Hydrogen production methods

By mixing and stirring metal silicon particles with alkaline electrolyzed water, the method addresses surface oxidation issues, achieving efficient and cost-effective hydrogen production with high purity and reduced environmental impact.

JP7568226B2Active Publication Date: 2024-10-16SHIN ETSU CHEMICAL CO LTD +1
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2021022737
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-02-16
Publication Date
2024-10-16
Estimated Expiration
2041-02-16

AI Technical Summary

Technical Problem

Existing methods for producing hydrogen through mechanochemical reactions face issues such as surface oxidation of metal particles, leading to reduced reaction amounts, complexity, and environmental and cost burdens due to waste liquid treatment and the need for stringent storage conditions.

Method used

A method involving the mixing and stirring of metal silicon particles with alkaline electrolyzed water, optimizing particle size and pH, and optionally adding alcohol, to maintain efficient hydrogen production without surface oxidation and thermal loss.

Benefits of technology

This approach allows for efficient, inexpensive hydrogen production at room temperature with high purity and reduced environmental impact, suppressing surface oxidation and maintaining reaction efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007568226000002
    Figure 0007568226000002
  • Figure 0007568226000003
    Figure 0007568226000003
  • Figure 0007568226000004
    Figure 0007568226000004
Patent Text Reader

Abstract

To provide a method which can produce hydrogen without causing an amount of reaction to gradually decrease, with a simple and inexpensive technique.SOLUTION: A production method of hydrogen comprises producing the hydrogen by mixing and stirring (A) a metallic silicon particle and (B) alkali electrolyzed water.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an efficient method for producing hydrogen. [Background technology]

[0002] A method for producing hydrogen using mechanochemical reactions has been developed as a simple and inexpensive method for producing hydrogen. When powders of inorganic substances such as silicon and aluminum are mixed with water or an alkaline aqueous solution in which an alkaline substance such as sodium hydroxide is added to water, by applying mechanical energy in a planetary ball mill, a mechanochemical reaction occurs due to the mixing energy, and hydrogen is produced at room temperature (Patent Document 1). However, in the above production method, the surface of the inorganic substance is oxidized, suppressing the amount of hydrogen generated. As a countermeasure, multiple inorganic substances that cause oxidation and reduction reactions are added to produce hydrogen through mechanochemical reactions (Patent Document 2). However, this production method is complicated because metal compounds resulting from various inorganic substances are generated in the hydrogen production solvent, and waste liquid treatment is required.

[0003] On the other hand, it has been reported that hydrogen can be produced in large quantities by mechanochemical reactions, and that the hydrogen production rate was 580 mL / min·g when 12 nm-sized silicon particles were reacted with a KOH aqueous solution (pH=13.0) at 50°C (Non-Patent Document 1). This production method requires HF treatment and nitric acid treatment to prepare the fine silicon particles used as raw materials, which makes them difficult to handle and makes wastewater treatment difficult. It also increases the cost of the hydrogen produced. Furthermore, nanoparticles of a size of about 10 nm react with oxygen and water vapor during storage and oxidize, and all of the nanoparticles with small substance amounts before hydrogen is produced may be oxidized before the reaction and become unusable. To prevent this, it is necessary to store the nanoparticles under conditions without oxygen and moisture, at low temperatures, and in a dark place, and attention must be paid to the expiration date. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2016-47789 A [Patent Document 2] International Publication No. 2019 / 172152 [Non-patent literature]

[0005] [Non-Patent Document 1] J Nanopart Res (2016) 18:116 Summary of the Invention [Problem to be solved by the invention]

[0006] In the above-mentioned conventional technology, hydrogen is generated by a mechanochemical reaction between metal particles and an alkaline aqueous solution, but there is a problem in that the surface of the metal particles is oxidized and the reaction amount gradually decreases. The present invention has been made to solve the above problems, and has an object to provide a method capable of producing hydrogen in a simple and inexpensive manner. [Means for solving the problem]

[0007] In order to solve the above problems, the present invention provides a method for producing hydrogen, which is characterized by producing hydrogen by mixing and stirring (A) metallic silicon particles and (B) alkaline electrolyzed water.

