Paper and Board Products
The integration of microfibrillated cellulose and inorganic particulates in a paperboard product addresses the challenges of improving optical and mechanical properties, achieving enhanced whiteness and strength with reduced material weight and environmental impact through a cost-effective, energy-efficient manufacturing process.
Patent Information
- Application Number
- JP2023068512
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2016-04-05
- Filing Date
- 2023-04-19
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2037-03-31
AI Technical Summary
Existing paper and paperboard products face challenges in achieving improved optical, surface, and mechanical properties suitable for printing while being cost-effective and environmentally friendly, with conventional methods requiring extensive rebuilding and high energy consumption.
A paper or paperboard product comprising a cellulose-containing base material with a top ply containing microfibrillated cellulose and inorganic particulate material, applied as a composite at the wet end of a paper machine, enhancing optical and mechanical properties through a low-cost, energy-efficient process.
The solution provides paper and paperboard products with enhanced whiteness, smoothness, and strength, suitable for printing, while reducing material weight and environmental impact, using a composite of microfibrillated cellulose and inorganic particulates.
Smart Images

Figure 0007568775000007 
Figure 0007568775000008 
Figure 0007568775000009
Abstract
Description
[Technical field]
[0001] The present invention is directed to a paper or paperboard product comprising a substrate and at least one top ply comprising a composite of microfibrillated cellulose and at least one inorganic particulate material in an amount suitable to impart improved optical, surface and / or mechanical properties to such paper or paperboard product making it suitable for printing and other end use requirements, a method of making the paper or paperboard product by a process of applying the composite of microfibrillated cellulose and at least one inorganic particulate material to a wet substrate on a wire in the wet end of a papermaking machine, and related uses of such paper or paperboard products. [Background technology]
[0002] Paper and paperboard products are many and varied. There is a continuing need to improve the quality of paper and paperboard products with optical, surface and / or mechanical properties to make them suitable for printing and other end use requirements, as well as to improve the processes for making such paper and paperboard products with improved printability and surface properties by reducing costs, making the processes more energy efficient and environmentally friendly, and / or improving the recyclability of the paper products.
[0003] White top linerboard is conventionally made on a multiformer paper machine. The top layer of white top linerboard often comprises lightly refined bleached hardwood kraft (short) fibers and may contain fillers in amounts up to about 20% by weight. The top layer is conventionally applied to improve the optical appearance of the linerboard and to cover the base with a layer to achieve a high brightness surface suitable for printing or as a base for coating. The base layer usually comprises either unbleached kraft pulp or recycled paperboard ("OCC", waste corrugated cardboard), and is therefore very rough and not suitable for coating with conventional equipment, so a pulp-based layer is conventionally used. White top linerboard is printed with some offset printing, but is most often flexographically printed, with inkjet technology becoming increasingly important.
[0004] With the decline of traditional printing and writing grades, many mills have sought to convert their printing paper machines for linerboard or other packaging products. Converting a single ply machine to a multiformer requires major rebuilds and investments that would otherwise limit the machine to making simple linerboard grades. Application of a suitable coating composite to produce a white top linerboard product through a suitable coating device operating at the wet end of the paper machine offers a simple, low-cost possibility for the machine to economically produce a white top linerboard product. Application of a low solids content slurry of microfibrillated cellulose and organic particulate material to the surface of the linerboard substrate at this point in the linerboard manufacturing process allows the white top linerboard to be drained using existing drainage elements and the resulting white top linerboard to be pressed and dried like a conventional sheet.
[0005] Coating onto a wet, newly formed substrate presents challenges. Among these challenges is the fact that the surface of the wet substrate will be much rougher than the pressed and dried sheet. For this reason, the top ply slurry of the composite of microfibrillated cellulose and organic particulate material must form a uniform flow or curtain of composite material at a suitable flow rate. Furthermore, the top ply slurry must be introduced evenly onto the wet web to obtain a contoured coating. Once pressed and dried, the top ply must present a surface suitable for either direct printing or single coating. Thus, low air permeability and good surface strength are very important properties for a finished white top linerboard. Summary of the Invention
[0006] According to a first aspect of the present invention, (i) a cellulose-containing substrate; (ii) a top ply comprising an inorganic particulate material, and at least about 5% by weight, based on the total weight of the top ply, of microfibrillated cellulose; wherein the weight ratio of inorganic particulate material to microfibrillated cellulose in the top ply is from about 20:1 to about 3:1, and further wherein the top ply has a brightness according to ISO standard 11475 of at least about 65%. A paper or paperboard product is provided.
[0007] In some embodiments, the paperboard product is white top paperboard or white top linerboard.
[0008] According to a second aspect of the present invention, (i) a cellulose-containing substrate; (ii) a top ply comprising in the range of about 67% by weight to about 90% by weight of inorganic particulate material, and at least about 10% by weight of microfibrillated cellulose, based on the total weight of the top ply; and the top ply comprises about 15 g / m 2 ~about 40g / m 2 is present in an amount in the range A paper or paperboard product is provided.
[0009] In one embodiment of the second aspect, the top ply has a mass of about 20 g / m 2 ~about 30g / m 2 In particular, in an amount of at least about 30 g / m 2 is present in an amount of
[0010] In certain embodiments of the first and second aspects, the whiteness measured (by ISO Standard 11475 (F8; D65-400 nm)) for the top ply is increased compared to the whiteness measured for the substrate on the surface opposite the top ply.
[0011] Advantageously, in one embodiment, the top ply provides good optical and physical coverage on dark substrates, e.g., about 30 g / m on a substrate with a brightness of 15-25. 2 At least about 65%, at least about 70%, or at least about 80% improved brightness may be obtained at a coating weight of 100%.
[0012] In some embodiments, the product comprises or is a paperboard product, and in some embodiments, the product is a white top paperboard, cardboard, or linerboard product. Additionally, the improvement in whiteness is greater than about 30 g / m 2 can be made utilizing the first and second embodiments with a coating of typically 50-60 g / m at a lower filler loading of typically 5-15 wt %. 2 This achieves whiteness levels of over 80% compared to traditional white top coatings that require
[0013] According to a third aspect, (i) a cellulose-containing substrate; (ii) a top ply comprising an inorganic particulate material in the range of about 67% to about 92% by weight, and microfibrillated cellulose in the range of 5% to about 30% by weight, based on the total weight of the top ply; A paper or paperboard product is provided, comprising:
[0014] In certain embodiments, the weight ratio of inorganic particulate material to microfibrillated cellulose in the top ply is from about 8:1 to about 1:1, or from about 6:1 to about 3:1, or from about 5:1 to about 2:1, or from about 5:1 to about 3:1, or from about 4:1 to about 3:1.
[0015] According to a fourth aspect of the present invention, there is provided a method of making a paper or board product, the method comprising: (a) providing a wet web of pulp; and (b) providing a top ply slurry on the wet web of pulp, wherein (i) the top slurry has a density of 15 g / m 2 ~40g / m 2 (ii) the top ply slurry comprises microfibrillated cellulose in an amount sufficient to provide a product having a top ply comprising at least about 5 weight percent microfibrillated cellulose, based on the total weight of the top ply, and (iii) the top ply slurry comprises inorganic particulate material and microfibrillated cellulose. In additional embodiments, the top ply comprises at least about 10 weight percent, at least about 20 weight percent, or no more than about 30 weight percent, based on the total weight of the top ply.
[0016] According to a fifth aspect, the present invention is directed to the use of a top ply comprising at least about 20% by weight of microfibrillated cellulose as a white top layer of a paperboard substrate, based on the total weight of the top ply. In an additional embodiment, the present invention is directed to the use of a top ply comprising no more than about 30% by weight of microfibrillated cellulose as a white top layer of a paperboard substrate, based on the total weight of the top ply. In an embodiment, the present invention is directed to the use of a top ply comprising an inorganic particulate material in the range of about 67% to about 92% by weight, and microfibrillated cellulose in the range of about 5% to about 30% by weight, based on the total weight of the top ply.
[0017] According to a sixth aspect, the invention is directed to applying a top ply to a wet substrate on a wire in the wet end of a papermaking machine by forming a curtain or film through an unpressurized or pressurized slot opening to apply the top ply to the substrate to produce a paper or paperboard product according to the first to third aspects.
[0018] In some additional embodiments, the composite of microfibrillated cellulose and inorganic particulate material may be applied as a white top layer or other top layer. Advantageously, the process may be carried out utilizing low-cost equipment for application, such as curtain coaters, pressurized extrusion coaters, secondary headboxes, or pressurized or non-pressurized slot coaters, compared to applying traditional secondary fiber layers or coatings to dry or semi-dry paper or paperboard products. Additionally, existing drainage elements, such as the drainage table of a Fourdrinier machine, and the pressurizing section of a paper machine may be utilized for water removal. The top ply of microfibrillated cellulose and inorganic particulate material has the ability to remain on top of the substrate and provide good optical and physical coverage on low basis weight paper or paperboard products. [Brief description of the drawings]
[0019] [Figure 1] 1 shows the structure of sheets made at various basis weights according to Example 1. [Diagram 2] 1 is a graph summarizing the brightness of sheets made at various basis weights according to Example 1. [Diagram 3] 1 is a graph summarizing the PPS roughness of sheets made at various basis weights according to Example 1. [Figure 4] 1 is a plot of brightness versus coating weight level for Tests 1-4 of Example 2. [Diagram 5] FIG. 13 is a scanning electron microscope image of a substrate coated with a 35 g / m2 top ply comprising 20 wt. % microfibrillated cellulose and 80 wt. % ground calcium carbonate applied to an 85 g / m2 substrate at test point T2. [Figure 6] FIG. 13 is a scanning electron microscope image of a substrate coated with a 48 g / m2 top ply containing 20 wt. % microfibrillated cellulose, 20 wt. % ground calcium carbonate and 60 wt. % talc applied to an 85 g / m2 substrate at test point T4. [Figure 7] 1 shows a cross section of a flexographically printed sample. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0020] Surprisingly, it has been found that a ply comprising a composite of inorganic particulate material and microfibrillated cellulose can be added onto a paper web at the wet end of a papermaking machine (such as a Fourdrinier), immediately after the formation of the wet line and where the web is still less than 10-15% solids by weight. The top ply paper or paperboard products made by the disclosed process provide advantageous optical properties (e.g., brightness), as well as reduced weight and / or improved surface properties (e.g., smoothness and reduced air permeability), while maintaining suitable mechanical properties (e.g., strength for end use).
