Cerium-based composite oxide powder, friction material composition, and friction material

The cerium-based composite oxide powder addresses fade resistance and friction stability issues in NAO brake pads by enhancing μ value consistency and stability, resulting in improved braking comfort.

JP7568857B2Active Publication Date: 2024-10-16DAIICHI KIGENSO KAGAKU KOGYO CO LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2023529854
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-06-14
Filing Date
2022-06-13
Publication Date
2024-10-16
Estimated Expiration
2042-06-13

AI Technical Summary

Technical Problem

Brake pads without asbestos (NAO brake pads) face issues with fade resistance, high μ value, and friction stability, leading to uncomfortable braking sensations due to variations in μ values during sudden and light braking.

Method used

A cerium-based composite oxide powder containing cerium, aluminum, and optionally zirconium, with specific surface area, crystallite diameter, and content ratios, is used as a friction material to enhance fade resistance, high μ value, and friction stability.

Benefits of technology

The cerium-based composite oxide powder provides brake pads with excellent fade resistance, high μ value, and improved friction stability, reducing discomfort during braking by minimizing μ value variations.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007568857000005
    Figure 0007568857000005
  • Figure 0007568857000001
    Figure 0007568857000001
  • Figure 0007568857000002
    Figure 0007568857000002
Patent Text Reader

Abstract

This complex oxide powder contains cerium and aluminum, and has a specific surface area of 0.5-10 m2 / g.<sp / >
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a cerium-based composite oxide powder, a friction material composition, and a friction material. [Background technology]

[0002] Brake pads are often used for braking in automobiles. Traditionally, brake pads were mainly made by adding asbestos to obtain the desired performance. However, in recent years, asbestos-free brake pads have been in demand due to environmental load issues, and research and development into them is being actively carried out.

[0003] Conventionally, zircon ore powder or zirconium oxide powder obtained by removing impurities such as silicon from raw ore has been used as friction materials for brake pads. However, problems have arisen in recent years, such as the soaring price of raw materials and the inclusion of radioactive elements derived from the ore.

[0004] Patent Document 1 discloses a friction material in which a fiber base material and a friction modifier are bonded with a thermosetting resin, and the friction modifier contains a rare earth oxide as at least a part of the friction modifier. Patent Document 1 also discloses that rare earth oxides such as CeO2, La2O3, and Y2O3 have a lower hardness and are less likely to deteriorate than general abrasive materials such as alumina, and therefore can reduce aggressiveness to mating materials while obtaining a high and stable friction coefficient.

[0005] Patent Document 2 discloses a friction material composition containing a binder, an organic filler, an inorganic filler, and a fiber base material, which does not contain copper as an element in the friction material composition, and the inorganic filler is one or more selected from gamma alumina having an average particle size of 10 nm to 50 μm, dolomite having an average particle size of 1 to 20 μm, calcium carbonate having an average particle size of 1 to 20 μm, magnesium carbonate having an average particle size of 1 to 20 μm, manganese dioxide having an average particle size of 1 to 20 μm, zinc oxide having an average particle size of 10 nm to 1 μm, iron oxide having an average particle size of 1.0 μm or less, cerium oxide having an average particle size of 0.5 to 5 μm, and zirconia having an average particle size of 5 to 50 nm. Patent Document 2 also discloses that, as an effect, when used in friction materials such as automobile disc brake pads, the composition has excellent fade resistance and wear resistance at high temperatures exceeding 500 ° C., even without using copper, which has a high environmental load.

[0006] Patent Document 3 discloses a friction material composition containing a binder, an organic filler, an inorganic filler, and a fibrous base material, which does not contain copper as an element in the friction material composition and contains potassium titanate having a plurality of convex shapes and zirconium silicate having an average particle size of 1 to 2.5 μm. Patent Document 3 also discloses that, as an effect, the composition has excellent wear resistance at high temperatures and produces little abnormal noise, even without using copper, which has a high environmental impact. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] Japanese Patent Application Publication No. 9-13009 [Patent Document 2] International Publication No. 2016 / 060129 [Patent Document 3] JP 2016-79246 A Summary of the Invention [Problem to be solved by the invention]

[0008] In recent years, research and development has been conducted on brake pads that do not use asbestos (non-asbestos organic brake pads (NAO brake pads)). A weakness of NAO brake pads is the decrease in braking force due to continuous use (fade phenomenon). If the decrease in μ value due to fade is large, it will lead to an uncomfortable feeling when braking. Also, in recent years, there has been a trend toward brake pads with high μ values, but a problem occurs in that a high μ value tends to increase the difference between the μ value during hard braking and the μ value during light braking. If the difference between the μ value during hard braking and the μ value during light braking becomes large, it will lead to an uncomfortable feeling when braking. Hereinafter, in this specification, a small difference between the μ value during hard braking and the μ value during light braking is referred to as excellent friction stability.

[0009] The present invention has been made in view of the above problems, and an object of the present invention is to provide a cerium-based composite oxide powder which, when used as a friction material for brake pads, makes it possible to obtain a friction material which is excellent in fade resistance and has a high μ value while being excellent in friction stability. Another object of the present invention is to provide a friction material composition containing the cerium-based composite oxide powder. Another object of the present invention is to provide a friction material composed of a molded body of the friction material composition. [Means for solving the problem]

[0010] The present inventors have conducted extensive research into powders to be used as friction materials for brake pads, and have surprisingly found that a friction material having excellent fade resistance, high μ value, and excellent friction stability can be obtained by mixing ceria powder with alumina powder, melting, and pulverizing the powder, and have completed the present invention.

[0011] That is, the cerium-based composite oxide powder according to the present invention has the following properties: Contains cerium and aluminum, Specific surface area is 0.5m 2 / g or more 10m 2 / g or less.

[0012] According to the research of the present inventors, cerium oxide (ceria) powder that does not contain aluminum has excellent fade resistance, but it is not possible to obtain a high μ value and also has poor friction stability. In contrast, in the present invention, cerium oxide (ceria) powder that contains aluminum in addition to cerium and has a specific surface area of ​​10 m 2 The cerium-based composite oxide powder has a surface roughness of 0.01 μm or less and a surface roughness of 0.01 μm or less. Therefore, when the cerium-based composite oxide powder is used as a friction material for a brake pad, it is possible to obtain a friction material having excellent fade resistance and high μ value while also having excellent friction stability. This is also clear from the examples. By using a cerium-based composite oxide powder containing aluminum in addition to cerium, it is possible to obtain a friction material that has excellent fade resistance and a high μ value while also having excellent friction stability. Although the details are not clear, the inventors of the present invention speculate as follows. Cerium's main role is to contribute to fade resistance. Cerium is known to have a high oxygen storage capacity. During high-load braking, the brake pad surface can reach 400°C or higher due to frictional heat. This can cause the resin that solidifies the brake pad to burn, generating strong reducing gas. It is believed that this gas can reduce the metal oxide added as an abrasive, reducing the coefficient of friction. Cerium has the property of releasing oxygen when the atmosphere is reducing at around 400°C. Therefore, it is expected that the metal oxide will not be reduced and the coefficient of friction will not be reduced. Also, the main role of cerium aluminate is to contribute to high μ value and friction stability. Alumina alone is too hard and highly aggressive to the rotor disk, making it impractical. Also, cerium alone does not provide the necessary friction coefficient. On the other hand, cerium aluminate has fewer disadvantages than alumina alone or cerium alone, and it is possible to obtain a friction material that has excellent fade resistance, a high μ value, and excellent friction stability.

[0013] In the above-mentioned composition, it is preferable that zirconium is contained.

[0014] When a cerium-based composite oxide powder containing zirconium and aluminum in addition to cerium is used, it becomes easy to obtain a friction material that has excellent fade resistance and a high μ value while also having excellent friction stability. When a cerium-based composite oxide powder containing zirconium and aluminum in addition to cerium is used, it becomes easy to obtain a friction material that has excellent fade resistance and a high μ value while also having excellent friction stability. Although the details are not clear, the inventors of the present invention presume that such characteristics are obtained because the cerium-based composite oxide powder has two crystal phases, a crystal phase in which zirconia and ceria are solid-dissolved, and a crystal phase containing cerium and aluminum. In addition, when the specific surface area is 10 m 2 / g or less, it is presumed that this allows for a high hardness and a high μ value.

[0015] Patent Documents 1 to 3 do not disclose a cerium-based composite oxide powder containing the three elements cerium, zirconium, and aluminum. Patent Documents 1 to 3 also do not disclose the problem or effect of combining the three properties of excellent fade resistance, high μ value, and excellent friction stability.

[0016] In the above-mentioned configuration, the crystallite size is preferably within the range of 10 nm or more and 80 nm or less.

