Cement Composition
The cement composition with crushed scallop shell sand and silica fume enhances compressive and bending strength, addressing application limitations and ensuring fluidity for 3D printer discharge.
Patent Information
- Application Number
- JP2022024231
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-02-18
- Publication Date
- 2024-10-17
- Estimated Expiration
- 2042-02-18
AI Technical Summary
Existing cement compositions using scallop shells for porous concrete lack sufficient compressive strength and bending strength, limiting their application, and they are not suitable for 3D printer discharge due to fluidity and viscosity issues.
A cement composition incorporating crushed scallop shell sand with a specific particle size and aspect ratio, combined with silica fume and coarse aggregate, to enhance rigidity, bending strength, and fluidity, making it applicable for 3D printer discharge.
The cement composition achieves improved compressive strength, bending strength, and desirable appearance, while maintaining appropriate fluidity and viscosity, suitable for precast concrete and 3D printer applications.
Smart Images

Figure 0007569039000003 
Figure 0007569039000004 
Figure 0007569039000005
Abstract
Description
[Technical field]
[0001] The present disclosure relates to cement compositions. [Background technology]
[0002] It is known that cement, which is a hydraulic material used in cement compositions, generates carbon dioxide during production, and various attempts have been made to reduce carbon dioxide in cement compositions. Scallop shells have traditionally been disposed of as waste. Scallop shells are produced by absorbing carbon dioxide from seawater in a short period of time, and are known to be capable of fixing and storing carbon dioxide from the atmosphere or seawater. Scallop shells contain a lot of calcium carbonate and promote the hardening of hydraulic materials, so that their use as a cement additive has been considered in the past. However, scallop shells have problems such as uneven crushing, flat shape, and salt content, and even if they are added to a cement composition to produce a hardened body, the hardened body obtained does not have sufficient strength such as compressive strength and bending strength, so that the use of cement compositions containing scallop shells is currently limited to civil engineering applications. In response to this, a proposal has been made to effectively utilize shells such as scallop shells by kneading a mixture containing shells, hydraulic material powder, and water, and then hardening the mixture using a formwork, in the form of porous concrete (see Patent Document 1). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2004-51461 A Summary of the Invention [Problem to be solved by the invention]
[0004] The porous concrete described in Patent Document 1 requires that the entire surface of the shell be covered with a stable outer shell layer in order to improve its strength, and furthermore, the compressive strength of the resulting porous concrete is insufficient, limiting its uses.
[0005] The problem to be solved by an embodiment of the present disclosure is to provide a cement composition that contains crushed scallop shell sand and that can give a hardened body that has good rigidity, bending strength, and appearance. Another problem to be solved by another embodiment of the present disclosure is to provide a cement composition that contains crushed scallop shell sand, has suitable fluidity and viscosity, and is applicable to 3D printer ejection applications. [Means for solving the problem]
[0006] Means for solving the above-mentioned problems include the following embodiments. <1> A cement composition comprising a hydraulic material, water, and fine aggregate, wherein the fine aggregate contains crushed scallop shell sand in an amount of 10% by mass to 70% by mass based on the total mass of the fine aggregate, and the crushed scallop shell sand is a fraction of crushed scallop shells, has a maximum particle size of 0.5 mm to 4.0 mm, and has an aspect ratio in the range of 1 to 25.
[0007] <2> Further containing 5.0% by mass to 20.0% by mass of silica fume based on the total solid content of the cement composition. <1> The cement composition according to claim 1. <3> Further containing coarse aggregate consisting of limestone <1> or <2> The cement composition according to claim 1. <4> For precast concrete <1> ~ <3> 13. The cement composition according to claim 12 .
[0008] <5> A cement composition comprising a hydraulic material, water, and fine aggregate, wherein the fine aggregate contains crushed scallop shell sand in an amount of 10% by mass to 100% by mass based on the total mass of the fine aggregate, and the crushed scallop shell sand is a fraction of crushed scallop shells, has a maximum particle size of 75 μm or more and less than 500 μm, and has an aspect ratio in the range of 1 to 2. <6> For 3D printer ejection <5> The cement composition according to claim 1. Effect of the Invention
[0009] According to an embodiment of the present disclosure, a cement composition can be provided that contains crushed scallop shell sand and can give a hardened body that has excellent rigidity, bending strength, and appearance. According to another embodiment of the present disclosure, a cement composition can be provided that contains crushed scallop shell sand, has suitable fluidity and viscosity, and is suitable for use in 3D printer ejection. [Brief description of the drawings]
[0010] [Figure 1] 1 is a graph showing compressive strengths of hardened cement compositions of Examples 1 to 5 and Comparative Example 1 at ages of 7 days and 28 days. [Diagram 2] 1 is a graph showing the bending fracture energy of hardened cement compositions of Examples 1, 2, 4, 5, 6 and Comparative Example 1. [Diagram 3] 1 is a graph showing load-deformation curves of hardened concrete compositions of Examples 7 to 11 and Comparative Example 2. [Figure 4] 1 is a graph showing the compressive strength at 1 day after removal from the form and the compressive strength at 28 days after the hardened concrete compositions of Examples 7 to 11 and Comparative Example 2. [Diagram 5] 1 is a graph showing the ratios of the compressive strengths of Examples 7 to 11 at 28 days, assuming that the compressive strength of the hardened concrete composition of Comparative Example 2 at 28 days is 100. [Figure 6] 1 is a graph showing fracture energy at compressive fracture of hardened concrete compositions of Examples 7 to 11 and Comparative Example 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] The cement composition of the present disclosure will be described in detail below, but the description of the constituent elements described below is an example (representative example) of the embodiment of the present invention, and is not limited to these contents. Various modifications can be made within the scope of the gist of the present invention. In addition, the term "cement composition" in this disclosure is used to include a mortar composition containing only fine aggregate and a concrete composition containing fine aggregate and coarse aggregate.
