Positive electrode for non-aqueous electrolyte storage element, and non-aqueous electrolyte storage element including the same

By using a lithium-excess positive electrode active material with amorphous carbon and graphite, the electrode density of non-aqueous electrolyte storage devices is improved without sacrificing discharge capacity or cycle performance.

JP7569505B2Active Publication Date: 2024-10-18GS YUASA CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023108732
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2023-06-30
Publication Date
2024-10-18
Estimated Expiration
2039-05-09

AI Technical Summary

Technical Problem

Existing non-aqueous electrolyte storage devices face challenges in achieving high electrode density while maintaining high discharge capacity, particularly when using lithium-excess positive electrode active materials.

Method used

Incorporating a lithium-excess positive electrode active material with a composition formula Li1+α Me1-α O2 (Me: Ni and Mn) and adding amorphous carbon and graphite, where the graphite content is 2% by mass or less, to improve electrode density without compromising discharge capacity.

Benefits of technology

The solution results in a positive electrode with enhanced electrode density and maintains high discharge capacity and charge/discharge cycle performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007569505000005
    Figure 0007569505000005
  • Figure 0007569505000006
    Figure 0007569505000006
  • Figure 0007569505000007
    Figure 0007569505000007
Patent Text Reader

Abstract

To provide a positive electrode for a non-aqueous electrolyte electricity-storage element with high electrode density without losing a high discharge capacity.SOLUTION: An embodiment of the present invention provides a positive electrode for a non-aqueous electrolyte electricity-storage element, in which it is expressed by a composition formula Li1+αMe1-αO2 (Me: Ni and Mn, or a transition metal containing Ni, Co, and Mn), a value of (1+α) / (1-α) as a mol ratio of Li / Me of Li to the transition metal (Me) is larger than 1.1 and 1.5 or less, a lithium excessive type positive electrode active material of which a mol ratio of Mn / Me of Mn to the transition metal (Me) is larger than 0.5, an amorphous material carbon, and a graphite are contained, and in which a content amount of the graphite is 2 mass% or less to a mass of a positive electrode mixture layer.SELECTED DRAWING: Figure 7
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a positive electrode for a nonaqueous electrolyte storage element, and a nonaqueous electrolyte storage element including the same. [Background technology]

[0002] Due to their high energy density, non-aqueous electrolyte storage elements typified by lithium ion secondary batteries are widely used in electronic devices such as personal computers and communication terminals, automobiles, etc. In addition, as non-aqueous electrolyte storage elements other than lithium ion secondary batteries, capacitors such as lithium ion capacitors and electric double layer capacitors are also widely used.

[0003] As positive electrode active materials for non-aqueous electrolyte storage elements, LiCoO2, LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2, LiNi 0.5 Co 0,2 Mn 0.3 These so-called "LiMeO2-type" active materials have an α-NaFeO2-type crystal structure and a molar ratio of Li to transition metal (Me) (Li / Me) of less than 1.1, typically around 1.

[0004] On the other hand, as a positive electrode active material for a non-aqueous electrolyte storage element that can obtain a high discharge capacity, a lithium-excess active material is known in which the composition ratio Li / Me of lithium (Li) to transition metal (Me) is greater than 1, for example, Li / Me is 1.1 to 1.6. The lithium-excess active material is represented by the composition formula Li 1+α Me 1-α O2(α>0). Here, if the composition ratio Li / Me of lithium (Li) to the ratio of transition metal (Me) is β, then β=(1+α) / (1-α), so for example, when Li / Me is 1.5, α=0.2.

[0005] There is a demand for further miniaturization of non-aqueous electrolyte electricity storage elements from the viewpoints of loading space and portability. One means for solving this problem is to improve the electrode mix density (hereinafter referred to as "electrode density").

[0006] Patent Document 1 states that "By setting the average thickness of the flaky graphite to 0.5 μm or less, the deformability of the flaky graphite is improved, and the flaky graphite can be deformed according to the shape of the positive electrode active material, so that the density of the positive electrode active material layer can be improved" (paragraph 0019). And, lithium nickel composite oxide LiNi 0.8 Co 0.1 Mn 0.1 O2 is used as the positive electrode active material, and the "density of the positive electrode active material layer at the same linear pressure" is 3.60 g / cm 3 (Example 1, Table 1) However, Patent Document 1 does not disclose any improvement in electrode density when using an excess lithium type positive electrode active material.

[0007] In Tables 2 and 3 of Patent Document 2, a lithium-excess positive electrode active material having a Ni / Co / Mn ratio of 30 / 15 / 55 and a Li / Me ratio of 1.2 is used, and the "mixture density" is 2.56 g / cm 3 ~3.05g / cm 3 In addition, Table 4 shows a positive electrode in which the "mixture density" is 2.64 g / cm using lithium-excess positive electrode active materials of various compositions. 3 ~3.07g / cm 3 A positive electrode is described in which [Prior art documents] [Patent documents]

[0008] [Patent Document 1] WO2017 / 149927 [Patent Document 2] JP 2018-073752 A Summary of the Invention [Problem to be solved by the invention]

[0009] An object of the present invention is to provide a positive electrode that contains a lithium-excess positive electrode active material and has a high electrode density without impairing a high discharge capacity. [Means for solving the problem]

[0010] One aspect of the present invention is Composition formula Li 1+α Me 1-α O 2 (Me:Ni and Mn, or transition metals including Ni, Co and Mn), the molar ratio of Li to the transition metal (Me), Li / Me, (1+α) / (1-α) is greater than 1.1 and less than or equal to 1.5, and the molar ratio of Mn to the transition metal (Me) Mn / Me is greater than 0.5. The positive electrode active material includes a lithium excess type positive electrode active material, amorphous carbon, and graphite. and the content of the graphite is 2 mass% or less with respect to the mass of the positive electrode mixture layer. A positive electrode for a non-aqueous electrolyte storage element. Effect of the Invention

[0011] According to the present invention, it is possible to provide a positive electrode that contains a lithium-excess positive electrode active material and has a high electrode density without impairing a high discharge capacity, and a nonaqueous electrolyte electricity storage element using the same. [Brief description of the drawings]

[0012] [Figure 1] 1 is an external perspective view showing one embodiment of a nonaqueous electrolyte storage element. [Diagram 2] 1 is a schematic diagram showing one embodiment of an electricity storage device formed by assembling a plurality of nonaqueous electrolyte electricity storage elements. [Diagram 3] FIG. 1 is a diagram for explaining a presumed action mechanism of an embodiment. [Figure 4] 1 is a SEM image of the graphite powder used in the examples. [Diagram 5] FIG. 2 is an X-ray diffraction diagram of the pressed positive electrodes according to Example 1-1 and Comparative Example 1-1. [Figure 6] FIG. 4 is a graph showing the correlation between the peak differential pore volume of a positive electrode active material and the electrode density of a positive electrode. [Figure 7] FIG. 2 is a graph showing the correlation between the graphite content in a positive electrode and the electrode density, and between the graphite content in a positive electrode and the 2C discharge capacity of a nonaqueous electrolyte storage element. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] One aspect of the present invention Aspects teeth, Composition formula Li 1+α Me 1-α O 2 (Me:Ni and Mn, or transition metals including Ni, Co and Mn), the molar ratio of Li to the transition metal (Me), Li / Me, (1+α) / (1-α) is greater than 1.1 and less than or equal to 1.5, and the molar ratio of Mn to the transition metal (Me) Mn / Me is greater than 0.5. The positive electrode active material includes a lithium excess type positive electrode active material, amorphous carbon, and graphite. and the content of the graphite is 2 mass% or less with respect to the mass of the positive electrode mixture layer. A positive electrode for a non-aqueous electrolyte storage element.

[0014] Here, the lithium-excess type positive electrode active material has a peak differential pore volume of 0.5 mm 3 / (g nm) or more.

[0015] Another embodiment of the present invention is a nonaqueous electrolyte storage element using the above-described positive electrode for the nonaqueous electrolyte storage element.

[0016] The configuration and effects of the present invention will be explained together with the technical concept. However, the mechanism of action includes assumptions, and the correctness or incorrectness of such assumptions does not limit the present invention. The present invention can be embodied in various other forms without departing from its essence or main features. Therefore, the embodiments or examples described below are merely illustrative in all respects and should not be interpreted as being restrictive. Furthermore, all modifications and changes within the scope of the claims are within the scope of the present invention.

[0017] The positive electrode of the nonaqueous electrolyte storage element is completed by applying a positive electrode paste containing a positive electrode active material to a positive electrode substrate, drying the paste to form a positive electrode mixture layer, and then performing a pressing process. By increasing the pressing pressure in the pressing process, the electrode density can be increased.

