Electromagnetic wave shielding laminate, method for manufacturing electromagnetic wave shielding laminate, shielded printed wiring board, method for manufacturing shielded printed wiring board, semiconductor package, and electronic device

The electromagnetic shielding laminate with a compound-bonded shield, adhesive, and insulating layers addresses delamination and maintains shielding performance by enhancing interlayer bonding and bending resistance.

JP7569254B2Active Publication Date: 2024-10-17HOKOSHA TECH CORP +1
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2021057888
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-03-30
Publication Date
2024-10-17
Estimated Expiration
2041-03-30

AI Technical Summary

Technical Problem

Conventional electromagnetic shielding laminates face issues with delamination and reduced shielding performance due to the accumulation of volatile components during heating processes, particularly in flexible printed wiring boards, and the low strength of shielding layers leads to deterioration when bent.

Method used

An electromagnetic shielding laminate is designed with a shield layer bonded to an adhesive layer and an insulating layer via a compound containing a benzene ring, an alkoxysilyl group, and one or more azide, azidosulfonyl, or diazomethyl groups, enhancing interlayer bonding and resistance to bending.

Benefits of technology

The laminate exhibits improved interlayer adhesion, reduced delamination, and maintained shielding performance even under bending stress, ensuring high durability and effective electromagnetic shielding.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007569254000018
    Figure 0007569254000018
  • Figure 0007569254000019
    Figure 0007569254000019
  • Figure 0007569254000020
    Figure 0007569254000020
Patent Text Reader

Abstract

To provide an electromagnetic shielding laminate or the like that is less susceptible to delamination when a shield printed wiring board is manufactured.SOLUTION: An electromagnetic shielding laminate according to an embodiment of the present invention includes a shield layer, and at least one of an adhesive layer and an insulating layer bonded to the shield layer via a compound α, and the compound α is one of a compound α1 having, in one molecule, a benzene ring, an alkoxysilyl group, and one or more groups selected from the group consisting of an azide group, an azidosulfonyl group, and a diazomethyl group, and a compound α2 obtained by hydrolytic condensation of a hydrolyzable silane compound containing the compound α1.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an electromagnetic wave shielding laminate, a method for manufacturing an electromagnetic wave shielding laminate, a shielded printed wiring board, a method for manufacturing a shielded printed wiring board, a semiconductor package, and an electronic device. [Background technology]

[0002] 2. Description of the Related Art Conventionally, an electromagnetic wave shielding laminate has been attached to a printed wiring board such as a flexible printed wiring board (FPC) to shield against external electromagnetic waves.

[0003] An electromagnetic shielding laminate typically has a configuration in which a conductive adhesive layer, a shielding layer made of a metal thin film or the like, and an insulating layer are laminated in this order. This electromagnetic shielding laminate is superimposed on a printed wiring board and then hot-pressed, whereby the electromagnetic shielding laminate is adhered to the printed wiring board by the conductive adhesive layer to produce a shielded printed wiring board. After this adhesion, components are typically mounted on the printed wiring board by solder reflow. Furthermore, printed wiring boards typically have a configuration in which a printed circuit on a base film is covered with an insulating film.

[0004] When a shielded printed wiring board is manufactured, if the shielded printed wiring board is heated by a hot press, solder reflow, or the like, gas is generated from the conductive adhesive layer of the electromagnetic shield laminate, the insulating film of the printed wiring board, and the like. In addition, if the base film of the printed wiring board is formed of a highly hygroscopic resin such as polyimide, water vapor may be generated from the base film by heating. These volatile components generated from the conductive adhesive layer, the insulating film, the base film, and the like cannot pass smoothly through the shield layer, and therefore accumulate between the shield layer and the conductive adhesive layer. Therefore, if rapid heating is performed in a solder reflow process, etc., the volatile components accumulated between the shield layer and the conductive adhesive layer may destroy the interlayer adhesion between the shield layer and the conductive adhesive layer, and the shielding performance may be reduced.

[0005] In order to solve such problems, Patent Document 1 describes an electromagnetic wave shielding laminate in which a shielding layer (metal thin film) is provided with multiple openings to improve breathability. When multiple openings are provided in the shielding layer, volatile components can pass through the shielding layer through the openings. It is therefore believed that this can prevent volatile components from accumulating between the shielding layer and the conductive adhesive layer, and can prevent a decrease in shielding performance due to the breakdown of interlayer adhesion. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] International Publication No. 2014 / 192494 Summary of the Invention [Problem to be solved by the invention]

[0007] In the electromagnetic shielding laminate described in Patent Document 1, an opening is formed in the shielding layer, so the strength of the shielding layer is weak. Therefore, when the electromagnetic shielding laminate described in Patent Document 1 is used in a flexible printed wiring board, the following problems arise. Flexible printed wiring boards are repeatedly folded when used. Therefore, the electromagnetic shielding laminate used in such a flexible printed wiring board and the shielding layer constituting this electromagnetic shielding laminate are also repeatedly folded. As described above, the shielding layer of the electromagnetic shielding laminate described in Patent Document 1 has a weak strength, so that when repeatedly folded, the shielding layer may be broken, leading to a decrease in shielding performance. In addition, a shielding layer for shielding electromagnetic waves may also be provided in a semiconductor package, etc., and the adhesion between the shielding layer and other layers such as an insulating layer is important.

[0008] The present invention has been made based on the above-mentioned circumstances, and an object of the present invention is to provide an electromagnetic shielding laminate that is less likely to cause interlayer delamination when, for example, producing a shielded printed wiring board, a method for producing such an electromagnetic shielding laminate, a shielded printed wiring board using such an electromagnetic shielding laminate, a method for producing a shielded printed wiring board, a semiconductor package, and an electronic device. [Means for solving the problem]

[0009] One embodiment of the present invention is an electromagnetic wave shielding laminate comprising a shielding layer and at least one of an adhesive layer and an insulating layer bonded to the shielding layer via a compound α, wherein the compound α is at least one of compound α1 having, in one molecule, a benzene ring, an alkoxysilyl group, and one or more groups selected from the group consisting of an azide group, an azide sulfonyl group, and a diazomethyl group, and compound α2 obtained by hydrolysis and condensation of a hydrolyzable silane compound containing the compound α1.

[0010] Another embodiment of the present invention is a method for producing an electromagnetic wave shielding laminate, comprising a step of bonding a shielding layer to at least one of an adhesive layer and an insulating layer via a compound α, wherein the compound α is at least one of compound α1 having, in one molecule, a benzene ring, an alkoxysilyl group, and one or more groups selected from the group consisting of an azide group, an azide sulfonyl group, and a diazomethyl group, and compound α2 obtained by hydrolysis and condensation of a hydrolyzable silane compound containing the compound α1.

[0011] Another aspect of the present invention is a shielded printed wiring board comprising a printed wiring board and the above-described electromagnetic shield laminate adhered to the printed wiring board.

[0012] Another aspect of the present invention is a method for producing a shielded printed wiring board, comprising a step of adhering the above-mentioned electromagnetic shielding laminate, or an electromagnetic shielding laminate obtained by the above-mentioned method for producing an electromagnetic shielding laminate, to a printed wiring board.

[0013] Another aspect of the present invention is a semiconductor package including the electromagnetic wave shielding laminate described above.

[0014] Another aspect of the present invention is an electronic device including the above-described shielded printed wiring board or the above-described semiconductor package. Effect of the Invention

[0015] According to one embodiment of the present invention, it is possible to provide an electromagnetic wave shielding laminate that is less likely to undergo interlayer delamination during, for example, the production of a shielded printed wiring board, a method for producing such an electromagnetic wave shielding laminate, a shielded printed wiring board using such an electromagnetic wave shielding laminate, a method for producing a shielded printed wiring board, and an electronic device. [Brief description of the drawings]

[0016] [Figure 1] FIG. 1 is a schematic cross-sectional view showing an electromagnetic wave shielding laminate according to one embodiment of the present invention. [Diagram 2] FIG. 2 is a schematic cross-sectional view showing an electromagnetic wave shielding laminate according to an embodiment different from that shown in FIG. [Diagram 3] FIG. 3 is a flow diagram of the electroless plating process in the reference example. [Figure 4] FIG. 4 is a flow diagram of thermocompression bonding in a reference example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] <Electromagnetic wave shielding laminate> The electromagnetic shielding laminate according to one embodiment of the present invention includes a shielding layer and at least one of an adhesive layer and an insulating layer bonded to the shielding layer via a predetermined compound α. Examples of the electromagnetic shielding laminate according to the present invention include a form including a shielding layer and an adhesive layer, a form including a shielding layer and an insulating layer, and a form including an adhesive layer, a shielding layer and an insulating layer in this order. When the electromagnetic shielding laminate according to the present invention includes an adhesive layer, a shielding layer and an insulating layer, at least one of the adhesive layer and the shielding layer and the insulating layer may be bonded via a compound α. In the electromagnetic shielding laminate according to one embodiment of the present invention, at least one of the adhesive layer and the shielding layer and the shielding layer and the insulating layer is bonded via a compound α, so that peeling between these layers is unlikely to occur and the bending resistance is sufficiently high. Hereinafter, a specific description will be given mainly of the form of the electromagnetic shielding laminate including an adhesive layer, a shielding layer and an insulating layer in this order, and each layer is bonded via a compound α.

[0018] The electromagnetic shield laminate 10 according to one embodiment of the present invention shown in FIG. 1 is a laminate including an adhesive layer 11, a shield layer 12, and an insulating layer 13 in this order. The adhesive layer 11 and the shield layer 12 are bonded together via a compound α, and a first compound α layer 14a is present between these layers. The shield layer 12 and the insulating layer 13 are also bonded together via a compound α, and a second compound α layer 14b is present between these layers. The first compound α layer 14a and the second compound α layer 14b may be present as a continuous layer or as an intermittent layer. The first compound α layer 14a and the second compound α layer 14b are usually very thin layers, so they do not need to be confirmed as layers using an optical microscope or the like, and it is sufficient to confirm that the compound α exists between the adhesive layer 11 and the shield layer 12, and between the shield layer 12 and the insulating layer 13.

[0019] In the electromagnetic shielding laminate 10, the adhesive layer 11 and the shielding layer 12, and the shielding layer 12 and the insulating layer 13 are chemically bonded at the interface by the compound α. Therefore, when the electromagnetic shielding laminate 10 is used to manufacture a shielded printed wiring board, delamination is unlikely to occur, and the bending resistance is also sufficiently high. Specifically, for example, when performing hot pressing, solder reflow, etc. to manufacture a shielded printed wiring board using the electromagnetic shielding laminate 10, even if a volatile component is generated between the adhesive layer 11 and the shielding layer 12 and penetrates the interface, delamination at the interface is unlikely to occur. As a result, it is possible to suppress the destruction of the interlayer adhesion, and therefore the electromagnetic shielding performance is also improved. Furthermore, even when the electromagnetic shielding laminate 10 is used in a flexible printed wiring board, etc., the bending resistance is sufficiently high, so that disconnection and the like are unlikely to occur.

[0020] In another embodiment, either the adhesive layer 11 and the shield layer 12 or the shield layer 12 and the insulating layer 13 may be bonded by other means. At least one of the adhesive layer 11 and the shield layer 12 and the shield layer 12 and the insulating layer 13 is bonded via the compound α, so that delamination is unlikely to occur during the manufacture of a shielded printed wiring board, and bending resistance is sufficiently high. However, since volatile components tend to accumulate, it is preferable that at least the adhesive layer 11 and the shield layer 12 are bonded via the compound α, and from the viewpoint of further improving bending resistance, it is more preferable that both the adhesive layer 11 and the shield layer 12 and the shield layer 12 and the insulating layer 13 are bonded via the compound α.