[0012] In the present disclosure, a numerical range indicated using "~" indicates a range that includes the numerical values before and after "~" as the minimum and maximum values, respectively. In the present disclosure, the amount of each component contained in the composition means the total amount of multiple substances corresponding to each component, unless otherwise specified, when the composition contains multiple substances corresponding to each component. In the numerical ranges described in the present disclosure in stages, the upper or lower limit value described in one numerical range may be replaced with the upper or lower limit value of another numerical range described in stages. In addition, in the numerical ranges described in the present disclosure, the upper or lower limit value of the numerical range may be replaced with a value shown in the examples. In this disclosure, combinations of preferred aspects are more preferred aspects. In the present disclosure, the term "process" includes not only an independent process but also a process that cannot be clearly distinguished from other processes as long as the intended purpose of the process is achieved. In the present disclosure, when a plurality of substances corresponding to each component are present in the composition, the amount of each component in the composition means the total amount of the plurality of substances present in the composition, unless otherwise specified. In the present disclosure, the term "total solids content" refers to the total amount of all components contained in a composition, excluding the solvent. In the present disclosure, "aspect ratio" refers to the ratio (b / a) of the minimum diameter (a) of a particle to the maximum diameter (b). In this disclosure, room temperature refers to 25° C. unless otherwise specified.
[0013] [Cement composition: first embodiment] The cement composition of the present disclosure is a cement composition comprising a hydraulic material, water, and fine aggregate, wherein the fine aggregate comprises 10% by mass to 70% by mass of crushed scallop shell sand relative to the total mass of the fine aggregate, and the crushed scallop shell sand is a fraction of crushed scallop shells, has a maximum particle size of 0.5 mm to 4.0 mm, and an aspect ratio in the range of 1 to 25. A cement composition containing the above amount of crushed scallop shell sand of the above size is hereinafter referred to as the first embodiment of the cement composition of the present disclosure. In the following description of the present disclosure, unless otherwise specified, when referring to a "cement composition of the present embodiment," it refers to the first embodiment of the cement composition, and when referring to a "cement composition of the present disclosure," it refers to a cement composition including the first embodiment and the second embodiment described below.
[0014] (hydraulic material) The hydraulic material in the cement composition of the present disclosure is not particularly limited, and any known hydraulic material can be appropriately selected and used. Examples of hydraulic materials include known cements such as ordinary Portland cement, white cement, moderate-heat Portland cement, low-heat Portland cement, and high-early-strength Portland cement, blast furnace slag cement containing a specified amount of blast furnace slag, fly ash cement containing a specified amount of fly ash, and silica cement containing a specified amount of siliceous admixture, and these can be used according to the purpose. Among these, when forming a hardened precast concrete body, high-early-strength Portland cement is preferably used from the viewpoint of realizing earlier demolding. Furthermore, in applications that do not require extremely high compressive strength, such as producing wall material panels, it is preferable to use blast furnace cement, from the viewpoints of promoting the effective use of waste materials and reducing carbon dioxide emissions during the production of the cement composition.
[0015] (water) The cement composition of the present disclosure contains water. The water used in the preparation of the cement composition is not particularly limited, and may be tap water. The content ratio of the hydraulic material to the water in the cement composition, that is, the water / binder ratio, can be appropriately adjusted depending on the purpose of the cement composition, added components, and the like. Water / binder ratios in this disclosure are by weight unless otherwise specified. When the water / binder ratio is low, a high-strength hardened cement product can be obtained, but the fluidity of the cement composition itself tends to decrease. In applications such as the manufacture of general structural materials, the water / binder ratio is about 50 to 60. However, according to the cement composition of the present disclosure, even if a formulation with a relatively small amount of water, that is, a water / binder ratio of 40 or more but less than 50, is used, a desired hardened cement composition can be obtained. In the present disclosure, the binder applied to the calculation of water / binder is used to include fine powders involved in the hardening of the cement composition hardened body. The binder includes various cements that are the main components of the cement composition, as well as optional components that are used together with cement, such as silica fume, blast furnace slag, and fly ash.
