Composition for polishing
The polishing composition with abrasive grains and collagen peptides addresses the challenge of selectively polishing polysilicon at a high rate by enhancing the polysilicon polishing rate and improving selectivity over silicon oxide and silicon nitride.
Patent Information
- Application Number
- JP2020143709
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-08-27
- Publication Date
- 2024-10-17
- Estimated Expiration
- 2040-08-27
AI Technical Summary
Existing polishing compositions struggle to selectively polish polysilicon at a high rate while maintaining a high ratio of polysilicon polishing rate to silicon oxide and silicon nitride polishing rates.
A polishing composition containing abrasive grains and collagen peptides with specific molecular weight and pH, which enhances the polishing rate of polysilicon and improves the selectivity by nucleophilic attack and protective film formation.
The composition achieves a high polishing rate for polysilicon with a significantly higher selectivity ratio to silicon oxide and silicon nitride, optimizing the polishing process.
Smart Images

Figure 0007569180000001 
Figure 0007569180000002 
Figure 0007569180000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a polishing composition. [Background technology]
[0002] In recent years, new microfabrication technologies have been developed to accompany the high integration and high performance of LSI (Large Scale Integration). Chemical mechanical polishing (CMP) is one of these technologies, and is frequently used in the LSI manufacturing process, especially in the multi-layer wiring formation process, for planarizing interlayer insulating films, forming metal plugs, and forming buried wiring (damascene wiring).
[0003] CMP has been applied to various processes in semiconductor manufacturing, and one example of its application is the gate formation process in transistor fabrication. When fabricating a transistor, Si-containing materials such as silicon, polycrystalline silicon (polysilicon), silicon oxide (silicon oxide), and silicon nitride (silicon nitride) are often polished, and depending on the transistor structure, it is necessary to control the polishing rate of each Si-containing material.
[0004] For example, Patent Document 1 discloses a polishing composition containing a water-soluble polymer and at least one type of abrasive grain selected from colloidal silica and fumed silica, containing no oxidizing agent, and having a pH of 1 to 8. With such a polishing composition, polysilicon can be polished at a high polishing rate. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2013-251561 A Summary of the Invention [Problem to be solved by the invention]
[0006] Among the demands for controlling the polishing rate of each Si-containing material, there is also a demand for polishing polysilicon at a high polishing rate while selectively polishing polysilicon over other Si-containing materials.
[0007] Therefore, an object of the present invention is to provide a polishing composition that can polish polysilicon at a high polishing rate and has a sufficiently high ratio of the polishing rate of polysilicon to the polishing rate of silicon oxide and silicon nitride (i.e., a high selectivity ratio). [Means for solving the problem]
[0008] The present inventors have conducted extensive research to solve the above problems, and have found that the above problems can be solved by a polishing composition that contains abrasive grains and a collagen peptide having a weight-average molecular weight of 2000 or more and 100000 or less, and has a pH of less than 4.0. Effect of the Invention
[0009] According to the present invention, there is provided a polishing composition which is capable of polishing polysilicon at a high polishing rate and has a sufficiently high ratio of the polishing rate of polysilicon to the polishing rate of silicon oxide and silicon nitride. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] An embodiment according to one aspect of the present invention will be described below, but the present invention is not limited to the following embodiment.
[0011] In this specification, the range "X to Y" means "X or more and Y or less." Furthermore, unless otherwise specified, the operations and measurements of physical properties are performed under conditions of room temperature (20 to 25°C) and relative humidity of 40 to 50% RH.
[0012] <Polishing composition> One aspect of the present invention is a polishing composition that contains abrasive grains and a collagen peptide having a weight-average molecular weight of 2000 to 100000, and has a pH of less than 4.0. With this composition, polysilicon can be polished at a high polishing rate, and the ratio of the polishing rate of polysilicon to the polishing rate of silicon oxide and silicon nitride can be made sufficiently high (i.e., the selectivity can be made high).