[0017] When the crystallite size is 10 nm or more, sufficient crystal growth is achieved, and properties such as a high μ value can be easily obtained.

[0018] In the above configuration, the particle diameter D 50 It is preferable that the thickness is 0.5 μm or more and 20 μm or less.

[0019] Particle size D 50 When the thickness is 0.5 μm or more and 20 μm or less, characteristics such as a high μ value can be more easily obtained.

[0020] In the above configuration, the particle diameter D99 It is preferable that the thickness is 60 μm or less.

[0021] Particle size D 99 When the thickness is 60 μm or less, properties such as a high μ value can be more easily obtained.

[0022] In the above-mentioned composition, the single grain crushing strength is preferably within the range of 50N or more and 300N or less.

[0023] When the single grain crushing strength is 50N or more, the strength of the particles is high, and properties such as a high μ value can be particularly easily obtained.

[0024] In the above-mentioned configuration, the content of cerium is 40% by mass or more and 95% by mass or less in terms of oxide, The zirconium content is within the range of 0.1 mass% to 50 mass% in terms of oxide, The aluminum content is preferably within the range of 0.1% by mass to 24% by mass in terms of oxide.

[0025] When the cerium content is within the range of 40% by mass or more and 95% by mass or less in terms of oxide, the zirconium content is within the range of 0.1% by mass or more and 50% by mass or less in terms of oxide, and the aluminum content is within the range of 0.1% by mass or more and 24% by mass or less in terms of oxide, these are suitable ratios for obtaining characteristics such as a high μ value. As described above, the inventors presume that the cerium-based composite oxide powder has two crystal phases, namely, a crystal phase in which zirconia and ceria are solid-dissolved, and a crystal phase containing cerium and aluminum, and therefore properties such as a high μ value can be easily obtained. Here, when the cerium content is 40% by mass or more and 95% by mass or less, calculated as the oxide, the zirconium content is within the range of 0.1% by mass or more and 50% by mass or less, calculated as the oxide, and the aluminum content is within the range of 0.1% by mass or more and 24% by mass or less, calculated as the oxide, it is presumed that the two phases, a crystalline phase in which zirconia and ceria are dissolved, and a crystalline phase containing cerium and aluminum, will be in a suitable ratio for obtaining characteristics such as a high μ value.

[0026] In the above-mentioned structure, the aluminum content is preferably within the range of 0.1% by mass to 10% by mass in terms of oxide.

[0027] In the above-mentioned configuration, the zirconium content is within a range of 0.1 mass% or more and 40 mass% or less in terms of oxide, The aluminum content is preferably within the range of 0.1% by mass to 10% by mass in terms of oxide.

[0028] In the above-mentioned configuration, the content of cerium is 49% by mass or more and 91% by mass or less in terms of oxide, The zirconium content is within the range of 1% by mass or more and 43% by mass or less in terms of oxide, The aluminum content is preferably within the range of 1% by mass to 8% by mass in terms of oxide.

[0029] When the cerium content is within the range of 49% by mass or more and 91% by mass or less in terms of oxide, the zirconium content is within the range of 1% by mass or more and 43% by mass or less in terms of oxide, and the aluminum content is within the range of 1% by mass or more and 8% by mass or less in terms of oxide, these are more suitable ratios for obtaining characteristics such as a high μ value.

[0030] In the above-mentioned composition, the total content of cerium, zirconium and aluminum is preferably 60 mass % or more calculated as oxide.

[0031] In the above composition, it is preferable that CeAlO3 is contained.

[0032] When CeAlO3 is contained, the material has excellent properties such as a high μ value.

[0033] In the above composition, it is preferable to contain a rare earth element other than cerium.

[0034] When a rare earth element other than cerium is contained, the crystal phase becomes stable and a higher μ value can be achieved.

[0035] In the above-mentioned composition, it is preferable that rare earth elements other than cerium are contained in an amount of 0.1% by mass to 40% by mass in terms of oxide.

[0036] When a rare earth element other than cerium is contained in the range of 0.1 mass % to 40 mass % in terms of oxide, the crystal phase becomes more stable and a higher μ value can be achieved.

[0037] In the above-mentioned structure, the rare earth element other than cerium is preferably one or more elements selected from the group consisting of yttrium and lanthanum.

[0038] When the rare earth element other than cerium is at least one selected from the group consisting of yttrium and lanthanum, the crystal phase is stable and a high μ value can be achieved.

[0039] The above-mentioned composition may contain an alkaline earth element.

[0040] The inclusion of an alkaline earth element makes the material less stable than rare earth elements such as yttria, but it can be produced more inexpensively.

[0041] In the above-mentioned configuration, it is preferable that the composition is for use as a friction material.

[0042] When the cerium-based composite oxide powder is used as a friction material for brake pads, it is possible to obtain a friction material that has excellent fade resistance and excellent friction stability while having a high μ value, and therefore it can be suitably used as a friction material.

[0043] The friction material composition according to the present invention includes a friction modifier, a fibrous base material, and a binder, The friction modifier contains the cerium-based composite oxide powder.

[0044] According to the above-mentioned configuration, since the cerium-based composite oxide powder is contained as a friction modifier, when the friction material composition is molded and used as a friction material for a brake pad, it is possible to obtain a friction material that has excellent fade resistance and excellent friction stability while having a high μ value.

[0045] In the above-mentioned composition, the content of the cerium-based composite oxide powder is preferably within a range of 5% by mass to 20% by mass, when the entire friction material composition is taken as 100% by mass.

[0046] When the content of the cerium-based composite oxide powder is within the range of 5 mass % or more and 20 mass % or less when the entire friction material composition is taken as 100 mass %, characteristics such as a high μ value can be more easily obtained.

[0047] The friction material according to the present invention is characterized in that it is composed of a molded product of the friction material composition.

[0048] According to the above-mentioned configuration, since the friction material is constituted by a molded article of the friction material composition, it is possible to obtain a friction material that has excellent fade resistance and excellent friction stability while having a high μ value.

[0049] In the above-mentioned configuration, the first fade test is performed nine times under the following measurement condition A in accordance with the Society of Automotive Engineers of Japan standard JASO C406, and the average value of the maximum and minimum μ values ​​when the minimum friction coefficient is shown at the obtained behavior peak is calculated, and it is preferable that the average value is 0.20 μ or more. <Measurement condition A> Initial braking speed 100km / h Braking interval 35 seconds Brake temperature before braking during the first measurement: 80℃ Braking deceleration 0.45G Braking times: 9

[0050] If the above numerical value is 0.20μ or more, the discomfort during braking can be further reduced.

[0051] In the above-mentioned configuration, it is preferable that the friction coefficient μ value, which is the average value of the friction coefficient measured under the following measurement condition B in accordance with the Society of Automotive Engineers of Japan standard JASO C406, is 0.39 or more. <Measurement condition B> Initial braking speed 65km / h Brake temperature before braking: 120℃ Braking deceleration 0.35G Measurements taken 200 times

[0052] When the friction coefficient μ value is 0.39 or more, a stronger braking force can be obtained with a smaller pressing force.

[0053] In the above configuration, the friction coefficient X is defined as the average value of the friction coefficient measured eight times in the second friction test measured under the following measurement conditions C in accordance with the Society of Automotive Engineers of Japan standard JASO C406, In accordance with the JASO C406 standard, the friction coefficient Y is the average value of the friction coefficient measured 8 times in the second effectiveness test under the following measurement conditions D. The difference in the friction coefficients [(friction coefficient X)-(friction coefficient Y)] is preferably 0.12 or less. <Measurement conditions C> Initial braking speed 100km / h Brake temperature before braking: 80℃ Braking deceleration 0.2G Measurements taken 8 times <Measurement condition D> Initial braking speed 100km / h Brake temperature before braking: 80℃ Braking deceleration 0.7G Measurements taken 8 times

[0054] When the difference in the friction coefficients [(friction coefficient X)-(friction coefficient Y)] is 0.12 or less, the discomfort felt during braking can be further reduced. Effect of the Invention

[0055] According to the present invention, it is possible to provide a cerium-based composite oxide powder that, when used as a friction material for brake pads, enables the production of a friction material that has excellent fade resistance and high μ value while also having excellent friction stability. It is also possible to provide a friction material composition that contains the cerium-based composite oxide powder. It is also possible to provide a friction material that is composed of a molded body of the friction material composition. [Brief description of the drawings]

[0056] [Figure 1] 1 is an X-ray diffraction spectrum of the cerium-based composite oxide powder according to Example 4. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0057] Hereinafter, the embodiments of the present invention will be described. However, the present invention is not limited to these embodiments. In this specification, zirconia (zirconium oxide) is a general one, and contains 10 mass % or less of impurity metal compounds (unavoidable impurities) including hafnia.