[0016] (fine aggregate) The cement composition of the present embodiment contains fine aggregate. The cement composition of the present embodiment contains 10% by mass to 70% by mass of crushed scallop shell sand relative to the total mass of the fine aggregate. The crushed scallop shell sand used as fine aggregate is a fraction of crushed scallop shells, with a maximum particle size of 0.5 mm to 4.0 mm and an aspect ratio in the range of 1-25. Crushed scallop shell sand is, for example, a classified product obtained by heat-treating scallop shells at 350°C to 450°C in an oxidizing atmosphere, crushing them, and then classifying the resulting crushed material using a sieve specified in JIS A 5005 (2020). Through the above classification, the crushed scallop shell sand is adjusted to have a maximum particle size in the range of 0.5 mm to 4.0 mm, and through crushing, crushed sand with an aspect ratio in the range of 1 to 25 is obtained due to the physical properties of the scallop shells.
[0017] The maximum particle size of the crushed scallop shell sand used in this embodiment can be in the range of 0.5 mm to 4.0 mm, and from the viewpoint of further improving the fluidity of the obtained cement composition and the strength of the hardened cement composition, the range of 0.5 mm to 2.0 mm is preferable, and the range of 0.5 mm to 1.0 mm is more preferable. The crushed scallop shell sand can be adjusted so that the maximum particle size falls within the above range by classifying it with a sieve, as described above. The crushed scallop shell sand of this embodiment, which has a maximum particle size of 0.5 mm to 4.0 mm, is crushed sand with a uniform particle size, which is due to being classified by sieving and contains almost no crushed material with a maximum particle size of less than 0.5 mm or more than 4.0 mm. Therefore, when used as a fine aggregate in a cement composition, it can be easily mixed uniformly. The amount of crushed material with a maximum particle diameter of less than 0.5 mm and crushed material with a maximum particle diameter of more than 4.0 mm contained in the classified product is preferably 5% by mass or less, and more preferably 3% by mass or less, of the total mass of the crushed scallop shell sand, within the desired maximum particle diameter range. The maximum particle size of the crushed scallop shell sand in this embodiment refers to the maximum size of the projected area of each particle. The crushed scallop shell sand of this embodiment has an aspect ratio of 1 to 25, and therefore contains particles that are nearly spherical and particles with a flat shape. It is believed that the hardened body of the cement composition of this embodiment has good rigidity and bending strength due to the inclusion of flat particles in the crushed scallop shell sand. From the viewpoint that the flat-shaped crushed scallop shell sand contributes to improving the rigidity of the hardened cement composition, it is preferable that the cement composition of this embodiment contains 50 mass% or more of crushed scallop shell sand having a larger aspect ratio range of 3 to 25, based on the total mass of the crushed scallop shell sand. The aspect ratio of the crushed scallop shell sand in this disclosure is a value measured by using a digital microscope VHX5000 (product name: manufactured by Keyence Corporation).
[0018] The content of crushed scallop shell sand relative to the total mass of the fine aggregate can be 10% by mass to 70% by mass, and from the viewpoint of improving the bending properties of the hardened body, it is more preferable that it be 30% by mass to 70% by mass.
[0019] (Fixation of carbon dioxide in crushed scallop shell sand) Scallop shells contain 98% calcium carbonate by mass. It is known that scallops are capable of fixing and storing carbon dioxide from the atmosphere or seawater as they grow. The amount of carbon dioxide estimated from the calcium carbonate content of crushed scallop shell sand is about 44% by mass of the crushed scallop shell sand, meaning that 44% by mass of carbon dioxide is absorbed and fixed from the atmosphere or seawater relative to the total amount of crushed scallop shell sand. Compared with cement compositions using only known fine aggregates, the cement composition of the present disclosure containing crushed scallop shell sand has good carbon dioxide fixation properties. Therefore, the inventors believe that by using crushed scallop shell sand, which grows in 2 to 3 years, for example, to produce a precast concrete hardened body as described below, and continuing to use it as part of a building material in a building, the carbon dioxide fixation effect is exerted, resulting in an environmentally favorable cement composition.
[0020] As fine aggregates other than crushed scallop shell sand, known fine aggregates can be used. Examples of known fine aggregates include natural sand such as mountain sand and sea sand, crushed sand obtained by crushing minerals, and processed sand. Among them, from the viewpoint of good strength and appearance of the obtained cement composition hardened body, limestone crushed sand, mountain sand, silica crushed sand, silica sand, etc. are preferably mentioned, and limestone crushed sand is more preferable. As the fine aggregate, it is preferable to use fine aggregates that fall under the provisions of JIS A5005 (2020) Crushed stone and crushed sand for concrete and JIS A5308 (2019) Ready Mixed Concrete.
[0021] (Other components that may be included in cement composition) In addition to the hydraulic material, water, and fine aggregate, the cement composition of the present disclosure may further contain other components that are typically used in cement compositions depending on the purpose. Other components include admixtures, coarse aggregates, inorganic pigments, chemical admixtures such as water reducing agents, AE agents (air entraining agents), defoamers, retarders, and the like.
