Manufacturing method of copper clad laminate

The method accelerates crystallite enlargement in copper-clad laminates by combining electrolytic plating with controlled heating and tension, addressing the slow crystallite growth in existing methods and improving high-frequency signal transmission.

JP7569006B2Active Publication Date: 2024-10-17SUMITOMO METAL MINING CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2020178361
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-10-23
Publication Date
2024-10-17
Estimated Expiration
2040-10-23

AI Technical Summary

Technical Problem

Existing copper-clad laminates take a long time to achieve sufficient crystallite size for low surface resistivity, which is necessary for reducing transmission loss in high-frequency signal processing.

Method used

A manufacturing method involving electrolytic plating followed by a heating process with specific temperature and tension settings to accelerate crystallite enlargement in a copper plating film.

Benefits of technology

The crystallites of the copper plating film are enlarged in a short time, achieving low surface resistivity and reduced transmission loss in flexible printed wiring boards.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007569006000002
    Figure 0007569006000002
  • Figure 0007569006000003
    Figure 0007569006000003
  • Figure 0007569006000004
    Figure 0007569006000004
Patent Text Reader

Abstract

To provide a manufacturing method of a copper clad laminate sheet, capable of increasing a crystallite of a copper plating coat in a short time.SOLUTION: A manufacturing method of a copper clad laminate sheet 1, comprises: an electrolytic plating step of obtaining the copper clad laminate sheet 1 by forming a copper plating coat 20 onto a front surface of a substrate 10; and a heating step of performing the heating while conveying the copper clad laminate sheet 1 with a roll-to-roll. In the heating step, a conveying tension is set a value of between 50 to 105 N / m and a heating temperature is set to a value of between 134 to 170°C, or the conveying tension is set to a value of between 105 to 160 N / m and the heating temperature is set to a value of between 113 to 170°C. Thus, a crystallite of a copper coat 20 can be increased in a short time.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention ,copper More specifically, the present invention relates to a method for producing a laminated board used in the production of a flexible printed circuit board (FPC) or the like. Copper The present invention relates to a method for producing a laminate. [Background technology]

[0002] Flexible printed wiring boards in which wiring patterns are formed on the surface of a resin film are used in electronic devices such as liquid crystal panels, notebook computers, digital cameras, and mobile phones. Flexible printed wiring boards are manufactured from copper-clad laminates in which copper foil is laminated on a resin film. Copper-clad laminates are obtained by forming a base metal layer on a resin film by dry plating, and then forming a copper plating film by electrolytic plating (for example, Patent Document 1).

[0003] The amount of information processed by electronic devices is increasing year by year, and electronic devices are required to process high-frequency signals. Accordingly, flexible printed wiring boards are required to reduce transmission loss in high-frequency signal processing. For example, mobile terminals such as smartphones are required to have high-speed data communication in order to cope with the increase in data transmission and reception in recent years. Flexible printed wiring boards used in mobile terminals are required to reduce transmission loss when performing high-frequency wireless communication. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2010-205799 A Summary of the Invention [Problem to be solved by the invention]

[0005] When the pulses flowing through the wiring reach a high frequency range, a large amount of current flows on the surface of the wiring due to the skin effect. Therefore, by lowering the surface resistivity of the wiring, transmission loss can be kept low. The larger the crystallites in the copper plating film that makes up the wiring, the lower the surface resistivity of the wiring. The crystallites in the copper plating film are small immediately after plating, and grow larger over time due to room-temperature recrystallization. However, it takes a long time (e.g., several weeks) for the crystallites to reach a sufficient size through room-temperature recrystallization.

[0006] In view of the above circumstances, the present invention provides a method for producing a copper-clad laminate capable of enlarging the crystallites of a copper plating film in a short period of time. Law The purpose is to provide. [Means for solving the problem]

[0007] The method for producing a copper-clad laminate of the present invention comprises an electrolytic plating step of forming a copper plating film on a surface of a substrate to obtain a copper-clad laminate, and a heating step of heating the copper-clad laminate while transporting it by roll-to-roll, wherein the heating step is characterized in that the transport tension is 50 to 105 N / m and the heating temperature is 134 to 170° C., or the transport tension is 105 to 160 N / m and the heating temperature is 113 to 170° C. 。 Effect of the Invention

