Grinding liquid composition

A polishing liquid composition with silica particles, cationic and nonionic polymers addresses the challenge of surface defects and roughness in semiconductor substrates, improving polishing speed and quality.

JP7569655B2Active Publication Date: 2024-10-18KAO CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020171483
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-10-09
Publication Date
2024-10-18
Estimated Expiration
2040-10-09

AI Technical Summary

Technical Problem

The increasing demand for higher storage capacity in semiconductor devices has led to shallow depth of focus in photolithography, causing surface defects (LPD and LPD-N) and surface roughness (haze) on silicon substrates, necessitating a polishing liquid composition that improves polishing speed while reducing these defects.

Method used

A polishing liquid composition comprising silica particles, a cationic water-soluble polymer with a nitrogen-containing group, and a nonionic water-soluble polymer with an alkylene oxide group or hydroxyl group, formulated to enhance polishing speed and reduce surface roughness and defects by optimizing the mass ratios and pH.

Benefits of technology

The composition improves polishing rate, reduces surface roughness (haze), and minimizes surface defects (LPD and LPD-N) without impairing polishing efficiency, thereby enhancing the quality of semiconductor substrates.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007569655000001
    Figure 0007569655000001
Patent Text Reader

Abstract

To provide a polishing liquid composition that can achieve all of improved polishing rates, reduced surface roughness (haze) of a silicon substrate, and reduced surface defects (LPD and / or LPD-N).SOLUTION: This invention relates to a polishing liquid composition for silicon substrates that contains the following components A, B, and D, wherein the mass ratio of the content of component D to the content of component A, D / A, is 0.01 or more and 0.2 or less, and the pH is more than 8.5 to 14 or less. Component A: silica particles. Component B: a cationic water-soluble polymer having a nitrogen-containing group (excluding polyalkyleneimine). Component D: a nonionic water-soluble polymer having in each molecule an alkylene oxide group or a hydroxy group, with a weight average molecular weight of 2,000 or more and less than 500,000.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a polishing composition, a polishing method using the same, and a method for producing a semiconductor substrate. [Background technology]

[0002] In recent years, the design rules for semiconductor devices have become finer due to the increasing demand for higher storage capacity of semiconductor memories. As a result, the depth of focus in photolithography used in the manufacturing process of semiconductor devices has become shallower, and the demand for reducing surface defects (LPD: Light Point Defects, LPD-N: Light Point Defect Non-cleanable) and surface roughness (haze) of silicon substrates (bare wafers) has become increasingly strict. Here, LPD and LPD-N refer to foreign matter generally known as particles.

[0003] In order to improve the quality of silicon substrates, polishing of silicon substrates is carried out in multiple stages. In particular, the final polishing stage is carried out to reduce haze and surface defects such as particles, scratches, and pits.

[0004] For example, Patent Document 1 proposes a polishing composition containing silica particles, a nitrogen-containing basic compound, and a water-soluble polymer in which the ratio of the number of oxygen atoms derived from hydroxyl groups to the number of oxygen atoms derived from polyoxyalkylene is 0.8 to 10. Patent Document 2 proposes a semiconductor polishing composition that contains abrasive grains, a basic compound, and two or more water-soluble polymers, the water-soluble polymers including a cationic water-soluble polymer containing a nitrogen-containing group. In the examples of the document, a semiconductor polishing composition containing colloidal silica, ammonia, tetramethylammonium hydroxide, hydroxyethylcellulose having a weight-average molecular weight of 800,000, and polyethyleneimine is described. Patent Document 3 proposes a semiconductor wafer polishing composition containing surface-modified silica and a non-ionic water-soluble polymer (claim 10). The document lists hydroxyethyl cellulose, polyvinyl alcohol, etc. as non-ionic water-soluble polymers, and describes that the preferred concentration of the non-ionic water-soluble polymer is 0.025 to 0.3% by weight relative to silicon oxide (paragraph

[0053] ). The example of the document describes a polishing composition containing surface-modified silica, tetramethylammonium hydroxide, and diallyldimethylammonium maleic acid copolymer. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2015-109423 A [Patent Document 2] JP 2006-352042 A [Patent Document 3] JP 2016-20294 A Summary of the Invention [Problem to be solved by the invention]

[0006] In recent years, requirements for the surface quality of silicon substrates such as silicon wafers have become increasingly stringent, and there is a demand for a polishing composition that can improve the removal rate while reducing the surface roughness (haze) of the silicon substrate and reducing surface defects (LPD and / or LPD-N).

[0007] Therefore, the present disclosure provides a polishing composition that can achieve an improvement in the polishing rate, a reduction in the surface roughness (haze) of a silicon substrate, and a reduction in surface defects (LPD and / or LPD-N), as well as a polishing method using the same and a method for manufacturing a semiconductor substrate. [Means for solving the problem]

[0008] In one aspect, the present disclosure relates to a polishing liquid composition for silicon substrates, comprising the following component A, the following component B, and the following component D, wherein a mass ratio D / A of the content of component D to the content of component A is 0.01 or more and 0.2 or less, and a pH is more than 8.5 and 14 or less. Component A: Silica particles Component B: Cationic water-soluble polymer having a nitrogen-containing group (excluding polyalkyleneimine) Component D: A nonionic water-soluble polymer having an alkylene oxide group or a hydroxyl group in the molecule and a weight average molecular weight of 2,000 or more and less than 500,000.

[0009] In one aspect, the present disclosure relates to a method for polishing a silicon substrate, comprising a step of polishing a silicon substrate to be polished with the polishing liquid composition of the present disclosure.

[0010] In one aspect, the present disclosure relates to a method for producing a semiconductor substrate, the method including: polishing a silicon substrate to be polished with the polishing liquid composition of the present disclosure; and cleaning the polished silicon substrate. Effect of the Invention

[0011] According to the present disclosure, it is possible to provide a polishing liquid composition that can achieve an improvement in the polishing rate, a reduction in the surface roughness (haze) of a silicon substrate, and a reduction in surface defects (LPD and / or LPD-N), as well as a polishing method that uses the polishing liquid composition and a method for manufacturing a semiconductor substrate. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] The present disclosure is based on the finding that by adding a water-soluble polymer having a cationic group and a specific hydrophobic group to a polishing composition containing silica particles and a nitrogen-containing basic compound, it is possible to achieve an improvement in the polishing rate, a reduction in surface roughness (haze), and a reduction in surface defects (LPD and / or LPD-N).

[0013] That is, in one aspect, the present disclosure relates to a polishing liquid composition for silicon substrates (hereinafter also referred to as the "polishing liquid composition of the present disclosure") that contains the following component A, the following component B, and the following component D, wherein the mass ratio D / A of the content of component D to the content of component A is 0.01 or more and 0.2 or less, and the pH is more than 8.5 and 14 or less. Component A: Silica particles Component B: Cationic water-soluble polymer having a nitrogen-containing group (excluding polyalkyleneimine) Component D: A nonionic water-soluble polymer having an alkylene oxide group or a hydroxyl group in the molecule and a weight average molecular weight of 2,000 or more and less than 500,000.