[0021] (adhesive layer) The adhesive layer 11 is usually the innermost layer of the electromagnetic shielding laminate 10, and is a layer for attaching the electromagnetic shielding laminate 10 to a printed wiring board or the like.

[0022] The adhesive layer 11 usually contains a resin that functions as an adhesive (adhesive resin). As this resin, a conventionally known resin used as an adhesive can be used. Examples of the resin include thermoplastic resins such as polyamide resin, polyester resin, acrylic resin, polyolefin resin (polyethylene resin, polypropylene resin, etc.), polyimide resin, polystyrene resin, polyvinyl acetate resin, etc., thermosetting resins such as epoxy resin, polyurethane resin, polyurethane urea resin, melamine resin, alkyd resin, phenol resin, etc., and active energy ray curable resins such as resins having a plurality of (meth)acryloyloxy groups. These resins may be homopolymers, copolymers, or variously modified resins. One or more types of resins can be used. The adhesive layer 11 preferably contains at least one resin selected from the group consisting of polyamide resin, polyester resin, acrylic resin, epoxy resin, polyurethane resin, and polyurethane urea resin, from the viewpoint of exhibiting good adhesiveness. In addition, the resin contained in the adhesive layer 11 is preferably a thermosetting resin, and more preferably an epoxy resin. The resin contained in the adhesive layer 11 exists in an adhesive state (for example, in an uncured state).

[0023] The lower limit of the resin content in the adhesive layer 11 is preferably 50% by mass, more preferably 60% by mass, and even more preferably 70% by mass. By making the resin content in the adhesive layer equal to or greater than the above lower limit, it is possible to increase the adhesiveness of the adhesive layer 11. On the other hand, the upper limit of the resin content in the adhesive layer 11 is preferably 99% by mass, more preferably 95% by mass, and even more preferably 90% by mass.

[0024] The adhesive layer 11 is preferably conductive. The conductive adhesive layer 11 also functions as a layer that shields electromagnetic waves. Therefore, the electromagnetic shielding laminate 10 including such an adhesive layer 11 can be more suitably used as an electromagnetic shielding laminate for a printed wiring board or the like. For this reason, the adhesive layer 11 preferably contains conductive particles.

[0025] The shape of the conductive particles is not particularly limited, but may be spherical, flat, flaky, dendritic, rod-like, fibrous, or the like.

[0026] Examples of the conductive particles include metal particles and carbon particles, with metal particles being preferred. Examples of the metal particles (metal powders) include silver powder, copper powder, nickel powder, solder powder, aluminum powder, silver-coated copper powder obtained by silver plating copper powder, and fine particles obtained by coating polymer fine particles, glass beads, etc. with metal. Among these, copper powder and silver-coated copper powder are preferred from the viewpoint of economy and the like.

[0027] The average particle size of the conductive particles is preferably 0.5 μm or more and 15 μm or less. When the average particle size of the conductive particles is in the above range, the adhesive layer 11 has good adhesion, shielding performance, etc. Furthermore, when the average particle size of the conductive particles is equal to or less than the above upper limit, it is possible to reduce the thickness of the adhesive layer 11. In this specification, the "average particle size" refers to the volume average value measured by dispersing specific target particles in a dispersion medium and measuring the volume average value by dynamic light scattering.

[0028] The lower limit of the conductive particle content in the adhesive layer 11 is preferably 5 mass%, more preferably 10 mass%, and even more preferably 15 mass%. By making the conductive particle content equal to or greater than the above lower limit, it is possible to improve the shielding performance and the like of the adhesive layer 11. On the other hand, the upper limit of the conductive particle content in the adhesive layer is preferably 80 mass%, more preferably 60 mass%, and even more preferably 40 mass%. By making the conductive particle content equal to or less than the above upper limit, it is possible to ensure sufficient adhesiveness of the adhesive layer 11.

[0029] The adhesive layer 11 preferably has anisotropic conductivity. When the adhesive layer 11 has anisotropic conductivity, the transmission characteristics of a high-frequency signal transmitted through a signal circuit of a printed wiring board are improved, for example, compared to when the adhesive layer 11 has isotropic conductivity.

[0030] The adhesive layer 11 may contain, as necessary, a curing accelerator, a tackifier, an antioxidant, a pigment, a dye, a plasticizer, an ultraviolet absorber, an antifoaming agent, a leveling agent, a filler, a flame retardant, a viscosity adjuster, and the like.

[0031] The average thickness of the adhesive layer 11 is not particularly limited and can be set appropriately as necessary, but the lower limit is preferably 0.2 μm, more preferably 1 μm, and even more preferably 5 μm. By setting the average thickness of the adhesive layer 11 to be equal to or greater than the above lower limit, sufficient adhesiveness and sufficient shielding performance when conductive particles are contained can be exhibited. On the other hand, the upper limit of the average thickness of the adhesive layer 11 is preferably 40 μm, more preferably 30 μm, and even more preferably 20 μm. By setting the average thickness of the adhesive layer 11 to be equal to or less than the above upper limit, it is possible to reduce the overall thickness of the electromagnetic shield laminate 10.

[0032] (Shield layer) The shield layer 12 may be formed of any material as long as it has a shielding performance against electromagnetic waves, but is preferably formed mainly of a metal. In particular, the shield layer 12 is preferably a metal layer. The metal content in the shield layer 12 is preferably 70 mass % or more, more preferably 90 mass % or more, and even more preferably 99 mass % or more. When the metal content in the shield layer 12 is high, it is possible to exhibit good shielding performance. The shield layer 12 preferably contains at least one metal selected from the group consisting of nickel, copper, silver, tin, gold, palladium, aluminum, chromium, titanium, and zinc, and more preferably contains at least one metal of copper and silver. The metal content in the shield layer 12 is preferably 90 mass % or more, and more preferably 99 mass % or more. When the shield layer 12 is formed of such a metal, it is possible to exhibit good shielding performance.

[0033] As a material for forming the shield layer 12, for example, a metal nanoink can be used, specifically, for example, the metal nanoinks described in JP 2016-026237 A, JP 2017-218664 A, JP 2018-183934 A, JP 2018-184553 A, Japanese Patent No. 5833540, and Japanese Patent No. 6029721 can be used. These descriptions are included in the present specification.

[0034] Such metal nano-ink is usually applied by screen printing or inkjet. In the case of inkjet, it is necessary to adjust the viscosity of the solution to suit inkjet discharge. Metal nano-ink with well-adjusted solution viscosity often does not contain polymer, and generally, when it does not contain polymer, the formed shielding layer may have low adhesion to other layers. Therefore, by treating the surface of the other layer with compound α, i.e., providing compound α on the surface of the other layer, and then applying metal nano-ink to the surface of the other layer, a shielding layer with excellent adhesion can be formed. In addition, it is also possible to form a shielding layer specifically on a part of the surface of the other layer by inkjet application or the like. For example, in the manufacture of semiconductor packages, partial shielding layer formation is preferably performed.

[0035] The shield layer 12 may be a layer formed from something other than metal nano-ink, such as a layer formed by plating, vapor deposition, or the like, or a layer made of metal foil.

[0036] The shield layer 12 may be a layer containing a single metal, or may be a layer containing multiple metals. The shield layer 12 may be a single layer or may be multi-layered. When the shield layer 12 is in a multi-layer form, the shield layer preferably has a layer containing copper and a layer containing silver. This form will be described in detail later.

[0037] The lower limit of the average thickness of the shield layer 12 is preferably 0.2 μm, more preferably 0.5 μm, and further preferably 1 μm. By setting the average thickness of the shield layer 12 to the above lower limit or more, the shielding performance is improved. In particular, when the average thickness of the shield layer 12 is 1 μm or more, the transmission characteristics are improved in a signal transmission system that transmits a high-frequency signal having a frequency of 0.01 to 10 GHz. On the other hand, in a conventional electromagnetic shield laminate, when the average thickness of the shield layer is 1 μm or more, peeling between layers tends to occur easily when repeatedly folded. However, in the electromagnetic shield laminate 10, since the bending resistance is sufficiently high, even when the shield layer 12 is thick, peeling between layers is unlikely to occur, and good shielding performance can be maintained. On the other hand, the upper limit of the average thickness of the shield layer 12 is preferably 10 μm, and more preferably 5 μm. By setting the average thickness of the shield layer 12 to the above upper limit or less, the bending resistance can be improved.

[0038] It is preferable that no openings are formed in the shield layer 12. By forming no openings in the shield layer 12, good shielding performance is exhibited, and the strength of the shield layer 12 is increased, improving bending resistance.

[0039] (insulating layer) The insulating layer 13 is a layer having insulating properties. The insulating layer 13 is not particularly limited as long as it has sufficient insulating properties and can preferably protect the shield layer 12 and the like, but is preferably a resin layer.

[0040] Examples of the resin constituting the insulating layer 13 include a thermoplastic resin, a thermosetting resin, an active energy ray curable resin, etc. Specific examples of these resins include the resins exemplified for the adhesive layer 11.

[0041] The insulating layer 13 may contain, as necessary, a curing accelerator, a tackifier, an antioxidant, a pigment, a dye, a plasticizer, an ultraviolet absorber, an antifoaming agent, a leveling agent, a filler, a flame retardant, a viscosity adjuster, an antiblocking agent, and the like.

[0042] The average thickness of the insulating layer 13 is not particularly limited and can be appropriately set as necessary, but the lower limit is preferably 1 μm, more preferably 3 μm. By setting the average thickness of the insulating layer 13 to the above lower limit or more, sufficient insulation and protection properties can be exhibited. On the other hand, the upper limit of the average thickness of the insulating layer 13 is preferably 15 μm, more preferably 10 μm. By setting the average thickness of the insulating layer 13 to the above upper limit or less, the insulating layer 13 becomes easier to bend and is less likely to be broken when bent. In other words, by setting the average thickness of the insulating layer 13 to the above upper limit or less, the bending resistance can be improved.

[0043] (Compound α) The compound α that bonds between the adhesive layer 11 and the shield layer 12 and between the shield layer 12 and the insulating layer 13 will be described below. The compound α forms the first compound α layer 14a and the second compound α layer 14b. The first compound α layer 14a and the second compound α layer 14b may contain components other than the compound α. The compound α that bonds between the adhesive layer 11 and the shield layer 12 and the compound α that bonds between the shield layer 12 and the insulating layer 13 may be the same or different. The compound α is a material for forming a bond (bond) of two substances by interfacial molecular bonding. The interfacial molecular bonding means that a certain compound is interposed at the interface between two substances, and each substance and the compound are chemically bonded by a chemical reaction to bond the two substances, or the bond that results from the result.

[0044] The compound α is at least one of a compound α1 having a benzene ring, an alkoxysilyl group, and one or more groups selected from the group consisting of an azide group, an azide sulfonyl group, and a diazomethyl group in one molecule, and a compound α2 obtained by hydrolysis and condensation of a hydrolyzable silane compound containing the compound α1. Two or more kinds of the compound α can be used, and the compound α1 and the compound α2 can also be used in combination.