[0013] The reason why the polishing composition of this embodiment exhibits the above-mentioned effect is not necessarily clear, but it is believed that the electrons on the nitrogen atoms in the peptide bonds of the collagen peptide nucleophilically attack the polysilicon and hydrophilize the polysilicon surface, thereby improving the polishing rate of the polysilicon. On the other hand, since the collagen peptide functions as a protective film against silicon oxide and silicon nitride, it is believed that the ratio of the polishing rate of polysilicon to the polishing rate of silicon oxide and silicon nitride can be sufficiently increased (i.e., the selectivity can be increased). This mechanism is based on speculation, and the present invention is not limited to the above mechanism.
[0014] [Abrasive grain] The polishing composition of the present embodiment contains abrasive grains.
[0015] In one embodiment, specific examples of the abrasive grains according to this embodiment include particles made of metal oxides such as silica, alumina, zirconia, and titania. The abrasive grains may be used alone or in combination of two or more kinds. The abrasive grains may be commercially available products or synthetic products. Among these abrasive grains, silica is preferred, fumed silica and colloidal silica are more preferred, and colloidal silica is particularly preferred. Therefore, in a preferred embodiment, the abrasive grains according to this embodiment include colloidal silica.
[0016] The colloidal silica can be produced by a method such as a sodium silicate method or a sol-gel method, and any method for producing the colloidal silica can be suitably used as the abrasive grains according to the present embodiment. Among them, the colloidal silica produced by the sol-gel method, which can produce the colloidal silica with high purity, is preferred.
[0017] In a preferred embodiment, the abrasive grains according to the present invention have a negative zeta potential, from the viewpoint of further improving the polishing rate of polysilicon. Here, the "zeta potential" refers to the potential difference that occurs at the interface between a solid and a liquid in contact with each other when they undergo relative motion.
[0018] The zeta potential of the abrasive grains is, for example, from -80 mV to -5 mV, preferably from -70 mV to -10 mV, more preferably from -60 mV to -20 mV, and most preferably from -50 mV to -30 mV. When the abrasive grains have a zeta potential in this range, the effects of the present invention can be more effectively exhibited.
[0019] The abrasive grains according to this embodiment may have a surface modified to have a negative zeta potential at a pH of less than 4.0. Such abrasive grains can be obtained by, for example, mixing a metal such as aluminum, titanium, or zirconium or an oxide thereof with the abrasive grains and doping the surface of the abrasive grains, or by immobilizing an organic acid. Among them, abrasive grains having an organic acid immobilized on the surface are preferred. More preferred is silica having an organic acid chemically bonded to the surface. In such a form, a negative zeta potential can be obtained at a pH of less than 4.0. The organic acid is not particularly limited, but examples thereof include sulfonic acid, carboxylic acid, and phosphoric acid, and is preferably sulfonic acid. In addition, silica having an organic acid immobilized on its surface has an acidic group (e.g., a sulfo group, a carboxyl group, a phosphoric acid group, etc.) derived from the organic acid immobilized on the surface of the silica by covalent bonding (in some cases via a linker structure). Here, the linker structure means any structure interposed between the surface of the silica and the organic acid. Therefore, the silica with organic acid fixed on the surface may have the acidic group derived from organic acid fixed directly on the surface of silica by covalent bond, or may have the acidic group fixed on the surface of silica by covalent bond via linker structure.The method of introducing these organic acids to the silica surface is not particularly limited, and there is a method of introducing them to the silica surface in the form of mercapto group or alkyl group, etc., and then oxidizing them to sulfonic acid or carboxylic acid, as well as a method of introducing them to the silica surface in the form of a protective group bonded to the organic acid group, and then removing the protective group.
[0020] As a specific method for synthesizing silica having an organic acid fixed on its surface, if sulfonic acid, which is a type of organic acid, is fixed on the surface of silica, it can be performed by, for example, the method described in “Sulfonic acid-functionalized silica through quantitative oxidation of thiol groups”, Chem. Commun. 246-247 (2003). Specifically, a silane coupling agent having a thiol group, such as 3-mercaptopropyltrimethoxysilane, is coupled to silica, and then the thiol group is oxidized with hydrogen peroxide to obtain silica having a sulfonic acid fixed on its surface. The colloidal silica having a surface modified with sulfonic acid in the examples of the present invention is also produced in the same manner.