[0022] (Admixture) The cement compositions of the present disclosure may include admixtures. As the admixture, known admixtures such as silica fume, ground granulated blast furnace slag, ground limestone, and fly ash can be appropriately used. In particular, the cement composition of the present embodiment preferably contains silica fume as an admixture, and more preferably further contains 5.0 mass % to 20.0 mass % of silica fume relative to the total solid content of the cement composition. Silica fume contains a large amount of spherical fine particles, which is expected to improve the fluidity of the unhardened cement composition, and because it contains a large amount of silicon dioxide, it is expected to further improve the strength of the resulting hardened cement composition. The cement composition of the present disclosure may contain only one type of silica fume, or may contain two or more types. The content of silica fume in the cement composition is preferably 5.0 mass% to 20.0 mass%, more preferably 5.0 mass% to 15.0 mass%, based on the total solid content of the cement composition. Silica fume is a by-product produced during the production of commonly used ferrosilicon and silicon metal, so using silica fume is an effective use of the by-product.
[0023] (coarse aggregate) The cement composition of the present embodiment may further contain a coarse aggregate. In particular, it is preferable that the cement composition further contains a coarse aggregate made of limestone. By including coarse aggregate, the cement composition of the present disclosure can be used as a concrete composition suitable for producing a hardened body having higher strength. The maximum particle size of the coarse aggregate is preferably 20 mm or less, more preferably 15 mm or less. Coarse aggregates that can be used in the cement composition of the present disclosure include, without limitation, the coarse aggregates suitable for crushed stone and crushed sand for concrete described in JIS A5005 (2020) described above, but by using a coarse aggregate made of limestone, combined with the color of the crushed scallop shell sand, which is close to the white color, a concrete composition hardened body having a good appearance can be obtained. Therefore, the cement composition can be suitably used, for example, in a usage form in which it is directly used as an interior material such as a wall material, an exterior wall panel of a building, etc.
[0024] (Other Ingredients) The cement composition of the present disclosure may further contain other components that are typically used in concrete compositions, such as a water-reducing agent such as a polycarboxylic acid-based water-reducing agent, a retarder, and a defoaming agent, depending on the purpose.
[0025] As a method for obtaining the hardened product of the cement composition of the present embodiment, known methods for producing hardened products of cement compositions and hardened products of concrete compositions can be directly applied. That is, a hydraulic material, fine aggregate, and optional admixtures, inorganic pigments, etc. are mixed, water is added and kneaded, and then an optional coarse aggregate is added and kneaded to prepare a concrete composition. The concrete composition obtained is then poured into a formwork and hardened to produce a hardened body. As a curing method after pouring into the formwork, a known curing method applicable to hardened bodies of hydraulic materials may be appropriately applied depending on the required physical properties of the hardened body to be produced.
[0026] The use of the cement composition of the present embodiment is not particularly limited, and it can be applied to the same uses as known mortar compositions, cement compositions, and concrete compositions, taking into consideration the formulation according to the purpose. The cement composition of the present embodiment can be applied to various uses such as the production of structures by exposed casting, the production of hardened precast concrete bodies, finishing mortar for plastering, and slope mortar.
[0027] As will be apparent from the examples described later, the hardened product of the cement composition of this embodiment has a compressive strength of 30 N / mm at 28 days. 2 The above has been achieved, and the composition shows a compressive strength that is practically acceptable. The hardened product of the cement composition of this embodiment may show a slight decrease in strength compared to a hardened product of a general cement composition that does not use crushed scallop shell sand as fine aggregate, but the compressive strength is in the range of about 80 to 110, assuming that the compressive strength of a hardened product of a general cement composition at 28 days is 100, and the composition shows a compressive strength that is practically sufficient. Furthermore, the hardened product of the cement composition of this embodiment has good bending strength due to the crushed scallop shell sand contained as fine aggregate, and has the advantage of being white and excellent in appearance.
[0028] (Cement composition for precast concrete) The cement composition of the present embodiment can be suitably used for precast concrete. A preferred embodiment in which the cement composition of the present embodiment is used for producing a hardened precast concrete body will be described. When the cement composition of the present embodiment is used for precast concrete, examples of the hydraulic material include cement, in particular, high-early-strength Portland cement, white cement, JIS-specified Portland cement, and mixed cement, and from the viewpoint of improving the strength at the time of removal from the form, high-early-strength Portland cement is preferred.
[0029] The admixture is not particularly limited, and the admixtures described above can be used without limitation. Among them, it is preferable to use silica fume from the viewpoint of supplementing the physical properties of the flat scallop shell crushed sand having the above aspect ratio and further improving the fluidity and compressive strength. As the coarse aggregate, any coarse aggregate satisfying the above-mentioned JIS regulations can be used appropriately. Among them, it is preferable to use crushed limestone from the viewpoint of improving the appearance.