[0045] The alkoxysilyl group refers to a group in which an alkoxy group (oxyhydrocarbon group) is bonded to a silicon atom. The alkoxy group refers to a group in which a hydrocarbon group is bonded to an oxygen atom, and examples thereof include a methoxy group, an ethoxy group, a propoxy group, a vinyloxy group, a phenoxy group, and a benzyloxy group. The number of alkoxy groups bonded to a silicon atom may be 1, 2, or 3, and is preferably 3. In the alkoxysilyl group, a group other than an alkoxy group may be bonded to a silicon atom, and examples of such a group include an alkyl group, a phenyl group, a hydroxyl group, and a hydrogen atom. The alkoxy group is preferably an alkoxy group having 1 to 3 carbon atoms, and more preferably a methoxy group, an ethoxy group, and a propoxy group. Examples of the alkoxysilyl group include a trimethoxysilyl group, a triethoxysilyl group, and a tribenzyloxysilyl group.

[0046] The alkoxysilyl group of the compound α can form a chemical bond of "-Si-OM-type" mainly with inorganic material M such as metal through a chemical reaction. The azide group, azidosulfonyl group, or diazomethyl group of the compound α can form a chemical bond of "-NC-type" mainly with organic material such as resin through a chemical reaction. Here, the chemical bond means a covalent bond, an ionic bond, a bond due to intermolecular force, etc., and preferably means a covalent bond or an ionic bond. Therefore, the compound α can firmly bond (join) between the shield layer 12, which is usually mainly composed of a metal, and the adhesive layer 11 and the insulating layer 13, which are usually mainly composed of a resin.

[0047] The compound α is preferably a compound in which one or more groups selected from the group consisting of an azide group, an azide sulfonyl group, and a diazomethyl group are directly bonded to a benzene ring. When an azide group or the like is directly bonded to a benzene ring, the reaction rate of a reaction in which a nitrogen molecule (N2) is released from the azide group or the like by ultraviolet irradiation treatment or heat treatment is higher than when the azide group or the like is not directly bonded to the benzene ring. In addition, an azide group or the like directly bonded to a benzene ring has a feature that the reaction rate of a photodecomposition reaction is sufficiently high even with long-wavelength ultraviolet light compared to an azide group or the like directly bonded to a triazine ring. That is, in the case of a triazine ring, the reaction rate of the photodecomposition reaction has a peak of a certain wavelength width centered on a specific wavelength of short-wavelength ultraviolet light, whereas in the case of a benzene ring, the reaction rate of the photodecomposition reaction has a peak of the same wavelength width centered on a specific wavelength of longer-wavelength ultraviolet light. Therefore, by using a compound α in which an azide group or the like is directly bonded to a benzene ring, it is possible to efficiently treat a material to be surface-treated even when it is irradiated with long-wavelength ultraviolet light that does not deteriorate the material to be surface-treated. Moreover, the treatment can be carried out efficiently at a relatively low temperature for a short period of time.

[0048] (Compound α1) The compound α1 is preferably a compound represented by the following formula (1) or (2).

[0049] [ka]

[0050] In formula (1), R 1 is a hydrogen atom, an alkyl group having 1 to 12 carbon atoms, a phenyl group, an alkoxy group having 1 to 12 carbon atoms, or a hydroxy group. 2 are each independently a hydrogen atom, a halogen, or a monovalent organic group. 1 is an azide group, an azidosulfonyl group, or a diazomethyl group. 1 is a single bond, ester group, ether group, thioether group, amide group, urethane group, urea group, -NHR 3R is a group represented by the formula (3a) or (3b): 3 is an alkyl group having 1 to 6 carbon atoms. 1 is a single bond, a methylene group, an alkylene group having 2 to 12 carbon atoms, or a group containing one or more of -NH-, -O-, -S-, and -S(O)- at the terminal or between the carbon-carbon bonds of an alkylene group having 2 to 12 carbon atoms. m is an integer of 1 to 3. R 1 , X 1 , Y 1 and Z 1 When each of R is more than one, each of them independently satisfies the above definition. 1 At least one of the groups is an alkoxy group having 1 to 12 carbon atoms.

[0051] In formula (2), multiple R 4 , R 5 and R 6 are each independently a hydrogen atom, an alkyl group having 1 to 12 carbon atoms, a phenyl group, an alkoxy group having 1 to 12 carbon atoms, or a hydroxyl group; 4 , R 5 and R 6 At least one of R is an alkoxy group having 1 to 12 carbon atoms. 7 are each independently a hydrogen atom, a halogen, or a monovalent organic group. 2 is an azide group, an azidosulfonyl group, or a diazomethyl group. 2 are each independently a single bond, a methylene group, an alkylene group having 2 to 12 carbon atoms, or a group containing one or more of -NH-, -O-, -S-, and -S(O)- at the terminal or between carbon-carbon bonds of an alkylene group having 2 to 12 carbon atoms.

[0052] [ka]

[0053] In formula (3a), R 8 is a hydrogen atom or a methyl group.

[0054] R 1 , R 4 , R 5 and R 6 Examples of the alkyl group having 1 to 12 carbon atoms represented by the formula (I) include a methyl group, an ethyl group, a propyl group, a butyl group, and an octyl group. R 1 , R 4 , R 5 and R 6 Examples of the alkoxy group having 1 to 12 carbon atoms represented by the following formula include the above-mentioned alkoxy groups. R 2 and R 7 Examples of the halogen represented by the formula (I) include a fluorine atom, a chlorine atom, and a bromine atom. R 2 and R 7 The monovalent organic group represented by the formula (I) includes a monovalent hydrocarbon group, an alkoxy group, -Y 1 -Z 1 -Si-R 1 3(Y 1 , Z 1 and R 1 is Y in formula (1). 1 , Z 1 and R 1 ) group represented by -COO-N-(-Z 2 -SiR 4 R 5 R 6 )2(Z 2 , R 4 , R 5 and R 6 is Z in formula (2) 2 , R 4 , R 5 and R 6 and the like, and a group represented by the formula (14) described below. R 3 Examples of the alkyl group having 1 to 6 carbon atoms represented by the formula (I) include a methyl group, an ethyl group, a propyl group, and a butyl group.

[0055] The preferred forms of the compound represented by formula (1) are as follows: R 1As the alkoxy group, an alkoxy group having 1 to 12 carbon atoms is preferable, an alkoxy group having 1 to 6 carbon atoms is more preferable, and an alkoxy group having 1 to 3 carbon atoms is even more preferable. R 2 is preferably a hydrogen atom. X 1 As X, an azide group and an azide sulfonyl group are preferred. 1 is Y 1 It is preferred that the bond is at the para or meta position relative to the group containing the above. Y 1 As the alkyl group, an amide group is preferable, and an amide group represented by *-CONH- (* indicates a bonding site with a benzene ring) is more preferable. Z 1 As the alkylene group, an alkylene group having 2 to 12 carbon atoms is preferable, and an alkylene group having 2 to 6 carbon atoms is more preferable. m is preferably 3.

[0056] A preferred form of the compound represented by formula (2) is as follows. R 4 , R 5 and R 6 As the alkoxy group, an alkoxy group having 1 to 12 carbon atoms is preferable, an alkoxy group having 1 to 6 carbon atoms is more preferable, and an alkoxy group having 1 to 3 carbon atoms is even more preferable. R 7 is preferably a hydrogen atom. X 2 As X, an azide group and an azide sulfonyl group are preferred. 2 is -COO-N-(-Z 2 -SiR 4 R 5 R 6 It is preferable that the bond is at the para or meta position relative to the group represented by (2). Z 2 As the alkylene group, an alkylene group having 2 to 12 carbon atoms is preferable, and an alkylene group having 2 to 6 carbon atoms is more preferable.

[0057] It is also preferable that the compound α1 is a compound represented by the following formula (11), (12) or (13).

[0058] [ka]

[0059] In formulas (11) to (14), X 10 , X 11 and X 12 are each independently an azide group, an azidosulfonyl group, or a diazomethyl group. 11 and E 12 are each independently >C=O, a methylene group, or an alkylene group having 2 to 12 carbon atoms. 11 , Y 12 , Y 13 and Y 14 each independently represents a hydrogen atom, an alkyl group having 1 to 12 carbon atoms, or -J 13 -Si(OA 10 ) 3-k (R 10 ) k It is a group represented by the formula: 11 , J 12 and J 13 are each independently a methylene group, an alkylene group having 2 to 12 carbon atoms, or a group containing an oxygen atom (-O-) between the carbon-carbon bonds of an alkylene group having 2 to 12 carbon atoms. 15 -R 15 OR-OA 15 Y is a group represented by the formula: 16 -R 16 OR-OA 16 A is a group represented by the formula: 10 , A 15 and A 16 R are each independently an alkyl group having 1 to 4 carbon atoms, a benzyl group, or a hydrogen atom. 10 , R 15 and R 16 are each independently an alkyl group having 1 to 4 carbon atoms or a benzyl group. k is an integer of 0 or more and 2 or less. Q 10 is a hydrogen atom or an organic group represented by formula (4). In formulas (11) and (12), Y 11 and Y 12 At least one of Y and Y contains an oxygen atom.15 and Y 16 At least one of the groups X and X b bonded to the benzene ring contains an oxygen atom. 11 and X 12 are each independently bonded at the para or meta position.

[0060] (Method of synthesizing compound α1) The synthesis method of compound α1 is not particularly limited, but for example, it can be obtained by reacting a silane coupling agent A having an alkoxysilyl group and a reactive group a other than an alkoxysilyl group with a compound B having a reactive group b capable of bonding and reacting with the reactive group a, a benzene ring, and one or more groups selected from the group consisting of an azide group, an azide sulfonyl group, and a diazomethyl group, by a known method. Examples of the combination of the reactive group a and the reactive group b include a combination of an isocyanate group, an epoxy group, an amino group, etc., and a carboxy group.

[0061] Examples of the silane coupling agent A include 3-isocyanatepropyltriethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, 3-glycidoxypropyltrimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltriethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, N-2-(aminoethyl)-3-aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, bis(3-triethoxysilylpropyl)amine, bis(3-trimethoxysilylpropyl)amine, bis(3-aminopropyl)diethoxysilane, and bis(3-aminopropyl)dimethoxysilane.

[0062] Examples of compound B include azidobenzoic acid, azidosulfonylbenzoic acid, diazomethylbenzoic acid, 3-(4-azidophenyl)propionic acid, chlorides of these carboxylic acids, azidoaniline, and azidophenol.

[0063] (Compound α2) In the compound α2, an unreacted alkoxysilyl group usually remains. That is, the compound α2 also usually has a benzene ring, an alkoxysilyl group, and one or more groups selected from the group consisting of an azide group, an azide sulfonyl group, and a diazomethyl group in one molecule.

[0064] Compound α2 obtained by hydrolysis and condensation of a hydrolyzable silane compound including compound α1 has a structural unit A derived from compound α1. Compound α2 may be obtained by another synthesis method as long as the structure is the same as that of the compound obtained by hydrolysis and condensation of a hydrolyzable silane compound including compound α1. Compound α2 is preferably a silsesquioxane compound. Compound α2 preferably has at least one of an alkoxysilyl group and a hydroxysilyl group, and more preferably has a hydroxysilyl group.

[0065] The structural unit A may be a structural unit represented by the following formula (4): The structural unit represented by the following formula (4) is a structural unit derived from a compound α1 represented by formula (1) in which m is 3.

[0066] [ka]

[0067] In formula (4), R 1 , R 2 , X 1 , Y 1 and Z 1 is R in formula (1). 1 , R 2 , X 1 , Y 1 and Z 1 a is an integer from 0 to 2.