[0021] Carboxylic acid can be immobilized on the surface of silica by, for example, the method described in “Novel Silane Coupling Agents Containing a Photolabile 2-Nitrobenzyl Ester for Introduction of a Carboxy Group on the Surface of Silica Gel”, Chemistry Letters, 3, 228-229 (2000). Specifically, a silane coupling agent containing a photoreactive 2-nitrobenzyl ester is coupled to silica, followed by light irradiation to obtain silica with a carboxylic acid immobilized on the surface.
[0022] The lower limit of the average primary particle size of the abrasive grains according to this embodiment is preferably 1 nm or more, more preferably 5 nm or more, even more preferably 7 nm or more, and most preferably 10 nm or more. The upper limit of the average primary particle size of the abrasive grains according to this embodiment is preferably 100 nm or less, more preferably 50 nm or less, even more preferably 30 nm or less, and most preferably 20 nm or less. Within this range, polysilicon can be polished at a high polishing rate. The average primary particle size of the abrasive grains is calculated, for example, based on the specific surface area of the abrasive grains measured by the BET method.
[0023] The lower limit of the average secondary particle size of the abrasive grains according to this embodiment is preferably 2 nm or more, more preferably 10 nm or more, and even more preferably 15 nm or more. The upper limit of the average secondary particle size of the abrasive grains according to this embodiment is preferably 200 nm or less, more preferably 150 nm or less, even more preferably 100 nm or less, and most preferably 50 nm or less. Within such a range, polysilicon can be polished at a high polishing rate. The average secondary particle size of the abrasive grains can be measured, for example, by a dynamic light scattering method, such as a laser diffraction scattering method.
[0024] The shape of the abrasive grain according to the present embodiment is not particularly limited, and may be spherical or non-spherical. Specific examples of non-spherical shapes include polygonal prisms such as triangular prisms and square prisms, cylinders, bales of cylinders in which the center is more bulging than the ends, donuts with a disk penetrating the center, plates, cocoon shapes (shapes with a constriction in the center), associative spheres (shapes in which multiple particles are integrated), confetti shapes (shapes with multiple protrusions on the surface), and rugby ball shapes.
[0025] The content (concentration) of the abrasive grains according to this embodiment is, for example, 0.1% by mass or more and 25% by mass or less, preferably 0.5% by mass or more and 15% by mass or less, more preferably 1% by mass or more and 10% by mass or less, and most preferably 2% by mass or more and 5% by mass or less, based on the polishing composition. In such a range, the polishing speed for polysilicon can be further improved. When the polishing composition contains two or more kinds of abrasive grains, the content of the abrasive grains means the total amount of these.
[0026] [Collagen peptide] The polishing composition of this embodiment contains a collagen peptide having a weight average molecular weight of 2,000 or more and 100,000 or less.
[0027] Collagen peptide is a collagen that has been depolymerized. The method of depolymerizing collagen is not particularly limited, and may be, for example, a method of treating collagen with alkali. Collagen peptide can be produced from collagen derived from, for example, cow or pig skin, fish (flounder, salmon, sea bass, etc.) skin, scales, etc.
[0028] Collagen peptides contain a tripeptide structure represented by the structural formula [Gly-Xaa-Yaa]. Here, Gly represents glycine. Xaa and Yaa represent amino acids. Examples of amino acids that are Xaa and Yaa include proline (Pro), hydroxyproline (Hyp), alanine (Ala), arginine (Arg), aspartic acid (Asp), glutamine (Gln), glutamic acid (Glu), leucine (Leu), methionine (Met), phenylalanine (Phe), and serine (Ser).
[0029] From the viewpoint of further improving the polishing rate of polysilicon, the weight average molecular weight of the collagen peptide is preferably 2,000 or more and 20,000 or less, more preferably 2,000 or more and 10,000 or less, and even more preferably 2,000 or more and 5,000 or less.