[0008] In this hydrogen production method, the metal particles are stirred in the alkaline electrolyzed water, so that the surfaces of the metal particles are always in sufficient contact with the alkaline electrolyzed water, and the reaction amount does not gradually decrease due to oxidation of the surfaces of the metal particles, making it possible to produce hydrogen using a simple and inexpensive method.

[0009] The (A) metallic silicon particles may have an average particle size of 0.01 to 200 μm.

[0010] By using such component (A), hydrogen can be produced more efficiently by mixing and stirring with alkaline electrolyzed water. In the present invention, silicon particles are considered to be included in the "metal particles".

[0011] In addition, it is preferable to use alkaline electrolyzed water having a pH of 10.5 to 13.5 and a metal ion compound content of 0.5 mass % or less in terms of metal as the alkaline electrolyzed water (B).

[0012] By using such (B) alkaline electrolyzed water, the efficiency of the hydrogen generation reaction is improved and the purity of the hydroxide generated in the alkaline electrolyzed water is increased.

[0013] In addition, (C) alcohol can be further added to the (B) alkaline electrolyzed water.

[0014] By adding (C) alcohol in this manner, it is possible to control the wettability between (A) metallic silicon particles and (B) alkaline electrolytic water, the solubility of high-purity metal hydroxides produced in the alkaline electrolytic water, and the structure of the produced metal hydroxides.

[0015] In this case, the mixing ratio (mass ratio) of the (A) metal silicon particles, the (B) alkaline electrolyzed water, and the (C) alcohol is preferably 0.05 to 10.0 / 99.95 to 80.0 / 0 to 10.0 (mass %; (A) / (B) / (C)).

[0016] By using such a mixture ratio, it is possible to obtain a good balance between the generation of hydrogen and the generation of high purity metal hydroxide.

[0017] The mixing and stirring can be carried out using a stirring blade.

[0018] By using a stirring blade to mix and stir components (A) and (B), hydrogen can be produced more efficiently. Effect of the Invention

[0019] As described above, according to the present invention, by mixing and stirring (A) metal silicon particles and (B) alkaline electrolytic water, hydrogen can be produced inexpensively and simply at room temperature. Furthermore, by mixing and stirring, it is possible to avoid a decrease in hydrogen production due to a change in pH of the alkaline electrolytic water near the metal particle surface caused by the reaction. In addition, by mixing and stirring, temperature unevenness is eliminated, making it possible to achieve an efficient reaction and suppress heat energy loss. In addition, a highly pure metal hydroxide is obtained as a by-product contained in the reaction aqueous solution. In particular, by using metal silicon particles with an average particle size of 0.01 to 200 μm as component (A), hydrogen can be produced more effectively. [Brief description of the drawings]

[0020] [Figure 1] FIG. 1 is a conceptual diagram of a hydrogen production device used in the present invention. [Diagram 2] FIG. 1 is a schematic diagram of a planetary ball mill used to produce silicon powder in the present invention. [Diagram 3] FIG. 2 is a conceptual diagram showing pulverization by rotating a container in the present invention. [Figure 4] 1 is a photograph showing an example of an electron microscope image of the silicon powder used in the present invention. [Diagram 5] 1 is a graph showing an example of the size distribution of the silicon powder used in the present invention. [Figure 6] 4 is a photograph showing another example of an electron microscope image of the silicon powder used in the present invention. [Figure 7] 4 is a graph showing another example of the size distribution of the silicon powder used in the present invention. [Figure 8] 1 is a photograph showing an example of an electron microscope image of silicon powder before pulverization. [Figure 9] 1 is a graph showing an example of the change over time in the amount of hydrogen generated by the reaction between the silicon powder used in the present invention and alkaline electrolyzed water. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] As described above, there has been a demand for the development of a method for producing hydrogen that suppresses the decrease in the reaction amount, has a high hydrogen production rate, and produces a large amount of hydrogen.