[0014] According to the present disclosure, in one or more embodiments, it is possible to achieve an improvement in the polishing rate, a reduction in the surface roughness (haze) of the silicon substrate, and a reduction in surface defects (LPD, LPD-N). According to the present disclosure, in one or more embodiments, it is possible to reduce the surface roughness (haze) and surface defects without significantly impairing the polishing rate. According to the present disclosure, in one or more embodiments, it is possible to improve the polishing rate and suppress the surface roughness (haze) and surface defects. According to the present disclosure, in one or more embodiments, it is possible to improve the polishing rate and suppress the reduction in the surface roughness (haze) and surface defects.

[0015] Although the details of the mechanism by which the effects of the present disclosure are exerted are not clear, it is presumed as follows. In the present disclosure, it is believed that the cationic water-soluble polymer (component B) is adsorbed to the silica particles (component A), thereby increasing the frequency of contact of the silica particles (component A) with the silicon substrate to be polished, thereby contributing to an improvement in the polishing rate. In addition, when the cationic water-soluble polymer (component B) is used in combination with a specified amount of a specific nonionic water-soluble polymer (component D), the two types of water-soluble polymers are thickly adsorbed onto the surface of the silicon substrate to be polished, which is thought to suppress corrosion of the silicon substrate surface and reduce surface roughness (haze) and surface defects (LPD, LPD-N). However, the present disclosure need not be construed as being limited to these mechanisms.

[0016] [Silica particles (component A)] The polishing liquid composition of the present disclosure contains silica particles (hereinafter also referred to as "Component A") as an abrasive. Examples of Component A include colloidal silica, fumed silica, pulverized silica, and surface-modified silica thereof, and from the viewpoint of achieving an improvement in the polishing rate, a reduction in surface roughness (haze), and a reduction in surface defects (LPD, LPD-N), colloidal silica is preferred. Component A may be one type or a combination of two or more types.

[0017] From the viewpoint of operability, the use form of component A is preferably a slurry form.When component A contained in the polishing liquid composition of the present disclosure is colloidal silica, from the viewpoint of preventing contamination of silicon substrate by alkali metal, alkaline earth metal, etc., the colloidal silica is preferably obtained from the hydrolysis product of alkoxysilane.The silica particles obtained from the hydrolysis product of alkoxysilane can be produced by a conventionally known method.

[0018] From the viewpoint of achieving an improvement in polishing rate, a reduction in surface roughness (haze), and a reduction in surface defects (LPD, LPD-N), the average primary particle diameter of component A is preferably 10 nm or more, more preferably 15 nm or more, even more preferably 20 nm or more, and preferably 40 nm or less, more preferably 35 nm or less, and even more preferably 30 nm or less. From the same viewpoint, the average primary particle diameter of component A is preferably 10 nm or more and 40 nm or less, more preferably 15 nm or more and 35 nm or less, even more preferably 15 nm or more and 30 nm or less, and even more preferably 20 nm or more and 30 nm or less. In particular, when colloidal silica is used as component A, from the same viewpoint, the average primary particle diameter of component A is preferably 10 nm or more, more preferably 15 nm or more, even more preferably 20 nm or more, and preferably 40 nm or less, more preferably 35 nm or less, and even more preferably 30 nm or less.

[0019] In the present disclosure, the average primary particle size of component A is defined as the specific surface area S (m 2 The specific surface area can be measured, for example, by the method described in the Examples.

[0020] From the viewpoint of achieving an improvement in the polishing rate, a reduction in surface roughness (haze), and a reduction in surface defects (LPD, LPD-N), the average secondary particle diameter of component A is preferably 20 nm or more, more preferably 30 nm or more, even more preferably 40 nm or more, and is preferably 80 nm or less, more preferably 75 nm or less, and even more preferably 70 nm or less. From the same viewpoint, the average secondary particle diameter of component A is preferably 20 nm or more and 80 nm or less, more preferably 30 nm or more and 75 nm or less, and even more preferably 40 nm or more and 70 nm or less. In the present disclosure, the average secondary particle diameter is a value measured by a dynamic light scattering (DLS) method, and can be measured, for example, using the device described in the examples.

[0021] From the viewpoints of improving the polishing rate, reducing surface roughness (haze), and reducing surface defects (LPD, LPD-N), the degree of association of component A is preferably 3 or less, more preferably 2.5 or less, even more preferably 2.3 or less, and preferably 1.1 or more, more preferably 1.5 or more, and even more preferably 1.8 or more. When component A is colloidal silica, from the same viewpoints, the degree of association is preferably 3 or less, more preferably 2.5 or less, even more preferably 2.3 or less, and preferably 1.1 or more, more preferably 1.5 or more, and even more preferably 1.8 or more.

[0022] In the present disclosure, the degree of association of component A is a coefficient representing the shape of the silica particles and is calculated by the following formula. Degree of association = average secondary particle size / average primary particle size

[0023] The degree of association of Component A can be adjusted by using the methods described in, for example, JP-A-6-254383, JP-A-11-214338, JP-A-11-60232, JP-A-2005-060217, JP-A-2005-060219, and the like.

[0024] The shape of component A is preferably a so-called sphere type and / or a so-called cocoon type.

[0025] From the viewpoints of improving the polishing rate, reducing surface roughness (haze), and reducing surface defects (LPD, LPD-N), the content of component A in the polishing liquid composition of the present disclosure is preferably 0.01 mass% or more, more preferably 0.05 mass% or more, even more preferably 0.07 mass% or more, and even more preferably 0.1 mass% or more, and is preferably 2.5 mass% or less, more preferably 1 mass% or less, even more preferably 0.8 mass% or less, even more preferably 0.5 mass% or less, even more preferably 0.3 mass% or less, and even more preferably 0.2 mass% or less, calculated as SiO2. From the same viewpoint, the content of Component A in the polishing liquid composition of the present disclosure is preferably 0.01 mass % or more and 2.5 mass % or less, more preferably 0.05 mass % or more and 1 mass % or less, even more preferably 0.07 mass % or more and 0.8 mass % or less, even more preferably 0.1 mass % or more and 0.5 mass % or less, and even more preferably 0.1 mass % or more and 0.3 mass % or less, calculated as SiO2. When Component A is a combination of two or more kinds, the content of Component A refers to the total content thereof.

[0026] [Cationic water-soluble polymer (component B)] In one or more embodiments, the polishing composition of the present disclosure contains a cationic water-soluble polymer having a nitrogen-containing group (hereinafter also referred to as "Component B") from the viewpoint of achieving an improvement in the polishing rate, a reduction in surface roughness (haze), and a reduction in surface defects (LPD, LPD-N). In one or more embodiments, Component B does not contain a polyalkyleneimine. Component B may be one type or a combination of two or more types.