[0030] In this specification, the weight-average molecular weight of collagen peptide is a value calculated in terms of polystyrene measured by gel permeation chromatography (GPC). When a commercially available product is used, the value in the product information provided by the supplier is used.
[0031] The collagen peptide content (concentration) is, for example, from 0.01% by mass to 20% by mass, preferably from 0.1% by mass to 10% by mass, more preferably from 0.2% by mass to 5% by mass, even more preferably from 0.2% by mass to 1% by mass, and most preferably from 0.2% by mass to 0.5% by mass.
[0032] [Dispersion medium] The polishing composition of this embodiment may contain a dispersion medium. As the dispersion medium, water is preferable. From the viewpoint of preventing the influence of impurities on other components of the polishing composition, it is preferable to use water with as high purity as possible. As such water, for example, water with a total content of transition metal ions of 100 ppb or less is preferable. Here, the purity of water can be increased by, for example, removing impurity ions using ion exchange resin, removing foreign matter with a filter, distillation, and other operations. Specifically, as water, for example, deionized water (ion-exchanged water), pure water, ultrapure water, distilled water, and the like are preferably used. Usually, 90% by volume or more of the dispersion medium contained in the polishing composition is preferably water, more preferably 95% by volume or more of water, even more preferably 99% by volume or more of water, and particularly preferably 100% by volume of water.
[0033] The dispersion medium may be a mixed solvent of water and an organic solvent for dispersing or dissolving each component. In this case, examples of the organic solvent used include acetone, acetonitrile, ethanol, methanol, isopropanol, glycerin, ethylene glycol, propylene glycol, etc., which are organic solvents miscible with water. These organic solvents may be used without being mixed with water, and then each component may be dispersed or dissolved, and then mixed with water. These organic solvents may be used alone or in combination of two or more kinds.
[0034] [pH adjuster] The polishing composition of this embodiment may contain a pH adjuster to adjust the pH to less than 4.0.
[0035] The pH adjuster is not particularly limited as long as it is a compound having a pH adjusting function, and a known compound can be used. The pH adjuster is not particularly limited as long as it is a compound having a pH adjusting function, and examples thereof include acids and alkalis.
[0036] As the acid, either an inorganic acid or an organic acid may be used. As the inorganic acid, there is no particular limitation, but examples thereof include sulfuric acid, nitric acid, boric acid, carbonic acid, hypophosphorous acid, phosphorous acid, and phosphoric acid. As the organic acid, there is no particular limitation, but examples thereof include formic acid, acetic acid, propionic acid, butyric acid, valeric acid, 2-methylbutyric acid, n-hexanoic acid, 3,3-dimethylbutyric acid, 2-ethylbutyric acid, 4-methylpentanoic acid, n-heptanoic acid, 2-methylhexanoic acid, n-octanoic acid, 2-ethylhexanoic acid, benzoic acid, glycolic acid, salicylic acid, glyceric acid, oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, maleic acid, phthalic acid, malic acid, tartaric acid, citric acid, and lactic acid, and other carboxylic acids, as well as methanesulfonic acid, ethanesulfonic acid, and isethionic acid. Among these, inorganic acids are preferred, and maleic acid is more preferred.
[0037] The alkali is not particularly limited, but examples thereof include alkali metal hydroxides such as potassium hydroxide, ammonia, quaternary ammonium salts such as tetramethylammonium and tetraethylammonium, and amines such as ethylenediamine and piperazine.
[0038] The pH adjusters may be used alone or in combination of two or more kinds.
[0039] The content of the pH adjuster is not particularly limited, and the pH value is set to a value within the preferred range described below. It is preferable that the amount is an amount that can be obtained by the above-mentioned method.
[0040] [Other ingredients] The polishing composition of the present invention may further contain known additives such as chelating agents, thickeners, oxidizing agents, dispersants, surface protective agents, wetting agents, surfactants, rust inhibitors, preservatives, and fungicides, within the range that does not impair the effects of the present invention. The content of the additives may be appropriately set depending on the purpose of their addition.