[0058] [Cerium-based composite oxide powder] The cerium-based composite oxide powder according to this embodiment is Contains cerium and aluminum, Specific surface area is 0.5m 2 / g or more 10m 2 / g or less.

[0059] The cerium-based composite oxide powder according to this embodiment (hereinafter also referred to as "composite oxide powder") contains aluminum in addition to cerium and has a specific surface area of ​​10 m 2 The composite oxide powder has a surface roughness of 0.1 to 1.0 μm / g or less, and therefore, when the composite oxide powder is used as a friction material for a brake pad, it is possible to obtain a friction material having excellent fade resistance and high μ value, while also having excellent friction stability. This is also clear from the examples.

[0060] (Composition of composite oxide powder) The composite oxide powder according to the present embodiment contains cerium (Ce) and aluminum (Al) as a whole, and is formed as a composite of multiple oxides. The composite oxide powder according to the present embodiment preferably further contains zirconium (Zr). The composite of multiple oxides refers to a combination of two or more oxides with different composition ratios. The composite oxide powder according to the present embodiment is not a mixture of ceria (cerium oxide) and alumina (aluminum oxide). When zirconium is further contained, the composite oxide powder according to the present embodiment is not a mixture of ceria (cerium oxide), zirconia (zirconium dioxide) and alumina (aluminum oxide).

[0061] The content of cerium in the composite oxide powder is preferably 40 mass% or more, more preferably 49 mass% or more, even more preferably 53 mass% or more, particularly preferably 56 mass% or more, and especially preferably 60 mass% or more, calculated as oxide. The content of cerium in the composite oxide powder is preferably 95 mass% or less, calculated as oxide, more preferably 92 mass% or less, even more preferably 91 mass% or less, particularly preferably 90 mass% or less, and especially preferably 88 mass% or less. When the temperature of the friction material surface reaches 400 to 800°C due to frictional heat, the resin component contained in the friction material evaporates. At that time, the evaporated gas creates a strong reducing atmosphere. Since the composite oxide powder according to the present embodiment contains cerium oxide, the reduction of the friction material can be suppressed by supplying oxygen due to a change in the valence of cerium oxide. In particular, when a large amount of cerium oxide is contained (when cerium is contained in an amount of 40 mass% or more in terms of oxide), the reduction of the friction material can be further suppressed. Normally, since friction materials are oxides, oxygen is taken away in a strong reducing atmosphere, and there is a possibility that the hardness will decrease. However, in the present embodiment, since cerium oxide is contained, the reduction of the friction material due to reduction is suppressed.

[0062] The zirconium content in the composite oxide powder is preferably 0.1 mass% or more, more preferably 1 mass% or more, even more preferably 3 mass% or more, particularly preferably 4 mass% or more, and especially preferably 5 mass% or more, calculated as the oxide. The zirconium content in the composite oxide powder is preferably 50 mass % or less, more preferably 45 mass % or less, further preferably 43 mass % or less, particularly preferably 35 mass % or less, and particularly preferably 30 mass % or less, calculated as the oxide.

[0063] The content of aluminum in the composite oxide powder is preferably 0.1% by mass or more, more preferably 1% by mass or more, further preferably 2% by mass or more, and particularly preferably 3% by mass or more, calculated as oxide. The aluminum content in the composite oxide powder is preferably 24 mass% or less, more preferably 10 mass% or less, more preferably 8 mass% or less, even more preferably 7 mass% or less, particularly preferably 6 mass% or less, and especially preferably 5 mass% or less, calculated as the oxide.

[0064] The contents of cerium, zirconium and aluminum contained in the composite oxide powder are preferably such that the cerium content is in the range of 40% by mass or more and 95% by mass or less, calculated as oxide, the zirconium content is in the range of 0.1% by mass or more and 50% by mass or less, calculated as oxide, and the aluminum content is in the range of 0.1% by mass or more and 24% by mass or less, calculated as oxide. It is more preferable that the cerium content is in the range of 49% by mass or more and 91% by mass or less in terms of oxide, the zirconium content is in the range of 1% by mass or more and 43% by mass or less in terms of oxide, and the aluminum content is in the range of 1% by mass or more and 8% by mass or less in terms of oxide.

[0065] When the contents of cerium, zirconium, and aluminum are within the above-mentioned ranges, the ratios are suitable for obtaining properties such as a high μ value.

[0066] The total content of cerium, zirconium and aluminum is preferably 60% by mass or more in terms of oxide. The total content is more preferably 72% by mass or more in terms of oxide, further preferably 75% by mass or more, particularly preferably 80% by mass or more, particularly preferably 85% by mass or more, and especially preferably 87% by mass. The higher the total content, the more preferable it is, for example, 100% by mass or less, 97% by mass or less, 95% by mass or less, 90% by mass or less, etc. in terms of oxide.

[0067] The composite oxide powder may contain a rare earth element other than cerium, which stabilizes the crystal phase and allows the powder to have a higher μ value.

[0068] Examples of rare earth elements other than cerium include scandium, yttrium, lanthanum, praseodymium, neodymium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium, and lutetium. The rare earth elements other than cerium contained in the composite oxide powder may be one type or two or more types. Among them, the rare earth elements other than cerium are preferably one or more selected from the group consisting of yttrium and lanthanum, and particularly yttrium. When yttrium or lanthanum is contained, especially when yttrium is contained, the crystal phase is more stable and the μ value can be further increased.

[0069] The content of the rare earth elements other than cerium is preferably 0.1% by mass or more, and more preferably 1% by mass or more, calculated as oxide, when the entire composite oxide powder is taken as 100% by mass. The content of rare earth elements other than cerium is preferably 40 mass% or less, calculated as oxide, when the entire composite oxide powder is taken as 100 mass%, more preferably 15 mass% or less, even more preferably 10 mass% or less, particularly preferably 5 mass% or less, especially preferably 4 mass% or less, and especially preferably 3 mass% or less. When a rare earth element other than cerium is contained in the range of 0.1 mass % or more and 26 mass % or less in terms of oxide, the crystal phase becomes more stable and a higher μ value can be achieved.

[0070] The composite oxide powder may contain other elements within a range that does not impair the effects of the present invention. Examples of the other elements include alkali elements, alkaline earth elements, and transition metal elements. Specific examples of the other elements include calcium, magnesium, silicon, and titanium. These elements are preferably contained in the composite oxide powder as oxides. The content of the other elements is preferably 40% by mass or less, calculated as oxide, when the entire composite oxide powder is taken as 100% by mass.

[0071] (specific surface area) The specific surface area of ​​the composite oxide powder is 0.5 m 2 / g or more 10m 2 / g or less. The specific surface area is 1 m 2 / g or more, and 1.5m 2 / g or more is more preferable, and 1.8m 2 / g or more is more preferable, 2 It is particularly preferable that the molecular weight is at least 1 / g. The specific surface area is 4.5 m 2 / g or less, and 2 / g or less is more preferable, and 3.5m 2 More preferably, it is 3.2m / g or less. 2 / g or less is particularly preferable, 2 It is especially preferred that the ionic liquid is equal to or less than 1 / g. The specific surface area is 0.5 m 2 / g or more 10m 2 When the content of the composite oxide powder is less than or equal to 1 / g, the composite oxide powder can be easily formed into a melt-solidified product having the desired crystallinity and strength. Note that, due to the characteristics of the manufacturing method, the melt-solidified product may also include a semi-molten solidified product. As a method for obtaining a composite oxide powder having the above-mentioned specific surface area, there may be mentioned a method in which ceria powder is mixed with zirconia powder and alumina powder, followed by melting and pulverizing. The specific surface area of ​​the composite oxide powder refers to a value obtained by the method described in the Examples.

[0072] (Crystallite size) The crystallite diameter of the composite oxide powder is preferably in the range of 10 nm to 80 nm. The crystallite diameter is more preferably 20 nm or more, even more preferably 30 nm or more, and particularly preferably 35 nm or more. The crystallite diameter is more preferably 70 nm or less, even more preferably 65 nm or less, and particularly preferably 60 nm or less. When the crystallite diameter is 10 nm or more, sufficient crystal growth is achieved, and characteristics such as a high μ value can be easily obtained. On the other hand, it is not necessary to promote crystal growth excessively. There is no particular upper limit to the crystallite diameter, but considering productivity, it is preferable that the crystallite diameter is 80 nm or less. The crystallite size is calculated by applying the measurement results of the peak at 2θ of 40° to 42° in XRD measurement to the following Scherrer formula. Dp = (K × λ) / βcosθ Here, Dp is the crystallite diameter of the composite oxide powder, λ is the wavelength of the X-ray, θ is the diffraction angle, K is a constant called the shape factor, and β is the peak width after correction for the broadening of the diffraction line due to the instrument. The peak with 2θ of 40° to 42° is a peak derived from (111) of CeAlO3. Detailed conditions for the XRD measurement are as described in the Examples. As a method for obtaining a composite oxide powder having the above crystallite size, there may be mentioned a method in which ceria powder is mixed with zirconia powder and alumina powder, followed by melting and pulverizing.