[0027] From the viewpoint of achieving both an improvement in the polishing rate and a reduction in surface roughness (haze), the nitrogen-containing group of Component B is preferably at least one group selected from an amino group, a quaternary ammonium group, and salts thereof, and more preferably at least one group selected from an allylamino group, a diallylamino group, a quaternary ammonium group, and salts thereof. Examples of the salt include hydrochloride, hydrobromide, acetate, sulfate, nitrate, sulfite, phosphate, amidosulfate, methanesulfonate, and ethanesulfonate.

[0028] From the viewpoint of achieving both an improvement in the polishing rate and a reduction in surface roughness (haze), Component B is preferably a cationic polymer having, at least in the main chain and side chains, at least one nitrogen-containing group selected from an allylamino group, a diallylamino group, a quaternary ammonium group, and a salt thereof, and more preferably contains a constituent unit derived from at least one monomer selected from allylamine, diallylamine, dimethylallylamine, methyldiallylamine, diallyldimethylammonium, diallylmethylethylammonium, and a salt thereof.

[0029] In one or a plurality of embodiments, Component B may be at least one selected from allylamine polymers, allylamine hydrochloride polymers, allylamine hydrochloride-sulfur dioxide copolymers, diallylamine polymers, diallylamine hydrochloride polymers, diallylamine hydrochloride-sulfur dioxide copolymers, allylamine acetate-diallylamine acetate copolymers, allylamine hydrochloride-dimethylallylamine hydrochloride copolymers, methyldiallylamine polymers, methyldiallylamine hydrochloride polymers, diallyldimethylammonium chloride polymers, diallyldimethylammonium chloride-sulfur dioxide copolymers, diallyldimethylammonium chloride-acrylamide copolymers, diallylamine amide sulfate-maleic acid copolymers, methyldiallylamine-maleic acid copolymers, diallyldimethylammonium chloride-maleic acid copolymers, and maleic acid-diallyldimethylammonium ethyl sulfate-sulfur dioxide copolymers.

[0030] From the viewpoint of achieving both an improvement in the polishing rate and a reduction in surface roughness (haze), the weight-average molecular weight of component B is preferably 800 or more, more preferably 1,000 or more, and even more preferably 2,000 or more, and from the same viewpoint, it is preferably 200,000 or less, more preferably 100,000 or less, and even more preferably 60,000 or less. The weight-average molecular weight of component B can be measured by the method described in the Examples below.

[0031] The content of component B in the polishing liquid composition of the present disclosure is preferably 10 mass ppm or more, more preferably 20 mass ppm or more, even more preferably 30 mass ppm or more, and even more preferably 50 mass ppm or more from the viewpoint of achieving an improvement in the polishing rate, a reduction in surface roughness (haze), and a reduction in surface defects (LPD, LPD-N). From the viewpoint of dispersibility of the polishing liquid and a reduction in surface roughness (haze), it is preferably 500 mass ppm or less, more preferably 200 mass ppm or less, even more preferably 150 mass ppm or less, and even more preferably 120 mass ppm or less. From the same viewpoint, the content of component B in the polishing liquid composition of the present disclosure is preferably 10 mass ppm or more and 500 mass ppm or less, more preferably 20 mass ppm or more and 200 mass ppm or less, even more preferably 30 mass ppm or more and 150 mass ppm or less, and even more preferably 50 mass ppm or more and 120 mass ppm or less. When component B is a combination of two or more kinds, the content of component B refers to the total content thereof. In this disclosure, 1% by mass is equal to 10,000 ppm by mass (the same applies below).

[0032] In the polishing liquid composition of the present disclosure, the ratio B / A of the content of component B to the content of component A (mass ratio B / A) is preferably 0.005 or more, more preferably 0.01 or more, even more preferably 0.02 or more, and preferably 0.2 or less, more preferably 0.15 or less, and even more preferably 0.1 or less, from the viewpoint of achieving an improvement in the polishing rate, a reduction in surface roughness (haze), and a reduction in surface defects (LPD, LPD-N). From the same viewpoint, the mass ratio B / A in the polishing liquid composition of the present disclosure is preferably 0.005 or more and 0.2 or less, more preferably 0.01 or more and 0.15 or less, and even more preferably 0.02 or more and 0.1 or less.

[0033] In the polishing liquid composition of the present disclosure, the ratio B / D of the content of component B to the content of component D (mass ratio B / D) is preferably 0.1 or more, more preferably 0.2 or more, even more preferably 0.3 or more, and preferably 2 or less, more preferably 1.2 or less, and even more preferably 0.9 or less, from the viewpoint of achieving an improvement in the polishing rate, a reduction in surface roughness (haze), and a reduction in surface defects (LPD, LPD-N). From the same viewpoint, the mass ratio C / D in the polishing liquid composition of the present disclosure is preferably 0.1 or more and 2 or less, more preferably 0.2 or more and 2 or less, more preferably 0.2 or more and 1.2 or less, and even more preferably 0.3 or more and 0.9 or less.

[0034] [Nonionic water-soluble polymer (ingredient D)] In one or more embodiments, the polishing composition of the present disclosure contains a nonionic water-soluble polymer (hereinafter also referred to as "Component D") having an alkylene oxide group or a hydroxyl group in the molecule and having a weight-average molecular weight of 2,000 or more and less than 500,000, from the viewpoint of achieving an improvement in the polishing rate, a reduction in surface roughness (haze), and a reduction in surface defects (LPD, LPD-N). Component D may be one type or a combination of two or more types. In the present disclosure, "water-soluble" refers to having a solubility in water (20° C.) of 0.5 g / 100 mL or more, preferably a solubility of 2 g / 100 mL or more.

[0035] When Component D has an alkylene oxide group in the molecule, examples of the alkylene oxide group include an ethylene oxide group and a propylene oxide group.