[0021] By "top" ply, it is meant that the top ply is applied on or to a substrate, and the substrate may have intermediate plies or layers below the top ply. In some embodiments, the top ply is an outer ply, i.e., it does not have another ply above it. In some embodiments, the top ply has a coating weight of at least about 15 g / m 2 ~about 40g / m 2 The sheet has a basis weight of 1.0 g.
[0022] "Microfibrillated cellulose" refers to a cellulose composition in which cellulose microfibrils are liberated or partially liberated as individual seeds or as smaller aggregates compared to the cellulose fibers prior to microfibrillation. Microfibrillated cellulose may be obtained by microfibrillating cellulose, including but not limited to the processes described herein. Typical cellulose fibers suitable for use in papermaking (i.e., pulp prior to microfibrillation or pulp not yet fibrillated) contain larger aggregates of hundreds to thousands of individual cellulose microfibrils. Microfibrillating cellulose imparts certain characteristics and properties to microfibrillated cellulose and compositions comprising microfibrillated cellulose, including but not limited to the characteristics and properties described herein.
[0023] There are many types of paper or paperboard products that can be made with the disclosed microfibrillated cellulose and inorganic particulate material compositions by the manufacturing process disclosed herein. There is no clear distinction between paper and paperboard products. The latter tend to be thicker paper-based materials with increased basis weight. The paperboard may be a single ply to which a top ply of a composite of microfibrillated cellulose and inorganic particulate material is applied, or the paperboard may be a multi-ply substrate. The present invention is directed to many forms of paperboard, including but not limited to boxboard or cartonboard, including folding cartons and rigid assembly boxes and folding box boards, such as liquid container boards. The paperboard may be chipboard or white-lined chipboard. The paperboard may be kraft board, laminate board. The paperboard may be bleached or unbleached. Various forms of cardboard, such as corrugated fiberboard (which is an assembly material, not the paper or paperboard product itself), linerboard or bookbinding board, are encompassed by the paperboard products of the present invention. The paperboard described herein may be suitable for wrapping and packaging a variety of end products, including, for example, food products.
[0024] In some embodiments, the product is or includes cardboard, and the substrate and top ply are suitable for use in or as cardboard. In some embodiments, the product is or includes one of a brown kraft liner, a white top kraft liner, a test liner, a white top test liner, a brown lightweight recycled liner, a heathered test liner, and a white top recycled liner.
[0025] In some embodiments, the product is or comprises cartonboard.
[0026] In some embodiments, the product is or comprises kraft paper.
[0027] In some embodiments, the substrate comprises or is suitable for use in or as a paperboard product. In some embodiments, the substrate is suitable for use in a white top paperboard product, for example as a linerboard. In some embodiments, the product comprises or is a paperboard product, for example as a linerboard. In some embodiments, the product comprises or is a white top paperboard product, for example as a linerboard. In such embodiments, the paperboard product may be, for example, a corrugated board, with the product comprising the substrate and the top ply as a linerboard. In some embodiments, the paperboard product is single-sided, single-wall, double-wall or triple-wall corrugated.
[0028] Unless otherwise stated, amounts are based on the total dry weight of the top ply and / or substrate.
[0029] Unless otherwise indicated, particle size characteristics referred to herein for inorganic particulate materials are measured by well-known methods using a Sedigraph 5100 machine (herein referred to as the "Micromeritics Sedigraph 5100 unit") supplied by Micromeritics Instruments Corporation, Norcross, GA, USA (Tel: +1 770 662 3620; Website: www.micromeritics.com) by sedimentation of particulate material fully dispersed in an aqueous medium. Such a machine measures and provides a plot of the cumulative weight percent of particles having a size less than a given esd value, referred to in the art as the "equivalent sphere diameter (esd)". The average particle size d 50 is the thus determined value of particle ESD, and d 50 50% by weight of particles have an equivalent spherical diameter smaller than this value.
[0030] Alternatively, where indicated, particle size properties referred to herein for inorganic particulate materials are measured by well-known conventional methods used in the field of laser light scattering, using a Malvern Mastersizer S machine supplied by Malvern Instruments Ltd (or by other methods that give essentially the same results). In laser light scattering, the size of particles in powders, suspensions and emulsions can be measured using the diffraction of a laser beam based on the application of Mie theory. Such machines measure and provide a plot of the cumulative volume percent of particles having a size less than a given esd value, referred to in the art as the "equivalent sphere diameter (esd)". Average particle size d 50 is the thus determined value of particle ESD, and d 50 50% by volume of particles have an equivalent sphere diameter smaller than this value.
[0031] Unless otherwise stated, the particle size properties of the microfibrillated cellulose material are measured by well known conventional methods used in the field of laser light scattering, using a Malvern Mastersizer S machine supplied by Malvern Instruments Ltd (or by other methods giving essentially the same results).
[0032] Details of the procedure used to characterize the particle size distribution of mixtures of inorganic particulate material and microfibrillated cellulose using a Malvern Mastersizer S machine are provided below.
[0033] Top ply In some embodiments, the top ply comprises at least about 5% by weight of microfibrillated cellulose, based on the total weight of the top ply. In some embodiments, the top ply comprises from about 5% to about 30% by weight of microfibrillated cellulose, for example from 5% to about 25% by weight, or from about 10% to about 25% by weight, or from about 15% to about 25% by weight, or from about 17.5% to about 22.5% by weight of microfibrillated cellulose, based on the total weight of the top ply.
[0034] In some embodiments, the top ply comprises at least about 67 wt. % inorganic particulate material, or at least about 70 wt. % inorganic particulate material, or at least about 75 wt. % inorganic particulate material, or at least about 80 wt. % inorganic particulate material, or at least about 85 wt. % inorganic particulate material, or at least about 90 wt. % inorganic particulate material, and optionally, 0-3 wt. % other additives, based on the total weight of the top ply.
[0035] In one embodiment, the microfibrillated cellulose and inorganic particulate material are about 15 g / m 2 ~about 40g / m 2 In this and other embodiments, the weight ratio of inorganic particulate material to microfibrillated cellulose in the top ply is about 20:1, or about 10:1, or about 5:1, or about 4:1, or about 3:1, or about 2:1.
[0036] In one embodiment, the top ply comprises about 70% to about 90% by weight of inorganic particulate material, and about 10% to about 30% by weight of microfibrillated cellulose, and optionally up to 3% by weight of other additives, based on the total weight of the top ply.
[0037] In some embodiments, the top ply may optionally contain additional organic compounds, ie, organic compounds other than microfibrillated cellulose.
[0038] In certain embodiments, the top ply may optionally contain a cationic polymer, an anionic polymer, and / or a polysaccharide hydrocolloid.
[0039] In some embodiments, the top ply may optionally contain wax, polyolefin, and / or silicone.
[0040] In some embodiments, the top ply does not contain an optical brightener.
[0041] In certain embodiments, the top ply consists essentially of inorganic particulate material and microfibrillated cellulose, and thus includes about 3% or less by weight of additives other than inorganic particulate material and microfibrillated cellulose, e.g., about 2% or less by weight, or about 1% or less by weight, or about 0.5% or less by weight. In such embodiments, the top ply may include about 3% or less by weight of additives selected from flocculants, formation / drainage aids (e.g., poly(acrylamide-co-diallyldimethylammonium chloride), Polydadmac®), water-soluble thickeners, starches (e.g., cationic starches), sizing agents, such as rosin, alkyl ketene dimers ("AKD"), alkenyl succinic anhydrides ("ASA"), or similar materials and combinations thereof, e.g., about 2% or less by weight of such additives, or about 1% or less by weight of such additives, or about 0.5% or less by weight of such additives.
[0042] In one embodiment, it has been found that the addition of small amounts of retention / drainage aids, such as poly(acrylamide-co-diallyldimethylammonium chloride) solutions (Polydadmac®), as opposed to the much larger amounts used in conventional papermaking, has a positive effect on dewatering, although the reduced amount of retention aid causes microscale flocculation without any visible adverse effect on the substrate structure. This results in a significant increase in dewatering rate.
[0043] In one embodiment, the top ply is comprised of inorganic particulate material and microfibrillated cellulose and thus contains, other than the inorganic particulate material and microfibrillated cellulose, less than about 0.25 wt. %, for example less than about 0.1 wt. %, of additives selected from flocculants, formation / drainage aids (e.g., poly(acrylamide-co-diallyldimethylammonium chloride) solutions (Polydadmac®)), water-soluble thickeners, starches (e.g., cationic starches), and combinations thereof, or no additives.
[0044] The microfibrillated cellulose may be from any suitable source.
[0045] In one embodiment, the microfibrillated cellulose has a d in the range of about 5 μm to about 500 μm as measured by laser light scattering. 50 In an embodiment, the microfibrillated cellulose has a d of about 400 μm or less, e.g., about 300 μm or less, or about 200 μm or less, or about 150 μm or less, or about 125 μm or less, or about 100 μm or less, or about 90 μm or less, or about 80 μm or less, or about 70 μm or less, or about 60 μm or less, or about 50 μm or less, or about 40 μm or less, or about 30 μm or less, or about 20 μm or less, or about 10 μm or less. 50 has.
[0046] In one embodiment, the microfibrillated cellulose has a modal fiber particle size in the range of about 0.1 to about 500 μm. In one embodiment, the microfibrillated cellulose has a modal fiber particle size of at least about 0.5 μm, such as at least about 10 μm, or at least about 50 μm, or at least about 100 μm, or at least about 150 μm, or at least about 200 μm, or at least about 300 μm, or at least about 400 μm.
[0047] Additionally or alternatively, the microfibrillated cellulose may have a fibre steepness, as measured by Malvern, of about 10 or greater. The fibre steepness (i.e. the slope of the fibre particle size distribution) is given by the following formula: Gradient = 100 × (d 30 / d 70 ) is determined by.