[0073] (crystalline phase) As described above, the composite oxide powder contains cerium and aluminum as a whole, and is formed as a composite of a plurality of oxides. When the composite oxide powder further contains zirconium, the composite oxide powder contains cerium, zirconium, and aluminum as a whole, and is formed as a composite of a plurality of oxides. Each oxide constituting the composite only needs to contain at least one of cerium, zirconium, and aluminum, and does not need to contain all three. The composite may further contain an oxide other than cerium, zirconium, and aluminum as a part of the composite. The composite may also contain a compound (element) other than an oxide as a part of the composite.

[0074] The composite oxide powder is preferably a composite containing an oxide containing cerium and zirconia (hereinafter also referred to as crystalline phase A) and an oxide containing cerium and aluminum (hereinafter also referred to as crystalline phase B). The crystalline phase A is a solid solution of zirconia in ceria and does not have a specific composition formula. When the composite oxide powder has the crystalline phase A, it has oxygen storage and release capacity, and the decrease in hardness is suppressed. In addition, it has excellent properties such as a high μ value. The formula of the crystal phase B is CeAlO3. When the composite oxide powder has two phases, ie, crystalline phase A and crystalline phase B, it is possible to obtain a friction material that has excellent fade resistance, a high μ value, and excellent friction stability.

[0075] When the composite oxide powder contains a rare earth element other than cerium, an oxide corresponding to the amount of the rare earth element other than cerium added is contained as a part of the composite. In particular, when the composite oxide powder contains yttrium and lanthanum as rare earth elements other than cerium, they are solid-dissolved in ceria and zirconia.

[0076] (Particle diameter D 50 ) The particle diameter D of the composite oxide powder 50 The particle diameter D is preferably 20 μm or less. 50is more preferably 0.8 μm or more, further preferably 1 μm or more, particularly preferably 1.5 μm or more, particularly preferably 2 μm or more, and especially preferably 2.3 μm or more. 50 is more preferably 15 μm or less, further preferably 10 μm or less, particularly preferably 7 μm or less, particularly preferably 5 μm or less, and especially preferably 4 μm or less. The particle diameter D 50 When the thickness is 20 μm or less, properties such as a high μ value can be more easily obtained.

[0077] (Particle diameter D 90 ) The particle diameter D of the composite oxide powder 90 The particle diameter D is preferably 25 μm or less. 90 is more preferably 3 μm or more, further preferably 5 μm or more, and particularly preferably 6.5 μm or more. 90 is more preferably 21 μm or less, further preferably 15 μm or less, particularly preferably 10 μm or less, and particularly preferably 8 μm or less. The particle diameter D 90 When the thickness is 25 μm or less, properties such as a high μ value can be more easily obtained.

[0078] (Particle diameter D 99 ) The particle diameter D of the composite oxide powder 99 The particle diameter D is preferably 60 μm or less. 99 is more preferably 50 μm or less, further preferably 48 μm or less, particularly preferably 20 μm or less, and particularly preferably 15 μm or less. 99 is preferably 5 μm or more, more preferably 7 μm or more, further preferably 10 μm or more, and particularly preferably 11 μm or more. The particle diameter D 99 When the thickness is 60 μm or less, properties such as a high μ value can be more easily obtained.

[0079] The particle diameter D of the composite oxide powder 50、 Particle size D90 , particle diameter D 99 The particle diameter D 50 , the particle diameter D 90 , the particle diameter D 99 is measured on a volume basis, and the particle diameter D 50 is the particle size at 50% cumulatively from the minimum particle size measured by a laser diffraction method, and the particle size D 90 is the particle size at 90% cumulative from the minimum particle size measured by a laser diffraction method, and the particle size D 99 is the particle size that is 99% cumulative from the minimum particle size value, measured by laser diffraction method. The particle diameter D 50 , the particle diameter D 90 , the particle diameter D 99 As a method for obtaining a composite oxide powder having the above formula, there can be mentioned a method in which ceria powder is mixed with zirconia powder and alumina powder, melted, and pulverized to obtain a composite oxide powder by controlling the pulverization conditions.

[0080] (Single grain crushing strength) The single grain crushing strength of the composite oxide powder is preferably within the range of 50 N or more and 300 N or less. The single grain crushing strength is more preferably 70 N or more, further preferably 80 N or more, particularly preferably 90 N or more, particularly preferably 100 N or more, and especially preferably 110 N or more. There is no particular upper limit to the single grain crushing strength, but the single grain crushing strength can be 250 N or less, 230 N or less, 210 N or less, 190 N or less, 180 N or less, etc. The single grain crushing strength is measured on particles before crushing. The particles before crushing have a particle diameter in the range of 2.36 mm to 2.80 mm. Particles with the above particle diameter can be obtained using a commercially available sieve. The number of particles measured is 50, and the average value is taken as the single grain crushing strength. A tensile compression tester is used as the measuring device. Specifically, the SV-201-NSL manufactured by Imada Seisakusho Co., Ltd. is used as the tensile compression tester. The load speed is 0.50 mm / min. The details of the method for measuring the single grain crushing strength are as described in the Examples. As a method for obtaining a composite oxide powder having the above-mentioned single grain crushing strength, there can be mentioned a method in which ceria powder is mixed with zirconia powder and alumina powder, followed by melting and pulverizing.

[0081] (Density (true specific gravity)) The true specific gravity of the composite oxide powder is 6.0 g / cm 3 More than 7.2g / cm 3 The true specific gravity is preferably 6.3 g / cm or less. 3 More preferably, 6.5 g / cm 3 More preferably, 6.7 g / cm 3 The true specific gravity is preferably 7.1 g / cm 3 Less than or equal to 7.0 g / cm 3 More preferably, 6.9 g / cm 3 The following is the result. The true specific gravity is 6.0g / cm 3 More than 7.2g / cm 3 If it is equal to or less than this, characteristics such as a high μ value can be more easily obtained. The true specific gravity refers to a value measured in accordance with JIS Z8807:2012. As a method for obtaining a composite oxide powder having the above-mentioned true specific gravity, there may be mentioned a method in which ceria powder is mixed with zirconia powder and alumina powder, followed by melting and pulverizing.

[0082] The composite oxide powder according to this embodiment has been described above.

[0083] [Method of manufacturing composite oxide powder] An example of the method for producing the composite oxide powder will be described below, however, the method for producing the composite oxide powder according to the present invention is not limited to the following example.

[0084] The method for producing the composite oxide powder according to this embodiment is as follows: Step 1 of preparing a starting material; a step 2 of melting the starting materials by applying a predetermined amount of heat to the starting materials; A step 3 of cooling the melt obtained in the step 2 to form an ingot; A step 4 of pulverizing the ingot obtained in the step 3 into a powder; The method includes a step 5 of heating the powder obtained in the step 4 under an atmosphere at 400 to 1100°C.

[0085] <Process 1> In the method for producing a composite oxide powder according to the present embodiment, starting materials are first prepared. Specifically, for example, a cerium raw material and an aluminum raw material are prepared. Furthermore, if necessary, a zirconium raw material is also prepared.

[0086] The cerium raw material is a material for mainly introducing cerium element into the composite oxide powder. "Mainly introducing cerium element into the composite oxide powder" means introducing a larger amount (more than equimolar amount) of cerium element compared to other elements (zirconium, aluminum, and rare earth elements other than cerium). In other words, the cerium raw material may contain rare earth elements other than zirconium, aluminum, and cerium as long as the amount (number of moles) is smaller than that of cerium element. The cerium raw material is not particularly limited, but preferably contains cerium oxide. Cerium oxide can be synthesized from various raw materials such as nitrate, carbonate, sulfate, acetate, chloride, bromide, etc. The cerium raw material may be a composite oxide of cerium and aluminum. The cerium raw material may be a composite oxide of cerium, zirconium, and aluminum. The cerium raw material may contain a compound such as cerium nitrate, carbonate, sulfate, chloride, bromide, etc. The cerium raw material may contain a compound such as zirconium nitrate, carbonate, sulfate, chloride, bromide, etc.