[0036] As component D, from the viewpoints of improving the polishing rate, reducing surface roughness (haze), and reducing surface defects (LPD, LPD-N), at least one selected from polyglycerin, polyglycerin alkyl ether, polyglycerin alkyl ester, hydroxyalkyl cellulose, polyvinyl alcohol, and polyhydroxyethyl acrylamide is preferable, polyglycerin or hydroxyalkyl cellulose is more preferable, and polyglycerin is even more preferable. The alkyl group of the polyglycerol alkyl ether is preferably an alkyl group having 3 to 22 carbon atoms, more preferably an alkyl group having 5 to 16 carbon atoms, and even more preferably an alkyl group having 7 to 12 carbon atoms, from the viewpoint of improving wettability, and is preferably 5 or more, more preferably 10 or more, more preferably 15 or more, and even more preferably 18 or more, and is preferably 100 or less, more preferably 60 or less, more preferably 45 or less, and even more preferably 25 or less, from the viewpoint of improving polishing speed, reducing surface roughness (haze), and reducing surface defects (LPD, LPD-N). Examples of the polyglycerol alkyl ether include polyglycerol lauryl ether, polyglycerol decyl ether, and polyglycerol myristyl ether. The alkyl group of the polyglycerol alkyl ester is preferably an alkyl group having 3 to 22 carbon atoms, more preferably an alkyl group having 5 to 16 carbon atoms, and even more preferably an alkyl group having 7 to 12 carbon atoms, from the viewpoint of improving wettability, and is preferably 5 or more, more preferably 10 or more, more preferably 15 or more, and even more preferably 18 or more, and is preferably 100 or less, more preferably 60 or less, more preferably 45 or less, and even more preferably 25 or less, from the viewpoint of achieving both an improvement in polishing rate and a reduction in surface roughness (haze). Examples of the polyglycerol alkyl ester include polyglycerol lauryl ester, polyglycerol decyl ester, and polyglycerol myristyl ester. From the viewpoint of improving the polishing rate, reducing surface roughness (haze), and reducing surface defects (LPD, LPD-N), the hydroxyalkyl cellulose is preferably at least one selected from hydroxyethyl cellulose (hereinafter also referred to as "HEC"), hydroxypropyl cellulose, and hydroxybutyl cellulose, and HEC is more preferable. Among these, from the viewpoints of achieving an improvement in the polishing rate, a reduction in surface roughness (haze), and a reduction in surface defects (LPD, LPD-N), component D is preferably at least one selected from polyglycerin, polyvinyl alcohol (PVA), and hydroxyethyl cellulose (HEC).

[0037] From the viewpoints of improving the polishing rate, reducing surface roughness (haze), and reducing surface defects (LPD, LPD-N), the weight-average molecular weight of component D is preferably 2,000 or more, more preferably 2,500 or more, and even more preferably 2,800 or more. From the same viewpoints and also from the viewpoint of filterability of the polishing liquid, the weight-average molecular weight is preferably less than 500,000, more preferably 400,000 or less, and even more preferably 300,000 or less. When component D is polyglycerol, from the same viewpoint, the weight average molecular weight of component C is preferably 2,000 or more, more preferably 2,500 or more, even more preferably 2,800 or more, and is preferably 10,000 or less, more preferably 8,000 or less, even more preferably 6,000 or less. When component D is PVA, from the same viewpoint, the weight average molecular weight of component D is preferably 5,000 or more, more preferably 10,000 or more, and even more preferably 20,000 or more, and is preferably 150,000 or less, more preferably 120,000 or less, and even more preferably 100,000 or less. When component D is HEC, from the same viewpoint, the weight average molecular weight of component D is preferably 50,000 or more, more preferably 100,000 or more, and even more preferably 150,000 or more, and is preferably 500,000 or less, more preferably 400,000 or less, and even more preferably 300,000 or less. The weight average molecular weight of Component D can be measured by the method described in the Examples below.

[0038] The content of component D in the polishing composition of the present disclosure is preferably 10 mass ppm or more, more preferably 30 mass ppm or more, even more preferably 50 mass ppm or more, and preferably 1,000 mass ppm or less, more preferably 500 mass ppm or less, and even more preferably 300 mass ppm or less, from the viewpoint of achieving an improvement in the polishing rate, a reduction in surface roughness (haze), and a reduction in surface defects (LPD, LPD-N). From the same viewpoint, the content of component D is preferably 10 mass ppm or more and 1,000 mass ppm or less, more preferably 30 mass ppm or more and 500 mass ppm or less, and even more preferably 50 mass ppm or more and 300 mass ppm or less. When component D is a combination of two or more kinds, the content of component D refers to the total content thereof.

[0039] In the polishing composition of the present disclosure, the ratio D / A (mass ratio D / A) of the content of component D to the content of component A is 0.01 or more, preferably 0.02 or more, more preferably 0.03 or more, even more preferably 0.04 or more, even more preferably 0.05 or more, even more preferably 0.06 or more, even more preferably 0.07 or more, and 0.2 or less, preferably 0.19 or less, more preferably 0.18 or less, even more preferably 0.17 or less, and even more preferably 0.16 or less, from the viewpoint of achieving an improvement in the polishing rate, a reduction in surface roughness (haze), and a reduction in surface defects (LPD, LPD-N). From the same viewpoint, the mass ratio D / A is 0.01 or more and 0.2 or less, preferably 0.02 or more and 0.19 or less, and even more preferably 0.03 or more and 0.18 or less.

[0040] [water] In one or more embodiments, the polishing liquid composition of the present disclosure may contain water. Examples of water include ion-exchanged water and ultrapure water, and ultrapure water is preferred from the viewpoint of both improving the polishing rate and reducing the surface roughness (haze). The content of water in the polishing liquid composition of the present disclosure may be, for example, the remainder of component A, component B, component D, and other components described below.

[0041] [Nitrogen-containing basic compound (component C)] In one or more embodiments, the polishing liquid composition of the present disclosure may contain a nitrogen-containing basic compound (hereinafter, also referred to as "component C"). From the viewpoint of achieving an improvement in the polishing rate, a reduction in surface roughness (haze), and a reduction in surface defects (LPD, LPD-N), component C is preferably a water-soluble nitrogen-containing basic compound. In the present disclosure, "water-soluble" refers to a solubility of 0.5 g / 100 mL or more, preferably 2 g / 100 mL or more, in water (20°C). In the present disclosure, "water-soluble nitrogen-containing basic" refers to a nitrogen-containing compound that exhibits basicity when dissolved in water. In one or more embodiments, component C does not include a cationic water-soluble polymer (component B) having a nitrogen-containing group. Component C may be one type or a combination of two or more types.

[0042] In one or more embodiments, component C may be at least one selected from an amine compound and an ammonium compound. For example, component C may be one or a combination of two or more selected from ammonia, ammonium hydroxide, ammonium carbonate, ammonium hydrogen carbonate, dimethylamine, trimethylamine, diethylamine, triethylamine, monoethanolamine, diethanolamine, triethanolamine, N-methylethanolamine, N-methyl-N,N-diethanolamine, N,N-dimethylethanolamine, N,N-diethylethanolamine, N,N-dibutylethanolamine, N-(β-aminoethyl)ethanolamine, monoisopropanolamine, diisopropanolamine, triisopropanolamine, ethylenediamine, hexamethylenediamine, piperazine hexahydrate, anhydrous piperazine, 1-(2-aminoethyl)piperazine, N-methylpiperazine, diethylenetriamine, tetramethylammonium hydroxide, and hydroxylamine. Among these, from the viewpoint of achieving an improvement in the polishing rate, a reduction in surface roughness (haze), and a reduction in surface defects (LPD, LPD-N), Component C is preferably ammonia or a mixture of ammonia and hydroxyamine, and more preferably ammonia.