[0018] As shown in the Reference Example described later, when a so-called "LiMeO2 type" active material having an α-NaFeO2 type crystal structure and a molar ratio of Li to transition metal (Me) (Li / Me) of less than 1.1 is used for the positive electrode, the maximum capacity is 3.3 g / cm 3However, although it depends on the thickness and composition of the positive electrode mixture layer, for example, when the content of the positive electrode active material in the positive electrode mixture is 90 mass % or more and the electrode density is 3.3 g / cm 3 In positive electrodes exceeding this value, the porosity of the positive electrode mixture layer decreases, and the permeability of the electrolyte decreases, resulting in a decrease in electrochemical properties such as charge / discharge cycle performance. Therefore, in positive electrodes using the so-called "LiMeO2-type" active material, there is no need to increase the electrode density any further.

[0019] On the other hand, as can be seen from the above Patent Documents 1 and 2, a positive electrode using a lithium-excess type positive electrode active material has a lower electrode density than a positive electrode using a so-called "LiMeO2 type" active material.

[0020] As a result of intensive research into the above problems, the present inventors have found that in a positive electrode using a lithium-excess positive electrode active material, the electrode density can be improved by using amorphous carbon and graphite as materials constituting the positive electrode mixture.

[0021] The mechanism of action of the present invention is presumed to be as follows. As shown in Table 1 below, the lithium-excess type positive electrode active material has a larger peak differential pore volume than the so-called "LiMeO2 type" active material. In addition, the total pore volume (cm 3 / g) is large, and the pore diameter (nm) at which the differential pore volume reaches its maximum is also large. From this, it is considered that the lithium-excess type positive electrode active material is composed of particles with a large number of pores with a large pore diameter compared to the so-called "LiMeO2 type" active material. Therefore, it is considered that a large frictional resistance occurs between the positive electrode active material particles that make up the positive electrode mixture layer and other constituent materials in the pressing process after applying a positive electrode paste containing the positive electrode active material to the positive electrode substrate and drying it to form a positive electrode mixture layer, and this is considered to be the reason why a positive electrode with a high electrode density cannot be obtained.

[0022] The mechanism by which the electrode density is improved by the configuration of the present invention will be described with reference to Fig. 3. Graphite has a structure in which graphene is regularly laminated. Therefore, when pressure is applied from the top and bottom of the figure as shown in Fig. 3(A), a shift occurs between the graphene layers as shown in Fig. 3(B), reducing the frictional resistance between the graphite and other constituent materials. As a result, it is believed that the electrode density can be improved compared to a system that does not contain graphite in the positive electrode.

[0023] It is also known to add carbon nanotubes to the positive electrode in order to improve the electrode density, but carbon nanotubes are very difficult to handle due to their poor dispersibility, and are also expensive.

[0024] A positive electrode for a nonaqueous electrolyte storage element according to one embodiment of the present invention will be described in detail below.

[0025] (Lithium-excess positive electrode active material) The lithium-excess type positive electrode active material according to this embodiment is typically represented by the composition formula Li 1+α Me 1-α O2 (Me:Ni and Mn, or transition metals including Ni, Co and Mn). In order to obtain a nonaqueous electrolyte storage element with a large discharge capacity, the molar ratio Li / Me of Li to the transition metal (Me), i.e., (1+α) / (1-α), is preferably greater than 1.1, more preferably 1.2 or more, and particularly preferably 1.3 or more. It is also preferably 1.5 or less, more preferably 1.45 or less, and particularly preferably 1.4 or less.

[0026] Since Ni has the effect of improving the discharge capacity of the active material, the molar ratio Ni / Me of Ni to the transition metal (Me) is preferably 0.15 or more, more preferably 0.25 or more, and particularly preferably 0.3 or more. The molar ratio Ni / Me is preferably less than 0.5, more preferably 0.45 or less, and particularly preferably 0.4 or less. From the viewpoint of material cost and because Mn has the effect of improving charge-discharge cycle performance, the molar ratio Mn / Me of Mn to the transition metal (Me) is preferably greater than 0.5, more preferably 0.6 or more, and particularly preferably 0.65 or more, and is preferably 0.8 or less, more preferably 0.75 or less, and particularly preferably 0.7 or less. Co has the effect of increasing the electronic conductivity of the active material particles and improving the high-rate discharge performance, but it is an optional element that is preferably present in small amounts in terms of charge / discharge cycle performance and economic efficiency. The molar ratio Co / Me of Co to the transition metal (Me) is preferably 0.20 or less, more preferably 0.15 or less, even more preferably 0.05 or less, and may be 0. Note that when a raw material containing Ni is used, Co may be contained as an impurity.

[0027] The peak differential pore volume of the lithium-excess positive electrode active material is 0.5 mm 3 / (g·nm) or more is preferable, and 0.6 mm 3 / (g·nm) or more is more preferable, and 0.7 mm 3 / (g nm) or more is even more preferable. From the viewpoint of charge-discharge cycle performance, 2.6 mm 3 / (g·nm) or less is preferable, 2.0mm 3 / (g·nm) or less is preferable, and 1.5 mm 3 / (g nm) or less is even more preferable. That is, the peak differential pore volume of the lithium-excess positive electrode active material is 0.5 to 2.6 mm from the viewpoint of discharge capacity and charge / discharge cycle performance. 3 / (g nm) is preferable, 0.6 to 2.0 mm 3 / (g nm) is more preferable, and 0.7 to 1.5 mm 3 / (g nm) is even more preferred.

[0028] The pore diameter at which the differential pore volume of the lithium-excess positive electrode active material exhibits a maximum value is preferably in the range of 20 to 150 nm, and more preferably in the range of 20 to 100 nm, from the viewpoints of discharge capacity and high-rate discharge performance.

[0029] The lower limit of the total pore volume of the lithium-excess positive electrode active material is 0.02 cm from the viewpoint of discharge capacity and high-rate discharge performance. 3 / g, and preferably 0.04 cm 3 / g, more preferably 0.06 cm 3 / g. The upper limit of the total pore volume is preferably 0.5 cm 3 / g, and 0.3 cm 3 / g, and 0.15 cm 3 / g.

[0030] The lithium-excess positive electrode active material can be synthesized by mixing and baking a compound containing a transition metal element and a lithium compound. The X-ray diffraction pattern of the powder after synthesis (before charging and discharging) using CuKα radiation shows diffraction peaks at 2θ=18.6±1°, 36.8±1°, and 44.0±1° originating from the crystal system belonging to the space group R3-m, as well as a superlattice peak at 2θ=20.8±1° originating from the crystal system belonging to the space group C2 / m, C2 / c, or P3112. The space group C2 / m, C2 / c, or P3112 is a crystal structure model in which the atomic positions of the 3a, 3b, and 6c sites in the space group R3-m are subdivided. Note that "R3-m" is originally written with a bar "-" on the "3" of "R3m".

[0031] The lithium-excess type positive electrode active material according to the present embodiment is preferably made of an alkali metal such as Na or K, an alkaline earth metal such as Mg or Ca, or a 3d transition metal such as Fe, within a range that does not significantly impair the characteristics of the material. It may contain small amounts of other metals, such as representative transition metals.

[0032] The surfaces of the primary particles and / or secondary particles of the lithium-excess positive electrode active material may be coated with and / or solid-dissolved with an aluminum compound. The presence of the aluminum compound on the particle surfaces prevents direct contact with the non-aqueous electrolyte, suppresses deterioration such as structural changes accompanying charge and discharge, and improves charge and discharge cycle performance.

[0033] As the positive electrode active material, a lithium-excess type positive electrode active material may be used alone, or two or more types of lithium-excess type positive electrode active materials having different physical properties may be mixed. In addition, as long as the effect of the present invention is not impaired, a positive electrode active material other than the lithium-excess type positive electrode active material may be mixed and used for the purpose of improving low-temperature characteristics, improving output characteristics, etc. In this case, the mixing ratio of the positive electrode active material other than the lithium-excess type positive electrode active material in the positive electrode active material may be 20 mass% or less.

[0034] The average particle size of the lithium-excess positive electrode active material is preferably 0.1 μm or more, more preferably 1 μm or more, and more preferably 5 μm or more. It is also preferably 20 μm or less. By setting the average particle size of the positive electrode active material to the above lower limit or more, the positive electrode active material can be easily manufactured or handled. By setting the average particle size of the positive electrode active material to the above upper limit or less, the electronic conductivity of the positive electrode mixture layer is improved. Here, the "average particle size" means a value at which the volume-based cumulative distribution calculated in accordance with JIS-Z-8819-2 (2001) is 50% based on the particle size distribution measured by the laser diffraction / scattering method for a diluted solution obtained by diluting particles with a solvent in accordance with JIS-Z-8825 (2013).

[0035] In this embodiment, the amorphous carbon used in the positive electrode is preferably carbon black. Examples of carbon black include furnace black, acetylene black, and ketjen black.

