Metal Injection Molding One-time Sintering Manufacturing Process of Bimetal Assembly Golf Head
The unified MIM process for golf heads with matched shrinkage rates addresses inefficiencies in traditional methods by integrating tungsten alloy and stainless steel in a single sintering step, reducing costs and improving quality and toughness.
Patent Information
- Application Number
- JP2023079055
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2023-03-09
- Filing Date
- 2023-05-12
- Publication Date
- 2024-10-17
- Estimated Expiration
- 2043-05-12
AI Technical Summary
Traditional manufacturing methods for golf heads with bimetallic assemblies, such as those combining a stainless steel body and tungsten alloy balance weights, are inefficient, costly, environmentally harmful, and prone to cracking due to separate production and assembly processes, which include precision casting, forging, CNC machining, and welding, leading to long cycles, high costs, and low production capacity.
A unified manufacturing process through metal injection molding (MIM) that adjusts the ratio of tungsten alloy and stainless steel to match shrinkage rates, allowing for a one-time sintering of a bimetallic golf head by embedding tungsten alloy within stainless steel, using a specific blend of materials and conditions including nitrogen gas sintering.
This method reduces manufacturing steps, time, and costs while enhancing the toughness and quality of the golf head, minimizing cracking risks and achieving high yield rates.
Smart Images

Figure 0007569115000001
Abstract
Description
[Technical field]
[0001] The present invention relates to the field of materials processing, and more particularly to a metal injection molding, one-sinter manufacturing process for bimetallic assembly golf heads. [Background technology]
[0002] Golf heads often include two assemblies: a general metal body (stainless steel, low alloy steel) and a high-density balance weight (tungsten alloy). For example, attaching a high-density balance weight to the bottom of an iron or sand wedge can increase the moment of inertia during a swing and increase the flight distance, while attaching a high-density balance weight to both sides of a putter can reduce shaking and improve stability during a shot. Currently, the manufacturing method is to manufacture two different assemblies by different processes (e.g., precision casting, forging, CNC machining, powder metallurgy, etc.), and then assemble them by welding, nut fixing, riveting, etc. The traditional golf head metal processing process has the disadvantages of long process flow, large environmental protection pressure, many steps, high manufacturing costs, long manufacturing cycle, etc., specifically, as follows: (a) Precision casting requires the production of a mold first. The drying cycle of the mold is about 10 days, and the entire production cycle is about 15 days. The mold produces a large amount of solid waste such as sand and powder. The environmental protection pressure is large, the working environment is poor, and there are occupational hygiene problems due to high temperature and dust. The surface of the casting is rough, the polishing cost of post-processing is high, and the internal porosity of the casting reduces the yield rate. (b) The forging cost is high, and the forging process needs to be done one by one, which means low production capacity and cannot meet customer demand. It is not possible to manufacture parts with complex structures. After forging the molding, there is a lot of machining allowance, and it is necessary to combine CNC processing, which is expensive. (c) CNC machining has the lowest production capacity. It takes 1-2 hours to process one golf head using CNC equipment. Only a large investment in equipment can meet the demand, and the demand for labor is also high.
[0003] When assembling two parts with different metal components into a golf head, currently, the metal body with normal specific gravity and the balance weight of high specific gravity tungsten alloy are separately manufactured and then assembled together. The assembly process includes welding, screws, riveting, etc., and the steps are large, and the toughness of tungsten alloy is low, so it is easy to break brittle, and cracks will occur during the manufacturing and use process, leading to breakage.
[0004] Metal injection molding (MIM) based on powder metallurgy technology has become a mature process for manufacturing golf heads. Golf head body assemblies can be manufactured, and tungsten alloy balance weight assemblies can also be manufactured, but the two metal materials need to be manufactured separately and then assembled together due to differences in the MIM process. These differences include, but are not limited to, the sintering temperature is different, the sintering temperature of tungsten alloy is 1400°C or higher, and the sintering temperature of stainless steel and low alloy steel is 1200-1380°C (a); the sintering shrinkage rate is different, the shrinkage rate of tungsten alloy is 1.20 or higher, and the shrinkage rate of stainless steel and low alloy steel is 1.165-1.216 (b); and the sintering atmosphere is different, the tungsten alloy needs to be sintered at normal pressure under the protection of hydrogen gas or inert gas, and the stainless steel and low alloy steel need to be sintered in vacuum under the protection of inert gas (c). Summary of the Invention [Problem to be solved by the invention]
[0005] To solve the above problems, the present invention combines tungsten alloy powder to obtain a powder that can be injection molded in a stainless steel metal mold and subjected to a series of subsequent operations.