[0048] The microfibrillated cellulose may have a fiber gradient of about 100 or less. The microfibrillated cellulose may have a fiber gradient of about 75 or less, or about 50 or less, or about 40 or less, or about 30 or less. The microfibrillated cellulose may have a fiber gradient of about 20 to about 50, or about 25 to about 40, or about 25 to about 35, or about 30 to about 40.
[0049] The inorganic particulate material may be, for example, calcium carbonate, magnesium carbonate, alkaline earth metal carbonates or sulfates such as dolomite, gypsum, hydrous kandite clays such as kaolin, halloysite or ball clay, anhydrous (calcined) kandite clays such as metakaolin or fully calcined kaolin, talc, mica, huntite, hydromagnesite, powdered glass, perlite or diatomaceous earth, or wollastonite, or titanium dioxide, or magnesium hydroxide, or aluminum trihydrate, lime, graphite, or combinations thereof.
[0050] In certain embodiments, the inorganic particulate material includes or is calcium carbonate, magnesium carbonate, dolomite, gypsum, anhydrous kandite clay, perlite, diatomaceous earth, wollastonite, magnesium hydroxide, or aluminum trihydrate, titanium dioxide, or combinations thereof.
[0051] An exemplary inorganic particulate material for use in the present invention is calcium carbonate. Hereinafter, the present invention may tend to be discussed in terms of calcium carbonate and in terms of the manner in which calcium carbonate is processed and / or treated. The present invention should not be construed as being limited to such embodiments.
[0052] The particulate calcium carbonate used in the present invention may be obtained by grinding natural raw materials. Ground calcium carbonate (GCC) is typically obtained by crushing and then grinding mineral raw materials such as chalk, marble, limestone, which may be followed by a particle size classification step to obtain a product with the desired fineness. Other techniques such as bleaching, flotation, magnetic separation may be used to obtain a product with the desired fineness and / or color. The particulate solid material may be ground spontaneously, i.e. by abrasion of the particles of the solid material themselves, or in the presence of particulate grinding media comprising particles of a material different from the calcium carbonate to be ground. These processes may be carried out in the presence or absence of dispersants and biocides, which may be added at any stage of the process.
[0053] In the present invention, precipitated calcium carbonate (PCC) may be used as a source of particulate calcium carbonate and may be produced by any of the known methods available in the art. Pages 34-35 of TAPPI Monograph Series No. 30 "Paper Coating Pigments" describe three major commercial processes for preparing precipitated calcium carbonate suitable for use in preparing products for use in the paper industry, which may also be used in the practice of the present invention. In all three processes, a calcium carbonate source, such as limestone, is first calcined to produce quicklime, which is then slaked in water to obtain calcium hydroxide or milk of lime. In the first process, the milk of lime is directly carbonated with carbon dioxide gas. This process has the advantage that no by-products are formed, and the nature and purity of the calcium carbonate product is relatively easy to control. In the second process, the milk of lime is contacted with soda ash to produce a precipitate of calcium carbonate and a solution of sodium hydroxide by double decomposition. When this process is used commercially, the sodium hydroxide may be substantially completely separated from the calcium carbonate. In the third major commercial process, milk of lime is first contacted with ammonium chloride to obtain a calcium chloride solution and ammonia gas. The calcium chloride solution is then contacted with soda ash to produce a solution of light calcium carbonate and sodium chloride by metathesis. Depending on the particular reaction process used, crystals can be produced in a variety of different shapes and sizes. The three main forms of PCC crystals are aragonite, rhombohedral and skarnohedral (e.g., calcite), all of which are suitable for use in the present invention, including mixtures thereof.
[0054] In one embodiment, PCC may be formed during the production process of microfibrillated cellulose.
[0055] Wet-grinding of calcium carbonate involves the formation of an aqueous suspension of calcium carbonate, which may then be ground, optionally in the presence of a suitable dispersant. For further information regarding wet-grinding of calcium carbonate, reference may be made, for example, to EP-A-614948, the contents of which are incorporated herein in their entirety by reference.
[0056] When the inorganic particulate material of the present invention is obtained from natural sources, some mineral impurities may contaminate the ground material. For example, natural calcium carbonate may exist with other minerals. Thus, in some embodiments, the inorganic particulate material contains a certain amount of impurities. However, generally, the inorganic particulate material used in the present invention will contain less than about 5% by weight, or less than about 1% by weight, of other mineral impurities.
[0057] The inorganic particulate material may have a particle size distribution in which at least about 10% by weight of the particles have an ESD of less than 2 μm, for example, at least about 20% by weight, or at least about 30% by weight, or at least about 40% by weight, or at least about 50% by weight, or at least about 60% by weight, or at least about 70% by weight, or at least about 80% by weight, or at least about 90% by weight, or at least about 95% by weight, or about 100% by weight of the particles have an ESD of less than 2 μm.
[0058] In another embodiment, the inorganic particulate material has a particle size distribution in which at least about 10% by volume of the particles have an esd of less than 2 μm, for example, at least about 20% by volume, or at least about 30% by volume, or at least about 40% by volume, or at least about 50% by volume, or at least about 60% by volume, or at least about 70% by volume, or at least about 80% by volume, or at least about 90% by volume, or at least about 95% by volume, or about 100% by volume have an esd of less than 2 μm, as measured using a Malvern Mastersizer S machine.
[0059] Details of the procedure used to characterize the particle size distribution of mixtures of inorganic particulate material and microfibrillated cellulose using a Malvern Mastersizer S machine are provided below.
[0060] In some embodiments, the inorganic particulate material is kaolin clay. Hereafter, this section of the specification may tend to be discussed in terms of kaolin and in terms of the manner in which kaolin is processed and / or treated. The present invention should not be construed as being limited to such embodiments. Thus, in some embodiments, kaolin is used in raw form.
[0061] The kaolin clay used in the present invention can be a processed material derived from natural raw materials, i.e., raw natural kaolin clay minerals. Processed kaolin clays typically contain at least about 50% by weight of kaolinite. For example, most commercial processed kaolin clays contain more than about 75% by weight of kaolinite, and can contain more than about 90% by weight, and in some cases more than about 95% by weight of kaolinite.
[0062] The kaolin clay used in the present invention may be prepared from raw natural kaolin clay minerals by one or more other processes well known to those skilled in the art, such as known smelting or beneficiation processes.
[0063] For example, the clay minerals may be bleached with a reducing bleaching agent such as sodium hydrosulfite. If sodium hydrosulfite is used, after the sodium hydrosulfite bleaching step, the bleached clay minerals may optionally be dehydrated, optionally washed, and optionally dehydrated again.
[0064] The clay minerals may be treated to remove impurities, for example by flocculation, flotation or magnetic separation methods well known in the art, or the clay minerals used in the first aspect of the invention may be untreated, either as a solid or in an aqueous suspension.
[0065] The process for preparing the particulate kaolin clay used in the present invention may also include one or more comminution steps, such as grinding or milling. Light comminution of the crude kaolin is used to provide suitable exfoliation thereof. Comminution may be accomplished using plastic (e.g., nylon) beads or granules, sand or ceramic grinding or mill grinding aids. The crude kaolin may be refined using well-known procedures to remove impurities and improve physical properties. The kaolin clay may be treated with known particle size classification procedures, such as sieving and centrifugation (or both), to obtain the desired d. 50 Particles having a value or particle size distribution can be obtained.
[0066] Base material The substrate (and microfibrillated cellulose) may be derived from a cellulose-containing pulp and may be prepared by any suitable chemical or mechanical treatment, or combination thereof, known in the art. The pulp may be derived from any suitable source, such as wood, grasses (e.g., sugar cane, bamboo), or waste textiles (e.g., textile waste, cotton, hemp, or flax). The pulp may be bleached according to processes known to those skilled in the art, and those processes suitable for use in the present invention will be readily apparent. In an embodiment, the pulp is unbleached. Bleached or unbleached cellulose pulp is prepared by mixing with a cellulose pulp having a defined freeness (known in the art as Canadian Standard Freeness (CSF) in cm 3 The pulp is then beaten, refined, or both to a final yield (reported as 0.1%). A suitable stock is then prepared from the beaten pulp, which may be bleached or unbleached.
[0067] In some embodiments, the substrate comprises or is derived from kraft pulp and is natural color (i.e., unbleached). In some embodiments, the substrate comprises or is derived from dark kraft pulp, recycled pulp, or a combination thereof. In some embodiments, the substrate comprises or is derived from recycled pulp.
[0068] The stock from which the substrate is prepared may contain other additives known in the art. For example, the stock contains a nonionic, cationic or anionic retention aid, or a particulate retention system. It may also contain a size, which may be, for example, a long chain alkyl ketene dimer ("AKD"), a wax emulsion or a succinic acid derivative, such as an alkenyl succinic anhydride ("ASA"), rosin with alum or a cationic rosin emulsion. The stock for the substrate composition may contain dyes and / or optical brighteners. The stock may also include dry and wet strength aids, such as, for example, starch or epichlorohydrin copolymers.
[0069] product In one embodiment, the substrate has a basis weight suitable for use in or as a cardboard product, for example, about 50 g / m 2 ~about 500g / m 2 In this and other embodiments, the top ply has a basis weight in the range of about 10 g / m 2 ~about 50g / m 2 , specifically, about 15 g / m 2 ~40g / m 2 and more specifically, about 20 g / m 2 ~30g / m 2 The composition may have a basis weight in the range of 1000 to 2000 gram.
[0070] In one embodiment, the substrate has a thickness of about 75 g / m 2 ~about 400g / m 2 , for example, about 100 g / m 2 ~Approx. 375g / m 2 , or about 100 g / m 2 ~Approx. 350g / m 2 , or about 100 g / m 2 ~about 300g / m 2 , or about 100 g / m 2 ~275g / m 2 , or about 100 g / m 2 ~about 250g / m 2 , or about 100 g / m 2 ~Approx. 225g / m 2, or about 100 g / m 2 ~about 200g / m 2 In this and other embodiments, the top ply has a basis weight of about 15 g / m 2 ~40g / m 2 , or about 25 g / m 2 ~35g / m 2 The composition may have a basis weight in the range of 1000 to 2000 gram.