[0036] The lower limit of the amorphous carbon content in the positive electrode mixture layer is preferably 1 mass% and more preferably 2 mass% relative to the mass of the positive electrode mixture layer. The upper limit of the amorphous carbon content is preferably 7 mass% and more preferably 5 mass% relative to the mass of the positive electrode mixture layer. By setting the amorphous carbon content in the above range, the charge-discharge cycle performance can be improved.

[0037] The graphite used in the positive electrode according to this embodiment is a carbonaceous material that has a peak with a half-width of 0.6° or less at 2θ=26.4±1° in X-ray diffraction measurement using CuKα radiation. In an X-ray diffraction measurement using CuKα radiation, the half-width of the peak at 2θ=26.4±1° being 0.6° or less means that the graphene is regularly stacked in the c-axis direction and has high crystallinity. Therefore, when a compressive force is applied to an electrode containing a lithium-rich positive electrode active material, amorphous carbon, and graphite using a roll press or a flat press, the graphene layers are displaced, which is thought to improve the electrode density (see FIG. 3). The upper limit of the half-width of the peak at 2θ=26.4±1° is more preferably 0.5°, and even more preferably 0.4°.

[0038] The lower limit of the average particle size of the graphite used in the positive electrode is preferably 3 μm, more preferably 9 μm. The upper limit of the average particle size is preferably 16 μm, more preferably 13 μm. By setting the average particle size of the graphite in the above range, a positive electrode with excellent charge-discharge cycle performance can be provided. Here, the average particle size means a value at which the volume-based cumulative distribution calculated in accordance with JIS-Z-8819-2 (2001) is 50% based on the particle size distribution measured by a laser diffraction / scattering method for a diluted solution obtained by diluting particles with a solvent in accordance with JIS-Z-8825 (2013).

[0039] The lower limit of the BET specific surface area of ​​graphite used in the positive electrode is 3 m 2 / g is preferred, 4m 2 / g is more preferable. The upper limit of the BET specific surface area is 12 m 2 / g is preferred, and 10m 2 By setting the BET specific surface area of ​​the graphite in the above range, a positive electrode having excellent charge-discharge cycle performance can be provided.

[0040] The shape and type of graphite used in the positive electrode are not particularly limited, as shown in the examples described later. For example, it may be spherical graphite, massive graphite, scaly graphite, or flaky graphite. The shape of spherical graphite and massive graphite is significantly different from the shape of scaly graphite and flaky graphite in terms of aspect ratio. In general, the aspect ratio of spherical graphite and massive graphite is 1 or more and less than 10, and the aspect ratio of scaly graphite and flaky graphite is 10 or more and 25 or less. In this embodiment, graphite with an aspect ratio of 10 or more and 25 or less is preferred.

[0041] In the case of graphite having an aspect ratio of 10 to 25, the upper limit of the thickness may be 2 μm, 1 μm, or 0.5 μm. The thickness of the graphite can be determined, for example, from a cross-sectional SEM image of a positive electrode containing the graphite. The thickness of the graphite refers to the maximum dimension of the graphite particle in a direction perpendicular to the surface of the graphite particle when viewed from the direction in which the area of ​​the graphite particle is the largest.

[0042] The lower limit of the graphite content in the positive electrode mixture layer is preferably 0.2 mass% relative to the mass of the positive electrode mixture layer. By setting it to the lower limit or more, the electrode density can be improved. The upper limit of the graphite content is preferably 2 mass%, more preferably 1 mass%, and even more preferably 0.5 mass% relative to the mass of the positive electrode mixture layer. By setting it to the upper limit or less, the risk of the electrochemical properties being deteriorated can be reduced. Therefore, the graphite content in the positive electrode mixture layer is preferably 0.2 to 2 mass%, more preferably 0.2 to 1 mass%, and even more preferably 0.2 to 0.5 mass% relative to the mass of the positive electrode mixture layer. By setting the graphite content in the above range, the electrode density can be improved while the risk of the electrochemical properties being deteriorated can be reduced.

[0043] The lower limit of the graphite mass ratio (= graphite mass / (graphite mass+amorphous carbon mass))×100(%), which represents the mass ratio of amorphous carbon and graphite contained in the positive electrode mixture layer, is preferably 4%, and more preferably 6%. By setting it to the lower limit or higher, the electrode density of the positive electrode can be improved. Moreover, the upper limit of the graphite mass ratio is preferably 40%, more preferably 25%, and even more preferably 10%. By setting it to the upper limit or lower, the risk of deterioration of the electrochemical characteristics can be reduced.

[0044] <X-ray diffraction measurement> In this specification, the X-ray diffraction measurement is performed using an X-ray diffraction device manufactured by Rigaku (product number: RINT-TTR3) under the following conditions: the radiation source is CuKα, the X-ray output is 50 kV, 300 mA, the scan mode is CONTINUOUS, the step width is 0.02 deg, the scan speed is 4.0 deg / min, the entrance slit is 1 / 3 deg, the length limiting slit is 10 mm, the receiving slit 1 is 1 / 3 deg, and the receiving slit 2 is 0.3 mm.

[0045] <Peak differential pore volume measurement> In this specification, the peak differential pore volume measurement is measured by the following method. 1.00 g of the powder sample to be measured is placed in a sample tube for measurement and vacuum dried at 120°C for 6 hours and at 180°C for 6 hours to thoroughly remove moisture from the sample. Next, the adsorption and desorption isotherms are measured at relative pressures P / P0 (P0 = approximately 770 mmHg) ranging from 0 to 1 using a nitrogen gas adsorption method using liquid nitrogen. The desorption isotherm is then used to determine a cumulative pore volume curve by the BJH method. From this curve, the total pore volume (cm 3 / g) Next, the cumulative pore volume curve is linearly differentiated to obtain the pore diameter (nm) on the horizontal axis and the differential pore volume (mm 3A differential pore volume curve is obtained in which the peak differential pore volume is the maximum value of the differential pore volume curve. A large "peak differential pore volume" means that there are many pores with a certain pore diameter. In addition, in this specification, the "pore diameter at which the differential pore volume is at its maximum value" means that there is a large number of pores with a certain pore diameter.

[0046] <Measurement of average particle size> The measuring device used is the Microtrac (model number: MT3000) manufactured by Nikkiso Co., Ltd. The above measuring device consists of an optical bench, a sample supply unit, and a computer equipped with control software. A wet cell with a laser light transmission window is installed on the optical bench. The measurement principle is a method of irradiating a wet cell in which a dispersion liquid in which the sample to be measured is dispersed in a dispersion medium is circulating with laser light, and converting the scattered light distribution from the measurement sample into a particle size distribution. The above dispersion liquid is stored in the sample supply unit and circulated and supplied to the wet cell by a pump. Ethanol is used as the dispersion medium. Microtrac DHS for Win98 (MT3000) is used as the measurement control software. Regarding the "substance information" set and input to the above measuring device, "Reflection (REFLECTING)" is selected as the "transparency". Also, 1.36 is set as the "refractive index" of the solvent. Prior to measuring the sample, a "Set Zero" operation is performed. The "Set Zero" operation is an operation to subtract the influence of disturbance factors other than the scattered light from the particles (such as glass, dirt on the glass wall surface, glass unevenness, etc.) on the subsequent measurement. Only ethanol, which is the dispersion medium, is put into the sample supply unit, and background measurement is performed in a state where only ethanol, which is the dispersion medium, is circulating in the wet cell, and the background data is stored in the computer. Subsequently, a "Sample LD (Sample Loading)" operation is performed. The Sample LD operation is an operation to optimize the sample concentration in the dispersion liquid circulated and supplied to the wet cell during measurement, and it is an operation of manually injecting the sample to be measured into the sample supply unit according to the instructions of the measurement control software until the optimal amount is reached. Subsequently, the measurement operation is performed by pressing the "Measurement" button. The above measurement operation is repeated twice, and the measurement result is output from the control computer as the average value. The measurement result is obtained as the particle size distribution and the values of D10, D50, and D90 (D10, D50, and D90 are the particle sizes at which the cumulative volume in the particle size distribution of the secondary particles is 10%, 50%, and 90% respectively). The division width of the particle size distribution is set to 0.0376 for the particle size with the common logarithm of the horizontal axis and 0.01% for the frequency of the vertical axis. The obtained value of D50 is used as the average particle size.

[0047] <Measurement of BET Specific Surface Area> Using a Yuasa Ionics specific surface area measuring device (product name: MONOSORB), the amount of nitrogen adsorption (m 2 The amount of adsorption thus obtained is divided by the mass (g) of the sample to obtain the BET specific surface area (m 2 / g). For the measurement, gas adsorption is performed by cooling using liquid nitrogen. In addition, preheating is performed at 120°C for 15 minutes before cooling. The amount of the measurement sample is 0.2g ± 0.01g for graphite.