[0087] The zirconium raw material is a material for mainly introducing zirconium element into the composite oxide powder. "Mainly introducing zirconium element into the composite oxide powder" means introducing a larger amount (more than equimolar amount) of zirconium element compared to other elements (cerium, aluminum, rare earth elements other than cerium). In other words, the zirconium raw material may contain rare earth elements other than zirconium, aluminum, and cerium as long as the amount (number of moles) is smaller than that of zirconium element. The zirconium raw material is not particularly limited, and may be, for example, various zirconium-based materials such as baddeleyite, desiliconized zirconia, zirconium oxide, or other zirconium materials containing zirconium oxide. Zirconium oxide can be synthesized from various raw materials such as nitrates, carbonates, sulfates, acetates, chlorides, bromides, or the like. The zirconium raw material may contain a composite oxide of zirconium and at least one of cerium and rare earth elements other than cerium. The zirconium raw material may contain a compound such as cerium nitrates, carbonates, sulfates, chlorides, bromides, or the like. The zirconium raw material may contain a compound such as zirconium nitrates, carbonates, sulfates, chlorides, bromides, or the like. It is desirable to use a raw material that does not contain radioactive elements as the zirconium raw material.

[0088] The aluminum raw material is a material for mainly introducing aluminum element into the composite oxide powder. "Mainly introducing aluminum element into the composite oxide powder" means introducing a larger amount (more than equimolar amount) of aluminum element compared to other elements (cerium, zirconium, rare earth elements other than cerium). In other words, the aluminum raw material may contain rare earth elements other than cerium, zirconium, and cerium as long as the amount (number of moles) is smaller than that of aluminum element. The aluminum raw material is not particularly limited, but preferably contains aluminum oxide. Aluminum oxide can be synthesized from various raw materials such as nitrate, carbonate, sulfate, acetate, chloride, bromide, etc. The aluminum raw material may be a composite oxide of zirconium and at least one element selected from the group consisting of cerium and rare earth elements other than cerium. The aluminum raw material may contain a compound such as cerium nitrate, carbonate, sulfate, chloride, bromide, etc. The aluminum raw material may contain a compound such as zirconium nitrate, carbonate, sulfate, chloride, bromide, etc.

[0089] In step 1, a raw material containing a rare earth element other than cerium (hereinafter also referred to as a "third element raw material") may be prepared as the raw material.

[0090] The third element raw material is a material for mainly introducing a rare earth element other than cerium (hereinafter also referred to as the "third element") into the composite oxide powder. "Mainly introducing the third element into the composite oxide powder" means introducing a larger amount (more than equimolar amount) of cerium compared to other elements (cerium, zirconium, aluminum). In other words, the third element raw material may contain cerium, zirconium, or aluminum as long as the amount is smaller (fewer moles) than the third element. The third element is preferably yttria. Yttria (yttrium oxide) can be synthesized from various raw materials such as nitrates, carbonates, sulfates, acetates, chlorides, and bromides.

[0091] In this specification, "step 1 of preparing raw materials" means that in this step 1, a material for introducing cerium element and a material for introducing aluminum element are finally prepared as a whole, and it is not necessary to prepare a cerium raw material and an aluminum raw material separately.

[0092] The purity of the cerium raw material, the zirconium raw material, the aluminum raw material, and the third element raw material is not particularly limited, but is preferably 99.9% or more in terms of increasing the purity of the target product. As described above, each of the cerium raw material, the zirconium raw material, the aluminum raw material, and the third element raw material may contain other substances to the extent that the properties of the composite oxide powder are not impaired. As described above, examples of the other substances include nitrates, carbonates, sulfates, chlorides, bromides, etc. of cerium and zirconium. In addition, other substances may include alkali elements, alkaline earth elements, transition metal elements, etc. Among them, alkaline earth elements are preferable. When the composite oxide powder contains an alkaline earth element, the stability is slightly inferior to that of rare earth elements such as yttria, but it can be produced at a low cost. As the alkaline earth element, Ca, Mg, Sr, and Ba are preferable, Ca, Mg, and Sr are more preferable, Ca and Mg are further preferable, and Ca is particularly preferable. Ca is not only an inexpensive raw material, but also relatively easily dissolves in zirconia, making production easy.

[0093] After preparing the raw materials, the raw materials are blended together so that the contents of cerium and aluminum are within the prescribed ranges. In the case of including zirconium, after preparing the raw materials, the raw materials are blended together so that the contents of cerium, zirconium, and aluminum are within the prescribed ranges.

[0094] <Process 2> Next, a predetermined amount of heat is applied to the starting materials to melt the starting materials. In step 2, it is preferable to melt all the raw materials. When all the raw materials are melted, the crystal structure of the resulting composite oxide powder is stable, and properties such as high μ can be obtained. To melt all the raw materials, heat is applied to the starting materials so that the temperature becomes equal to or higher than the highest melting point of the various raw materials contained in the starting materials.

[0095] The method for melting the starting materials is not particularly limited, and examples thereof include melting methods such as arc type, high-frequency thermal plasma type, etc. Among them, it is preferable to adopt a general electric melting method, that is, a melting method using an arc type electric furnace (melting device).

[0096] The starting materials can be heated by applying heat at a power consumption rate of, for example, 0.5 to 2.5 kWh / kg. This heating can raise the temperature of the starting materials to a temperature exceeding the highest melting point of the various materials contained in the starting materials, thereby obtaining a molten product of the starting materials.

[0097] When the melting method using the above-mentioned electric arc furnace is adopted, a predetermined amount of coke or the like may be added as a conductive material to the starting materials in advance in order to promote initial current flow when performing the heating step (step 2). However, the amount of coke to be added, etc., can be appropriately determined according to the mixing ratio of each raw material used in step 1.

[0098] The atmosphere in which the starting materials are melted in step 2 is not particularly limited, and may be air, nitrogen, or an inert gas atmosphere such as argon or helium. The pressure in which the materials are melted is also not particularly limited, and may be atmospheric pressure, elevated pressure, or reduced pressure, but is usually atmospheric pressure.

[0099] <Process 3> Next, the melt obtained in step 2 is cooled (preferably slowly cooled) to form an ingot. The method of forming the ingot is not particularly limited, but for example, when the melting in step 2 is performed in an electric furnace, a carbon cover is attached to the electric furnace and the melt is slowly cooled for 10 to 60 hours. The slow cooling time is preferably 20 to 50 hours, more preferably 30 to 45 hours, and even more preferably 35 to 40 hours. In addition, when slowly cooling the melt, for example, it is sufficient to allow the melt to cool in the air so that the temperature of the melt becomes 100°C or less, preferably 50°C or less. If there is a risk that the temperature of the melt will drop rapidly and the slow cooling time will be shorter than 20 to 60 hours, it is sufficient to appropriately heat the melt during the slow cooling step to avoid a sudden temperature drop of the melt. As described above, by performing the slow cooling while avoiding a sudden drop in temperature of the molten material during the slow cooling step, the elements contained in the raw materials tend to combine uniformly with each other.

[0100] <Step 4> Next, the ingot obtained in step 3 is pulverized to obtain a powder. The method of pulverizing the ingot is not particularly limited, but examples include a method of pulverizing the ingot with a pulverizer such as a jaw crusher or a roll crusher. The pulverization may be performed by using a plurality of pulverizers in combination. When pulverizing the ingot, the powder may be pulverized so that the average particle size of the pulverized powder is 3 mm or less, or 1 mm or less as necessary, in consideration of the handling of the powder in the subsequent steps. After pulverization, classification may be performed, and for example, it is possible to collect powder of a desired average particle size using a sieve or the like.

[0101] <Process 5> Next, the powder obtained in step 4 is heated in an atmosphere of 400 to 1100°C. When the heating is performed, it is preferable to separate impurities from the powder by magnetic separation in advance. After that, the powder may be heated in an atmosphere of 400 to 1100°C using an electric furnace or the like. The powder is heated and fired by this heating, and the suboxides generated in the melting step in step 3 and the distortion in the crystals generated by supercooling can be removed. The heating temperature is preferably 400°C to 1000°C, more preferably 600°C to 800°C, and in either case, the suboxides and the distortion in the crystals are easily removed. The heating time is not particularly limited, but can be, for example, 1 to 5 hours, preferably 2 to 3 hours. The heating may be performed in air or in an oxygen atmosphere. In this manner, a solid or powdered composite oxide is obtained. When a powdered composite oxide is obtained, this may be used as the composite oxide powder according to the present embodiment.

[0102] <Process 6> The solid or powdered composite oxide obtained in step 5 may be further pulverized in a pulverizer such as a planetary mill, a ball mill, or a jet mill. The pulverization may be carried out appropriately depending on the intended use of the composite oxide. When pulverizing, the composite oxide may be treated in the pulverizer for about 5 to 30 minutes. When pulverizing the composite oxide, the average particle size of the composite oxide is preferably in the above range. In this manner, the composite oxide powder according to the present embodiment can be obtained.

[0103] [Friction material composition] The friction material composition according to the present embodiment includes a friction modifier, a fiber base material, and a binder, and includes the composite oxide powder as the friction modifier. Since the composite oxide powder is contained as a friction modifier, when the friction material composition is molded and used as a friction material for brake pads, it is possible to obtain a friction material that has excellent fade resistance, a high μ value, and excellent friction stability.

