Magnetic cores, magnetic components and electronic devices

The magnetic core achieves high magnetic permeability and withstand voltage with minimal variations by optimizing the composition and structure of its magnetic powder, particularly through large-diameter particles with specific circularity and amorphous or nanoheterostructure, addressing the limitations of existing cores.

JP7569641B2Active Publication Date: 2024-10-18TDK CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2020141722
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-08-25
Publication Date
2024-10-18
Estimated Expiration
2040-08-25

AI Technical Summary

Technical Problem

Existing magnetic cores face challenges in achieving high magnetic permeability and withstand voltage with minimal variations in withstand voltage.

Method used

The magnetic core is designed with a specific composition and structure, including magnetic powder with a total area ratio of 75% to 90% and large-diameter particles having an average circularity of 0.70 or more, along with an amorphous or nanoheterostructure, to enhance both magnetic permeability and withstand voltage stability.

Benefits of technology

The solution results in a magnetic core with improved magnetic permeability and withstand voltage, along with reduced variations in withstand voltage, making it suitable for applications requiring miniaturization, weight reduction, and high reliability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007569641000011
    Figure 0007569641000011
  • Figure 0007569641000012
    Figure 0007569641000012
  • Figure 0007569641000013
    Figure 0007569641000013
Patent Text Reader

Abstract

To provide a magnetic core with high permeability, high withstand voltage, and small variation in withstand voltage, a magnetic component, and an electronic device.SOLUTION: In a manufacturing method for a magnetic core containing magnetic powder, the total area ratio of magnetic powder particles in a cross-section of the magnetic core is 75% or more and 90% or less. Magnetic powder particles are extracted from a cross-section of the magnetic core in an order of particle diameter from the largest to the smallest. The extracted particles in a case where the total area fraction of the extracted particles is the smallest area fraction that exceeds 20% of the total area fraction of the magnetic powder particles are considered as large diameter particles. The average circularity of the large diameter particles is 0.70 or greater.SELECTED DRAWING: Figure 4A
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a magnetic core, a magnetic component, and an electronic device. [Background technology]

[0002] Patent Document 1 describes a core using a composite magnetic material in which an insulating binder is further mixed into a mixed magnetic powder obtained by mixing an iron-based crystalline alloy magnetic powder and an iron-based amorphous alloy magnetic powder.

[0003] Patent document 2 describes an inductor that uses a composite magnetic material in which each particle contained in a mixed magnetic powder obtained by mixing hard amorphous alloy magnetic powder with Fe-Ni alloy magnetic powder is coated with a thermosetting resin. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2004-197218 A [Patent Document 2] JP 2004-363466 A Summary of the Invention [Problem to be solved by the invention]

[0005] An object of the present invention is to provide a magnetic core that has high magnetic permeability, high voltage resistance, and small variation in voltage resistance. [Means for solving the problem]

[0006] In order to achieve the above object, the magnetic core of the present invention comprises: A magnetic core comprising a magnetic powder, The total area ratio of the magnetic powder particles in the cross section of the magnetic core is 75% or more and 90% or less, The magnetic powder particles are extracted in order of largest particle diameter from the cross section of the magnetic core, and the extracted particles are defined as large-diameter particles when the total area ratio of the extracted particles is the smallest area ratio that exceeds 20% of the total area ratio of the magnetic powder particles, and the average circularity of the large-diameter particles is 0.70 or more.

[0007] By virtue of the above-mentioned characteristics, the magnetic core of the present invention has high magnetic permeability, high voltage resistance, and small variation in voltage resistance.

[0008] In a cross section of the magnetic core, the large diameter particles may have an average circularity of 0.80 or more.

[0009] In a cross section of the magnetic core, the large diameter particles may have a particle diameter of 5 μm or more and 50 μm or less.

[0010] In a cross section of the magnetic core, the particles of the magnetic powder may have an average ellipticity of 0.90 or more.

[0011] In a cross section of the magnetic core, the large grains may have an amorphous structure.

[0012] In a cross section of the magnetic core, the large diameter grains may have a nanoheterostructure in which microcrystals having a crystal grain size of 0.3 nm or more and less than 5 nm exist in an amorphous structure.

[0013] In a cross section of the magnetic core, the large diameter particles may have a structure made of nanocrystals with a crystal grain size of 5 nm or more and 50 nm or less.

[0014] The magnetic core may further include a resin.

[0015] The magnetic component of the present invention includes the above-mentioned magnetic core.

[0016] The electronic device of the present invention includes the above magnetic core. [Brief description of the drawings]

[0017] [Figure 1] FIG. 1 is a schematic diagram of a Weibull plot. [Diagram 2] FIG. 2 is an example of a chart obtained by X-ray crystal structure analysis. [Diagram 3] FIG. 3 is an example of a pattern obtained by profile fitting the chart of FIG. [Figure 4A] FIG. 4A is a schematic diagram of an atomizing device. [Figure 4B] FIG. 4B is an enlarged schematic view of a main part of FIG. 4A. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] Hereinafter, a magnetic core according to an embodiment of the present invention will be described.

[0019] The magnetic core contains magnetic powder as a magnetic material, and may contain iron-based soft magnetic alloy powder, which will be described later, as the magnetic powder.

[0020] Furthermore, the magnetic core may contain a resin. There is no particular restriction on the type and content of the resin. Examples of the type of resin include thermosetting resins such as phenolic resin and epoxy resin. The content of the resin may be 1% by mass or more and 5% by mass or less with respect to the magnetic powder.

[0021] The total area ratio of the magnetic powder particles in the cross section of the magnetic core is 75% or more and 90% or less. Then, the magnetic powder particles are extracted in order from the largest particle diameter in the cross section of the magnetic core, and the extracted particle having the smallest total area ratio exceeding 20% ​​of the total area ratio of the magnetic powder particles is defined as a large diameter particle, and the average circularity of the large diameter particles is 0.70 or more. The average circularity of the large diameter particles may be 0.80 or more, 0.90 or more, or 0.95 or more.

[0022] The larger the total area ratio of the magnetic powder particles, the easier it is to improve the relative permeability. The smaller the total area ratio of the magnetic powder particles, the longer the distance between the magnetic powder particles, and the resin fills between the magnetic powder particles to form a resin layer. Therefore, the smaller the total area ratio of the magnetic powder particles, the easier it is to improve the withstand voltage. Therefore, it was found that it is sufficient to evaluate the withstand voltage and the relative permeability comprehensively by the withstand voltage x relative permeability. The higher the withstand voltage x relative permeability, the better the balance of both the withstand voltage and the relative permeability. In particular, the withstand voltage x relative permeability is preferably used to evaluate the influence of the difference in the shape of the magnetic powder particles for magnetic cores in which the total area ratio of the magnetic powder particles is approximately the same and the shapes of the magnetic powder particles are different from each other.