[0022] As a result of extensive investigations into the above-mentioned problems, the inventors have discovered that hydrogen can be produced in a simple and inexpensive manner by mixing and stirring (A) metallic silicon particles and (B) alkaline electrolyzed water, and have completed the present invention.

[0023] That is, the present invention provides a method for producing hydrogen, which comprises mixing and stirring (A) metallic silicon particles and (B) alkaline electrolyzed water to produce hydrogen.

[0024] Hereinafter, a detailed description will be given of a method for producing hydrogen according to an embodiment of the present invention, i.e., a method for producing hydrogen by mixing and stirring (A) metal silicon particles and (B) alkaline electrolyzed water, but the present invention is not limited thereto.

[0025] <(A) Metal silicon particles> (A) Metal silicon particles are silicon (Si) metal particles that serve as the raw material for producing the desired hydrogen when mixed with alkaline electrolyzed water. The average particle size of the (A) metal silicon particles is preferably 0.01 to 200 μm, more preferably 0.1 to 200 μm, even more preferably 0.1 to 10 μm, and even more preferably 0.2 to 3 μm, as a median diameter measured by a scanning electron microscope. In particular, when the (A) metal silicon particles and (B) alkaline electrolyzed water are mixed using a simple stirring blade, the average particle size is preferably 0.05 to 5 μm. By using component (A) having such an average particle size, hydrogen can be produced more efficiently by mixing and stirring with alkaline electrolyzed water.

[0026] The metal particles used may be commercially available products, or may be crushed as necessary. In order to obtain metal particles having a desired particle size (particle size distribution), the metal particles may be classified.

[0027] Specific examples of (A) metallic silicon particles (metal powder) will be described below, but the present invention is not limited to these.

[0028] Silicon metal particles (powder) can be obtained by pulverizing raw material silicon powder under specified conditions. The grinding machine used for grinding solids is not particularly limited, and examples of grinding machines that can be used include ball mills, bead mills, rod mills, jet mills, SAG (Semi-Autogenous Grinding) mills, ROM (Run Of Mine) mills, rotary stone mills, etc., but are not limited to these. Figure 2 shows a planetary ball mill, a representative grinding machine. Figure 3 shows the inside of the grinding vessel. These will be described below with reference to the figures. As shown in the conceptual diagram of Figure 2, the planetary ball mill apparatus 10 includes a rotationally driven central shaft 11, a table 13 that rotates integrally with the central shaft 11, and a plurality of containers 12 rotatably supported on the table 13. As shown in Figures 2 and 3, the containers 12 revolve around the central shaft 11 in the direction of arrow A in the figures, while rotating around the central axis 12a of the containers 12 in the direction of arrow B in the figures. As a result, the metal powder 22 is pulverized by the grinding media 21 in each container 12. At this time, a solvent (not shown) may be introduced into the container 12 as necessary.

[0029] As an example, electron microscope photographs of silicon particles (powders) that can be used in the present invention are shown in Figures 4, 6, and 8, which will be described later. Also, size distributions of these silicon particles (powders) are shown in Figures 5 and 7, which will be described later.