[0104] (Friction modifier) The friction modifier includes an inorganic filler and an organic filler.

[0105] The inorganic filler is added for the purpose of preventing deterioration of the heat resistance of the friction material, improving the wear resistance, improving the friction coefficient, improving the lubricity, and the like.

[0106] The inorganic filler contains the composite oxide powder.

[0107] The content of the complex oxide powder in the friction material composition is preferably 5% by mass to 20% by mass, and more preferably 7% by mass to 15% by mass, when the entire friction material composition is taken as 100% by mass. When the content of the complex oxide powder is in the range of 5% by mass to 20% by mass, when the entire friction material composition is taken as 100% by mass, properties such as a high μ value can be more easily obtained.

[0108] In addition to the composite oxide powder, the inorganic filler may be, for example, tin sulfide, bismuth sulfide, molybdenum disulfide, iron sulfide, antimony trisulfide, zinc sulfide, calcium hydroxide, calcium oxide, sodium carbonate, barium sulfate, coke, mica, vermiculite, calcium sulfate, talc, clay, zeolite, mullite, chromite, titanium oxide, magnesium oxide, silica, graphite, mica, dolomite, calcium carbonate, magnesium carbonate, granular or plate-like titanate, calcium silicate, manganese dioxide, zinc oxide, iron oxide trioxide, PTFE (polytetrafluoroethylene), etc., which may be used alone or in combination of two or more. As the granular or plate-like titanate, potassium hexatitanate, potassium octatitanate, lithium potassium titanate, magnesium potassium titanate, sodium titanate, etc. may be used.

[0109] The content of the inorganic filler in the friction material composition (the total content of the inorganic filler including the composite oxide powder) is preferably 20 to 70 mass %, more preferably 30 to 65 mass %, and particularly preferably 35 to 60 mass %, when the total friction material composition is taken as 100 mass %. By setting the content of the inorganic filler within the above range, deterioration of heat resistance can be avoided, and it is also preferable in terms of the content balance of other components of the friction agent.

[0110] The organic filler is added for the purpose of adjusting friction in order to improve the noise and vibration performance and wear resistance of the friction material.

[0111] The organic filler is not particularly limited as long as it can exhibit the above-mentioned properties, and any commonly used organic filler can be used, such as cashew dust or a rubber component. The cashew dust is obtained by pulverizing hardened cashew nut shell oil. Examples of the rubber component include tire rubber, acrylic rubber, isoprene rubber, NBR (nitrile butadiene rubber), SBR (styrene butadiene rubber), chlorinated butyl rubber, butyl rubber, and silicone rubber. One or a combination of two or more selected from these can be used. The content of the organic filler in the friction material composition is preferably 1 to 25 mass%, more preferably 1 to 10 mass%, and particularly preferably 2 to 7 mass%, when the entire friction material composition is taken as 100 mass%. By setting the content of the organic filler within the above range, the elastic modulus of the friction material is increased, and deterioration of noise and vibration performance such as brake squeal can be effectively suppressed, and further deterioration of heat resistance and decrease in strength due to thermal history can also be effectively suppressed.

[0112] (Textile base material) The fiber base material exhibits a reinforcing effect in the friction material.

[0113] The friction material composition may use organic fibers, inorganic fibers, metal fibers, carbon-based fibers, etc., which are generally used as fiber base materials, and these may be used alone or in combination of two or more kinds.

[0114] As the organic fibers, aramid fibers, cellulose fibers, acrylic fibers, phenolic resin fibers, etc. can be used, and these can be used alone or in combination of two or more kinds.

[0115] As the inorganic fibers, ceramic fibers, biodegradable ceramic fibers, mineral fibers, glass fibers, silicate fibers, etc. can be used, and one or more of them can be used in combination.

[0116] The metal fibers are not particularly limited as long as they are typically used in friction materials. For example, fibers whose main component is a metal or alloy such as aluminum, iron, cast iron, zinc, tin, titanium, nickel, magnesium, silicon, copper, or brass can be used (however, in order to comply with the 2020 regulations, it is desirable for the copper content to be 5% or less).

[0117] As the carbon-based fiber, flame-retardant fiber, pitch-based carbon fiber, PAN-based carbon fiber, activated carbon fiber, etc. can be used, and these can be used alone or in combination of two or more kinds.

[0118] The content of the fiber base material in the friction material composition is preferably 5 to 40 mass%, more preferably 5 to 20 mass%, and particularly preferably 5 to 15 mass%, when the entire friction material composition is taken as 100 mass%. By setting the content of the fiber base material in the range of 5 to 40 mass%, an optimal porosity for the friction material can be obtained, squeal can be prevented, appropriate material strength can be obtained, wear resistance can be expressed, and moldability can be improved.

[0119] (Binding material) The binder has the function of binding and integrating the various materials constituting the friction material composition, and improving the strength as a friction material (brake friction material).

[0120] As the binder, a thermosetting resin can be used as a commonly used binder.

[0121] Examples of the thermosetting resin include epoxy resin, acrylic resin, silicon resin, thermosetting fluorine resin, phenol resin, various elastomer-dispersed phenol resins such as acrylic elastomer-dispersed phenol resin and silicon elastomer-dispersed phenol resin, acrylic-modified phenol resin, silicon-modified phenol resin, cashew-modified phenol resin, epoxy-modified phenol resin, alkylbenzene-modified phenol resin, etc. These can be used alone or in combination of two or more. In particular, it is preferable to use phenol resin, acrylic-modified phenol resin, silicon-modified phenol resin, and alkylbenzene-modified phenol resin, which can provide excellent heat resistance, moldability, and friction coefficient.

[0122] The content of the binder in the friction material composition is preferably 3 to 20 mass %, and more preferably 5 to 10 mass %, when the entire friction material composition is taken as 100 mass %. By setting the content within this range, the strength of the friction material can be maintained high, and the porosity of the friction material can be reduced, and deterioration of noise and vibration performance such as brake squeal caused by an increase in elastic modulus can be more effectively suppressed.

[0123] The friction material composition can be obtained by blending the above-mentioned components and optional components in a predetermined ratio, and preferably includes a step of grinding and mixing the above-mentioned components and optional components in a dispersion medium for a predetermined time using a ball mill or the like, drying to remove the dispersion medium, and sizing the particles using a sieve or the like.

[0124] [Friction material] The friction material according to this embodiment is constituted by a molded product of the friction material composition.

[0125] The friction material can be obtained by molding the friction material composition and sintering it as necessary. In the molding and sintering steps, known ceramic molding and sintering methods can be used. Examples of the molding method include dry molding methods such as uniaxial pressure molding and cold isostatic pressing. In addition to the dry molding method, injection molding, extrusion molding, slip casting, pressure casting, rotary casting, doctor blade method, etc. can also be applied as the molding method. Examples of the sintering method include atmospheric sintering, reactive sintering, atmospheric sintering, and thermal plasma sintering. The sintering temperature and the holding time at the sintering temperature can be appropriately set depending on the raw materials used. Note that sintering may be performed in the atmosphere or in an inert gas such as nitrogen gas or argon gas, or in a reducing gas such as carbon monoxide gas or hydrogen gas, depending on the type of ceramic and the type of material to be added. Sintering may also be performed in a vacuum. Furthermore, sintering may be performed while applying pressure. Thereafter, cutting, grinding, polishing, etc. are performed as necessary to obtain the friction material according to this embodiment. The friction material can be integrated with a back plate of metal such as iron to form a brake pad having the friction material and the back plate, or can be thermoformed together with the friction material composition to form a brake pad having the friction material and the back plate.