[0023] The present inventors have found a method for further increasing both the relative permeability and the withstand voltage of a magnetic core using a magnetic powder, increasing the withstand voltage x the relative permeability, and reducing the variation in the withstand voltage. Specifically, they have found that controlling the average circularity of the large-diameter particles is more important than controlling the average circularity of the entire magnetic powder particles.

[0024] A magnetic core having the above characteristics has both higher relative permeability and higher voltage resistance, higher voltage resistance x relative permeability, and smaller variation in voltage resistance, compared to a magnetic core having approximately the same total area ratio of magnetic powder particles but not having the above characteristics.

[0025] The particle size distribution of the magnetic powder contained in the magnetic core can be measured by SEM observation. Specifically, the particle diameter (Heywood diameter) of each magnetic powder particle contained in any cross section of the magnetic core is calculated from an SEM image. There is no particular limit to the magnification of the SEM observation, as long as the particle diameter of the magnetic powder particles can be measured. In addition, there is no particular limit to the size of the observation range of the SEM observation, but it should be large enough to include at least 500 magnetic powder particles, preferably 1000 magnetic powder particles or more.

[0026] Then, in the above observation range set on the cross section of the magnetic core, magnetic powder particles are extracted in order of diameter, and the extracted particles are determined as large diameter particles when the total area ratio of the extracted particles is the smallest area ratio exceeding 20% ​​of the total area ratio of the magnetic powder particles. In other words, magnetic powder particles included in the above observation range set on the cross section of the magnetic core are extracted, arranged in order of diameter, and areas are added up from the magnetic powder particles with the largest particle diameter, and the particles with the total area ratio exceeding 20% ​​of the total area ratio of the magnetic powder particles in the above observation range are determined as large diameter particles.

[0027] The definition of large-diameter particles will be further explained using a hypothetical example. In the hypothetical example, the area ratios of the particles of each magnetic powder are 10%, 7%, 5%, and 4% in order from largest to smallest, and the area ratios of the particles of the other magnetic powders are all 3% or less. In this case, when extracting magnetic powder particles in order from largest to smallest particle diameter, 10% particles, 7% particles, and 5% particles are extracted in that order. Then, the total area ratio of the extracted particles is 17% when 7% particles are extracted, which does not exceed 20%. When 5% particles are further extracted, it is 22%, which exceeds 20%. If 4% or less particles are further extracted, the total area ratio of the extracted particles will be even larger. Therefore, the total area ratio when 5% particles are extracted is 22%, which is the smallest area ratio exceeding 20%. The particles extracted in this case, i.e., 10% particles, 7% particles, and 5% particles, are large-diameter particles.

[0028] The particle size of the large particles is not particularly limited. For example, it may be 1 μm or more and 150 μm or less, 3 μm or more and 100 μm or less, or 5 μm or more and 50 μm or less.

[0029] There is also no particular restriction on the D50 of the magnetic powder particles in the particle size distribution based on the number of particles in the cross section of the magnetic core. For example, D50 may be 0.1 μm to 100 μm, 0.5 μm to 50 μm, or 0.5 μm to 20 μm. D50 refers to the particle size when the cumulative value of the particle size of the magnetic powder particles is 50%.

[0030] The average circularity of the large particles in the magnetic core using the magnetic powder can be changed mainly by controlling the manufacturing method of the magnetic powder.

[0031] The circularity of the large particles contained in the magnetic core is calculated by 2×(π×S), where S is the cross-sectional area of ​​the large particle and L is the perimeter of the large particle. 1 / 2 It is expressed as / L.

[0032] The average circularity of the large diameter particles can be obtained by calculating the circularity of each of the large diameter particles specified by the above method and averaging them.

[0033] The magnetic powder particles contained in the magnetic core preferably have an average ellipticity of 0.90 or more, more preferably 0.95 or more. The higher the average ellipticity of the magnetic powder particles, the easier it is to improve the withstand voltage and reduce the variation in withstand voltage.

[0034] The ellipticity of a magnetic powder particle is expressed as 4×S / (l×s×π), where S is the area of ​​the magnetic powder particle in cross section, l is the length of the major axis, and s is the length of the minor axis.

[0035] In general, when a particle is flat, the circularity is low. However, even when a particle is flat, the elliptical circularity is high. On the other hand, even when a particle has a concave or distorted shape, the circularity may not be low. However, when a particle has a concave or distorted shape, the elliptical circularity is low. In addition, when a particle has a shape with large irregularities, both the circularity and the elliptical circularity are low. That is, in order to evaluate whether a particle is deformed other than flat when viewed from a perfect circle, for example, whether a particle has a concave, a distortion, or an irregularity, it may be preferable to use the elliptical circularity.

[0036] Here, whether the particles contained in the magnetic core are flattened or not does not affect the voltage resistance. On the other hand, whether the particles are deformed other than flattened or not, for example, whether the particles contained in the magnetic core are recessed or not, distorted or not, or whether they have large irregularities or not, is likely to affect the voltage resistance. This is because the voltage resistance of the magnetic core is improved as the number of places where the electric field is concentrated when voltage is applied is reduced, and the number of places where the electric field is concentrated is less dependent on whether the particles are flattened or not, and is more dependent on whether the particles are deformed other than flattened or not.

[0037] There is no particular limitation on the method for evaluating the variation in withstand voltage. Hereinafter, an evaluation method using the Weibull distribution will be described as an example of the method for evaluating the variation in withstand voltage.

[0038] According to the Weibull distribution, the failure rate λ(t) relative to time t is expressed by the following formula (I): where m is the Weibull coefficient and α is called the scale parameter.

[0039] λ(t)=(m / α m )×t m-1 Formula (I)

[0040] Here, when m<1, formula (I) represents the property that the failure rate decreases over time. When m=1, formula (I) represents the property that the failure rate is constant over time. When m>1, formula (I) represents the property that the failure rate increases over time. The method for calculating the Weibull coefficient m is explained below.

[0041] The reliability (probability of not failing) R(t) of a product having the above failure rate λ(t) is expressed by the following equation (II).

[0042] R(t) = exp{-(t / α) m} ...Formula (II)

[0043] The unreliability (cumulative failure rate) F(t) is expressed by the following equation (III).