[0048] <Preparation of measurement sample> Samples to be used for each measurement of the positive electrode active material according to this embodiment and the active material contained in the positive electrode of the nonaqueous electrolyte storage element according to this embodiment are prepared according to the following procedures and conditions. If the sample to be subjected to the measurement is a powder sample prior to the preparation of a positive electrode, it is subjected to the measurement as it is. When taking samples from the positive electrode removed by dismantling a battery, before dismantling the battery, discharge the battery at a constant current (A) that is one-tenth of the current that passes the same amount of electricity as the nominal capacity (Ah) of the battery in one hour until the battery voltage reaches the lower limit of the specified voltage. If the battery is dismantled and uses a metallic lithium electrode as the negative electrode, No additional work is performed, and the positive electrode mixture taken from the positive electrode is the subject of measurement. In the case of a battery that does not use a metallic lithium electrode as the negative electrode, in order to accurately control the positive electrode potential, the battery is disassembled and the removed positive electrode is used as the working electrode, and a new battery is assembled with a metallic lithium electrode as the counter electrode. A constant current discharge is performed at a current value of 10 mA per 1 g of positive electrode mixture until the voltage reaches 2.0 V, and the battery is disassembled again after adjusting to a discharged state. The removed positive electrode is thoroughly washed to remove any non-aqueous electrolyte attached thereto using dimethyl carbonate, and the positive electrode mixture is collected from the positive electrode after drying at room temperature for a day and night. The work from disassembling the battery to disassembling it again, as well as the washing and drying of the positive electrode plate, are performed in an argon atmosphere with a dew point of -60°C or less. The sample to be subjected to the X-ray diffraction measurement is prepared by crushing the mixture in an agate mortar and then subjecting it to the measurement. The sample to be used for peak differential pore volume measurement is prepared by firing the mixture at 600° C. for 2 hours in a small electric furnace to remove the conductive agent and binder, and the resulting powder is used for measurement.

[0049] <Configuration of Nonaqueous Electrolyte Energy Storage Element> A nonaqueous electrolyte storage element (hereinafter also simply referred to as "storage element") according to one embodiment of the present invention includes a positive electrode, a negative electrode, and a nonaqueous electrolyte. As an example of the nonaqueous electrolyte storage element, a nonaqueous electrolyte secondary battery (hereinafter also simply referred to as "secondary battery") will be described.

[0050] (positive electrode) The positive electrode has a positive electrode substrate and a positive electrode mixture layer disposed on the positive electrode substrate directly or via an intermediate layer.

[0051] The positive electrode substrate has electrical conductivity. As the material of the positive electrode substrate, metals such as aluminum, titanium, tantalum, stainless steel, or alloys thereof are used. Among these, aluminum or aluminum alloys are preferred from the viewpoints of potential resistance, high electrical conductivity, and cost. Examples of the positive electrode substrate include foils and vapor deposition films, and foils are preferred from the viewpoint of cost. Therefore, aluminum foil or aluminum alloy foil is preferred as the positive electrode substrate. Examples of aluminum or aluminum alloys include A1085, A3003, etc., as specified in JIS-H-4000 (2014).

[0052] The lower limit of the average thickness of the positive electrode substrate is preferably 5 μm, more preferably 10 μm. The upper limit of the average thickness of the positive electrode substrate is preferably 30 μm, more preferably 20 μm. By making the average thickness of the positive electrode substrate equal to or greater than the lower limit, the strength of the positive electrode substrate can be increased. By making the average thickness of the positive electrode substrate equal to or less than the upper limit, the energy density per volume of the secondary battery can be increased. The "average thickness" refers to the average value of thicknesses measured at any ten points. The "average thickness" is defined similarly when used for other members, etc.

[0053] The intermediate layer is a layer disposed between the positive electrode substrate and the positive electrode mixture layer. The intermediate layer contains conductive particles such as carbon particles to reduce the contact resistance between the positive electrode substrate and the positive electrode mixture layer. The configuration of the intermediate layer is not particularly limited, and may contain, for example, a resin binder and conductive particles.

[0054] The positive electrode mixture layer contains a positive electrode active material and, as necessary, optional components such as a conductive agent, a binder, a thickener, and a filler.

[0055] In order to obtain powder in a desired shape, a pulverizer, a classifier, etc. are used. Examples of the pulverization method include a method using a mortar, a ball mill, a sand mill, a vibration ball mill, a planetary ball mill, a jet mill, a counter jet mill, a swirling airflow type jet mill, or a sieve. During pulverization, wet pulverization in the presence of water or an organic solvent such as hexane can also be used. As a classification method, a sieve, a wind classifier, etc. are used as necessary for both the dry and wet methods.

[0056] The lower limit of the content of the positive electrode active material in the positive electrode mixture layer is preferably 90 mass%, more preferably 93 mass%, and even more preferably 95 mass%, based on the mass of the positive electrode mixture layer. By making the content of the positive electrode active material equal to or greater than the lower limit, the discharge capacity can be increased. The upper limit of the content of the positive electrode active material is preferably 99 mass%, more preferably 97 mass%, based on the mass of the positive electrode mixture layer. By making the content of the positive electrode active material particles equal to or less than the upper limit, the production of the positive electrode becomes easier.

[0057] Examples of binders (binding agents) include thermoplastic resins such as fluororesins (polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF), etc.), polyethylene, polypropylene, and polyimide; elastomers such as ethylene-propylene-diene rubber (EPDM), sulfonated EPDM, styrene-butadiene rubber (SBR), and fluororubber; and polysaccharide polymers.

[0058] The lower limit of the binder content in the positive electrode mixture layer is preferably 1 mass % and more preferably 3 mass % relative to the mass of the positive electrode mixture layer. The upper limit of the binder content is preferably 7 mass % and more preferably 5 mass % relative to the mass of the positive electrode mixture layer. By setting the binder content within the above range, the active material can be stably held.

[0059] Examples of the thickener include polysaccharide polymers such as carboxymethyl cellulose (CMC), methyl cellulose, etc. When the thickener has a functional group that reacts with lithium or the like, this functional group may be deactivated in advance by methylation or the like.

[0060] The filler is not particularly limited, and examples of the filler include polyolefins such as polypropylene and polyethylene, silica, alumina, zeolite, glass, and aluminosilicate.

[0061] The positive electrode mixture layer may contain typical nonmetallic elements such as B, N, P, F, Cl, Br, and I, typical metallic elements such as Li, Na, Mg, Al, K, Ca, Zn, Ga, and Ge, and transition metallic elements such as Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Mo, Zr, Nb, and W as components other than the positive electrode active material, conductive agent, binder, thickener, and filler.

[0062] (Negative electrode) The negative electrode has a negative electrode substrate and a negative electrode mixture layer disposed on the negative electrode substrate directly or via an intermediate layer. The configuration of the intermediate layer is not particularly limited and can be selected from the configurations exemplified for the positive electrode.

[0063] The negative electrode substrate has electrical conductivity. The material of the negative electrode substrate is copper, nickel, stainless steel, nickel-plated steel, or an alloy thereof. Among these, copper or a copper alloy is preferred. The negative electrode substrate may be a foil, a vapor deposition film, or the like, and from the viewpoint of cost, a foil is preferred. Therefore, the negative electrode substrate is preferably a copper foil or a copper alloy foil. Examples of the copper foil include rolled copper foil and electrolytic copper foil.

[0064] The lower limit of the average thickness of the negative electrode substrate is preferably 3 μm, more preferably 5 μm. The upper limit of the average thickness of the negative electrode substrate is preferably 30 μm, more preferably 20 μm. By making the average thickness of the negative electrode substrate equal to or greater than the lower limit, the strength of the negative electrode substrate can be increased. By making the average thickness of the negative electrode substrate equal to or less than the upper limit, the energy density per volume of the secondary battery can be increased.

[0065] The negative electrode mixture layer contains a negative electrode active material. The negative electrode mixture layer may contain a conductive agent, a binder (a binder), etc., as necessary. The optional components, such as the conductive agent, binder, thickener, and filler, can be selected from the materials exemplified for the positive electrode above.

[0066] The negative electrode mixture layer may contain typical nonmetallic elements such as B, N, P, F, Cl, Br, and I, typical metallic elements such as Li, Na, Mg, Al, K, Ca, Zn, Ga, and Ge, and transition metallic elements such as Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Mo, Zr, Ta, Hf, Nb, and W as components other than the negative electrode active material, conductive agent, binder, thickener, and filler.

[0067] The negative electrode active material can be appropriately selected from known negative electrode active materials. A material capable of absorbing and releasing lithium ions is usually used as the negative electrode active material for lithium ion secondary batteries. Examples of the negative electrode active material include metal Li; metals or semimetals such as Si and Sn; metal oxides or semimetal oxides such as Si oxide, Ti oxide, and Sn oxide; and Li4Ti5O 12 , LiTiO 2、 Examples of the material include titanium-containing oxides such as TiNb2O7, polyphosphate compounds, silicon carbide, and carbon materials such as graphite and non-graphitic carbon (easily graphitized carbon or non-graphitizable carbon). Among these materials, graphite and non-graphitic carbon are preferred. In the negative electrode mixture layer, one of these materials may be used alone, or two or more of them may be used in combination.