[0041] [pH of polishing composition] The pH of the polishing composition of this embodiment is not particularly limited as long as it is less than 4.0, and can be appropriately adjusted according to the combination of abrasive grain and collagen peptide used.The lower limit of pH is, for example, 1.0 or more, preferably 1.5 or more, more preferably 2.0 or more.The upper limit of pH is preferably 3.5 or less, more preferably 3.0 or less.
[0042] The pH value can be confirmed using a pH meter (manufactured by Horiba Ltd., model number: LAQUA (registered trademark)).
[0043] [Electrical Conductivity of Polishing Composition] The upper limit of the electrical conductivity of the polishing composition of this embodiment is preferably 4.0 mS / cm or less, more preferably 3.0 mS / cm or less, from the viewpoint of suppressing the aggregation of abrasive grains. The lower limit of the electrical conductivity of the polishing composition of this embodiment is preferably 0.1 mS / cm or more, more preferably 0.5 mS / cm or more, from the viewpoint of solubility. The electrical conductivity can be confirmed by a tabletop electrical conductivity meter (manufactured by Horiba Ltd., model number: DS-71).
[0044] The electrical conductivity regulator is not particularly limited, but a salt compound can be used. Examples of salt compounds include acid salts and base salts, such as potassium nitrate, ammonium nitrate, potassium hydrogen carbonate, ammonium carbonate, ammonium hydrogen carbonate, diammonium hydrogen phosphate, ammonium dihydrogen phosphate, ammonium sulfate, potassium chloride, sodium chloride, potassium bromide, potassium iodide, ammonium citrate, potassium hydroxide, sodium hydroxide, tetramethylammonium hydroxide, and tetraethylammonium hydroxide, and among these, ammonium sulfate is preferred. The salt compounds may be used alone or in combination of two or more.
[0045] The content (concentration) of the electrical conductivity regulator can be appropriately adjusted according to the desired electrical conductivity.
[0046] [Polished object] The object to be polished using the polishing composition of this embodiment is not particularly limited, and examples thereof include silicon oxide (SiO2), silicon nitride (SiN), silicon carbonitride (SiCN), polycrystalline silicon (polysilicon), non-crystalline silicon (amorphous silicon), metal, SiGe, and the like.
[0047] The object to be polished according to the present embodiment preferably contains polycrystalline silicon (polysilicon), more preferably contains polycrystalline silicon (polysilicon), silicon oxide (SiO2) and silicon nitride (SiN). Therefore, the polishing composition according to the present embodiment is preferably used for polishing an object to be polished that contains polysilicon, more preferably used for polishing an object to be polished that contains polysilicon, silicon oxide and silicon nitride.
[0048] Examples of films containing silicon oxide include TEOS (Tetraethyl Orthosilicate) type silicon oxide films (hereinafter simply referred to as "TEOS films") produced using tetraethyl orthosilicate as a precursor, HDP (High Density Plasma) films, USG (Undoped Silicate Glass) films, PSG (Phosphorus Silicate Glass) films, BPSG (Boron-Phospho Silicate Glass) films, and RTO (Rapid Thermal Oxidation) films.
[0049] Examples of metal-containing films include tungsten (W) films, titanium nitride (TiN) films, and Ru film, platinum (Pt) film, gold (Au) film, hafnium (Hf) film, cobalt (Co) film, nickel (Ni) film, copper (Cu) film, aluminum (Al) film, tantalum ( Ta) film.
[0050] <Method of manufacturing the polishing composition> The method for producing the polishing composition of this embodiment is not particularly limited, and can be obtained, for example, by stirring and mixing abrasive grains and collagen peptide, and other components as necessary, in a dispersion medium.A pH adjuster can be appropriately used to make the pH of the polishing composition less than 4.0.Therefore, the present invention provides a method for producing a polishing composition, which comprises mixing abrasive grains and a peptide bond-containing compound.
[0051] The temperature at which the components are mixed is not particularly limited, but is preferably 10° C. to 40° C., and may be heated to increase the dissolution rate. The mixing time is also not particularly limited as long as the components can be mixed uniformly.