[0006] The core of the present invention is to adjust the ratio of stainless steel and tungsten alloy, and make the shrinkage rate of tungsten alloy and stainless steel the same, and then use in-mold injection molding to fit them together, and obtain the golf head with high molding rate and excellent quality, which is manufactured by in-mold injection molding and one-time sintering process. [Means for solving the problem]
[0007] The technical means of the present invention are as follows:
[0008] The bimetal assembly golf head of the present invention is characterized in that the manufacturing raw materials include a tungsten alloy, a stainless steel and an adhesive, the mass content of tungsten in the tungsten alloy is 30-99%, and the mass content of other alloy components is 0-20%, and the stainless steel is selected from iron-based raw materials, and is one selected from 304 stainless steel, 316L stainless steel and 17-4PH stainless steel.
[0009] The other alloying components of the present invention include nickel with a content of 4 to 15 parts by weight, and copper / iron with a content of 2 to 10 parts by weight.
[0010] Furthermore, the weight ratio of the tungsten alloy powder to the stainless steel powder is 1:40 to 1:20.
[0011] Furthermore, the stainless steel powder and the adhesive are mixed in a ratio of 1-3:0.4-0.8 parts by weight.
[0012] Furthermore, the method for manufacturing the golf head further comprises: Step 1: mixing tungsten alloy powder, stainless steel powder, and adhesive; Step 2: the tungsten alloy input material is first injection molded to obtain an in-mold injection molding embedded part, and then the stainless steel input material is put into the mold for in-mold injection molding to obtain an injection molding body in which the stainless steel input material encases the tungsten alloy input material; Step 3 is to degrease the compact in a three-step process; and step 4 of sintering the degreased green body at a temperature of 1380-1420° C. in a mixed gas atmosphere of nitrogen and hydrogen at 40-45 Kpa to obtain a sintered product of the bimetal golf head.
[0013] Furthermore, the plasticization temperature of the injection molding process described in step 2 is set to 180° C. to 220° C., the heating temperature of the mold is set to 90° C. to 120° C., and the injection pressure is set to 110 to 130 MPa.
[0014] Furthermore, the density of the tungsten alloy before sintering is 8 to 9 g / cm 3 After sintering, it has a density of 14-15g / cm 3 It is.
[0015] Furthermore, the three-stage degreasing method described in step 3 involves first pre-cleaning the molded body, placing it in a degreasing furnace, and degreasing it for 13 to 22 hours in a nitrogen gas atmosphere at a nitrogen gas flow rate of 0.8 L / min at a temperature of 100°C to 140°C, and then post-cleaning to obtain a roughly molded crude golf head.
[0016] Furthermore, the sintering process described in step 4 is divided into three steps, which are negative pressure debinding, vacuum sintering and partial pressure sintering, respectively.
[0017] Additionally, the adhesive is comprised of 90% polyoxymethylene, 3% ethylene copolymer, 4% ethylene propylene rubber, 1% glycerol monostearate, 1% 2,6-di-tert-butyl-4-methylphenol, and 1% high density polyethylene HDPE. Effect of the Invention
[0018] The present invention provides a bimetal assembly golf head manufacturing process, which is completed by the process of bimetal injection molding followed by degreasing and sintering at one time, injection molding a metal tungsten alloy, embedding the molded tungsten alloy injection molding into a stainless steel injection mold, and injection molding the stainless steel input material and the tungsten alloy injection molding to obtain an integrated injection molding by in-mold injection molding, and then degreasing and sintering to manufacture a bimetal assembly golf head. The present invention is applicable to the golf head that needs to assemble a balance weight, which is completed by the process of bimetal injection molding followed by degreasing and sintering at one time, which breaks through the limitation of only manufacturing one metal component part at one time in the traditional metal injection molding (MIM) technology, and can mold stainless steel and tungsten alloy metal parts at one time, which has the advantages of fewer manufacturing steps, shorter construction time, and lower cost, and the manufactured golf head has good appearance, high toughness, and is not easily cracked. [Brief description of the drawings]
[0019] [Figure 1] FIG. 1 is a schematic diagram of a bimetal assembly golf head. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0020] Example 1 In the bimetal assembly golf head of this embodiment, the manufacturing materials include a tungsten alloy, a stainless steel, and an adhesive, and the tungsten alloy includes, by mass percentage, 80% tungsten, 15% copper, and 5% nickel, and the stainless steel is selected from 17-4PH stainless steel.