[0030] <(B) Alkaline electrolyzed water> (B) Alkaline electrolyzed water is alkaline water obtained by electrolysis of water, and is obtained from the cathode chamber of an electrolysis device (see, for example, JP 2005-319427 A and JP 4021083 A). The alkaline electrolyzed water is not particularly limited and may contain metal ion compounds (for example, those derived from the electrolyte contained in the electrolytic solution), but the smaller the amount, the better, as described below. (B) Alkaline electrolyzed water inhibits the formation of a passive film on the surface of metal particles and improves the efficiency of the hydrogen production reaction, thereby increasing the amount of hydrogen produced. (B) alkaline electrolytic water can be an alkaline aqueous solution with a pH of 10.5 to 13.5, and the content of metal ion compounds can be 0.5 mass% or less in terms of metal. If the pH is 10.5 or more, the amount of hydrogen generated by mixing and stirring with (A) metal silicon particles is sufficient, and the generation rate is also sufficiently fast. If the pH is 13.5 or less, the workability such as handling as an alkali is not deteriorated. In addition, in order to prevent the amount of hydrogen generated from being suppressed by the generation of oxide on the surface of (A) metal silicon particles, the pH is preferably 10.5 to 13.5, more preferably 11.5 to 13.5, and even more preferably 12.0 to 13.3. The content of metal ion compounds is preferably 0.4 mass% or less in terms of metal, more preferably 0.3 mass% or less, and even more preferably 0.1 mass% or less. The less the metal ion compounds, the higher the purity of hydroxides generated in the alkaline electrolytic water.

[0031] In particular, from the viewpoint of improving the efficiency of the hydrogen generation reaction and increasing the purity of the hydroxides produced in the alkaline electrolyzed water, it is preferable to use alkaline electrolyzed water (B) having a pH of 10.5 to 13.5 and a metal ion compound content of 0.5 mass% or less in terms of metal.

[0032] The alkaline aqueous solutions such as sodium hydroxide solutions that have been used in conventional hydrogen production contain a large amount of metal ions, which makes the process complicated and requires waste liquid treatment, as described above, and also places a heavy burden on the environment. In contrast, the alkaline electrolyzed water used in the present invention is obtained by electrolysis of water as described above, and therefore contains very little metal ion compounds (such as those contained in the water used in the electrolysis reaction).In addition, it improves the efficiency of the hydrogen generation reaction, and is therefore excellent in both improving productivity and reducing the environmental load.

[0033] <(C) Alcohol> In order to control the wettability of (A) metal silicon particles with (B) alkaline electrolytic water, the solubility of high-purity metal hydroxides produced in alkaline electrolytic water, and the structure of the produced metal hydroxides, (C) alcohol can be added within any range.

[0034] The alcohol can be selected from, for example, the following group of aliphatic hydrocarbon alcohols having 1 to 10 carbon atoms. The alcohol can be used alone or in combination. Representative examples of the alcohol include methyl alcohol, ethyl alcohol, n-propyl alcohol, isopropanol, butyl alcohol, hexyl alcohol, and octyl alcohol. From the viewpoints of compatibility with alkaline electrolytic water and waste liquid treatment of the aqueous solution after hydrogen generation, alcohols with fewer carbon atoms are preferred, and methyl alcohol and ethyl alcohol are more preferred.

[0035] The mixing ratio (mass ratio) of the (A) metal silicon particles, the (B) alkaline electrolyzed water, and the (C) alcohol is arbitrary, but the mixing ratio is preferably 0.05 to 10.0 / 99.95 to 80.0 / 0 to 10.0 (mass %; (A) / (B) / (C)). By using such a mixture ratio, it is possible to obtain a good balance between the generation of hydrogen and the generation of high purity metal hydroxide.

[0036] <Hydrogen production methods> A method for producing hydrogen will now be described. In the present invention, hydrogen is produced by mixing and stirring (A) metallic silicon particles and (B) alkaline electrolytic water. For example, a simple device as shown in FIG. 1 can be used. Thus, the method for producing hydrogen of the present invention makes it possible to produce hydrogen in a simple and inexpensive manner by mixing and stirring (A) metallic silicon particles and (B) alkaline electrolytic water.

[0037] 1 shows a hydrogen generating device 1 in which (A) metal silicon particles and (B) alkaline electrolyzed water react with each other through the operation of a stirring means. However, hydrogen can be produced by any device that can mix and stir (A) metal silicon particles and (B) alkaline electrolyzed water.