[0043] When the polishing composition of the present disclosure contains component C, the content of component C in the polishing composition of the present disclosure is preferably 5 mass ppm or more, more preferably 10 mass ppm or more, even more preferably 20 mass ppm or more, and preferably 500 mass ppm or less, more preferably 300 mass ppm or less, and even more preferably 100 mass ppm or less, from the viewpoint of achieving an improvement in the polishing rate, a reduction in surface roughness (haze), and a reduction in surface defects (LPD, LPD-N). From the same viewpoint, the content of component C in the polishing composition of the present disclosure is preferably 5 mass ppm or more and 500 mass ppm or less, more preferably 10 mass ppm or more and 300 mass ppm or less, and even more preferably 20 mass ppm or more and 100 mass ppm or less. When component C is a combination of two or more kinds, the content of component C refers to the total content thereof.

[0044] From the viewpoints of achieving an improvement in the polishing rate, a reduction in surface roughness (haze), and a reduction in surface defects (LPD, LPD-N), the ratio C / A of the content of component C to the content of component A (mass ratio C / A) in the polishing liquid composition of the present disclosure is preferably 0.002 or more, more preferably 0.01 or more, even more preferably 0.025 or more, and preferably 1 or less, more preferably 0.5 or less, and even more preferably 0.1 or less. From the same viewpoint, the mass ratio C / A in the polishing liquid composition of the present disclosure is preferably 0.002 or more and 1 or less, more preferably 0.01 or more and 0.5 or less, and even more preferably 0.025 or more and 0.1 or less.

[0045] [Water-soluble polymer having an alkylene oxide group (Component E)] In one or more embodiments, the polishing liquid composition of the present disclosure may contain a water-soluble polymer having an alkylene oxide group with a weight average molecular weight of less than 2,000 other than components B and D (hereinafter, simply referred to as "component E") from the viewpoint of reducing surface roughness (haze) and reducing surface defects (LPD, LPD-N). Examples of the alkylene oxide group include an ethylene oxide group and a propylene oxide group. Examples of component E include polyethylene glycol, polypropylene glycol, polyethylene oxide-polypropylene oxide random copolymer, polyethylene oxide-polypropylene oxide block copolymer, and the like. Component E may be one type or a combination of two or more types.

[0046] From the viewpoint of improving the polishing rate, reducing surface roughness (haze), and reducing surface defects (LPD, LPD-N), the weight average molecular weight of component E is preferably 200 or more, more preferably 400 or more, and even more preferably 800 or more, and from the same viewpoint, it is preferably 1,800 or less, more preferably 1,600 or less, and even more preferably 1,500 or less. From the same viewpoint, the weight average molecular weight of component E is preferably 200 or more and 1,800 or less, more preferably 400 or more and 1,600 or less, and even more preferably 800 or more and 1,500 or less. The weight average molecular weight of component E can be measured by the method described in the Examples below.

[0047] When the polishing composition of the present disclosure contains component E, the content of component E in the polishing composition of the present disclosure is preferably 1 mass ppm or more, more preferably 4 mass ppm or more, and even more preferably 8 mass ppm or more from the viewpoint of improving the polishing rate and reducing surface roughness (haze) and from the viewpoint of reducing surface defects (LPD). And, from the viewpoint of improving the polishing rate, it is preferably 100 mass ppm or less, more preferably 50 mass ppm or less, and even more preferably 20 mass ppm or less. When component E is a combination of two or more kinds, the content of component E refers to the total content thereof.

[0048] In the polishing liquid composition of the present disclosure, the ratio of the content of component E to the content of component D (mass ratio E / D) is, from the viewpoints of achieving an improvement in the polishing rate, a reduction in surface roughness (haze), and a reduction in surface defects (LPD, LPD-N), preferably 0.01 or more, more preferably 0.04 or more, and even more preferably 0.08 or more, and from the viewpoint of improving the polishing rate, preferably 1 or less, more preferably 0.5 or less, and even more preferably 0.2 or less.

[0049] [Other ingredients] The polishing liquid composition of the present disclosure may further contain other components to the extent that the effects of the present disclosure are not impaired. In one or more embodiments, the other components include at least one selected from water-soluble polymers other than Components B, D, and E, surfactants other than Components B, D, and E, pH adjusters other than Component C, preservatives, alcohols, chelating agents, and oxidizing agents.

[0050] The pH of the polishing liquid composition of the present disclosure is more than 8.5, preferably 9 or more, more preferably 9.5 or more, and more preferably 10 or more, from the viewpoint of improving the polishing rate and storage stability, and is 14 or less, preferably 13 or less, more preferably 12.5 or less, more preferably 12 or less, more preferably 11.5 or less, and more preferably 11 or less, from the viewpoint of improving the surface quality. From the same viewpoint, the pH of the polishing liquid composition of the present disclosure is more than 8.5 to 14 or less, preferably 9 to 13 or less, more preferably 9.5 to 12.5 or less, more preferably 9.5 to 12 or less, more preferably 9.5 to 11.5 or less, and more preferably 10 to 11 or less. The pH of the polishing liquid composition of the present disclosure can be adjusted using component C or a known pH adjuster. In the present disclosure, the above pH is a value measured by the method described in the Examples.

[0051] The polishing liquid composition of the present disclosure can be produced, for example, by blending component A, component B, component D, and, if desired, optional components (component C, component E, other components) by a known method. That is, in another aspect, the present disclosure relates to a method for producing a polishing liquid composition, which includes a step of blending at least component A, component B, and component D. In the present disclosure, "blending" includes mixing component A, component B, component D, and optional components (component C, component E, other components) simultaneously or in any order as necessary. The blending can be performed using, for example, a stirrer such as a homomixer, a homogenizer, an ultrasonic disperser, a wet ball mill, or a bead mill. The preferred blending amount of each component in the method for producing a polishing liquid composition of the present disclosure can be the same as the preferred content of each component in the polishing liquid composition of the present disclosure described above.

[0052] In the present disclosure, "the content of each component in the polishing liquid composition" refers to the content of each component at the time of use, that is, at the time when the polishing liquid composition is started to be used for polishing.

[0053] The polishing liquid composition of the present disclosure may be produced as a concentrate from the viewpoint of storage and transportation, and diluted at the time of use. The dilution ratio is preferably 2 times or more, more preferably 10 times or more, even more preferably 30 times or more, even more preferably 50 times or more from the viewpoint of production and transportation costs and storage stability, and is preferably 180 times or less, more preferably 140 times or less, even more preferably 100 times or less, even more preferably 70 times or less from the viewpoint of storage stability. The polishing liquid composition concentrate of the present disclosure can be used by diluting with water (component D) so that the content of each component at the time of use is the above-mentioned content (i.e., the content at the time of use). In the present disclosure, the "time of use" of the polishing liquid composition concentrate refers to the state in which the polishing liquid composition concentrate is diluted.