[0008] According to the present invention, the crystallites of the copper plating film can be enlarged by setting a specific heating temperature and conveying tension in the heating step performed after the electrolytic plating step, and therefore the crystallites of the copper plating film can be enlarged in a short period of time. [Brief description of the drawings]

[0009] [Figure 1] 1 is a cross-sectional view of a copper-clad laminate according to one embodiment of the present invention. [Diagram 2] 1 is a graph showing the relationship between the heating temperature of a heating furnace and the crystallite size of a copper plating film. [Diagram 3] 1 is a graph showing the relationship between crystallite size and surface resistivity of a copper plating film. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Next, an embodiment of the present invention will be described with reference to the drawings. As shown in Fig. 1, a copper-clad laminate 1 produced by a method according to one embodiment of the present invention comprises a substrate 10 and a copper plating film 20 formed on the surface of the substrate 10. The copper plating film 20 may be formed on only one side of the substrate 10 as shown in Fig. 1, or the copper plating film 20 may be formed on both sides of the substrate 10.

[0011] The substrate 10 is formed by depositing a metal layer 12 on the surface of an insulating base film 11. A resin film such as a polyimide film or a liquid crystal polymer (LCP) film can be used as the base film 11. The metal layer 12 is deposited by, for example, a sputtering method. The metal layer 12 is made of an underlying metal layer 13 and a copper thin film layer 14. The underlying metal layer 13 and the copper thin film layer 14 are laminated in this order on the surface of the base film 11. In general, the underlying metal layer 13 is made of nickel, chromium, or a nickel-chromium alloy. Although not particularly limited, the thickness of the base film 11 is generally 30 to 40 μm, the thickness of the underlying metal layer 13 is generally 5 to 50 nm, and the thickness of the copper thin film layer 14 is generally 50 to 400 nm.

[0012] The undercoat metal layer 13 may be omitted. The copper thin film layer 14 may be formed on the surface of the base film 11 via the undercoat metal layer 13, or may be formed directly on the surface of the base film 11 without the undercoat metal layer 13.

[0013] The copper plating film 20 is formed on the surface of the thin copper layer 14. Although not particularly limited, the thickness of the copper plating film 20 is generally 8 to 12 μm in the case of a copper-clad laminate 1 processed by a subtractive method, and generally 0.1 to 5 μm in the case of a copper-clad laminate 1 processed by a semi-additive method. The metal layer 12 and the copper plating film 20 are collectively referred to as the "conductor layer."

[0014] The method for manufacturing the copper-clad laminate 1 according to this embodiment includes an electrolytic plating step and a heating step. A roll-to-roll plating apparatus is used. This plating apparatus performs electrolytic plating on the long strip-shaped substrate 10 while transporting the substrate 10 by roll-to-roll.

[0015] The plating apparatus has a supply device that pays out the substrate 10 wound in a roll, and a winding device that winds up the substrate 10 (copper-clad laminate 1) after plating in a roll. On the transport path between the supply device and the winding device, it is preferable to arrange a pre-treatment tank, plating tank, post-treatment tank, liquid cutting device, and heating furnace in this order from upstream to downstream. In the pre-treatment tank, the substrate 10 is pickled. In the plating tank, an electrolytic plating process is performed. In the post-treatment tank, anti-rust treatment is performed on the copper-clad laminate 1. The liquid adhering to the copper-clad laminate 1 is cut off by the liquid cutting device. In the heating furnace, a heating process is performed.

[0016] In this way, by arranging the plating tank and the heating furnace on the transport path of the substrate 10, the electrolytic plating process and the heating process can be completed by transporting the substrate 10 once. Therefore, the manufacture of the copper-clad laminate 1, including the heating process, can be completed in a short time. In addition, it is preferable to provide tension-reducing mechanisms before and after the heating furnace on the transport path of the substrate 10. This allows the transport tension of the copper-clad laminate 1 in the heating furnace to be set as desired.

[0017] (Electrolytic plating process) An electrolytic plating process is carried out in the plating tank. While the substrate 10 is transported through the plating tank, a copper plating film 20 is formed on the surface of the substrate 10 by electrolytic plating. In this way, a long strip-shaped copper-clad laminate 1 is obtained.

[0018] A copper plating solution is stored in the plating tank. The copper plating solution contains a water-soluble copper salt. Any water-soluble copper salt generally used in copper plating solutions may be used without any particular limitation. The copper plating solution may contain sulfuric acid. The pH and sulfate ion concentration of the copper plating solution can be adjusted by adjusting the amount of sulfuric acid added. The copper plating solution may contain additives that are generally added to plating solutions. As the additive, one selected from a brightener component, a leveler component, a polymer component, a chlorine component, etc. may be used alone, or two or more types may be used in combination.