[0126] The friction material is subjected to a first fade test nine times under the following measurement condition A in accordance with the Society of Automotive Engineers of Japan standard JASO C406, and the average value of the maximum and minimum μ values ​​when the minimum friction coefficient is shown at the obtained behavior peak is calculated, and the average value is preferably 0.20μ or more, more preferably 0.22μ or more, even more preferably 0.24μ or more, particularly preferably 0.25μ or more, especially preferably 0.27μ or more, and especially preferably 0.28μ or more. The higher this value, the more the discomfort during braking can be reduced. The larger the average value of the friction coefficient, the more preferable it is, and examples thereof include 0.4 or less, 0.35 or less, and 0.33 or less. <Measurement condition A> Initial braking speed 100km / h Braking interval 35 seconds Brake temperature before braking during the first measurement: 80℃ Braking deceleration 0.45G Braking times: 9

[0127] The friction material preferably has a friction coefficient μ value of 0.39 or more, more preferably 0.40 or more, even more preferably 0.405 or more, particularly preferably 0.41 or more, especially preferably 0.42 or more, especially preferably 0.43 or more, and more especially preferably 0.44 or more. The larger the friction μ value, the more preferable it is, and examples of the friction μ value include 0.6 or less, 0.55 or less, and 0.53 or less. When the friction μ value is 0.39 or more, a stronger braking force can be obtained with a smaller pressing force. <Measurement condition B> Initial braking speed 65km / h Brake temperature before braking: 120℃ Braking deceleration 0.35G Measurements taken 200 times

[0128] The friction material is measured in the second effect test under the following measurement conditions C in accordance with the Society of Automotive Engineers of Japan standard JASO C406, and the average value of the friction coefficient in the second effect test under the following measurement conditions D in accordance with the Society of Automotive Engineers of Japan standard JASO C406 is taken as the friction coefficient X, and the average value of the friction coefficient in the second effect test under the following measurement conditions D in accordance with the Society of Automotive Engineers of Japan standard JASO C406 is taken as the friction coefficient Y. The difference in the friction coefficient [(friction coefficient X)-(friction coefficient Y)] is preferably 0.12 or less, more preferably 0.11 or less, even more preferably 0.10 or less, particularly preferably 0.09 or less, particularly preferably 0.08 or less, and especially preferably 0.05 or less. The smaller the difference in the friction coefficient [(friction coefficient X)-(friction coefficient Y)], the more preferable it is, and examples of the difference include 0.01 or more, 0.02 or more, 0.03 or more, etc. When the difference in the friction coefficient [(friction coefficient X)-(friction coefficient Y)] is 0.12 or less, the discomfort during braking can be further reduced. <Measurement conditions C> Initial braking speed 100km / h Brake temperature before braking: 80℃ Braking deceleration 0.2G Measurements taken 8 times <Measurement condition D> Initial braking speed 100km / h Brake temperature before braking: 80℃ Braking deceleration 0.7G Measurements taken 8 times EXAMPLES

[0129] The present invention will be described in detail below using examples, but the present invention is not limited to the following examples as long as it does not deviate from the gist of the invention. The composite oxide powder, friction material composition, and friction material in the examples and comparative examples contain 1.3 to 2.5 mass % of hafnium oxide as an inevitable impurity relative to zirconium oxide (calculated by the following formula (Z)). <Formula (Z)> ([Mass of hafnium oxide] / ([Mass of zirconium oxide]+[Mass of hafnium oxide]))×100(%)

[0130] Example 1 <Preparation of composite oxide powder> High-purity cerium oxide (purity 99.9%, manufactured by Mitsuwa Chemical Co., Ltd.), high-purity zirconium oxide (purity 99.9%, manufactured by Daiichi Kigenso Kagaku Kogyo Co., Ltd.), and high-purity aluminum oxide (purity 98.0%, manufactured by Nippon Light Metal Co., Ltd.) were mixed uniformly according to the composition ratio shown in Table 1.

[0131] Next, an electric arc furnace was used, and 2.0 kWh / kg was applied for 2 hours in terms of the unit power consumption, and melting was performed at 2400°C or higher. 300 g of coke was used to promote the initial current flow. After melting, the electric furnace was covered with a carbon lid and slowly cooled in the air for 24 hours to obtain an ingot. The obtained ingot was crushed to a particle size (diameter) of 3 mm or less using a jaw crusher and a roll crusher, and then the powder of 1 mm or less was collected using a sieve.

[0132] The collected powder was heat-treated to remove suboxides generated during the melting process and distortions in the crystals due to supercooling. The heat treatment was carried out in an electric furnace in air at 600°C for 3 hours. The powder was then ground for 15 minutes in a planetary mill (Fritsch Japan, device name: PULVERISETTE 6). Specifically, the powder was ground under the following conditions: <Dry grinding conditions> Grinding equipment: Planetary ball mill ZrO2 pot: 500cc ZrO2 beads (φ5mm): 900g Rotational speed: 400 rpm Grinding time: 15 min

[0133] In this manner, a composite oxide powder according to Example 1 was obtained.

[0134] <Preparation of Friction Material Composition> The materials were mixed uniformly according to the blending ratios shown in Table 2 to obtain a friction material composition according to Example 1. An Eirich Intensive Mixer manufactured by Nippon Eirich Co., Ltd. was used for mixing.

[0135] <Production of friction materials and brake pads> The obtained friction material composition was preformed in a molding press (preform machine). The obtained preform was thermoformed together with an iron back plate. The thermoforming conditions were: friction surface 155°C, B / P side 160°C, middle die 140°C, and molding pressure 500 kg / cm. 2 The gas removal conditions were 8 times on the friction surface (total 300 seconds) and 8 times for 10 seconds on the B / P side. A thermoforming press (manufactured by Marushichi Co., Ltd., product name: MA250 type) was used for thermoforming.

[0136] Next, the obtained molded product was heat-treated under the conditions of a temperature of 250°C and a pressure of 5 kg / cm. 2 The test was performed for 5 hours. As a result, a laminate of the back plate and the molded product of the friction material composition (friction material) was obtained.

[0137] The resulting laminate of the back plate and the friction material was polished using a rotary polisher, then scorched at 500° C., and further grooved to obtain the brake pad according to Example 1.

[0138] (Examples 2 to 29) <Preparation of composite oxide powder, friction material composition, friction material, and brake pad> Except for changing the mixing ratio of the starting materials to the blending ratio shown in Table 1, the composite oxide powder, friction material composition, friction material and brake pad according to Examples 2 to 29 were obtained in the same manner as in Example 1. In addition, Y2O3 shown in Table 1 is high-purity yttrium oxide (purity 99.99%, manufactured by Wako Pure Chemical Industries, Ltd.), La2O3 is high-purity lanthanum oxide (purity 99.9%, manufactured by Wako Pure Chemical Industries, Ltd.), CaO is high-purity calcium oxide (purity 99.0%, manufactured by Wako Pure Chemical Industries, Ltd.), MgO is high-purity magnesium oxide (purity 97.0%, manufactured by Kishida Chemical Co., Ltd.), SiO2 is high-purity silica (purity 99.0%, grade 1, manufactured by Kishida Chemical Co., Ltd.), and TiO2 is high-purity titanium oxide (purity 99.5%, manufactured by Kishida Chemical Co., Ltd.).

[0139] (Comparative Example 1 and Comparative Example 2) <Preparation of composite oxide powder, friction material composition, friction material, and brake pad> Composite oxide powders, friction material compositions, friction materials, and brake pads according to Comparative Examples 1 and 2 were obtained in the same manner as in Example 1, except that the blending ratios of high-purity cerium oxide, high-purity zirconium oxide, and high-purity aluminum oxide were changed to the blending ratios shown in Table 1.

[0140] [Table 1]

[0141] [Table 2]

[0142] [Composition measurement of complex oxide powder] The compositions (oxide equivalent) of the composite oxide powders prepared in the examples and comparative examples were analyzed using an ICP-AES ("ULTIMA-2" manufactured by HORIBA). As a result, it was confirmed that the blending ratios were as shown in Table 1.

[0143] [Measurement of specific surface area of ​​composite oxide powder] The specific surface areas of the composite oxide powders of the examples and comparative examples were measured by the BET method using a specific surface area meter ("Maxsorb", manufactured by Mountec). The results are shown in Table 3.

[0144] [Measurement of crystallite size of composite oxide powder] For the composite oxide powders of the examples and comparative examples, X-ray diffraction spectra were obtained using an X-ray diffractometer ("RINT2500" manufactured by Rigaku Corporation). The measurement conditions were as follows. <Measurement conditions> Measurement equipment: X-ray diffraction equipment (Rigaku, RINT2500) Source: CuKα source Sampling interval: 0.02° Scan speed: 2θ=1.0° / min Divergence slit (DS): 1° Divergence vertical limit slit: 5mm Scattering slit (SS): 1° Receiving slit (RS): 0.3 mm Monochrome receiving slit: 0.8 mm Tube voltage: 50kV Tube current: 300mA

[0145] Thereafter, the measurement results of the peak at 2θ of 40° to 42° in the XRD measurement were applied to the following Scherrer equation to calculate the crystallite size. Dp = (K × λ) / βcosθ Here, Dp is the crystallite diameter of the composite oxide powder, λ is the wavelength of the X-ray, θ is the diffraction angle, K is a constant called the shape factor, and β is the peak width after correction for the broadening of the diffraction line due to the instrument. The peak with 2θ of 40° to 42° is a peak derived from (111) of CeAlO3. The results are shown in Table 3. For reference, the X-ray diffraction spectrum of the composite oxide powder according to Example 4 is shown in FIG.