[0068] The graphite used in the negative electrode has an average lattice spacing (d 002 ) is 0.33 nm or more and less than 0.34 nm. Examples of graphite include natural graphite and artificial graphite. Artificial graphite is preferred from the viewpoint of availability of materials with stable physical properties.

[0069] "Non-graphitic carbon" refers to carbon that has an average lattice spacing (d 002 ) is 0.34 nm or more and 0.42 nm or less. Examples of non-graphitizable carbon include non-graphitizable carbon and graphitizable carbon. Examples of non-graphitizable carbon include resin-derived materials, petroleum pitch or petroleum pitch-derived materials, petroleum coke or petroleum coke-derived materials, plant-derived materials, and alcohol-derived materials.

[0070] "Non-graphitizable carbon" means the above d 002 This refers to carbon materials with a particle size of 0.36 nm or more and 0.42 nm or less.

[0071] "Graphitizable carbon" means the above d 002 This refers to carbon materials with a particle size of 0.34 nm or more and less than 0.36 nm.

[0072] The average particle size of the negative electrode active material can be, for example, 1 μm or more and 100 μm or less. By setting the average particle size of the negative electrode active material to the above lower limit or more, the negative electrode active material can be easily manufactured or handled. By setting the average particle size of the negative electrode active material to the above upper limit or less, the electronic conductivity of the mixture layer is improved. In order to obtain the powder in a predetermined shape, a pulverizer, a classifier, or the like is used. The pulverization method and the powder classification method can be selected, for example, from the methods exemplified for the positive electrode above.

[0073] The lower limit of the content of the negative electrode active material in the negative electrode mixture layer is preferably 60 mass%, more preferably 80 mass%, and even more preferably 90 mass%. By making the content of the negative electrode active material equal to or greater than the lower limit, the electric capacity of the secondary battery can be increased. The upper limit of the content of the negative electrode active material is preferably 99 mass%, more preferably 98 mass%. By making the content of the negative electrode active material particles equal to or less than the upper limit, the production of the negative electrode becomes easier.

[0074] (Separator) The separator can be appropriately selected from known separators. For example, , a separator consisting of only a substrate layer, a separator in which a heat-resistant layer containing heat-resistant particles and a binder is formed on one or both surfaces of the substrate layer, etc. can be used. Examples of the material for the substrate layer of the separator include woven fabric, nonwoven fabric, and porous resin film. Among these materials, porous resin film is preferred from the viewpoint of strength, and nonwoven fabric is preferred from the viewpoint of non-aqueous electrolyte retention. As the material for the substrate layer of the separator, polyolefins such as polyethylene and polypropylene are preferred from the viewpoint of shutdown function, and polyimide and aramid are preferred from the viewpoint of oxidation decomposition resistance. A material in which these resins are combined may be used as the substrate layer of the separator.

[0075] The heat-resistant particles contained in the heat-resistant layer preferably have a weight loss of 5% or less at 500°C in air, and more preferably have a weight loss of 5% or less at 800°C in air. Examples of materials with a weight loss of a predetermined amount or less include inorganic compounds. Examples of inorganic compounds include oxides such as iron oxide, silicon oxide, aluminum oxide, titanium oxide, barium titanate, zirconium oxide, and aluminum oxide-silicon oxide composite oxide; nitrides such as aluminum nitride and silicon nitride; poorly soluble ion crystals such as calcium fluoride, barium fluoride, and barium sulfate; covalent crystals such as silicon and diamond; mineral resource-derived substances such as talc, montmorillonite, boehmite, zeolite, apatite, kaolin, mullite, spinel, olivine, sericite, bentonite, and mica, or artificial products thereof. As the inorganic compound, a single substance or a complex of these substances may be used alone, or two or more types may be mixed and used. Among these inorganic compounds, silicon oxide, aluminum oxide, or aluminum oxide-silicon oxide composite oxide is preferable.

[0076] The porosity of the separator is preferably 80% by volume or less from the viewpoint of strength, and is preferably 20% by volume or more from the viewpoint of discharge performance. Here, "porosity" refers to a volume-based value measured with a mercury porosimeter.

[0077] As the separator, a polymer gel composed of a polymer and a non-aqueous electrolyte may be used. Examples of the polymer include polyacrylonitrile, polyethylene oxide, polypropylene oxide, polymethyl methacrylate, polyvinyl acetate, polyvinylpyrrolidone, and polyvinylidene fluoride. The use of the polymer gel has an effect of suppressing leakage. As the separator, the above-mentioned porous resin film or nonwoven fabric may be used in combination with the polymer gel.

[0078] (Non-aqueous electrolyte) The nonaqueous electrolyte may be appropriately selected from known nonaqueous electrolytes. The nonaqueous electrolyte may be a nonaqueous electrolyte solution. The nonaqueous electrolyte solution includes a nonaqueous solvent and an electrolyte salt dissolved in the nonaqueous solvent.

[0079] The non-aqueous solvent can be appropriately selected from known non-aqueous solvents. Examples of the non-aqueous solvent include cyclic carbonates, chain carbonates, carboxylates, phosphates, sulfonates, ethers, amides, and nitriles. As the non-aqueous solvent, those in which some of the hydrogen atoms contained in these compounds are substituted with halogens may be used.

[0080] Examples of cyclic carbonates include ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), vinylene carbonate (VC), vinylethylene carbonate (VEC), chloroethylene carbonate, fluoroethylene carbonate (FEC), difluoroethylene carbonate (DFEC), styrene carbonate, 1-phenylvinylene carbonate, 1,2-diphenylvinylene carbonate, etc. Among these, EC is preferred.

[0081] Examples of the chain carbonate include diethyl carbonate (DEC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), diphenyl carbonate, trifluoroethyl methyl carbonate, bis(trifluoroethyl) carbonate, etc. Among these, EMC is preferable.

[0082] As the non-aqueous solvent, it is preferable to use a cyclic carbonate or a chain carbonate, and it is more preferable to use a combination of a cyclic carbonate and a chain carbonate. By using a cyclic carbonate, it is possible to promote dissociation of the electrolyte salt and improve the ionic conductivity of the non-aqueous electrolyte. By using a chain carbonate, it is possible to keep the viscosity of the non-aqueous electrolyte low. When using a cyclic carbonate and a chain carbonate in combination, it is preferable that the volume ratio of the cyclic carbonate to the chain carbonate (cyclic carbonate:chain carbonate) is, for example, in the range of 5:95 to 50:50.

[0083] The electrolyte salt can be appropriately selected from known electrolyte salts. Examples of the electrolyte salt include lithium salts, sodium salts, potassium salts, magnesium salts, onium salts, etc. Among these, lithium salts are preferred.

[0084] Examples of the lithium salt include inorganic lithium salts such as LiPF6, LiPO2F2, LiBF4, LiClO4, and LiN(SO2F)2, and lithium salts having a halogenated hydrocarbon group such as LiSO3CF3, LiN(SO2CF3)2, LiN(SO2C2F5)2, LiN(SO2CF3)(SO2C4F9), LiC(SO2CF3)3, and LiC(SO2C2F5)3. Among these, inorganic lithium salts are preferred, and LiPF6 is more preferred.

[0085] The lower limit of the content of the electrolyte salt in the nonaqueous electrolyte solution is preferably 0.1 mol / L, more preferably 0.3 mol / L, even more preferably 0.5 mol / L, and particularly preferably 0.7 mol / L. The upper limit of the content of the electrolyte salt is, for example, preferably 2.5 mol / L, more preferably 2 mol / L, and even more preferably 1.5 mol / L.