[0030] The strength of precast concrete is adjusted according to the shape and intended use, but the design standard strength is 18N / mm 2~60N / mm 2 can range from 30N / mm 2 More than this is preferable. To achieve the above strength, the unit water amount can be 140 kg to 220 kg, and preferably 180 kg to 200 kg, and the unit cement amount can be 300 kg to 700 kg, and preferably 350 kg to 600 kg. The content of the fine aggregate in the total amount of aggregate in the cement composition can be in the range of 35% by mass to 60% by mass, and preferably 40% by mass to 50% by mass. The water / binder ratio can be 20 to 60, and preferably 40 to 50, calculated as mass equivalent, depending on the application of the hardened body.
[0031] The strength required for the precast concrete to be removed from the form is 12N / mm, which is easy to handle. 2 For smaller products, the demold strength must be 12N / mm 2 There may be no problem if it is less than this. There is no particular limitation on the curing method after the cement composition is poured into the formwork, and generally used methods such as normal pressure steam curing and natural curing may be used.
[0032] The obtained precast concrete hardened body is white and has a good appearance, so it may be used as is, or as a finishing process, it may be scraped off to expose the aggregate, with an emphasis on aesthetics, or it may be finished by tiling, stone laying, metal paneling, etc. In addition, because of its good appearance, it can be used as exposed concrete, and because the crushed scallop shell sand has internal pores that easily absorb colorants, it can also be finished with paint. Furthermore, the cement composition itself may be used as a color concrete finish by combining white cement, inorganic pigments, etc., and the surface of the color concrete by combining white cement, inorganic pigments, etc. may be subjected to treatments such as sandblasting, polishing, washing, etc. to perform a surface processing finish that exposes the aggregate, thereby achieving an appearance with superior design.
[0033] In the cement composition of this embodiment, cement is used as the hydraulic material, crushed scallop shell sand (main component: CaCO3) and crushed limestone sand (main component: CaCO3) are used as fine aggregates, and crushed limestone (main component: CaCO3) is used as coarse aggregate. As a result, the obtained precast concrete hardened body has the advantage that all of the raw materials can be used as raw materials for cement after dismantling, making it a completely recycled concrete.
[0034] [Cement composition: second embodiment] The cement composition of the present disclosure is a cement composition comprising a hydraulic material, water, and fine aggregate, wherein the fine aggregate comprises 10% by mass to 100% by mass of crushed scallop shell sand relative to the total mass of the fine aggregate, and the crushed scallop shell sand is a fraction of crushed scallop shells, having a maximum particle size of 75 μm or more and less than 500 μm, and an aspect ratio in the range of 1 to 2. A cement composition containing the above amount of crushed scallop shell sand of the above size is hereinafter referred to as the second embodiment of the cement composition of the present disclosure. The hydraulic material and water used in the cement composition of the second embodiment can be the same as those in the cement composition of the first embodiment described above. The aspect ratio of the crushed scallop shell sand in the second embodiment is a value measured using a digital microscope VHX5000 (product name: manufactured by Keyence Corporation). In addition, since the crushed scallop shell sand of the second embodiment has finer particles than the crushed scallop shell sand of the first embodiment, the maximum particle size is measured using a laser diffraction particle distribution analyzer (product name: SALD-200, manufactured by Shimadzu Corporation).
[0035] (fine aggregate) The cement composition of the second embodiment includes fine aggregate. The cement composition of the second embodiment contains 10% by mass to 100% by mass of crushed scallop shell sand relative to the total mass of the fine aggregate, that is, the fine aggregate may be entirely crushed scallop shell sand. The crushed scallop shell sand used as fine aggregate may be fine crushed scallop shell sand having a maximum particle size of less than 0.5 mm, an aspect ratio in the range of 1 to 2, and a spherical or nearly spherical shape, which is the residue of the classified crushed scallop shell material of the first embodiment described above. The crushed scallop shell sand is, for example, fine crushed scallop shell sand obtained by heat-treating scallop shells at 350°C to 450°C in an oxidizing atmosphere, crushing the resulting crushed material, and then classifying the resulting material with a sieve specified in JIS A 5005 (2020) and passing it through a 0.5 mm mesh sieve. The crushed scallop shell sand that has passed through the 0.5 mm mesh may be further crushed for the purpose of making the particle size uniform, adjusting the aspect ratio to 1 to 2, etc.
[0036] The content of crushed scallop shell sand relative to the total mass of the fine aggregate can be 10% by mass to 100% by mass, and from the viewpoint of ensuring stable rheological properties such as the plastic viscosity and yield value of the cement composition, and improving stable fluidity when poured, it is more preferable that it be 40% by mass to 90% by mass.
[0037] As the fine aggregate other than the crushed scallop shell sand used in the cement composition of the second embodiment, a known fine aggregate can be used, as in the cement composition of the first embodiment. Examples of known fine aggregates include natural sand such as mountain sand and sea sand, crushed sand obtained by crushing minerals, processed sand, etc. Among them, from the viewpoint of good strength and appearance of the obtained hardened cement composition body, crushed limestone sand, mountain sand, crushed silica sand, silica sand, etc. are preferred, and crushed limestone sand is more preferred.