[0054] [Polished silicon substrate] In one or more embodiments, the polishing liquid composition of the present disclosure is a polishing composition for silicon substrates, and can be used, for example, in a polishing step of polishing a silicon substrate in a manufacturing method of a semiconductor substrate, or in a polishing step of polishing a silicon substrate in a polishing method of a silicon substrate. In one or more embodiments, the silicon substrate to be polished using the polishing liquid composition of the present disclosure may be a silicon substrate, and in one or more embodiments, a single crystal silicon substrate or a polysilicon substrate. Examples of single crystal silicon substrates include a single crystal 100-face silicon substrate, a 111-face silicon substrate, and a 110-face silicon substrate. In addition, the resistivity of the silicon substrate is preferably 0.0001 Ω·cm or more, more preferably 0.001 Ω·cm or more, even more preferably 0.01 Ω·cm or more, even more preferably 0.1 Ω·cm or more, and is preferably 100 Ω·cm or less, more preferably 50 Ω·cm or less, and even more preferably 20 Ω·cm or less, from the viewpoint of achieving an improvement in the polishing rate, a reduction in surface roughness (haze), and a reduction in surface defects (LPD, LPD-N).

[0055] [Polishing liquid kit] In another aspect, the present disclosure relates to a polishing liquid kit for producing the polishing liquid composition of the present disclosure (hereinafter, sometimes abbreviated as "the kit of the present disclosure"). According to the kit of the present disclosure, a polishing liquid composition that can achieve an improvement in removal rate, a reduction in surface roughness (haze), and a reduction in surface defects (LPD, LPD-N) can be obtained. In one or more embodiments, the kit of the present disclosure may be a polishing liquid kit containing a solution containing component A, component B, and component D. The solution may contain the above-mentioned optional components (component C, component E, and other components) as necessary. The solution may be diluted with water as necessary at the time of use. In one or more embodiments, the polishing liquid kit of the present disclosure includes a polishing liquid kit (two-liquid type polishing liquid composition) that contains a silica dispersion (Liquid 1a) containing Components A and C and an additive aqueous solution (Liquid 2a) containing Components B, D, and E in a mutually unmixed state, which are mixed at the time of use and diluted with water as necessary. Liquids 1a and 2a may contain other components as necessary. In one or more embodiments, the polishing liquid kit of the present disclosure includes a polishing liquid kit (two-liquid type polishing liquid composition) that contains, in a mutually unmixed state, a silica dispersion liquid (Liquid 1b) containing Components A, C, and D, and an additive aqueous solution (Liquid 2b) containing Component B, which are mixed at the time of use and diluted with water as necessary. Liquids 1b and 2b may contain Component E and other components as necessary.

[0056] [Silicon substrate polishing method] In another aspect, the present disclosure relates to a method for polishing a silicon substrate (hereinafter also referred to as the polishing method of the present disclosure), which includes a step of polishing a silicon substrate to be polished using the polishing composition of the present disclosure (hereinafter also referred to as the "polishing step"). According to the polishing method of the present disclosure, since the polishing composition of the present disclosure is used, it is possible to achieve an improvement in the polishing rate, a reduction in surface roughness (haze), and a reduction in surface defects (LPD, LPD-N).

[0057] In the polishing step of the polishing method of the present disclosure, for example, the silicon substrate can be pressed against a platen to which a polishing pad is attached, and the silicon substrate can be polished at a polishing pressure of 3 to 20 kPa. In the present disclosure, the polishing pressure refers to the pressure of the platen applied to the surface of the silicon substrate during polishing.

[0058] In the polishing step of the polishing method of the present disclosure, for example, a silicon substrate to be polished can be pressed against a platen to which a polishing pad is attached, and the silicon substrate to be polished can be polished with a polishing liquid composition and a polishing pad surface temperature of 15° C. to 40° C. From the viewpoint of achieving both an improvement in the polishing rate and a reduction in surface roughness (haze), the temperature of the polishing liquid composition and the polishing pad surface temperature are preferably 15° C. or higher or 20° C. or higher, and preferably 40° C. or lower or 30° C. or lower.

[0059] [Method of manufacturing semiconductor substrate] In another aspect, the present disclosure relates to a method for producing a semiconductor substrate (hereinafter also referred to as the "semiconductor substrate production method of the present disclosure"), which includes a step of polishing a silicon substrate to be polished using the polishing liquid composition of the present disclosure (hereinafter also referred to as the "polishing step") and a step of cleaning the polished silicon substrate (hereinafter also referred to as the "cleaning step"). According to the semiconductor substrate production method of the present disclosure, by using the polishing liquid composition of the present disclosure, it is possible to achieve an improvement in the polishing rate, a reduction in surface roughness (haze), and a reduction in surface defects (LPD, LPD-N), and therefore it is possible to produce high-quality semiconductor substrates with high yield and good productivity.

[0060] The polishing step in the semiconductor substrate manufacturing method of the present disclosure can include, for example, a lapping (rough polishing) step of planarizing a single crystal silicon substrate obtained by slicing a single crystal silicon ingot into a thin disk shape, and a finish polishing step of etching the lapped single crystal silicon substrate and then mirror-finishing the surface of the single crystal silicon substrate. The polishing composition of the present disclosure is more preferably used in the finish polishing step from the viewpoints of achieving an improvement in the polishing rate, a reduction in surface roughness (haze), and a reduction in surface defects (LPD, LPD-N).

[0061] The polishing step in the semiconductor substrate manufacturing method of the present disclosure can be performed under the same conditions (polishing pressure, polishing liquid composition, surface temperature of polishing pad, etc.) as those in the polishing step in the polishing method of the present disclosure described above.

[0062] In one or more embodiments, the method for producing a semiconductor substrate according to the present disclosure may include a dilution step of diluting a concentrate of the polishing liquid composition according to the present disclosure prior to the polishing step. The dilution medium may be, for example, water.

[0063] In the cleaning step in the semiconductor substrate manufacturing method of the present disclosure, it is preferable to perform inorganic cleaning from the viewpoint of reducing residues on the silicon substrate surface. Examples of the cleaning agent used in inorganic cleaning include inorganic cleaning agents containing at least one selected from hydrogen peroxide, ammonia, hydrochloric acid, sulfuric acid, hydrofluoric acid, and ozone water.

[0064] In one or a plurality of embodiments, the semiconductor substrate manufacturing method of the present disclosure can further include, after the cleaning step, a step of rinsing the cleaned silicon substrate with water and drying it. EXAMPLES

[0065] The present disclosure will be described in more detail below with reference to examples, but these are merely illustrative and the present disclosure is not limited to these examples.