[0071] In one embodiment, the top ply is 40 g / m 2 or less than 35g / m 2 or less than 30g / m 2 or less than 25g / m 2 or less than 2.5g / m 2 or less than 20g / m 2 or less than 18g / m 2 or less than 15g / m 2 It has the following basis weight:
[0072] In one embodiment, the top ply is 40 g / m 2 or less than 35g / m 2 or less than 30g / m 2 or less than 25g / m 2 or less than 2.5g / m 2 or less than 20g / m 2 or less than 18g / m 2 or less than 15g / m 2 It has the following basis weight:
[0073] Advantageously, the application of a top ply comprising inorganic particulate material and microfibrillated cellulose allows for the production of products, such as paperboard or cardboard, with desired optical, surface, and mechanical properties, while utilizing a relatively small amount of a top ply having a high filler content, thereby providing a lighter product compared to conventional top ply / substrate configurations. Additionally, any loss in mechanical properties that may occur with subsequent application of the top ply can be offset by increasing the basis weight of the substrate, which is a relatively inexpensive material.
[0074] Thus, in one embodiment, the product comprises: (i) an increased whiteness measured (by ISO Standard 11475 (F8; D65-400 nm)) for the top ply compared to the whiteness measured for the substrate without the top ply or for the substrate on the surface opposite the top ply, and / or a whiteness measured for the top ply by ISO Standard 11475 (F8; D65-400 nm) of at least about 60.0%; (ii) a PPS roughness measured on the top ply (@1000 kPa) of about 6.0 μm or less, and / or a PPS roughness measured on the top ply (@1000 kPa) that is at least 2.0 μm less than the PPS roughness of the substrate without the top ply; has one or more of:
[0075] In some embodiments, the whiteness measured for the top ply is at least about 70.0%, e.g., at least about 75.0%, or at least about 80.0%, or at least about 81.0%, or at least about 82.0%, or at least about 83.0%, or at least about 84.0%, or at least about 85.0%. Whiteness may be measured using an Elrepho spectrophotometer.
[0076] In some embodiments, the product has a PPS roughness (@1000 kPa) measured on the top ply of less than about 5.9 μm, such as less than about 5.8 μm, or less than about 5.7 μm, or less than about 5.6 μm, or less than about 5.5 μm. In some embodiments, the PPS roughness is from about 5.0 μm to about 6.0 μm, such as from about 5.2 μm to about 6.0 μm, or from about 5.2 μm to about 5.8 μm, or from about 5.2 μm to about 5.6 μm.
[0077] In one embodiment, the top ply has a thickness of about 30 to about 50 g / m 2 %, a brightness of at least about 65.0%, and optionally a PPS roughness of less than about 5.6 μm.
[0078] In an embodiment, the product comprises an additional layer or ply(s) above the ply comprising at least about 50% by weight of microfibrillated cellulose, for example, one or more layers or plies, or at least two additional layers or plies, or up to about five additional layers or plies, or up to about four additional layers or plies, or up to about three additional layers or plies.
[0079] In an embodiment, the or at least one of the further layers or plies is a barrier layer or ply, or a wax layer or ply, or a silicone layer or ply, or a combination of two or three of such layers.
[0080] Another advantageous feature of the top ply coated substrates comprising the microfibrillated cellulose and inorganic particulate materials of the present disclosure is improved printability onto the top ply. Conventional white top liners typically have a white surface comprised of white paper with a relatively low filler content, typically in the 5-15% filler range. As a result, such white top liners tend to have a coarse pore structure and are quite open and rough. This is not ideal for receiving printing inks.
[0081] FIG. 6 below illustrates the improvement in printability achieved by application of a top ply of the present invention comprising microfibrillated cellulose and organic particulate material.
[0082] Overall, the low air permeability of the plies may improve properties in barrier applications, and the use of such plies may provide a "greener" packaging product since it allows non-recyclable coatings such as wax, PE and silicone to be replaced with recyclable compositions, overall obtaining equal or improved performance from non-recyclable counterparts.
[0083] Manufacturing method A method of making a paper product is provided, the method comprising: (a) providing a wet web of pulp; (b) providing a top pry slurry onto the wet web of pulp; The top ply slurry contains (i) 15 g / m 2 ~40g / m 2 (ii) the top ply slurry comprises microfibrillated cellulose in an amount sufficient to provide a product having a top ply comprising at least about 5% by weight of microfibrillated cellulose; and (iii) the top ply slurry comprises at least about 67% by weight of inorganic particulate material.
[0084] This method is a "wet-on-wet" method that differs from conventional paper coating methods in which an aqueous coating is applied to a substantially dry paper product (ie, "wet-on-dry").
[0085] In one embodiment, the top slurry has a viscosity of 15 g / m 2 ~40g / m 2 It is provided in amounts ranging from
[0086] In one embodiment, the top ply slurry contains a sufficient amount of microfibrillated cellulose to provide a product having the necessary strength properties to meet the end use requirements. Typically, this will mean a top ply containing at least about 5% by weight of microfibrillated cellulose, based on the total weight of the top ply (i.e., the total dry weight of the top ply of the paper product).
[0087] The top ply slurry may be applied by any suitable application method. In one embodiment, the top ply slurry is applied through a non-pressurized or pressurized slot applicator having an opening located above the wet substrate on the wire of the wet end of the paper machine. Examples of known applicators that may be used include, but are not limited to, air knife coaters, blade coaters, rod coaters, bar coaters, multi-head coaters, roll coaters, roll or blade coaters, cast coaters, laboratory coaters, gravure coaters, kiss coaters, slot die coaters (including, for example, non-contact metering slot die coaters), jet coaters, liquid application systems, reverse roll coaters, headboxes, secondary headboxes, curtain coaters, spray coaters, and extrusion coaters.
[0088] In some embodiments, the top ply slurry is applied using a curtain coater. Further, in some embodiments where the top ply slurry is applied as a white top liner layer, the use of a curtain coater eliminates the need for a twin headbox paper machine and the associated costs and energy.
[0089] In one embodiment, the top pry slurry is spray applied, for example, using a spray coater.
[0090] In the process, the use of a high solids composition is desirable because less water is left behind to be drained, however, as is well known in the art, the solids level should not be so high that high viscosity and leveling problems occur.
[0091] The coating method may be carried out using a suitable applicator, such as an air knife coater, blade coater, rod coater, bar coater, multi-head coater, roll coater, roll or blade coater, cast coater, laboratory coater, gravure coater, kiss coater, slot die coater (including, for example, non-contact metering slot die coater, and non-pressurized or pressurized slot coater), jet coater, liquid coating system, reverse roll coater, headbox, secondary headbox, curtain coater, spray coater or extrusion coater to apply the top ply to the substrate.
[0092] In one embodiment, the top ply slurry is applied as a coating to the substrate by a non-pressurized or pressurized slot opening onto the wet substrate on a wire in the wet end of a paper machine, such as a Fourdrinier machine.
[0093] In some embodiments, the pulp wet web comprises more than about 50% water by weight based on the total weight of the pulp wet web, for example, at least about 60%, or at least about 70%, or at least about 80%, or at least about 90% water by weight based on the total weight of the pulp wet web. Typically, the pulp wet web comprises about 85-95% water by weight.
[0094] In one embodiment, the top ply slurry contains inorganic particulate material and a sufficient amount of microfibrillated cellulose to obtain a paper product having a top ply that contains at least about 5% by weight of microfibrillated cellulose, based on the total weight of the top ply, and such that the paper product has enough microfibrillated cellulose to obtain a paper product with the necessary strength properties for its end use.
[0095] In some embodiments, the top ply slurry contains a sufficient amount of inorganic particulate material to obtain a paper product having a top ply containing at least about 67% by weight of inorganic particulate material, based on the total weight of the top ply of the paper product. In such embodiments, the objective is to incorporate as little microfibrillated cellulose as possible with as much inorganic particulate material as possible as a top layer on the surface of the substrate material. Thus, a ratio of inorganic particulate material to microfibrillated cellulose in the top ply is preferably 4:1 or greater.
[0096] In some embodiments, the top ply slurry has a total solids content of about 20% by weight or less, e.g., about 15% by weight or less, or 12% by weight or less, or about 10% by weight or less, or about 1% to about 10% by weight, or about 2% to 12% by weight, or about 5% to about 10% by weight, or about 1% to about 20% by weight, or about 2% to about 12% by weight. The relative amounts of inorganic particulate material and microfibrillated cellulose may be varied depending on the amount of each component desired in the final product.
[0097] After application of the top pry slurry and appropriate residence time, the paper product is pressed and dried using any suitable method.
[0098] Method for producing microfibrillated cellulose and inorganic particulate materials In certain embodiments, the microfibrillated cellulose may be prepared in the presence or absence of inorganic particulate material.
[0099] The microfibrillated cellulose is derived from a fibrous substrate containing cellulose. The fibrous substrate containing cellulose may be derived from any suitable raw material, such as wood, grasses (e.g., sugar cane, bamboo) or waste textiles (e.g., textile waste, cotton, hemp or flax). The fibrous substrate containing cellulose may be in the form of a pulp (i.e., a suspension of cellulose fibers in water) and may be prepared by any suitable chemical or mechanical treatment, or combination thereof. For example, the pulp may be a chemical pulp, or a chemi-thermomechanical pulp, or a mechanical pulp, or a recycled pulp, or a papermaking broken, or a papermaking waste stream, or a waste from a paper mill, or a dissolving pulp, a kenaf pulp, a market pulp, a partially carboxymethylated pulp, an abaca pulp, a hemlock pulp, a birch pulp, a grass pulp, a bamboo pulp, a palm pulp, a peanut shell, or a combination thereof. Cellulose pulp is generally known in the art as having a Canadian Standard Freeness (CSF) of cm 3 The pulp may be beaten (e.g., in a Valley beater) and / or otherwise refined (e.g., processing in a conical or plate refiner) to a predefined freeness, reported in 2001. CSF refers to the freeness or drainage rate value of the pulp, measured by the rate at which a pulp suspension can be drained. For example, cellulose pulp has a freeness of about 10 cm before microfibrillation. 3 The cellulose pulp may have a Canadian Standard Freeness of about 700 cm 3 For example, about 650 cm 3 Less than or equal to 600cm 3 Less than or equal to 550cm 3 Less than or equal to 500cm 3 Less than or equal to 450cm 3 Less than or equal to 400cm 3 Less than or equal to 350cm 3 Less than or equal to 300cm 3 Less than or equal to 250cm 3 Less than or equal to 200cm 3 Less than or equal to 150cm 3 Less than or equal to 100cm 3Less than or equal to 50cm 3 The CSFs may be:
[0100] The cellulose pulp may then be dewatered by methods well known in the art, for example, the pulp may be filtered through a screen to obtain a wet sheet containing at least about 10% solids, for example at least about 15% solids, or at least about 20% solids, or at least about 30% solids, or at least about 40% solids. The pulp may be utilized in an unbeaten state, i.e., without being beaten or dewatered or otherwise refined.