[0038] (Other components that may be included in cement composition) The cement composition of the second embodiment may also contain, in addition to the hydraulic material, water and fine aggregate, other components that are usually used in cement compositions depending on the purpose. Other components include admixtures, coarse aggregates, inorganic pigments, chemical admixtures such as water reducing agents, air entraining agents, defoamers, retarders, etc.
[0039] As in the first embodiment, examples of the admixture in the cement composition of the second embodiment include silica fume, ground granulated blast furnace slag, ground limestone, and fly ash, and among these, it is preferable to include silica fume. The content of silica fume is preferably 5.0% by mass to 20.0% by mass based on the total solid content of the cement composition.
[0040] The cement composition of the second embodiment of the present disclosure is suitably used for discharging from a 3D printer. The cement composition of the second embodiment contains fine particles of crushed scallop shell sand that are nearly spherical in shape as fine aggregate, so it maintains appropriate fluidity and has good pumpability and 3D printer ejectability. For 3D printer discharge applications, the water / binder ratio can be about 30 to 50 from the standpoint of fluidity. By satisfying the above-mentioned preferred contents of crushed scallop shell sand, silica fume, etc., and the specified water / binder ratio, the cement composition of the second embodiment has an appropriate viscosity.
[0041] The cement composition of the second embodiment maintains its shape after being ejected from a 3D printer by adjusting the shape, aspect ratio, yield value due to the particle size characteristics, and plastic viscosity of the crushed scallop shell sand. By allowing it to harden by natural curing, a hardened cement composition of any shape can be easily formed using a 3D printer. The yield value due to the particle size characteristics in the cement composition of the second embodiment is preferably about 2 Pa to 10 Pa, and the plastic viscosity is preferably about 3 Pa·s to 7 Pa·s. The plastic viscosity can be measured using a Brookfield B-type viscometer capable of adjusting the rotation speed and measurement time. In addition, the cement composition after being discharged by the 3D printer may be subjected to known curing such as room temperature steam curing while maintaining its shape. 3D printers to which the cement composition of the present disclosure can be applied include gantry-type, robot arm-type, and manual printers. EXAMPLES
[0042] The present invention will be described in detail below with reference to examples. However, the following examples are merely examples of one embodiment and are not intended to limit the scope of the present invention. In the following examples, room temperature means 25° C. unless otherwise specified.
[0043] [Examples 1 to 6, Comparative Example 1] (Mixture of cement (mortar) composition) <Materials used> (cement) Cement: High-early-strength Portland cement (C) (manufactured by Taiheiyo Cement Corporation, density: 3.14 g / cm 3 ) (water) Water: Tap water (W) (Admixture) Silica fume (Sp): Silica fume Grade 940 (product name: Elkem Japan Co., Ltd., average particle size 0.15 μm, density 2.2 g / cm 3 ) (fine aggregate) Fine aggregate: crushed limestone sand (Ls) (from Torigatayama, Kochi Prefecture, particle size 5 mm or less, surface dry density: 2.65 g / cm 3 ) Fine aggregate: Crushed scallop shell sand (Hs) (maximum particle size: 1 mm, aspect ratio: 5, surface dry density: 2.62 g / cm 3 ) (Other additives) Chemical admixture: Polycarboxylic acid ether compound (Ad): High-performance water reducer (product name: 8000s, manufactured by Pozzolith)
[0044] The following Table 1 shows the cement mixes of the examples and the comparative examples. The materials used in the mixes are indicated by the above symbols, and the details of each material are as described above. In Table 1, (C×) indicates the content ratio of the chemical admixture to the hydraulic material.
[0045] [Table 1]
[0046] (Adjustment of cement composition) According to the formulation in Table 1 above, the entire amounts of water, cement, fine aggregate, admixtures, etc. were mixed together in a mixer (mortar mixer), and the entire amount was added to the mixer and stirred for 3 minutes at a speed of 90 rpm (revolutions per minute) to prepare a cement composition.
[0047] (Evaluation of cement compositions) 1.Compressive strength Each of the obtained cement compositions was poured into a form for cylindrical specimens (diameter 50 mm, height 100 mm) and subjected to sealed curing at 20°C (for 7 days and 28 days) to obtain hardened cement composition bodies as cylindrical specimens for measuring the compressive strength of the cement compositions. The obtained cylindrical specimens were measured for compressive strength at 7 days and 28 days according to JIS A 1108 (2018): Compressive strength method for concrete. Three specimens were prepared for each example and comparative example, and the average value was used as the compressive strength. The compressive strength was measured for the hardened bodies of Examples 1 to 5 and Comparative Example 1. The results are shown in FIG. FIG. 1 is a graph showing the 7-day compressive strength and the 28-day compressive strength of the hardened cement compositions of Examples 1 to 5 and Comparative Example 1.