[0066] 1. Preparation of Polishing Compositions (Examples 1 to 16 and Comparative Examples 1 to 5) Polishing liquid compositions of Examples 1 to 16 and Comparative Examples 1 to 5 were obtained by stirring and mixing silica particles (component A) shown in Table 1, cationic water-soluble polymers (component B or non-component B) shown in Table 1, ammonia (component C), nonionic water-soluble polymers (component D or non-component D) shown in Table 1, polyethylene glycol (component E) and ultrapure water. The content of each component in Table 1 is the content of each component at the time of use of the polishing liquid composition (mass % or mass ppm, active content). The content of ultrapure water is the remainder excluding component A and component B or non-component B, component C, component D or non-component D and component E. The pH of each polishing liquid composition (at the time of use) at 25°C was 10.3.

[0067] The following components A, B, non-component B, C, D, non-component D, and E were used in preparing each polishing composition. (Component A) Colloidal silica [average primary particle size 35 nm, average secondary particle size 70 nm, degree of association 2.0] Colloidal silica [average primary particle size 25 nm, average secondary particle size 49 nm, degree of association 2.0] (Component B) B1: Diallyldimethylammonium chloride-sulfur dioxide copolymer [Nittobo Medical PAS-A-5, weight average molecular weight 4,000] B2: Allylamine (free) polymer [Nittobo Medical PAA-03, weight average molecular weight 3,000] B3: Allylamine acetate / diallylamine acetate copolymer [Nittobo Medical PAA-D19A, weight average molecular weight 40,000] B4: Allylamine hydrochloride-dimethylallylamine hydrochloride copolymer [Nittobo Medical PAA-1112CL, weight average molecular weight 1,000] B5: Diallylamine polymer [Nittobo Medical PAS-21, weight average molecular weight 5,000] B6: Methyldiallylamine hydrochloride polymer [Nittobo Medical PAS-M-1, weight average molecular weight 20,000] B7: Diallyldimethylammonium chloride polymer [Nittobo Medical PAS-H-5L, weight average molecular weight 30,000] B8: Diallylamine hydrochloride-sulfur dioxide copolymer [Nittobo Medical PAS-92, weight average molecular weight 5,000] (Non-ingredient B) B9: Polyethyleneimine [Nippon Shokubai Co., Ltd., SP-200, weight average molecular weight 10,000] (Component C) Ammonia [28% by weight ammonia water, Kishida Chemical Co., Ltd., special grade reagent] (Component D) D1: Polyglycerin [Daicel's "XPW", polymerization degree 40, weight average molecular weight 2,980] D2: HEC (hydroxyethyl cellulose) [manufactured by Daicel Corporation, SE400, weight average molecular weight 250,000] (Non-ingredient D) D3: HEC (hydroxyethyl cellulose) [Sumitomo Seika Chemicals, CF-V, weight average molecular weight 800,000] (Component E) PEG (polyethylene glycol) [NOF Corporation, PEG#1000, weight average molecular weight 1,000]

[0068] 2.Measuring methods for various parameters (1) Measurement of the average primary particle size of silica particles (component A) The average primary particle size (nm) of component A is calculated by the BET (nitrogen adsorption) method. 2 / g) using the following formula: Average primary particle diameter (nm)=2727 / S

[0069] The specific surface area S of component A was measured by carrying out the following [pretreatment], and then weighing out approximately 0.1 g of the measurement sample into a measurement cell to four decimal places, drying the sample for 30 minutes in an atmosphere at 110°C immediately before measuring the specific surface area, and then measuring the specific surface area by the nitrogen adsorption method (BET method) using a specific surface area measuring device (Micromeritic automatic specific surface area measuring device "Flowsorb III2305", manufactured by Shimadzu Corporation). [Preprocessing] (a) The pH of the slurry of component A is adjusted to 2.5±0.1 with an aqueous solution of nitric acid. (b) The slurry of component A, adjusted to pH 2.5±0.1, is placed in a petri dish and dried in a hot air dryer at 150°C for 1 hour. (c) After drying, the obtained sample is finely ground in an agate mortar. (d) The ground sample is suspended in ion-exchanged water at 40°C and filtered through a membrane filter with a pore size of 1 μm. (e) The residue on the filter is washed five times with 20 g of ion-exchanged water (40°C). (f) The filter with the filtrate attached thereto is placed in a petri dish and dried in an atmosphere at 110°C for 4 hours. (g) The dried filtrate (component A) was taken, being careful not to mix in any filter debris, and finely ground in a mortar to obtain a measurement sample.

[0070] (2) Average secondary particle size of silica particles (component A) The average secondary particle diameter (nm) of component A was measured by adding an abrasive to ion-exchanged water so that the concentration of component A was 0.25 mass%, and then placing the resulting aqueous dispersion in a disposable sizing cuvette (a 10 mm polystyrene cell) to a height of 10 mm from the bottom, and using a dynamic light scattering method (apparatus name: Zetasizer Nano ZS, manufactured by Sysmex Corporation).

[0071] (3) Measurement of weight average molecular weight of water-soluble polymers (component B, non-component B, component D, non-component D, component E) The weight average molecular weights of the water-soluble polymers (component B, non-component B, component D, non-component D, and component E) were calculated based on peaks in a chromatogram obtained by applying gel permeation chromatography (GPC) under the following conditions. <Nonionic water-soluble polymer> Equipment: HLC-8320 GPC (Tosoh Corporation, detector integrated) Column: GMPWXL+GMPWXL (anion) Eluent: 0.2M phosphate buffer / CH3CN=9 / 1 Flow rate: 0.5mL / min Column temperature: 40℃ Detector: Shodex RI SE-61 differential refractive index detector Standard: Monodisperse polyethylene glycol with known molecular weight <Cationic water-soluble polymer (component B or non-component B)> Equipment: HLC-8320 GPC (Tosoh Corporation, detector integrated) Column: α-M + α-M Eluent: 0.15mol / L Na2SO4,1%CH3COOH / water Flow rate: 1.0mL / min Column temperature: 40℃ Detector: Shodex RI SE-61 differential refractive index detector Standard: Monodisperse polyethylene glycol with known molecular weight

[0072] 3. Polishing method etc. Each polishing composition was filtered with a filter (compact cartridge filter "MCP-LX-C10S", manufactured by Advantech Co., Ltd.) immediately before polishing, and finish polishing and cleaning were performed on the following silicon substrates under the following polishing conditions. <Silicon substrate to be polished> Single crystal silicon substrate [single-sided mirror-finished silicon substrate with a diameter of 200 mm, conductivity type: P, crystal orientation: 100, resistivity: 0.1 Ω·cm or more but less than 100 Ω·cm] The single crystal silicon substrate was previously subjected to rough polishing using a commercially available polishing composition. The haze of the single crystal silicon substrate subjected to finish polishing after rough polishing was 2 to 3 ppm. The haze was measured using a dark field wide grazing incidence channel (DWO) using a KLA Tencor "Surfscan SP1-DLS".