[0044] F(t)=1-R(t)=1-exp{-(t / α) m} ...Formula (III)

[0045] Here, formula (III) is transformed into the following formula (IV).

[0046] ln[ln{1 / (1-F(t))}]=mlnt-mlnα...Equation (IV)

[0047] Here, if y = ln[ln{1 / (1-F(t))}] and x = lnt, we obtain the following equation (V).

[0048] y=mx-mlnα Equation (V)

[0049] In other words, plotting y=ln[ln{1 / (1-F(t))}] against x=lnt produces a straight line, and the Weibull coefficient m can be calculated from the slope of the line. This method is called a Weibull plot.

[0050] When m>1, the larger the Weibull coefficient m, the more rapidly the unreliability (cumulative failure rate) F(t) rises near a certain time t. In other words, the larger the Weibull coefficient m, the smaller the variation in the time until an individual product fails.

[0051] A schematic diagram of a Weibull plot is shown in Figure 1. In Figure 1, when m=3, F(t) increases rapidly near a certain time t, compared to when m=1.5. In other words, when m is large, many products fail simultaneously near a certain time t, and the variation in the time until each product fails is small. Note that in the Weibull plot, the further to the right the line moves, the longer the time until each product fails.

[0052] The Weibull coefficient m can be found by measuring the withstand voltage of multiple magnetic cores and making a Weibull plot of the measurement results. The applied voltage when a voltage is applied to the magnetic core and a current of a specified magnitude flows is the withstand voltage. The above "time t" can be set to "applied voltage V per unit length" and the above "failure" can be set to "current of a specified magnitude flows" to make a Weibull plot. There are no particular limitations to the method of Weibull plotting. In addition to the method of plotting test results on Weibull probability paper and calculating m, computer programs that automatically make a Weibull plot and calculate the Weibull coefficient m when test results are input are also widely used in recent years.

[0053] From the above, when the variation in withstand voltage is evaluated using the Weibull distribution, the larger the Weibull coefficient m, the smaller the variation in withstand voltage.

[0054] There is no particular limitation on the composition of the magnetic powder. A soft magnetic alloy powder may be used as the magnetic powder. In addition, as described below, two or more types of magnetic powders having different particle sizes may be mixed.

[0055] The magnetic core is made up of the composition formula (Fe (1-(α+β)) X1 α X2 β ) (1-(a+b+c+d+e+f)) M a B b P c S d C e S f It consists of: X1 is one or more selected from the group consisting of Co and Ni; X2 is one or more selected from the group consisting of Al, Mn, Ag, Zn, Sn, As, Sb, Cu, Cr, Bi, N, O and rare earth elements; M is one or more selected from the group consisting of Nb, Hf, Zr, Ta, Mo, W, Ti and V; 0≦a≦0.150 0≦b≦0.200 0≦c≦0.200 0≦d≦0.200 0≦e≦0.200 0≦f≦0.0200 0.100≦a+b+c+d+e≦0.300 α ≧ 0 β ≧ 0 0≦α+β≦0.50 The magnetic powder may contain, as the magnetic powder, an iron-based soft magnetic alloy powder represented by the formula (1).

[0056] In a cross section of the magnetic core, the total area ratio of the iron-based soft magnetic alloy powder particles to the total area ratio of the magnetic powder particles may be 50% or more.

[0057] By including particles of the iron-based soft magnetic alloy powder having the above composition within the above range in the magnetic core, the coercive force HcJ of the magnetic core decreases, and the relative permeability of the magnetic core tends to be further improved.

[0058] The total area ratio of the particles of the iron-based soft magnetic alloy powder may be 70% or more, or may be 90% or more.

[0059] The particles of the iron-based soft magnetic alloy powder may contain elements other than those mentioned above as unavoidable impurities, for example, in an amount of 0.1% by mass or less relative to 100% by mass of the particles of the iron-based soft magnetic alloy powder.

[0060] The particles of the iron-based soft magnetic alloy powder contained in the magnetic core according to the present embodiment preferably contain nanocrystals having a crystal grain size of 5 nm to 50 nm and a bcc crystal structure. By containing the above-mentioned nanocrystals in the particles of the iron-based soft magnetic alloy powder, the HcJ of the magnetic core is further reduced and the relative permeability is easily improved.

[0061] A method for manufacturing the magnetic core according to this embodiment will now be described.

[0062] First, the magnetic powder contained in the magnetic core is prepared. There is no particular limitation on the manufacturing method of the magnetic powder. For example, atomization is used. The type of atomization is also arbitrary, and examples include water atomization and gas atomization. Below, a method for manufacturing a magnetic core containing iron-based soft magnetic alloy powder as the magnetic powder is described.

[0063] When the iron-based soft magnetic alloy powder obtained by the atomization method has an amorphous structure, nanocrystals having a crystal grain size of 5 nm to 50 nm and a bcc crystal structure can be precipitated by heat treatment. Then, an iron-based soft magnetic alloy powder having a structure made of nanocrystals is obtained. The heat treatment conditions are, for example, 350°C to 800°C and 0.1 minutes to 120 minutes. Note that a single iron-based soft magnetic alloy powder particle usually contains a large number of nanocrystals. That is, the particle size of the iron-based soft magnetic alloy powder particle is different from the crystal grain size of the nanocrystal. In addition, the crystal structure of the iron-based soft magnetic alloy powder can be confirmed by XRD or a transmission electron microscope. When evaluating the microstructure of the iron-based soft magnetic alloy powder in the magnetic core, it can be confirmed by a bright field method and a selected area diffraction method using a transmission electron microscope. When the iron-based soft magnetic alloy powder contains nanocrystals, the HcJ of the magnetic core obtained in the end tends to be low and the relative permeability tends to be high. In addition, the microstructure of the iron-based soft magnetic alloy powder and the microstructure of the particles of the iron-based soft magnetic alloy powder may be the same.

[0064] The microstructure of the iron-based soft magnetic alloy powder will now be described.

[0065] In order to make the iron-based soft magnetic alloy powder contain nanocrystals, it is common to heat-treat the iron-based soft magnetic alloy powder having an amorphous structure to precipitate the nanocrystals. Here, the amorphous structure refers to a structure in which the amorphous ratio X shown in the following formula (1) is 85% or more. And the crystalline structure refers to a structure in which the amorphous ratio X is less than 85%. X = 100 - (Ic / (Ic + Ia) × 100) ... (1) Ic: Crystalline scattering integrated intensity Ia: Amorphous scattering integrated intensity

[0066] The amorphous ratio X is calculated by performing X-ray crystal structure analysis by XRD on the iron-based soft magnetic alloy powder, identifying the phase, reading the peaks of crystallized Fe or compounds (Ic: crystalline scattering integrated intensity, Ia: amorphous scattering integrated intensity), determining the crystallization ratio from the peak intensity, and calculating the crystallization ratio according to the above formula (1). The calculation method will be described in more detail below.