[0086] The non-aqueous electrolyte may contain an additive. Examples of the additive include halogenated carbonate esters such as fluoroethylene carbonate (FEC) and difluoroethylene carbonate (DFEC); salts having an oxalic acid group such as lithium bis(oxalate)borate (LiBOB), lithium difluorooxalateborate (LiFOB), and lithium bis(oxalate)difluorophosphate (LiFOP); imide salts such as lithium bis(fluorosulfonyl)imide (LiFSI); aromatic compounds such as biphenyl, alkylbiphenyl, terphenyl, partially hydrogenated terphenyl, cyclohexylbenzene, t-butylbenzene, t-amylbenzene, diphenyl ether, and dibenzofuran; partial halides of the above aromatic compounds such as 2-fluorobiphenyl, o-cyclohexylfluorobenzene, and p-cyclohexylfluorobenzene; 2,4-difluoroanisole, 2,5-difluoroanisole, 2,6-difluoroanisole, 3,5-difluoroanisole, 4,5-difluoroanisole, 5,5-difluoroanisole, 6,5-difluoroanisole, 7,5-difluoroanisole, 8,5-difluoroanisole, 9,5-difluoroanisole, 10,5-difluoroanisole, 11,5-difluoroanisole, 12,5-difluoroanisole, 13,5-difluoroanisole, 14,5-difluoroanisole, 15,5-difluoroanisole, 16,5-difluoroanisole, 17,5-difluoroanisole, 18,5-difluoroanisole, 19,5-difluoroanisole, 20,5-difluoroanisole, 21,5-difluoroanisole, 22,5-difluoroanisole, 23,5-difluoroanisole, 24,5-difluoroanisole, 25,5-difluoroanisole Halogenated anisole compounds such as difluoroanisole; vinylene carbonate, methyl vinylene carbonate, ethyl vinylene carbonate, succinic anhydride, glutaric anhydride, maleic anhydride, citraconic anhydride, glutaconic anhydride, itaconic anhydride, cyclohexane dicarboxylic anhydride; ethylene sulfite, propylene sulfite, dimethyl sulfite, propane sultone, propene sultone, butane sultone, methyl methanesulfonate, busulfan, methyl toluenesulfonate, dimethyl sulfate, ethylene sulfate, sulfolane, dimethyl sulfone, diethyl sulfone, dimethyl sulfoxide, diethyl sulfoxide, tetramethylene sulfoxide, diphenyl sulfide, 4,4'-bis(2,2-dioxo-1,3,2-dioxathiolane, 4-methylsulfonyloxymethyl-2,2-dioxo-1,3,2-dioxathiolane, thioanisole, diphenyl disulfide, dipyridinium disulfide, perfluoro Examples of the additives include tetrakis(trimethylsilyl) borate, tris(trimethylsilyl) phosphate, tetrakis(trimethylsilyl) titanate, lithium monofluorophosphate, lithium difluorophosphate, etc. These additives may be used alone or in combination of two or more.

[0087] The lower limit of the content of these additives in the entire non-aqueous electrolyte is preferably 0.01% by mass, more preferably 0.1% by mass, and even more preferably 0.2% by mass. The upper limit of the content of the additives is preferably 10% by mass, more preferably 7% by mass, more preferably 5% by mass, and even more preferably 3% by mass. By setting the content of the additives within the above range, it is possible to improve the capacity retention performance or charge / discharge cycle performance after high-temperature storage, and to further improve safety.

[0088] The non-aqueous electrolyte may be a solid electrolyte, or a non-aqueous electrolyte solution and a solid electrolyte may be used in combination.

[0089] The solid electrolyte can be selected from any material that has ion conductivity such as lithium, sodium, calcium, etc., and is solid at room temperature (for example, 15° C. to 25° C.) Examples of the solid electrolyte include sulfide solid electrolytes, oxide solid electrolytes, oxynitride solid electrolytes, polymer solid electrolytes, etc.

[0090] In the case of a lithium ion secondary battery, the sulfide solid electrolyte may be, for example, a Li2S-P2S5 system. Examples of the sulfide solid electrolyte include Li2S-P2S5, LiI-Li2S-P2S5, and Li 10 Ge-P2S 12 , etc.

[0091] The shape of the energy storage element of this embodiment is not particularly limited, and examples thereof include a cylindrical battery, a laminate film battery, a square battery, a flat battery, a coin battery, and a button battery. 1 shows an example of a square nonaqueous electrolyte secondary battery as one embodiment of the energy storage element of the present invention. An electrode assembly 2 having a positive electrode and a negative electrode wound with a separator sandwiched therebetween is housed in a square case 3. The positive electrode is electrically connected to a positive electrode terminal 4 via a positive electrode lead 4'. The negative electrode is electrically connected to a negative electrode terminal 5 via a negative electrode lead 5'.

[0092] <Configuration of Nonaqueous Electrolyte Electricity Storage Device> The energy storage element of this embodiment can be mounted as an energy storage unit (battery module) formed by assembling a plurality of energy storage elements 1 in a power source for an automobile such as an electric vehicle (EV) or a plug-in hybrid vehicle (PHEV), a power source for electronic devices such as a personal computer or a communication terminal, or a power storage power source, etc. In this case, the technology of the present invention may be applied to at least one energy storage element included in the energy storage device. 2 shows an example of an energy storage device 30 in which energy storage units 20, each of which is an assembly of two or more electrically connected energy storage elements 1, are further assembled. The energy storage device 30 may include a bus bar (not shown) that electrically connects the two or more energy storage elements 1, and a bus bar (not shown) that electrically connects the two or more energy storage units 20. The energy storage units 20 or the energy storage device 30 may include a status monitoring device (not shown) that monitors the status of the one or more energy storage elements.

[0093] <Method of Manufacturing Nonaqueous Electrolyte Storage Element> The method for producing the energy storage element of the present embodiment can be appropriately selected from known methods. The method for producing the energy storage element of the present embodiment includes, for example, a step of preparing an electrode body, a step of preparing a non-aqueous electrolyte, and a step of housing the electrode body and the non-aqueous electrolyte in a container. The step of preparing the electrode body includes a step of preparing a positive electrode and a negative electrode, and a step of forming the electrode body by stacking or rolling the positive electrode and the negative electrode with a separator interposed therebetween.

[0094] The step of placing the non-aqueous electrolyte in the container can be appropriately selected from known methods. For example, when a non-aqueous electrolyte solution is used as the non-aqueous electrolyte, the non-aqueous electrolyte solution may be injected through an injection port formed in the container, and then the injection port may be sealed.

[0095] <Other embodiments> The energy storage element of the present invention is not limited to the above-described embodiment, and various modifications may be made without departing from the scope of the present invention. For example, the configuration of one embodiment may be added to the configuration of another embodiment, and a part of the configuration of one embodiment may be replaced with the configuration of another embodiment or a well-known technique. Furthermore, a part of the configuration of one embodiment may be deleted. Also, a well-known technique may be added to the configuration of one embodiment.

[0096] In the above embodiment, the case where the storage element is used as a chargeable and dischargeable non-aqueous electrolyte secondary battery (e.g., a lithium ion secondary battery) has been described, but the storage element may be of any type, shape, size, capacity, etc. The present invention can also be applied to various secondary batteries, primary batteries, electric double layer capacitors, lithium ion capacitors, and other capacitors. EXAMPLES

[0097] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples.

[0098] [Preparation of lithium-excess positive electrode active material (LR1)] <Synthesis of lithium-excess positive electrode active material> 17.7 g of nickel sulfate hexahydrate and 32.5 g of manganese sulfate pentahydrate were weighed, and the total amount was dissolved in 200 mL of ion-exchanged water to prepare a 1.0 mol / L sulfate aqueous solution with a molar ratio of Ni:Mn of 33.3:66.7. Meanwhile, 750 mL of ion-exchanged water was poured into a 2 L reaction vessel, and CO2 gas was bubbled for 30 min to dissolve CO2 in the ion-exchanged water. The temperature of the reaction vessel was set to 50°C (±2°C), and the above sulfate aqueous solution was dripped at a rate of 2 mL / min while stirring the inside of the reaction vessel at a rotation speed of 700 rpm using a paddle blade equipped with a stirring motor. Here, the pH in the reaction vessel was controlled to always be kept at 7.9 (±0.05) by appropriately dripping an aqueous solution containing 1.0 mol / L of sodium carbonate from the start to the end of the drip. After the dripping was completed, stirring in the reaction vessel was continued for another 5 h. After stirring was stopped, the mixture was allowed to stand for 12 hours or more. Next, the coprecipitated carbonate particles formed in the reaction tank were separated using a suction filter, and sodium ions attached to the particles were washed off using ion-exchanged water. The particles were then dried in an air atmosphere at normal pressure and 80°C for 20 hours using an electric furnace. After that, the particles were ground in an agate mortar for several minutes to make the particle size uniform. In this way, the coprecipitated carbonate precursor was produced.

[0099] 1.2 g of lithium carbonate was added to 2.8 g of the above coprecipitated carbonate precursor, and mixed thoroughly using an agate mortar to prepare a mixed powder with a molar ratio of Li:Me (total of Ni and Mn) of 1.33. Using a pellet molding machine, the mixture was molded at a pressure of 40 MPa to obtain a pellet with a diameter of 25 mm. The amount of the mixed powder used for pellet molding was determined by converting it so that the mass of the expected final product was 2.5 g. One of the above pellets was placed on the lid of an alumina crucible with a total length of about 50 mm, placed in a box-type electric furnace (model number: AMF20), and heated from room temperature to a temperature of 890°C over 10 hours in an air atmosphere under normal pressure, and fired at the temperature after the temperature increase for 9 hours. The internal dimensions of the box-type electric furnace were 10 cm long, 20 cm wide, and 30 cm deep, with heating wires spaced 20 cm apart in the width direction. After firing, the heater was turned off and the alumina crucible was left in the furnace with the lid on, and allowed to cool naturally. As a result, the temperature of the furnace dropped to about 200°C after 5 hours, but the rate of temperature drop thereafter was somewhat slow. After a day and night, it was confirmed that the temperature of the furnace was below 100°C, and the pellets were then taken out and crushed in an agate mortar for several minutes to make the particle size uniform. In this way, the lithium-excess positive electrode active material Li 1.14 Ni 0.29 Mn 0.57 O2 (Li / Me=1.33) was produced.