[0038] The hydrogen generating device 1 in Fig. 1 is composed of a hydrogen generating reaction vessel 2 equipped with a stirrer (stirring means) 3, a hydrogen outlet 5, and a thermometer 6, and metal silicon particles 22 and alkaline electrolyzed water 4 in the vessel 2. The stirrer is not particularly limited, and for example, a magnetic stirrer or a stirring device equipped with a stirring blade can be used, but it is preferable to use a stirring blade for mixing and stirring. In addition, the mixing and stirring of (A) metal silicon particles and (B) alkaline electrolyzed water may also include a mechanochemical reaction between the metal silicon particles sandwiched between the stirring blade and the hydrogen generating reaction vessel and the alkaline electrolyzed water. By mixing and stirring the components (A) and (B) in this manner, hydrogen can be produced more efficiently.

[0039] In the hydrogen generating device 1 of FIG. 1, the metal silicon particles 22 and the alkaline electrolytic water 4 in the hydrogen generating reaction vessel 2 are mixed and stirred by the stirrer 3, which is a magnetic stirrer, to generate hydrogen. In the present embodiment, the stirrer 3 is a magnetic stirrer equipped with a temperature control function (heater) and heats the vessel 2. The configuration of the stirrer 3 is not limited thereto, and may be any other device that has a temperature control function for the vessel, such as an oil bath or a thermostatic bath, and a stirring function for the metal silicon particles 22 and the alkaline electrolytic water 4. The heating temperature of the vessel 2 is preferably 30 to 95°C, more preferably 60 to 80°C, and may be, for example, 70°C. This promotes the reaction between the metal silicon particles 22 and the alkaline electrolytic water 4, and increases the amount of hydrogen generated. The generated hydrogen is supplied to a collection vessel (not shown) or the like from a hydrogen outlet 5. If necessary, a purification means such as a dehydrating agent and a temperature control means (cooling, etc.) may be further provided.

[0040] As described above, the hydrogen production method of the present invention can produce hydrogen in a simple and inexpensive manner by mixing and stirring (A) metallic silicon particles and (B) alkaline electrolytic water, so that the metallic silicon particle surface can always be in sufficient contact with the alkaline electrolytic water, and the reaction amount does not gradually decrease due to oxidation of the metallic silicon particle surface. Furthermore, by mixing and stirring, it is possible to avoid a decrease in hydrogen production due to a change in pH of the alkaline electrolytic water near the metallic silicon particle surface caused by the reaction. In addition, by mixing and stirring, temperature unevenness is eliminated, allowing for an efficient reaction and suppressing the loss of thermal energy. Since alkaline electrolytic water contains a small amount of alkali metal ions, it suppresses the oxidation of the surface of metal silicon particles, which contributes to increasing the amount of hydrogen generated. Furthermore, alkaline electrolytic water, in which metal silicon particles react with water to generate hydrogen, contains silicon hydroxide as a by-product, and this compound has the characteristic of being a highly pure hydroxide that is not bound to alkali metals. EXAMPLES

[0041] The present invention will be described below based on examples. Note that the present invention is not limited to these examples, and these examples can be modified or changed based on the spirit of the present invention, and they are not excluded from the scope of the present invention.

[0042] [Examples 1-11, Comparative Examples 1-3] Using the hydrogen generation device shown in Figure 1, hydrogen was generated by mixing (A) metallic silicon particles and (B) alkaline electrolytic water as follows. The hydrogen generation rate was measured as follows. In the following, the average particle size of metallic silicon particles is the median size measured by a scanning electron microscope, and the K + The amount of ions (mass%) is a value calculated as metal, measured by inductively coupled plasma emission spectrometry.