[0067] X-ray crystal structure analysis is performed on the iron-based soft magnetic alloy powder by XRD to obtain a chart as shown in Fig. 2. This is then profile-fitted using the Lorentz function of the following formula (2) to obtain a crystalline component pattern α , which shows the crystalline scattering integrated intensity as shown in Fig. 3. c , amorphous component pattern α showing amorphous scattering integral intensity a , and the combined pattern α c+a From the crystalline scattering integrated intensity and the amorphous scattering integrated intensity of the obtained pattern, the amorphization rate X is calculated by the above formula (1). The measurement range is the diffraction angle 2θ=30° to 60°, where an amorphous-derived halo can be confirmed. In this range, the error between the integrated intensity actually measured by XRD and the integrated intensity calculated using the Lorentz function is set to within 1%.

[0068]

number

[0069] In general, the higher the amorphous ratio X of the iron-based soft magnetic alloy powder, the lower the coercive force. Furthermore, when the iron-based soft magnetic alloy powder after heat treatment has a structure made of nanocrystals, the saturation magnetic flux density of the magnetic core tends to be higher and the coercive force tends to be lower than when the iron-based soft magnetic alloy powder has an amorphous structure. When a magnetic core is made using an iron-based soft magnetic alloy powder with low coercive force, the magnetic permeability of the magnetic core tends to be improved.

[0070] A method for producing iron-based soft magnetic alloy powder by gas atomization will be described below.

[0071] The inventors have found that when the atomizing apparatus shown in Figures 4A and 4B is used as the atomizing apparatus, it is easy to produce iron-based soft magnetic alloy powder with a large particle size, and it is also easy to obtain iron-based soft magnetic metal powder having an amorphous structure.

[0072] 4A, the atomizing apparatus 10 has a molten metal supplying section 20 and a cooling section 30 disposed vertically below the metal supplying section 20. In the drawing, the vertical direction is along the Z-axis.

[0073] The molten metal supply unit 20 has a heat-resistant container 22 that contains the molten metal 21. In the heat-resistant container 22, raw materials of each metal element weighed so as to form the composition of the finally obtained soft magnetic alloy powder are melted by a heating coil 24 to become the molten metal 21. The temperature during melting, i.e., the temperature of the molten metal 21, may be determined in consideration of the melting points of the raw materials of each metal element, and may be, for example, 1200 to 1600°C.

[0074] The molten metal 21 is discharged as dripping molten metal 21a from the discharge port 23 toward the cooling section 30. High-pressure gas is sprayed from the gas spray nozzle 26 toward the discharged dripping molten metal 21a, and the dripping molten metal 21a becomes a number of droplets, which are carried toward the inner surface of the cylinder 32 along the gas flow.

[0075] The gas injected from the gas injection nozzle 26 is preferably an inert gas or a reducing gas. As the inert gas, for example, nitrogen gas, argon gas, helium gas, etc. can be used. As the reducing gas, for example, an ammonia decomposition gas can be used. However, when the molten metal 21 is a metal that is difficult to oxidize, the gas injected from the gas injection nozzle 26 may be air.

[0076] The dripping molten metal 21a conveyed toward the inner surface of the cylinder 32 collides with the cooling liquid flow 50 formed in an inverted cone shape inside the cylinder 32, where it is further divided and atomized, and is cooled and solidified to become a solid alloy powder. The axis O of the cylinder 32 is inclined at a predetermined angle θ1 with respect to the vertical line Z. The predetermined angle θ1 is not particularly limited, but is preferably 0 to 45 degrees. By setting the angle in this range, it becomes easier to discharge the dripping molten metal 21a from the discharge port 23 toward the cooling liquid flow 50 formed in an inverted cone shape inside the cylinder 32.

[0077] A discharge part 34 is provided below along the axis O of the cylinder 32, and allows the alloy powder contained in the cooling liquid flow 50 to be discharged to the outside together with the cooling liquid. The alloy powder discharged together with the cooling liquid is separated from the cooling liquid in an external storage tank or the like and taken out. The cooling liquid is not particularly limited, but cooling water is used.

[0078] In this embodiment, the dripping molten metal 21a collides with the cooling liquid flow 50 formed in an inverted cone shape, so the flight time of the droplets of the dripping molten metal 21a is shortened compared to when the cooling liquid flow is along the inner surface 33 of the cylinder 32. The shortened flight time promotes the rapid cooling effect and improves the amorphization rate X of the obtained iron-based soft magnetic alloy powder. In addition, the shortened flight time makes it difficult for the droplets of the dripping molten metal 21a to be oxidized, so that the fineness of the obtained iron-based soft magnetic alloy powder is promoted and the quality of the iron-based soft magnetic alloy powder is improved.

[0079] In this embodiment, in order to form the coolant flow in an inverted cone shape inside the cylindrical body 32, the flow of the coolant is controlled in a coolant inlet portion (coolant outlet portion) 36 for introducing the coolant into the inside of the cylindrical body 32. The configuration of the coolant inlet portion 36 is shown in FIG.

[0080] 4B, the frame 38 defines an outer portion (outer space) 44 located on the radially outer side of the cylindrical body 32, and an inner portion (inner space) 46 located on the radially inner side of the cylindrical body 32. The outer portion 44 and the inner portion 46 are separated by a partition portion 40, and the outer portion 44 and the inner portion 46 are connected by a passage portion 42 formed at the upper portion of the partition portion 40 in the axial center O direction, allowing the coolant to flow therethrough.

[0081] A single or multiple nozzles 37 are connected to the outer portion 44, and the cooling liquid flows into the outer portion 44 from the nozzles 37. In addition, a cooling liquid discharge portion 52 is formed below the inner portion 46 in the axial direction O, and the cooling liquid in the inner portion 46 is discharged (guided) from there into the cylindrical body 32.

[0082] The outer peripheral surface of the frame 38 forms a flow passage inner peripheral surface 38b that guides the flow of the cooling liquid inside the inner portion 46, and an outer convex portion 38a1 that is continuous with the flow passage inner peripheral surface 38b of the frame 38 and protrudes radially outward is formed at the lower end 38a of the frame 38. Therefore, the ring-shaped gap between the tip of the outer convex portion 38a1 and the inner surface 33 of the cylindrical body 32 forms the cooling liquid discharge portion 52. A flow passage deflection surface 62 is formed on the upper surface of the outer convex portion 38a1 on the flow passage side.