[0068] R in Equation (4) 1 , R 2 , X 1 , Y 1 and Z 1Specific examples of R in formula (1) are 1 , R 2 , X 1 , Y 1 and Z 1 The specific example is the same as that of the formula (4). 1 From the viewpoint of reactivity, etc., a is preferably a hydroxy group or an alkoxy group, and more preferably a hydroxy group.

[0069] The lower limit of the content of the structural unit A relative to all structural units in the compound α2 is preferably 10 mol%, more preferably 20 mol%, and even more preferably 30 mol%, while the upper limit of this content is preferably 90 mol%, more preferably 80 mol%, and even more preferably 70 mol%.

[0070] It is preferable that the compound α2 has a structural unit B containing an amino group (-NH2). When the compound α2 has the structural unit B, there is an advantage that the water solubility of the compound α2 is improved. Examples of hydrolyzable silane compounds that provide the structural unit B include 3-aminopropyltrimethoxysilane and 3-aminopropyltriethoxysilane.

[0071] The lower limit of the content of the structural unit B relative to all structural units in the compound α2 is preferably 10 mol%, more preferably 20 mol%, and even more preferably 30 mol%, while the upper limit of this content is preferably 90 mol%, more preferably 80 mol%, and even more preferably 70 mol%.

[0072] The compound α2 may have a structural unit C other than the structural unit A and the structural unit B. Examples of the hydrolyzable silane compound that provides the structural unit C include compounds represented by the following formula (C).

[0073] [ka]

[0074] In formula (C), R dis a hydrogen atom, an alkyl group having 1 to 10 carbon atoms, an alkenyl group having 2 to 10 carbon atoms, an aryl group having 6 to 15 carbon atoms, or an organic group having a reactive group, and d may be the same or different. e is a hydrogen atom, an alkyl group having 1 to 10 carbon atoms, an acyl group having 2 to 6 carbon atoms, or an aryl group having 6 to 15 carbon atoms, and e may be the same or different. x represents an integer of 0 to 3. Furthermore, these alkyl groups, alkenyl groups, and aryl groups may be either unsubstituted or substituted, and can be selected depending on the properties.

[0075] R d and R e Specific examples of the alkyl group represented by the formula (I) include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, a t-butyl group, an n-hexyl group, an n-decyl group, a trifluoromethyl group, a 3,3,3-trifluoropropyl group, a 3-glycidoxypropyl group, a 2-(3,4-epoxycyclohexyl)ethyl group, a [(3-ethyl-3-oxetanyl)methoxy]propyl group, a 3-mercaptopropyl group, and a 3-isocyanatopropyl group. d Specific examples of the alkenyl group represented by the formula (R) include a vinyl group, a 3-acryloxypropyl group, and a 3-methacryloxypropyl group. d and R e Specific examples of the aryl group represented by the formula (I) include a phenyl group, a tolyl group, a p-hydroxyphenyl group, a p-methoxyphenyl group, a 1-(p-hydroxyphenyl)ethyl group, a 2-(p-hydroxyphenyl)ethyl group, a 4-hydroxy-5-(p-hydroxyphenylcarbonyloxy)pentyl group, and a naphthyl group. d Examples of the organic group having a reactive group represented by the formula (R) include an isocyanate group, and a group having an isocyanurate structure and an alkoxysilyl group. d The number of carbon atoms of the organic group having a reactive group represented by the formula (I) is preferably 1 or more and 40 or less. e A specific example of the acyl group represented by the formula (I) is an acetyl group.

[0076] In formula (C), when x=0 it is a tetrafunctional silane, when x=1 it is a trifunctional silane, when x=2 it is a difunctional silane, and when x=3 it is a monofunctional silane.

[0077] Specific examples of the hydrolyzable silane compound represented by formula (C) include tetrafunctional silanes such as tetramethoxysilane, tetraethoxysilane, tetrapropoxysilane, tetraacetoxysilane, and tetraphenoxysilane, methyltrimethoxysilane, methyltriethoxysilane, methyltriisopropoxysilane, methyltri-n-butoxysilane, ethyltrimethoxysilane, ethyltriethoxysilane, ethyltriisopropoxysilane, ethyltri-n-butoxysilane, n-propyltrimethoxysilane, n-propyltriethoxysilane, n-butyltrimethoxysilane, n-butyltriethoxysilane, n-hexyltrimethoxysilane, n-hexyltriethoxysilane, decyltrimethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropyltriethoxysilane, 3-acryloxypropyltriethoxysilane, and 3-acryloxypropyltriethoxysilane. Propyltrimethoxysilane, phenyltrimethoxysilane, phenyltriethoxysilane, p-hydroxyphenyltrimethoxysilane, p-methoxyphenyltrimethoxysilane, 1-(p-hydroxyphenyl)ethyltrimethoxysilane, 2-(p-hydroxyphenyl)ethyltrimethoxysilane, 4-hydroxy-5-(p-hydroxyphenylcarbonyloxy)pentyltrimethoxysilane, 1-naphthyltrimethoxysilane, 2-naphthyltrimethoxysilane, trifluoromethyltrimethoxysilane, trifluoromethyltriethoxysilane, 3,3,3-trifluoropropyltrimethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 2-(3,Examples of the silanes include trifunctional silanes such as 4-epoxycyclohexyl)ethyltriethoxysilane, [(3-ethyl-3-oxetanyl)methoxy]propyltrimethoxysilane, [(3-ethyl-3-oxetanyl)methoxy]propyltriethoxysilane, 3-mercaptopropyltrimethoxysilane, and 3-trimethoxysilylpropylsuccinic acid; bifunctional silanes such as dimethyldimethoxysilane, dimethyldiethoxysilane, dimethyldiacetoxysilane, di-n-butyldimethoxysilane, diphenyldimethoxysilane, (3-glycidoxypropyl)methyldimethoxysilane, and (3-glycidoxypropyl)methyldiethoxysilane; and monofunctional silanes such as trimethylmethoxysilane, tri-n-butylethoxysilane, (3-glycidoxypropyl)dimethylmethoxysilane, and (3-glycidoxypropyl)dimethylethoxysilane.

[0078] The hydrolyzable silane compounds represented by formula (C) also include compounds having five or more alkoxy groups bonded to silicon atoms, such as 1,3,5-tris[3-(trimethoxysilyl)propyl]isocyanurate.

[0079] The hydrolyzable silane compounds may be used alone or in combination of two or more.

[0080] The weight average molecular weight (Mw) of the compound α2 is not particularly limited, but is preferably 1,000 to 100,000, and more preferably 2,000 to 50,000, in terms of polystyrene measured by gel permeation chromatography (GPC).

[0081] (Method of synthesizing compound α2) Compound α2 can be obtained by (i) hydrolysis and condensation of a hydrolyzable silane compound including compound α1, or (ii) a hydrolysis and condensation product of a hydrolyzable silane compound, which is obtained by reacting a compound having structural unit B with "a compound X having a reactive group capable of bonding with an amino group, a benzene ring, and one or more groups selected from the group consisting of an azide group, an azide sulfonyl group, and a diazomethyl group" (azidobenzoic acid, azidosulfonylbenzoic acid, diazomethylbenzoic acid, etc.). In the above (ii), the amino group in structural unit B reacts with compound X to form structural unit A.

[0082] A general method can be used for hydrolysis and condensation to obtain compound α2. For example, a solvent, water, and optionally a catalyst are added to a hydrolyzable silane compound, and the mixture is heated and stirred at 30 to 150° C. for about 0.5 to 100 hours. During stirring, hydrolysis by-products (alcohols such as methanol) and condensation by-products (water) may be removed by distillation, if necessary.

[0083] There is no particular limitation on the catalyst added as necessary, but acid catalysts and base catalysts are preferably used. Specific examples of acid catalysts include hydrochloric acid, nitric acid, sulfuric acid, hydrofluoric acid, phosphoric acid, acetic acid, trifluoroacetic acid, formic acid, polycarboxylic acids or their anhydrides, ion exchange resins, etc. Specific examples of base catalysts include triethylamine, tripropylamine, tributylamine, tripentylamine, trihexylamine, triheptylamine, trioctylamine, diethylamine, triethanolamine, diethanolamine, sodium hydroxide, potassium hydroxide, alkoxysilanes having amino groups, ion exchange resins, etc. The amount of catalyst added is preferably 0.01 to 10 parts by mass relative to 100 parts by mass of hydrolyzable silane compound.

[0084] From the viewpoint of storage stability of the solution containing compound α2, it is preferable that the solution after hydrolysis and condensation does not contain a catalyst, and the catalyst can be removed as necessary. There is no particular limitation on the removal method, but preferred examples include washing with water and / or treatment with an ion exchange resin. Washing with water is a method in which the solution is diluted with an appropriate hydrophobic solvent, washed with water several times, and the organic layer obtained is concentrated with an evaporator. Treatment with an ion exchange resin is a method in which the solution is brought into contact with an appropriate ion exchange resin.

[0085] The solvent used in the hydrolysis condensation reaction is not particularly limited, but a compound having an alcoholic hydroxyl group is preferably used. The compound having an alcoholic hydroxyl group is not particularly limited, but a compound having a boiling point of 110 to 250°C under atmospheric pressure is preferably used.

[0086] Specific examples of compounds having an alcoholic hydroxyl group include acetol, 3-hydroxy-3-methyl-2-butanone, 4-hydroxy-3-methyl-2-butanone, 5-hydroxy-2-pentanone, 4-hydroxy-4-methyl-2-pentanone (diacetone alcohol), ethyl lactate, butyl lactate, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol mono n-propyl ether, propylene glycol mono n-butyl ether, propylene glycol mono t-butyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, dipropylene glycol monomethyl ether, dipropylene glycol monoethyl ether, 3-methoxy-1-butanol, 3-methoxy-3-methyl-1-butanol, etc. These compounds having an alcoholic hydroxyl group may be used alone or in combination of two or more.

[0087] In addition, other solvents may be used together with the compound having an alcoholic hydroxyl group as the solvent. Examples of other solvents include esters such as ethyl acetate, n-propyl acetate, isopropyl acetate, n-butyl acetate, isobutyl acetate, propylene glycol monomethyl ether acetate, 3-methoxy-1-butyl acetate, 3-methyl-3-methoxy-1-butyl acetate, and ethyl acetoacetate, ketones such as methyl isobutyl ketone, diisopropyl ketone, diisobutyl ketone, and acetylacetone, ethers such as diethyl ether, diisopropyl ether, di-n-butyl ether, diphenyl ether, diethylene glycol methyl ethyl ether, and diethylene glycol dimethyl ether, γ-butyrolactone, γ-valerolactone, δ-valerolactone, propylene carbonate, N-methylpyrrolidone, cyclopentanone, cyclohexanone, and cycloheptanone.

[0088] (Specific examples of compound α) More specifically, compound α can be a compound represented by the following formula (15), (16), (17), (18a), (18b), (18c) or (19).

[0089] [ka]

[0090] [ka]

[0091] The compound represented by formula (19) is a silsesquioxane compound composed of l, m, and n of the three types of structural units shown in formula (19) bonded together, where X is an azide group, l is an integer of 0 or more, m is an integer of 1 or more, and n is an integer of 0 or more. a , R b and R c are each independently a hydrogen atom, a hydroxyl group, an alkoxy group, or -O-. fis a hydrogen atom, a hydroxyl group, an alkoxy group, an alkyl group having 1 to 10 carbon atoms, an alkenyl group having 2 to 10 carbon atoms, an aryl group having 6 to 15 carbon atoms, or an organic group having a reactive group, and a plurality of R f may be the same or different. These alkyl, alkenyl, and aryl groups may be either unsubstituted or substituted, and may be selected according to the properties. The compound represented by formula (19) ("IMB-4KP") is water-soluble, for example, when l:m:n=1:1:0. In general, this compound is water-soluble except when the value of the ratio l / (m+n) is close to 0 (for example, less than 0.2 or less than 0.1). That is, from the viewpoint of water solubility, the lower limit of the value of the ratio l / (m+n) is preferably 0.2, more preferably 0.5, and even more preferably 1. The upper limit of the value of the ratio l / (m+n) is preferably 5, and more preferably 2.