[0101] In some embodiments, the pulp may be beaten in the presence of an inorganic particulate material such as calcium carbonate.
[0102] In the preparation of microfibrillated cellulose, the fibrous substrate containing cellulose may be added in a dry state to a grinding vessel or homogenizer. For example, dry paper fragments may be added directly to the grinding vessel. The aqueous environment in the grinding vessel will then promote the formation of a pulp.
[0103] The microfibrillation step may be carried out in any suitable equipment, including but not limited to a refiner. In one embodiment, the microfibrillation step is carried out in a grinding vessel under wet grinding conditions. In another embodiment, the microfibrillation step is carried out in a homogenizer. Each of these embodiments is described in more detail below.
[0104] Wet grinding The grinding is suitably carried out in a conventional manner. The grinding may be an attrition grinding process in the presence of a particulate grinding medium, or an autogenous grinding process, i.e., in the absence of a grinding medium. By grinding medium is meant a medium other than an inorganic particulate material that may be co-ground with the fibrous substrate, including cellulose, in an embodiment.
[0105] Particulate grinding media, when present, may be of natural or synthetic material. Grinding media may include, for example, balls, beads, or pellets of any hard mineral, ceramic, or metallic material. Such materials may include, for example, alumina, zirconia, zirconium silicate, aluminum silicate, or mullite-rich materials produced by calcining kaolin clay at temperatures ranging from about 1300° C. to about 1800° C. For example, in some embodiments, Carbolite® grinding media is used. Alternatively, natural sand particles of suitable particle size may be used.
[0106] In one embodiment, hardwood grinding media (eg, wood flour) may be used.
[0107] In general, the type and particle size of the grinding media selected for use in the present invention may depend on the characteristics of the feed suspension of the material to be ground, such as particle size and chemical composition. In some embodiments, the particulate grinding media comprises particles having an average diameter in the range of about 0.1 mm to about 6.0 mm, such as about 0.2 mm to about 4.0 mm. The grinding media(s) may be present in an amount of about 70% or less by volume of the input. The grinding media may be present in an amount of at least about 10% by volume of the input, such as at least about 20% by volume of the input, or at least about 30% by volume of the input, or at least about 40% by volume of the input, or at least about 50% by volume of the input, or at least about 60% by volume of the input.
[0108] Comminution can be carried out in one or more stages: for example, coarse inorganic particulate material can be milled in a milling vessel to a predetermined particle size distribution, after which fibrous material containing cellulose is added and milling continued until a desired level of microfibrillation is obtained.
[0109] The inorganic particulate material may be wet or dry milled in the absence or presence of grinding media. In the case of wet milling, the coarse inorganic particulate material is milled in an aqueous suspension in the presence of grinding media.
[0110] In one embodiment, the average particle size (d 50 ) decreases during the co-grinding process. For example, the d 50 can be reduced by at least about 10% (as measured by a Malvern Mastersizer S machine), e.g., the d 50 may be reduced by at least about 20%, or at least about 30%, or at least about 50%, or at least about 60%, or at least about 70%, or at least about 80%, or at least about 90%. For example, a d of 2.5 μm before co-milling may be reduced by at least about 20%, or at least about 30%, or at least about 50%, or at least about 60%, or at least about 70%, or at least about 80%, or at least about 90%. 50 After co-milling, the d 50 would have undergone a 40% particle size reduction.
[0111] In one embodiment, the average particle size of the inorganic particulate material is not significantly reduced during the co-grinding process. 50 This means that the decrease in d of inorganic particulate materials is less than about 10%. 50 The decrease is less than about 5%.
[0112] Fibrous substrates containing cellulose have a d in the range of about 5 μm to about 500 μm as measured by laser light scattering. 50 The cellulose-containing fibrous substrate may be microfibrillated, optionally in the presence of inorganic particulate material, to obtain microfibrillated cellulose having a d of about 400 μm or less, for example, about 300 μm or less, or about 200 μm or less, or about 150 μm or less, or about 125 μm or less, or about 100 μm or less, or about 90 μm or less, or about 80 μm or less, or about 70 μm or less, or about 60 μm or less, or about 50 μm or less, or about 40 μm or less, or about 30 μm or less, or about 20 μm or less, or about 10 μm or less. 50 The cellulose may be microfibrillated, optionally in the presence of inorganic particulate material, to obtain a microfibrillated cellulose having
[0113] Fibrous substrates comprising cellulose may be microfibrillated, optionally in the presence of inorganic particulate material, to obtain microfibrillated cellulose having a modal fiber particle size in the range of about 0.1 to 500 μm, and a modal inorganic particulate material particle size in the range of 0.25 to 20 μm. Fibrous substrates comprising cellulose may be microfibrillated, optionally in the presence of inorganic particulate material, to obtain microfibrillated cellulose having a modal fiber particle size of at least about 0.5 μm, for example at least about 10 μm, or at least about 50 μm, or at least about 100 μm, or at least about 150 μm, or at least about 200 μm, or at least about 300 μm, or at least about 400 μm.
[0114] A fibrous substrate comprising cellulose may be microfibrillated, optionally in the presence of inorganic particulate material, to obtain microfibrillated cellulose having a fiber gradient as described above.
[0115] Grinding can be carried out, for example, in a rotary mill (e.g., rod, ball and autogenous grinding), an agitated mill (e.g., SAM or IsaMill), a tower mill, a stirred media detritor (SMD), or a grinding vessel, such as a grinding vessel containing rotating parallel grinding plates between which the feedstock to be ground is fed.
[0116] In one embodiment, the grinding tank is a tower mill. The tower mill may include a stationary zone above one or more grinding zones. The stationary zone is a region located toward the top of the interior of the tower mill where minimal or no grinding occurs and contains microfibrillated cellulose and any inorganic particulate material. The stationary zone is a region where particles of grinding media settle into one or more grinding zones of the tower mill.
[0117] The tower mill may include a classifier above one or more grinding zones. In one embodiment, the classifier is mounted at the top and located adjacent to the stationary zone. The classifier may be a hydrocyclone.
[0118] The tower mill may include a screen above one or more grinding zones. In one embodiment, the screen is located adjacent to the quiescent zone and / or the classifier. The screen may be sized to separate the grinding media from the product aqueous suspension containing the microfibrillated cellulose and any inorganic particulate material and to enhance settling of the grinding media.
[0119] In one embodiment, the grinding is carried out under plug flow conditions. Under plug flow conditions, the flow through the tower is such that the mixing of the grinding material through the tower is limited. This means that at different points along the length of the tower mill, the viscosity of the aqueous environment changes as the fineness of the microfibrillated cellulose increases. Thus, in effect, the grinding region in the tower mill can be considered to include one or more grinding zones with characteristic viscosities. Those skilled in the art will understand that there is no sharp boundary in terms of viscosity between adjacent grinding zones.
[0120] In one embodiment, water is added at the top of the mill adjacent to the stationary zone above one or more grinding zones or to the classifier or screen to reduce the viscosity of the aqueous suspension containing microfibrillated cellulose and any inorganic particulate material in these zones of the mill. It has been found that diluting the product microfibrillated cellulose and any inorganic particulate material at this point in the mill improves the prevention of carryover of grinding media to the stationary zone and / or to the classifier and / or screen. Furthermore, limited mixing through the tower allows processing at higher solids content further down the tower and allows dilution at the top with limited backflow of dilution water down the tower into one or more grinding zones. Any suitable amount of water effective to reduce the viscosity of the product aqueous suspension containing microfibrillated cellulose and any inorganic particulate material can be added. Water can be added continuously, at regular intervals, or at irregular intervals during the grinding process.
[0121] In another embodiment, water can be added to one or more grinding zones via one or more water injection points positioned along the length of the tower mill, or each water injection point is located at a point corresponding to one or more grinding zones. Advantageously, the ability to inject water at various points along the tower allows for further adjustment of grinding conditions at any or all positions along the mill.
[0122] A tower mill may include a vertical impeller shaft with a series of impeller rotor disks running along its length, the action of which creates a series of distinct grinding zones throughout the mill.
[0123] In another embodiment, the grinding is carried out in a screen grinder, such as a stirred media detritor. The screen grinder may include one or more screens having a nominal opening size of at least about 250 μm, for example, the one or more screens may have a nominal opening size of at least about 300 μm, or at least about 350 μm, or at least about 400 μm, or at least about 450 μm, or at least about 500 μm, or at least about 550 μm, or at least about 600 μm, or at least about 650 μm, or at least about 700 μm, or at least about 750 μm, or at least about 800 μm, or at least about 850 μm, or at least about 900 μm, or at least about 1000 μm.
[0124] The screen sizes listed immediately above are applicable to the tower mill embodiments described above.
[0125] As mentioned above, the grinding may be carried out in the presence of a grinding medium, in one embodiment, the grinding medium is a coarse medium comprising particles having an average diameter ranging from about 1 mm to about 6 mm, e.g., about 2 mm, or about 3 mm, or about 4 mm, or about 5 mm.
[0126] In another embodiment, the grinding media has a specific gravity of at least about 2.5, e.g., at least about 3, or at least about 3.5, or at least about 4.0, or at least about 4.5, or at least about 5.0, or at least about 5.5, or at least about 6.0.
[0127] In another embodiment, the grinding media comprises particles having an average diameter in the range of about 1 mm to about 6 mm and has a specific gravity of at least about 2.5.
[0128] In another embodiment, the grinding media comprises particles having an average diameter of about 3 mm and a specific gravity of about 2.7.