[0146] [Particle diameter of composite oxide powder D 50 , particle diameter D 90 , and particle diameter D 99 Measurement of The particle sizes of the composite oxide powders of the examples and comparative examples were measured using a laser diffraction / scattering type particle size distribution analyzer "LA-950" (manufactured by Horiba, Ltd.) More specifically, 0.15 g of the sample and 40 ml of a 0.2% aqueous solution of sodium hexametaphosphate were placed in a 50 ml beaker, which was then placed in the device (laser diffraction / scattering type particle size distribution analyzer "LA-950") for measurement. The measurement conditions were as follows. The results are shown in Table 3. Dispersion conditions: Ultrasonic dispersion at 100W for 2 minutes Refractive index: 1.70-0.0i

[0147] [Measurement of single grain crushing strength of composite oxide powder] The single grain crushing strength of the composite oxide powders of the Examples and Comparative Examples was measured using particles before being crushed in a planetary mill (particles before being crushed in a planetary mill to produce the composite oxide powders of the Examples and Comparative Examples). The particles before being crushed had a particle diameter in the range of 2.36 mm to 2.80 mm. Particles with the above particle diameter were obtained using a commercially available sieve. 50 particles were measured, and the average value was taken as the single grain crushing strength. A tensile compression tester was used as the measuring device. Specifically, the SV-201-NSL manufactured by Imada Seisakusho Co., Ltd. was used as the tensile compression tester. The load speed was 0.5 mm / min. The results are shown in Table 3.

[0148] [Measurement of true specific gravity of composite oxide powder] The true specific gravity of the composite oxide powders of the examples and comparative examples was measured in accordance with JIS Z8807: 2012. The results are shown in Table 3.

[0149] [Table 3]

[0150] [Measurement of fitting μ value] In accordance with the JASO C406 standard, the friction coefficients were measured 200 times under the following measurement condition B. The average value of the 200 friction coefficients was calculated and used as the friction coefficient μ value. The results are shown in Table 4. <Measurement condition B> Initial braking speed 65km / h Brake temperature before braking: 120℃ Braking deceleration 0.35G Measurements taken 200 times For each of the 200 measurements, a test piece that had not been used for any other test after production was used.

[0151] [Friction stability evaluation] In accordance with the Society of Automotive Engineers of Japan standard JASO C406, a second effectiveness test was conducted under the following measurement condition C, and the average value of the friction coefficients measured eight times was calculated as the friction coefficient X. In addition, a second effectiveness test was conducted under the following measurement condition D in accordance with the Society of Automotive Engineers of Japan standard JASO C406, and the average value of the friction coefficients measured eight times was calculated as the friction coefficient Y. Then, the difference in the friction coefficients [(friction coefficient X) - (friction coefficient Y)] was calculated. The results are shown in Table 4. <Measurement conditions C> Initial braking speed 100km / h Brake temperature before braking: 80℃ Braking deceleration 0.2G Measurements taken 8 times <Measurement condition D> Initial braking speed 100km / h Brake temperature before braking: 80℃ Braking deceleration 0.7G Measurements taken 8 times For each of the eight measurements, a sample that had not been used for any other test after production was used.

[0152] [Fade resistance evaluation] In accordance with the Society of Automotive Engineers of Japan standard JASO C406, the first fade test was conducted under the following measurement condition A, and the friction coefficients were obtained nine times. The largest and smallest friction coefficients, as well as the difference between the largest and smallest friction coefficients, are shown in Table 4. <Measurement condition A> Initial braking speed 100km / h Braking interval 35 seconds Brake temperature before braking during the first measurement: 80℃ Braking deceleration 0.45G Braking times: 9

[0153] [Rotor wear evaluation] After conducting all tests under the conditions of the general brake performance test items (based on JASO-C406), the average amount of rotor wear on the inner and outer sides of the rotor was calculated. The less rotor wear, the better the performance.

[0154] [Table 4]

Claims

1. Contains cerium, zirconium, and aluminum; The cerium content is 40% by mass or more and 95% by mass or less in terms of oxide, The zirconium content is within a range of 0.1 mass% or more and 50 mass% or less in terms of oxide, The aluminum content is within a range of 0.1 mass % or more and 24 mass % or less in terms of oxide, Specific surface area is 0.5m 2 / g or more 10m 2 / g or less.

2. 2. The cerium-based composite oxide powder according to claim 1, characterized in that the crystallite size is within the range of 10 nm to 80 nm.

3. Particle diameter D 50 3. The cerium-based composite oxide powder according to claim 1, wherein the average particle size is 0.5 μm or more and 20 μm or less.

4. Particle diameter D 99 4. The cerium-based composite oxide powder according to claim 1, wherein the particle size is 60 μm or less.

5. 5. The cerium-based composite oxide powder according to claim 1, characterized in that the single grain crushing strength is within the range of 50N or more and 300N or less.

6. 6. The cerium-based composite oxide powder according to claim 1, wherein the aluminum content is within the range of 0.1% by mass to 10% by mass in terms of oxide.

7. The zirconium content is within a range of 0.1 mass% to 40 mass% in terms of oxide, 7. The cerium-based composite oxide powder according to claim 1, characterized in that the aluminum content is within the range of 0.1% by mass to 10% by mass in terms of oxide.

8. The cerium content is 49% by mass or more and 91% by mass or less in terms of oxide, The zirconium content is within the range of 1 mass% or more and 43 mass% or less in terms of oxide, 8. The cerium-based composite oxide powder according to claim 1, wherein the aluminum content is within a range of 1% by mass or more and 8% by mass or less in terms of oxide.

9. 9. The cerium-based composite oxide powder according to any one of claims 1 to 8, characterized in that the total content of cerium, zirconium and aluminum is 60 mass % or more calculated as oxides.

10. CeAlO 3 The cerium-based composite oxide powder according to any one of claims 1 to 9, characterized in that it contains

11. The cerium-based composite oxide powder according to any one of claims 1 to 10, further comprising a rare earth element other than cerium.

12. 12. The cerium-based composite oxide powder according to claim 1, characterized in that it contains rare earth elements other than cerium in an amount of 0.1% by mass or more and 40% by mass or less in terms of oxide.

13. 13. The cerium-based composite oxide powder according to claim 11, wherein the rare earth element other than cerium is at least one element selected from the group consisting of yttrium and lanthanum.

14. 14. The cerium-based composite oxide powder according to any one of claims 1 to 13, characterized in that it contains an alkaline earth element.

15. The cerium-based composite oxide powder according to any one of claims 1 to 14, which is used for a friction material.

16. The friction modifier, the fibrous base material, and the binder are included, A friction material composition comprising the cerium-based composite oxide powder according to any one of claims 1 to 15 as the friction modifier.

17. 17. The friction material composition according to claim 16, wherein the content of the cerium-based composite oxide powder is in the range of 5% by mass to 20% by mass, where the entire friction material composition is taken as 100% by mass.

18. A friction material comprising a molded product of the friction material composition according to claim 16 or 17.

19. The friction material according to claim 18, characterized in that a first fade test measured under the following measurement condition A in accordance with the Automotive Engineering Society standard JASO C406 is performed nine times, and at the obtained behavior peak, an average value of the maximum μ value and the minimum μ value when the minimum friction coefficient is shown is calculated, and the average value is 0.20 μ or more. <Measurement Condition A> Initial braking speed 100km / h Braking interval 35 seconds Brake temperature before braking at the first measurement: 80°C Braking deceleration 0.45G Braking times: 9

20. 20. The friction material according to claim 18, wherein the friction coefficient measured under the following measurement condition B in accordance with the Automotive Engineering Society standard JASO C406 has a friction coefficient μ value of 0.39 or more. <Measurement Condition B> Initial braking speed 65km / h Brake temperature before braking: 120℃ Braking deceleration 0.35G Measurements taken 200 times

21. In accordance with the Automotive Engineering Society standard JASO C406, the average value of the friction coefficient measured 8 times in the second effectiveness test under the following measurement conditions C is defined as the friction coefficient X. In accordance with the JASO C406 standard, the second friction test is performed under the following measurement conditions D. The average value of the friction coefficient measured 8 times in the second friction test is defined as the friction coefficient Y.

21. The friction material according to claim 18, wherein a difference in friction coefficient [(friction coefficient X)-(friction coefficient Y)] is 0.12 or less. <Measurement conditions C> Initial braking speed 100km / h Brake temperature before braking: 80℃ Braking deceleration 0.2G Measurements were performed 8 times <Measurement Condition D> Initial braking speed 100km / h Brake temperature before braking: 80℃ Braking deceleration 0.7G Measurements were performed 8 times.

Citation Information

Patent Citations

  • Friction material

    JP1997013009A

  • Apparatus for purifying hydrogen

    JP2000302410A

  • glass-ceramic

    JP2004536771A

  • Rare earth element-added cerium oxide powder containing aluminum oxide

    JP2007022835A

  • Method for producing mixed oxides by spray pyrolysis

    JP2008529758A