A

  • Powder material, electrode structure, manufacture thereof and lithium secondary battery

    JP1999214005A