[0019] The content of each component in the copper plating solution can be selected arbitrarily. However, the copper plating solution preferably contains 15 to 70 g / L of copper and 20 to 250 g / L of sulfuric acid. In this way, the copper plating film 20 can be formed at a sufficient speed. The copper plating solution preferably contains 1 to 50 mg / L of a brightener component. In this way, the precipitated crystals can be made fine and the surface of the copper plating film 20 can be made smooth. The copper plating solution preferably contains 1 to 300 mg / L of a leveller component. In this way, protrusions can be suppressed and a flat copper plating film 20 can be formed. The copper plating solution preferably contains 10 to 1,500 mg / L of a polymer component. In this way, current concentration on the edge of the substrate 10 can be alleviated and a uniform copper plating film 20 can be formed. The copper plating solution preferably contains 20 to 80 mg / L of a chlorine component. In this way, abnormal deposition can be suppressed.

[0020] The temperature of the copper plating solution is preferably 20 to 35° C. In addition, it is preferable to stir the copper plating solution in the plating tank. For example, the copper plating solution can be stirred by spraying the copper plating solution from a nozzle onto the substrate 10.

[0021] (Heating process) A heating step is carried out in the heating furnace. That is, after the copper plating film 20 is formed, the copper plating film 20 is heated with hot air. The heating step is carried out by blowing hot air onto the copper plating film 20 to heat it while transporting the copper-clad laminate 1 by roll-to-roll.

[0022] The purpose of the heating step is usually to dry the copper plating film 20. Therefore, the heating temperature (the temperature of the copper-clad laminate 1) is usually 50 to 70° C., and the treatment time is about 1 minute.

[0023] However, when the inventors of the present application performed heating at a high temperature, which is not normally performed, it was confirmed that the higher the heating temperature, the larger the crystallites of the copper plating film 20. It was also confirmed that, when heating at a high temperature, the higher the conveying tension of the copper-clad laminate 1, the larger the crystallites of the copper plating film 20. From this, the inventors of the present application came up with the idea of ​​enlarging the crystallites of the copper plating film 20 by setting the heating temperature and conveying tension in the heating step to specific conditions. That is, the heating step in this embodiment is intended to promote recrystallization of the copper plating film 20 and enlarge the crystallites.

[0024] Specifically, the conveying tension may be set to 50-105 N / m and the heating temperature may be set to 134-170°C, or the conveying tension may be set to 105-160 N / m and the heating temperature may be set to 113-170°C. In this way, the crystallite diameter of the copper plating film 20 can be made 1,500 Å or more. If the crystallite diameter of the copper plating film 20 is made 1,500 Å or more, the surface resistivity becomes 0.25 Ω / □ or less. Therefore, the transmission loss in the processing of high-frequency signals of a flexible printed wiring board manufactured from the copper-clad laminate 1 can be kept low.

[0025] From the viewpoint of manufacturing costs, a lower heating temperature is preferable. Therefore, within the above range, it is preferable to lower the heating temperature while increasing the conveying tension. In this way, it is possible to suppress an increase in costs due to heating while achieving the desired crystallite size of the copper plating film 20.

[0026] As described above, by using a specific heating temperature and conveying tension in the heating step performed after the electrolytic plating step, the crystallites of the copper plating film 20 can be made large. The processing time for the heating step can be 1 to 2 minutes. It takes several weeks to make the crystallites large enough by room temperature recrystallization. In comparison, the crystallites of the copper plating film 20 can be made large in an extremely short time.

[0027] The electrolytic plating step and the heating step may be performed in separate devices. That is, after the copper-clad laminate 1 is produced in a plating device and wound into a roll by a winding device, the copper-clad laminate 1 may be heated in a separate heating device while being transported in a roll-to-roll manner. In this case, however, the base material 10 (copper-clad laminate 1) must be unwound and wound twice, which makes the work complicated and increases the processing time.