[0092] The first compound α layer 14a and the second compound α layer 14b may contain other components besides the compound α. Examples of other components include unreacted materials and by-reaction products when the compound α is synthesized. However, the lower limit of the content of the compound α in the first compound α layer 14a and the second compound α layer 14b is preferably 50% by mass, more preferably 70% by mass, and even more preferably 90% by mass. In this way, the high content of the compound α in the first compound α layer 14a and the second compound α layer 14b can further increase the bonding (bonding) between the layers.

[0093] (Other embodiments) The electromagnetic shielding laminate 20 shown in Fig. 2 is an electromagnetic shielding laminate in which the shielding layer 22 has a two-layer structure including a copper layer 22a (a layer containing copper) and a silver layer 22b (a layer containing silver). The electromagnetic shielding laminate 20 is similar to the electromagnetic shielding laminate 10 in Fig. 1 except that the shielding layer 22 has a two-layer structure, and therefore other components are given the same numbers as the electromagnetic shielding laminate 10 in Fig. 1 and descriptions thereof will be omitted.

[0094] In the two-layered shield layer 22, the copper layer 22a is disposed on the adhesive layer 11 side. The copper content in the copper layer 22a is preferably 90 mass % or more, and more preferably 99 mass % or more. The copper layer 22a may be a layer formed from a copper alloy, and may contain components other than metals.

[0095] The copper layer 22a can be effectively formed, for example, by plating copper. The lower limit of the average thickness of the copper layer 22a is preferably 0.1 μm, more preferably 0.4 μm. On the other hand, the upper limit of this average thickness is preferably 10 μm, more preferably 4 μm.

[0096] In the two-layered shield layer 22, the silver layer 22b is disposed on the insulating layer 13 side. The silver content in the silver layer 22a is preferably 90 mass % or more, and more preferably 99 mass % or more. The silver layer 22a may be a layer formed from a silver alloy, and may contain components other than metals.

[0097] The silver layer 22b can be formed, for example, by applying a silver paste. That is, the silver layer 22b preferably contains silver particles. The shape of the silver particles contained in the silver layer 22b, or the silver particles contained in the silver paste when the silver layer 22b is formed with the silver paste, is not particularly limited, and may be spherical, flaky, dendritic, needle-like, fibrous, or the like. The lower limit of the average particle size of the silver particles is preferably 1 nm, and more preferably 10 nm. On the other hand, the upper limit of this average particle size is preferably 100 nm, and more preferably 50 nm. By using silver particles with such an average particle size, it is possible to form the silver layer 22b with high homogeneity.

[0098] The average thickness of the silver layer 22a is preferably 5 nm or more and 500 nm or less.

[0099] The electromagnetic shielding laminate of the present invention may not have an adhesive layer. That is, an electromagnetic shielding laminate having a shielding layer and an insulating layer, and the shielding layer and the insulating layer are bonded via a compound α, is also one embodiment of the present invention. The specific and preferred embodiments of the shielding layer, insulating layer, and compound α in the electromagnetic shielding laminate of this embodiment are the same as the shielding layer, insulating layer, and compound α in the electromagnetic shielding laminate 10 and the electromagnetic shielding laminate 20 described above. The electromagnetic shielding laminate of this embodiment is also unlikely to cause interlayer peeling, can exhibit sufficient shielding performance, and is particularly suitable for use in semiconductor packages. For example, the sealing material in a semiconductor package corresponds to the insulating layer, and a shielding layer is provided on this insulating layer via a compound α to form an electromagnetic shielding laminate. In this way, the insulating layer does not have to be in the form of a thin film.

[0100] (Other configurations) The electromagnetic wave shielding laminate according to one embodiment of the present invention may have layers other than the adhesive layer, the shielding layer, the insulating layer, and the compound α layer. For example, an anchor coat layer may be provided on the surface of the insulating layer facing the shielding layer. An anchor coat layer may be provided on the surface of a layer other than the insulating layer. Materials for the anchor coat layer include urethane resin, acrylic resin, core-shell type composite resin with urethane resin as the shell and acrylic resin as the core, epoxy resin, imide resin, amide resin, melamine resin, phenol resin, urea-formaldehyde resin, blocked isocyanate obtained by reacting a blocking agent such as phenol with polyisocyanate, polyvinyl alcohol, polyvinylpyrrolidone, etc.

[0101] In addition, the electromagnetic shielding laminate according to one embodiment of the present invention may have a support film laminated on the insulating layer on the side opposite to the shielding layer, and a peelable film laminated on the adhesive layer on the side opposite to the shielding layer. When the electromagnetic shielding laminate has at least one of a support film and a peelable film, the electromagnetic shielding laminate becomes easier to handle during transportation and during the process of manufacturing a shielded printed wiring board or the like using the electromagnetic shielding laminate. When the electromagnetic shielding laminate is placed on a shielded printed wiring board or the like, the support film and the peelable film are peeled off.

[0102] (Applications, etc.) The electromagnetic shielding laminate according to one embodiment of the present invention preferably has an electromagnetic shielding characteristic of 85 dB or more at 200 MHz as measured by the KEC method, and such an electromagnetic shielding laminate has sufficiently high shielding performance.

[0103] The electromagnetic shielding laminate according to one embodiment of the present invention may be used for any purpose as long as it is intended to block electromagnetic waves. The electromagnetic shielding laminate may be an electromagnetic shielding film. The electromagnetic shielding laminate is preferably used for a printed wiring board, in particular a flexible printed wiring board. The electromagnetic shielding laminate is unlikely to cause interlayer delamination during the manufacture of a shielded printed wiring board, and has sufficiently high bending resistance. Therefore, the electromagnetic shielding laminate is unlikely to break even when used for a flexible printed wiring board and is repeatedly folded. Therefore, the electromagnetic shielding laminate can be suitably used as an electromagnetic shielding laminate for a flexible printed wiring board. The electromagnetic shielding laminate according to one embodiment of the present invention is also suitable as an electromagnetic shielding laminate for a semiconductor package.

[0104] The electromagnetic wave shielding laminate according to one embodiment of the present invention is preferably used in a signal transmission system that transmits signals having a frequency of 0.01 GHz or more and 10 GHz or less.

[0105] <Method of manufacturing electromagnetic wave shielding laminate> A method for producing an electromagnetic wave shielding laminate according to one embodiment of the present invention includes a step of bonding a shielding layer to at least one of an adhesive layer and an insulating layer via a compound α, where the compound α is at least one of the compound α1 and the compound α2.

[0106] According to this manufacturing method, it is possible to manufacture an electromagnetic wave shielding laminate that is less susceptible to delamination during the manufacture of a shielded printed wiring board, and that has sufficiently high bending resistance.

[0107] When manufacturing an electromagnetic shielding laminate having an adhesive layer, a shielding layer, and an insulating layer in this order, the method includes a step of bonding the insulating layer and the shielding layer (step 1) and a step of bonding the shielding layer and the adhesive layer (step 2), and in at least one of the two bonding steps (step 1 and step 2), the layers (between the insulating layer and the shielding layer, or between the shielding layer and the adhesive layer) are bonded via compound α. The order of step 1 and step 2 in the manufacturing method is not particularly limited, and either may be performed first, or they may be performed simultaneously. However, it is preferable to perform step 1 and step 2 in that order. In addition, when manufacturing an electromagnetic shielding laminate that does not have either the adhesive layer or the insulating layer, only one of step 1 and step 2 may be performed.

[0108] (Method of manufacturing electromagnetic wave shielding laminate: First embodiment) As a first specific embodiment of the method for producing an electromagnetic shielding laminate having an adhesive layer, a shielding layer, and an insulating layer in this order, a method for forming an insulating layer on one side of a shielding layer and an adhesive layer on the other side will be described. The production method of this embodiment preferably includes a step of providing a compound α on at least one side of the shielding layer (step A), a step of providing an insulating layer on one side of the shielding layer (step B), and a step of providing an adhesive layer on the other side of the shielding layer (step C). In this embodiment, step B is step 1 (a step of bonding the insulating layer and the shielding layer), and step C is step 2 (a step of bonding the shielding layer and the adhesive layer). Note that steps B and C are usually performed after step A. However, when an insulating layer or an adhesive layer is provided without providing compound α on one side of the shielding layer, step B or step C may be performed before step A. The order of steps B and C is not particularly limited, but it is preferable to perform steps B and C in that order.

[0109] (Process A) In the step (step A) of providing compound α on at least one surface of the shielding layer, a solution containing compound α is coated on at least one surface of the shielding layer, and at least one of light irradiation and heat drying is performed to chemically fix compound α to the surface of the shielding layer. In this embodiment, a metal foil or the like can be used as the shielding layer. In this step, it is preferable to provide compound α on both surfaces of the shielding layer.

[0110] The solution containing the compound α contains a solvent. As the solvent, there can be used alcohols such as methanol, ethanol, isopropanol, ethylene glycol, propylene glycol, cellosolve, carbitol, 3-methoxy-3-methyl-1-butanol, ketones such as acetone, methyl ethyl ketone, cyclohexanone, aromatic hydrocarbons such as benzene, toluene, xylene, aliphatic hydrocarbons such as hexane, octane, decane, dodecane, octadecane, esters such as ethyl acetate, methyl propionate, methyl phthalate, ethers such as tetrahydrofuran (THF), ethyl butyl ether, anisole, propylene glycol monomethyl ether acetate (PGMEA), water, etc. In addition, the solvents exemplified as the solvents used in hydrolysis condensation can also be used. Among these, alcohols, ethers, and water are preferable. The solvents can be used alone or in a mixture of two or more.

[0111] The concentration of compound α in the solution containing compound α is preferably 0.05% by mass or more and 5% by mass or less. By setting the concentration of compound α within the above range, a layer of compound α with an appropriate thickness can be effectively formed, and therefore, the bond (adhesion) between layers can be improved.

[0112] The solution containing compound α may contain other components other than compound α and the solvent. Examples of other components include surfactants. However, the content of compound α relative to the total solid content in the solution (all components other than the solvent) is preferably 50% by mass or more, more preferably 70% by mass or more, and even more preferably 90% by mass or more. The content of compound α relative to the total solid content in the solution may be 100% by mass.

[0113] Examples of a method for coating a solution containing compound α include conventionally known coating methods, such as gravure coating, kiss coating, die coating, lip coating, comma coating, blade coating, roll coating, knife coating, spray coating, bar coating, spin coating, dip coating, etc. The thickness of the coating film (wet thickness) when the solution containing compound α is coated is preferably, for example, 1 μm or more and 100 μm or less.

[0114] The heating and drying conditions after coating with the solution containing compound α are preferably, for example, 80° C. to 120° C. and 1 minute to 30 minutes. The light irradiation is preferably, for example, ultraviolet light having a wavelength range of 230 nm to 300 nm.