[0073] <Finish polishing conditions> Polishing machine: Single-sided 8-inch polishing machine "GRIND-X SPP600s" (manufactured by Okamoto Kogyo) Polishing pad: Suede pad (manufactured by Toray Co., Ltd., Asker hardness: 64, thickness: 1.37 mm, nap length: 450 μm, opening diameter: 60 μm) Silicon substrate polishing pressure: 100g / cm 2 Plate rotation speed: 60 rpm Polishing time: 5 minutes Supply rate of polishing composition: 150 g / min Temperature of the polishing composition: 23°C Carrier rotation speed: 62 rpm

[0074] <Cleaning method> After the finish polishing, the silicon substrate was subjected to ozone cleaning and dilute hydrofluoric acid cleaning as described below. In the ozone cleaning, an aqueous solution containing 20 ppm ozone was sprayed from a nozzle at a flow rate of 1 L / min toward the center of the silicon substrate rotating at 600 rpm for 3 minutes. The temperature of the ozone water was kept at room temperature. Next, dilute hydrofluoric acid cleaning was performed. In the dilute hydrofluoric acid cleaning, an aqueous solution containing 0.5 mass% ammonium hydrogen fluoride (special grade, Nacalai Tesque, Inc.) was sprayed from a nozzle at a flow rate of 1 L / min toward the center of the silicon substrate rotating at 600 rpm for 6 seconds. The above ozone cleaning and dilute hydrofluoric acid cleaning were performed as one set, for a total of two sets, and finally spin drying was performed. In the spin drying, the silicon substrate was rotated at 1,500 rpm.

[0075] 4. Evaluation [Polishing speed] The weight of each silicon substrate before and after polishing was measured using a precision balance ("BP-210S" manufactured by Sartorius), and the weight difference obtained was divided by the density, area and polishing time of the silicon substrate to obtain the single-sided polishing rate per unit time. The results are shown in Table 1. The weight of the silicon substrate after polishing refers to the weight of the silicon substrate after the above-mentioned finish polishing and cleaning were performed.

[0076] [Evaluation of surface roughness (haze) and surface defects (LPD, LPD-N) of silicon substrates] The surface roughness (haze) of the silicon substrate surface after cleaning was evaluated using the value (DWO haze) measured in the dark field wide grazing incidence channel (DWO) using a surface roughness measuring device "Surfscan SP1-DLS" (KLA Tencor). The smaller the haze (DWO) value, the smoother the surface. The surface defect (LPD) was measured at the same time as the haze measurement and was evaluated by counting the number of particles with a diameter of 45 nm or more on the silicon substrate surface. The smaller the value of the surface defect (LPD), the fewer the surface defects. Surface defects (LPD-N) were measured at the same time as the haze measurement and were evaluated by counting the number of particles with a particle size of 80 nm or more on the silicon substrate surface. The smaller the value of surface defects (LPD-N), the fewer the surface defects. Measurements of surface roughness (haze) and surface defects (LPD, LPD-N) were performed on two silicon substrates each, and the average values ​​were calculated. The results are shown in Table 1. The evaluation criteria for surface defects (LPD, LPD-N) are shown below. <Evaluation criteria for surface defects (LPD)> A: Less than 100 surface defects (LPD) B: Number of surface defects (LPD) is between 100 and 300 C: Number of surface defects (LPD) is between 300 and 500 D: Number of surface defects (LPD) is 500 or more <Evaluation criteria for surface defects (LPD-N)> A: The number of surface defects (LPD-N) is less than 10 B: Number of surface defects (LPD-N) is 10 or more and less than 30 C: Number of surface defects (LPD-N) is 30 or more and less than 50 D: Number of surface defects (LPD-N) is 50 or more

[0077] [Table 1]

[0078] As shown in Table 1, it was found that the polishing compositions of Examples 1 to 16 were able to achieve improved removal rate, reduced haze, and reduced surface defects (LPD, LPD-N) compared to the polishing compositions of Comparative Examples 1 to 5. [Industrial Applicability]

[0079] By using the polishing composition of the present disclosure, both an improvement in the polishing rate and a reduction in surface roughness (haze) can be achieved. Therefore, the polishing composition of the present disclosure is useful as a polishing composition used in the manufacturing process of various semiconductor substrates, and is particularly useful as a polishing composition for finish polishing of silicon substrates.

Claims

1. Contains the following component A, the following component B, and the following component D, a mass ratio D / A of the content of component D to the content of component A is 0.01 or more and 0.2 or less; The pH is greater than 8.5 and less than or equal to 14; A polishing composition for silicon substrates, for use in polishing single crystal silicon substrates or polysilicon substrates. Component A: Silica particles Component B: Cationic water-soluble polymer having a nitrogen-containing group (excluding polyalkyleneimine) Component D: A nonionic water-soluble polymer having an alkylene oxide group or a hydroxyl group in the molecule and a weight average molecular weight of 2,000 or more and less than 500,000.

2. 2. The polishing composition according to claim 1, wherein component B is a cationic polymer having at least one nitrogen-containing group selected from an allylamino group, a diallylamino group, a quaternary ammonium group, and salts thereof at least in the main chain and in the side chains.

3. 3. The polishing composition according to claim 1, wherein Component B contains a structural unit derived from at least one monomer selected from the group consisting of allylamine, diallylamine, dimethylallylamine, methyldiallylamine, diallyldimethylammonium, diallylmethylethylammonium, and salts thereof.

4. 4. The polishing composition according to claim 1, wherein Component D is at least one selected from the group consisting of polyglycerin, polyglycerin alkyl ether, polyglycerin alkyl ester, hydroxyalkyl cellulose, polyvinyl alcohol, and polyhydroxyethylacrylamide.

5. 5. The polishing composition according to claim 1, wherein a mass ratio B / D of the content of component B to the content of component D is 0.2 or more and 2 or less.

6. 6. The polishing composition according to claim 1, further comprising a water-soluble polymer (component E) having an alkylene oxide group and a weight-average molecular weight of less than 2,000, other than components B and D.

7. A polishing composition described in any one of claims 1 to 6, having a pH of greater than 10.

8. A method for polishing a silicon substrate, comprising the step of polishing a silicon substrate to be polished with the polishing composition according to claim 1 .

9. A step of polishing a silicon substrate to be polished using the polishing composition according to any one of claims 1 to 7; and cleaning the polished silicon substrate.

Citation Information

Patent Citations

  • Composition for polishing semiconductor

    JP2006352042A

  • Polishing slurry for barrier layer

    JP2007095713A

  • Polishing liquid composition for silicon wafers

    JP2015109423A

  • Colloidal silica and composition for polishing semiconductor wafer containing the same

    JP2016020294A

  • Polishing liquid composition for silicon wafer

    JP2018006538A