[0043] The silicon particles used in the examples are as shown in Table 1. Among them, the silicon particles used in Examples 1 and 4 are as follows. Fig. 5 shows the size distribution of the silicon particles used in Example 1, which was prepared by grinding at a rotation speed of 300 rpm for 3 minutes, and Fig. 4 shows an electron microscope photograph of the same. Fig. 7 shows the size distribution of the silicon particles used in Example 4, which was prepared by grinding at a rotation speed of 600 rpm for 5 minutes, and Fig. 6 shows an electron microscope photograph of the same. Fig. 8 shows an electron microscope photograph of the silicon particles before grinding.

[0044] (Measurement of hydrogen production rate) The hydrogen production rate under mixing and stirring by stirring means was measured as follows. First, the gas inside the vessel at the start of the reaction was set to 1 atm, with only Ar. Since hydrogen produced by the reaction increases the internal pressure inside the vessel, the hydrogen outlet of the reaction vessel was opened to atmospheric pressure, and the volume of hydrogen produced that contributed to the increase in internal pressure was measured. The amount of hydrogen produced in 1 minute from the start of the reaction (volume under standard conditions) was divided by the hydrogen production time (1 minute), and then divided by the mass (g) of silicon particles used to obtain the "hydrogen production rate per 1 g of silicon particles [ml / min g]." The volume of hydrogen produced was also expressed in moles of substance, and the hydrogen production rate per hour [mmol / h g] is also shown.

[0045] Example 1 In a 250 ml flask, 0.1 g of silicon particles with an average particle size of 1.15 μm (1150 nm) as metal silicon particles and alkaline electrolytic water (pH = 12.4, K + The mixture was heated to a temperature of 70° C. and stirred and mixed at a stirring bar speed of 700 rpm for 4 hours to generate hydrogen. The hydrogen production rate was 290 mmol / h g (108 ml / min g).

[0046] Example 2 In the same manner as in Example 1, 0.1 g of silicon particles having an average particle size of 452 nm as metal silicon particles and alkaline electrolytic water (pH = 12.4, K +The mixture was heated to 70°C and stirred at 700 rpm for 4 hours to generate hydrogen. The hydrogen generation rate was 700 mmol / h g (261 mL / min g).

[0047] Example 3 In the same manner as in Example 1, 0.1 g of silicon particles having an average particle size of 621 nm as metal silicon particles and alkaline electrolytic water (pH = 12.4, K + The mixture was heated to 70°C and stirred and mixed at a stirrer speed of 700 rpm for 4 hours to generate hydrogen. The hydrogen generation rate was 1370 mmol / h g (513 ml / min g). Figure 9 shows the change in the amount of hydrogen generated over the first 4 hours after the start of the reaction.

[0048] Example 4 In the same manner as in Example 1, 0.1 g of silicon particles having an average particle size of 404 nm as metal silicon particles and alkaline electrolytic water (pH = 12.4, K + The mixture was heated to 70°C and stirred at 700 rpm for 4 hours to generate hydrogen. The hydrogen generation rate was 1290 mmol / h g (483 mL / min g).

[0049] Example 5 In the same manner as in Example 1, 0.1 g of silicon particles having an average particle size of 517 nm as metal silicon particles and alkaline electrolytic water (pH = 12.4, K + The mixture was heated to 70°C and stirred at 700 rpm for 4 hours to generate hydrogen. The hydrogen generation rate was 960 mmol / h g (360 mL / min g).

[0050] Example 6 In the same manner as in Example 1, 0.1 g of silicon particles having an average particle size of 426 nm as metal silicon particles and alkaline electrolytic water (pH = 12.4, K+ The mixture was stirred and mixed at 700 rpm for 4 hours at 70 °C to generate hydrogen. The hydrogen generation rate was 550 mmol / h g (208 mL / min g).

[0051] Example 7 In the same manner as in Example 1, 0.1 g of silicon particles having an average particle size of 426 nm as metal silicon particles and alkaline electrolytic water (pH = 12.4, K + The mixture was stirred and mixed at 700 rpm for 4 hours at 70 °C to generate hydrogen. The hydrogen production rate was 430 mmol / h g (161 mL / min g).