[0028] Furthermore, if the copper-clad laminate 1 wound in a roll is heated in that state, a temperature difference occurs between the outside and inside of the roll, and the copper plating film 20 cannot be heated uniformly. Moreover, if the inside of the roll is heated, a long time (e.g., several hours) is required. In contrast, if the copper plating film 20 is heated while being transported from roll to roll, the copper plating film 20 can be heated uniformly and the treatment can be completed in a short time (1 to 2 minutes). EXAMPLES

[0029] (Common conditions) A long strip of polyimide film (Upilex-35SGAV1 manufactured by Ube Industries, Ltd.) with a thickness of 35 μm was prepared as the base film. The base film was set in a magnetron sputtering device. A nickel-chromium alloy target and a copper target were installed in the magnetron sputtering device. The composition of the nickel-chromium alloy target was 20 mass % Cr and 80 mass % Ni. Under a vacuum atmosphere, a 25 nm thick base metal layer made of nickel-chromium alloy was formed on both sides of the base film, and a 100 nm thick copper thin film layer was formed thereon.

[0030] A copper-clad laminate was obtained by forming a copper plating film on both sides of the substrate using a roll-to-roll plating device. A plating tank and a circulating hot air heating furnace were placed on the substrate transport path, so that electrolytic plating and heating were performed in one transport of the substrate.

[0031] The copper plating solution stored in the plating tank contains 120g / L copper sulfate, 70g / L sulfuric acid, 16mg / L brightener, 20mg / L leveler, 1,100mg / L polymer, and 50mg / L chlorine. Bis(3-sulfopropyl)disulfide (a reagent manufactured by RASCHIG GmbH) was used as the brightener. Diallyldimethylammonium chloride-sulfur dioxide copolymer (PAS-A-5 manufactured by Nittobo Medical Co., Ltd.) was used as the leveler. Polyethylene glycol-polypropylene glycol copolymer (UNILUBE 50MB-11 manufactured by NOF Corporation) was used as the polymer. Hydrochloric acid (35% hydrochloric acid manufactured by Wako Pure Chemical Industries, Ltd.) was used as the chlorine.

[0032] The substrate was fed into the plating tank, and a copper plating film having a thickness of 2.0 μm was formed on both sides of the substrate by electrolytic plating. The current conditions for electrolytic plating were a current density of 1.0 A / dm 2 for 1 minute, 3.0A / dm 2 for 1 minute, 5.0A / dm 2 The plating time was 1 minute at 100° C. The temperature of the copper plating solution was set to 31° C. During the electrolytic plating, the copper plating solution was agitated by spraying the copper plating solution from a nozzle substantially perpendicularly to the surface of the substrate. The conveying tension during the electrolytic plating was set to 105 N / m.

[0033] The heating process was carried out in a circulating hot air heating furnace. Suction rollers that can cut the conveying tension are installed before and after the heating furnace, so the conveying tension inside the furnace can be set as desired. The heating treatment time was 1 minute.

[0034] The crystallite size of the copper plating film of the obtained copper-clad laminate was measured. The measurement was performed using a fully automatic multipurpose X-ray diffractometer SmartLab manufactured by Rigaku Corporation, and was calculated using the Scherrer formula from the half-width of the (200) plane peak. The measurement was performed 18 hours after the completion of electrolytic plating.

[0035] (Test 1) The conveying tension in the heating process was set to 50 N / m. The heating temperatures were 80, 100, and 11 The temperature was either 0, 130, 150, or 170° C. The crystallite sizes of the copper-clad laminates produced under each condition are shown in Table 1 and FIG.

[0036] (Test 2) The conveying tension in the heating step was 105 N / m, and the heating temperature was either 50, 60, 70, 80, 100, 110, 130, 150, or 170° C. The crystallite diameters of the copper-clad laminates produced under each condition are shown in Table 1 and FIG.

[0037] (Test 3) The conveying tension in the heating step was 160 N / m, and the heating temperature was either 80, 100, 110, 130, 150, or 170° C. The crystallite diameters of the copper plating films produced under each condition are shown in Table 1 and Figure 2.

[0038] [Table 1]

[0039] As can be seen from Table 1 and the graph in Figure 2, the crystallite diameter of the copper plating film hardly changes with heating temperature when the heating temperature is in the range of 50 to 70°C. In contrast, when the heating temperature is 80°C or higher, the crystallite diameter of the copper plating film increases as the heating temperature increases. In addition, when the heating temperature is 80°C or higher, the crystallite diameter of the copper plating film increases as the conveying tension increases.