[0021] The weight ratio of the tungsten alloy powder to the stainless steel powder is 1:20.
[0022] The stainless steel powder and adhesive are mixed in a ratio of 3:0.8 parts by weight.
[0023] The manufacturing method of the golf head of the embodiment includes the following steps 1 to 4.
[0024] In step 1, the tungsten alloy and adhesive powder are mixed and kneaded, and then injection molded to form a primary injection molded body.
[0025] Step 2: In the input material formation, the stainless steel metal powder is preheated to 180°C, stirred, and the rotation speed is 15r / min, adhesive is added, and the temperature is 180°C and kneaded for 2.5h, then cooled to 160°C, kneaded for 2h, stirred, and the rotation speed is 45r / min, and the kneading is completed, and the granular input material is extruded and granulated.
[0026] The adhesive used was mainly composed of 90% polyoxymethylene, 3% ethylene copolymer, 4% ethylene propylene rubber, 1% glycerol monostearate, 1% 2,6-di-tert-butyl-4-methylphenol and 1% high density polyethylene HDPE (formulation components of case 9 of adhesive for metal injection molding approved by CN2018108977446).
[0027] Step 3: The tungsten alloy and adhesive powder are mixed and kneaded, and then injection molded to form a primary injection molded body; the 304 stainless steel powder is made into an input material form and then injection molded; then the tungsten alloy compact is put into the injection molding machine together with the injection molded tungsten alloy compact; when the 304 stainless steel alloy is injection molded, the tungsten alloy compact is put into the injection mold, and then injection molded again together with the 304 stainless steel alloy; the two metals are integrated into one mold to obtain a bimetal golf head compact, the case material of which is the stainless steel alloy 304, and the tungsten nickel iron alloy balance weight is embedded inside; The conditions for bimetal in-mold injection molding are a plasticization temperature of 210°C, a mold heating temperature of 120°C, and an injection pressure of 130 MPa. Once a bimetal injection molded golf head body is obtained, a primary molded body can be obtained.
[0028] Step 4: The bimetal injection molded golf head is degreased and sintered. The molded body is pre-cleaned, put into a degreasing furnace, and degreased in nitrogen gas atmosphere at 120°C for 22 hours, then post-cleaned. The degreasing and sintering parameters are: temperature in the degreasing furnace is 130°C, nitrogen gas flow rate is 0.8L / min, and degreasing time is 24 hours. The temperature in the sintering furnace is 1380°C, the sintering time is 24 hours, and the sintering atmosphere does not require the hydrogen gas atmosphere required for sintering tungsten alloy, but is directly sintered in nitrogen gas atmosphere, and the pressure is 40Kpa. A bimetal injection molded golf head crude product is obtained. After going through post-processing steps such as polishing and sandblasting, the final product, a bimetal injection molded golf head, is obtained.
[0029] Example 2 In the bimetal assembly golf head of this embodiment, the manufacturing materials include tungsten alloy, stainless steel and adhesive, the tungsten alloy includes, by mass percentage, 80% tungsten, 15% iron and 5% nickel, and the stainless steel is selected as 304 stainless steel.
[0030] The weight ratio of the tungsten alloy input material to the stainless steel input material is 1:30.
[0031] The stainless steel powder and adhesive are mixed in a ratio of 2:0.6 parts by weight.
[0032] The manufacturing method of the golf head of the second embodiment is the same as that of the first embodiment.