[0115] (Process B) In the step of providing an insulating layer (step B), an insulating layer is formed by coating one side of the shield layer with an insulating layer-forming material and curing it. It is preferable that compound α (compound α layer) is provided on one side of this shield layer. As a method for coating the insulating layer-forming material, the method exemplified as the method for coating the solution containing compound α in step A can be mentioned. As a method for curing the insulating layer-forming material, various conventionally known methods can be adopted depending on the type of insulating layer-forming material.

[0116] (Process C) In the step of providing an adhesive layer (step C), the other side of the shielding layer is coated with an adhesive layer forming material to form an adhesive layer. It is preferable that the other side of the shielding layer is provided with compound α (compound α layer). As a method for coating the adhesive layer forming material, the method exemplified as the method of coating the solution containing compound α in step A can be mentioned.

[0117] (Method of manufacturing electromagnetic wave shielding laminate: second embodiment) As a second specific embodiment of the method for producing an electromagnetic shielding laminate having an adhesive layer, a shielding layer, and an insulating layer in this order, an example of a method for producing an electromagnetic shielding laminate in which the shielding layer has a two-layer structure of a copper layer and a silver layer will be described. The production method of this embodiment preferably includes a step of providing compound α on one surface of the insulating layer (step i), a step of providing a silver layer on the surface of the insulating layer provided with compound α (step ii), a step of providing a copper layer on the surface of the silver layer (step iii), a step of providing compound α on the surface of the copper layer (step iv), and a step of providing an adhesive layer on the surface of the copper layer provided with compound α (step v). In this embodiment, steps ii and iii are step 1 (a step of joining the insulating layer and the shielding layer), and step v is step 2 (a step of joining the shielding layer and the adhesive layer).

[0118] (Process i) In the step of providing compound α on one surface of the insulating layer (step i), a solution containing compound α is coated on one surface of the insulating layer, and at least one of light irradiation and heat drying is performed to chemically fix compound α to the surface of the insulating layer. In this embodiment, a resin film prepared by a conventionally known method can be used as the insulating layer. The specific form of the solution containing compound α, the coating method, light irradiation, and heat drying in step i can be the same as that of step A described above.

[0119] (Step ii) In the step (step ii) of providing a silver layer on the surface of the insulating layer provided with compound α (or compound α layer), for example, a silver paste or silver ink is printed as a plating catalyst on the surface of the insulating layer provided with compound α. Examples of methods for printing the silver paste include intaglio printing such as gravure printing, relief printing such as flexographic printing, screen printing, offset printing, and inkjet printing. The silver paste or silver ink usually contains silver particles and a dispersion medium, and may also contain various additives such as a dispersant, a thickener, a leveling agent, and an antifoaming agent.

[0120] (Step iii) In the step (step iii) of providing a copper layer on the surface of the silver layer, a copper layer is provided on the surface of the silver layer, for example, by copper plating. The copper plating method is not particularly limited, and can be performed by conventional electroless plating, electrolytic plating, etc. When plating copper by electroless plating, it is preferable to use a plating solution containing copper sulfate, a reducing agent, and a solvent such as an aqueous medium or an organic solvent. When plating copper by electrolytic plating, it is preferable to use a plating solution containing copper sulfate, sulfuric acid, and an aqueous medium. In addition, it is preferable to control the plating process time, current density, amount of plating additive, etc. so as to obtain a desired copper layer thickness.

[0121] By steps ii and iii, a shield layer having a two-layer structure of a copper layer and a silver layer can be formed.

[0122] (Step iv) In the step of providing the compound α on the surface of the copper layer (step iv), the surface of the copper layer is coated with a solution containing the compound α, and at least one of light irradiation and heat drying is performed to chemically fix the compound α on the surface of the copper layer (shield layer). The specific form of the solution containing the compound α, the coating method, the light irradiation and the heat drying in step iv can be the same as that of the above-mentioned step A.

[0123] (Process v) In the step (step v) of providing an adhesive layer on the surface of the copper layer provided with compound α (or compound α layer), an adhesive layer is formed by coating the surface of the copper layer (shield layer) provided with compound α with an adhesive layer forming material. Examples of the method of coating the adhesive layer forming material include the methods exemplified as the method of coating the solution containing compound α in step A.

[0124] <Shielded printed wiring board> A shielded printed wiring board according to one embodiment of the present invention includes a printed wiring board and an electromagnetic shielding laminate. The electromagnetic shielding laminate included in the shielded printed wiring board is the electromagnetic shielding laminate according to one embodiment of the present invention. The electromagnetic shielding laminate used in the shielded printed wiring board typically includes an adhesive layer and is bonded to the printed wiring board by this adhesive layer.

[0125] The printed wiring board may have a conventionally known structure. The printed wiring board has, for example, a base member (such as a base film) on which a printed circuit is formed, and an insulating film provided on the base member so as to cover the printed circuit. The printed wiring board is preferably a flexible printed wiring board. The shielded printed wiring board according to one embodiment of the present invention includes an electromagnetic wave shielding laminate having sufficient bending resistance. Therefore, the shielded printed wiring board also has sufficient bending resistance.

[0126] <Method of manufacturing shielded printed wiring board> A method for producing a shielded printed wiring board according to one embodiment of the present invention comprises a step of adhering an electromagnetic shielding laminate according to one embodiment of the present invention, or an electromagnetic shielding laminate obtained by a method for producing an electromagnetic shielding laminate according to one embodiment of the present invention, to a printed wiring board. The electromagnetic shielding laminate used in the method for producing a shielded printed wiring board typically comprises an adhesive layer.

[0127] The electromagnetic shielding laminate and the printed wiring board can be bonded by a conventionally known method, for example, by overlapping the printed wiring board and the electromagnetic shielding laminate so that the adhesive layer of the electromagnetic shielding laminate is in contact with the surface of the printed wiring board, and then hot pressing in this state.

[0128] The method for manufacturing the shielded printed wiring board may further include a step of mounting components by solder reflow after the bonding step.

[0129] According to this manufacturing method for a shielded printed wiring board, a strong interlayer bond is maintained and interlayer delamination is unlikely to occur even when volatile components accumulate between layers of the electromagnetic wave shielding laminate due to hot pressing, solder reflow, etc. In addition, the shielded printed wiring board obtained by this manufacturing method has sufficiently high bending resistance.

[0130] <Semiconductor packages> A semiconductor package according to an embodiment of the present invention includes an electromagnetic wave shielding laminate according to an embodiment of the present invention. For example, a compound α is provided on an insulating layer (sealing material or the like) of a semiconductor package, and then a metal nano-ink is applied by screen printing, inkjet method or the like to partially form a shielding layer. Among metal nano-inks, particularly by using an ink containing silver nanoparticles, a shielding layer excellent in adhesion, conductivity, electromagnetic wave shielding performance, and the like can be formed. Therefore, according to the semiconductor package according to an embodiment of the present invention, it is possible to achieve high functionality of the semiconductor package.

[0131] <Electronic equipment> An electronic device according to an embodiment of the present invention includes a shielded printed wiring board according to an embodiment of the present invention or a semiconductor package according to an embodiment of the present invention. The shielded printed wiring board according to an embodiment of the present invention has strong interlayer bonding and has sufficient bending resistance. Therefore, even when the shielded printed wiring board is incorporated into an electronic device in a folded state, it is unlikely to be damaged. Therefore, the electronic device according to an embodiment of the present invention can narrow the space for arranging the shielded printed wiring board. Therefore, the electronic device can be made thinner and smaller. Furthermore, the semiconductor package according to an embodiment of the present invention has a shielding layer formed with high adhesion, and an electronic device including such a semiconductor package can be made highly functional.

[0132] <Other embodiments> The present invention is not limited to the above-described embodiment, and should be understood to include various modified examples that are implemented within the scope that does not deviate from the gist of the present invention.

[0133] For example, when the electromagnetic shielding laminate of the present invention has an adhesive layer, a shielding layer, and an insulating layer in this order, either the adhesive layer and the shielding layer or the shielding layer and the insulating layer may not be bonded via compound α. Examples of such a bond include a bond via another compound, a bond directly without compound α, etc. EXAMPLES

[0134] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the embodiments of these examples.

[0135] [Preparation Example 1] Preparation of Compound α Solution 1 5.5g of 4-azidobenzoic acid, 400g of THF (tetrahydrofuran), and 74g of 3-aminopropyltriethoxysilane were weighed into a 2L flask. 5.4g of 1,1-carbonylimidazole dissolved in 50g of THF was added successively while stirring, and the mixture was allowed to react for 24 hours with stirring. After the reaction was completed, the THF was distilled off using a rotary evaporator to obtain 12g of reaction mixture A containing N-(3-triethoxysilylpropyl)-4-azidobenzamide (IMB-4K) represented by the above formula (15). 500g of 3-methoxy-3-methyl-1-butanol was added to 1g of reaction mixture A to obtain compound α solution 1.

[0136] [Preparation Example 2] Preparation of Compound α Solution 2 10 g of reaction mixture A, 860 g of 3-methoxy-3-methyl-1-butanol, 27 g of water, and 3.3 g of 3-aminopropyltriethoxysilane were weighed into a 2 L flask and stirred at 40° C. for 24 hours to obtain reaction mixture B. 50 g of reaction mixture B and 450 g of 3-methoxy-3-methyl-1-butanol were mixed to obtain compound α solution 2.

[0137] [Preparation Example 3] Preparation of Compound α Solution 3 Compound α solution 3 was prepared in the same manner as in Preparation Example 2, except that 3.3 g of 3-aminopropyltriethoxysilane was replaced with 9.2 g of 1,3,5-tris[3-(trimethoxysilyl)propyl]isocyanurate.

[0138] [Preparation Example 4] Preparation of silver paste Silver particles having an average particle size of 30 nm were dispersed in a mixed dispersion medium of 35 parts by mass of ethanol and 65 parts by mass of ion-exchanged water using a polyethyleneimine compound as a dispersant, thereby obtaining a silver paste with a silver concentration of 15% by mass.

[0139] [Example 1] Production of electromagnetic wave shielding laminate (Process i) An insulating layer (epoxy resin film) made of epoxy resin and having an average thickness of 5 μm was prepared. Compound α solution 1 obtained in Preparation Example 1 was applied to one side of this insulating layer using a bar coater (ROD No. #10; wet thickness: 22.9 μm), and then heated and dried at 100° C. for 10 minutes.

[0140] (Step ii) Next, the silver paste obtained in Preparation Example 4 was screen-printed on the surface of the insulating layer on which the compound α was provided, and baked at 120° C. for 2 hours to provide a silver layer with an average thickness of 100 nm.

[0141] (Step iii) Next, the insulating layer on which the silver layer was provided via the compound α was immersed in an electroless copper plating solution ("ARG Copper" manufactured by Okuno Pharmaceutical Co., Ltd., pH 12.5) at 55°C for 20 minutes to provide an electroless copper plating film (average thickness 0.5 μm) on the surface of the silver layer. Next, the surface of the electroless copper plating film obtained above was placed on the cathode, phosphorus-containing copper was placed on the anode, and an electroplating solution containing copper sulfate was used to plate the insulating layer at a current density of 2.5 A / dm 2Electroplating was performed for 30 minutes. As a result, a copper layer (copper plating layer) with an average total thickness of 1 μm, including the electroless copper plating film, was formed on the surface of the silver layer. The electroplating solution used was a solution of 70 g / L copper sulfate, 200 g / L sulfuric acid, 50 mg / L chloride ions, and 5 g / L Top Lucina SF (a brightener manufactured by Okuno Chemical Industries Co., Ltd.).