[0083] As shown in FIG. 4B, the radial width D1 of the coolant discharge portion 52 is narrower than the radial width D2 of the main portion of the inner portion 46 due to the outward convex portion 38a1. Since D1 is narrower than D2, the coolant flowing down the axis O along the flow path inner circumferential surface 38b inside the inner portion 46 flows next along the flow path deflection surface 62 of the frame 38 and collides with the inner surface 33 of the cylindrical body 32 to be reflected. As a result, as shown in FIG. 4A, the coolant is discharged from the coolant discharge portion 52 into the inside of the cylindrical body 32 in an inverted cone shape, forming a coolant flow 50. When D1=D2, the coolant discharged from the coolant discharge portion 52 forms a coolant flow along the inner surface 33 of the cylindrical body 32.

[0084] D1 / D2 is preferably 2 / 3 or less, more preferably 1 / 2 or less. D1 / D2 is preferably 1 / 10 or more. The smaller D1 / D2 is, the more the quenching effect is promoted, and the amorphous ratio X of the obtained iron-based soft magnetic alloy powder tends to be larger. However, the smaller D1 / D2 is, the lower the circularity of the obtained iron-based soft magnetic alloy powder tends to be. That is, in order to achieve both the quenching effect (high amorphous ratio X of the iron-based soft magnetic alloy powder) and the circularity of the iron-based soft magnetic alloy powder, it is necessary to appropriately adjust D1 / D2.

[0085] The coolant flow 50 flowing out from the coolant discharge portion 52 is an inverted conical flow proceeding straight from the coolant discharge portion 52 toward the axis O, but may be a spiral inverted conical flow.

[0086] The amount of molten metal ejected, the gas injection pressure, the pressure inside the cylindrical body 32, the cooling liquid discharge pressure, D1 / D2, etc. may be appropriately set according to the particle diameter of the target soft magnetic alloy powder. The amount of molten metal ejected may be, for example, 1 kg / min or more and 20 kg / min or less. The gas injection pressure may be, for example, 0.5 MPa or more and 19 MPa or less. The pressure inside the cylindrical body 32 may be, for example, 0.5 MPa or more and 19 MPa or less. The cooling liquid discharge pressure (pump pressure) may be, for example, 0.5 MPa or more and 19 MPa or less.

[0087] The smaller the amount of molten metal ejected, the smaller the particle size, and the easier it is to produce iron-based soft magnetic alloy powder with an amorphous structure. The amorphous structure includes an amorphous structure that does not contain crystals and is made up of only amorphous material, and a nanoheterostructure in which microcrystals (crystals with a crystal grain size of 0.3 nm or more and less than 5 nm) exist in the amorphous material. It is possible to confirm whether an iron-based soft magnetic alloy powder has an amorphous structure and whether it has a nanoheterostructure by bright-field observation using a transmission electron microscope and by selected area diffraction. When an iron-based soft magnetic alloy powder has an amorphous structure, it is easier to precipitate nanocrystals by heat treatment.

[0088] The higher the gas injection pressure, the pressure inside the cylindrical body 32, and the coolant discharge pressure, the smaller the particle size and the smaller the circularity of the particles tend to be.

[0089] Then, nanocrystals may be precipitated in the iron-based soft magnetic alloy powder having an amorphous structure by the above-mentioned heat treatment, thereby obtaining an iron-based soft magnetic alloy powder having a nanocrystalline structure.

[0090] The particle size of the iron-based soft magnetic alloy powder can be adjusted by changing the atomization conditions described above. It is also possible to adjust the particle size by adjusting the particle size through dry classification or wet classification. Examples of dry classification methods include sieve classification using a dry sieve and airflow classification. Examples of wet classification methods include classification by wet filter filtration and classification by centrifugation. In other words, by adjusting the powder preparation conditions and classification method in atomization in the iron-based soft magnetic alloy powder produced by the atomization method described above, it is possible to adjust the particle size of the large diameter powder in the magnetic core cross section and control the average circularity of the large diameter powder.

[0091] In sieve classification, the powder is classified using a dry sieve. In wet filter filtration classification, the powder is dispersed in a dispersion medium, and the dispersion medium in which the powder is dispersed is filtered through a filter to classify the powder. In general, classification using a dry sieve tends to result in a smaller average circularity of large-diameter powder in the cross section of the magnetic core. In other words, classification using a dry sieve makes it relatively difficult to remove powder particles with irregular shapes.

[0092] In the sieve classification, the particle size of the iron-based soft magnetic alloy powder can be adjusted by changing, for example, the amount of powder charged per time, the classification time, and / or the mesh size. Also, by increasing the number of times the powder is passed through the mesh, powder particles with irregular shapes can be easily removed.

[0093] Furthermore, the particle size may be adjusted by blending a plurality of types of iron-based soft magnetic alloy powders having different particle size distributions and / or circularities, and the average circularity, particularly the average circularity of the large-diameter powder in the magnetic core cross section, may be adjusted. For example, an iron-based soft magnetic alloy powder classified by a dry sieve and an iron-based soft magnetic alloy powder classified by wet filter filtration may be blended.

[0094] Next, a magnetic powder is prepared. The above iron-based soft magnetic alloy powder may be used as the magnetic powder as it is, or another powder may be blended with the above iron-based soft magnetic alloy powder to prepare a magnetic powder. There is no particular limit to the composition of the powder to be blended. For example, pure iron powder, carbonyl iron powder, permalloy powder, Fe-Si soft magnetic alloy powder, Fe-Si-Cr soft magnetic alloy powder, Fe-Co soft magnetic alloy powder, etc. may be blended. Also, iron-based soft magnetic alloy powders with different compositions may be blended. By controlling the particle size distribution of the various magnetic powders to be blended, the filling rate of the magnetic powder in the magnetic core finally obtained can be controlled. Also, an insulating coating may be formed on the various magnetic powders.

[0095] When preparing magnetic powder by blending another powder with an iron-based soft magnetic alloy powder, the proportion of the iron-based soft magnetic alloy powder in the magnetic powder may be 50 mass% or more, 70 mass% or more, or 90 mass% or more.

[0096] The particle size distribution of the magnetic powder before compaction based on the number of particles may be confirmed using a Morphologi G3 (Malvern Panatical). The Morphologi G3 is a device that disperses the powder with air and projects and evaluates the shape of each particle. The particle shape, which is within the range of particle diameter of approximately 0.5 μm to several mm, can be confirmed using an optical microscope or laser microscope.