[0129] As noted above, the grinding media(s) may be present in an amount up to about 70% by volume of the input. The grinding media may be present in an amount of at least about 10% by volume of the input, such as at least about 20% by volume of the input, or at least about 30% by volume of the input, or at least about 40% by volume of the input, or at least about 50% by volume of the input, or at least about 60% by volume of the input.
[0130] In one embodiment, the grinding media is present in an amount of about 50% by volume of the charge.
[0131] The term "feed" refers to the composition that is the feedstock that is provided to the grinding vessel. The feed includes water, grinding media, fibrous substrates including cellulose, and any inorganic particulate materials, and any other additives as described herein.
[0132] The use of relatively coarse and / or dense media has the advantage of improved (i.e. faster) settling velocity and reduced carryover of media through the quiescent zone and / or classifier and / or screen(s).
[0133] A further advantage of using relatively coarse grinding media is that the average particle size (d 50) is not significantly reduced, the energy input to the grinding system is primarily used for microfibrillation of the cellulose-containing fibrous substrate.
[0134] An additional advantage of using a relatively coarse screen is that a relatively coarse or dense grinding media can be used in the microfibrillation process. In addition, the use of a relatively coarse screen (i.e., having a nominal opening size of at least about 250 μm) allows for the processing and removal of relatively high solids products from the grinder, thereby allowing relatively high solids feedstocks (including fibrous substrates and inorganic particulate materials, including cellulose) to be processed in a commercially viable process. As described below, it has been found that feedstocks with high initial solids content are desirable from an energy efficiency standpoint. It has also been found that products produced at lower solids (for a given energy) have a coarser particle size distribution.
[0135] The grinding is carried out in a cascade of grinding tanks, one or more of which may contain one or more grinding zones. For example, fibrous substrates containing cellulose and inorganic particulate materials may be ground in a cascade of two or more grinding tanks, for example a cascade of three or more grinding tanks, or a cascade of four or more grinding tanks, or a cascade of five or more grinding tanks, or a cascade of six or more grinding tanks, or a cascade of seven or more grinding tanks, or a cascade of eight or more grinding tanks, or a cascade of nine or more grinding tanks in series, or a cascade containing ten or fewer grinding tanks. The cascade of grinding tanks may be operatively connected in series, or in parallel, or in a combination of series and parallel. The output from one or more of the grinding tanks and / or the input to one or more of the grinding tanks constituting the cascade may be subjected to one or more screening steps and / or one or more classification steps.
[0136] The circuit may include one or more grinding bed and homogenizer combinations.
[0137] In one embodiment, the grinding is performed in a closed circuit. In another embodiment, the grinding is performed in an open circuit. The grinding can be performed in a batch mode. The grinding can be performed in a recirculating batch mode.
[0138] As mentioned above, the grinding circuit may include a pre-grinding step in which coarse inorganic particles are ground to a predetermined particle size distribution in a grinding vessel, after which the fibrous material comprising cellulose is combined with the pre-ground inorganic particulate material and grinding is continued in the same or a different grinding vessel until the desired level of microfibrillation is obtained.
[0139] Since the suspension of the material to be milled may be relatively viscous, a suitable dispersing agent may be added to the suspension before milling. The dispersing agent may be, for example, a water-soluble condensed phosphate, a polysilicic acid or salt thereof, or a polyelectrolyte, for example a water-soluble salt of poly(acrylic acid) or poly(methacrylic acid) having a number average molecular weight of 80,000 or less. The amount of dispersing agent used will generally be in the range of 0.1 to 2.0% by weight based on the weight of the dry inorganic particulate solid material. The suspension may be suitably milled at a temperature in the range of 4°C to 100°C.
[0140] Other additives that may be included in the microfibrillation process include carboxymethylcellulose, amphoteric carboxymethylcellulose, oxidizing agents, 2,2,6,6-tetramethylpiperidine-1-oxyl (TEMPO), TEMPO derivatives, and wood degrading enzymes.
[0141] The pH of the suspension of the material to be ground may be about 7 or greater than about 7 (i.e., basic), for example, the pH of the suspension may be about 8, or about 9, or about 10, or about 11. The pH of the suspension of the material to be ground may be less than about 7 (i.e., acidic), for example, the pH of the suspension may be about 6, or about 5, or about 4, or about 3. The pH of the suspension of the material to be ground may be adjusted by the addition of a suitable amount of acid or base. Suitable bases include alkali metal hydroxides, such as NaOH. Other suitable bases are sodium carbonate and ammonia. Suitable acids include inorganic acids, such as hydrochloric acid and sulfuric acid, or organic acids. An exemplary acid is orthophosphoric acid.
[0142] The amount of inorganic particulate material, if present, and the amount of cellulose pulp in the co-ground mixture may be varied or further adjusted, for example with the addition of additional inorganic particulate material, to produce a slurry suitable for use as a top pry slurry or pry slurry.
[0143] Homogenization Microfibrillation of fibrous substrates comprising cellulose can be achieved by a method in which a mixture of cellulose pulp and any inorganic particulate material is pressurized (e.g., up to a pressure of about 500 bar) under wet conditions, optionally in the presence of inorganic particulate material, and then sent to a lower pressure zone. The velocity of the mixture sent to the lower pressure zone is high enough, and the pressure in the lower pressure zone is low enough to cause microfibrillation of the cellulose fibers. For example, the pressure drop can be caused by forcing the mixture through an annular opening with a narrow inlet orifice and a much wider outlet orifice. The sudden pressure drop as the mixture accelerates into a larger volume (i.e., the lower pressure zone) induces cavitation, which causes microfibrillation. In one embodiment, microfibrillation of fibrous substrates comprising cellulose can be achieved in a homogenizer under wet conditions, optionally in the presence of inorganic particulate material. In the homogenizer, the cellulose pulp and any inorganic particulate material are pressurized (e.g., up to a pressure of about 500 bar) and forced through a small nozzle or orifice. The mixture may be pressurized to a pressure of about 100 bar to about 1000 bar, for example, 300 bar or more, or about 500 bar or more, or about 200 bar or more, or about 700 bar or more. Homogenization subjects the fibers to high shear forces, and as the pressurized cellulose pulp exits the nozzle or orifice, cavitation causes microfibrillation of the cellulose fibers in the pulp. Additional water may be added to improve the flowability of the suspension through the homogenizer. The resulting aqueous suspension containing the microfibrillated cellulose and any inorganic particulate material may be returned to the inlet of the homogenizer for multiple passes through the homogenizer. If inorganic particulate material is present, and if the inorganic particulate material is a naturally occurring plate-like mineral such as kaolin, homogenization may promote not only microfibrillation of the cellulose pulp, but also exfoliation of the plate-like particulate material.
[0144] An exemplary homogenizer is a Manton Gaulin (APV) homogenizer.
[0145] After the microfibrillation step, the aqueous suspension containing the microfibrillated cellulose and any inorganic particulate material may be sieved to remove fibers larger than a certain size and any grinding media. For example, the suspension may be sieved using a sieve with a selected nominal opening size to remove fibers that do not pass through the sieve. By nominal opening size is meant the nominal center distance between the opposite sides of a square opening, or the nominal diameter of a circular opening. The sieve may be a BSS sieve (according to BS 1796) with a nominal opening size of 150 μm, for example 125 μm, or 106 μm, or 90 μm, or 74 μm, or 63 μm, or 53 μm, 45 μm, or 38 μm. In one embodiment, the aqueous suspension is sieved using a BSS sieve with a nominal opening size of 125 μm. The aqueous suspension may then be optionally dewatered.
[0146] As a result, it will be appreciated that once the milled or homogenized suspension has been treated to remove fibers larger than a selected size, the amount (i.e., weight percent) of microfibrillated cellulose in the aqueous suspension after milling or homogenization will be less than the amount of dry fibers in the pulp. Thus, the relative amounts of pulp and any inorganic particulate material fed to the mill or homogenizer can be adjusted depending on the amount of microfibrillated cellulose required in the aqueous suspension after removal of fibers larger than a selected size.
[0147] In some embodiments, microfibrillated cellulose may be prepared by a method comprising microfibrillating a fibrous substrate comprising cellulose by grinding in an aqueous environment in the presence of a grinding medium (as described herein), the grinding being carried out in the absence of inorganic particulate material. In some embodiments, inorganic particulate material may be added after grinding to produce a top ply slurry or ply slurry.
[0148] In some embodiments, the grinding media is removed after grinding.
[0149] In other embodiments, the grinding media is retained after grinding and serves as, or at least a portion of, the inorganic particulate material. In some embodiments, additional inorganic particulate material may be added after grinding to produce a top pry slurry or pry slurry.
[0150] The following procedure can be used to characterize the particle size distribution of a mixture of inorganic particulate material (eg, GCC or kaolin) and microfibrillated cellulose pulp fibers.
[0151] Calcium carbonate A sample of the co-ground slurry sufficient to obtain 3 g of dry material was weighed into a beaker, diluted to 60 g with deionized water, and diluted with 5 cm of a solution of sodium polyacrylate with an active ingredient of 1.5 w / v%. 3 Then add deionized water with stirring until the final slurry weight is 80 g.
[0152] Kaolin A sample of the co-ground slurry sufficient to give 5 g of dry material was weighed into a beaker, diluted to 60 g with deionized water, and diluted with 5 cm of a solution of 1.0 wt. % sodium carbonate and 0.5 wt. % sodium hexametaphosphate. 3 Then add deionized water with stirring until the final slurry weight is 80 g.
[0153] The slurry was then diluted with water in a sample preparation unit attached to a Mastersizer S until it showed an optimal level of obscuration (usually 10–15%). 3 Next, perform the light scattering analysis procedure. The instrument range selected was 300RF:0.05-900, and the beam length was set to 2.4 mm.
[0154] For co-ground samples containing calcium carbonate and fiber, the refractive index of calcium carbonate (1.596) is used. For co-ground samples of kaolin and fiber, the refractive index of kaolin (1.5295) is used.
[0155] The particle size distribution is calculated from Mie theory and output as a volume-difference based distribution. The presence of two distinct peaks is interpreted as being due to minerals (finer peak) and fibers (coarser peak).