[0052] <Polishing method and semiconductor substrate manufacturing method> One aspect of the present invention is a polishing method including a step of polishing an object to be polished with the polishing composition.
[0053] Another aspect of the present invention is a method for producing a semiconductor substrate, comprising the polishing method described above.
[0054] As a polishing device, a general polishing device can be used which is equipped with a holder for holding a substrate or the like having an object to be polished, a motor whose rotation speed can be changed, and a polishing platen onto which a polishing pad (polishing cloth) can be attached.
[0055] The polishing pad may be made of any material, including general nonwoven fabric, polyurethane, porous fluororesin, etc. It is preferable that the polishing pad has grooves formed thereon to allow the polishing liquid to accumulate.
[0056] Regarding the polishing conditions, for example, the rotation speed of the polishing platen was 10 rpm (0.17 s -1 ) or more 500rpm (8.3s -1) is preferred. The pressure (polishing pressure) applied to the substrate having the object to be polished is preferably 0.5 psi (3.4 kPa) or more and 10 psi (68.9 kPa) or less. There is no particular limitation on the method of supplying the polishing composition to the polishing pad, and for example, a method of continuously supplying the composition using a pump or the like is adopted. There is no limitation on the amount of supply, but it is preferred that the surface of the polishing pad is always covered with the polishing composition according to one embodiment of the present invention.
[0057] After polishing, the substrate is washed with running water, and water droplets adhering to the substrate are removed by a spin dryer or the like, followed by drying to obtain a substrate having a metal-containing layer.
[0058] The polishing composition according to one embodiment of the present invention may be a one-liquid type or a multi-liquid type such as a two-liquid type. The polishing composition according to one embodiment of the present invention may be prepared by diluting the stock solution of the polishing composition, for example, 10 times or more, with a diluent such as water. EXAMPLES
[0059] The present invention will be described in more detail using the following examples and comparative examples. However, the technical scope of the present invention is not limited to the following examples. Unless otherwise specified, "%" and "parts" mean "% by mass" and "parts by mass", respectively. In the following examples, unless otherwise specified, the operations were performed under the conditions of room temperature (20 to 25°C) / relative humidity 40 to 50% RH.
[0060] [Preparation of polishing composition] Example 1 As abrasive grains, sulfonic acid-modified colloidal silica (average primary particle size 14 nm, average secondary particle size 33 nm) was added to ion-exchanged water at a final concentration of 3 mass%, and collagen peptide (weight-average molecular weight 85000) was added to 0.3 mass%. The mixture was then stirred and mixed at room temperature (25°C) for 30 minutes, and the pH was adjusted to 2.5 using maleic acid as a pH adjuster to prepare a polishing composition.
[0061] Example 2 A polishing composition was prepared in the same manner as in Example 1, except that the collagen peptide (weight average molecular weight 85,000) was changed to a collagen peptide (weight average molecular weight 15,000).
[0062] Example 3 A polishing composition was prepared in the same manner as in Example 1, except that the collagen peptide (weight average molecular weight 85,000) was changed to a collagen peptide (weight average molecular weight 2,000).
[0063] Example 4 A polishing composition was prepared in the same manner as in Example 2, except that the pH was adjusted to 1.5.
[0064] Example 5 A polishing composition was prepared in the same manner as in Example 2, except that the pH was adjusted to 3.5.
[0065] Comparative Example 1 As an abrasive, sulfonic acid-modified colloidal silica (average primary particle size 14 nm, average secondary particle size 33 nm) was added to ion-exchanged water to a final concentration of 3 mass %. After that, the mixture was stirred and mixed at room temperature (25°C) for 30 minutes, and the pH was adjusted to 2.5 using maleic acid as a pH adjuster to prepare a polishing composition.
[0066] Comparative Example 2 A polishing composition was prepared in the same manner as in Comparative Example 1, except that the pH was adjusted to 4.5.
[0067] Comparative Example 3 A polishing composition was prepared in the same manner as in Example 1, except that the collagen peptide (weight average molecular weight: 85,000) was changed to a collagen peptide (weight average molecular weight: 300,000).