[0097] Morphologi G3 can create and evaluate the projections of many particles at once, making it possible to evaluate the shapes of many particles in a short time. Therefore, it is suitable for evaluating the particle size distribution, etc., of soft magnetic alloy powder before compaction. For example, it is possible to create projections of approximately 20,000 soft magnetic alloy powder particles, automatically calculate the particle size and circularity of each particle, and calculate the average circularity of particles whose particle sizes are within a specific range.

[0098] The particle size distribution based on the number of magnetic powder particles confirmed by Morphologi G3 does not match the particle size distribution based on the number of magnetic powder particles in the cross section of the final magnetic core. The D50 and D90 of the magnetic powder particles in the cross section of the final magnetic core are somewhat smaller than the D50 and D90 based on the number of magnetic powder particles confirmed by Morphologi G3. This is because the magnetic powder particles are cut at random locations when the magnetic core is cut. In other words, even if the particles are large, they may be observed as small particles depending on the cut location.

[0099] However, there is a correlation between the particle size distribution and circularity of the magnetic powder on a number basis confirmed by Morphologi G3 and the particle size distribution and circularity of the magnetic powder on a number basis in the cross section of the magnetic core finally obtained. Therefore, by confirming the particle size distribution and circularity of the magnetic powder with Morphologi G3, it is possible to predict to some extent the particle size distribution of the magnetic powder on the cross section of the magnetic core finally obtained. In other words, it is easy to control the particle size distribution and circularity of the magnetic powder on a number basis in the cross section of the magnetic core finally obtained by controlling the particle size distribution and circularity of the magnetic powder on a number basis before compaction.

[0100] The magnetic powder thus obtained can then be molded to obtain a magnetic core. There are no particular limitations on the molding method. As an example, a method of obtaining a magnetic core by pressure molding will be described.

[0101] First, the magnetic powder is mixed with a resin. By mixing the resin, it becomes easier to obtain a molded body with high strength by molding. There is no particular limit to the type of resin. Examples include phenol resin and epoxy resin. There is also no particular limit to the amount of resin added. When resin is added, it may be added in an amount of 1% by mass or more and 5% by mass or less relative to the magnetic powder.

[0102] The mixture of magnetic powder and resin is granulated to obtain granulated powder. There is no particular limitation on the granulation method. For example, granulation may be performed using a stirrer. There is no particular limitation on the particle size of the granulated powder.

[0103] The granulated powder is then pressed to obtain a green body. There are no particular restrictions on the pressing pressure. For example, a surface pressure of 1 ton / cm 2 More than 10ton / cm 2 The higher the molding pressure, the higher the relative magnetic permeability tends to be, but if the particle size distribution of the magnetic powder is broad, the relative magnetic permeability can be increased even if the molding pressure is lower than that of normal pressure molding. This is because the resulting magnetic core is more likely to be densified.

[0104] The resin contained in the molded body is then cured to obtain the magnetic core. There are no particular limitations on the curing method, and heat treatment may be performed under conditions that can cure the resin used.

[0105] There is no particular limit to the use of the magnetic core. For example, it can be used as a magnetic core for an inductor, particularly a power inductor. It can also be used as an inductor in which the magnetic core and the coil are integrally molded.

[0106] Furthermore, the magnetic core and a magnetic part using the magnetic core can be suitably used in electronic devices.

[0107] In particular, the magnetic core has high magnetic permeability, high voltage resistance, and small variation in voltage resistance, and is therefore suitable for use in fields requiring miniaturization, weight reduction, and high reliability, such as magnetic cores, magnetic components, and electronic devices mounted on hybrid vehicles, plug-in hybrid vehicles, and electric vehicles. EXAMPLES

[0108] The present invention will be specifically described below with reference to examples.

[0109] (Experimental Example 1) The iron-based soft magnetic alloy powders A to F shown in Table 1 were prepared. 0.735 Nb 0.030 B 0.090 S 0.135 Cu 0.100 Ingots of various materials were prepared and weighed so as to obtain a master alloy having the composition given above, and were then placed in a crucible disposed in a gas atomizing device.

[0110] Next, the master alloy was placed in the heat-resistant container 22 arranged in the atomizing apparatus 10. Subsequently, after the inside of the cylindrical body 32 was evacuated, the heat-resistant container 22 was heated by high-frequency induction using the heating coil 24 provided outside the heat-resistant container 22, and the raw metals in the heat-resistant container 22 were melted and mixed to obtain a molten metal (molten metal) at 1500°C.

[0111] The obtained molten metal was injected into the housing 32 of the cooling section 30 at 1500°C, and argon gas was injected at a gas injection pressure shown in Table 1 to form a large number of droplets. The amount of molten metal ejected and the pump pressure of the cooling water were set to the values ​​shown in Table 1. The droplets collided with an inverted cone-shaped cooling water flow formed by the cooling water supplied at the pump pressure shown in Table 1, turned into fine powder, and were then collected.

[0112] In the atomizing apparatus 10 shown in FIGS. 4A and 4B, the inner diameter of the inner surface of the cylindrical body 32 was 300 mm, the angle θ1 was 20 degrees, and D1 / D2 was set under the conditions shown in Table 1.

[0113] Further, the powder was heat-treated at 550°C for 60 minutes. The powder was then classified using the methods shown in Table 1. In the classification using a dry sieve, the powder was classified using a sieve in the air. In the classification using a wet filter, the powder was dispersed using IPA as a dispersion medium, and the dispersion medium in which the powder was dispersed was filtered using a filter.

[0114] In addition to the conditions listed in Table 1, the particle size distribution based on the number of iron-based soft magnetic alloy powders and the average circularity of iron-based soft magnetic alloy powders with D90 or more were changed by changing the classification method and the mesh size of the sieve or filter. For iron-based soft magnetic alloy powders A and B, D10 was set to 2.0 to 4.0 μm, D50 was set to 7.0 to 12 μm, and D90 was set to 21 to 24 μm. For iron-based soft magnetic alloy powders C and D, D10 was set to 1.5 to 3.0 μm, D50 was set to 4.0 to 6 μm, and D90 was set to 8 to 15 μm. For iron-based soft magnetic alloy powders E and F, D10 was set to 3.0 to 8.0 μm, D50 was set to 15 to 25 μm, and D90 was set to 60 to 74 μm. In addition, the average circularity of the iron-based soft magnetic alloy powders A, C, and E of D90 or more is 0.60 to 0.65, and the average circularity of the iron-based soft magnetic alloy powders B, D, and F of D90 or more is 0.93 to 0.98. By setting the particle size distribution on a number basis of each iron-based soft magnetic alloy powder and the average circularity of the iron-based soft magnetic alloy powder of D90 or more within the above ranges, the average particle size and average circularity of the large-diameter powder in the core cross section shown in each table below can be obtained.