[0033] Example 3 In the bimetal assembly golf head of the present embodiment, the manufacturing materials include a tungsten alloy, a stainless steel, and an adhesive, and the tungsten alloy includes, by mass percentage, 90% tungsten carbide and 10% iron, and the stainless steel is selected as 316L stainless steel; The weight ratio of the tungsten alloy input material to the stainless steel input material is 7:2.
[0034] The stainless steel powder and adhesive are mixed in a ratio of 1:0.4 parts by weight.
[0035] The manufacturing method of the golf head of the third embodiment is the same as that of the first embodiment.
[0036] Comparative Example 1 Comparing Comparative Example 1 and Example 2, Comparative Example 1 differs in that the selected tungsten alloy contains, by mass percentage, 89% tungsten, 3.5% copper, and 7.5% molybdenum.
[0037] Comparative Example 2 Comparing Comparative Example 2 with Example 2, Comparative Example 2 differs in that 410 stainless steel is selected as the stainless steel.
[0038] Comparative Example 3 Comparing Comparative Example 3 with Example 2, Comparative Example 3 is different in that the ratio of the mass parts of the tungsten alloy powder to the stainless steel powder is 1:21.
[0039] Comparative Example 4 Comparing Comparative Example 4 with Example 2, Comparative Example 4 differs in that the stainless steel powder and adhesive are mixed in a mass ratio of 1:1 in Comparative Example 4.
[0040] Comparative Example 5 Comparing Comparative Example 5 with Example 2, Comparative Example 5 differs in that the plasticization temperature in the injection molding process is 160° C., the heating temperature of the mold is 70° C., and the injection pressure is 90 MPa.
[0041] Comparative Example 6 Comparing Comparative Example 6 with Example 2, Comparative Example 6 differs in that the sintering temperature is 1280°C.
[0042] Comparative Example 7 Comparing Comparative Example 7 with Example 2, Comparative Example 7 differs in that the sintering temperature is 1480°C.
[0043] (Test Results) The final product of the bimetal injection molded golf head manufactured in the embodiment has a yield rate of 94.0-97.0%. In Comparative Example 1, other tungsten alloy metal powder is used to obtain hollow metal powder, and the process is not successful. The final product of the bimetal injection molded golf head manufactured in Comparative Examples 2-7 has a yield rate of 70%-85.0%. As can be seen from Comparative Examples 2-4, the two kinds of metal input materials manufactured by selecting the blending ratio of stainless steel metal components of the present invention, the specific gravity of tungsten alloy and stainless steel, and the blending ratio of adhesive and stainless steel are more suitable for the integration process of injection molding, degreasing and sintering. As can be seen from Comparative Example 5, only by selecting the injection molding conditions of the present invention can the bimetal injection molded golf head be successfully injection molded, and the degree of matching of the two metals is high and the hollow rate is low. As can be seen from Comparative Examples 6-7, the sintering temperature of the present invention is the optimal sintering condition.
[0044] The blending ratio of tungsten nickel iron selected in the embodiment reduces the density of the tungsten alloy, matches the composition of the stainless steel alloy, improves the adhesion with the stainless steel alloy, and prevents the existence of voids between the tungsten alloy balance weight and the stainless steel metal case. The grain size range of the produced tungsten alloy powder is 0.5-40 μm, D50 is 2.0-4.0 μm, the grain size distribution range of the stainless steel powder is 2.62-23.66 μm, D50 is 8.00 μm, and the bulk density range is 3.10-3.20 g / cm 3 The tap density range is 4.80 to 4.90 g / cm 3 Tungsten alloy powder has a finer particle size than stainless steel powder, the time required for subsequent debinding and sintering of the compact is longer (22 hours), and the final product produced is more dense.
[0045] According to the selected tungsten alloy component ratio, the selected stainless steel component ratio, the used adhesive, and the adhesive / stainless steel / tungsten alloy ratio, the shrinkage rate of the tungsten alloy and the stainless steel can be unified, and the selected specific gravity of the tungsten alloy and the stainless steel can meet the process requirements of step 3 and step 4.
[0046] The injection molding process conditions selected in step 3 are adapted to the injection process of stainless steel metal and increase the matching degree of the two dissimilar metals.