[0068] Comparative Example 4 A polishing composition was prepared in the same manner as in Example 1, except that the collagen peptide (weight average molecular weight 85,000) was changed to glycine.
[0069] Comparative Example 5 A polishing composition was prepared in the same manner as in Example 1, except that the pH was adjusted to 4.5.
[0070] The composition of the polishing composition prepared above is shown in Table 1.
[0071] [Zeta potential measurement] The polishing compositions of Examples 1 to 5 and Comparative Examples 1 to 5 prepared above were subjected to measurement by the laser Doppler method (electrophoretic light scattering measurement method) using an ELS-Z2 manufactured by Otsuka Electronics Co., Ltd. and a flow cell at a measurement temperature of 25°C. The obtained data was analyzed by the Smoluchowski formula to calculate the zeta potential of the sulfonic acid-modified colloidal silica contained in the polishing composition. The results are shown in Table 2.
[0072] [Measurement of pH of polishing composition] The pH of the polishing composition (liquid temperature: 25° C.) was confirmed with a pH meter (manufactured by Horiba, Ltd., model number: LAQUA).
[0073] [Measurement of Electrical Conductivity of Polishing Composition] The electrical conductivity of the polishing composition after preparation was measured using a tabletop electrical conductivity meter (Model No. DS-71, manufactured by Horiba, Ltd.). The results are shown in Table 2.
[0074] [Evaluation of polishing speed] The object to be polished is 200mm wafer (Poly-Si) 200mm wafer (SiN (silicon nitride) film), 200mm wafer (TEOS (silicon oxide film)), Each wafer was polished using the polishing composition obtained above under the following polishing conditions, and the polishing rate was measured. Also, the selectivity was calculated.
[0075] Polishing conditions Polishing machine: CMP single-sided polishing machine for 200mm wafers Polishing pad: Polyurethane pad (IC1010: manufactured by Rohm and Haas) Pressure: 4.0 psi (approx. 27.6 kPa) Platen rotation speed: 90 rpm Head (carrier) rotation speed: 87 rpm Flow rate of polishing composition: 200ml / min Polishing time: 1 minute.
[0076] polishing speed The polishing speed (polishing rate) was calculated by the following formula.
[0077]
number
[0078] The film thickness was measured using an optical interference type film thickness measuring device (KLA-Tencor Corporation, type The results were calculated using the ASET (number: ASET) and the difference was divided by the polishing time. As shown in Table 2.
[0079] [Table 1]
[0080] [Table 2]
[0081] As shown in Table 2, it is understood that the polishing compositions of the Examples can polish polysilicon at a higher polishing rate than the polishing compositions of the Comparative Examples. Furthermore, it is understood that the polishing compositions of the Examples have a higher ratio of the polishing rate of polysilicon to TEOS or SiN than the polishing compositions of the Comparative Examples, and can polish polysilicon more selectively.
Claims
1. Abrasive grains and A collagen peptide having a weight average molecular weight of 2,000 or more and 100,000 or less, The pH is less than 4.0, A polishing composition for use in polishing objects containing polysilicon, silicon oxide, and silicon nitride.
2. The polishing composition according to claim 1 , wherein the abrasive grains have a negative zeta potential.
3. The polishing composition according to claim 1 or 2, wherein the collagen peptide has a weight average molecular weight of 20,000 or less.
4. 4. The polishing composition according to claim 1, wherein the abrasive grains contain colloidal silica.
5. 5. A polishing method comprising a step of polishing an object containing polysilicon, silicon oxide and silicon nitride with the polishing composition according to claim 1.
6. A method for producing a semiconductor substrate containing polysilicon, silicon oxide, and silicon nitride, comprising the polishing method according to claim 5.
Citation Information
Patent Citations
Synthetic quartz glass substrate abrasive and method of manufacturing synthetic quartz glass substrate using the same
JP2012024889A
Polishing composition and polishing method using the same
JP2013251561A
Polishing composition
JP2016188322A
Polishing composition, polishing method using the same and manufacturing method therefor
JP2017057398A
Polishing compositions containing charged abrasive
JP2019071413A