[0156] The finer mineral peak is fitted to the measured data points and mathematically subtracted from the distribution leaving the fiber peak, which is converted to a cumulative distribution. Similarly, the fiber peak is mathematically subtracted from the original distribution leaving the mineral peak, which is also converted to a cumulative distribution. Both of these cumulative curves are then fitted to the mean particle size (d 50 ) and the gradient of the distribution (d 30 / d 70 x 100). Differential curves may be used to determine the modal particle size for both the mineral and fibrous fractions.
[0157] Working Example Example 1 1. 150g / m 2 Brown sheets were produced on a handsheet. Percol® 292 was used as a retention aid at 600 ppm based on total solids in the final handsheet. 2. Once the brown sheet had formed, the retained water was removed by manually squeezing the sheet with three pieces of absorbent paper. No adhesion was observed between the absorbent paper and the sheet. 3. The brown base sheet was then turned upside down so that its smoother side was facing up. 4. To obtain the desired basis weight for the white top layer, specific amounts of microfibrillated Botnia pine bleached kraft pulp and calcium carbonate (Intracarb 60) at 7.88% total solids content by weight (18% microfibrillated cellulose) were measured (20 g / m 2 , 25g / m 2 , 30g / m 2 , 40g / m 2 , and 50 g / m 2 The sheets were then diluted to a final volume of 300 ml using tap water. 5. The sample was poured onto a brown sheet and a vacuum was applied. Polydadmac (0.2% solution, 1 ml) was used to induce the formation of a white top layer. 6. The waste water was then collected and returned to the formed sheet where a vacuum was applied for 1 minute. 7. The 2-ply sheet was transferred to a Rapid Kothen dryer (approximately 89°C, 1 bar) for 15 minutes. 8. The sample left in the residual water (see step 6) was collected on a filter paper and used to calculate the actual basis weight of the white tops for each individual sheet. 9. Each sheet was then left overnight in a conditioned laboratory prior to testing.
[0158] result: The structure of the sheets produced at the various basis weights is shown in Figure 1. The images were obtained as reflectance scans under identical conditions using a standard scanner so that they could be directly compared with each other.
[0159] The whiteness of the produced sheets is shown in Figure 2. The white top liner g / m 2 Brightness increased with increasing temperature. Brightness measurements on the brown side of the two-ply sheet showed that no penetration of the white top layer into the brown sheet had occurred.
[0160] The PPS roughness decreased with higher white top layer basis weight (see Figure 3). The roughness value of the brown sheet alone was 7.9 μm, indicating that the surface became smoother with increasing top layer basis weight.
[0161] Example 2 Tests 1-4 The Fourdrinier machine was operated at 60 ft / min (18 m / min). The coating was applied using a "secondary headbox," a custom-built device in which the furnish flows into a series of "ponds" and then over a weir onto the web. Because the custom-built secondary headbox does not require the same high flow rates to form a curtain as the GL&V Hydrasizer, it was possible to increase the microfibrillated cellulose and inorganic particulate material solids used and still achieve the target coating weight. Running at higher solids meant that the secondary headbox could be located further from the main headbox, in a position where the sheet was more compact, but the microfibrillated cellulose and inorganic particulate material slurry applied as the top ply could still be fully dewatered before pressing.
[0162] A secondary headbox was placed just after the wet line and a 1:1 ratio of microfibrillated cellulose to organic particulate material was applied to explore the boundaries of the process. It was clear that the 1:1 ratio microfibrillated cellulose to organic particulate material slurry drained faster than the 1:4 ratio of microfibrillated cellulose to organic particulate material, despite the higher basis weight of microfibrillated cellulose applied to the substrate. The coating was initially applied at 15 g / m 2 and then 30g / m 2 At a 1:1 ratio of microfibrillated cellulose to organic particulate material, although the coverage was good, the filler content was not high enough to obtain the desired whiteness.
[0163] Top layer g / m from sheet weight and ash content 2 The calculation was carried out as follows: W=weight, A=ash content Subscript t=top layer, b=bottom layer, s=two-layer sheet
[0164] The total ash content of the sheet is the sum of the ash content times the weight of each layer divided by the weight of the entire sheet.
number
[0165] The ash content of the bottom layer was measured on an uncoated control sheet, and the ash content of the top layer is directly related to the weight percent of the microfibrillated and inorganic particulate matter slurry. Observation and SEM cross sections of the sheets show that no penetration of the microfibrillated and inorganic particulate matter into the base of the top ply slurry composite occurs, thus achieving 100% retention. The weight of the bottom layer is W b =W s -W t , it can be removed from the above equation and therefore the above equation can be rearranged to give the weight of the top layer in terms of known quantities.
number
[0166] Tests 1-4 A series of additional trials were conducted using the configuration used in Trial 1. The Fourdrinier was utilized with different coating weights on a 100% softwood unbleached kraft base that was refined to approximately 500 ml of CSF. The top ply consisted of 20% microfibrillated cellulose, 80% mineral and a small amount of flocculant. result: The results are reported in Table 1. The following abbreviations are used in Table 1: BP: Base paper without coating T1: Approx. 28g / m 2 Composite top coating, 20% microfibrillated cellulose, 80% GCC. T2: Approx. 35g / m 2 Composite top coating, 20% microfibrillated cellulose, 80% GCC. T3: approx. 42g / m 2 Composite top coating, 20% microfibrillated cellulose, 80% GCC. T4: approx. 48g / m 2Composite top coating of 20% microfibrillated cellulose, 20% GCC, 60% talc. [Table 1]
[0167] The test was performed at 28 g / m 2 ~48g / m 2 The results for brightness, air permeability and smoothness are shown for various coating weights ranging from 100% to 150%. The Scott bond was not affected as the Z-strength test failures always occurred in the base sheet, i.e. the top ply was stronger than the base. Brightness versus coating weight is plotted in Figure 4.
[0168] A scanning electron microscope image of the substrate coated at test point T2 is shown in Figure 5. 2 A 35 g / m2 composite consisting of 20% by weight microfibrillated cellulose and 80% by weight ground calcium carbonate was applied to the substrate. 2 The top ply was applied at 48 g / m2. It is clear from Figure 5 that the top ply was formed as a separate top layer without penetration into the base substrate. Figure 6 shows the SEM image at test point 4. The coating was applied at 48 g / m2. 2 and applied at 85 g / m 2 The top ply applied to the substrate comprises 20% by weight microfibrillated cellulose and 20% by weight ground calcium carbonate and 60% by weight talc (i.e., a 1:4 ratio of microfibrillated cellulose and inorganic particulate material). Figure 6 clearly shows that the top ply is applied so that it desirably remains as a layer on the surface of the substrate.
[0169] Comparative Test Table 2 below shows the 82g / m 2 The data presented is for a conventional white top linerboard made on a similar paper machine utilizing a conventional top ply applied to a base substrate of 80 g / m. The base was made from unbleached softwood kraft fiber and the white top layer was made from bleached hardwood (birch) kraft fiber with a typical filler loading range of 20% or less. The substrate was 80 g / m. 2The white layer is 60g / m 2 was targeted. Table 2 shows typical results without microfibrillated cellulose, where a loading of 15 wt% Soekarnohedral PCC (Optical HB) was used for the white layer. It can be seen that the base was rather stronger than those in Tests 1-4 above, but the drop in mechanical property index with the addition of the top layer was also quite large. If the top ply layer in Tests 1-4 can reach the targeted whiteness at a lower basis weight than the conventional white top substrate, then the use of FiberLean for a fixed total basis weight allows the board maker to use a higher proportion of unbleached long fibers in the product, thus resulting in a stronger and stiffer product.
[0170] Table 2 below shows typical paper properties for various conventional linerboard grades. [Table 2]
[0171] Demonstration of the printing properties of the white top linerboard of the present invention. Figure 7 shows a cross section of a flexographically printed sample. The ink is on the top ply, just as it should be.
[0172] Example 3 The continuous production of coated substrates with different coating weights and base substrates was studied according to the configurations and parameters described in Examples 1 and 2. Tests 5 to 7 were run at 70 g / m 2 Base papers (BP) made of 70% hardwood and 30% softwood refined together in approximately 400 ml of CSF were utilized with a target basis weight of 1. The coatings applied to the BP in trials 5-7 are identified as follows: T5, approx. 20g / m on base paper BP 2 Composite coating (20% MFC, 80% GCC, no additives) T6, about 30g / m on base paper BP 2 Composite coating (20% MFC, 80% GCC, no additives) T7, approx. 40 g / m on base paper BP2 of composite coating (20% MFC, 80% GCC, no additives).
[0173] The data obtained in tests 5 to 7 are shown in Table 3. [Table 3]
[0174] From the data presented in Table 4, it is apparent that in all runs of Tests 5-7, the target brightness of the top ply coated on the dark substrate was achieved.
[0175] Example 4 Print property data for the top ply coated linerboard substrate is shown in Table 4.
[0176] Comparative Reference 1 and Comparative Reference 2 comprise a commercially available coated inkjet paper and a commercially available uncoated inkjet paper, respectively. The print samples consist of: a porous base (70% hardwood and 30% softwood, approximately 400 mL CSF, 70 g / m 2 ) 30g / m 2 Composite coating of (20% MFC, 80% GCC). Paper obtained in a continuous manufacturing process. Printed samples were prepared according to example 3. Roll-to-roll inkjet printing applied at 50 m / min.