[0047] The three-stage degreasing method used in step 4 can thoroughly burn off the low-boiling point adhesive material, and has high degreasing efficiency.
[0048] According to the above results, by the compounding ratio of the tungsten alloy components of the present invention, the compounding ratio of the stainless steel metal components, the specific gravity of tungsten alloy and stainless steel, the compounding components of the adhesive used, and the compounding ratio of adhesive to stainless steel and tungsten alloy, two kinds of metals have the same shrinkage rate, degreasing sintering temperature and atmosphere requirements, and can use in-mold injection molding process and one-time sintering molding process to manufacture golf head with very high final product yield rate.
[0049] A model golf head manufactured in the embodiment is shown in FIG. 1 and FIG.
[0050] It should be noted that the above embodiments are merely for explaining the technical means of the present invention, and do not limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, it should be understood that those skilled in the art can make modifications or equivalent substitutions to the technical means of the present invention without departing from the spirit and scope of the technical means of the present invention. [Explanation of symbols]
[0051] 1. High density tungsten alloy 2 Stainless steel.
Claims
1. The manufacturing raw materials include a tungsten alloy, a stainless steel, and an adhesive, the mass content of tungsten in the tungsten alloy is 30-99%, and the mass content of other alloy components is 0-20%, and the stainless steel is selected from iron-based raw materials and is one selected from 304 stainless steel, 316L stainless steel, and 17-4PH stainless steel; Step 1: mixing tungsten alloy powder, stainless steel powder, and adhesive; Step 2: the tungsten alloy input material is first injection molded to obtain an in-mold injection molding built-in part, and then the stainless steel input material is put into the mold for in-mold injection molding to obtain an injection molded body in which the stainless steel input material is wrapped around the tungsten alloy input material; Step 3 of degreasing the compact in a three-stage process; Step 4: sintering the degreased green body at a temperature of 1380-1420°C in a nitrogen and hydrogen mixed gas atmosphere at a pressure of 40-45 Kpa to obtain a sintered product of the golf head. A method for manufacturing a golf head.
2. The other alloying components include nickel in an amount of 4 to 15 parts by weight and copper / iron in an amount of 2 to 10 parts by weight.
2. The method for manufacturing a golf head according to claim 1.
3. The weight ratio of the tungsten alloy powder to the stainless steel powder is 1:40 to 1:20; 2. The method for manufacturing a golf head according to claim 1.
4. The stainless steel powder and adhesive are mixed in a weight ratio of 1:0.4 to 3:0.
8.
2. The method for manufacturing a golf head according to claim 1.
5. The plasticization temperature of the injection molding process described in step 2 is 180°C to 220°C, the heating temperature of the mold is 90°C to 120°C, and the injection pressure is 110 to 130MPa; 2. The method for manufacturing a golf head according to claim 1.
6. The density of the tungsten alloy before sintering is 8 to 9 g / cm 3 After sintering, it is 14 to 15 g / cm 3 That is, 2. The method for manufacturing a golf head according to claim 1.
7. The three-stage degreasing method described in step 3 is to first pre-clean the molded body, put it into a degreasing furnace, and degrease it in a nitrogen gas atmosphere at a nitrogen gas flow rate of 0.8 L / min at a temperature of 100°C to 140°C for 13 to 22 hours, and then post-clean it to obtain a crude golf head that is a primary molded product.
2. The method for manufacturing a golf head according to claim 1.
8. The sintering process described in step 4 is divided into three steps, which are negative pressure debinding, vacuum sintering and partial pressure sintering.
2. The method for manufacturing a golf head according to claim 1.
9. The adhesive is composed of 90% polyoxymethylene, 3% ethylene copolymer, 4% ethylene propylene rubber, 1% glycerol monostearate, 1% 2,6-di-tert-butyl-4-methylphenol and 1% high density polyethylene HDPE; 2. The method for manufacturing a golf head according to claim 1.
Citation Information
Patent Citations
Golf club head and its manufacture
JP2000334073A
Head of golf club
JP2002275593A
Iron golf club
JP2003245386A
Method of manufacturing golf club head
JP2003250939A