[0100] <Aluminum treatment of lithium-excess positive electrode active material> Aluminum sulfate hydrate and ion-exchanged water were mixed in a 300 mL Erlenmeyer flask to prepare an aluminum sulfate aqueous solution with an aluminum sulfate concentration of 0.5 mol / L. The aluminum sulfate aqueous solution was stirred at 25°C and 400 rpm using a stirrer, and 5.0 g of the lithium-excess positive electrode active material was added. After 30 seconds from the addition of the lithium-excess positive electrode active material, the lithium-excess positive electrode active material was collected on a filter paper by suction filtration. This lithium-excess type positive electrode active material was dried in air at normal pressure and 80° C. for 20 hours using a dryer to obtain an aluminum-treated lithium-excess type positive electrode active material.

[0101] <Heat treatment of aluminum-treated lithium-rich positive electrode active material> The above aluminum-treated lithium-rich positive electrode active material was placed on the lid of an alumina crucible, which was then placed in a box-type electric furnace (model number: AMF20) and heat-treated in air at a temperature rise rate of 5°C / min, a heat treatment temperature of 400°C, and a holding time of 4 hours to obtain an aluminum-coated lithium-rich positive electrode active material according to Example 1-1 (hereinafter referred to as "LR1"). The Li / Me of LR1 was 1.33, and the peak differential pore volume measured under the above conditions was 0.98 mm 3 / (g nm).

[0102] [Preparation of positive electrode active material (LR2)] A lithium-excess positive electrode active material Li according to Example 1-5 was prepared in the same manner as in Example 1-1, except that the firing temperature of the pellets in which the coprecipitated carbonate precursor and lithium carbonate were mixed was changed to 930°C. 1.14 Ni 0.29 Mn 0.57 The Li / Me ratio of LR2 was 1.33, and the peak differential pore volume measured under the above conditions was 0.72 mm 3 / (g nm).

[0103] [Preparation of positive electrode active material (LR3)] The molar ratio of Ni:Co:Mn in the coprecipitated carbonate precursor was changed to 19.5:12.3:68.2, and the precursor was used to prepare a mixed powder having a molar ratio of Li:Me (the sum of Ni, Co, and Mn) of 1.38. The pellets formed from the mixed powder were fired at 900° C., and the lithium-excess positive electrode active material Li according to Example 1-6 was prepared in the same manner as in Example 1-1. 1.17 Ni 0.16 Co 0.1 Mn 0.57 LR3 was prepared. Cobalt sulfate heptahydrate was used as the Co source. The Li / Me ratio of LR3 was 1.38, and the peak differential pore volume measured under the above conditions was 2.53 mm 3 / (g nm).

[0104] [Preparation of Positive Electrode According to Example 1-1] LR1 was used as the positive electrode active material, acetylene black (AB) was used as the amorphous carbon, flake graphite was used as the graphite, and polyvinylidene fluoride (PVdF) was used as the binder. A positive electrode paste was prepared containing the positive electrode active material, amorphous carbon, graphite, and binder in a ratio of 95.5:2.5:0.5:1.5 (solid equivalent) and N-methylpyrrolidone (NMP) as the dispersion medium. This positive electrode paste was applied to one side of aluminum foil, which is the positive electrode substrate. It was then dried at 100°C for 1 hour to remove the NMP from the electrode plate.

[0105] [Preparation of Positive Electrodes According to Examples 1-2 to 1-4] Positive electrodes according to Examples 1-2 to 1-4 were produced in the same manner as in Example 1-1, except that the graphite was changed from flaky graphite to flake graphite, spherical graphite, and lump graphite, respectively.

[0106] [Preparation of Positive Electrode According to Comparative Example 1-1] A positive electrode according to Comparative Example 1-1 was produced in the same manner as in Example 1-1, except that no graphite was used and the ratio of positive electrode active material: amorphous carbon: binder was 95.5:3.0:1.5 (solids equivalent).

[0107] [Preparation of Positive Electrodes According to Examples 1-5 and Comparative Examples 1-2] Positive electrodes according to Example 1-5 and Comparative Example 1-2 were produced in the same manner as in Example 1-1 and Comparative Example 1-1, except that the positive electrode active material was changed to the above-mentioned LR2.

[0108] [Preparation of Positive Electrodes According to Examples 1-6 and Comparative Examples 1-3] Positive electrodes according to Example 1-6 and Comparative Example 1-3 were produced in the same manner as in Example 1-1 and Comparative Example 1-1, except that the positive electrode active material was LR3.

[0109] [Preparation of Positive Electrodes According to Reference Examples 1-1 to 1-4] The positive electrode active material was the commercially available positive electrode active material LiNi 0.5 Co 0.2 Mn 0.3 O2 (hereinafter referred to as "NCM523"), or LiNi 0.33 Co 0.33 Mn 0.33 Except for using NCM111 (hereinafter referred to as "NCM111"), positive electrodes according to Reference Examples 1-1 and 1-3 were prepared in the same manner as in Example 1-1. In addition, positive electrodes according to Reference Examples 1-2 and 1-4 were prepared in the same manner as in Comparative Example 1-1. In addition, the peak differential pore volumes of these positive electrode active materials were also measured under the above conditions.

[0110] SEM images of flake graphite, scaly graphite, spherical graphite, and lump graphite are shown in Figure 4. In addition, the average particle size and BET specific surface area of ​​these graphites were determined under the above conditions.

[0111] <Press Test> A press test was carried out on the positive electrodes according to the above Examples 1-1 to 1-6, Comparative Examples 1-1 to 1-3, and Reference Examples 1-1 to 1-4. The plate before pressing is 2 x 2 cm 2 After punching out the electrode, roll pressing was performed at room temperature. Specifically, the electrode was passed through the press machine several times until there was no change in thickness. 3Here, the electrode density was calculated by subtracting the mass of the positive electrode substrate (unit: g) from the mass of the positive electrode substrate (unit: cm). 3 ) is the result.

[0112] <X-ray diffraction measurement> The positive electrodes according to Example 1-1 and Comparative Example 1-1 were pressed, and X-ray diffraction measurements were performed using a Cu tube under the above conditions. The results are shown in FIG. 5. In Example 1-1, a peak derived from graphite was observed near 26.4°. The half-width of this peak was 0.4° or less. Furthermore, as a result of X-ray diffraction measurements of the flake graphite, scaly graphite, spherical graphite, and lump graphite powder before use in the electrodes according to Examples 1-1 to 1-4, the half-width of the peak near 26.4° was 0.4° or less in all cases.

[0113] Tables 1 to 3 show the properties of the positive electrode active materials and graphite used in the positive electrodes of Examples 1-1 to 1-6, Comparative Examples 1-1 to 1-3, and Reference Examples 1-1 to 1-4, the composition ratios of the positive electrode mixtures, and the electrode densities of the obtained positive electrodes.

[0114] [Table 1]

[0115] [Table 2]

[0116] [Table 3]

[0117] Comparing Comparative Example 1-1 with Examples 1-1 to 1-4, it was found that by reducing the amount of amorphous carbon AB by 0.5 mass% and using 0.5 mass% graphite instead, the electrode density was improved regardless of the shape and physical properties of the graphite. In particular, the spherical graphite used in Example 1-3 had an average particle size of about 12 μm, which was large, but it still achieved the effect of improving the electrode density. This shows that the improvement in electrode density due to the use of graphite is due to factors other than the shape of the graphite. It is suggesting.

[0118] That is, the graphite powder used in the positive electrodes of Examples 1-1 to 1-4 all have an X-ray diffraction peak with a half-width of 0.4° or less at around 26.4°, and the graphite has high crystallinity. Therefore, when the electrode was pressed, slippage occurred between the graphene layers of the graphite, which is thought to have improved the electrode density. Among the graphites, the electrode density was most improved when flaky graphite was used. This is thought to be because the flaky graphite entered the gaps between the positive electrode active material particles and was deformed when pressure was applied.

[0119] Comparing Example 1-5 with Comparative Example 1-2, or Example 1-6 with Comparative Example 1-3, when LR2 and LR3, which have different peak differential pore volumes and active material compositions, were used as the positive electrode active materials, an improvement in electrode density was observed similar to when LR1 was used.

[0120] From Reference Examples 1-1 to 1-4, when NCM523 and NCM111 were used as the positive electrode active material, the electrode density was 3.3 g / cm 3 The results show that the density of the positive electrode is significantly higher than that of the positive electrode with excess lithium.