[0177] The print results of Comparative Reference 1 (specialty inkjet paper, coated and calendared) and Comparative Reference 2 (uncoated paper suitable for inkjet) versus print samples of embodiments of the present invention are shown in Table 4. [Table 4]
[0178] This application also includes the following inventions. (1) A paper or paperboard product comprising: (i) a cellulose-containing substrate; (ii) a top ply comprising an inorganic particulate material, and at least about 5% by weight, based on the total weight of the top ply, of microfibrillated cellulose; the inorganic particulate material content being about 67% by weight to about 92% by weight based on the total weight of the top ply, and the top ply having a brightness as measured by ISO standard 11475 (F8; D65-400 nm) of at least about 65%. Paper or paperboard products. (2) 13. The product of claim 1, wherein the product comprises or is a white top cardboard product. (3) 13. The product of claim 1, wherein the product comprises or is a white top paperboard product. (4) The substrate has a thickness of about 50 g / m 2 ~about 500g / m 2 and / or the top ply has a basis weight suitable for use in cardboard products, including a basis weight in the range of about 15 g / m 2 ~40g / m 2 The product described in (2) having a basis weight in the range of. (5) The top ply is about 15 to 40 g / m 2 The product according to (4), having a basis weight of (6) 2. The article of claim 1, wherein the substrate comprises recycled pulp, dark kraft, or a combination thereof. (7) 2. The product of claim 1, wherein the microfibrillated cellulose is present in the top ply in an amount of about 5% to about 30% by weight. (8) 2. The article of claim 1, wherein the inorganic particulate material and the microfibrillated cellulose constitute greater than 95% by weight of the top ply, based on the total weight of the top ply. (9) 2. The article of claim 1, wherein the top ply comprises at least 70% by weight of inorganic particulate material, based on a total weight of the top ply. (10) 2. The article of claim 1, wherein the top ply comprises at least about 80% by weight of inorganic particulate material, based on a total weight of the top ply. (11) 2. The article of claim 1, wherein the top ply comprises at least about 10% to about 20% by weight of microfibrillated cellulose, based on a total weight of the top ply. (12) 2. The product of claim 1, wherein the top ply comprises at least one inorganic particulate material selected from the group consisting of calcium carbonate, magnesium carbonate, dolomite, gypsum, anhydrous kandite clay, kaolin, perlite, diatomaceous earth, wollastonite, talc, magnesium hydroxide, titanium dioxide, or aluminum trihydrate, or combinations thereof. (13) 13. The product of claim 12, wherein the inorganic particulate material comprises or is calcium carbonate. (14) The article of claim 1, wherein the PPS roughness (@1000 kPa) measured for the top ply is about 6.0 μm or less, and / or the PPS roughness (@1000 kPa) measured for the top ply is at least 2.0 μm less than the PPS roughness of the substrate without the top ply. (15) 2. The product of claim 1, wherein the top ply comprises up to about 2% by weight of additives selected from the group consisting of flocculants, formation / drainage aids, water soluble thickeners, starches, retention aids, and combinations thereof. (16) 2. The article of claim 1, wherein the top ply does not contain added organic compounds. (17) 17. The article of claim 16, wherein the top ply does not contain a cationic polymer, an anionic polymer, or a polysaccharide hydrocolloid. (18) 2. The article of claim 1, wherein the top ply is an outer ply. (19) 2. The article of claim 1, wherein the top ply is free of wax, polyolefins, and silicones. (20) A paper or paperboard product comprising: and a top ply comprising at least about 10% by weight of microfibrillated cellulose based on the total weight of the top ply, said top ply comprising at least about 15 g / m 2 ~40g / m 2 present in an amount of Paper or paperboard products. (twenty one) 21. The article of claim 20, wherein the substrate comprises about 1 wt. % or less of a retention aid, based on the total weight of the substrate. (twenty two) 21. The article of claim 20, wherein the top ply consists essentially of, or consists of, inorganic particles and microfibrillated cellulose. (twenty three) 21. The article of claim 20, wherein the top ply comprises about 30% by weight or less of microfibrillated cellulose, based on the total weight of the top ply. (twenty four) 21. The article of claim 20, further comprising an additional layer or ply(s) on top of the ply comprising at least about 30% by weight of microfibrillated cellulose based on the total weight of the top ply. (twenty five) 25. The product of claim 24, wherein at least one of the further layers or plies is a barrier layer or ply, or a wax layer or ply, or a silicone layer or ply. (26) 1. A method of making a paper or board product comprising the steps of: (a) providing a wet web of pulp; (b) providing a top ply slurry onto said wet web of pulp; Including, (i) The top ply slurry is 15 g / m 2 ~40g / m 2 Available in amounts ranging from (ii) the top ply slurry comprises microfibrillated cellulose in an amount sufficient to provide a product having a top ply comprising at least about 5% by weight of microfibrillated cellulose, based on the total weight of the top ply; (iii) the top ply slurry comprises an amount of inorganic particulate material sufficient to provide a product having a top ply comprising at least 67 weight percent inorganic particulate material, based on a total weight of the top ply; method. (27) 27. The method according to claim 26, wherein the top ply slurry is applied onto a wet substrate on a wire in the wet end of a paper machine using an applicator suitable for forming a film through a non-pressurized or pressurized slot opening. (28) 27. The method of claim 26, wherein the pulp wet web comprises greater than about 50% by weight water, based on the total weight of the pulp wet web. (29) 27. The method of claim 26, wherein the pulp wet web comprises about 1 wt. % or less of a retention aid, based on the total weight of the pulp wet web. (30) 27. The method of claim 26, wherein the top ply slurry comprises inorganic particulate material and a sufficient amount of microfibrillated cellulose to provide a paper product having a top ply comprising at least about 15% by weight of microfibrillated cellulose, based on the total weight of the top ply. (31) 27. The method of claim 26, wherein the top ply slurry is applied onto the wet substrate on the wire in the wet end of the paper machine using a pressurized slot opening. (32) The method according to (26), wherein the top ply slurry is applied using a curtain coater. (33) 27. The method of claim 26, further comprising applying an additional layer or ply(s) onto the top ply comprising microfibrillated cellulose and inorganic particulate material. (34) 33. The method according to claim 32, wherein at least one of the further layers or plies is a barrier layer or ply, or a wax layer or ply, or a silicone layer or ply. (35) 21. The article of claim 20, wherein the top ply consists essentially of or consists of microfibrillated cellulose.
Claims
1. 1. A method of making a paper or paperboard product, comprising: (a) providing a substrate comprising a wet web of pulp, wherein the wet web of pulp comprises a cellulose-containing material selected from the group consisting of recycled pulp, paper broken, paper waste streams, paper mill waste, chemical pulp, or chemi-thermomechanical pulp, or mechanical pulp, or a combination thereof; (b) applying the top ply slurry through a slotted applicator positioned above the substrate to form a film on top of the substrate on the wire at the wet end of the papermaking machine; Including, (i) the top ply slurry comprises microfibrillated cellulose in an amount sufficient to provide a product having a top ply comprising 5% to 30% by weight of microfibrillated cellulose, based on the total weight of the top ply; (ii) the top ply slurry comprises an amount of inorganic particulate material sufficient to provide a product having a top ply comprising at least 67 weight percent inorganic particulate material, based on a total weight of the top ply; (iii) the total solids content of the top pry slurry is between 2% and 12% by weight; (iv) the top ply has a thickness of 10 g / m 2 ~50g / m 2 and having a basis weight in the range of (c) Dewatering and pressing the paper or paperboard product on a papermaking machine; (d) obtaining a paper or paperboard product comprising said top ply comprising microfibrillated cellulose and one or more inorganic particulate materials. method.
2. The method of claim 1 , wherein the cellulose-containing material comprises recycled pulp.
3. The method of claim 2 , wherein the recycled pulp comprises waste corrugated paper.
4. The method of claim 1 , wherein the pulp wet web comprises greater than 50% by weight water, based on the total weight of the pulp wet web.
5. 10. The method of claim 1, wherein the pulp wet web comprises no more than 1 weight percent retention aid, based on the total weight of the pulp wet web.
6. 2. The method of claim 1, wherein the top ply slurry comprises inorganic particulate material and a sufficient amount of microfibrillated cellulose to provide a paper product having a top ply comprising at least 5% by weight of microfibrillated cellulose, based on the total weight of the top ply.
7. 2. The method of claim 1, wherein the top ply slurry comprises inorganic particulate material and a sufficient amount of microfibrillated cellulose to obtain a paper product having a top ply comprising at least 10% by weight, or at least 15% by weight, or at least 20% by weight, or at least 25% by weight of microfibrillated cellulose, based on the total weight of the top ply.
8. 10. The method of claim 1, wherein the top ply slurry is applied onto the wet web of pulp on the wire in the wet end of the paper machine using a pressurized slot opening.
9. The method of claim 1 , wherein the paperboard product is a white top board product.
10. The substrate has a basis weight of 50 g / m2, which is suitable for use as a cardboard product. 2 Up to 500 g / m 2 The method of claim 1 having a basis weight in the range of
11. The method of claim 1 , wherein the at least one inorganic particulate material and the microfibrillated cellulose comprise greater than 95% by weight of the top ply, based on a total weight of the top ply.
12. The method of claim 1 , wherein the top ply comprises at least 70% by weight, or at least 80% by weight, of inorganic particulate material, based on a total weight of the top ply.
13. The method of claim 1 , wherein the top ply comprises at least 10% to 20% by weight of microfibrillated cellulose, based on a total weight of the top ply.
14. 10. The method of claim 1, wherein the top ply comprises at least one inorganic particulate material selected from the group consisting of calcium carbonate, magnesium carbonate, dolomite, gypsum, anhydrous kandite clay, kaolin, perlite, diatomaceous earth, wollastonite, talc, magnesium hydroxide, titanium dioxide, or aluminum trihydrate, or combinations thereof.
15. The method of claim 1 , wherein the inorganic particulate material comprises or is calcium carbonate.
16. 10. The method of claim 1, wherein the top ply comprises up to 2% by weight total of additives selected from the group consisting of flocculating agents, formation / drainage aids, water soluble thickeners, starches, retention aids, and combinations thereof.
17. The method of claim 1 , wherein the top ply is free of added organic compounds.
18. The method of claim 1 , wherein the top ply does not include a cationic polymer, an anionic polymer, or a polysaccharide hydrocolloid.
19. The method of claim 1 , wherein the top ply is an outer ply.
20. The method of claim 1 , wherein the top ply is free of wax, polyolefins, and silicones.
21. The method of claim 1 , wherein the top ply consists essentially of inorganic particulate material and microfibrillated cellulose.
22. 2. The method of claim 1, wherein the top ply has a whiteness (measured by ISO standard 11475 (F8; D65-400 nm)) of at least 65%.
Citation Information
Patent Citations
Paper filler composition
JP2012514137A
Composition
JP2014503696A
Cellulose-derived composition
JP2016505727A
Coated paper
WO2010113805A1
Transparent moisture barrier coatings for containers