[0048] From the graph in FIG. 1, it can be seen that the hardened cement compositions of Examples 1 to 5 all had a compressive strength of 30 N / mm 2 All of the compressive strengths exceeded the limits of the test, and no practical problems were observed. Compared to the specimen of Comparative Example 1 which did not contain crushed scallop shell sand as fine aggregate, the specimens of Example 1 which contained 50% by mass of crushed scallop shell sand and Example 3 which contained 70% by mass tended to have lower compressive strength. The specimen of Example 2, which contained 5 mass% silica fume as an admixture, had improved compressive strength compared to the specimen of Example 1, which contained the same level of crushed scallop shell sand. The specimen of Example 4, which contained 5 mass% silica fume as an admixture, and the specimen of Example 5, which contained 10 mass% silica fume as an admixture, both had improved compressive strength compared to the specimen of Example 3, which contained the same level of crushed scallop shell sand. These results show that the further inclusion of silica fume as an admixture improves the compressive strength of the hardened cement composition obtained by the cement composition of the present disclosure.
[0049] 2. Bending strength Each of the obtained cement compositions was poured into a form for a rectangular columnar test specimen (40×40×160 mm), sealed and cured at 20° C. to obtain hardened cement composition specimens as rectangular columnar test specimens for bending fracture strength. In accordance with JIS R 5201 (2015): Physical testing methods for cement, three hardened rectangular column specimens aged 28 days were prepared, and the bending fracture strength was measured using a three-wire central point loading method. The bending breaking strength was evaluated for the test specimens of Example 1, Example 2, Example 4, Example 5, and Example 6 containing 30 mass % of crushed scallop shell sand. The results are shown in FIG. FIG. 2 is a graph showing the bending fracture energy of the hardened cement compositions (test specimens) of Examples 1, 2, 4, 5, and 6 and Comparative Example 1. In terms of bending strength, the specimen of Example 1, in which the content of crushed scallop shell sand in the fine aggregate was 50 mass%, showed strength approximately equal to that of the specimen of Comparative Example 1, which did not contain crushed scallop shell sand, but the specimens of Examples 2, 4, 5, and 6 all had bending strengths at a higher level than that of the specimen of Comparative Example 1. This is thought to be because the inclusion of an effective amount of flat crushed scallop shell sand with an aspect ratio of 5 as fine aggregate did not adversely affect the bending strength, but rather improved resistance to bending, thereby further improving the bending strength.
[0050] [Examples 7 to 11, Comparative Example 2] In the following examples and comparative examples, the cement composition of the present disclosure was prepared as a concrete composition to which coarse aggregate was added.
[0051] (Concrete composition mix) <Materials used> (cement) Cement: High-early-strength Portland cement (C) (manufactured by Taiheiyo Cement Corporation, density: 3.14 g / cm 3 ) (water) Water: Tap water (W) (Admixture) Silica fume (Sp): SF-CP (product name: Tomoe Engineering Co., Ltd., average particle size 0.15 μm, density 2.2 g / cm 3 ) (fine aggregate) Fine aggregate: crushed limestone sand (Ls) (from Torigatayama, Kochi Prefecture, particle size: 5 mm or less, surface dry density: 2.65 g / cm 3 ) Fine aggregate: Crushed scallop shell sand (Hs) (maximum particle size: 1 mm, aspect ratio: 5, surface dry density: 2.62 g / cm 3 ) (coarse aggregate) Coarse aggregate: crushed limestone (Lg) (from Torigatayama, Kochi Prefecture, particle size: 20 mm or less, surface dry density: 2.65 g / cm 3 ) (Other additives) Chemical admixture: Polycarboxylic acid ether compound (Ad): High-performance water reducer (product name: 8000s, manufactured by Pozzolith) Chemical admixture: Air entraining (AE) agent (AE): Natural resin acid salt (product name: Vinsol W, manufactured by Yamaso Chemical Co., Ltd.)
[0052] The following Table 2 shows the cement mixes of the examples and comparative examples. The materials used in the mixes are indicated by the above symbols, and the details of each material are as described above. In Table 2, (C×) indicates the content ratio of the chemical admixture (Ad) or the air-entraining agent (AE) to the hydraulic material.
[0053] [Table 2]
[0054] (Adjustment of concrete composition) The crushed limestone sand as fine aggregate, crushed scallop shell sand, cement, and optionally, silica fume were charged into a mixer (pan-type mixer) in that order, and the mixture was stirred for 30 seconds by dry mixing to mix the fine aggregate and cement and to enhance dispersibility. Thereafter, water was added to the mixture containing cement obtained above using a mixer (pan-type mixer), and the mixture was stirred at a speed of 90 rpm for 60 seconds to obtain a mortar composition. Furthermore, coarse aggregate was added in an amount selected taking into consideration the bulk volume of the coarse aggregate, and the mixture was mixed for 90 seconds to prepare a concrete composition.