[0040] The larger the crystallite size of the copper plating film, the lower the surface resistivity and the smaller the transmission loss of the high frequency pulse, so the larger the crystallite size of the copper plating film, the more preferable it is.

[0041] To achieve a crystallite diameter of 1,500 Å or more in the copper plating film, the conveying tension should be 50-105 N / m and the heating temperature should be 134-170°C, or the conveying tension should be 105-160 N / m and the heating temperature should be 113-170°C.

[0042] To achieve a crystallite diameter of 2,000 Å or more in the copper plating film, the conveying tension should be 50-105 N / m and the heating temperature should be 152-170°C, or the conveying tension should be 105-160 N / m and the heating temperature should be 125-170°C.

[0043] To achieve a crystallite diameter of 2,500 Å or more in the copper plating film, the conveying tension should be 50-105 N / m and the heating temperature should be 162-170°C, or the conveying tension should be 105-160 N / m and the heating temperature should be 140-170°C.

[0044] Figure 3 shows the relationship between the crystallite size and surface resistivity of the copper plating film. The graph in Figure 3 was obtained from a test carried out in the following procedure. A substrate was prepared using the procedure and conditions described in the common conditions, and a copper plating film was formed on both sides of the substrate. The heating temperature in the circulating hot air heating furnace was 50°C, and the conveying tension was 105 N / m. The crystallite size and surface resistivity of the obtained copper-clad laminate were measured 2 hours, 40 hours, 85 hours, and 229 hours after the completion of electrolytic plating. A Mitsubishi Chemical Analytical Loresta AX MCP-T370 was used to measure the surface resistivity.

[0045] The graph in Figure 3 shows that the larger the crystallite diameter of the copper plating film, the lower the surface resistivity. If the crystallite diameter of the copper plating film is 1,500 Å or more, the surface resistivity can be reduced to 0.25 Ω / □ or less. If the crystallite diameter of the copper plating film is 2,000 Å or more, the surface resistivity can be reduced to 0.23 Ω / □ or less. If the crystallite diameter of the copper plating film is 2,500 Å or more, the surface resistivity can be reduced to 0.22 Ω / □ or less.

[0046] It takes about one week for the crystallite diameter of the copper plating film to reach 1,500 Å by room temperature recrystallization, and about two weeks for it to reach 3,000 Å. In comparison, this embodiment makes it possible to increase the crystallite size of the copper plating film in an extremely short time. [Explanation of symbols]

[0047] 1 Copper-clad laminate 10 Base material 11 Base film 12 metal layer 13 Undercoat metal layer 14 Copper thin film layer 20 Copper plating film

Claims

1. an electrolytic plating step of forming a copper plating film on the surface of the substrate to obtain a copper-clad laminate; a liquid draining step of draining the liquid adhering to the copper-clad laminate after the electrolytic plating step; A heating step of heating the copper-clad laminate while transporting it by roll-to-roll after the liquid-draining step, In the heating step, the conveying tension is set to 50 to 105 N / m and the heating temperature is set to 134 to 170° C., or the conveying tension is set to 105 to 160 N / m and the heating temperature is set to 113 to 170° C. A method for producing a copper-clad laminate comprising the steps of:

2. A plating tank for carrying out the electrolytic plating step, a liquid draining device for carrying out the liquid draining step, and a heating furnace for carrying out the heating step are arranged on a roll-to-roll transport path of the base material. The method for producing a copper-clad laminate according to claim 1 .

3. In the heating step, the conveying tension is set to 50 to 105 N / m and the heating temperature is set to 152 to 170° C., or the conveying tension is set to 105 to 160 N / m and the heating temperature is set to 125 to 170° C.

3. The method for producing a copper-clad laminate according to claim 1 or 2.

4. In the heating step, the conveying tension is set to 50 to 105 N / m and the heating temperature is set to 162 to 170° C., or the conveying tension is set to 105 to 160 N / m and the heating temperature is set to 140 to 170° C.

3. The method for producing a copper-clad laminate according to claim 1 or 2.

Citation Information

Patent Citations

  • Apparatus for producing film having plated film, and method therefor

    JP2007002296A

  • Method for forming metallic pattern, metallic pattern, and printed wiring board

    JP2007287994A

  • Two-layer plated substrate and method of manufacturing the same

    JP2010205799A

  • Method and apparatus for manufacturing metallized resin film

    JP2012001793A

  • Two-layered flexible wiring substrate, and flexible wiring board using the same

    JP2015108187A