[0052] Example 8 In the same manner as in Example 1, 0.1 g of silicon particles having an average particle size of 426 nm as metal silicon particles and alkaline electrolytic water (pH = 12.4, K + The mixture was stirred and mixed at 700 rpm for 4 hours at 70 °C to generate hydrogen. The hydrogen generation rate was 230 mmol / h g (87 mL / min g).

[0053] Example 9 In the same manner as in Example 1, 0.1 g of silicon particles having an average particle size of 426 nm as metal silicon particles and alkaline electrolytic water (pH = 12.4, K + The mixture was stirred and mixed at 700 rpm for 4 hours at 70 °C to generate hydrogen. The hydrogen generation rate was 670 mmol / h g (250 mL / min g).

[0054] Example 10 The alkaline electrolyzed water of Example 1-9 was mixed with another alkaline electrolyzed water (pH = 12.5, K +The mixture was changed to a 250-mL flask containing 0.1 g of silicon particles with an average particle size of 426 nm as metal particles and 150 mL of alkaline electrolyzed water, and hydrogen was generated by mixing and stirring at a temperature of 70 °C and a stirrer speed of 700 rpm for 4 hours. The hydrogen generation rate was 590 mmol / h g (226 ml / min g).

[0055] Example 11 Hydrogen was generated in the same manner as in Example 1, except that component (A) and component (B) were mixed and stirred at 30° C. The hydrogen generation rate was 134 mmol / h g (50 ml / min g).

[0056] Comparative Example 1 In the same manner as in Example 1, 0.4 g of titanium particles with an average particle size of 30 μm instead of metallic silicon particles and 150 mL of alkaline electrolyzed water (pH = 12.4, containing 0.33 mass% K+ ions) were added to a 200 mL flask, heated to a temperature of 70°C, and stirred and mixed at a stirrer speed of 700 rpm for 4 hours to generate hydrogen. The hydrogen generation rate was 0.54 mmol / h g (0.2 ml / min g).

[0057] Comparative Example 2 Hydrogen was generated in the same manner as in Example 1, except that component (A) and component (B) were not mixed or stirred (stirrer rotation speed: 0 rpm). The hydrogen generation rate was 80 mmol / h g (30 ml / min g).

[0058] Comparative Example 3 The alkaline electrolyzed water of Example 1 was mixed with pure water (pH = 7.0, K + The hydrogen generation rate was 6.8 mmol / h g (2.54 ml / min g).

[0059] The results of Examples 1-11 and Comparative Examples 1-3 are summarized in Table 1. [Table 1]

[0060] As is clear from Table 1, the hydrogen production method of the present invention (Examples 1-11) can produce hydrogen in a simple and inexpensive manner by mixing and stirring (A) metal silicon particles and (B) alkaline electrolytic water. From the results of Example 11, it can be seen that hydrogen can be produced even at room temperature. In addition, from FIG. 9 showing the change over time in hydrogen generation in Example 3, it can be seen that a large amount of hydrogen is generated in a short time from the start of the reaction (about one-third of the theoretical amount of hydrogen is generated in the first minute), and the amount of hydrogen generated increases over time without decreasing. In other words, it shows that the present invention is a hydrogen production method that suppresses the decrease over time in the reaction amount (amount of hydrogen generated) caused by the oxidation of the surface of the metal particles, has a fast initial hydrogen generation rate, and produces a large amount of hydrogen. The solubility of SiO2, which is an oxide of silicon, increases sharply in the alkaline region of pH 9 or more, but in the above examples, strong alkaline electrolytic water of pH 12.4 or more is used and stirred, so it is thought that even if the surface of the silicon metal particles is covered with the generated SiO2, this is dissolved and removed, suppressing the decrease over time in the amount of hydrogen generated. From Examples 6-9, when methyl alcohol was added to the reaction system as the alcohol, the amount of hydrogen generated decreased as the amount of alcohol added increased, which shows that the rate of hydrogen generation can be adjusted by adjusting the amount of alcohol added. On the other hand, the amount of hydrogen produced was small in Comparative Example 1, in which titanium particles were used as the metal particles, in Comparative Example 2, in which no mixing or stirring was performed, and in Comparative Example 3, in which pure water was used instead of alkaline electrolyzed water. From the above, it is clear that the hydrogen production method of the present invention is superior.