[0121] [Evaluation of electrochemical properties] The electrochemical characteristics of the positive electrodes for which good results were obtained as described above were evaluated. A positive electrode was prepared in the same manner as in Example 1-1, except that LR1 was used as the positive electrode active material, flake graphite was used as the graphite type, and the contents of AB and graphite were as shown in Table 4. The positive electrode was pressed to obtain a pressed positive electrode.

[0122] [Preparation of test cells according to Examples 2-1 to 2-4 and Comparative Example 2-1 (negative electrode: metallic lithium)] Using the pressed positive electrode, a test cell was prepared in the following procedure. As the non-aqueous electrolyte (electrolytic solution), a solution was used in which LiPF6 was dissolved in a mixed solvent in which fluoroethylene carbonate and 2,2,2-trifluoroethyl methyl carbonate were mixed in a volume ratio of 3:7, so that the concentration was 1 mol / L. As the separator, a microporous membrane made of polypropylene with a surface modification by polyacrylate was used. Metallic lithium was used for the negative electrode. As the exterior body, a metal resin composite film made of polyethylene terephthalate (15 μm) / aluminum foil (50 μm) / metal adhesive polypropylene film (50 μm) was used, and the electrodes were stored so that the open ends of the positive electrode terminal and the negative electrode terminal were exposed to the outside, and the fusion margin where the inner surfaces of the metal resin composite film faced each other was hermetically sealed except for the part that became the liquid injection hole, and the above-mentioned electrolyte was injected, and the liquid injection hole was sealed.

[0123] [Capacity verification test (negative electrode: metallic lithium)] The above test cell was subjected to a capacity confirmation test in a thermostatic chamber at 25° C. according to the following procedure. (1) Charging process The battery was charged at a constant current and constant voltage with a charging current of 0.1 C and a charging voltage of 4.7 V. The charging was terminated when the current attenuated to 0.05 C. After charging was completed, the battery was rested for 10 minutes. (2)Discharge process A constant current discharge was performed with a discharge cut-off voltage of 2.0 V. After the discharge was completed, a 10-minute pause was performed.

[0124] The above (1) charging step and (2) discharging step were counted as one charging / discharging step, and this charging / discharging step was repeated three times. The discharge current was 0.1 C for the first and second discharges, and 2 C for the third discharge. The second discharge capacity (mAh) was divided by the mass of the positive electrode active material contained in the positive electrode and recorded as the "0.1C discharge capacity (mAh / g, lithium counter electrode)". Similarly, the third discharge capacity (mAh) was divided by the mass of the positive electrode active material contained in the positive electrode and recorded as the "2C discharge capacity (mAh / g, lithium counter electrode)".

[0125] [Preparation of test cells according to Examples 2-1 to 2-3 and Comparative Example 2-1 (negative electrode: graphite)] Graphite was used as the negative electrode active material, carboxymethyl cellulose was used as the binder, and styrene butadiene rubber was used as the thickener. A negative electrode paste was prepared containing the negative electrode active material, binder, and thickener in a mass ratio (solid content equivalent) of 96.7:2.1:1.2, with water as the dispersion medium. This negative electrode paste was applied onto copper foil, which was the negative electrode substrate, and then dried and pressed to prepare a graphite negative electrode.

[0126] Test cells using graphite negative electrodes according to Examples 2-1 to 2-3 and Comparative Example 2-1 were produced in the same manner as above, except that the graphite negative electrode was used instead of metallic lithium.

[0127] [Capacity verification test (negative electrode: graphite)] The above test cell was subjected to the following capacity confirmation test in a thermostatic chamber at 25° C. according to the following procedure. (1') Charging process Constant-current, constant-voltage charging was performed with a charging current of 0.1 C and a charging voltage of 4.6 V. The charging termination condition was when the current attenuated to 0.05 C. After charging was completed, a 10-minute break was performed. (2') Discharge process A constant current discharge was performed with a discharge current of 0.1 C and a discharge cut-off voltage of 2.0 V. After the discharge was completed, a 10-minute pause was performed.

[0128] The (1') charging step and the (2') discharging step were counted as one charging / discharging step, and this charging / discharging step was repeated twice. The second discharge capacity was recorded as the "initial discharge capacity."

[0129] [Charge-discharge cycle test (negative electrode: graphite)] The test cells used in the capacity confirmation test were subjected to a charge-discharge cycle test in a thermostatic chamber at 25° C. according to the following procedure. (1'') Charging process The battery was charged at a constant current and constant voltage with a charging current of 0.5 C and a charging voltage of 4.6 V. The charging was terminated when the current attenuated to 0.1 C. After charging was completed, a 10-minute break was taken. (2'')Discharge process A constant current discharge was performed with a discharge current of 1 C and a discharge cut-off voltage of 2.0 V. After discharge was completed, a 10-minute pause was performed.

[0130] The (1'') charging step and the (2'') discharging step were counted as one charging / discharging step, and this charging / discharging step was repeated 50 times.

[0131] [Capacity confirmation test after charge / discharge cycle test] After the charge-discharge cycle test, the cells were discharged at a constant current of 0.1 C and a discharge cut-off voltage of 2.0 V, and then charged and discharged once in the same manner as in the "Capacity Verification Test (Graphite Counter Electrode)". The capacity at this time was recorded as the "Discharge Capacity after 50 Cycles". The percentage of the "Discharge Capacity after 50 Cycles" to the "Initial Discharge Capacity" was calculated as the "Retention Rate after 50 Cycles (%, Graphite Counter Electrode)".

[0132] For each example and comparative example, the "electrode density (g / cm 3 ), "0.1C discharge capacity (mAh / g, lithium counter electrode)", "2C discharge capacity (mAh / g, lithium counter electrode)", and "retention rate after 50 cycles (%, graphite counter electrode)" are shown in Table 4. Figure 7 shows the relationship between the graphite content in the positive electrode, the electrode density, and the 2C discharge capacity of the nonaqueous electrolyte storage element. Here, the electrode density is shown by "● (first axis)" and the 2C discharge capacity by "△ (second axis)".

[0133] [Table 4]

[0134] 7, in Examples 2-1 to 2-4 using positive electrodes containing 0.2 to 2 mass % of graphite, the effect of improving the electrode density was confirmed compared to Comparative Example 2-1. Also, as shown in Table 4, it was confirmed that Examples 2-1 to 2-3 exhibited excellent discharge performance and charge / discharge cycle performance equivalent to Comparative Example 2-1.

[0135] That is, by using amorphous carbon and graphite in a positive electrode containing a lithium-excess positive electrode active material, it is possible to improve the electrode density without impairing high discharge performance and charge / discharge cycle performance. [Industrial Applicability]

[0136] The present invention can provide a positive electrode having a high electrode density without impairing high discharge capacity. Therefore, a nonaqueous electrolyte storage element using this positive electrode is useful not only for portable devices such as mobile phones and personal computers, but also as an on-board rechargeable battery for electric vehicles (EVs), plug-in hybrid vehicles (PHVs), and the like. [Explanation of symbols]

[0137] 1 Nonaqueous electrolyte secondary battery 2 electrode groups 3 Battery container 4 Positive terminal 4' Positive lead 5 Negative terminal 5' Negative lead 20 Energy Storage Unit 30 Energy storage device

Claims

1. Composition formula Li 1+α Me 1-α O 2 a lithium-excess type positive electrode active material represented by the formula Me: (Me: transition metal containing Ni and Mn, or Ni, Co and Mn), in which the molar ratio of Li to the transition metal (Me), Li / Me, (1+α) / (1-α), is greater than 1.1 and not greater than 1.5, and the molar ratio of Mn to the transition metal (Me) Mn / Me is greater than 0.5; amorphous carbon; and graphite, in which the graphite content is 2 mass% or less with respect to the mass of the positive electrode mixture layer.

2. The peak differential pore volume of the lithium-excess positive electrode active material is 0.5 mm 3 2. The positive electrode for a nonaqueous electrolyte storage element according to claim 1, wherein the surface area of ​​the positive electrode is 100 nm or more.

3. A non-aqueous electrolyte storage element comprising the positive electrode for a non-aqueous electrolyte storage element according to claim 1 or 2.

Citation Information

Patent Citations

  • Positive electrode active material for nonaqueous electrolyte secondary battery, nonaqueous electrolyte secondary battery, and manufacturing method of positive electrode active material for nonaqueous electrolyte secondary battery

    JP2009016302A

  • Positive electrode active material for lithium secondary battery, positive electrode and secondary battery

    JP2015118945A

  • Positive electrode active material, method for manufacturing the same, and nonaqueous electrolyte secondary battery

    JP2018056118A

  • Positive electrode active material for nonaqueous electrolyte secondary battery, method for manufacturing positive electrode active material for nonaqueous electrolyte secondary battery, electrode for nonaqueous electrolyte secondary battery, and nonaqueous electrolyte secondary battery

    JP2018073752A

  • Positive electrode for lithium ion secondary batteries, and lithium ion secondary battery

    WO2017149927A1