[0142] (Step iv) Next, the compound α solution 1 obtained in Preparation Example 1 was applied to the surface of the copper layer using a bar coater (ROD No. #10; wet thickness: 22.9 μm), and then heated and dried at 100° C. for 10 minutes.

[0143] (Process v) Next, the surface of the copper layer provided with the compound α was coated with an adhesive forming material (conductive adhesive) obtained by adding 20 parts by mass of Ag-coated Cu powder to 80 parts by mass of phosphorus-containing epoxy resin so as to have an average thickness of 15 μm, to provide an adhesive layer. Note that the lip coating method was used as the coating method. Through the above steps, the electromagnetic shielding laminate of Example 1 was obtained.

[0144] [Examples 2 and 3] Each of the electromagnetic wave shielding laminates of Examples 2 and 3 was obtained in the same manner as in Example 1, except that in step i and step iv, each of the compound α solutions shown in Table 1 was used instead of compound α solution 1.

[0145] [Comparative Example 1] An electromagnetic wave shielding laminate of Comparative Example 1 was obtained in the same manner as in Example 1, except that steps i and iv were not performed, i.e., a silver layer was provided directly on the surface of the insulating layer in step ii, and an adhesive layer was provided directly on the surface of the copper layer in step v.

[0146] [evaluation] (Delamination) The delamination of each electromagnetic shielding laminate was evaluated by the following method. First, the electromagnetic shielding laminate was attached to a printed wiring board by heat pressing to obtain a shielded printed wiring board. Next, this shielded printed wiring board was left in a clean room at 23°C and 63% RH for 7 days, and then exposed to the temperature conditions during reflow for 30 seconds to evaluate the presence or absence of delamination. Note that the temperature conditions during reflow were set to a maximum temperature profile of 265°C, assuming lead-free solder. Those that did not experience delamination were rated as "A," and those that experienced delamination were rated as "B." The evaluation results are shown in Table 1.

[0147] (Bending resistance) The bending resistance of each electromagnetic shielding laminate was evaluated by the following method. The electromagnetic shielding laminate was attached to both sides of a polyimide film with an average thickness of 50 μm by hot pressing, and cut to a size of 130 mm in length and 15 mm in width to prepare a test piece. The bending resistance (folding resistance) of this test piece was measured using an MIT folding fatigue tester (manufactured by Yasuda Seiki Seisakusho Co., Ltd., No. 307 MIT type folding resistance tester) based on the method specified in JIS P8115:2001 and JIS C 6471:1995. The test conditions were as follows. Bending clamp tip R: 0.38 mm Bend angle: ±135° Folding speed: 175cpm Load: 500gf Detection method: The built-in electrical device detects breaks in the electromagnetic shield laminate. Those that did not break even after 600 bending cycles were rated as "A," and those that broke even after less than 600 bending cycles were rated as "B." The evaluation results are shown in Table 1.

[0148] (Electromagnetic wave shielding properties) The electromagnetic shielding properties of each electromagnetic shielding laminate were evaluated by the following method: The electromagnetic shielding laminate was cut into a 15 cm square, and the electromagnetic shielding properties were measured at 200 MHz under conditions of a temperature of 25°C and a relative humidity of 30 to 50% using an electromagnetic shielding effectiveness measuring device developed by the Kansai Electronics Industry Development Center (KEC). The electromagnetic shielding characteristics at 200 MHz, measured using the KEC method, were rated as "A" if they were 85 dB or higher, and "B" if they were less than 85 dB. The evaluation results are shown in Table 1.

[0149] [Table 1]

[0150] As shown in Table 1, the electromagnetic shielding laminates of Examples 1 to 3, in which the adhesive layer and the shielding layer, and the shielding layer and the insulating layer were bonded via a specified compound α, were less susceptible to interlayer delamination even after undergoing a heating process, had sufficiently high bending resistance, and also had good electromagnetic shielding properties.

[0151] [Reference example] <Synthesis of compound α> The compounds were identified using a Fourier transform infrared spectrophotometer IRTracer-100 manufactured by Shimadzu Corporation, a nuclear magnetic resonance spectrometer NMR spectrometer Z manufactured by JEOL Ltd., and a gas chromatograph mass spectrometer GCMS-QP2020 NX manufactured by Shimadzu Corporation.

[0152] (1) Synthesis of 4-azidobenzoyl chloride (production of raw material) [ka] 2.6 g of 4-azidobenzoic acid (N3C6H4COOH) was dissolved in a mixed solvent of 30 mL of methylene chloride (CH2Cl2) and 0.3 mL of DMF (N,N-dimethylformamide C3H7NO). Under a nitrogen gas atmosphere, 7.3 g of thionyl chloride (SOCl2) dissolved in 20 mL of methylene chloride was added dropwise at room temperature while stirring. Stirring was continued for another 2 hours to complete the reaction. After the reaction was completed, low boiling point substances including methylene chloride were distilled off to obtain a yellow oil containing 4-azidobenzoic acid chloride (N3C6H4COCl). This oil was directly used in the next reaction without further purification.

[0153] (2) Synthesis of N-(3-triethoxysilylpropyl)-4-azidobenzamide (IMB-4K) [ka]

[0154] 1.8 g of 4-azidobenzoyl chloride (N3C6H4COCl) was dissolved in 15 mL of THF (tetrahydrofuran). Under a nitrogen gas atmosphere, 3.6 g of 3-triethoxysilylpropylamine and 2.1 g of TEA (triethylamine) were dissolved in 20 mL of THF and added dropwise at room temperature while stirring. Stirring was continued for another 2 hours to complete the reaction. After the reaction was completed, the solution containing THF was distilled off, and the obtained crude product was purified by column chromatography (eluent: acetone / hexane = 85 / 15) to obtain a pale yellow oil with a yield of 66% (2.4 g). IR, NMR and QCMS analyses confirmed that the product was N-(3-triethoxysilylpropyl)-4-azidobenzamide.

[0155] (3) Synthesis of N-(3-triethoxysilylpropyl)-3-azidobenzamide (IMB-3K) [ka]

[0156] 1.8 g of 3-azidobenzoyl chloride (N3C6H4COCl) was dissolved in 15 mL of THF. Under a nitrogen gas atmosphere, 3.6 g of 3-triethoxysilylpropylamine (H2N(CH2)2Si(OC2H5)3) and 2.1 g of TEA were dissolved in 20 mL of THF and added dropwise at room temperature while stirring. Stirring was continued for another 2 hours to complete the reaction. After the reaction was completed, the solution containing THF was distilled off, and the obtained crude product was purified by column chromatography (eluent: acetone / hexane = 85 / 15) to obtain a pale yellow oil with a yield of 62% (2.2 g). From the spectrum, etc., it was confirmed that the product was N-(3-triethoxysilylpropyl)-3-azidobenzamide.

[0157] (4) Synthesis of N,N-bis(3-triethoxysilylpropyl)-4-azidobenzamide (IMB-4KB) [ka]

[0158] 1.8 g of 4-azidobenzoyl chloride (N3C6H4COCl) was dissolved in 15 mL of THF. Under a nitrogen gas atmosphere, 6 g of bis(3-triethoxysilylpropyl)amine (HN((CH2)3Si(OC2H5)3)2) and 2.1 g of TEA were dissolved in 20 mL of THF and added dropwise at room temperature while stirring. Stirring was continued for another 2 hours to complete the reaction. After the reaction was completed, the solution containing THF was distilled off, and the obtained crude product was purified by column chromatography (eluent: acetone / hexane = 85 / 15) to obtain a pale yellow oil with a yield of 61%. From the spectrum, etc., it was confirmed that the product was N,N-bis(3-triethoxysilylpropyl)-4-azidobenzamide.

[0159] (5) Synthesis of N,N-bis(3-triethoxysilylpropyl)-3-azidobenzamide (IMB-3KB) [ka]

[0160] 1.8 g of 3-azidobenzoyl chloride (N3C6H4COCl) was dissolved in 15 mL of THF. Under a nitrogen gas atmosphere, 6 g of bis(3-triethoxysilylpropyl)amine (HN((CH2)3Si(OC2H5)3)2) and 2.1 g of TEA were dissolved in 20 mL of THF and added dropwise at room temperature while stirring. Stirring was continued for another 2 hours to complete the reaction. After the reaction was completed, the solution containing THF was distilled off, and the obtained crude product was purified by column chromatography (eluent: acetone / hexane = 85 / 15) to obtain a pale yellow oil with a yield of 62%. From the spectrum, etc., it was confirmed that the product was N,N-bis(3-triethoxysilylpropyl)-3-azidobenzamide.

[0161] (6) Synthesis of N,N'-((diethoxysilanediyl)bis(3-propyl-3,1-diyl)bis(4-azidobenzamide) [ka]

[0162] 2.8 g of 4-azidobenzoyl chloride (N3C6H4COCl) was dissolved in 30 mL of THF. Under a nitrogen gas atmosphere, bis(3-aminopropyl)diethoxysilane (2.3 mL) and 2.1 g of TEA were dissolved in 20 mL of THF and added dropwise at room temperature while stirring. Stirring was continued at room temperature overnight. Stirring was continued for another 2 hours to complete the reaction. After the reaction was completed, the solution containing THF was distilled off, and the obtained crude product was purified by column chromatography (eluent: acetone / hexane = 85 / 15) to obtain a pale yellow oil with a yield of 50%. From the spectrum, it was confirmed that the product was N,N'-((diethoxysilanediyl)bis(3-propyl-3,1-diyl)bis(4-azidobenzamide).

[0163] (7) Production of the silsesquioxane compound (IMB-4KP) represented by the above formula (19) 3-Azidobenzoyl chloride (N3C6H4COCl) was dissolved in THF. Under a nitrogen gas atmosphere, raw material oligomer (Gelest, USA), which is a hydrolysis condensation product of 3-aminopropyltriethoxysilane, and TEA were dissolved in THF and added dropwise at room temperature while stirring. Stirring was continued to complete the reaction. After the reaction was completed, the solution containing THF was distilled off, and the obtained crude product was purified to obtain the target product. This target product was a silsesquioxane compound represented by formula (19). From the spectrum, it was confirmed that in the product, l, m, and n in formula (19) were l:m:n=1:1:0.

[0164] <1. Effect of IMB-K in electroless plating on various resin substrates> For each resin substrate shown in Table 2, a 20 μm-thick copper coating was formed according to the flow diagram shown in Figure 3, and the adhesion was tested. As shown in Table 2, in the degreasing and cleaning step S1, acetone or ethanol was used depending on the resin substrate. In the pretreatment step S2, a corona discharge treatment or an oxygen plasma treatment (100 mL / min, 5 min, 200 W) was performed depending on the resin substrate. In the IMB (compound α) supporting treatment S3, the substrate was immersed in an ethanol solution of IMB-4K for 30 seconds. In the post-treatment step S4, the sample was exposed to an irradiation energy of 200 mJ / cm from a UV-LED irradiator. 2The resin substrate was irradiated with ultraviolet light at 100°C. Steps S3 and S4 were repeated twice. In the post-IMB heat treatment step S6, the resin substrate was held at 80°C, 110°C, or 125°C for 10 minutes depending on the resin substrate. After the electroless plating step S7 and the electrolytic plating step S8, a copper coating of 20 μm thickness was obtained. In order to relieve the residual stress of the plating, an annealing treatment was performed by holding at 150°C for 10 minutes. The appearance of the copper coating formed on each resin substrate was observed after electroless plating, electrolytic plating, and annealing. In addition, the peel strength of the copper coating was measured for each resin substrate. A force gauge ZTA-50N was attached to a vertical motorized measuring stand MX2-500N (manufactured by Imada Co., Ltd.) to constitute a 90° peel strength tester. The peel speed was 50 mm / min. Three samples were prepared for each resin substrate, and measurements were taken on the front and back surfaces, and the maximum and average peel strengths were averaged.