[0055] (Evaluation of concrete composition) 1.Compressive strength Each concrete composition obtained was poured into a form for cylindrical specimens (diameter 100 mm, height 200 mm), sealed and cured at 20°C (1 day and 28 days), to obtain a hardened concrete composition as a cylindrical specimen for measuring the compressive strength of the concrete composition. Three cylindrical specimens were prepared for each of the examples and comparative examples, and the average value of the three specimens was used as the evaluation result. The compressive strength of the obtained cylindrical specimen was measured according to JIS A 1108 (2018): Compressive strength test method for concrete. The relationship between load (kN) and deformation (mm) was plotted to obtain a load-deformation curve. The results are shown in Figure 3. Fig. 3 is a graph showing the load-deformation curves of the hardened concrete compositions of Examples 7 to 11 and Comparative Example 2. The results of Fig. 3 show that the specimen of Example 11 had improved compressive strength compared to the specimen of Comparative Example 2, which did not contain crushed scallop shell sand. The specimens of Comparative Examples 7 to 10 showed a slight decrease in compressive strength, but showed larger deformation at the time of compressive fracture, indicating superior toughness.
[0056] According to the above-mentioned concrete compression test method, the compressive strength at 1 day and 28 days, which are the form-removal strength, were measured. The results are shown in Figure 4. FIG. 4 is a graph showing the 1-day demold strength and 28-day compressive strength of the hardened concrete compositions (cylindrical test specimens) of Examples 7 to 11 and Comparative Example 2.
[0057] From the graph of FIG. 4, all of the specimens of Examples 7 to 11 had a compressive strength of 12 N / mm 2 The compressive strength at 28 days is also above the desired level of 30N / mm 2 All of the compressive strengths exceeded the limits of the test, and no practical problems were observed. Fig. 5 shows the ratios of the compressive strengths of the test specimens of Examples 7 to 11, where the compressive strength of the test specimen of Comparative Example 2 at 28 days is taken as 100. Fig. 5 is a graph showing the compressive strengths of Examples 7 to 11 at 28 days, where the compressive strength of the hardened concrete composition of Comparative Example 2 at 28 days is taken as 100. From the results of FIG. 5, the compressive strength ratio of the specimens of Example 7, Example 8, and Example 10 containing crushed scallop shell sand as fine aggregate was about 80% to 90% of the compressive strength of the specimen of Comparative Example 2, and a slight decrease in compressive strength was observed. The specimen of Example 9 containing 5 mass% of silica fume as an admixture was found to have an improved compressive strength compared to the specimen of Example 8. The compressive strength of the specimen of Example 11 containing 20 mass% of silica fume as an admixture was 110.88 compared to the specimen of Comparative Example 2, compared to the level of Example 10 containing 70 mass% of crushed scallop shell sand, and it was found that the compressive strength was further improved by adding silica fume as an admixture in addition to the crushed scallop shell sand.
[0058] Fig. 6 is a graph showing the fracture energy at compressive fracture of the hardened concrete compositions of Examples 7 to 11 and Comparative Example 2. The results of Fig. 6 show that by including crushed scallop shell sand as fine aggregate, the compressive strength is slightly reduced compared to the hardened concrete compositions that do not include crushed scallop shell sand, whereas by including crushed scallop shell sand as fine aggregate, the fracture energy at compressive fracture is increased, and fracture resistance is improved.
[0059] 2.Appearance evaluation When the test specimens of Examples 7 to 11 were visually observed, all of them were white hardened concrete compositions with excellent appearance.
[0060] From the results of the Examples and Comparative Examples, it was confirmed that the cement composition of the present disclosure, which contains crushed scallop shell sand, can obtain a hardened body having good rigidity, bending strength, and appearance. It was also found that the compressive strength of the hardened body of the cement composition was at a level that was acceptable for use in the Examples.
Claims
1. A cement composition comprising a hydraulic material, water, and fine aggregate, The fine aggregate contains 10% by mass to 70% by mass of crushed scallop shell sand based on the total mass of the fine aggregate, The crushed scallop shell sand is a fraction of crushed scallop shells, and has a maximum particle size of 0.5 mm to 4.0 mm and an aspect ratio in the range of 1 to 25.
2. 2. The cement composition of claim 1, further comprising 5.0% to 20.0% by weight of silica fume, based on the total solids content of the cement composition.
3. 3. The cement composition according to claim 1 or 2, further comprising a coarse aggregate made of limestone.
4. The cement composition according to any one of claims 1 to 3, which is for precast concrete.
5. A cement composition comprising a hydraulic material, water, and fine aggregate, The fine aggregate contains 10% by mass to 100% by mass of crushed scallop shell sand based on the total mass of the fine aggregate, The crushed scallop shell sand is a fraction of crushed scallop shells, and has a maximum particle size of 75 μm or more and less than 500 μm and an aspect ratio in the range of 1 to 2.
6. The cement composition according to claim 5, which is for ejection by a 3D printer.
Citation Information
Patent Citations
Manufacture of dressing construction material utilizing shell
JP1982166358A
Immobilization of toxic elements in incinerator ash in environmentally safe soil cement compositions and method of production
JP1993508376A
Cement mortar containing shell and its product
JP1997165252A
New powder, artificial sand, artificial culture soil, decorative material and aggregate
JP1998139425A
Shell concrete and its producing process
JP2004051407A