[0115] The average circularity of the iron-based soft magnetic alloy powders with D10, D50, D90, and D90 or more on a number basis was measured by observing the shape of 20,000 powder particles at 10x magnification using a Morphologi G3 (Malvern Panalytical). Specifically, 3cc of powder was dispersed at an air pressure of 1-3 bar and a projected image was taken with a laser microscope. The average circularity of the iron-based soft magnetic alloy powders with D10, D50, D90, and D90 or more on a number basis was calculated from the particle diameter of each powder particle. The particle diameter of each powder particle was taken as the Heywood diameter.

[0116] It was confirmed by ICP analysis that the composition of the master alloy and the composition of the iron-based soft magnetic alloy powder were roughly the same.

[0117] It was confirmed whether each iron-based soft magnetic alloy powder was made of amorphous or crystalline. The peaks due to crystals were confirmed using XRD, and it was confirmed that they were amorphous. Furthermore, each iron-based soft magnetic alloy powder was heat-treated at 550°C for 1 hour, and the peaks due to crystals were confirmed again using XRD, and the crystal grain size of the crystal grains was 5 nm or more and 50 nm or less. In other words, it was confirmed that all of the above iron-based soft magnetic alloy powders contained nanocrystals.

[0118] Next, carbonyl iron powder was prepared as iron powder separately from the soft magnetic alloy powder. The particle size distribution of the volume distribution of the carbonyl iron powder obtained by the laser diffraction method was D50 of 1.0 μm.

[0119] [Table 1]

[0120] Next, a toroidal core and a cylindrical core were produced using the above iron-based soft magnetic alloy powders A to F and carbonyl iron powder.

[0121] Magnetic powder was obtained by mixing iron-based soft magnetic alloy powder and carbonyl iron powder in the mass ratios shown in Tables 2 to 4. Next, the magnetic powder was mixed with resin (phenolic resin). The amount of resin relative to the magnetic powder was mixed in the amount shown in Table 2. Next, the mixture was granulated using a general planetary mixer as the agitator to obtain granulated powder with a particle size of about 500 μm. Next, the obtained granulated powder was subjected to a surface pressure of 4 ton / cm. 2 (392MPa)~8ton / cm 2 (784 MPa) and adjusted to obtain the total area of ​​the magnetic powder particles shown in Table 2. By pressure molding, a toroidal shaped compact with an outer diameter of 11 mmφ, an inner diameter of 6.5 mmφ, and a height of 6.0 mm, and a cylindrical shaped compact with a diameter of 8.0 mmφ and a height of 8.0 mm were produced. The obtained compacts were hardened at 150°C to produce a toroidal core and a cylindrical core. The number of these cores required for the tests described below were produced.

[0122] Total area ratio of magnetic powder particles The toroidal core was cut at an arbitrary cross section and observed at a magnification of 500 times using an SEM. The observation range was set to a size where at least 1000 magnetic powder particles were observed. Then, the total area ratio of the magnetic powder particles, that is, the total area ratio of the iron-based soft magnetic alloy powder particles and the carbonyl iron powder particles, was calculated. If it was difficult to distinguish between the magnetic powder particles and the resin layer at the above magnification, the magnification was increased for observation. In that case, the total area of ​​the observation range was set to the same area. For example, when observing at a magnification of 1000 times, four times the number of images were used so that the total area of ​​the observation range was the same as when observed at a magnification of 500 times.

[0123] Average ellipticity of magnetic powder particles For the above observation range, the ellipticity of all the magnetic powder particles was calculated and averaged.

[0124] Average particle size and average circularity of large particles The particle size distribution of the magnetic powder in the toroidal core was confirmed by calculating the circle equivalent diameter (Heywood diameter) of all the magnetic powder particles in the above observation range. Then, in the above observation range set on the cross section of the magnetic core, the magnetic powder particles were extracted in order of particle diameter from the largest, and the extracted particle with the smallest area ratio of the total area ratio of the extracted particles exceeding 20% ​​of the total area ratio of the magnetic powder particles was determined as the large diameter particle. Then, the average particle diameter and average circularity of the large diameter particles were calculated. In addition, it was confirmed by the EDS composition map that all the large diameter particles were particles of any of the iron-based soft magnetic alloy powders A to F in all the experimental examples.

[0125] In all experimental examples, the D50 of the magnetic powder in the cross section of the toroidal core was calculated and confirmed to be 1 μm or more and 100 μm or less.

[0126] relative permeability The UEW wire was wound around a toroidal core, and the relative permeability was measured at 100 kHz using a 4284A PRECISION LCR METER (Hewlett-Packard). The comparative example was used as the standard, which was carried out under the same conditions except that the average circularity of the large-diameter particles was too low because the iron-based soft magnetic alloy powders B, D, and F were not used. The relative permeability was rated as good when it was 1.04 times or more higher than the relative permeability of the comparative example.

[0127] Withstand voltage and m value For the 20 cylindrical cores, In-Ga electrodes were formed on two surfaces perpendicular to the thickness direction. Next, a voltage was applied using a source meter (THK-2011ADMPT manufactured by Tama Densoku Co., Ltd.) to measure the voltage when a current of 1 mA flowed. The voltage was then divided by the thickness of the cylindrical core to measure the withstand voltage of the cylindrical core. The average value of the withstand voltages of the 20 cylindrical cores was taken as the withstand voltage of each experimental example. Furthermore, a Weibull plot was made for the withstand voltages of the 20 cylindrical cores, and the m value of each experimental example was calculated. An m value of 3.0 or more was considered to be good.

[0128] The comparative example was used as a standard, which was carried out under the same conditions except that the average circularity of the large diameter particles was too low because the iron-based soft magnetic alloy powders B, D and F were not used. The samples with a withstand voltage of 1.08 times or more the withstand voltage of the comparative example were evaluated as good.

[0129] Furthermore, in evaluating the voltage resistance x relative permeability, a comparative example was used as a standard, which was carried out under the same conditions except that the average circularity of the large-diameter particles was too low because the iron-based soft magnetic alloy powders B, D, and F were not used. A value of 1.2 times or more of the voltage resistance x relative permeability of the comparative example was deemed good.