[0165] [Table 2]

[0166] Without IMB loading treatment, electroless copper plating does not form on any of these resin substrates, or if it does form, the adhesion strength of the copper coating is extremely weak, but by carrying out IMB loading treatment prior to electroless plating, a copper coating with good appearance and adhesion was formed.In addition, for the fluororesin composite substrate of sample #9, we had previously obtained a maximum peel strength of 6.82 N / cm by a process that combined IMB loading treatment using 2,4-diazide-6-(3-triethoxysilylpropyl)amino-1,3,5-triazine and electroless plating, but we found that by carrying out IMB loading treatment using IMB-4K and electroless plating, a peel strength much higher than that could be achieved.

[0167] <2. Effects of various compounds α in electroless plating of cycloolefin polymer (COP) sheets> A 20 μm thick copper coating was formed on a COP sheet (0.1 mm thick, sample #41) according to the flow diagram shown in FIG. 3, and the adhesion was tested. Acetone was used in the degreasing and cleaning step S1. In the pretreatment step S2, oxygen plasma treatment (100 mL / min, 2 min, 200 W) was performed. In the IMB carrying treatment S3, the sample was immersed in an ethanol solution of IMB-4K for 30 seconds. In the posttreatment step S4, the sample was irradiated with 200 mJ / cm irradiated energy from a UV-LED irradiator. 2 The specimen was irradiated with ultraviolet light at 100°C. Then, a heat treatment was performed at 125°C for 15 minutes. Steps S3 and S4 were repeated twice in total. The post-IMB heat treatment step S6 was not performed. A copper coating with a thickness of 20 μm was obtained through the electroless plating step S7 and the electrolytic plating step S8. In the electroless plating step S7, an annealing step S75 was performed at 110°C for 60 minutes. After electrolytic plating, the peel strength of the copper coating was measured. Three samples were prepared for each specimen and measurements were taken for each sample, and the average peel strength was calculated. The peel strength was 6.09 N / cm.

[0168] For COP sheets (samples #42 to #45) of the same material and thickness as sample #41, a 20 μm thick copper coating was formed in the same process as sample #41, except for the type of compound α used in the IMB loading process S3 and whether only heat treatment was performed in the post-processing step S4 (represented as "H") or both ultraviolet irradiation treatment and heat treatment were performed (represented as "UV+H"), and the peel strength was measured. The results are shown below. The conditions for ultraviolet irradiation in the post-processing step S4 were the same as those for sample #41, and the conditions for heat treatment in the post-processing step S4 were 125°C and 15 minutes. Sample Compound α Post-treatment Peel strength (N / cm) #41 IMB-4K UV+H 6.09 #42 IMB-3K UV+H 4.78 #43 IMB-3KB UV+H 4.23 #44 IMB-4K H 4.92 #45 IMB-3KB H 4.91

[0169] <3. Effects of various compounds α on the bond formed by thermocompression of sheet-like materials> According to the flow diagram shown in Fig. 4, a polytetrafluoroethylene (PTFE) sheet (sample #110) was prepared by thermocompression bonding a metal foil, and peel strength was examined. The PTFE sheet used was manufactured by Nitto Denko (defluorinated, thickness 0.18 mm). The metal foil used was a rolled copper foil with a thickness of 18 µm. The surface treatment step Sst for the PTFE sheet was performed according to the surface treatment step Sst in Fig. 3, but the degreasing and cleaning step S1 and the pretreatment step S2 were not performed, and in the IMB carrying treatment step S3, a 1 mass % ethanol solution of the compound IMB-4K was applied to a wet thickness of 20 µm. Furthermore, in the post-treatment step S4, irradiation energy of 100 mJ / cm was applied. 2 The UV irradiation was performed. The post-IMB heat treatment step S6 was not performed. Next, in the thermocompression bonding step Shp, rolled copper foil was thermocompression bonded to the surface of the PTFE sheet at a press temperature of 180°C, a press pressure of 8 MPa, and a press time of 10 minutes. After natural cooling, a peel strength test was performed, and a peel strength of 8.0 N / cm was obtained.

[0170] A bond was formed by thermocompression of two substances in the same manner as sample #110, except for the two substances to be thermocompressed and the type of compound α used in the IBM support processing step, and a peel strength test was performed. The results are shown below. The thickness of each substance was 20 μm or 18 μm. The solvent for IMB-4KP was water, and the solvent for the other compound α was ethanol. Sample Substance 1 Substance 2 Compound α Peel strength (N / cm) #110 PTFE Cu IMB-4K 8.0 #111 PTFE Cu IMB-3K 7.8 #112 PTFE Cu IMB-4KB 8.0 #113 PTFE Al IMB-4KP 6.5 #114 PI PI IMB-4K 7.2 #115 PI PTFE IMB-4K 8.9 #116 PI Cu IMB-4K 3.9 #117 PI Al IMB-4K 2.1 #118 PI Al None 0.0

[0171] From the results of the above-mentioned Reference Examples, it is found that a strong bond can be formed between a metal and a resin by using at least one of the compound α1 having a benzene ring, an alkoxysilyl group, and one or more groups selected from the group consisting of an azide group, an azide sulfonyl group, and a diazomethyl group in one molecule, and the compound α2 obtained by hydrolysis and condensation of a hydrolyzable silane compound containing the compound α1. Therefore, it is clear that when such a compound α is used for bonding between layers of an electromagnetic wave shielding laminate, an electromagnetic wave shielding laminate that is unlikely to cause interlayer peeling during the manufacture of a shielded printed wiring board and has sufficiently high bending resistance can be obtained, as in Example 1, etc. [Explanation of symbols]

[0172] 10, 20 Electromagnetic wave shielding laminate 11 Adhesive layer 12, 22 Shield layer 13 Insulating layer 14a First compound α layer 14b Second compound α layer 22a copper layer 22b Silver layer

Claims

1. A shielding layer; At least one of an adhesive layer and an insulating layer bonded to the shielding layer via a compound α; Equipped with The compound α is Within one molecule, A benzene ring; An alkoxysilyl group, one or more groups selected from the group consisting of an azide group, an azidosulfonyl group, and a diazomethyl group; Compound α1 having the formula Compound α2 obtained by hydrolysis and condensation of a hydrolyzable silane compound containing the compound α1 The electromagnetic wave shielding laminate is at least one of the above.

2. 2. The electromagnetic wave shielding laminate according to claim 1, wherein the compound α is a compound in which one or more groups selected from the group consisting of an azide group, an azidosulfonyl group, and a diazomethyl group are directly bonded to the benzene ring.

3. 3. The electromagnetic wave shielding laminate according to claim 1, wherein the compound α1 is a compound represented by the following formula (1) or (2): 【Chemistry 1】 In formula (1), R 1 is a hydrogen atom, an alkyl group having 1 to 12 carbon atoms, a phenyl group, an alkoxy group having 1 to 12 carbon atoms, or a hydroxy group. 2 are each independently a hydrogen atom, a halogen, or a monovalent organic group. 1 is an azide group, an azidosulfonyl group, or a diazomethyl group. 1 represents a single bond, an ester group, an ether group, a thioether group, an amide group, a urethane group, a urea group, -NHR 3 -, or a group represented by the following formula (3a) or (3b): 3 is an alkyl group having 1 to 6 carbon atoms. 1 is a single bond, a methylene group, an alkylene group having 2 to 12 carbon atoms, or a group containing one or more of -NH-, -O-, -S-, and -S(O)- at the terminal or between the carbon-carbon bonds of an alkylene group having 2 to 12 carbon atoms. m is an integer of 1 to 3. R 1 , X 1 , Y 1 and Z 1 When each of R is more than one, each of them independently satisfies the above definition. 1 At least one of the groups is an alkoxy group having 1 to 12 carbon atoms. In formula (2), a plurality of R 4 , R 5 and R 6 are each independently a hydrogen atom, an alkyl group having 1 to 12 carbon atoms, a phenyl group, an alkoxy group having 1 to 12 carbon atoms, or a hydroxyl group; 4 , R 5 and R 6 At least one of R is an alkoxy group having 1 to 12 carbon atoms. 7 are each independently a hydrogen atom, a halogen, or a monovalent organic group. 2 is an azide group, an azidosulfonyl group, or a diazomethyl group. 2 are each independently a single bond, a methylene group, an alkylene group having 2 to 12 carbon atoms, or a group containing one or more of -NH-, -O-, -S-, and -S(O)- at the terminal or between the carbon-carbon bonds of an alkylene group having 2 to 12 carbon atoms. 【Chemistry 2】 In formula (3a), R 8 is a hydrogen atom or a methyl group.

4. The adhesive layer is provided.

4. The electromagnetic wave shielding laminate according to claim 1, 2 or 3, wherein the adhesive layer contains at least one resin selected from the group consisting of polyamide resins, polyester resins, acrylic resins, epoxy resins, polyurethane resins and polyurethane urea resins.

5. The adhesive layer is provided.

4. The electromagnetic wave shielding laminate according to claim 1, wherein the adhesive layer is electrically conductive.

6. The shielding layer is provided.

6. The electromagnetic wave shielding laminate according to claim 1, wherein the shielding layer contains at least one metal selected from the group consisting of nickel, copper, silver, tin, gold, palladium, aluminum, chromium, titanium and zinc.

7. The shielding layer is provided.

6. The electromagnetic wave shielding laminate according to claim 1, wherein the shielding layer comprises a layer containing copper and a layer containing silver.

8. The electromagnetic wave shielding laminate according to any one of claims 1 to 7, which is used for a flexible printed wiring board.

9. The electromagnetic wave shielding laminate according to any one of claims 1 to 7, which is used for a semiconductor package.

10. The method includes a step of bonding a shielding layer to at least one of an adhesive layer and an insulating layer via a compound α, The compound α is Within one molecule, A benzene ring; An alkoxysilyl group, one or more groups selected from the group consisting of an azide group, an azidosulfonyl group, and a diazomethyl group; Compound α1 having the formula Compound α2 obtained by hydrolysis and condensation of a hydrolyzable silane compound containing the compound α1 The method for producing an electromagnetic wave shielding laminate is at least one of the above.

11. A printed wiring board; The electromagnetic shielding laminate according to any one of claims 1 to 8, which is adhered to the printed wiring board. A shielded printed wiring board comprising:

12. A step of adhering the electromagnetic shielding laminate according to any one of claims 1 to 8 or the electromagnetic shielding laminate obtained by the method for producing an electromagnetic shielding laminate according to claim 9 to a printed wiring board. A method for manufacturing a shielded printed wiring board comprising:

13. A semiconductor package comprising the electromagnetic shielding laminate according to claim 9.

14. An electronic device comprising the shielded printed wiring board according to claim 11 or the semiconductor package according to claim 13.

Citation Information

Patent Citations

  • Light transmissive electromagnetic wave shielding material, manufacturing method thereof, and filter for display

    JP2007242921A

  • Small bag for liquid, and liquid small bag packaging filled with liquid

    JP2008143582A

  • Laminated sheet and method for manufacturing conductive pattern sheet manufactured by using the laminated sheet

    JP2008230167A

  • Adhesive film for semiconductor device and semiconductor device

    JP2012124466A

  • Electromagnetic wave shielding film

    JP2021028985A