[0061] The hydrogen production method of the present invention suppresses the oxidation of the metal particle surface because alkaline electrolytic water contains a small amount of alkali metal ions, which contributes to an increase in the amount of hydrogen generated. Furthermore, alkaline electrolytic water in which hydrogen is generated by reaction between metal particles and water contains metal hydroxides as by-products, and this compound is characterized by the fact that a high-purity hydroxide is obtained without any alkali metal bond. Another characteristic is that hydrogen is produced at a high rate. Thus, the present invention is a hydrogen production method that suppresses a decrease in the reaction amount, produces hydrogen at a high rate, and produces a large amount of hydrogen. Furthermore, according to the present invention, hydrogen can be efficiently produced, and the metal hydroxide produced as a by-product has a high purity, so that the environmental load is small and the metal hydroxide itself can be effectively utilized.

[0062] (Industrial Applicability) The present invention provides a method for producing hydrogen with a large amount of hydrogen generated by a simple and inexpensive method, and is therefore suitable for hydrogen production equipment in hydrogen production facilities used for automobile fuel cells, etc. Furthermore, the present invention is not limited to hydrogen production facilities, and can be applied to hydrogen production equipment for small power sources such as in-vehicle and home use.

[0063] The present invention is not limited to the above-described embodiment. The above-described embodiment is merely an example, and anything that has substantially the same configuration as the technical idea described in the claims of the present invention and exhibits similar effects is included in the technical scope of the present invention. [Explanation of symbols]

[0064] 1...hydrogen generation device, 2...hydrogen generation reaction vessel, 3...mixer, 4...alkaline electrolyzed water, 5...hydrogen outlet, 6...thermometer, 10...planetary ball mill device, 11...center shaft, 12 ... grinding container, 12a ... central shaft, 13 ... table, 21 ... grinding media, 22... Metal powder (metal silicon particles), A... Revolution of the grinding vessel, B... Rotation of the grinding vessel

Claims

1. A method for producing hydrogen, comprising mixing and stirring (A) metal silicon particles (excluding silicon scraps generated in semiconductor device production lines, silicon shavings generated in the cutting process of silicon in the production of semiconductor products, and silicon polishing scraps) and (B) alkaline electrolyzed water obtained by electrolysis of water.

2. 2. The method for producing hydrogen according to claim 1, wherein the (A) metallic silicon particles have an average particle size of 0.01 to 200 μm.

3. The method for producing hydrogen according to claim 1 or 2, characterized in that the alkaline electrolyzed water (B) is an alkaline electrolyzed water having a pH of 10.5 to 13.5 and a content of metal ion compounds of 0.5 mass% or less in terms of metal.

4. The method for producing hydrogen according to any one of claims 1 to 3, characterized in that (C) alcohol is further added to the (B) alkaline electrolyzed water.

5. The method for producing hydrogen according to claim 4, characterized in that the mixing ratio (mass ratio) of the (A) metal silicon particles, the (B) alkaline electrolyzed water, and the (C) alcohol is 0.05 to 10.0 / 99.95 to 80.0 / 0 to 10.0 (mass %; (A) / (B) / (C)).

6. 6. The method for producing hydrogen according to claim 1, wherein the mixing and stirring are performed using a stirring blade.

Citation Information

Patent Citations

  • Production of hydrogen

    JP1992059601A

  • Device and method for producing hydrogen

    JP2000191303A

  • Antihypertensive agent

    JP2005330240A

  • Method for purifying sodium hydroxide

    JP2012091981A

  • Method for producing hydrogen

    JP2016047789A