[0130] [Table 2]

[0131] [Table 3]

[0132] [Table 4]

[0133] From Tables 2 to 4, in each Example in which the total area ratio of the magnetic powder particles is 75% or more and 90% or less, and the average circularity of the large diameter particles is 0.70 or more, the relative permeability and withstand voltage are high, and the variation in withstand voltage is small, compared to each Comparative Example having substantially the same configuration except that the average circularity of the large diameter particles is less than 0.70. Furthermore, each Example also had a good withstand voltage x relative permeability. In the above Examples, the withstand voltage of the cylindrical core was measured, but it was confirmed that the withstand voltage of the colloidal core was also measured to obtain the same result as that of the cylindrical core.

[0134] (Experimental Example 2) The magnetic powders of sample numbers 19 to 24 were subjected to a phosphate treatment to form an insulating coating on the magnetic powder. The coating thickness of the soft magnetic alloy powder was 20 nm, and the coating thickness of the carbonyl iron powder was 10 nm. The results of evaluation in the same manner as in Experimental Example 1 are shown in Table 5.

[0135] [Table 5]

[0136] As can be seen from Table 5, the results obtained when an insulating coating was formed were similar to those obtained when an insulating coating was not formed.

[0137] (Experimental Example 3) For sample number 7, sample numbers 7a and 7b were prepared under the same conditions, except that the irregularly shaped powder contained in the carbonyl iron powder was removed by air classification. For sample number 12, sample numbers 12a and 12b were prepared under the same conditions, except that the irregularly shaped powder contained in the carbonyl iron powder was removed by air classification. By removing the irregularly shaped powder, the sphericity of the carbonyl iron powder increased, and the average ellipticity of the magnetic powder particles increased. The results are shown in Table 6.

[0138] [Table 6]

[0139] From Table 6, the results obtained when the irregularly shaped powder was removed were similar to those obtained when the irregularly shaped powder was not removed. Furthermore, the higher the average ellipticity of the magnetic powder particles, the higher the withstand voltage and m value.

[0140] (Experimental Example 4) For sample number 43 in Experimental Example 1, sample numbers 67, 70, and 72 were produced under the same conditions, except that the heat treatment conditions for powder A were changed to change the microstructure. Also, for sample number 44 in Experimental Example 1, sample numbers 68, 71, and 73 were produced under the same conditions, except that the heat treatment conditions for powders A and B were changed to change the microstructure. The results are shown in Table 7. Powders marked as "amorphous" in the microstructure column in Table 7 have an amorphous structure. Powders marked as "nanocrystalline" have a structure consisting of nanocrystals. He The powders described as "heterostructure" have a nanoheterostructure. The powders described as "crystalline" have a structure made of crystals with a crystal grain size of 100 nm or more. The examples and comparative examples, in which the crystalline state of the soft magnetic alloy powder is the same, are compared.

[0141] Furthermore, two types of powder A were prepared: one with a nanocrystalline structure obtained by heat treatment at 550°C for 1 hour, and one with an amorphous structure obtained without heat treatment. Furthermore, one with an amorphous structure obtained without heat treatment was prepared for powder B. Then, each powder was mixed in the mixing ratio shown in Table 8 to produce sample numbers 69a and 69. The results are shown in Table 8. Sample numbers 69a and 69 have in common that the mass ratio of the soft magnetic alloy powder having a nanocrystalline structure to the soft magnetic alloy powder having an amorphous structure is 70:30.

[0142] [Table 7]

[0143] [Table 8]

[0144] As can be seen from Tables 7 and 8, regardless of the crystalline state of the powder, the same results as in Experimental Example 1 were obtained. Furthermore, the magnetic properties were the best when the microstructure of Powders A and B was a structure consisting of nanocrystals.

[0145] (Experimental Example 5) Atomic ratio: Fe 0.78475 Nb 0.070 B 0.090 S 0.020 P 0.030 C 0.005 S 0.00025 Powder G was produced under the same conditions as Powder A, except that ingots of various materials were prepared so as to obtain a master alloy of the composition, and Powder H was produced under the same conditions as Powder B. Samples 74 to 79 were produced under the same conditions as Samples 19 to 24, except that Powder A was replaced with Powder G and Powder B was replaced with Powder H. The results are shown in Table 9.

[0146] [Table 9]

[0147] As can be seen from Table 9, the results were similar to those of Experimental Example 1, regardless of the powder composition. [Explanation of symbols]

[0148] 1…Particle shape measurement results 10...Atomization device 20…Molten metal supply section 21…Molten metal 21a…Dripping molten metal 30...Cooling section 36…Coolant inlet 38a1...Outward convex part 50…coolant flow

Claims

1. A magnetic core comprising a magnetic powder, The total area ratio of the magnetic powder particles in the cross section of the magnetic core is 75% or more and 90% or less, Particles of the magnetic powder are extracted in order of diameter from the largest in a cross section of the magnetic core, and the extracted particles having a minimum area ratio exceeding 20% ​​of the total area ratio of the particles of the magnetic powder are defined as large diameter particles, and the average circularity of the large diameter particles is 0.80 or more and 0.98 or less; A magnetic core, wherein the average ellipticity of the particles of the magnetic powder in a cross section of the magnetic core is 0.90 or more.

2. 2. The magnetic core according to claim 1, wherein the large diameter particles have a particle diameter of 5 μm or more and 50 μm or less in a cross section of the magnetic core.

3. 3. The magnetic core according to claim 1, wherein the large diameter grains have an amorphous structure in a cross section of the magnetic core.

4. 3. The magnetic core according to claim 1, wherein in a cross section of the magnetic core, the large diameter grains have a nano-hetero structure in which microcrystals having a crystal grain size of 0.3 nm or more and less than 5 nm exist in an amorphous structure.

5. 3. The magnetic core according to claim 1, wherein in a cross section of the magnetic core, the large diameter grains have a structure made of nanocrystals with a crystal grain size of 5 nm or more and 50 nm or less.

6. The magnetic core according to any one of claims 1 to 5, further comprising a resin.

7. A magnetic component comprising the magnetic core according to any one of claims 1 to 6.

8. 7. An electronic device comprising the magnetic core according to claim 1.

Citation Information

Patent Citations

  • Composite magnetic material, core using the same, and magnetic element

    JP2004197218A

  • Complex magnetic material and method for manufacturing inductor using the same

    JP2004363466A

  • Precursor for powder magnetic core, powder magnetic core, and electronic component

    JP2016012671A

  • Dust core and magnetic element

    JP2017107935A

  • Composite material, magnetic component, and reactor

    JP2017224851A